Catalyst-carrying honeycomb structure and method for manufacturing the same

The ceramic honeycomb structure with embedded electrodes and catalyst layers addresses the uniform heating challenge in ammonia decomposition, enhancing both conversion rates and catalyst longevity by leveraging electrical conductivity and controlled heat distribution.

WO2024247382A1PCT designated stage expired Publication Date: 2024-12-05TYK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/004704
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-02-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing ammonia decomposition catalyst-supported honeycomb structures face challenges in achieving uniform temperature distribution, leading to compromised ammonia conversion rates and catalyst lifespan due to the heating method used in prior technologies.

Method used

A ceramic honeycomb structure with a catalyst layer in the flow path and on the side surfaces, equipped with electrodes for uniform heating by electrical conductivity, utilizing silicon carbide and silicon nitride powders for sintering and electrical conduction, allowing for controlled heat generation and distribution.

Benefits of technology

This approach enables simultaneous improvement in ammonia conversion rates and catalyst lifespan by ensuring uniform heating of the honeycomb structure, optimizing the decomposition reaction efficiency and extending the catalyst's operational life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024004704_05122024_PF_FP_ABST
    Figure JP2024004704_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a catalyst-carrying honeycomb structure capable of improving the conversion rate of ammonia and improving the lifespan of a catalyst. A catalyst-carrying honeycomb structure (1) comprises: a ceramic honeycomb structure (2); a catalyst layer (3) that is formed in a flow path (2a) of the honeycomb structure (2) and decomposes ammonia; and electrodes (4a, 4b) that are formed on side surfaces of the honeycomb structure (2). The honeycomb structure (2) is energized.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst-supporting honeycomb structure and manufacturing method thereof

[0001] The present invention relates to a honeycomb structure supporting a catalyst for decomposing ammonia and a method for manufacturing the same.

[0002] In light of the recent global warming, efforts are being made to create a hydrogen society that focuses on using hydrogen as a combustion source. Ammonia is attracting attention for the production of hydrogen. Ammonia is composed of hydrogen and nitrogen atoms, and CO is produced in the decomposition reaction of ammonia. 2 This is because no hydrogen is generated. Also, there is no need for hydrogen stations to supply hydrogen or hydrogen pressure vessels filled with hydrogen. For this reason, technology that decomposes ammonia to produce hydrogen and oxygen is beginning to be used in automotive fuel cells and industrial furnaces.

[0003] Patent Document 1 discloses an invention in which a catalyst for decomposing ammonia is supported on a metal honeycomb structure, and the ammonia is passed through a flow path in the honeycomb structure to decompose the ammonia and generate hydrogen and oxygen. The ammonia decomposition reaction is an endothermic reaction. In order to supply the heat required for the decomposition of ammonia, the invention described in Patent Document 1 has a heater that is in contact with the upstream side of the honeycomb structure and supplies heat to the honeycomb structure.

[0004] JP 2010-195642 A

[0005] However, in the invention described in Patent Document 1, the metal honeycomb structure supporting the catalyst is heated by contacting it with a heater, which means that the temperature distribution in the honeycomb structure cannot be made uniform, and there is a problem in that it is not possible to improve both the ammonia conversion rate and the catalyst life.

[0006] To explain this, in the ammonia decomposition reaction, increasing the reaction temperature can improve the ammonia conversion rate. On the other hand, increasing the reaction temperature causes the growth of catalyst fine particles, shortening the catalyst life. In the invention described in Patent Document 1, an attempt to improve the ammonia conversion rate shortens the life of the high-temperature part of the catalyst, while an attempt to extend the catalyst life reduces the ammonia conversion rate in the low-temperature part of the catalyst.

[0007] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a catalyst-supported honeycomb structure and a manufacturing method thereof that can achieve both improved ammonia conversion rate and improved catalyst life.

[0008] In order to solve the above problems, one aspect of the present invention is a catalyst-supported honeycomb structure that includes a ceramic honeycomb structure, a catalyst layer that decomposes ammonia and is formed in the flow paths of the honeycomb structure, and electrodes that are formed on the side surfaces of the honeycomb structure, and that passes electricity through the honeycomb structure.

[0009] Another aspect of the present invention is a method for manufacturing a catalyst-supported honeycomb structure, comprising the steps of: sintering a honeycomb molded body containing silicon carbide powder, silicon nitride powder, and carbon to produce a honeycomb structure; forming electrodes on the side surfaces of the honeycomb structure; and forming a catalyst layer that decomposes ammonia in the flow paths of the honeycomb structure, and passing electricity through the honeycomb structure.

[0010] According to the present invention, the honeycomb structure can be uniformly heated, so that it is possible to improve both the ammonia conversion rate and the catalyst life.

[0011] 7(a) is a graph showing the temperature changes at T1, T2, and T3 when a current of 5 A is passed through the honeycomb structure, and FIG. 7(b) shows a thermograph of the honeycomb structure when T2 = 165°C. FIG. 8(a) is a graph showing the temperature changes at T1, T2, and T3 when a current of 10 A is passed through the honeycomb structure, and FIG. 8(b) shows a thermograph of the honeycomb structure when T2 = 300°C. FIG. 9(a) is a graph showing the temperature changes at T1, T2, and T3 when a current of 20 A is passed through the honeycomb structure, and FIG. 9(b) shows a thermograph of the honeycomb structure when T2=400°C.

[0012] Hereinafter, a catalyst-supported honeycomb structure and a manufacturing method thereof according to an embodiment of the present invention will be described with reference to the drawings. However, the catalyst-supported honeycomb structure and a manufacturing method thereof according to the present invention can be embodied in various forms and are not limited to the embodiments described in this specification. This embodiment is provided with the intention that those skilled in the art will be able to fully understand the invention by fully disclosing the specification. (Catalyst-supported honeycomb structure)

[0013] Fig. 1 is an external perspective view of a catalyst-supported honeycomb structure according to one embodiment of the present invention. The catalyst-supported honeycomb structure 1 of this embodiment comprises a ceramic honeycomb structure 2, a catalyst layer 3 formed in flow channels 2a of the honeycomb structure 2, and a pair of electrodes 4a, 4b formed on the side surfaces of the honeycomb structure 2. The catalyst-supported honeycomb structure 1 is housed in a reaction vessel (not shown) that is equipped with a gas inlet and a gas outlet. The shape of the catalyst-supported honeycomb structure 1, the number of flow channels 2a, etc. are not limited, and may be cylindrical (see Fig. 4), oval, rectangular parallelepiped, etc. (see Fig. 1).

[0014] When ammonia is supplied to the gas inlet of the reaction vessel, the ammonia flows through the flow passages 2a of the honeycomb structure 2. When the ammonia flows through the flow passages 2a, the catalyst layer 3 decomposes the ammonia according to the reaction formula 1 to generate hydrogen and nitrogen. The generated hydrogen and nitrogen are discharged from the gas outlet of the reaction vessel. (Formula 1) 2NH 3 →N 2 +3H 2

[0015] Formula 1 is an endothermic reaction. In order to reduce the amount of heat absorbed, ammonia and air may be supplied to the gas inlet of the reaction vessel and flowed through the flow passage 2a of the honeycomb structure 2. When ammonia and air are flowed through the flow passage 2a, heat is generated by the catalytic reaction between ammonia and oxygen as shown in Formula 2. This heat can reduce the amount of heat absorbed. (Formula 2) NH 3 +3 / 4O 2 →1 / 2N 2 +3 / 2H 2 O (honeycomb structure)

[0016] As shown in Fig. 2, the honeycomb structure 2 has a plurality of cells 2a that form flow paths 2a for ammonia to flow, extending from the inlet end face to the outlet end face, porous partition walls 2b that define the plurality of cells 2a, and an outer peripheral wall 2c located on the outermost periphery. The shape of the honeycomb structure 2, the number of cells 2a, the thickness of the partition walls 2b, etc. are not limited and can be designed appropriately as needed. For example, the shape of the honeycomb structure 2 may be an elongated cylinder.

[0017] The honeycomb structure 2 is made of ceramics. The honeycomb structure 2 is electrically conductive. The honeycomb structure 2 contains silicon carbide as a main component and nitrogen as an impurity. The honeycomb structure 2 containing silicon carbide as a main component means that the honeycomb structure 2 contains silicon carbide in an amount of 90 mass% or more of the entire honeycomb structure.

[0018] The honeycomb structure 2 is produced by sintering a honeycomb molded body containing silicon carbide powder, silicon nitride powder, and carbon. The silicon carbide powder is used as aggregate for the honeycomb structure 2. The silicon nitride powder and carbon are used as binders to bind the silicon carbide powder together.

[0019] 3(a) shows a schematic diagram of the particles of the honeycomb molded body before sintering. Reference numeral 5 denotes silicon carbide powder, reference numeral 6 denotes silicon nitride powder, and reference numeral 7 denotes carbon. When the honeycomb molded body is sintered, silicon nitride and carbon react to synthesize silicon carbide, as shown in the following formula 3. (Formula 3) Si 3 N 4 +3C→3SiC+2N 2

[0020] As shown in Figure 3(b), the synthesized silicon carbide 8 bonds the silicon carbide powder 5 used as aggregate. The reaction temperature in formula 3 is lower than the softening point of the silicon carbide particles. By using silicon nitride powder 6 and carbon 7 as binders to bind the silicon carbide powder 5, grain growth of the silicon carbide powder 5 can be suppressed, and a fine and uniform pore size distribution can be achieved in the honeycomb structure 2.

[0021] The honeycomb structure 2 contains nitrogen derived from the silicon nitride powder as an impurity. Nitrogen functions as a dopant that contributes to electrical conduction, making the honeycomb structure 2 electrically conductive. When electricity is applied to the honeycomb structure 2, the honeycomb structure 2 generates heat. Since the honeycomb structure 2 has a fine and uniform pore size distribution, the honeycomb structure 2 is heated uniformly.

[0022] An example of a method for manufacturing the honeycomb structure 2 will be described below. First, a molding raw material is prepared by adding water, a binder, etc. to silicon carbide powder, silicon nitride powder, and carbon. The average particle size of the silicon carbide powder is 1 to 50 μm. The content of the silicon carbide powder relative to the silicon carbide powder, silicon nitride powder, and carbon is 20 to 70 mass %. The carbon is graphite, carbon black, etc. The molar ratio of silicon constituting the silicon nitride to carbon is in the range of 1.0 to 2.0.

[0023] The binder is methyl cellulose or the like. The binder content is 2 to 15 parts by mass when the total mass of the silicon carbide powder, silicon nitride powder, and carbon is 100 parts by mass. The water content is 20 to 30 parts by mass when the total mass of the silicon carbide powder, silicon nitride powder, and carbon is 100 parts by mass. In addition to the above raw materials, surfactants such as ethylene glycol, dextrin, fatty acid soap, and polyalcohol may be added.

[0024] Next, the obtained forming raw materials are kneaded to prepare a clay, and then the clay is extruded to prepare a honeycomb formed body. After drying the honeycomb formed body, the honeycomb formed body is sintered at a temperature of, for example, 1800°C to 2300°C in a non-oxidizing atmosphere that does not contain nitrogen, such as a vacuum or an inert gas, to prepare the honeycomb structure 2.

[0025] The honeycomb structure 2 may be mainly composed of a silicon-silicon carbide composite material. The silicon-silicon carbide composite material contains silicon carbide particles as aggregate and metallic silicon as a binder that binds the silicon carbide particles. (Electrode)

[0026] As shown in Fig. 1, a pair of electrodes 4a, 4b are formed on the side surfaces of the honeycomb structure 2. The electrodes 4a, 4b are strip-shaped and extend in the same direction as the cells 2a of the honeycomb structure 2. The electrodes 4a, 4b are arranged to face each other across the center of the honeycomb structure 2.

[0027] The electrodes 4a, 4b are made of a conductive material. The material of the electrodes 4a, 4b may be a metal, a conductive ceramic, a composite material combining a metal and an oxide ceramic, or the like. The metal may be silver, copper, iron, aluminum, tungsten, alloy steel, or the like. The conductive ceramic may be silicon carbide, chromium silicide, boron carbide, chromium boride, tantalum silicide, or the like. The oxide ceramic may be glass, cordierite, mullite, or the like.

[0028] An intermediate layer (not shown) having a lower thermal expansion coefficient than the electrodes 4a, 4b may be provided on the honeycomb structure 2 side of the electrodes 4a, 4b. The electrodes 4a, 4b have a higher thermal expansion coefficient than the honeycomb structure 2. By providing the intermediate layer, it is possible to reduce the difference in thermal expansion coefficient between the electrodes 4a, 4b and the honeycomb structure 2. The intermediate layer is made of a metal, oxide ceramics, or the like, similar to the electrodes 4a, 4b.

[0029] The intermediate layer and electrodes 4a, 4b are formed, for example, as follows: Metal powder and glass powder are mixed to prepare a ceramic raw material; A binder, a surfactant, and water are added to the ceramic raw material to prepare a paste for the intermediate layer; The paste for the intermediate layer is applied to the honeycomb structure 2 and dried to form a coating; The honeycomb structure 2 with the coating formed thereon is sintered to form the intermediate layer.

[0030] The same applies to the electrodes 4a, 4b formed on the intermediate layer. That is, metal powder and glass powder are mixed to prepare ceramic raw material. A binder, a surfactant, and water are added to the ceramic raw material to prepare a paste for the electrodes. The electrode paste is applied to the intermediate layer of the honeycomb structure 2 and dried to form a coating film. The honeycomb structure 2 with the coating film formed thereon is sintered to form the electrodes 4a, 4b. Here, the honeycomb molded body and the intermediate layer may be sintered simultaneously, or the honeycomb molded body, the intermediate layer, and the electrodes 4a, 4b may be sintered simultaneously.

[0031] The intermediate layer and the electrodes 4a, 4b may be formed by thermally spraying a thermal spray material onto the honeycomb structure 2. In this case, the thermal spray material preferably contains tungsten carbide as a main component and nickel. The nickel content of the thermal spray material is preferably 3 to 40 mass %, and the tungsten carbide content of the thermal spray material is preferably 60 to 90 mass %. (Catalyst Layer)

[0032] As shown in Fig. 1, a catalyst layer 3 is formed in each cell 2a of a honeycomb structure 2. The catalytically active species used in the catalyst layer 3 is not particularly limited as long as it decomposes ammonia into hydrogen. As the catalytically active species, at least one element selected from the group consisting of Groups 6, 7, 8, 9, 10, and 11 is selected. Examples of the catalytic metal include ruthenium, rhodium, palladium, and platinum.

[0033] The catalytically active species can be supported on a catalyst support made of an oxide containing at least one element selected from the group consisting of Al, Si, Ti, Zr, Group 1, Group 2, and Group 3 elements. The oxide may be a composite oxide containing two or more oxides. The oxide may also be a zeolite. Supporting the catalytically active species on a catalyst support made of such an oxide contributes to improving the dispersibility of the catalytically active species and improving the mechanical strength of the catalyst.

[0034] Conventional methods can be used to form the catalyst layer 3. For example, there can be used a method of wet-pulverizing catalytically active species to produce a slurry and coating the honeycomb structure 2 with the slurry, a method of wet-pulverizing a powder in which catalytically active species are supported on a catalyst carrier made of an oxide to produce a slurry and coating the honeycomb structure 2 with the slurry, a method of wet-pulverizing a catalyst carrier made of an oxide to produce a slurry, coating the honeycomb structure 2 with the slurry, and then wet-pulverizing the catalytically active species to produce a slurry and further coating the honeycomb structure 2 with the slurry, etc. (Support for Longer Lengths)

[0035] When the catalyst-supported honeycomb structure 1 is elongated in the gas flow direction, a plurality of catalyst-supported honeycomb structures 1-1, 1-2, and 1-3 are arranged in the gas flow direction, and insulating layers 9 are provided between the catalyst-supported honeycomb structures 1-1, 1-2, and 1-3, as shown in Fig. 4. Electrodes 4a and 4b are provided on the catalyst-supported honeycomb structures 1-1, 1-2, and 1-3 so that they can be individually energized. Electric wires 16a and 16b are connected to the electrodes 4a and 4b to supply power.

[0036] When the catalyst-supported honeycomb structure 1 is elongated in the radial direction (direction perpendicular to the gas flow), as shown in Fig. 5, a plurality of catalyst-supported honeycomb structures 1-4, 1-5, and 1-6 are arranged in the direction perpendicular to the gas flow, and an insulating layer 9 is provided between the catalyst-supported honeycomb structures 1-4, 1-5, and 1-6. Electrodes 4a and 4b are provided on the catalyst-supported honeycomb structures 1-4, 1-5, and 1-6 so that they can be individually energized. Electric wires 16a and 16b are connected to the electrodes 4a and 4b to supply power. Note that a plurality of catalyst-supported honeycomb structures may be arranged in the direction perpendicular to the gas flow, and a plurality of catalyst-supported honeycomb structures may also be arranged in the direction of the gas flow.

[0037] The catalyst type and the catalyst loading amount of the catalyst-supported honeycomb structures 1-1, 1-2, and 1-3 shown in FIG. 4 may be the same or at least one may be different. Similarly, the catalyst type and the catalyst loading amount of the catalyst-supported honeycomb structures 1-4, 1-5, and 1-6 shown in FIG. 5 may be the same or at least one may be different. When at least one of the catalyst type and the catalyst loading amount is different, the heating temperature (amount of heat) may be changed depending on the catalyst type and the catalyst loading amount. For example, a catalyst capable of oxidizing and decomposing ammonia may be used in the upstream catalyst-supported honeycomb structure 1-1 in FIG. 4, and a catalyst capable of decomposing ammonia may be used in the downstream catalyst-supported honeycomb structures 1-2 and 1-3, and the heating temperature of the downstream catalyst-supported honeycomb structures 1-2 and 1-3 may be higher than the heating temperature of the upstream catalyst-supported honeycomb structure 1-1.

[0038] The insulating layer 9 is a plate-shaped insulator such as silica or alumina, or an air layer (gap) provided between the catalyst-supporting honeycomb structures 1-1, 1-2, and 1-3. When a plate-shaped insulator is used, the plurality of honeycomb molded bodies and the plate-shaped insulator are degreased and fired to be integrated, and electrodes 4a and 4b are formed on each honeycomb structure 2. (Effects) The effects of the catalyst-supporting honeycomb structure 1 of this embodiment will be described below.

[0039] According to the catalyst-supporting honeycomb structure 1 of this embodiment, the honeycomb structure 2 can be uniformly heated, so that it is possible to improve both the ammonia conversion rate and the catalyst life.

[0040] Since the honeycomb structure 2 is mainly composed of silicon carbide and contains nitrogen, the honeycomb structure 2 can be heated more uniformly.

[0041] A plurality of catalyst-supported honeycomb structures 1-1, 1-2, and 1-3 are arranged in the gas flow direction, and insulating layers 9 are provided between the catalyst-supported honeycomb structures 1-1, 1-2, and 1-3. This allows uniform heating of the plurality of catalyst-supported honeycomb structures 1-1, 1-2, and 1-3 elongated in the gas flow direction. Similarly, a plurality of catalyst-supported honeycomb structures 1-4, 1-5, and 1-6 are arranged in a direction perpendicular to the gas flow, and insulating layers 9 are provided between the catalyst-supported honeycomb structures 1-4, 1-5, and 1-6. This allows uniform heating of the plurality of catalyst-supported honeycomb structures 1-4, 1-5, and 1-6 elongated in the direction perpendicular to the gas flow. Furthermore, electricity can be separately applied to each of the plurality of catalyst-supported honeycomb structures 1-1, 1-2, and 1-3 or 1-4, 1-5, and 1-6. (Example)

[0042] The honeycomb structure 2 shown in FIG. 6 was fabricated. A molding raw material was prepared by adding water, a binder, etc. to silicon carbide powder, silicon nitride powder, and carbon. The average particle size of the silicon carbide powder was 10 μm. The content of the silicon carbide powder relative to the silicon carbide powder, silicon nitride powder, and carbon was 50 mass %. Carbon black was used as the carbon. The molar ratio of silicon constituting the silicon nitride to carbon was 1.5.

[0043] Methyl cellulose was used as the binder. The binder content was 10 parts by mass when the total mass of the silicon carbide powder, silicon nitride powder, and carbon was 100 parts by mass. The water content was 25 parts by mass when the total mass of the silicon carbide powder, silicon nitride powder, and carbon was 100 parts by mass.

[0044] The obtained molding raw materials were mixed to prepare a clay, which was then extruded to prepare a honeycomb molded body. After drying the honeycomb molded body, the honeycomb molded body was sintered at a temperature of 2100°C in a nitrogen-free non-oxidizing atmosphere to prepare a honeycomb structure 2.

[0045] The size of the honeycomb structure 2 was 50 mm square x 50 mm long, the structure of the cells 2a was 50 cpsi / 25 mil, and the resistance of the honeycomb structure 2 was 0.5 Ωcm. The resistance was measured by a four-terminal method in accordance with JIS R 1650-2:2002. In addition, the nitrogen concentration of the honeycomb structure 2 was measured in accordance with JIS R 1616:2007, and the presence of nitrogen was confirmed.

[0046] Carbon felts 11a and 11b were sandwiched between the honeycomb structure 2 and the electrodes 4a and 4b, and the electrodes 4a and 4b were pressed against each other from above and below. Constant currents of 5 A, 10 A, and 20 A were supplied to the honeycomb structure 2, and the temperatures T1, T2, and T3 of the lower, middle, and upper parts of the honeycomb structure 2 were measured.

[0047] As shown in Fig. 7(a), when a current of 5 A was supplied to the honeycomb structure 2, the temperatures T1, T2, and T3 increased with time, but were approximately the same value. Moreover, as shown in the thermograph at T2 = 165°C in Fig. 7(b), the entire honeycomb structure 2 was heated uniformly.

[0048] 8(a) and 8(b), when a current of 10 A was passed through the honeycomb structure 2, the results were substantially the same as when a current of 5 A was passed through the honeycomb structure 2. Note that FIG. 8(b) is a thermograph when T2=300°C.

[0049] As shown in Figure 9(a), when a constant current of 20 A was passed through the honeycomb structure 2, the influence of the contact resistance between the electrodes 4a, 4b, the carbon felts 11a, 11b, and the honeycomb structure 2 became large, resulting in slight variations in temperatures T1, T2, and T3. However, even in this case, as shown in the thermograph at T2 = 400°C in Figure 9(b), the entire honeycomb structure 2 could be heated almost uniformly. Because uniform heating is possible, the ammonia conversion rate can be improved when a catalyst is supported.

[0050] This specification is based on Japanese Patent Application No. 2023-087328, filed on May 26, 2023, the entire contents of which are incorporated herein by reference.

[0051] REFERENCE SIGNS LIST 1... catalyst-supporting honeycomb structure 2... honeycomb structure 3... catalyst layer 4a, 4b... electrodes 9... insulating layer

Claims

1. A catalyst-supporting honeycomb structure comprising: a ceramic honeycomb structure; a catalyst layer formed in a flow path of the honeycomb structure for decomposing ammonia; and electrodes formed on a side surface of the honeycomb structure, wherein electricity is passed through the honeycomb structure.

2. The catalyst-supporting honeycomb structure according to claim 1, characterized in that said honeycomb structure is composed mainly of silicon carbide and contains nitrogen.

3. A catalyst-supporting honeycomb structure as described in claim 1 or 2, characterized in that a plurality of said catalyst-supporting honeycomb structures are arranged in the gas flow direction and / or perpendicular to the gas flow, and an insulating layer is provided between said catalyst-supporting honeycomb structures.

4. A method for manufacturing a catalyst-loaded honeycomb structure, comprising the steps of: sintering a honeycomb formed body containing silicon carbide powder, silicon nitride powder, and carbon to produce a honeycomb structure; forming electrodes on the side surfaces of the honeycomb structure; and forming a catalyst layer for decomposing ammonia in the flow paths of the honeycomb structure, wherein electricity is passed through the honeycomb structure.

Citation Information

Patent Citations

  • Hydrogen generator

    JP2010195642A

  • Aqueous ink, ink cartridge, and inkjet recording method

    JP2023087328A

  • Electric heating honeycomb body

    JP1995096203A

  • Ammonia-decomposing catalyst and ammonia-decomposing method using the same

    JP2012005926A

  • Vehicle cabin purification system, method of controlling vehicle cabin purification system, program and storage medium

    JP2023047123A