Adhesive composition and adhesive sheet, laminated body, and printed wiring board containing adhesive composition
The adhesive composition, featuring an acid-modified resin and a polyolefin compound with specific properties, addresses the challenges of dielectric and heat resistance in FPCs, offering enhanced solder heat resistance and circuit embedding for high-frequency applications.
Patent Information
- Application Number
- PCT/JP2023/042510
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2023-11-28
- Publication Date
- 2024-12-05
AI Technical Summary
Existing adhesives for flexible printed wiring boards (FPCs) face challenges in achieving low dielectric properties, particularly high frequency signals, and insufficient circuit embedding due to high viscosity and insulation failure, with existing materials like epoxy resin and polyolefin blends not meeting requirements for dielectric loss tangent and heat resistance.
An adhesive composition comprising an acid-modified resin, a polyolefin compound (A) with specific molecular weight, melting point, and density, and a polyfunctional epoxy resin (B), optimized to provide excellent solder heat resistance, adhesive strength, and dielectric properties, ensuring effective circuit embedding and insulation.
The adhesive composition exhibits excellent solder heat resistance, adhesive strength, and dielectric properties, making it suitable for high-frequency applications, with improved circuit embedding and insulation, addressing the limitations of previous adhesives.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Adhesive composition, and adhesive sheet, laminate and printed wiring board containing the same
[0001] The present invention relates to an adhesive composition. More specifically, the present invention relates to an adhesive composition used for bonding a resin substrate to a resin substrate or a metal substrate. In particular, the present invention relates to an adhesive composition for flexible printed wiring boards (hereinafter abbreviated as FPC), and an adhesive sheet, a laminate, and a printed wiring board each containing the same.
[0002] FPCs have excellent flexibility, allowing them to accommodate the increasing functionality and miniaturization of personal computers (PCs) and smartphones. They are widely used to incorporate electronic circuit boards into narrow, complex interior spaces. In recent years, electronic devices have become smaller, lighter, more dense, and more powerful, resulting in increasingly demanding performance requirements for wiring boards (electronic circuit boards). In particular, high-frequency signals are increasingly being used to increase transmission speeds. Accordingly, there is a growing demand for FPCs with low dielectric properties (low dielectric constant, low dielectric dissipation factor) in the high-frequency range. To achieve such low dielectric properties, measures have been taken to reduce the dielectric loss of FPC substrates and adhesives. For FPC substrates, in addition to conventional polyimide (PI) and polyethylene terephthalate (PET), substrate films with low dielectric properties, such as liquid crystal polymers (LCPs) and fluororesins, have been proposed. Development of adhesives, such as combinations of polyolefins and epoxies (Patent Document 1 and Patent Document 3), and adhesives using polyphenylene ether (Patent Document 2), has been promoted.
[0003] In recent years, electronic circuits on FPCs have become increasingly miniaturized. While narrowing the circuit width to around 25 μm has made it possible to form high-density circuits, some adhesives are unable to completely fill the gaps between such fine circuits, resulting in poor insulation.
[0004] International Publication No. 2016 / 047289 International Publication No. 2020 / 196718 Patent No. 7192848
[0005] However, the adhesive described in Patent Document 1 contains an epoxy resin and an epoxy resin curing agent, and therefore has high polarity, and cannot satisfy high requirements, particularly for dielectric loss tangent. The adhesive described in Patent Document 2 cannot be said to have excellent heat resistance as an FPC adhesive, and its dielectric properties are also insufficient. The adhesive described in Patent Document 3 improves its dielectric properties by adding an unmodified polyolefin to a blend of acid-modified polyolefin and epoxy resin, but the unmodified polyolefin added has a large molecular weight and a high melt viscosity, resulting in insufficient circuit embeddability and the risk of insulation failure.
[0006] The present invention has been made in view of the above-mentioned problems in the prior art. That is, an object of the present invention is to provide an adhesive composition that has excellent solder heat resistance and adhesive strength, good circuit embeddability, and excellent dielectric properties such as low relative permittivity and dielectric loss tangent, as well as an adhesive sheet, laminate, and printed wiring board that contain the same.
[0007] As a result of extensive research, the present inventors have found that the above problems can be solved by the following means, and have arrived at the present invention. That is, the present invention has the following configuration.
[0008] [1] An adhesive composition comprising an acid-modified resin, a compound (A), and an epoxy resin (B), wherein the content of the compound (A) is 10 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the acid-modified resin. Compound (A): The adhesive composition has no heteroatom, a weight-average molecular weight of 10,000 or more and 70,000 or less, a melting point of 60°C or more and 120°C or less, and a density of 0.88 g / cm 3[2] The adhesive composition according to [1], wherein the acid-modified resin is an acid-modified polyolefin. [3] The adhesive composition according to [1] or [2], wherein the epoxy resin (B) is a polyfunctional epoxy resin. [4] The adhesive composition according to any one of [1] to [3], wherein the compound (A) has a melt viscosity at 170°C of 10,000 mPa s or less. [5] An adhesive sheet comprising the adhesive composition according to any one of [1] to [4]. [6] A laminate comprising the adhesive composition according to any one of [1] to [4]. [7] A printed wiring board comprising the laminate according to [6] as a component.
[0009] The adhesive composition of the present invention has excellent solder heat resistance and adhesive strength, as well as good circuit embedding properties and excellent dielectric properties, making it suitable for use in FPC adhesives, adhesive sheets, laminates, and printed wiring boards in the high frequency range.
[0010] An embodiment of the present invention will be described in detail below, however, the present invention is not limited to this embodiment and can be practiced in various modified forms within the scope of the above description.
[0011] <Adhesive Composition> The adhesive composition of the present invention is an adhesive composition containing an acid-modified resin, a compound (A), and an epoxy resin (B), characterized in that the content of the compound (A) is 10 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the acid-modified resin. Compound (A): does not contain a heteroatom, has a weight-average molecular weight of 10,000 or more and 70,000 or less, a melting point of 60°C or more and 120°C or less, and a density of 0.88 g / cm 3 In the present invention, an adhesive composition that exhibits excellent soldering heat resistance and adhesive strength, good circuit embeddability, and excellent dielectric properties is provided by blending a compound (A) having specific properties with an adhesive composition that contains an acid-modified resin and an epoxy resin (B) and further optimizing the blending amount of compound (A).
[0012] <Compound (A)> The compound (A) in the present invention does not contain a heteroatom, has a weight average molecular weight of 10,000 or more and 70,000 or less, a melting point of 60°C or more and 120°C or less, and a density of 0.88 g / cm 3 The polyolefin resin has a melting point, density, and weight-average molecular weight within the above ranges, making it possible to obtain an adhesive with excellent dielectric properties by not containing heteroatoms, and excellent solvent solubility by having a melting point, density, and weight-average molecular weight within the above ranges. Furthermore, by containing compound (A) whose melting point, density, and weight-average molecular weight satisfy the above conditions, the adhesive composition flows due to the heat generated during adhesion, making it possible to fill the gaps between circuits with the adhesive without voids. In particular, in recent years, electronic circuits have become narrower and denser, and an adhesive composition that exhibits good circuit embeddability, such as that of the present invention, is extremely useful from the perspective of improving the insulation of printed circuit boards.
[0013] The weight average molecular weight (Mw) of the compound (A) is preferably 11,000 or more and 52,000 or less, more preferably 12,000 or more and 47,000 or less, even more preferably 13,000 or more and 42,000 or less, even more preferably 14,000 or more and 35,000 or less, particularly preferably 14,100 or more and 33,000 or less, and particularly preferably 15,000 or more and 29,000 or less. By setting it below the upper limit, the flowability is improved and excellent circuit embedding properties can be achieved. Furthermore, by setting it above the lower limit, excellent solder heat resistance can be achieved.
[0014] The melting point of compound (A) is preferably 70°C or higher and 110°C or lower, more preferably 75°C or higher and 105°C or lower, and even more preferably 80°C or higher and 100°C or lower. By making the melting point of compound (A) equal to or higher than the lower limit, an adhesive composition with excellent workability is obtained. On the other hand, if the melting point exceeds the upper limit, compound (A) may not dissolve in the adhesive composition. Therefore, by making the melting point equal to or lower than the upper limit, the solubility of compound (A) can be improved. Furthermore, by making the melting point equal to or lower than the upper limit, the reaction with epoxy resin (B) becomes good in the reaction after embedding the circuit, which is advantageous for improving crosslink density (improving heat resistance).
[0015] The phrase "compound (A) does not contain heteroatoms (e.g., nitrogen atoms, oxygen atoms, sulfur atoms, chlorine atoms, etc.)" means that compound (A) does not contain atoms other than carbon atoms and hydrogen atoms in its molecular structure (i.e., compound (A) is a polyolefin resin consisting of carbon atoms and hydrogen atoms). Compound (A) particularly refers to an unmodified polyolefin resin, and more specifically refers to a polyolefin resin that has not been modified with an acid.
[0016] The density of the compound (A) is preferably 0.875 g / cm 3 or less, more preferably 0.873 g / cm 3 If the density of the compound (A) is too high, the crystallinity of the compound (A) may increase and the solubility may deteriorate, so the lower the density of the compound (A), the better. The lower limit is not particularly limited, but is generally 0.850 g / cm 3 That's all.
[0017] The melt viscosity of compound (A) at 170°C is, for example, 10,000 mPa s or less, preferably 7,000 mPa s or less, more preferably 5,000 mPa s or less, and even more preferably 3,000 mPa s or less. In consideration of the effect of compound (A) on circuit embeddability, the lower the melt viscosity at 170°C, the better. There is no particular lower limit, but it is generally 10 mPa s or more.
[0018] The content of compound (A) in the adhesive composition of the present invention is preferably 15 to 37 parts by mass, more preferably 25 to 35 parts by mass, per 100 parts by mass of the acid-modified resin (particularly the solid content of the acid-modified resin). If the content exceeds the upper limit, the amount of acid-modified resin decreases relatively, resulting in a decrease in crosslink density, which may result in a deterioration in solder heat resistance. On the other hand, if the content is below the lower limit, the effect of compound (A) is not fully exerted, which may result in a deterioration in circuit embeddability. Furthermore, as the content of compound (A) increases, the dielectric loss tangent tends to improve. In other words, by keeping the content within the above upper and lower limits, excellent dielectric properties, solder heat resistance, and circuit embeddability can be achieved.
[0019] In the present invention, the melting point, density, melt viscosity, and weight average molecular weight were determined by the following methods.
[0020] (Weight-Average Molecular Weight (Mw)) The weight-average molecular weight in the present invention is a value measured by gel permeation chromatography (hereinafter referred to as GPC, standard substance: polystyrene resin, mobile phase: tetrahydrofuran, column: Shodex KF-802 + KF-804L + KF-806L, column temperature: 30°C, flow rate: 1.0 ml / min, detector: RI detector) manufactured by Shimadzu Corporation.
[0021] (Measurement of Melting Point) The melting point in the present invention is a value measured using a differential scanning calorimeter (hereinafter referred to as DSC, manufactured by TA Instruments Japan, Q-2000) from the top temperature of the melting peak when the material is heated and melted at a rate of 20°C / min, cooled to form a resin, and then heated and melted again.
[0022] (Density) The density is a value measured at 23° C. in accordance with ISO 1183.
[0023] (Melt Viscosity) The melt viscosity is a value measured in accordance with DIN 53019 using a rotational viscometer at 170°C.
[0024] Polyolefin resin refers to polymers primarily composed of a hydrocarbon skeleton, such as homopolymers of olefin monomers exemplified by ethylene, propylene, butene, butadiene, isoprene, etc., or copolymers with other monomers, and hydrogenated or halogenated products of the resulting polymers, and includes cycloolefin polymers as well as propylene-α-olefin copolymers. Preferred polyolefin resins are polypropylene-based resins such as propylene homopolymers and propylene-α-olefin copolymers.
[0025] Propylene-α-olefin copolymers are produced by copolymerizing propylene as the main component with an α-olefin. Examples of α-olefins that can be used include one or more of ethylene, 1-butene, 1-heptene, 1-octene, 4-methyl-1-pentene, and vinyl acetate. Among these α-olefins, ethylene and 1-butene are preferred. The ratio of the propylene component to the α-olefin component in the propylene-α-olefin copolymer is not limited, but the propylene component is preferably 50 mol% or more, and more preferably 70 mol% or more. Furthermore, these raw materials are not limited to petroleum-derived raw materials; raw materials obtained using chemical recycling technology that utilizes biomass naphtha or waste plastics may also be used.
[0026] The cycloolefin polymer may be either a homopolymer (COP) made from only one cycloolefin monomer, or a copolymer (COC) composed of one or more cycloolefin monomers and comonomers.
[0027] Examples of the cycloolefin monomer include bicyclic compounds such as norbornene and norbornadiene, tricyclic compounds such as dicyclopentadiene and dihydroxypentadiene, tetracyclic compounds such as tetracyclododecene, pentacyclic compounds such as cyclopentadiene trimer, heptacyclic compounds such as tetracyclopentadiene, and alkyl (methyl, ethyl, propyl, butyl, etc.) substituted compounds, alkenyl (vinyl, etc.) substituted compounds, alkylidene (ethylidene, etc.) substituted compounds, aryl (phenyl, tolyl, naphthyl, etc.) substituted compounds of these polycyclic compounds. Among these, norbornene-based monomers selected from the group consisting of norbornene, tetracyclododecene, and alkyl-substituted compounds thereof are particularly preferred.
[0028] The comonomer may be any monomer copolymerizable with the cycloolefin monomer, and is preferably, for example, an alkene monomer. Examples of the alkene monomer include α-olefins such as ethylene, propylene, 1-butene, and 1-hexene, and isobutene. The alkene monomer may be linear or branched.
[0029] The monomer components constituting the cycloolefin polymer preferably contain 50 mass% or more of the cycloolefin-based monomer, more preferably 60 mass% or more of the cycloolefin-based monomer. When the cycloolefin monomer accounts for 50 mass% or more of the total monomer components, the solder heat resistance is good. There are no particular restrictions on the polymerization method and polymerization conditions when polymerizing the monomer components, and they may be appropriately set according to conventional methods.
[0030] <Acid-Modified Resin> The acid-modified resin used in the present invention is a resin modified with an acid component. By using the acid-modified resin, an adhesive layer having excellent adhesion to a metal substrate such as copper foil and excellent solder heat resistance can be formed by a crosslinking reaction with the epoxy group of the epoxy resin (B) described below.
[0031] The acid-modified resin used in the present invention can be prepared, for example, by modifying a base resin with an unsaturated carboxylic acid component, or by copolymerizing an unsaturated carboxylic acid component during polymerization of the base resin. The unsaturated carboxylic acid component is not particularly limited, and is preferably at least one of an α,β-unsaturated carboxylic acid and an acid anhydride thereof, and specific examples thereof include acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, citraconic acid, maleic anhydride, itaconic anhydride, fumaric anhydride, and citraconic anhydride. Among these, maleic acid, itaconic acid, citraconic acid, and anhydrides thereof are preferred, acid anhydrides are more preferred, and maleic anhydride is even more preferred.
[0032] The acid value of the acid-modified resin used in the present invention has a lower limit of 10 equivalents / 10 from the viewpoint of heat resistance and adhesion to resin substrates and metal substrates. 6 g or more, and more preferably 20 equivalents / 10 6 g or more, and more preferably 30 equivalents / 10 6 When the molecular weight is equal to or greater than the above value, the compatibility with the epoxy resin (B) or the like is improved, the adhesive strength is improved, and the crosslinking density is increased, so that the heat resistance can also be improved. The upper limit is 1000 equivalents / 10 6g or less, and more preferably 700 equivalents / 10 6 g or less, and more preferably 500 equivalents / 10 6 When the thickness is equal to or less than the above value, the adhesiveness and low dielectric properties are improved.
[0033] The weight-average molecular weight (Mw) of the acid-modified resin used in the present invention is preferably in the range of 10,000 to 1,000,000. It is more preferably in the range of 20,000 to 500,000, even more preferably in the range of 40,000 to 200,000, and particularly preferably in the range of 50,000 to 150,000. By ensuring that the Mw is equal to or greater than the lower limit, the cohesive strength is improved and excellent adhesive properties can be achieved. Furthermore, by ensuring that the Mw is equal to or less than the upper limit, excellent flowability and operability can be achieved.
[0034] The acid-modified resin used in the present invention is preferably an acid-modified resin obtained by acid-modifying a hydrocarbon-based resin because of its good low dielectric properties. For example, an acid-modified polystyrene resin, an acid-modified cycloolefin polymer, or an acid-modified polyolefin is preferred, with an acid-modified polyolefin being more preferred. Furthermore, from the viewpoint of pot life, an acid-modified polystyrene resin or an acid-modified cycloolefin polymer is preferred. One or more types of acid-modified resins can be used in combination.
[0035] The acid-modified resin of the present invention preferably has a relative dielectric constant (εc) of 2.7 or less at a frequency of 10 GHz. It is more preferably 2.6 or less, and even more preferably 2.3 or less. There is no particular lower limit, but in practice it is 2.0. Furthermore, the relative dielectric constant (εc) over the entire frequency range of 1 GHz to 60 GHz is preferably 2.7 or less, more preferably 2.6 or less, and even more preferably 2.3 or less.
[0036] The acid-modified resin of the present invention preferably has a dielectric loss tangent (tan δ) of 0.003 or less at a frequency of 10 GHz. It is more preferably 0.0025 or less, and even more preferably 0.002 or less. There is no particular lower limit, but in practice it is 0.0001 or more. Furthermore, the dielectric loss tangent (tan δ) over the entire frequency range of 1 GHz to 60 GHz is preferably 0.003 or less, more preferably 0.0025 or less, and even more preferably 0.002 or less.
[0037] The content of the acid-modified resin in the adhesive composition of the present invention is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more, based on 100% by mass of the solid content of the adhesive composition. It is also preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less, even more preferably 85% by mass or less, particularly preferably 80% by mass or less, and may even be 75% by mass or less. Being within the above range is preferable because it provides good adhesion and heat resistance.
[0038] <Acid-Modified Polyolefin> In the present invention, an acid-modified polyolefin can be preferably used as the acid-modified resin. The acid-modified polyolefin used in the present invention is not limited, but is preferably one obtained by grafting an unsaturated carboxylic acid component (preferably at least one of an α,β-unsaturated carboxylic acid and its acid anhydride) onto a polyolefin resin. Polyolefin resin refers to a polymer primarily composed of a hydrocarbon skeleton, such as a homopolymer of an olefin monomer, exemplified by ethylene, propylene, butene, butadiene, isoprene, etc., or a copolymer with other monomers, or a hydrogenated or halide product of the resulting polymer. The acid-modified polyolefin is preferably one obtained by grafting at least one of an α,β-unsaturated carboxylic acid and its acid anhydride onto at least one of polyethylene, polypropylene, and propylene-α-olefin copolymer.
[0039] Propylene-α-olefin copolymers are produced by copolymerizing propylene as the main component with an α-olefin. Examples of α-olefins that can be used include one or more of ethylene, 1-butene, 1-heptene, 1-octene, 4-methyl-1-pentene, and vinyl acetate. Among these α-olefins, ethylene and 1-butene are preferred. The ratio of the propylene component to the α-olefin component in the propylene-α-olefin copolymer is not limited, but the propylene component is preferably 50 mol% or more, and more preferably 70 mol% or more. Furthermore, these raw materials are not limited to petroleum-derived raw materials; raw materials obtained using chemical recycling technology that utilizes biomass naphtha or waste plastics may also be used.
[0040] The unsaturated carboxylic acid component is preferably at least one of an α,β-unsaturated carboxylic acid and an acid anhydride thereof, and specific examples are as described above, including maleic acid, itaconic acid, citraconic acid, and their acid anhydrides. Among these, acid anhydrides are preferred, and maleic anhydride is more preferred. That is, specific examples of acid-modified polyolefins include maleic anhydride-modified polypropylene, maleic anhydride-modified propylene-ethylene copolymer, maleic anhydride-modified propylene-butene copolymer, maleic anhydride-modified propylene-ethylene-butene copolymer, etc., and these acid-modified polyolefins can be used alone or in combination of two or more.
[0041] The acid value of the acid-modified polyolefin has a lower limit of 89 equivalents / 10 from the viewpoint of heat resistance and adhesion to resin substrates and metal substrates. 6 g or more, and more preferably 107 equivalents / 10 6 g or more, and more preferably 125 equivalents / 10 6 By adjusting the amount to be equal to or greater than the lower limit, compatibility with the epoxy resin (B) is improved, and excellent adhesive strength can be achieved. In addition, the crosslinking density is high, and solder heat resistance is improved. The upper limit is 713 equivalents / 10 6 g or less, and more preferably 534 equivalents / 10 6g or less, and more preferably 356 equivalents / 10 6 By adjusting the viscosity to the upper limit or less, the adhesiveness is improved. In addition, the viscosity and stability of the solution are improved, and an excellent pot life can be achieved. Furthermore, the production efficiency is improved.
[0042] The acid-modified polyolefin is preferably a crystalline acid-modified polyolefin. The term "crystalline" as used herein refers to a polyolefin that shows a clear melting peak during heating from -100°C to 250°C at a rate of 20°C / min using a differential scanning calorimeter (DSC).
[0043] The melting point (Tm) of the acid-modified polyolefin is preferably in the range of 50°C to 120°C, more preferably in the range of 60°C to 100°C, and most preferably in the range of 70°C to 90°C. By setting the melting point at or above the lower limit, the cohesive force derived from crystals becomes good, and excellent adhesive properties and solder heat resistance can be exhibited. Furthermore, by setting the melting point at or below the upper limit, excellent solution stability and flowability are achieved, and operability during bonding is improved.
[0044] The heat of fusion (ΔH) of the acid-modified polyolefin is preferably in the range of 5 J / g to 60 J / g, more preferably in the range of 10 J / g to 50 J / g, and most preferably in the range of 20 J / g to 40 J / g. By setting it to above the lower limit, the cohesive force derived from crystals becomes good, and excellent adhesive properties and solder heat resistance can be exhibited. Furthermore, by setting it to below the upper limit, excellent solution stability and fluidity are achieved, and operability during adhesion is improved.
[0045] The weight-average molecular weight (Mw) of the acid-modified polyolefin is preferably in the range of 10,000 to 500,000. More preferably, it is in the range of 20,000 to 400,000, even more preferably, it is in the range of 40,000 to 200,000, and particularly preferably, it is in the range of 50,000 to 100,000. By setting it to be equal to or greater than the lower limit, the cohesive strength is improved and excellent adhesive properties can be exhibited. Furthermore, by setting it to be equal to or less than the upper limit, excellent flowability and operability can be achieved.
[0046] The method for producing the acid-modified polyolefin is not particularly limited, and examples thereof include a radical graft reaction (i.e., a reaction in which radical species are generated on a polymer that becomes a main chain, and an unsaturated carboxylic acid component (preferably an α,β-unsaturated carboxylic acid and its acid anhydride) is graft-polymerized using the radical species as a polymerization initiation point).
[0047] <Acid-Modified Polystyrene Resin> In the present invention, an acid-modified polystyrene resin can be preferably used as the acid-modified resin. The acid-modified polystyrene resin is not limited, but is preferably an aromatic vinyl compound alone, or a copolymer mainly composed of a block and / or random structure of an aromatic vinyl compound and a conjugated diene compound, or a hydrogenated product thereof, modified with an unsaturated carboxylic acid component. Examples of aromatic vinyl compounds include, but are not limited to, styrene, t-butylstyrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-diethyl-p-aminoethylstyrene, vinyltoluene, and p-tert-butylstyrene. Examples of conjugated diene compounds include butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. These raw materials are not limited to petroleum-derived raw materials; raw materials obtained using chemical recycling technology utilizing biomass naphtha or waste plastics may also be used. Specific examples of copolymers of these aromatic vinyl compounds and conjugated diene compounds include styrene-butadiene block copolymers, styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-ethylene-propylene-styrene block copolymers (SEPS), and styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS). The unsaturated carboxylic acid component is preferably at least one of an α,β-unsaturated carboxylic acid and an acid anhydride thereof, and specific examples are as described above, including maleic acid, itaconic acid, citraconic acid, and their acid anhydrides. Of these, acid anhydrides are preferred, and maleic anhydride is more preferred.
[0048] The acid value of the acid-modified polystyrene resin has a lower limit of 10 equivalents / 10 from the viewpoint of heat resistance and adhesion to resin substrates and metal substrates. 6 g or more, and more preferably 20 equivalents / 10 6 g or more, and more preferably 50 equivalents / 10 6 By adjusting the amount to be equal to or greater than the lower limit, compatibility with the epoxy resin (B) is improved, and excellent adhesive strength can be achieved. In addition, the crosslinking density is high, and solder heat resistance is improved. The upper limit is 500 equivalents / 10 6 g or less, and more preferably 400 equivalents / 10 6 g or less, and more preferably 300 equivalents / 10 6 By adjusting the viscosity to the upper limit or less, the adhesiveness is improved. In addition, the viscosity and stability of the solution are improved, and an excellent pot life can be achieved. Furthermore, the production efficiency is improved.
[0049] <Acid-Modified Cycloolefin Polymer> In the present invention, it is also preferable to use an acid-modified cycloolefin polymer as the acid-modified resin. The acid-modified cycloolefin polymer is a cycloolefin polymer in which a carboxy group has been introduced by modifying the cycloolefin polymer with an unsaturated carboxylic acid component. As the cycloolefin polymer, either a homopolymer (COP) made from only one type of cycloolefin monomer, or a copolymer (COC) composed of one or more types of cycloolefin monomer and comonomer can be used. Furthermore, the unsaturated carboxylic acid component is preferably at least one of an α,β-unsaturated carboxylic acid and an acid anhydride thereof, specific examples of which are as described above, and examples include maleic acid, itaconic acid, citraconic acid, and the acid anhydrides thereof. Among these, acid anhydrides are preferred, and maleic anhydride is more preferred.
[0050] Examples of the cycloolefin monomer include bicyclic compounds such as norbornene and norbornadiene, tricyclic compounds such as dicyclopentadiene and dihydroxypentadiene, tetracyclic compounds such as tetracyclododecene, pentacyclic compounds such as cyclopentadiene trimer, heptacyclic compounds such as tetracyclopentadiene, and alkyl (methyl, ethyl, propyl, butyl, etc.)-substituted compounds, alkenyl (vinyl, etc.)-substituted compounds, alkylidene (ethylidene, etc.)-substituted compounds, and aryl (phenyl, tolyl, naphthyl, etc.)-substituted compounds of these polycyclic compounds. Among these, norbornene-based monomers selected from the group consisting of norbornene, tetracyclododecene, and alkyl-substituted compounds thereof are particularly preferred. Furthermore, these raw materials are not limited to petroleum-derived raw materials; raw materials obtained using chemical recycling technology using biomass naphtha or waste plastics may also be used.
[0051] The comonomer may be any monomer copolymerizable with the cycloolefin monomer, and is preferably, for example, an alkene monomer. Examples of the alkene monomer include α-olefins such as ethylene, propylene, 1-butene, and 1-hexene, and isobutene. The alkene monomer may be linear or branched.
[0052] The monomer components constituting the acid-modified cycloolefin polymer preferably contain 50 mass% or more of the cycloolefin monomer, more preferably 60 mass% or more of the cycloolefin monomer. When the cycloolefin monomer accounts for 50 mass% or more of the total monomer components, the solder heat resistance is good. There are no particular limitations on the polymerization method and polymerization conditions when polymerizing the monomer components, and they may be appropriately set according to conventional methods.
[0053] The weight average molecular weight (Mw) of the acid-modified cycloolefin polymer is preferably in the range of 10,000 to 500,000. More preferably, it is in the range of 20,000 to 400,000, even more preferably, it is in the range of 40,000 to 200,000, and particularly preferably, it is in the range of 50,000 to 100,000. By setting it to be equal to or greater than the lower limit, the cohesive strength is improved and excellent adhesive properties can be exhibited. Furthermore, by setting it to be equal to or less than the upper limit, excellent flowability and operability can be achieved.
[0054] The acid value of the acid-modified cycloolefin polymer has a lower limit of 89 equivalents / 10 from the viewpoint of heat resistance and adhesion to resin substrates and metal substrates. 6 g or more, and more preferably 107 equivalents / 10 6 g or more, and more preferably 125 equivalents / 10 6 By adjusting the amount to be equal to or greater than the lower limit, compatibility with the epoxy resin (B) is improved, and excellent adhesive strength can be achieved. In addition, the crosslinking density is high, and solder heat resistance is improved. The upper limit is 713 equivalents / 10 6 g or less, and more preferably 534 equivalents / 10 6 g or less, and more preferably 356 equivalents / 10 6 By adjusting the viscosity to the upper limit or less, the adhesiveness is improved. In addition, the viscosity and stability of the solution are improved, and an excellent pot life can be achieved. Furthermore, the production efficiency is improved.
[0055] <Epoxy Resin> The adhesive composition of the present invention contains an epoxy resin (B). The epoxy resin used in the present invention is not particularly limited as long as it has an epoxy group in the molecule, but is preferably a multifunctional epoxy resin having two or more epoxy groups in the molecule. Specifically, it is not particularly limited, but at least one selected from the group consisting of biphenyl-type epoxy resins, naphthalene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, novolac-type epoxy resins, alicyclic epoxy resins, dicyclopentadiene-type epoxy resins, glycidylamine-type epoxy resins, tetraglycidyldiaminodiphenylmethane, triglycidyl paraaminophenol, tetraglycidylbisaminomethylcyclohexanone, N,N,N',N'-tetraglycidyl-m-xylenediamine, diallyl monoglycidyl isocyanurate, diglycidyl monoallyl isocyanurate, and epoxy-modified polybutadiene can be used. Preferred are diglycidyl monoallyl isocyanurate, N,N,N',N'-tetraglycidyl-m-xylenediamine, biphenyl-type epoxy resin, novolac-type epoxy resin, dicyclopentadiene-type epoxy resin, glycidylamine-type epoxy resin, and epoxy-modified polybutadiene. Among them, those containing an unsaturated hydrocarbon group (preferably an allyl group CH) in the molecule are preferred. 2 =CH-CH 2 -*) is more preferred, and specifically, diglycidyl monoallyl isocyanurate. Diglycidyl monoallyl isocyanurate can exhibit particularly excellent dielectric properties and adhesive properties.
[0056] In the adhesive composition of the present invention, the content of the epoxy resin (B) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the acid-modified resin. By setting the content at or above the lower limit, a sufficient curing effect can be obtained, and excellent adhesion and solder heat resistance can be exhibited. Furthermore, the content is preferably 10 parts by mass or less, more preferably 5 parts by mass or less. By setting the content at or below the upper limit, the pot life and low dielectric properties can be improved. In other words, by setting the content within the above range, an adhesive composition having excellent adhesion, solder heat resistance, and low dielectric properties can be obtained.
[0057] <Polycarbodiimide> The adhesive composition of the present invention may contain a polycarbodiimide. The polycarbodiimide is not particularly limited as long as it has two or more carbodiimide bonds in the molecule. By using a polycarbodiimide, the carboxy group of the acid-modified resin or the epoxy group of the epoxy resin (B) reacts with the carbodiimide bond, thereby improving heat resistance and adhesiveness.
[0058] In the adhesive composition of the present invention, the content of polycarbodiimide is preferably 1 part by mass or more, more preferably 3 parts by mass or more, per 100 parts by mass of the acid-modified resin. By making the content equal to or greater than the lower limit, the crosslink density can be increased, resulting in good solder heat resistance. Furthermore, the content is preferably 20 parts by mass or less, more preferably 10 parts by mass or less. By making the content equal to or less than the upper limit, excellent solder heat resistance and low dielectric properties can be achieved. In other words, by making the content within the above range, an adhesive composition having excellent solder heat resistance and low dielectric properties can be obtained.
[0059] <Unsaturated Hydrocarbon> The adhesive composition of the present invention may contain an unsaturated hydrocarbon having a terminal unsaturated hydrocarbon group and a 5% weight loss temperature of 260°C or higher. When the unsaturated hydrocarbon contains a terminal unsaturated hydrocarbon group, the crosslink density can be increased by a curing reaction caused by radicals generated by using a radical initiator or the like, thereby improving solder heat resistance. Furthermore, since hydroxyl groups that deteriorate dielectric properties are not generated after the reaction, an adhesive with better dielectric properties can be obtained. It is preferable that one molecule contains two or more terminal unsaturated hydrocarbon groups, as this further increases the crosslink density.
[0060] The 5% weight loss temperature of the unsaturated hydrocarbon must be 260°C or higher. It is preferably 270°C or higher, more preferably 280°C or higher, and even more preferably 290°C or higher. When the 5% weight loss temperature is above this value, soldering can be performed without causing poor appearance even at temperatures exceeding the melting point of the solder. There is no particular upper limit, but 500°C is practical.
[0061] The unsaturated hydrocarbon preferably has an aromatic ring structure or an alicyclic structure as a structural unit. Having an aromatic ring structure or an alicyclic structure as a structural unit can improve solder heat resistance and also provide excellent dielectric properties. Among these, an aromatic ring structure or an alicyclic structure is preferred as the skeleton of the unsaturated hydrocarbon, and polyphenylene ether or phenol resin is preferred. Specific examples of polyphenylene ethers having terminal unsaturated hydrocarbon groups include SA-9000 from SABIC Corporation and OPE-2St from Mitsubishi Gas Chemical Company, Inc. Another example of a phenol resin having terminal unsaturated hydrocarbon groups is Resitop FTC-809AE from Gunei Chemical Industry Co., Ltd.
[0062] The number average molecular weight of the unsaturated hydrocarbon is preferably at least 500, more preferably at least 1000. It is also preferably at most 100,000, more preferably at most 10,000, and even more preferably at most 5,000. Within the above range, the solubility in solvents is good, and a uniform adhesive coating film can be formed.
[0063] The content of the unsaturated hydrocarbon in the adhesive composition of the present invention is preferably 1 part by mass or more, more preferably 2 parts by mass or more, per 100 parts by mass of the acid-modified resin. The content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less. Within this range, both excellent adhesive properties and solder heat resistance can be achieved.
[0064] <Radical Generator> The adhesive composition of the present invention preferably contains a radical generator. The radicals generated by the radical generator efficiently react the terminal unsaturated hydrocarbon groups of the unsaturated hydrocarbon, increasing the crosslink density and thereby improving solder heat resistance and dielectric properties. The radical generator is not particularly limited, but an organic peroxide is preferably used. Examples of organic peroxides include, but are not limited to, peroxides such as di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, dicumyl peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butylperoxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide, and lauroyl peroxide; and azonitriles such as azobisisobutyronitrile and azobisisopropionitrile.
[0065] The one-minute half-life temperature of the radical generator used in the present invention is preferably 140° C. or higher. By setting the temperature to 140° C. or higher, the initiation of a radical reaction can be prevented when the solvent in the adhesive composition varnish is volatilized to produce an adhesive sheet, and excellent adhesiveness can be achieved.
[0066] The amount of the radical generator used in the present invention is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, per 100 parts by mass of the unsaturated hydrocarbon. The amount is preferably 50 parts by mass or less, more preferably 10 parts by mass or less. By adjusting the amount within the above range, an optimal crosslink density can be achieved, and both adhesiveness and solder heat resistance can be achieved.
[0067] <Organic Solvent> The adhesive composition of the present invention may further contain an organic solvent. The organic solvent used in the present invention is not particularly limited as long as it dissolves the acid-modified resin, the compound (A), and the epoxy resin (B). Specific examples include aromatic hydrocarbons such as benzene, toluene, and xylene; aliphatic hydrocarbons such as hexane, heptane, octane, and decane; alicyclic hydrocarbons such as cyclohexane, cyclohexene, methylcyclohexane, and ethylcyclohexane; halogenated hydrocarbons such as trichloroethylene, dichloroethylene, chlorobenzene, and chloroform; alcoholic solvents such as methanol, ethanol, isopropyl alcohol, butanol, pentanol, hexanol, propanediol, and phenol; acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclohexanone, isophorone, and acetophenone. ketone-based solvents, cellosolves such as methyl cellosolve and ethyl cellosolve, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl propionate and butyl formate, glycol ether-based solvents such as ethylene glycol mono-n-butyl ether, ethylene glycol mono-iso-butyl ether, ethylene glycol mono-tert-butyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-iso-butyl ether, triethylene glycol mono-n-butyl ether and tetraethylene glycol mono-n-butyl ether, and the like, can be used alone or in combination of two or more thereof. Methylcyclohexane and toluene are particularly preferred from the viewpoint of working environment and drying properties.
[0068] The organic solvent is preferably in the range of 100 to 1,000 parts by mass per 100 parts by mass of the solid content of the adhesive composition. By setting the amount to be equal to or greater than the lower limit, the liquid state and pot life are improved. Furthermore, by setting the amount to be equal to or less than the upper limit, it is advantageous in terms of production costs and transportation costs.
[0069] The adhesive composition of the present invention may further contain other components as needed, such as a flame retardant, a tackifier, a filler, an antioxidant, and a silane coupling agent.
[0070] <Flame Retardant> The adhesive composition of the present invention may optionally contain a flame retardant. Examples of flame retardants include bromine-based, phosphorus-based, nitrogen-based, and metal hydroxide compounds. Phosphorus-based flame retardants are preferred, and known phosphorus-based flame retardants such as phosphate esters (e.g., trimethyl phosphate, triphenyl phosphate, tricresyl phosphate), phosphate salts (e.g., aluminum phosphinate), and phosphazenes can be used. These flame retardants may be used alone or in any combination of two or more. When a flame retardant is added, it is preferably contained in an amount of 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, and most preferably 10 to 100 parts by mass, per 100 parts by mass of the total of the acid-modified resin, compound (A), and epoxy resin (B). By keeping the amount within this range, flame retardancy can be achieved while maintaining adhesion, solder heat resistance, and electrical properties.
[0071] <Tackifier> The adhesive composition of the present invention may contain a tackifier as needed. Examples of tackifiers include polyterpene resins, rosin-based resins, aliphatic petroleum resins, alicyclic petroleum resins, copolymerized petroleum resins, styrene resins, and hydrogenated petroleum resins, and are used to improve adhesive strength. These may be used alone or in any combination of two or more. When a tackifier is added, it is preferably added in an amount of 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, and most preferably 10 to 100 parts by mass, per 100 parts by mass of the total of the acid-modified resin, compound (A), and epoxy resin (B). By keeping the amount within this range, the effects of the tackifier can be exerted while maintaining adhesion, solder heat resistance, and electrical properties.
[0072] <Filler> The adhesive composition of the present invention may contain a filler as needed. Examples of organic fillers include powders of heat-resistant resins such as polyimide, polyamideimide, fluororesin, and liquid crystal polyester. Examples of inorganic fillers include silica (SiO), alumina (AlO), titania (TiO), tantalum oxide (TaO), zirconia (ZrO), silicon nitride (SiN), boron nitride (BN), calcium carbonate (CaCO), calcium sulfate (CaSO), zinc oxide (ZnO), magnesium titanate (MgO.TiO), barium sulfate (BaSO), organic bentonite, clay, mica, aluminum hydroxide, and magnesium hydroxide. Among these, silica is preferred due to its ease of dispersion and improved heat resistance.
[0073] While hydrophobic silica and hydrophilic silica are commonly known as silica, hydrophobic silica treated with dimethyldichlorosilane, hexamethyldisilazane, octylsilane, or the like is preferred here for its moisture absorption resistance. When silica is added, the amount is preferably 0.05 to 30 parts by mass per 100 parts by mass of the total of the acid-modified resin, compound (A), and epoxy resin (B). By adding silica at or above the lower limit, further heat resistance can be achieved. Furthermore, by adding silica at or below the upper limit, poor dispersion of the silica and excessively high solution viscosity can be prevented, improving workability.
[0074] <Antioxidant> The adhesive composition of the present invention may contain an antioxidant as needed. The incorporation of an antioxidant is preferred because it can prevent deterioration of properties such as adhesiveness and dielectric properties even when the adhesive composition is used in a high-temperature environment exposed to air. The antioxidant is not particularly limited, but examples include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. These may be used alone or in combination of two or more.
[0075] When the adhesive composition contains an antioxidant, the content thereof is preferably 0.5 to 5 parts by mass, and more preferably 1 to 3 parts by mass, per 100 parts by mass of the solid content of the adhesive composition. When the content of the antioxidant is within the above range, deterioration of properties such as adhesiveness and dielectric properties can be suppressed even when the adhesive composition is used in a high-temperature environment where it is exposed to air.
[0076] <Silane Coupling Agent> The adhesive composition of the present invention may optionally contain a silane coupling agent. The inclusion of a silane coupling agent is highly preferred because it improves adhesion to metals and heat resistance. Silane coupling agents are not particularly limited, but examples include those containing unsaturated groups, epoxy groups, and amino groups. Among these, silane coupling agents containing epoxy groups, such as γ-glycidoxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, are more preferred from the perspective of heat resistance. When a silane coupling agent is included, the amount is preferably 0.5 to 20 parts by mass per 100 parts by mass of the total of the acid-modified resin, compound (A), and epoxy resin (B). By using a silane coupling agent within this range, solder heat resistance and adhesion can be improved.
[0077] <Laminate> The laminate of the present invention is a substrate to which an adhesive composition is laminated (a two-layer laminate of substrate / adhesive layer), or a substrate is further attached (a three-layer laminate of substrate / adhesive layer / substrate). Here, the adhesive layer refers to the layer of the adhesive composition of the present invention remaining after the adhesive composition of the present invention is applied to a substrate and dried. The laminate of the present invention can be obtained by applying the adhesive composition of the present invention to various substrates and drying it according to a conventional method, and then laminating another substrate on top of it.
[0078] <Substrate> In the present invention, the substrate is not particularly limited as long as it is possible to form an adhesive layer by applying and drying the adhesive composition of the present invention, and examples thereof include resin substrates such as film-like resins, metal substrates such as metal plates and metal foils, and paper.
[0079] Examples of the resin substrate include polyester resin, polyamide resin, polyimide resin, polyamideimide resin, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resin, and fluorine-based resin. A film-like resin (hereinafter also referred to as a substrate film layer) is preferred.
[0080] The metal substrate can be any conventionally known conductive material that can be used for circuit boards. Examples of materials include various metals such as SUS, copper, aluminum, iron, steel, zinc, and nickel, as well as their alloys, plated products, and metals treated with other metals such as zinc or chromium compounds. Metal foil is preferred, and copper foil is more preferred. The thickness of the metal foil is not particularly limited, but is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 10 μm or more. It is also preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less. If the thickness is too thin, it may be difficult to obtain sufficient electrical performance of the circuit, while if the thickness is too thick, processing efficiency during circuit fabrication may be reduced. Metal foil is usually provided in a roll form. The form of the metal foil used in manufacturing the printed wiring board of the present invention is not particularly limited. When a ribbon-shaped metal foil is used, its length is not particularly limited. Its width is also not particularly limited, but is preferably about 250 to 500 cm. The surface roughness of the substrate is not particularly limited, but is preferably 3 μm or less, more preferably 2 μm or less, and even more preferably 1.5 μm or less. In practical terms, it is preferably 0.3 μm or more, more preferably 0.5 μm or more, and even more preferably 0.7 μm or more.
[0081] Examples of the paper include fine paper, kraft paper, roll paper, glassine paper, etc. Examples of the composite material include glass epoxy, etc.
[0082] In view of adhesive strength with the adhesive composition and durability, the substrate is preferably a polyester resin, a polyamide resin, a polyimide resin, a polyamideimide resin, a liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, a polyolefin resin, a fluorine-based resin, an SUS steel plate, a copper foil, an aluminum foil, or a glass epoxy.
[0083] <Adhesive Sheet> In the present invention, the adhesive sheet is formed by laminating the substrate and a release substrate via an adhesive composition. Specific configurations include substrate / adhesive layer / release substrate, or release substrate / adhesive layer / substrate / adhesive layer / release substrate. Laminating the release substrate functions as a protective layer for the substrate. Furthermore, by using a release substrate, the release substrate can be released from the adhesive sheet and the adhesive layer can be transferred to another substrate.
[0084] The adhesive sheet of the present invention can be obtained by applying the adhesive composition of the present invention to various laminates and drying them according to conventional methods. Furthermore, by attaching a release substrate to the adhesive layer after drying, the adhesive can be wound up without causing offset onto the substrate, resulting in excellent operability, and the adhesive layer is protected, resulting in excellent storage stability and ease of use. Furthermore, after application to a release substrate and drying, the adhesive layer itself can be transferred to another substrate by attaching another release substrate as needed.
[0085] <Release Substrate> The release substrate is not particularly limited, but examples include paper such as fine paper, kraft paper, roll paper, and glassine paper, on both sides of which a coating layer of a filler such as clay, polyethylene, or polypropylene is provided, and each of these coating layers is further coated with a silicone-based, fluorine-based, or alkyd-based release agent. Other examples include various olefin films such as polyethylene, polypropylene, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer alone, and films such as polyethylene terephthalate coated with the above-mentioned release agent. Due to factors such as the release force between the release substrate and the adhesive layer and the adverse effect of silicone on electrical properties, it is preferable to use a polypropylene-sealed film on both sides of fine paper and then apply an alkyd-based release agent thereon, or a polyethylene terephthalate film on which an alkyd-based release agent is applied.
[0086] In the present invention, the method for coating the adhesive composition on a substrate is not particularly limited, but examples include a comma coater, reverse roll coater, die coater, etc. Alternatively, if necessary, an adhesive layer can be applied directly or by transfer method to rolled copper foil or polyimide film, which are components of printed wiring boards. The thickness of the adhesive layer after drying can be adjusted as needed, but is preferably in the range of 5 to 200 μm. By making the adhesive film thickness 5 μm or more, sufficient adhesive strength can be obtained. Furthermore, by making the thickness 200 μm or less, it is easier to control the amount of residual solvent during the drying process, and blisters are less likely to occur during pressing in the production of printed wiring boards. While the drying conditions are not particularly limited, a residual solvent ratio of 1% by mass or less after drying is preferred. By making the residual solvent thickness 1% by mass or less, blisters due to residual solvent are suppressed during pressing of the printed wiring board, making blisters less likely to occur.
[0087] <Printed Wiring Board> The printed wiring board of the present invention includes, as a component, a laminate formed from a metal foil forming a conductor circuit and a resin substrate. The printed wiring board is manufactured by a conventionally known method such as a subtractive method using a metal-clad laminate, for example. The term "printed wiring board" collectively refers to so-called flexible circuit boards (FPCs), flat cables, circuit boards for tape automated bonding (TAB), etc., in which a conductor circuit formed from metal foil is partially or entirely covered with a cover film, screen printing ink, etc., as necessary.
[0088] The printed wiring board of the present invention can have any laminated structure that can be used as a printed wiring board. For example, it can be a printed wiring board consisting of four layers: a base film layer, a metal foil layer, an adhesive layer, and a cover film layer. Alternatively, it can be a printed wiring board consisting of five layers: a base film layer, an adhesive layer, a metal foil layer, an adhesive layer, and a cover film layer.
[0089] Furthermore, if necessary, two or more of the above printed wiring boards may be stacked.
[0090] The adhesive composition of the present invention can be suitably used in each adhesive layer of a printed wiring board. In particular, when the adhesive composition of the present invention is used as an adhesive, it exhibits high adhesion not only to conventional polyimide, polyester film, and copper foil constituting printed wiring boards, but also to low-polarity resin substrates such as LCP, and can achieve solder reflow resistance, and the adhesive layer itself has excellent low dielectric properties. Therefore, it is suitable as an adhesive composition for use in coverlay films, laminates, resin-coated copper foils, and bonding sheets.
[0091] In the printed wiring board of the present invention, any resin film conventionally used as a substrate for printed wiring boards can be used as the substrate film. Examples of resins for the substrate film include polyester resins, polyamide resins, polyimide resins, polyamideimide resins, liquid crystal polymers, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resins, and fluorine-based resins. In particular, the film has excellent adhesion to low-polarity substrates such as liquid crystal polymers, polyphenylene sulfide, syndiotactic polystyrene, and polyolefin resins.
[0092] <Cover film> As the cover film, any insulating film conventionally known as an insulating film for printed wiring boards can be used. For example, films made from various polymers such as polyimide, polyester, polyphenylene sulfide, polyethersulfone, polyetheretherketone, aramid, polycarbonate, polyarylate, polyamideimide, liquid crystal polymer, syndiotactic polystyrene, and polyolefin resin can be used. Polyimide film or liquid crystal polymer film is more preferred.
[0093] The printed wiring board of the present invention can be manufactured by any conventionally known process, except for using the materials for each layer described above.
[0094] In a preferred embodiment, a semi-finished product is produced in which an adhesive layer is laminated on a cover film layer (hereinafter referred to as a "cover film side semi-finished product"). On the other hand, a semi-finished product is produced in which a metal foil layer is laminated on a base film layer to form a desired circuit pattern (hereinafter referred to as a "base film side two-layer semi-finished product"), or a semi-finished product is produced in which an adhesive layer is laminated on a base film layer and a metal foil layer is laminated on top of it to form a desired circuit pattern (hereinafter referred to as a "base film side three-layer semi-finished product"). The thus obtained cover film side semi-finished product and the base film side semi-finished product are bonded together to obtain a four-layer or five-layer printed wiring board.
[0095] The substrate film-side semi-finished product can be obtained, for example, by a manufacturing method including: (A) a step of applying a solution of a resin that will become the substrate film to the metal foil and initially drying the coating film; and (B) a step of heat-treating and drying the laminate of the metal foil and the initially dried coating film obtained in (A) (hereinafter referred to as the "heat treatment / solvent removal step").
[0096] The circuit can be formed on the metal foil layer by a conventionally known method. Either an additive method or a subtractive method may be used. The subtractive method is preferred.
[0097] The obtained semi-finished product on the base film side may be used as it is for bonding to the semi-finished product on the cover film side, or may be used for bonding to the semi-finished product on the cover film side after a release film has been attached and stored.
[0098] The cover film semi-finished product is produced, for example, by applying an adhesive to the cover film. If necessary, a crosslinking reaction can be carried out in the applied adhesive. In a preferred embodiment, the adhesive layer is semi-cured.
[0099] The obtained cover film side semi-finished product may be used as it is for bonding to the base film side semi-finished product, or may be used for bonding to the base film side semi-finished product after a release film has been attached and stored.
[0100] The substrate film-side semi-finished product and the cover film-side semi-finished product are stored, for example, in the form of a roll, and then bonded together to produce a printed wiring board. Any bonding method can be used, and for example, they can be bonded together using a press or a roll. They can also be bonded together while heating them using a heat press or a heat roll device.
[0101] For example, in the case of a reinforcing material that is soft and can be wound up, such as a polyimide film, the reinforcing material semi-finished product is preferably produced by applying an adhesive to the reinforcing material. Furthermore, in the case of a reinforcing plate that is hard and cannot be wound up, such as a metal plate such as SUS or aluminum, or a plate made of glass fiber cured with an epoxy resin, it is preferably produced by transfer coating an adhesive that has been applied in advance to a release substrate. If necessary, a crosslinking reaction can be carried out in the applied adhesive. In a preferred embodiment, the adhesive layer is semi-cured.
[0102] The obtained semi-finished product on the reinforcing material side may be used as it is for bonding to the rear surface of a printed wiring board, or may be used for bonding to a semi-finished product on the base film side after a release film has been attached and stored.
[0103] The base film side semi-finished product, the cover film side semi-finished product, and the reinforcing material side semi-finished product are all laminates for printed wiring boards of the present invention.
[0104] This application claims the benefit of priority based on Japanese Patent Application No. 2023-088669, filed on May 30, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-088669, filed on May 30, 2023, are incorporated herein by reference.
[0105] The present invention will be described in more detail below with reference to examples. In these examples and comparative examples, "parts" simply refers to parts by mass.
[0106] <Method for Evaluating Physical Properties> (Acid Value Measurement) The acid value (equivalent / 10 6In g), the acid-modified resin was dissolved in toluene and titrated with a methanol solution of sodium methoxide using phenolphthalein as an indicator.
[0107] (Weight-Average Molecular Weight (Mw)) The weight-average molecular weight in the present invention is a value measured by gel permeation chromatography (hereinafter referred to as GPC, standard substance: polystyrene resin, mobile phase: tetrahydrofuran, column: Shodex KF-802 + KF-804L + KF-806L, column temperature: 30°C, flow rate: 1.0 ml / min, detector: RI detector) manufactured by Shimadzu Corporation.
[0108] (Measurement of Melting Point) The melting point in the present invention is a value measured using a differential scanning calorimeter (hereinafter referred to as DSC, manufactured by TA Instruments Japan, Q-2000) from the top temperature of the melting peak when the material is heated and melted at a rate of 20°C / min, cooled to form a resin, and then heated and melted again.
[0109] (Density) The density is a value measured at 23° C. in accordance with ISO 1183.
[0110] (Melt Viscosity) The melt viscosity is a value measured in accordance with DIN 53019 using a rotational viscometer at 170°C.
[0111] The following describes examples of producing adhesive compositions according to the present invention and comparative examples.
[0112] The following compound (A) was used: (a1): LICOCENE PP 1302 (Clariant, polyolefin resin, weight average molecular weight 19,100, melt viscosity (170°C) 200 mPa s, melting point 90°C, density 0.87 g / cm 3 (a2): LICOCENE PP 1502 (Clariant, polyolefin resin, weight average molecular weight 46,900, melt viscosity (170 ° C) 1,800 mPa s, melting point 86 ° C, density 0.87 g / cm 3 (a3): LICOCENE PP 1602 (Clariant, polyolefin resin, weight average molecular weight 50,000, melt viscosity (170°C) 6,000 mPa s, melting point 88°C, density 0.87 g / cm 3(a4): LICOCENE PP 2502 (Clariant, polyolefin resin, weight average molecular weight 40,900, melt viscosity (170 ° C) 2,000 mPa s, melting point 103 ° C, density 0.87 g / cm 3 )
[0113] The acid-modified resin was produced as follows. (Production Example 1) 100 parts by mass of a cycloolefin polymer (ZEONEX (registered trademark) RS420 manufactured by Zeon Corporation), 150 parts by mass of toluene, 19 parts by mass of maleic anhydride, and 6 parts by mass of di-tert-butyl peroxide were added to a 1 L autoclave, and the mixture was heated to 140°C and stirred for an additional 3 hours. The resulting reaction liquid was then cooled and poured into a container containing a large amount of methyl ethyl ketone to precipitate a resin. The liquid containing the resin was then centrifuged to separate and purify the acid-modified cycloolefin polymer graft-polymerized with maleic anhydride, (poly)maleic anhydride, and low-molecular-weight substances. The mixture was then dried under reduced pressure at 70°C for 5 hours to obtain a maleic anhydride-modified cycloolefin polymer (acid-modified resin 1, acid value 339 equivalents / 10 6 The dielectric constant at a frequency of 10 GHz was 2.0, the dielectric loss tangent at a frequency of 10 GHz was 0.0008, and the weight average molecular weight was 90,000.
[0114] (Production Example 2) 100 parts by mass of a propylene-butene copolymer ("TAFMER (registered trademark) XM7080" manufactured by Mitsui Chemicals, Inc.), 150 parts by mass of toluene, 19 parts by mass of maleic anhydride, and 6 parts by mass of di-tert-butyl peroxide were added to a 1 L autoclave, and the mixture was heated to 140°C and stirred for an additional 3 hours. Thereafter, the resulting reaction liquid was cooled and poured into a container containing a large amount of methyl ethyl ketone to precipitate a resin. Thereafter, the liquid containing the resin was centrifuged to separate and purify the acid-modified propylene-butene copolymer graft-polymerized with maleic anhydride, (poly)maleic anhydride, and low-molecular-weight substances. Thereafter, the mixture was dried under reduced pressure at 70°C for 5 hours to obtain a maleic anhydride-modified propylene-butene copolymer (acid-modified resin 2, acid value 339 equivalents / 10 6 The polymer had a weight average molecular weight of 75,000, a temperature of 80°C, and a ΔH of 35 J / g.
[0115] Other acid-modified resins used were as follows: (Acid-modified resin 3): Tuftec M1943 (manufactured by Asahi Kasei Corporation, a polymer obtained by hydrogenating the double bond portion of a block copolymer of styrene and butadiene, modified with maleic anhydride, acid value 185 equivalents / 10 6 g)
[0116] The following epoxy resins were used as the epoxy resin (B): (b1): MA-DGIC (monoallyl diglycidyl isocyanurate, manufactured by Shikoku Chemical Industry Co., Ltd.) (b2): jER604 (glycidylamine-type epoxy resin, manufactured by Mitsubishi Chemical Corporation) (b3): EPICLON HP-7200 (multifunctional dicyclopentadiene-type epoxy resin, manufactured by DIC Corporation)
[0117] Other adhesive ingredients used were as follows: (c1): LICOCENE PP 2602 (Clariant, polyolefin resin, weight average molecular weight 65,100, melt viscosity (170°C) 6,300 mPa s, melting point 98°C, density 0.88 g / cm 3 (c2): LICOCENE PP 3602 (Clariant, polyolefin resin, weight average molecular weight 58,400, melt viscosity (170°C) 9,300 mPa s, melting point 111°C, density 0.90 g / cm 3 (c3): L-MODU S901 (manufactured by Idemitsu Kosan, polyolefin resin, weight average molecular weight 130,000, melting point 80°C) (c4): SA9000 (manufactured by SABIC, polyphenylene ether having vinyl groups, number average molecular weight 1700, 5% weight loss temperature 439°C) (c5): LICOCENE PP 6102 (manufactured by Clariant, polyolefin resin, weight average molecular weight 9,000, melt viscosity (170°C) 60 mPa s, melting point 145°C, density 0.90 g / cm 3 )
[0118] Example 1 30 parts of (a1) as compound (A), 100 parts of (acid-modified resin 2) as acid-modified resin, 4 parts of (b1) as epoxy resin (B), and 5 parts of (c4) as other components were blended and dissolved in toluene to a solids concentration of 24% to obtain a toluene adhesive composition (S1). The obtained adhesive composition (S1) was evaluated for its dielectric constant, dielectric loss tangent, peel strength, solder heat resistance, varnish solubility, and circuit embeddability. The results are shown in Table 1.
[0119] Examples 2 to 12, Comparative Examples 1 to 9 Adhesive compositions (S2) to (S21) were prepared and evaluated in the same manner as in Example 1, except that the types and amounts of each component of the adhesive composition were changed as shown in Tables 1 and 2. The results are shown in Tables 1 and 2.
[0120] <Evaluation of Adhesive Composition> (Dielectric Constant (εc) and Dielectric Loss Tangent (tan δ)) The adhesive composition was applied to a 100 μm thick Teflon® sheet so that the dried thickness would be 25 μm, and then dried at 130°C for 3 minutes. The adhesive composition was then cured by heat treatment at 180°C for 3 hours, and the Teflon® sheet was peeled off to obtain a test adhesive sheet. The test adhesive sheet was then cut into 8 cm x 3 mm strips to obtain test samples. The dielectric constant (εc) and dielectric loss tangent (tan δ) were measured using a network analyzer (manufactured by Anritsu Corporation) by a cavity resonator perturbation method at a temperature of 23°C and a frequency of 10 GHz. <Evaluation Criteria for Dielectric Constant> ○: 2.4 or less ×: More than 2.4 <Evaluation Criteria for Dielectric Loss Tangent> ○: 0.0010 or less △: More than 0.0010 and less than 0.0020 ×: 0.0020 or more
[0121] (Peel Strength (Adhesion)) The adhesive composition was applied to a 12.5 μm thick polyimide film (Apical (registered trademark), manufactured by Kaneka Corporation) so that the thickness after drying would be 25 μm, and then dried at 130°C for 3 minutes. The adhesive film (B-stage product) thus obtained was laminated to an 18 μm thick rolled copper foil (ESPANEX series, manufactured by Nippon Steel Chemical & Material Co., Ltd.). The laminate was bonded by pressing for 280 seconds at 170°C under a pressure of 2 MPa so that the shiny side of the rolled copper foil was in contact with the adhesive layer. The laminate was then heat-treated at 180°C for 3 hours to cure the foil, and a sample for peel strength evaluation was obtained. The peel strength was measured at 25°C, with film pulling, a tensile speed of 50 mm / min, and 90° peeling. This test indicates the adhesive strength at room temperature. <Evaluation Criteria> ○: 1.0 N / mm or more ×: Less than 1.0 N / mm
[0122] (Soldering heat resistance) Evaluation samples were prepared in the same manner as for measuring peel strength, and 2.0 cm x 2.0 cm sample pieces were immersed in a solder bath molten at 288°C, and the presence or absence of changes in appearance such as blistering was confirmed. <Evaluation criteria> ○: No blistering for 60 seconds or more △: Blistering for 30 seconds or more but less than 60 seconds ×: Blistering for less than 30 seconds
[0123] (Varnish Solubility) After blending the components, the adhesive composition was stirred at room temperature and the solubility of the resulting composition was confirmed. <Evaluation Criteria> ○: All components were completely dissolved △: Part of the components was not dissolved ×: The components were not completely dissolved
[0124] (Circuit Embedding Ability) The adhesive composition was applied to one side of a 12.5 μm thick polyimide film (Apical (registered trademark), manufactured by Kaneka Corporation) to a dried thickness of 25 μm, and then dried at 130°C for 3 minutes. The adhesive film (B-stage product) obtained in this manner was bonded to a substrate having a circuit formed at a 25 μm pitch on 18 μm thick rolled copper foil (ESPANEX series, manufactured by Nippon Steel Chemical & Material Co., Ltd.). The bonding was performed by pressing the circuit surface with the adhesive layer in contact with the adhesive layer for 280 seconds under a pressure of 2 MPa at 170°C. The amount of adhesive flowing out from the bonded surface along the circuit was measured using a microscope. This test was performed on an adhesive film (B-stage product) immediately after production and on an adhesive film stored at 25°C for 1 week, and changes in the measured values were observed. If the measured value after one week of storage at 25°C decreases to less than 50% of the initial measured value, the circuit embeddability under practical conditions will not be satisfactory, and there is a risk of poor insulation of the printed circuit board. <Evaluation criteria> ○: Rate of change 80% or more and 100% or less △: Rate of change 50% or more and less than 80% ×: Rate of change less than 50%
[0125]
[0126]
[0127] As is clear from Table 1, Examples 1 to 12 exhibit excellent dielectric properties, peel strength, solder heat resistance, and circuit embeddability. Examples 1 to 12 also exhibit good varnish solubility. As shown in Examples 2 to 5, increasing the content of compound (A) improves dielectric properties. Comparing Examples 1, 3, 6, and 7, it is clear that the solder heat resistance, varnish solubility, and circuit embeddability can be varied depending on the properties of compound (A). Comparing Examples 3, 10, and 11, it is clear that the dielectric properties can be further improved by incorporating an epoxy resin (B) containing an unsaturated hydrocarbon group in the molecule. Although Example 12 did not contain (c4), a comparison with Example 3 shows that (c4) contributes to excellent adhesion and improved solder heat resistance.
[0128] On the other hand, in Comparative Example 1, the amount of compound (A) was too small, so the adhesive film lost fluidity after storage at 25°C for one week, resulting in poor circuit embeddability. In Comparative Example 2, the amount of compound (A) was too large, resulting in a relatively reduced amount of acid-modified resin, and the solder heat resistance of the adhesive composition was poor. In Comparative Examples 3 and 4, high-density polyolefin resins were used instead of compound (A), but these polyolefin resins were highly crystalline and therefore could not be dissolved in solvents, making it impossible to perform various evaluations. In Comparative Examples 5 and 8, a polyolefin resin with a high weight-average molecular weight of 120,0000 was used, resulting in insufficient fluidity of the adhesive composition and poor circuit embeddability. In Comparative Examples 6 and 9, a very low-molecular-weight polyolefin with a weight-average molecular weight of less than 10,000 was used, resulting in poor solder heat resistance. In Comparative Example 7, no unmodified polyolefin resin was added, resulting in poor dielectric properties and poor circuit embeddability.
[0129] The adhesive composition of the present invention has excellent solder heat resistance and adhesive strength, a low dielectric constant and dielectric loss tangent, and good circuit embeddability, and is therefore useful as an adhesive or adhesive sheet for FPCs in the high frequency range.
Claims
1. An adhesive composition comprising an acid-modified resin, a compound (A) and an epoxy resin (B), characterized in that the content of the compound (A) is 10 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the acid-modified resin. Compound (A): does not have a heteroatom, has a weight average molecular weight of 10,000 or more and 70,000 or less, a melting point of 60°C or more and 120°C or less, and a density of 0.88 g / cm 3 Polyolefin resin having a viscosity of less than 1000 MPa.
2. The adhesive composition according to claim 1, wherein the acid-modified resin is an acid-modified polyolefin.
3. The adhesive composition according to claim 1 or 2, wherein the epoxy resin (B) is a multifunctional epoxy resin.
4. The adhesive composition according to claim 1 or 2, wherein the melt viscosity of compound (A) at 170°C is 10,000 mPa·s or less.
5. An adhesive sheet comprising the adhesive composition according to claim 1 or 2.
6. A laminate comprising the adhesive composition according to claim 1 or 2.
7. A printed wiring board comprising the laminate according to claim 6 as a component.
Citation Information
Patent Citations
Composition, coating agent, adhesive, and laminate
WO2018221331A1
Adhesive composition, and adhesive layer-equipped layered product using same
WO2019172109A1
Low-dielectric adhesive composition
WO2019230445A1