Surface-treated calcium carbonate filler, and resin composition and molded article using same
The surface-treated calcium carbonate filler, optimized with fatty acids and phosphoric acids, addresses the challenges of uniform dispersion and heat resistance in resin compositions, enhancing thermal stability and preventing processing issues in polyolefin resins.
Patent Information
- Application Number
- PCT/JP2023/031097
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2023-08-29
- Publication Date
- 2024-12-05
AI Technical Summary
Current resin compositions with inorganic fillers face challenges in achieving uniform dispersion and sufficient heat resistance, leading to issues like resin burning and clogging during processing, and inadequate thermal stability, especially in polyolefin resins used for various industrial applications.
A surface-treated calcium carbonate filler is developed, treated with fatty acids and phosphoric acids, which has a specific BET surface area, phosphorus content, and calcium conversion rate, ensuring uniform dispersion and enhanced heat resistance in resin compositions, thereby preventing resin burning and clogging.
The surface-treated calcium carbonate filler achieves excellent dispersibility and heat resistance in resin compositions, reducing the risk of resin burning and clogging, and improving the thermal stability of polyolefin resins for various industrial applications.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Surface-treated calcium carbonate filler, and resin composition and molded article using same
[0001] The present invention relates to a surface-treated calcium carbonate filler, and a resin composition and a molded article using the same. More specifically, the present invention relates to a surface-treated calcium carbonate filler that can improve the heat resistance of a resulting resin composition, and a resin composition and a molded article using the same.
[0002] Synthetic resin compositions such as polyolefin-based, polyester-based, polystyrene-based, and vinyl chloride-based compositions are characterized by excellent rigidity, impact resistance, heat resistance, moldability, transparency, and chemical resistance, and are therefore widely used in combination with calcium carbonate inorganic pigments and the like for a wide variety of applications, including various industrial materials, automobile-related parts, various containers for medical or cosmetic use, various films for daily necessities or industrial use, and fibers.
[0003] These resin compositions contain inorganic fillers for various purposes, such as imparting thermal stability, abrasion resistance, rigidity, impact resistance, and thixotropy. In order for resin products containing inorganic fillers to exhibit the desired performance, the inorganic fillers must be sufficiently dispersed in the resin composition. To this end, various improvements have been made to kneading machines and kneading conditions, while the inorganic fillers themselves have also been subjected to various surface treatments to improve their dispersibility in the resin composition, and surface treatment agents and methods for use in such surface treatments have been investigated.
[0004] For example, porous films made from polyolefin resin compositions are produced by forming the polyolefin resin composition into a film and stretching it, and then utilizing the difference in mechanical properties between the polyolefin resin and the inorganic filler to form voids at the interface between the resin and the filler. Such porous films have been researched and developed for a wide variety of applications, including synthetic paper, sanitary materials, medical materials, building materials, agricultural breathable sheets, and battery separators, and some have been put to practical use. However, in order to obtain films with even higher performance, it is necessary to reduce the variation in the size of the voids formed in the film and to ensure a uniform distribution of the voids within the film surface. Furthermore, porous films tend to have poor heat resistance due to the large number of voids formed by stretching during their production process, and improved heat resistance is therefore desired.
[0005] Thus, uniform dispersion of inorganic fillers in resin compositions is extremely important. However, relying solely on mechanical means for dispersion, even if a certain degree of dispersion is achieved, can lead to increased production costs, resin degradation, and even resin decomposition, generating gas and dust, leading to problems such as a poor working environment. Furthermore, if the resin composition has insufficient heat resistance, the inorganic filler and the resin and / or surface treatment agent remaining in the resin composition can burn during kneading and extrusion operations, forming aggregates (resin burnt), which can clog strainers attached inside the extruder die. In film applications, fine-mesh strainers are used, making them particularly susceptible to clogging. Replacing strainers not only requires labor, but also leads to loss of the resin composition used and loss of production time, resulting in significant cost increases.
[0006] To solve these problems, metal soaps such as calcium stearate, phenolic antioxidants, and phosphorus-based antioxidants have been added to these resins to enhance the stability of the resulting resin compositions. Also, calcium carbonate treated with fatty acids such as stearic acid or stearic acid soap has been added to the calcium carbonate itself to enhance the stability of the resin composition.
[0007] For further improvement, Patent Document 1 describes an inorganic filler whose dispersibility in a resin composition is improved by performing a surface treatment on inorganic particles using a surfactant and a chelating agent in combination. Patent Documents 2 and 3 describe further removal of aggregates by combining an operation such as classification.
[0008] The techniques described in Patent Documents 1 to 3 all improve the dispersibility of surface-treated calcium carbonate. However, in the production of such inorganic fillers, the chelating compound captures calcium ions, thereby preventing the reaction between fatty acids and calcium ions. As a result, the proportion of calcium salts of fatty acids produced decreases, and the proportion of remaining fatty acids increases.
[0009] These fatty acids and alkali metal salts of fatty acids are more thermally unstable than calcium salts of fatty acids, and therefore polyolefin resin compositions using these surface-treated calcium carbonates may not have sufficient heat resistance or durability.
[0010] It is possible to stabilize the resulting resin composition by adding a phenolic antioxidant or a phosphorus-based antioxidant to these resins, but because the amount of these added is very small, it is difficult to distribute them uniformly throughout the resin, and problems such as localized unevenness in concentration have been pointed out.
[0011] In recent years, polyolefin resins have been known as relatively environmentally friendly resins, and are expected to be used as base materials for green infrastructure applications. However, as mentioned above, their thermal stability has been pointed out as being insufficient, and there is a growing demand for further heat resistance and durability.
[0012] Japanese Patent Application Laid-Open No. 2002-363443 Japanese Patent Application Laid-Open No. 2006-169421 International Publication No. 2007 / 088707
[0013] The present invention is intended to solve the above problems, and an object of the present invention is to provide a surface-treated calcium carbonate filler that can be dispersed approximately uniformly in a resin composition and can impart high thermal stability to the resin composition, as well as a resin composition and a molded article using the same.
[0014] The present invention provides a surface-treated calcium carbonate filler that includes surface-treated calcium carbonate particles that have been surface-treated with a fatty acid and a phosphoric acid, and satisfies the following formulas (a), (b), and (c): (a) 3≦Sw≦20(m 2 / g) (b) 300≦Pw≦5000 (ppm) (c) 50≦Ca content≦95 (mass%) (Sw is the BET specific surface area (m 2 / g), Pw is the content (ppm) of phosphorus element in the surface-treated calcium carbonate particles measured by an inductively coupled plasma (ICP) atomic emission spectrometer, and the Ca content is the percentage of the mass (g) of fatty acid constituting fatty acid calcium relative to the total surface treatment amount (g) of the surface-treated calcium carbonate particles.
[0015] In one embodiment, the surface-treated calcium carbonate filler of the present invention further satisfies the following formulae (d), (e), and (f): (d) 0.1≦D50≦1.5 (μm) (e) 0.9≦(D90−D10) / D50≦2.0 (f) Da≦5.0 (μm) wherein D50 is the 50% diameter (μm) accumulated from the small particle side in the volume particle size distribution of the surface-treated calcium carbonate particles measured with a laser diffraction particle size distribution analyzer, D90 is the 90% diameter (μm) accumulated from the small particle side in the volume particle size distribution of the surface-treated calcium carbonate particles measured with the laser diffraction particle size distribution analyzer, and D10 is the 10% diameter (μm) accumulated from the small particle side in the volume particle size distribution of the surface-treated calcium carbonate particles measured with the laser diffraction particle size distribution analyzer. Da is the maximum particle size (μm) in the volume particle size distribution of the surface-treated calcium carbonate particles measured with the laser diffraction particle size distribution measuring device.
[0016] In one embodiment, the fatty acids are at least one compound selected from the group consisting of saturated fatty acids and saturated fatty acid salts.
[0017] In one embodiment, the surface-treated calcium carbonate filler of the present invention is used to constitute a polyolefin-based resin composition.
[0018] The present invention also relates to a resin composition containing a resin and the above-mentioned surface-treated calcium carbonate filler.
[0019] In one embodiment, the resin is a polyolefin resin.
[0020] The present invention also relates to a molded article made from the above resin composition.
[0021] In one embodiment, the molded article of the present invention has the form of a film.
[0022] According to the present invention, the surface-treated calcium carbonate filler of the present invention has good dispersibility in a resin composition and itself has excellent heat resistance. As a result, a resin composition containing the surface-treated calcium carbonate filler of the present invention can suppress, for example, scorching that occurs between the filler and the resin or the remaining surface treatment agent during kneading or extrusion operations, and can prevent or reduce clogging of a strainer attached inside the die of an extruder. Furthermore, the resin composition thus obtained also has excellent heat resistance.
[0023] 1. Surface-Treated Calcium Carbonate Filler The surface-treated calcium carbonate filler of the present invention contains surface-treated calcium carbonate particles, and is preferably composed of the surface-treated calcium carbonate particles as a main component.
[0024] (a) BET specific surface area (Sw) In the present invention, the surface-treated calcium carbonate particles have a predetermined BET specific surface area (Sw; m 2 In the present invention, the Sw of the surface-treated calcium carbonate particles is 3≦Sw≦20(m 2 / g), and preferably 4≦Sw≦16(m 2 / g), and more preferably 5≦Sw≦12(m 2 / g). The surface-treated calcium carbonate particles have a Sw of 3 (m 2 When the Sw of the surface-treated calcium carbonate particles is less than 20 (m / g), the primary particles become too large, which causes a decrease in the strength of the resin composition when the particles are blended into the resin composition. 2 If the amount exceeds 1 / g, it becomes difficult to uniformly disperse the polymer in the resin composition.
[0025] (Method of Measuring Sw) The Sw of the surface-treated calcium carbonate particles can be measured, for example, using a Macsorb HM model-1201 manufactured by Mountech Co., Ltd. as follows.
[0026] Specifically, 0.2 to 0.3 g of the surface-treated calcium carbonate filler to be measured is placed in a measuring device, and a pretreatment is performed by heating the filler at 200°C for 10 minutes in a mixed gas atmosphere of nitrogen and helium. Then, low-temperature, low-humidity physical adsorption is performed in a liquid nitrogen environment, thereby measuring Sw.
[0027] Sw can be controlled by varying various conditions during the production of the surface-treated calcium carbonate particles constituting the filler of the present invention. Conditions that can control Sw within the above range include, for example, the concentration of the milk of lime used in the carbonation reaction, the temperature employed in the carbonation reaction, the concentration of carbon dioxide gas used, the type of additive used in the carbonation reaction, and combinations of these, as described below. If these conditions are not set properly, it may be difficult to obtain surface-treated calcium carbonate particles that satisfy the above Sw range.
[0028] (b) Phosphorus Element Content (Pw) Measured with an Inductively Coupled Plasma (ICP) Atomic Emission Spectrometer In the present invention, the surface-treated calcium carbonate particles have a predetermined phosphorus content (Pw; ppm) measured with an ICP atomic emission spectrometer. In the present invention, the Pw of the surface-treated calcium carbonate particles is 300≦Pw≦5000 (ppm), preferably 400≦Pw≦3500 (ppm), and more preferably 500≦Pw≦2000 (ppm). If Pw is below 300 (ppm), the particles themselves do not have sufficient heat resistance. If Pw exceeds 5000 (ppm), the heat resistance of the particles cannot be further improved, and rather, a large amount of phosphorus will be contained in the wastewater during dehydration performed in the production of such surface-treated calcium carbonate particles, which will impose an excessive load on the wastewater treatment facility.
[0029] (Method of Measuring Pw) Pw can be measured, for example, using an ICP optical emission spectrometer SPS3500 manufactured by SII NanoTechnology Inc. as follows.
[0030] (1) First, 1.0 g of the surface-treated calcium carbonate filler to be measured is placed in a crucible and fired in an electric furnace at 300°C for 3 hours. (2) After firing, approximately 60 mL of distilled water and 7.5 mL of 1.38N nitric acid (Nitric acid (1.38), for measuring toxic metals, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) are placed in a beaker, and the mixture is boiled on an electric stove and slowly cooled. (3) The cooled mixture is added to a 100 mL measuring flask containing 100 μg of yttrium, and the mixture is made up to 100 mL with distilled water. (4) Next, the mixture is filtered through a 5C filter paper, and a sample for ICP measurement is prepared from the resulting filtrate. (5) The phosphorus content (ppm) of the sample is then measured using the ICP atomic emission spectrometer.
[0031] (c) Ca content ratio: In the present invention, the surface-treated calcium carbonate particles satisfy a predetermined Ca content ratio. Here, the term "Ca content ratio" used herein refers to the percentage of the mass (g) of fatty acid constituting the fatty acid calcium relative to the total surface treatment amount (g) of the surface-treated calcium carbonate particles. In the present invention, the Ca content ratio of the surface-treated calcium carbonate particles is 50≦Ca content ratio≦95 (mass%), preferably 55≦Ca content ratio≦85 (mass%), and more preferably 60≦Ca content ratio≦80 (mass%). If the Ca content ratio of the surface-treated calcium carbonate particles is less than 50 mass%, it is impossible to obtain surface-treated calcium carbonate particles with the required heat resistance. This may cause resin burning, in which the surface treatment agent remaining in the resin and / or resin composition and the inorganic filler are scorched during kneading or extrusion. If the Ca content ratio of the surface-treated calcium carbonate particles exceeds 95 mass%, their dispersibility in the resin composition may be reduced. (Method for Measuring the Ca Content Ratio) The Ca content ratio can be measured by a general extraction method. That is, among the surface treatment agents that can be used to obtain surface-treated calcium carbonate particles, fatty acid calcium salts are insoluble in 95% by mass of ethanol solvent, whereas fatty acids and alkali metal salts of fatty acids are soluble in 95% by mass of ethanol solvent. As a result, by utilizing this difference in solubility, the Ca content ratio of the surface-treated calcium carbonate particles can be measured as follows.
[0032] (1) First, 5.0 g of sample surface-treated calcium carbonate particles and 80 g of 95% by mass ethanol are added to a 300 mL Erlenmeyer flask. (2) Next, the Erlenmeyer flask is immersed in a water bath at 90°C or higher and refluxed for 1 hour to extract the surface treatment agent remaining on the surface-treated calcium carbonate particles. (3) After sufficient cooling to 20°C, the contents of the Erlenmeyer flask are suction-filtered using a Teflon (registered trademark) filter with a mesh size of 0.5 μm or less. (4) The resulting filtrate is transferred to a dried and measured 200 mL beaker and evaporated to dryness over a water bath at 90°C or higher to remove the solvent, and the mass of the resulting residue is measured (this mass of the residue corresponds to the total amount of fatty acid and fatty acid alkali metal salt in the surface treatment agent remaining on the surface-treated calcium carbonate particles). (5) The mass obtained in (4) above is the mass of the fatty acid and its alkali metal salt in the surface treatment agent per 5.0 g of surface-treated calcium carbonate particles. By multiplying this value by 1 / 5, the content of the fatty acid and its alkali metal salt in the surface treatment agent per 1.0 g of surface-treated calcium carbonate particles can be calculated as mass % (X). Note that this (X) is a value including alkali metal elements derived from the alkali metal salt of the fatty acid, etc. Therefore, to calculate the mass % of the fatty acid derived from the fatty acid and its alkali metal salt, the content of the alkali metal element (mass %; Y) contained in the surface-treated calcium carbonate particles is subtracted by atomic absorption spectrometry. (6) From these X (mass%) and Y (mass%) and the thermal loss TG (mass%) per 1 g of calcium carbonate from 200°C to 500°C, the percentage of the mass (g) of the fatty acid constituting the fatty acid calcium relative to the total surface treatment amount (g) of the surface-treated calcium carbonate particles (i.e., Ca content) is calculated by the following formula: Ca content (mass%) = {(Tg (mass%) - (X (mass%) - Y (mass%))} / TG (mass%) × 100
[0033] Here, the content (mass %; Y) of the alkali metal element contained in the surface-treated calcium carbonate particles is measured as follows.
[0034] (Method for measuring alkali metals by atomic absorption spectrometry) 1.0 g of surface-treated calcium carbonate particles was weighed into a crucible, placed in a muffle furnace (NMF-120, manufactured by Masuda Rika Kogyo Co., Ltd.), and calcined at 300°C for 2 hours. The mixture was then cooled to room temperature in a desiccator. The sample was then placed in a 200 mL beaker and 60 mL of distilled water was poured into it. Next, 7.5 mL of 1.38 N nitric acid (Nitric acid (1.38), for measuring hazardous metals, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, the beaker was covered with a watch glass, and the mixture was boiled using an electric heater. After cooling to room temperature, the mixture was placed in a 100 mL measuring flask and made up to 100 mL with distilled water to prepare a measurement sample. The alkali metal element content (mass %; Y) of the resulting measurement sample was measured using an atomic absorption spectrophotometer (AA-6700F, manufactured by Shimadzu Corporation).
[0035] The thermal loss TG (mass %) per gram of calcium carbonate at temperatures from 200°C to 500°C used in calculating the Ca content is measured as follows.
[0036] (Method for Measuring TG) Approximately 30 mg of surface-treated calcium carbonate particles are weighed into a platinum sample pan, and the temperature is then raised to 200 to 500°C at a heating rate of 30°C / min, at which point the thermal loss of the particles is measured using, for example, a differential thermal analyzer (DTG-60A manufactured by Shimadzu Corporation). This allows the thermal loss TG (mass%) per 1 g of the surface-treated calcium carbonate to be measured.
[0037] The Ca content can be adjusted by controlling the temperature history in the surface treatment step and the drying step when producing the surface-treated calcium carbonate particles constituting the filler of the present invention. Examples of this temperature history include the temperatures employed in the surface treatment step and the drying step, respectively, and the exposure time at those temperatures. Specific examples of the temperature history include the temperature of the calcium carbonate aqueous slurry used when surface-treating synthetic calcium carbonate obtained by a wet carbonation method or the like with a surface treatment agent (fatty acids and phosphoric acids) and the time required for the surface treatment; the temperature during bonding of the surface treatment agent with calcium carbonate (surface treatment) and the time required for the surface treatment; the temperature and the time required for dehydration after surface treatment; the time and the drying time required for the subsequent drying step; and combinations thereof. For example, if a conduction heat transfer dryer is selected when producing surface-treated calcium carbonate particles, drying will take longer than with an instantaneous dryer such as a spray dryer. However, if the Ca content is insufficient during surface treatment, the Ca content may be increased by adjusting the drying temperature and drying time. If the Ca content ratio is insufficient during the surface treatment and the drying time cannot be maintained sufficiently, it may be difficult to obtain surface-treated calcium carbonate particles that satisfy the above-mentioned Ca content ratio range.
[0038] Furthermore, the surface-treated calcium carbonate particles contained in the surface-treated calcium carbonate filler of the present invention preferably satisfy one or more of the following (d), (e) and (f) in addition to the above (a) to (c), and more preferably satisfy all of (d), (e) and (f):
[0039] (d) 50% Diameter (D50) Accumulated from the Small Particle Side in the Volume Particle Size Distribution In the present invention, the surface-treated calcium carbonate particles preferably have a 50% diameter (D50; μm) accumulated from the small particle side in the volume particle size distribution measured with a laser diffraction particle size distribution analyzer that satisfies a predetermined range. In the present invention, the D50 of the surface-treated calcium carbonate particles is preferably 0.1≦D50≦1.5 (μm), more preferably 0.2≦D50≦1.2 (μm), and even more preferably 0.3≦D50≦0.8 (μm). Surface-treated calcium carbonate particles having a D50 of less than 0.1 (μm) can be technically obtained, but this requires more advanced and precise technology, which may increase production costs. If the D50 exceeds 1.5 μm, clogging of the strainer may occur more easily.
[0040] (Method for Measuring D50) D50 can be measured, along with D10, D90, and Da, described below, using, for example, a laser diffraction particle size distribution analyzer (MT-3300EX II, manufactured by Microtrac-Bell Corporation), as follows. (1) First, 0.3 g of a sample of surface-treated calcium carbonate particles and 50 mL of a medium are added to a 100 mL beaker. (2) Next, the contents in the beaker are dispersed by irradiating them with ultrasonic waves at 300 μA for 60 seconds using, for example, an ultrasonic disperser US-300T, manufactured by Nippon Seiki Seisakusho Co., Ltd. (3) Thereafter, the volume particle size distribution of the surface-treated calcium carbonate particles in the sample is measured using the laser diffraction particle size distribution analyzer (MT-3300EX II, manufactured by Microtrac-Bell Corporation).
[0041] The media that can be used in the above measurement include methanol, ethanol, and a combination thereof.
[0042] The D50 can be controlled by varying various conditions during the production of the surface-treated calcium carbonate particles that constitute the filler of the present invention. Various methods for dispersing calcium carbonate particles have been known, including methods for reducing D50 by finely crushing the particles using mechanical techniques such as a ball mill, a sand grinder mill, an impact mill, a homogenizer, or a Dyno-mill. However, in the wet carbonation synthesis method, it is preferable to use Ostwald ripening, in which calcium carbonate particles are grown to a certain particle size and then dispersed, as a method for controlling the particle size of calcium carbonate particles.
[0043] (e) Sharpness Index of Volume Particle Size Distribution ((D90-D10) / D50) In the present invention, the surface-treated calcium carbonate particles preferably have a sharpness index ((D90-D10) / D50) in the volume particle size distribution measured with a laser diffraction particle size distribution analyzer that satisfies a predetermined range. Here, D50 is as described above, D90 is the 90% diameter (μm) accumulated from the smallest particle side in the volume particle size distribution measured with the laser diffraction particle size distribution analyzer, D10 is the 10% diameter (μm) accumulated from the smallest particle side in the volume particle size distribution measured with the laser diffraction particle size distribution analyzer, and Da is the maximum particle diameter (μm) in the volume particle size distribution measured with the laser diffraction particle size distribution analyzer. In the present invention, the sharpness index ((D90-D10) / D50) of the surface-treated calcium carbonate particles is preferably 0.9≦(D90-D10) / D50≦2.0, and more preferably 1.0≦(D90-D10) / D50≦1.6. Surface-treated calcium carbonate particles having a sharpness index of less than 0.9 are technically obtainable, but require more advanced and precise techniques, which may increase production costs. If the sharpness index of the surface-treated calcium carbonate particles exceeds 2.0, the size of voids formed in a molded product (e.g., a film) obtained by kneading the resulting surface-treated calcium carbonate filler with a resin will vary greatly, making it difficult to obtain a porous film with a uniform in-plane void distribution.
[0044] (Method for measuring sharpness index ((D90-D10) / D50)) D10, D90, and Da constituting the sharpness index can be measured in the same manner as for measuring D50 above, for example, using a laser diffraction particle size distribution measuring device (MT-3300EX II manufactured by Microtrac BEL Co., Ltd.) described above for measuring D50.
[0045] The sharpness index can be controlled by varying various conditions during production of the surface-treated calcium carbonate particles constituting the filler of the present invention. The sharpness index of calcium carbonate particles can be reduced (for example, by reducing the coarse and fine particles to sharpen the particle size distribution) by using the above-mentioned mechanical techniques such as a ball mill, sand grinder mill, impact mill, homogenizer, or Dyno-Mill, or by using elutriation, which separates fine particles from coarse particles by utilizing the difference in sedimentation velocity in water due to particle size. However, Ostwald ripening is preferred because it improves the uniformity of the particle size of calcium carbonate particles, which makes it easier to reduce the sharpness index.
[0046] (f) Maximum Particle Diameter (Da) in Volume Particle Size Distribution In the present invention, the surface-treated calcium carbonate particles preferably have a maximum particle diameter (Da) within a predetermined range in a volume particle size distribution measured with a laser diffraction particle size distribution analyzer. In the present invention, the Da of the surface-treated calcium carbonate particles is preferably Da≦5.0 (μm) (i.e., 0<Da≦5.0 (μm)), and more preferably Da≦4.0 (μm) (i.e., 0<Da≦4.0 (μm)). If Da exceeds 5.0 μm, for example, the resulting surface-treated calcium carbonate filler may be insufficiently dispersed during kneading with a resin, which may easily cause clogging of a strainer.
[0047] (Method for measuring Da) Da can be measured in the same manner as for measuring D50 above, for example, using a laser diffraction particle size distribution analyzer (MT-3300EX II manufactured by Microtrac-Bell Corporation) described above for measuring D50.
[0048] The maximum particle size (Da) in the volumetric particle size distribution can be controlled by varying various conditions during the production of the surface-treated calcium carbonate particles constituting the filler of the present invention. Methods for reducing the maximum particle size (Da) in the volumetric particle size distribution include, in order to remove impurities and coarse particles, classification using gravity, centrifugal force, flotation, etc., such as decantation, and removal using a sieve or filter, while the calcium carbonate is in the form of an aqueous slurry, and also, in order to remove agglomerates formed by drying, classification such as air classification, while the calcium carbonate is in the form of a powder.
[0049] (Surface-treated calcium carbonate particles surface-treated with a surface treatment agent) As described above, the surface-treated calcium carbonate particles contained in the surface-treated calcium carbonate filler of the present invention satisfy all of formulas (a), (b), and (c), and, if necessary, formulas (d), (e), and (f). Such surface-treated calcium carbonate particles have been surface-treated with a surface treatment agent. Note that the term "surface-treated" used in this specification is used to describe the "state" of the surface of the surface-treated calcium carbonate particles, while the term "to be surface-treated / has been surface-treated" used in this specification is used to describe that the surfaces of calcium carbonate particles that have not been subjected to surface treatment (i.e., before surface treatment) have been subjected to a process of modification (surface treatment), and is clearly distinguished from the above-mentioned "surface-treated."
[0050] The surface-treated calcium carbonate particles in the present invention are unmodified (before surface treatment) calcium carbonate particles that have been surface-treated with a surface treatment agent.
[0051] Here, the unmodified calcium carbonate particles are particles of synthetic calcium carbonate (e.g., light / colloidal calcium carbonate) whose particle size can be controlled uniformly, rather than natural products (heavy calcium carbonate) that contain a large amount of fine particles, from the viewpoint of degassing properties when kneaded with a resin. Regarding the crystal morphology, calcium carbonate containing calcite as the main component is preferred from the viewpoint of crystal stability, and colloidal calcium carbonate is particularly preferred because it contains few fine or coarse particles and relatively maintains particle uniformity.
[0052] Furthermore, for the purpose of further increasing the uniformity of the synthetic calcium carbonate particles, the calcium carbonate particles may be obtained by separating a light liquid (fine particle side) and a heavy liquid in an appropriate ratio using a separation device such as a liquid cyclone machine from an aqueous slurry used to obtain the synthetic calcium carbonate particles or an aqueous slurry containing calcium hydroxide prior to the production of the synthetic calcium carbonate particles.
[0053] The surface treatment agent contains fatty acids and phosphoric acids as main components.
[0054] The fatty acids that can be contained in the surface treatment agent have the ability to form fatty acid calcium by substitution reaction on at least a part, preferably the entire surface of the unmodified calcium carbonate particles, thereby modifying the surfaces of the calcium carbonate particles.
[0055] Fatty acids include fatty acids and fatty acid salts, and combinations thereof.
[0056] Fatty acids include, for example, saturated fatty acids, unsaturated fatty acids, and alicyclic carboxylic acids, and combinations thereof.
[0057] Examples of saturated fatty acids include capric acid, lauric acid, myristic acid, palmitic acid, and stearic acid, and combinations thereof. Examples of unsaturated fatty acids include oleic acid, linoleic acid, and linolenic acid, and combinations thereof. Examples of alicyclic carboxylic acids include naphthenic acid, which has a carboxyl group at the end of a cyclopentane or cyclohexane ring.
[0058] The fatty acid salts include alkali metal salts (e.g., sodium salts, potassium salts), alkaline earth metal salts (e.g., calcium salts, magnesium salts), ammonium salts, and amine salts of the above fatty acids, as well as combinations thereof. It is most preferable to use alkali metal salts of fatty acids because they have high solubility in water and are easy to treat the calcium carbonate surface.
[0059] Examples of the fatty acid salts include saturated fatty acid salts such as potassium laurate, potassium myristate, potassium palmitate, sodium palmitate, potassium stearate, and sodium stearate; unsaturated fatty acid salts such as potassium oleate and sodium oleate; and alicyclic carboxylic acid salts such as lead naphthenate and lead cyclohexylbutyrate, as well as combinations thereof.
[0060] The fatty acids may be, for example, modified or unmodified fatty acids derived from animals or plants, such as mixed fatty acids commonly used in the art, such as beef tallow fatty acids, palm oil fatty acids, palm kernel oil fatty acids, and soybean oil fatty acids; alkali metal salts thereof; or so-called hydrogenated mixed fatty acids or alkali metal salts thereof, which are obtained by hydrogenating these mixed fatty acids to reduce the degree of unsaturation.
[0061] When a fatty acid is used as it is as the fatty acid, it is preferred that the fatty acid be dissolved in advance in hot water heated to a temperature equal to or higher than the melting point of the fatty acid to be used, and then a known emulsifier such as an anionic surfactant or a nonionic surfactant is appropriately added thereto, followed by emulsifying the fatty acid in an emulsifying disperser such as a homomixer or a homogenizer, and then adding the emulsified fatty acid to the unmodified calcium carbonate, in order to enable a more uniform surface treatment of unmodified calcium carbonate particles.
[0062] Furthermore, among the above fatty acids, unsaturated fatty acids not only have high solubility in water but also a low melting point, which makes it easier to perform a more uniform surface treatment on the surface of unmodified calcium carbonate particles. However, from the viewpoint of heat resistance, unsaturated fatty acids are characterized by being susceptible to thermal degradation due to the presence of unsaturated double bonds. For this reason, in the present invention, the fatty acids are preferably saturated fatty acids and / or saturated fatty acid salts, since concerns about thermal degradation, such as those of the above unsaturated fatty acids, are eliminated in advance. Alternatively, the total amount of saturated fatty acids and saturated fatty acid salts is preferably 90% by mass or more, more preferably 100% by mass, of the total mass of the fatty acids.
[0063] The proportion of fatty acids present in the surface-treated calcium carbonate filler of the present invention can be easily measured by measuring the filler by gas chromatography, for example, as follows.
[0064] (1) First, 1.0 mg of a sample of surface-treated calcium carbonate particles contained as the surface-treated calcium carbonate filler and 10 μmL of tetramethylammonium hydroxide (10% by mass methanol solution) as an esterifying agent are weighed into a sample cell, and then pyrolyzed at 300° C. for 30 seconds using, for example, a pyrolyzer (Multi-Shot Pyrolyzer MODEL EGA / PY-3030D manufactured by Frontier Labs, Inc.) to vaporize the mixture. (2) The vaporized components can then be analyzed for fatty acid composition using a gas chromatography mass spectrometer (GCMS-QP2010Ultra, manufactured by Shimadzu Corporation) under the following conditions: (Gas chromatography conditions) Vaporization chamber temperature: 250°C, Column used: Rtx-5MS column (length 30 m, membrane pressure 0.25 μm, inner diameter 0.25 mmD), Column conditions: Heating rate 10°C / min, 40 to 300°C, 300°C hold time 10 minutes, Carrier gas: He, Pressure: 80 KPa, Total flow rate: 76.5 mL / min, Column flow rate: 1.5 mL / min, Split ratio: 46. (Mass spectrometry conditions) Ion source temperature: 230°C, Interface temperature: 250°C, Solvent elution time: 1.5 minutes.
[0065] Examples of the phosphoric acids that can be contained in the surface treatment agent include inorganic phosphoric acids, organic phosphoric acids, and combinations thereof.
[0066] Examples of inorganic phosphoric acids include phosphorous acid, phosphinic acid, orthophosphoric acid, pyrophosphoric acid, polyphosphoric acid, and condensed phosphoric acid, salts thereof (e.g., alkali metal salts such as sodium salts and potassium salts; alkaline earth metal salts such as magnesium salts; aluminum salts), and combinations thereof. Examples of organic phosphoric acids include phosphonic acid, phosphoric acid esters, acidic phosphoric acid esters, salts thereof (e.g., alkali metal salts such as sodium salts and potassium salts; alkaline earth metal salts such as magnesium salts; aluminum salts), and combinations thereof.
[0067] In the present invention, the phosphates are preferably compounds having a chelating ability with calcium ions.
[0068] In general, when an appropriate amount of, for example, an alkali metal salt of a fatty acid is dissolved as a surface treatment agent in an aqueous slurry of calcium carbonate particles, a part of the alkali metal salt reacts with calcium ions already eluted from the calcium carbonate particles into the aqueous slurry, and becomes a calcium salt of a fatty acid, which is liberated. This liberated calcium salt of a fatty acid does not contribute to the surface treatment of the calcium carbonate particles, resulting in insufficient surface treatment of the calcium carbonate.
[0069] In contrast, if a compound having chelating ability as a phosphoric acid is added to the aqueous slurry, this compound can preferentially capture calcium ions and prevent the generation of the calcium salt of the liberated fatty acid. As a result, most of the alkali metal salt of the fatty acid contributes to the surface treatment of the calcium carbonate particles, and the heat resistance of the surface-treated calcium carbonate particles obtained with a reduced amount of alkali metal salt of the fatty acid can be expected to be improved. Furthermore, since the calcium carbonate particles can be surface-treated more uniformly, the dispersibility of the surface-treated calcium carbonate particles obtained can be expected to be improved.
[0070] Furthermore, the capture of calcium ions as described above prevents the formation of calcium salts of fatty acids, and therefore the proportion of fatty acids with poor heat resistance or remaining as alkali metal salts of fatty acids increases, i.e., the Ca content decreases. However, by applying a sufficient amount of heat or time during surface treatment or drying to improve the decreased Ca content, the proportion of fatty acid calcium with better heat resistance can be increased.
[0071] Examples of such chelating phosphoric acids include inorganic condensed phosphates such as sodium hexametaphosphate, sodium polyphosphate, sodium pyrophosphate, and sodium ultraphosphate, as well as acidic phosphate esters, and combinations thereof.
[0072] Here, the chelating ability of the phosphoric acid can be expressed using the chelation value (CV) according to the Dow Chem. method. In the present invention, the chelating ability of the phosphoric acid is preferably expressed as the chelation value (CV) of 50 mg CaCO 3 / g ≦ chelate value, more preferably 100 mg CaCO 3 / g≦chelating value≦500 mg CaCO 3 / g. The chelate value of phosphoric acid is 50 mg CaCO 3 If the chelating value of the phosphoric acid is less than 500 mg CaCO 3 , it may be difficult to uniformly treat the surface of unmodified calcium carbonate particles. 3 If the content exceeds 1 / g, a small amount is sufficient to sequester the calcium ions constituting the unmodified calcium carbonate particles, but the content of the phosphorus element contained in the surface-treated calcium carbonate particles related to the Pw becomes insufficient, making it difficult to obtain the desired heat resistance.
[0073] In the present invention, the surface treatment agent may be contained in combination with other surface treatment agents, provided that the effects of the resulting surface-treated calcium carbonate particles are not impaired. Examples of such other surface treatment agents include aromatic sulfonic acids and their salts or esters, resin acids and their salts or esters, and surfactants such as alcohol-based surfactants, sorbitan fatty acid esters, amide-based surfactants, amine-based surfactants, polyoxyalkylene alkyl ethers, polyoxyethylene nonylphenyl ether, sodium alpha-olefin sulfonate, long-chain alkyl amino acids, amine oxides, alkylamines, and quaternary ammonium salts, as well as combinations thereof.
[0074] (Surface Treatment of Unmodified Calcium Carbonate Particles) The surface treatment of unmodified calcium carbonate particles with the above-mentioned surface treatment agent is carried out, for example, as follows.
[0075] To a water slurry containing unmodified calcium carbonate particles, the above-mentioned surface treatment agents, such as fatty acids and phosphoric acids, and optionally other surface treatment agents, are added. This method is generally called a wet treatment, and is preferred in that it can appropriately achieve both the degree of surface treatment of the calcium carbonate particles and production efficiency.
[0076] The amount of fatty acids used can be varied depending on the BET specific surface area of so-called unmodified calcium carbonate particles before surface treatment. For example, the larger the BET specific surface area of the unmodified calcium carbonate particles, the more preferably the amount of fatty acids used. The amount of fatty acids used is preferably 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of unmodified calcium carbonate particles. If the amount of fatty acids used is less than 0.1 part by mass, it may be difficult to disperse the fatty acids more uniformly among the unmodified calcium carbonate particles. If the amount of fatty acids used exceeds 10 parts by mass, bleeding may occur on the surface of a molded article made from a resin composition obtained by kneading the resulting surface-treated calcium carbonate filler with a resin, reducing the strength of the resulting molded article, and it may also be difficult to achieve the Ca content ratio of more than 50% by mass.
[0077] The amount of the phosphoric acid used is not particularly limited because it varies depending on the BET specific surface area and / or amount of the unmodified calcium carbonate particles, the content of the phosphorus element contained in the phosphoric acid itself, the type of resin to be finally kneaded, the kneading conditions, etc., and can be appropriately selected by a person skilled in the art so as to satisfy the above-mentioned range of Pw.
[0078] The order in which unmodified calcium carbonate particles are treated with the fatty acids and phosphoric acids is not particularly limited. For example, unmodified calcium carbonate particles may be first treated with a fatty acid and then with a phosphoric acid. Alternatively, unmodified calcium carbonate particles may be first treated with a phosphoric acid and then with a fatty acid. Alternatively, unmodified calcium carbonate particles may be treated with a fatty acid and a phosphoric acid together, i.e., simultaneously.
[0079] In the present invention, it is preferable to treat unmodified calcium carbonate particles by simultaneously adding a fatty acid and a phosphoric acid, because this can make the surface state of the resulting surface-treated calcium carbonate particles more uniform and can impart excellent dispersibility. Alternatively, it is most preferable to first treat the particles with a phosphoric acid and then with a fatty acid, because this can capture calcium ions in the aqueous slurry, thereby making the surface-treated state of the calcium carbonate particles more uniform and imparting excellent dispersibility.
[0080] When the surface treatment is performed in an aqueous slurry, the surface treatment is preferably performed at a temperature equal to or higher than the melting point of the fatty acids used as the surface treatment agent. If the surface treatment temperature is lower than the melting point of the fatty acids, not only will the surface treatment of the calcium carbonate particles be non-uniform, but the Ca content may also be too low. On the other hand, if the surface treatment temperature is higher than the melting point of the fatty acids, not only will the uniformity of the surface treatment and the Ca content increase, but the surface treatment can also be performed in a short time.
[0081] In one embodiment, the surface treatment temperature is preferably a temperature obtained by adding 0°C to 70°C, more preferably adding 10°C to 60°C, and even more preferably adding 20°C to 50°C to the melting point of the fatty acid used.
[0082] In one embodiment, the surface treatment temperature is preferably 20°C to 98°C, more preferably 40°C to 90°C, and even more preferably 60°C to 80°C.
[0083] After the surface treatment, the resulting particles may be powdered through any operation such as dehydration, drying, or pulverization according to a conventional method.
[0084] In the present invention, even if the surface treatment is insufficient in terms of heat and / or time, the uniformity of the surface treatment of the obtained surface-treated calcium carbonate particles and the Ca content can be improved by using a dryer that can impart a sufficient amount of heat, such as a conduction heat transfer dryer, when drying a dehydrated cake obtained by dehydrating a slurry containing the surface-treated calcium carbonate particles.
[0085] In this manner, a surface-treated calcium carbonate filler can be obtained which contains surface-treated calcium carbonate particles that have been surface-treated with a fatty acid and a phosphoric acid, and satisfies all of formulas (a), (b), and (c), and, if necessary, formulas (d), (e), and (f).
[0086] 2. Resin Composition Next, the resin composition of the present invention will be described.
[0087] The resin composition of the present invention contains a resin and the above-described surface-treated calcium carbonate filler.
[0088] The resin contained in the resin composition is not particularly limited, but examples thereof include polyolefin-based resins, polystyrene-based resins, acrylic-based resins, methacrylic-based resins, vinyl chloride-based resins, vinylidene chloride-based resins, polyamide-based resins, polyether-based resins, vinyl acetate-based resins, and polyvinyl alcohol-based resins, as well as combinations thereof. Specific examples of polyolefin-based resins include polyethylene resins such as low-density polyethylene (LDPE), high-density polyethylene (HDPE), linear low-density polyethylene (L-LDPE), and ultra-high molecular weight polyethylene (UHMWPE), polypropylene resins, ethylene-propylene copolymers, and copolymers of ethylene or propylene with other monomers. The resin may be derived from petroleum, plants (e.g., bioplastics), or a combination thereof. In the present invention, polyolefin-based resins are preferred because they have a relatively low molding temperature compared to engineering plastics and have sufficient heat resistance to withstand temperatures at which the surface-treated calcium carbonate particles can exhibit their heat resistance.
[0089] The content of the surface-treated calcium carbonate filler contained in the resin composition is not necessarily limited, as it varies depending on the type of resin used in combination, the application of the resulting resin composition, and the desired physical properties, but is, for example, 0.05 to 100 parts by mass, preferably 50 to 100 parts by mass, and more preferably 70 to 100 parts by mass per 100 parts by mass of resin. If the content of the surface-treated calcium carbonate filler contained in the resin composition exceeds 100 parts by mass (i.e., exceeds the content of the resin), the kneadability with the resin may decrease and the hue (whiteness) may decrease due to resin deterioration. If the content of the surface-treated calcium carbonate filler contained in the resin composition is less than 0.05 parts by mass, the resulting resin composition may not have sufficient heat resistance.
[0090] The resin composition of the present invention may contain other additives such as lubricants such as fatty acids, fatty acid amides, ethylene bisstearic acid amide, and sorbitan fatty acid esters; plasticizers; stabilizers such as heat stabilizers and light stabilizers; antioxidants; ultraviolet absorbers; neutralizing agents; antifogging agents; antiblocking agents; antistatic agents; slip agents; and colorants; as well as combinations thereof. The content of other additives is not particularly limited, and an appropriate amount can be selected by one skilled in the art as long as it does not inhibit the effects of the surface-treated calcium carbonate filler.
[0091] The resin and the surface-treated calcium carbonate filler, as well as other additives that may be included as needed, may be kneaded under heating using means known in the art (e.g., a single-screw or twin-screw extruder, a kneader, or a Banbury mixer).
[0092] This allows the resin composition of the present invention to be obtained.
[0093] The resin composition may be processed into pellets, for example, as a masterbatch, or may be used in the kneaded state to obtain a molded article as described below.
[0094] 3. Molded Article The molded article of the present invention is made from the above resin composition.
[0095] For example, the resin composition kneaded as described above can be formed into a sheet using a T-die or the like, and then uniaxially or biaxially stretched to obtain a porous film having fine pores on the surface. Alternatively, after the kneading, the resin composition can be formed into a film using a known molding machine such as T-die extrusion or inflation molding, and the film can be treated with acid to dissolve the surface-treated calcium carbonate filler present therein, thereby obtaining a porous film having fine pores on the surface. Furthermore, if necessary, a plurality of T-die extruders in the above process can be stacked, or the film can be laminated after stretching to form a multilayer film. Furthermore, in order to impart printability to the film, the film surface can be subjected to a surface treatment such as plasma discharge and coated with an ink-receiving layer.
[0096] Thus, the molded article of the present invention preferably has the form of a film.
[0097] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, % means % by mass and parts means parts by mass unless otherwise specified.
[0098] The materials, surface-treated calcium carbonate fillers, and pellets described in each of the examples and comparative examples were evaluated as follows.
[0099] (BET specific surface area of unmodified calcium carbonate) 0.2 to 0.3 g of the unmodified calcium carbonate particles used in each example and comparative example was placed in a measuring device (Macsorb HM model-1201 manufactured by Mountec Co., Ltd.), and subjected to a pretreatment of heating at 200°C for 10 minutes in a mixed gas atmosphere of nitrogen and helium, followed by low-temperature, low-humidity physical adsorption in a liquid nitrogen environment to measure the BET specific surface area (m 2 / g) was measured.
[0100] (1) BET Specific Surface Area (Sw) of Surface-Treated Calcium Carbonate Filler 0.2 to 0.3 g of the surface-treated calcium carbonate filler obtained in each Example and Comparative Example was placed in a measuring device (Macsorb HM model-1201 manufactured by Mountech Co., Ltd.), and subjected to a pretreatment of heating at 200°C for 10 minutes in a mixed gas atmosphere of nitrogen and helium, followed by low-temperature, low-humidity physical adsorption in a liquid nitrogen environment, thereby measuring the BET specific surface area (m 2 / g) was measured.
[0101] (2) The phosphorus element content (Pw) of the surface-treated calcium carbonate filler measured with an inductively coupled plasma (ICP) emission spectrometer
[0102] 1.0 g of the surface-treated calcium carbonate filler obtained in each Example and Comparative Example was placed in a crucible and fired in an electric furnace at 300°C for 3 hours. After firing, approximately 60 mL of distilled water and 7.5 mL of 1.38N nitric acid (nitric acid for toxic metal measurement (1.38), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to the beaker containing the mixture, which was then boiled on an electric stove and slowly cooled. The cooled mixture was added to a 100 mL measuring flask containing 100 μg of yttrium, and the resulting mixture was diluted to 100 mL with distilled water. The mixture was then filtered through a 5C filter paper, and a sample for ICP measurement was prepared from the resulting filtrate. The phosphorus content (ppm) of the sample was then measured using an inductively coupled plasma (ICP) optical emission spectrometer (ICP optical emission spectrometer SPS3500, manufactured by SII Nanotechnology Inc.).
[0103] (3) Ca content of surface-treated calcium carbonate filler 5.0 g of the surface-treated calcium carbonate filler obtained in each Example and Comparative Example and 80 g of 95% by volume ethanol were added to a 300 mL Erlenmeyer flask. Next, the Erlenmeyer flask was immersed in a water bath at 90°C or higher and refluxed for 1 hour to extract the surface treatment agent remaining in the surface-treated calcium carbonate particles constituting the filler.
[0104] After sufficient cooling to 20°C, the contents of the Erlenmeyer flask were subjected to suction filtration through a Teflon (registered trademark) filter of 0.5 μm or less to obtain a filtrate. This filtrate was placed in a dried and measured 200 mL beaker and evaporated to dryness in a water bath of 90°C or higher to remove the solvent, obtaining a residue, the mass of which was measured. Here, this mass is the mass of the fatty acid and the alkali metal salt of the fatty acid in the surface treatment agent per 5.00 g of the surface-treated calcium carbonate particles, and by multiplying this value by 1 / 5, the content of the fatty acid and the alkali metal salt of the fatty acid in the surface treatment agent per 1.0 g of the surface-treated calcium carbonate particles was calculated as % by mass (X).
[0105] Note that this content (X) is a value including alkali metals derived from alkali metal salts of fatty acids, etc. Therefore, in order to calculate the mass % of fatty acids and fatty acids derived from alkali metal salts of fatty acids, the content (mass %; Y) of alkali metals contained in the surface-treated calcium carbonate particles was measured by atomic absorption spectrometry as follows.
[0106] 1.0 g of surface-treated calcium carbonate particles was weighed into a crucible, placed in a muffle furnace (NMF-120, manufactured by Masuda Rika Kogyo Co., Ltd.), and fired at 300°C for 2 hours. The mixture was then cooled to room temperature in a desiccator. The sample was then placed in a 200 mL beaker and 60 mL of distilled water was poured into it. Next, 7.5 mL of 1.38 N nitric acid (Nitric acid for hazardous metal measurement (1.38), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, the beaker was covered with a watch glass, and the mixture was boiled using an electric heater. After cooling to room temperature, the mixture was placed in a 100 mL measuring flask and made up to 100 mL with distilled water to prepare a measurement sample. The alkali metal element content (mass%; Y) of the resulting measurement sample was measured using an atomic absorption spectrophotometer (AA-6700F, manufactured by Shimadzu Corporation).
[0107] From the contents X (mass%) and Y (mass%) and the thermal loss TG (mass%) per 1 g of calcium carbonate from 200°C to 500°C, the percentage of the mass (g) of the fatty acid constituting the fatty acid calcium relative to the total surface treatment amount (g) of the surface-treated calcium carbonate particles constituting the surface-treated calcium carbonate filler (i.e., Ca content) was calculated using the following formula: Ca content (mass%) = {(Tg (mass%) - (X (mass%) - Y (mass%))} / TG (mass%) × 100
[0108] The thermal loss TG (mass %) per gram of calcium carbonate at temperatures from 200°C to 500°C, which is used to calculate the Ca content, was measured as follows.
[0109] Approximately 30 mg of the surface-treated calcium carbonate filler obtained in each of the Examples and Comparative Examples was weighed out and placed in a platinum sample pan. The filler was then heated to 200 to 500°C at a heating rate of 30°C / min, and the thermal loss of the surface-treated calcium carbonate particles constituting the filler was measured as the thermal loss TG (mass%) per 1 g of the surface-treated calcium carbonate using a differential thermal analyzer (DTG-60A, manufactured by Shimadzu Corporation).
[0110] (4) D50, Sharpness Index ((D90-D10) / D50), and Da of Surface-Treated Calcium Carbonate Filler 0.3 g of the surface-treated calcium carbonate filler obtained in each Example and Comparative Example and 50 mL of methanol were added to a 100 mL beaker. Next, the contents of the beaker were irradiated with ultrasonic waves at 300 μA for 60 seconds using, for example, an ultrasonic disperser US-300T manufactured by Nippon Seiki Seisakusho Co., Ltd. to disperse the contents and obtain a sample. Thereafter, the volumetric particle size distribution of the surface-treated calcium carbonate particles in the sample was measured using a laser diffraction particle size distribution analyzer (MT-3300EX II manufactured by Microtrac-Bell Corporation). From the obtained volumetric particle size distribution results, the values of D50, D10, D90, and Da, as well as the sharpness index ((D90-D10) / D50) calculated using the results, were obtained.
[0111] (5) Thermal Oxidation Stability of Pellets Test pieces were prepared from the twice-kneaded pellets obtained in each Example and Comparative Example using a compression molding machine SFA-37 manufactured by Shinto Metal Industries Co., Ltd. adjusted to 200°C, using a mold having dimensions of 5 cm x 5 cm x 1 mm thick.
[0112] This test piece was heated in air in a forced draft oven at 140°C in accordance with Japanese Industrial Standard JIS K7368 (Plastics - Polypropylene and propylene copolymers - Measurement of thermal oxidative stability in air - Oven method) to accelerate deterioration, and the number of days required from the start of the test until localized cracking, crumbling and / or discoloration could be visually observed was recorded and evaluated according to the following criteria: ◎: No noticeable change even after 10 days. ○: Discoloration was observed after 10 days. △: Discoloration and cracking were observed after 10 days. ×: Discoloration and cracking were already observed after 5 days.
[0113] (6) Evaluation of Heat Resistance of Pellets The pellets obtained in each Example and Comparative Example were heated in air for 10 days in a forced draft oven at 140°C to accelerate degradation. The melt flow rate (MFR) values (g / 10 min) at 230°C were measured for the obtained heat-degraded pellets and for the initial pellets (not heat-degraded) using a MELT INDEXER F-F01 manufactured by Toyo Seiki Seisaku-sho, Ltd. Furthermore, the rate of change (%) in MFR was calculated from the obtained results according to the following formula:
[0114]
[0115] (7) Evaluation of pellet dispersibility The pellets obtained in each example and comparative example were kneaded and extruded into a twin-screw kneader (2D25W manufactured by Toyo Seiki Co., Ltd.) equipped with three strainers having openings of 100 μm, 60 μm, and 400 μm at 180° C., 150 rpm, and a feed rate of 3 kg / hour. The resin pressure after 60 minutes was measured, and dispersibility was evaluated according to the following criteria. ⊚: The resin pressure after 60 minutes of kneading was less than 3 MPa. ◯: The resin pressure after 60 minutes of kneading was 3 MPa or more and less than 5 MPa. Δ: The resin pressure after 60 minutes of kneading was 5 MPa or more and less than 8 MPa. ×: Vent-up occurred due to clogging of the strainer before 60 minutes of kneading had elapsed.
[0116] (Example 1-1: Preparation of surface-treated calcium carbonate filler (E1)) BET specific surface area: 8.0 m 2An aqueous slurry containing 10% by mass of precipitated calcium carbonate (100 mg / g) was prepared, and the temperature of this slurry was adjusted to 60° C. To this was added sodium hexametaphosphate (manufactured by Taihei Chemical Industry Co., Ltd., sodium metaphosphate; chelate value 125 mg CaCO ) in an amount of 0.60% by mass relative to the calcium carbonate solid content. 3 10% by mass of a phosphate solution containing 2.20% by mass of nonsal SK-1 (saturated fatty acid rate 100% by mass) manufactured by NOF Corporation based on the calcium carbonate solid content was dissolved in hot water at 70°C to give a concentration of 10% by mass, and then this was added as a fatty acid.
[0117] The Nonsal SK-1 manufactured by NOF Corporation used above had the following component composition (potassium myristate 3% by mass, potassium palmitate 27% by mass, potassium stearate 66% by mass, and others 4% by mass).
[0118] Next, for surface treatment, the mixture was stirred overnight at 60°C, dehydrated using a filter press, dried using an instantaneous dryer (an airflow dryer, Dry Meister DMR-1, manufactured by Hosokawa Micron Corporation), and crushed to obtain a surface-treated calcium carbonate filler (E1). The physical properties of the obtained filler (E1) are shown in Tables 1 and 3.
[0119] (Example 1-2: Preparation of Surface-Treated Calcium Carbonate Filler (E2)) Instead of the aqueous solution of phosphoric acids used in Example 1-1, an aqueous solution of sodium ultraphosphate (Ultraporin, manufactured by Taihei Chemical Co., Ltd.; chelate value: 406 mg CaCO 3 ) containing 0.40% by mass of calcium carbonate solids was used. 3 A surface-treated calcium carbonate filler (E2) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which 10% of phosphate-containing calcium carbonate (calcium carbonate / g) was dissolved was used to give a concentration of 10%, and drying was carried out for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E2) are shown in Tables 1 and 3.
[0120] (Example 1-3: Preparation of Surface-Treated Calcium Carbonate Filler (E3)) Instead of the aqueous solution of phosphoric acids used in Example 1, a solution of sodium polyphosphate (sodium tripolyphosphate, manufactured by Taihei Chemical Industry Co., Ltd.; chelating value: 130 mg CaCO 3 ) containing 0.25% by mass based on the calcium carbonate solid content was used. 3 A surface-treated calcium carbonate filler (E3) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which phosphate-containing calcium carbonate (phosphate-containing calcium carbonate / g) was dissolved to a concentration of 10 mass % was used, and drying was carried out for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E3) are shown in Tables 1 and 3.
[0121] (Example 1-4: Preparation of surface-treated calcium carbonate filler (E4)) Instead of the aqueous solution of phosphoric acids used in Example 1-1, potassium pyrophosphate (manufactured by Rasa Kogyo Co., Ltd.: chelating value 50 mg CaCO 3 ) was used in an amount of 0.20 mass % relative to the calcium carbonate solid content. 3 A surface-treated calcium carbonate filler (E4) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which phosphate-containing calcium carbonate (Pb / g) was dissolved to a concentration of 10 mass % was used, and drying was carried out for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E4) are shown in Tables 1 and 3.
[0122] (Example 1-5: Preparation of surface-treated calcium carbonate filler (E5)) Instead of the aqueous solution of phosphoric acids used in Example 1-1, a solution of orthophosphoric acid (manufactured by Rasa Kogyo Co., Ltd., 75% phosphoric acid: chelate value 0 mg CaCO 3 ) containing 1.50 mass % of pure orthophosphoric acid relative to the calcium carbonate solid content was used. 3A surface-treated calcium carbonate filler (E5) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which 1.60% by mass of lauric acid 50 (saturated fatty acid rate 84%) manufactured by Miyoshi Oil & Fats Co., Ltd. was dissolved in hot water at 70°C to a concentration of 10% based on the calcium carbonate solids content, and saponified with an equivalent amount of sodium hydroxide was used instead of the fatty acids used in Example 1-1. The surface treatment was carried out by stirring at 60°C for 4 hours, and the solution was dried for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E5) are shown in Tables 1 and 3.
[0123] The Lauric Acid 50 manufactured by Miyoshi Oil & Fats Co., Ltd. used above had the following component composition (lauric acid 54% by mass, myristic acid 17% by mass, palmitic acid 10% by mass, stearic acid 2% by mass, oleic acid 14% by mass, and others 3% by mass).
[0124] (Example 1-6: Preparation of Surface-Treated Calcium Carbonate Filler (E6)) Instead of the aqueous solution of phosphoric acids used in Example 1-1, a solution of 1.80 mass % of aluminum monophosphate (manufactured by Taihei Chemical Co., Ltd.; chelating value: 0 mg CaCO 3 A surface-treated calcium carbonate filler (E6) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which NAAR-122 (100% saturated fatty acid content, 1.60% by mass relative to the calcium carbonate solids content) was dissolved in water at 70°C to a concentration of 10% was used instead of the fatty acids used in Example 1-1, and the solution was saponified with an equivalent amount of sodium hydroxide and dried for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E6) are shown in Tables 1 and 3.
[0125] (Example 1-7: Preparation of Surface-Treated Calcium Carbonate Filler (E7)) Instead of the aqueous solution of phosphoric acids used in Example 1-1, a solution of 0.30 mass% nitrilotrismethylenephosphonic acid (PH320, manufactured by Cherest Co., Ltd., chelating value 200 mg CaCO 3 ) was used. 3 A surface-treated calcium carbonate filler (E7) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which NAAR-122 lauric acid (100% saturated fatty acid / g) was dissolved to a concentration of 10% by mass was used, and instead of the fatty acids used in Example 1-1, 1.60% by mass, based on the calcium carbonate solids content, of NAAR-122 (saturated fatty acid content 100%) lauric acid manufactured by Nippon Oil & Fats Corporation and 0.03% by mass, based on the calcium carbonate solids content, of an emulsifier (Hitenol NF-08 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) were dissolved in hot water at 70°C to a total concentration of 10% by mass, and the resulting mixture was emulsified at 10,000 rpm for 5 minutes using a T.K. Robomix (Homomixer MARK II manufactured by Tokushu Kika Kogyo Co., Ltd.), and dried for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E7) are shown in Tables 1 and 3.
[0126] (Example 1-8: Preparation of surface-treated calcium carbonate filler (E8)) BET specific surface area 13.0 m 2 A water slurry containing 10% by mass of precipitated calcium carbonate (100 mg / g) was prepared, and the temperature of this slurry was adjusted to 60° C. To this was added 1.00% by mass of sodium hexametaphosphate (sodium metaphosphate, manufactured by Taihei Chemical Industry Co., Ltd.; chelate value: 125 mg CaCO ) based on the calcium carbonate solid content. 3 A surface-treated calcium carbonate filler (E8) was obtained in the same manner as in Example 1-1, except that an aqueous solution of phosphoric acids in which a phosphate buffer solution containing 10% by mass of phosphate buffer solution (1 / g) was dissolved to a concentration of 10% by mass was added, and further, 3.00% of Nonsal SK-1 (saturated fatty acid rate 100%) manufactured by NOF Corporation, based on the calcium carbonate solids content, dissolved in hot water at 70°C to a concentration of 10% was added as a fatty acid. The physical properties of the obtained filler (E8) are shown in Tables 1 and 3.
[0127] (Example 1-9: Preparation of Surface-Treated Calcium Carbonate Filler (E9)) Instead of the aqueous solution of phosphoric acids used in Example 1-8, an aqueous solution of sodium ultraphosphate (Ultraporin, manufactured by Taihei Chemical Co., Ltd.; chelate value: 406 mg CaCO 3 ) containing 1.00% by mass of calcium carbonate solids was used. 3 A surface-treated calcium carbonate filler (E9) was obtained in the same manner as in Example 1-8, except that an aqueous solution of phosphoric acids in which NAAR-122 lauric acid (100% saturated fatty acid content, 2.20% by mass relative to the calcium carbonate solids content) manufactured by NOF Corporation was dissolved in hot water at 70°C to a concentration of 10% and saponified with an equivalent amount of sodium hydroxide was used instead of the fatty acids used in Example 1-8, and the resultant mixture was stirred at 60°C for 4 hours for surface treatment, followed by dehydration using a filter press, and then dried for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer. The physical properties of the obtained filler (E9) are shown in Tables 1 and 3.
[0128] (Example 1-10: Preparation of surface-treated calcium carbonate filler (E10)) BET specific surface area: 16.8 m 2 An aqueous slurry containing 10% by mass of precipitated calcium carbonate (1.20% by mass, based on the calcium carbonate solid content) was prepared, and the temperature of this slurry was adjusted to 60° C. To this was added sodium ultraphosphate (Ultraporin, manufactured by Taihei Chemical Co., Ltd.; chelate value: 406 mg CaCO ) in an amount of 1.20% by mass based on the calcium carbonate solid content. 3 A surface-treated calcium carbonate filler (E10) was obtained in the same manner as in Example 1-8, except that an aqueous solution of phosphoric acids in which a phosphate-containing phosphate salt (a phosphate salt of 1.5g / g) had been dissolved to a concentration of 10% was added, and further, 4.00 mass% of Nonsal SK-1 (saturated fatty acid rate 100%) manufactured by NOF Corporation, based on the calcium carbonate solids, dissolved in hot water at 70°C to a concentration of 10% was added as a fatty acid salt. The physical properties of the obtained filler (E10) are shown in Tables 1 and 3.
[0129] (Example 1-11: Preparation of Surface-Treated Calcium Carbonate Filler (E11)) Instead of the aqueous solution of phosphoric acids used in Example 1-10, sodium hexametaphosphate (manufactured by Taihei Chemical Industry Co., Ltd., sodium metaphosphate: chelate value 125 mg CaCO 3 ) was used in an amount of 1.20 mass % relative to the calcium carbonate solid content. 3 A surface-treated calcium carbonate filler (E11) was obtained in the same manner as in Example 1-10, except that the surface treatment was carried out using an aqueous solution of phosphoric acids in which 10% phosphate-containing calcium carbonate (calcium carbonate / g) was dissolved to a concentration of 10%, followed by stirring at 80°C for 6 hours and dehydrating using a filter press, and that the surface treatment was carried out using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer at a steam pressure of 0.25 MPa for 2 hours. The physical properties of the obtained filler (E11) are shown in Tables 1 and 3.
[0130] Example 1-12: Preparation of surface-treated calcium carbonate filler (E12) A surface-treated calcium carbonate filler (E12) was obtained in the same manner as in Example 1-11, except that instead of the aqueous solution of phosphoric acids used in Example 1-11, a mixed fatty acid salt B (saturated fatty acid rate 92%) prepared to the following composition was used as the fatty acid salt, in an amount of 4.00 mass% relative to the calcium carbonate solids content, dissolved in hot water at 70°C to a concentration of 10%, and an instantaneous dryer (an airflow dryer, Dry Meister DMR-1, manufactured by Hosokawa Micron Corporation) was used. The physical properties of the obtained filler (E12) are shown in Tables 2 and 4.
[0131] The mixed fatty acid salt B used above had the following component composition (sodium laurate 10% by mass, sodium myristate 2% by mass, sodium palmitate 20% by mass, potassium stearate 60% by mass, and sodium oleate 8% by mass).
[0132] Comparative Example 1-1: Preparation of Surface-Treated Calcium Carbonate Filler (C1) A surface-treated calcium carbonate filler (C1) was obtained in the same manner as in Example 1-12, except that the surface treatment was carried out by stirring at 80°C for 30 minutes. The physical properties of the obtained filler (C1) are shown in Tables 2 and 4.
[0133] Comparative Example 1-2: Preparation of Surface-Treated Calcium Carbonate Filler (C2) A surface-treated calcium carbonate filler (C2) was obtained in the same manner as in Example 1-12, except that the surface treatment was carried out by stirring at 60° C. for 4 hours. The physical properties of the obtained filler (C2) are shown in Tables 2 and 4.
[0134] (Comparative Example 1-3: Preparation of Surface-Treated Calcium Carbonate Filler (C3)) Instead of the aqueous solution of phosphoric acids used in Example 1-11, sodium hexametaphosphate (sodium metaphosphate, manufactured by Taihei Chemical Industry Co., Ltd., chelating value 125 mg CaCO 3 ) was used in an amount of 3.60 mass % based on the calcium carbonate solid content. 3 A surface-treated calcium carbonate filler (C3) was obtained in the same manner as in Example 1-11, except that an aqueous solution of a phosphoric acid in which 1,2,3-trimethylsilyl phosphate (Pt / g) was dissolved to a concentration of 10 mass % was used. The physical properties of the obtained filler (C3) are shown in Tables 2 and 4.
[0135] Comparative Example 1-4: Preparation of surface-treated calcium carbonate filler (C4) A surface-treated calcium carbonate filler (C4) was obtained in the same manner as in Example 1-11, except that the aqueous solution of a phosphoric acid was not added. The physical properties of the obtained filler (C4) are shown in Tables 2 and 4.
[0136] Comparative Example 1-5: Preparation of Surface-Treated Calcium Carbonate Filler (C5) Instead of the aqueous solution of phosphoric acids used in Example 1-11, a solution of 0.30 mass% nitrilotrismethylenephosphonic acid (PH320, manufactured by Cherest Co., Ltd., chelating value 200 mg CaCO 3 ) was used. 3A surface-treated calcium carbonate filler (C5) was obtained in the same manner as in Example 1-11, except that an aqueous solution of phosphoric acids in which 2.00% by mass of Sakura stearate (saturated fatty acid content 100%) manufactured by NOF Corporation and 0.03% by mass of an emulsifier (Hitenol NF-08 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) based on the calcium carbonate solids content was dissolved in 80°C hot water to a total concentration of 10% by mass, and the resulting mixture was emulsified at 10,000 rpm for 5 minutes using a T.K. Robomix (Homomixer MARK II manufactured by Tokushu Kika Kogyo Co., Ltd.), and stirred overnight at 90°C for the surface treatment. The physical properties of the obtained filler (C5) are shown in Tables 2 and 4.
[0137] The Sakura Stearic Acid manufactured by NOF Corporation used above had the following component composition (2% by mass of myristic acid, 31% by mass of palmitic acid, 66% by mass of stearic acid, and 1% by mass of others).
[0138] (Example 1-13: Preparation of surface-treated calcium carbonate filler (E13)) BET specific surface area: 20.5 m 2 An aqueous slurry containing 10% by mass of precipitated calcium carbonate (100 mg / g) was prepared, and the temperature of this slurry was adjusted to 60° C. To this was added 3.00% by mass of sodium hexametaphosphate (sodium metaphosphate, manufactured by Taihei Chemical Industry Co., Ltd.; chelate value: 125 mg CaCO ) based on the calcium carbonate solid content. 3 An aqueous solution of phosphoric acids in which 10% by mass of 10% saturates (1 / g) of calcium carbonate was dissolved was added, and further, 5.00% by mass of NONSAL SK-1 (saturated fatty acid rate 100%) manufactured by NOF Corporation was dissolved in hot water at 70°C to a concentration of 10% based on the calcium carbonate solids content as a fatty acid salt. Next, the mixture was stirred overnight at 60°C for surface treatment, dehydrated using a filter press, dried for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer, and crushed to obtain a surface-treated calcium carbonate filler (E13). The physical properties of the obtained filler (E13) are shown in Tables 2 and 4.
[0139] (Comparative Example 1-6: Preparation of Surface-Treated Calcium Carbonate Filler (C6)) BET Specific Surface Area 2.0 m 2 / g of heavy calcium carbonate (Super #2000 manufactured by Maruo Calcium Co., Ltd.) was stirred in a Henschel mixer while adding 0.20 mass% of sodium hexametaphosphate (sodium metaphosphate manufactured by Taihei Chemical Industry Co., Ltd.; chelate value 125 mg CaCO ) based on the calcium carbonate solid content. 3 An aqueous solution of phosphoric acid in which a phosphate buffer solution containing 10% phosphate (1 / g) was dissolved to a concentration of 10% was added, and further, 1.00 mass% of Sakura stearate (saturated fatty acid rate 100%) manufactured by NOF Corporation was added as a fatty acid based on the calcium carbonate solids content. Next, for surface treatment, the mixture was stirred at 110°C for 30 minutes to evaporate the water, thereby obtaining a surface-treated calcium carbonate filler (C6). The physical properties of the obtained filler (C6) are shown in Tables 2 and 4.
[0140] (Comparative Example 1-7: Preparation of Surface-Treated Calcium Carbonate Filler (C7)) BET Specific Surface Area: 28.0 m 2 A water slurry containing 10% by mass of precipitated calcium carbonate (100 mg / g) was prepared, and the temperature of this slurry was adjusted to 60° C. To this was added sodium hexametaphosphate (sodium metaphosphate, manufactured by Taihei Chemical Industry Co., Ltd., chelate value 125 mg CaCO ) in an amount of 1.20% by mass relative to the calcium carbonate solid content. 3 An aqueous solution of phosphoric acid in which 10% of a phosphate-containing phosphate-containing phosphate (1 / g) was dissolved to a concentration of 10% was added, and further, 7.00% by mass of NONSAL SK-1 (saturated fatty acid rate 100%) manufactured by NOF Corporation (based on the calcium carbonate solids content) was dissolved in hot water at 70°C to a concentration of 10% was added as a fatty acid salt. For surface treatment, the mixture was stirred overnight at 60°C, dehydrated using a filter press, dried for 2 hours at a steam pressure of 0.25 MPa using a CD dryer manufactured by Kurimoto, Ltd. as a conduction heat transfer dryer, and crushed to obtain a surface-treated calcium carbonate filler (C7). The physical properties of the obtained filler (C7) are shown in Tables 2 and 4.
[0141]
[0142]
[0143]
[0144]
[0145] (Examples 2-1 to 2-13 and Comparative Examples 2-1 to 2-7: Preparation of twice-kneaded pellets (NE1) to (NE13) and (NC1) to (NC7)) 30 parts by mass of the surface-treated calcium carbonate filler prepared in each of Examples 1-1 to 1-13 and Comparative Examples 1-1 to 1-7 and 70 parts by mass of a polypropylene resin (Novatec PP FB3B, MFR 7.5, manufactured by Japan Polypropylene Corporation) were mixed to obtain a resin mixture (10 kg) which was charged into a twin-screw kneader (2D25W manufactured by Toyo Seiki Co., Ltd.) equipped with a strainer having an opening of 100 μm. The mixture was kneaded and extruded at 180° C., 150 rpm, and a feed rate of 3 kg / hour, and then cut with a pelletizer to prepare crude pellets. These crude pellets were then dried at 60°C for 24 hours, and then kneaded and dried under the same conditions to obtain twice-kneaded pellets (NE1) to (NE13) and (NC1) to (NC7), respectively.
[0146] The evaluation results of the twice-kneaded pellets (NE1) to (NE13) and (NC1) to (NC7) are shown in Tables 5 and 6.
[0147]
[0148]
[0149] As shown in Tables 5 and 6, the twice-kneaded pellets (NE1) to (NE13) produced in Examples 2-1 to 2-13 had the same or better thermal oxidation stability as the twice-kneaded pellets (NC1) to (NC7) of Comparative Examples 2-1 to 2-7, and were able to keep the rate of change in the heat resistance test relatively low. Furthermore, the results of the dispersibility evaluation for the pellets (NE1) to (NE13) of Examples 2-1 to 2-13 were the same as or better than the pellets (NC1) to (NC7) of Comparative Examples 2-1 to 2-7.
[0150] This shows that the surface-treated calcium carbonate fillers (E1) to (E13) produced in Examples 1-1 to 1-13 used in the twice-kneaded pellets (NE1) to (NE13) produced in Examples 2-1 to 2-13 were all more stable and heat-resistant than the surface-treated calcium carbonate fillers (C1) to (C7) of Comparative Examples 2-1 to 2-7 used in the twice-kneaded pellets (NC1) to (NC7) of Comparative Examples 2-1 to 2-7, and had the property of being sufficiently and uniformly dispersed in the resin.
[0151] The present invention is useful in, for example, the fields of resin molding, construction and housing, paint, and a wide range of related technical fields.
Claims
1. A surface-treated calcium carbonate filler comprising calcium carbonate particles that have been surface-treated with a fatty acid and a phosphoric acid, and satisfying the following formulas (a), (b) and (c): (a) 3≦Sw≦20(m 2 / g), (b) 300≦Pw≦5000 (ppm), (c) 50≦Ca content≦95 (mass%), where Sw is the BET specific surface area (m 2 / g), Pw is the content (ppm) of phosphorus element in the surface-treated calcium carbonate particles measured by an inductively coupled plasma (ICP) optical emission spectrometer, and the Ca content is the percentage of the mass (g) of fatty acid constituting fatty acid calcium relative to the total surface treatment amount (g) of the surface-treated calcium carbonate particles.
2. The surface-treated calcium carbonate filler according to claim 1, further satisfying the following formulae (d), (e) and (f): (d) 0.1≦D50≦1.5 (μm); (e) 0.9≦(D90-D10) / D50≦2.0; (f) Da≦5.0 (μm); D50 is the 50% diameter (μm) accumulated from the small particle side in the volumetric particle size distribution of the surface-treated calcium carbonate particles measured with a laser diffraction particle size distribution measuring device; D90 is the 90% diameter (μm) accumulated from the small particle side in the volumetric particle size distribution of the surface-treated calcium carbonate particles measured with the laser diffraction particle size distribution measuring device; D10 is the 10% diameter (μm) accumulated from the small particle side in the volumetric particle size distribution of the surface-treated calcium carbonate particles measured with the laser diffraction particle size distribution measuring device; Da is the maximum particle size (μm) in the volume particle size distribution of the surface-treated calcium carbonate particles measured with the laser diffraction particle size distribution measuring device.
3. The surface-treated calcium carbonate filler according to claim 1, wherein the fatty acid is at least one compound selected from the group consisting of saturated fatty acids and salts of saturated fatty acids.
4. The surface-treated calcium carbonate filler according to claim 1, which is used to constitute a polyolefin-based resin composition.
5. A resin composition comprising a resin and the surface-treated calcium carbonate filler according to any one of claims 1 to 3.
6. The resin composition according to claim 5, wherein the resin is a polyolefin resin.
7. A molded article made from the resin composition according to claim 5.
8. The molded article according to claim 7, which has the form of a film.
Citation Information
Patent Citations
Surface-treated inorganic filler and resin composition containing the same compounded therewith
JP2002363443A
Filler for porous film and porous film containing it
JP2006169421A
Filler for light reflection porous film and light reflection porous film incorporated with the filler
JP2006265472A
Calcium carbonate based filler for resin, covered with amorphous calcium phosphate and resin composition obtained by blending the filler
JP2011011924A
Resin composition
JP2013006891A