Flame-retardant non-woven fabric and vehicle interior material

The combination of modacrylic fibers with magnesium compounds and silica-containing regenerated cellulose fibers in a specific ratio addresses the limitations of conventional flame-retardant nonwoven fabrics, achieving superior flame retardancy, texture, and sound insulation while eliminating antimony-related concerns.

WO2024247409A1PCT designated stage expired Publication Date: 2024-12-05KANEKA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007137
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-21
Filing Date
2024-02-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional flame-retardant nonwoven fabrics for vehicle interiors, particularly those containing antimony-containing modacrylic fibers, raise environmental and health concerns due to elution and discharge issues, and often compromise on texture and flame retardancy, failing to meet high standards like the V-0 standard in UL94 vertical flammability tests.

Method used

A flame-retardant nonwoven fabric comprising modacrylic fibers with a magnesium compound and regenerated cellulose fibers containing silica, with a specific blending ratio of 15-45% modacrylic fibers and 55-85% regenerated cellulose fibers, and a magnesium compound content of 0.75% or more, which enhances both texture and flame retardancy while avoiding antimony compounds.

Benefits of technology

The solution achieves high flame retardancy meeting the V-0 standard in UL94 vertical flammability tests, improves texture, and provides excellent sound-insulating properties, reducing environmental and health concerns associated with antimony compounds, while being cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

One or more embodiments of the present invention relate to a flame-retardant non-woven fabric that includes a modacrylic fiber A and a regenerated cellulose fiber B, wherein the modacrylic fiber A contains a magnesium compound, the regenerated cellulose fiber B contains silica, the flame-retardant non-woven fabric contains 15-45 mass% of the modacrylic fiber A and 55–85 mass% of the regenerated cellulose fiber B, the flame-retardant non-woven fabric contains 0.75 mass% or more of a magnesium compound derived from the modacrylic fiber A, the basis weight of the flame-retardant non-woven fabric is 80 g / m2 or greater, and the flame-retardant non-woven fabric satisfies the V-0 standard of the UL94 vertical flammability test.
Need to check novelty before this filing date? Find Prior Art

Description

Flame-retardant nonwoven fabric and vehicle interior materials

[0001] The present invention relates to a flame-retardant nonwoven fabric containing modacrylic fibers and regenerated cellulose fibers, and to a vehicle interior material.

[0002] From the viewpoint of safety, nonwoven fabrics having flame retardancy are used for interior materials such as seats and their covering materials for vehicles such as aircraft, automobiles, railroad cars, and ships. For example, Patent Document 1 proposes a flame-retardant nonwoven fabric having a three-layer structure in which halogen- and antimony-containing modacrylic fibers are used in the back and middle layers as a nonwoven fabric for use in interior materials such as seat covering materials.

[0003] JP 2009-299199 A

[0004] However, while Patent Document 1 uses antimony-containing modacrylic fibers, in recent years there have been concerns about the impact of antimony compounds eluted or emitted into the environment and the human body, and improvements are being sought. Furthermore, interior materials such as vehicle seats are often in contact with the human body, and therefore excellent texture is required.

[0005] In order to solve the above-mentioned problems of the prior art, the present invention provides a flame-retardant nonwoven fabric that has a good texture and high flame retardancy in a vertical combustion test, and a vehicle interior material containing the same.

[0006] One or more embodiments of the present invention are a flame-retardant nonwoven fabric comprising modacrylic fiber A and regenerated cellulose fiber B, wherein the modacrylic fiber A contains a magnesium compound and the regenerated cellulose fiber B contains silica, the flame-retardant nonwoven fabric comprises 15 to 45 mass% of the modacrylic fiber A and 55 to 85 mass% of the regenerated cellulose fiber B, the flame-retardant nonwoven fabric contains 0.75 mass% or more of the magnesium compound derived from the modacrylic fiber A, and the basis weight of the flame-retardant nonwoven fabric is 80 g / m 2 The flame-retardant nonwoven fabric satisfies the V-0 standard of the UL94 vertical flame test.

[0007] One or more embodiments of the present invention relate to a vehicle interior material comprising the flame-retardant nonwoven fabric.

[0008] According to the present invention, it is possible to provide a flame-retardant nonwoven fabric that has a good texture and high flame retardancy in a vertical combustion test, and a vehicle interior material containing the same.

[0009] The inventors of the present invention conducted extensive research to improve the flame retardancy and texture of nonwoven fabrics used in vehicle interior materials. As a result, they discovered that using modacrylic fiber A containing a magnesium compound in combination with regenerated cellulose fiber B containing silica improves the texture of the nonwoven fabric, and that by adjusting the blending ratio of modacrylic fiber A and regenerated cellulose fiber B in the nonwoven fabric and the content of the magnesium compound derived from modacrylic fiber A to a predetermined amount, the nonwoven fabric exhibits high flame retardancy, meeting the highest level of V-0 in the UL94 vertical flame resistance test. This effect is unique and cannot be achieved by using modacrylic fiber containing a magnesium compound in combination with other flame-retardant fibers, such as regenerated cellulose fiber or polyester fiber containing a phosphorus-based flame retardant. The reason for this is speculative and does not limit the present invention, but it is speculated that the synergistic effect of the magnesium compound derived from modacrylic fiber A and the silica derived from regenerated cellulose fiber B improves shrinkage resistance, resulting in high flame retardancy. In particular, the flame-retardant nonwoven fabric described above has excellent soundproofing or sound-absorbing properties and can be suitably used as a flame-retardant soundproofing material or a flame-retardant sound-absorbing material. Furthermore, in one or more embodiments of the present invention, the flame-retardant nonwoven fabric and modacrylic fiber A are substantially free of antimony compounds, thereby reducing concerns about the impact of antimony compounds on the environment and human body due to elution or emission, and also reducing costs. In this specification, "substantially free of antimony compounds" means that antimony compounds are not intentionally added to the fiber or nonwoven fabric as a flame retardant. For example, when antimony compounds are contained as impurities (e.g., 0.001% by mass or less), this is considered to be "substantially free of antimony compounds."

[0010] In this specification, when a numerical range is indicated with "to", the numerical range includes both end values ​​(upper and lower limits). For example, a numerical range of "A to B" includes both end values ​​A and B, and is the same range as "A or more and B or less". Any number within that range and any range included within that range are specifically disclosed. In addition, when multiple numerical ranges are described in this specification, they are intended to include numerical ranges obtained by appropriately combining the upper and lower limits of different numerical ranges. In addition, when multiple upper and lower limits are described separately for a numerical range, they are intended to include numerical ranges obtained by appropriately combining each of the upper and lower limits.

[0011] The flame-retardant nonwoven fabric of one or more embodiments of the present invention comprises modacrylic fibers A and regenerated cellulose fibers B.

[0012] (Modacrylic Fiber A) Modacrylic Fiber A contains a modacrylic polymer and a magnesium compound, but is substantially free of antimony compounds. Specifically, Modacrylic Fiber A contains a magnesium compound within the fiber. The content of the magnesium compound in Modacrylic Fiber A is not particularly limited, as long as the content of the magnesium compound in the flame-retardant nonwoven fabric satisfies the range described below. For example, the content is preferably 2 to 25 parts by mass, more preferably 3 to 20 parts by mass, even more preferably 4 to 15 parts by mass, even more preferably 4 to 10 parts by mass, and even more preferably 4 to 8 parts by mass, per 100 parts by mass of the modacrylic polymer. When the magnesium compound is 2 parts by mass or more, the flame retardancy of the flame-retardant nonwoven fabric containing Modacrylic Fiber A is improved. When the magnesium compound is 25 parts by mass or less, static electricity generation in Modacrylic Fiber A during carding is suppressed, improving processability, particularly mass productivity.

[0013] Examples of magnesium compounds include magnesium oxide, magnesium peroxide, magnesium hydroxide, magnesium fluoride, magnesium chloride, magnesium bromide, magnesium iodide, magnesium hydride, magnesium diboride, magnesium nitride, magnesium sulfide, magnesium carbonate, calcium magnesium carbonate, magnesium nitrate, magnesium sulfate, magnesium sulfite, magnesium perchlorate, trimagnesium phosphate, magnesium permanganate, and magnesium phosphate. Among these, from the viewpoint of ease of handling, one or more selected from the group consisting of magnesium oxide and magnesium hydroxide are preferably used, and from the viewpoint of further improving processability, magnesium hydroxide is preferably used.

[0014] The magnesium hydroxide is not particularly limited, but examples include powders obtained by crushing natural bruce ore, powders obtained by neutralizing an aqueous magnesium salt solution with an alkali, powders obtained by treating magnesium hydroxide particles with phosphates, borates, etc., and powders obtained by gradually hydrating magnesium oxide to produce magnesium hydroxide. Furthermore, magnesium hydroxide may have a coating layer formed by adsorbing an adsorbable substance around the magnesium hydroxide particles or by surface treatment with a surface treatment agent. Among these, magnesium hydroxide having a coating layer formed by surface treatment with a silane coupling agent is preferred from the perspective of static electricity suppression. While the reason why surface treatment with a silane coupling agent improves static electricity suppression is only speculative, it is thought to be as follows: It is believed that silane coupling treatment of the magnesium hydroxide particle surface improves the compatibility between modacrylic fiber and the silane coupling-treated magnesium hydroxide, resulting in static electricity suppression. Furthermore, if an oil agent is applied to the fiber surface to improve processability, the oil agent's effect is fully extended to the surface of the magnesium hydroxide particles, significantly improving processability. The type of silane coupling agent is preferably one that improves compatibility with the modacrylic polymer, and may be either a crosslinked or non-crosslinked type, with no particular limitation. The magnesium hydroxide surface-treated with a silane coupling agent is not particularly limited, but may be, for example, a commercially available product such as Kisuma (registered trademark) 5P or Kisuma (registered trademark) 5L manufactured by Kyowa Chemical Industry Co., Ltd.

[0015] The average particle size of the magnesium compound, represented by the median diameter (D50), is preferably 0.3 to 3.0 μm, more preferably 1.0 to 2.5 μm. When the average particle size is 0.3 μm or more, the surface area of ​​the magnesium compound particles does not increase too much, suppressing static electricity generation during the fiber processing step and facilitating processing. When the average particle size is 3.0 μm or less, clogging of the spinneret does not occur during the spinning step, resulting in good spinnability. Herein, the average particle size of the magnesium compound can be measured, for example, by laser diffraction / scattering in the case of a powder, or by laser diffraction / scattering or dynamic light scattering in the case of a dispersion (dispersion liquid) in water or an organic solvent. The average particle size of the magnesium compound in the fiber can also be confirmed, for example, by measuring the particle sizes of 100 magnesium compound particles in the fiber using a microscope and calculating the arithmetic mean diameter.

[0016] The modacrylic polymer preferably contains 30 to 85% by mass of structural units derived from acrylonitrile, 15 to 70% by mass of structural units derived from halogen-containing monomers, and 0 to 5% by mass of structural units derived from other copolymerizable vinyl monomers; more preferably contains 35 to 80% by mass of structural units derived from acrylonitrile, 20 to 65% by mass of structural units derived from halogen-containing monomers, and 0 to 5% by mass of structural units derived from other copolymerizable vinyl monomers; and even more preferably contains 40 to 70% by mass of structural units derived from acrylonitrile, 30 to 60% by mass of structural units derived from halogen-containing monomers, and 0 to 5% by mass of structural units derived from other copolymerizable vinyl monomers.

[0017] The halogen-containing monomer is preferably one or more selected from the group consisting of halogen-containing vinyl monomers and halogen-containing vinylidene monomers. Examples of halogen-containing vinyl monomers include vinyl chloride and vinyl bromide, and examples of halogen-containing vinylidene monomers include vinylidene chloride and vinylidene bromide. From the viewpoints of improving flame retardancy and suppressing coloration of the modacrylic polymer, the halogen-containing monomer preferably includes vinyl chloride. These halogen-containing monomers may be used alone or in combination of two or more.

[0018] Other copolymerizable vinyl monomers include, but are not limited to, unsaturated carboxylic acids and their salts, such as acrylic acid and methacrylic acid; methacrylic acid esters, such as methyl methacrylate; esters of unsaturated carboxylic acids, such as glycidyl methacrylate; vinyl esters, such as vinyl acetate and vinyl butyrate; and sulfonic acid group-containing vinyl monomers. From the viewpoint of dyeability, sulfonic acid group-containing vinyl monomers are preferred. Examples of sulfonic acid group-containing vinyl monomers that can be used include allyl sulfonic acid, methallyl sulfonic acid, styrene sulfonic acid, isoprene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, and metal salts and amine salts thereof, such as sodium salts. The sulfonic acid group-containing vinyl monomers may be used alone or in combination of two or more. The sulfonic acid group-containing vinyl monomer is used as needed, but if the content of structural units derived from the sulfonic acid group-containing vinyl monomer in the modacrylic polymer is 3% by mass or less, the production stability in the spinning step will be superior.

[0019] The modacrylic polymer preferably contains 30 to 85% by mass of structural units derived from acrylonitrile, 15 to 70% by mass of structural units derived from a halogen-containing monomer, and 0 to 3% by mass of structural units derived from a sulfonic acid group-containing vinyl monomer, and more preferably contains 35 to 80% by mass of structural units derived from acrylonitrile, 19.5 to 64.5% by mass of structural units derived from a halogen-containing monomer, and 0.5 to 3% by mass of structural units derived from a sulfonic acid group-containing vinyl monomer.

[0020] The modacrylic polymer can be obtained by known polymerization methods such as bulk polymerization, suspension polymerization, emulsion polymerization, and solution polymerization, among which suspension polymerization, emulsion polymerization, and solution polymerization are preferred from an industrial viewpoint.

[0021] Modacrylic fiber A may contain 80 to 98% by mass of modacrylic polymer and 2 to 20% by mass of magnesium, 83 to 97% by mass of modacrylic polymer and 3 to 17% by mass of magnesium, 85 to 96% by mass of modacrylic polymer and 4 to 15% by mass of magnesium, or 87 to 96% by mass of modacrylic polymer and 4 to 13% by mass of magnesium. Modacrylic fiber A may also contain other additives, such as antistatic agents, coloring inhibitors, light resistance improvers, whiteness improvers, devitrification inhibitors, and colorants, as needed, within the range that does not impair the effects of the present invention. The amount of other additives may be 5 parts by mass or less, 3 parts by mass or less, or 1 part by mass or less, per 100 parts by mass of modacrylic polymer.

[0022] The cross-sectional shape of the modacrylic fiber A is not particularly limited, and may be, for example, circular or irregular (non-circular) such as a dog-bone shape.

[0023] Modacrylic fiber A can be produced by wet spinning in the same manner as for ordinary modacrylic fibers, except that a spinning solution containing, but not limited to, a modacrylic polymer, a magnesium compound, and, if necessary, other additives is used. In wet spinning, for example, a resin solution in which a modacrylic polymer is dissolved in a solvent is mixed with a magnesium compound (and, if necessary, other additives), and the resulting spinning solution is extruded through a nozzle into a coagulation bath to coagulate it. The resulting solution is then washed with water, dried, stretched, heat-treated, and cut to obtain modacrylic fiber A. The solvent is not particularly limited, and examples thereof include organic solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, acetone, and dimethyl sulfoxide, as well as inorganic solvents such as an aqueous rhodanide solution and an aqueous nitric acid solution. The nozzle hole may be circular.

[0024] The single fiber fineness of the modacrylic fiber A is not particularly limited, but from the viewpoints of strength and sound absorption coefficient, it is preferably 0.5 to 20 dtex, more preferably 0.6 to 15 dtex, even more preferably 0.7 to 10 dtex, still more preferably 0.8 to 8 dtex, even more preferably 0.9 to 5 dtex, and particularly preferably 1 to 3 dtex. The fiber length of the modacrylic fiber A is also not particularly limited, but from the viewpoint of strength, it is preferably 38 to 127 mm, more preferably 38 to 76 mm. The modacrylic fiber A may be used singly or in combination of two or more types.

[0025] The regenerated cellulose fiber B is not particularly limited as long as it is a regenerated cellulose fiber containing silica. Examples of regenerated cellulose fibers include rayon fiber, cupra, and lyocell. As the regenerated cellulose fiber B, silica-containing rayon fiber is preferably used from the viewpoints of ease of dyeing, flame retardancy, cost, and availability. From the viewpoint of washing durability, silica-containing regenerated cellulose fiber is preferably one containing silica inside the fiber. As silica-containing rayon fiber containing silica inside the fiber, commercially available products such as "Silica Rayon" manufactured by China Hailong Fiber Co., Ltd. and "FR CORONA (registered trademark)" manufactured by Daiwabo Rayon Co., Ltd. may be used. The regenerated cellulose fiber B may be used alone or in combination of two or more types.

[0026] From the viewpoint of flame retardancy, the regenerated cellulose fiber B preferably contains 10% by mass or more of silica, more preferably 13% by mass or more, and even more preferably 15% by mass or more. From the viewpoint of fiber strength and nonwoven fabric strength, the regenerated cellulose fiber B preferably contains 30% by mass or less of silica, more preferably 25% by mass or less, and even more preferably 20% by mass or less. Specifically, the regenerated cellulose fiber B may contain 10 to 30% by mass, 13 to 25% by mass, or 15 to 20% by mass of silica.

[0027] The single fiber fineness of the regenerated cellulose fiber B is not particularly limited, but from the viewpoint of strength and sound absorption coefficient, it is preferably 0.5 to 20 dtex, more preferably 0.6 to 15 dtex, even more preferably 0.7 to 10 dtex, still more preferably 0.8 to 8 dtex, even more preferably 0.9 to 5 dtex, and particularly preferably 1 to 3 dtex. The fiber length of the regenerated cellulose fiber B is not particularly limited, but from the viewpoint of strength, it is preferably 38 to 127 mm, more preferably 38 to 76 mm.

[0028] The flame-retardant nonwoven fabric contains 15 to 45% by mass of modacrylic fiber A and 55 to 85% by mass of regenerated cellulose fiber B. If the modacrylic fiber A is less than 15% by mass or the regenerated cellulose fiber B is less than 55% by mass, the flame retardancy is poor and the fabric does not meet the V-0 standard in the UL94 vertical flame test. The flame-retardant nonwoven fabric preferably contains 18 to 42% by mass of modacrylic fiber A and 58 to 82% by mass of regenerated cellulose fiber B, and more preferably contains 20 to 40% by mass of modacrylic fiber A and 60 to 80% by mass of regenerated cellulose fiber B.

[0029] The flame-retardant nonwoven fabric contains 0.75% by mass or more of a magnesium compound derived from modacrylic fiber A. If the magnesium compound content is less than 0.75% by mass, the flame retardancy will be poor and the fabric will not meet the V-0 standard in the UL94 vertical flame resistance test. The flame-retardant nonwoven fabric preferably contains 0.80% by mass or more of a magnesium compound derived from modacrylic fiber A, more preferably 0.85% by mass or more, even more preferably 0.90% by mass or more, and particularly preferably 0.95% by mass or more. The upper limit of the magnesium compound content in the flame-retardant nonwoven fabric is not particularly limited, but from the viewpoints of suppressing static electricity during card passage and improving productivity, particularly mass productivity, it is preferably 6.0% by mass or less, more preferably 5.0% by mass or less, even more preferably 4.5% by mass or less, even more preferably 4.0% by mass or less, and even more preferably 3.5% by mass or less. More specifically, the flame-retardant nonwoven fabric may contain 0.75 to 6.0 mass%, 0.80 to 5.0 mass%, 0.85 to 4.5 mass%, 0.90 to 4.0 mass%, or 0.95 to 3.5 mass% of the magnesium compound derived from modacrylic fiber A.

[0030] The content of magnesium compounds in modacrylic fibers or flame-retardant nonwoven fabrics can be determined by subjecting the modacrylic fibers or flame-retardant nonwoven fabrics to X-ray fluorescence analysis. The mass of regenerated cellulose fibers B contained in a flame-retardant nonwoven fabric can be determined by immersing the nonwoven fabric in an organic solvent such as dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), or N,N-dimethylacetamide (DMAc), heating the nonwoven fabric to dissolve the modacrylic fibers B, and extracting the remaining regenerated cellulose fibers B.

[0031] The flame-retardant nonwoven fabric is not particularly limited, but from the viewpoint of further enhancing flame retardancy and improving strength, it preferably contains 7.5 to 20 mass %, and more preferably 8.0 to 15 mass %, of silica derived from regenerated cellulose fiber B. The silica content in regenerated cellulose fiber B or the flame-retardant nonwoven fabric can be measured by SEM-EDS analysis.

[0032] The flame-retardant nonwoven fabric may contain other fibers as long as the purpose and effects of the present invention are not impaired. Examples of other fibers include natural fibers and chemical fibers other than modacrylic fiber A and regenerated cellulose fiber B. Examples of natural fibers include natural animal fibers such as wool fiber, cashmere fiber, and silk fiber. Examples of chemical fibers include polyester fibers (such as polyethylene terephthalate fibers and polyethylene naphthalate fibers), aramid fibers, acrylic fibers, polyvinyl chloride fibers, polyvinylidene chloride fibers, polyethylene fibers, polyurethane fibers, and polyimide fibers. The flame-retardant nonwoven fabric may contain up to 10% by mass of other fibers, up to 8% by mass, or up to 1% by mass.

[0033] The single fiber fineness of the other fibers is not particularly limited, but from the viewpoint of strength and sound absorption coefficient, it is preferably 0.5 to 20 dtex, more preferably 0.6 to 15 dtex, even more preferably 0.7 to 10 dtex, still more preferably 0.8 to 8 dtex, still more preferably 0.9 to 5 dtex, and particularly preferably 1 to 3 dtex. The fiber length of the other fibers is not particularly limited, but from the viewpoint of strength, it is preferably 38 to 127 mm, more preferably 38 to 76 mm.

[0034] The flame-retardant nonwoven fabric has a basis weight of 80 g / m 2 The basis weight is 80 g / m 2 If the weight is less than 85 g / m, the flame retardancy is poor and the standard of V-0 in the UL94 vertical flame resistance test cannot be met. 2 From the viewpoint of texture and cost, the weight per unit area of ​​the flame-retardant nonwoven fabric is preferably 350 g / m or more. 2 Preferably, the weight is 300 g / m or less. 2 More preferably, it is 250 g / m or less. 2 More preferably, it is 230 g / m or less. 2 More specifically, the basis weight of the flame-retardant nonwoven fabric is 80 to 350 g / m 2 , 80-300g / m 2 , 85-250g / m2 , or 85 to 230 g / m 2 That's fine too.

[0035] The thickness of the flame-retardant nonwoven fabric is not particularly limited, but when it is used as a sheet for vehicle interior materials such as soundproofing materials and ceiling materials, it is preferably 0.5 to 6 mm, and more preferably 1 to 5 mm.

[0036] The bulk density of the flame-retardant nonwoven fabric is not particularly limited, but from the viewpoint of lightness and sound absorption, for example, it is preferably 0.01 to 0.10 g / cm 3 is preferably 0.015 to 0.08 g / cm 3 More preferably, it is 0.018 to 0.07 g / cm 3 More preferably, it is 0.02 to 0.06 g / cm 3 It is even more preferred that:

[0037] The flame-retardant nonwoven fabric is not particularly limited, but examples thereof include carded nonwoven fabrics, air-laid nonwoven fabrics, thermally bonded nonwoven fabrics, chemically bonded nonwoven fabrics, needle-punched nonwoven fabrics, hydroentangled nonwoven fabrics, and stitch-bonded nonwoven fabrics. From the viewpoint of cost, it is preferable to use one or more selected from the group consisting of thermally bonded nonwoven fabrics and needle-punched nonwoven fabrics. From the viewpoint of further enhancing flame retardancy, needle-punched nonwoven fabrics are more preferable. Furthermore, the flame-retardant nonwoven fabric may have a uniform structure in the thickness, width, and length directions, a clearly laminated structure, or an indefinitely laminated structure. In the case of a laminated structure, it is preferable that each layer contains modacrylic fiber A and regenerated cellulose fiber B. From the viewpoint of breathability and flexibility, a single-layer nonwoven fabric is preferable.

[0038] The flame-retardant nonwoven fabric has excellent flame retardancy and satisfies the V-0 standard in the UL94 vertical flame test. Preferably, in the UL94 vertical flame test, the burning time of each test piece after both the first and second contact with a flame is 5 seconds or less, the total burning time after 10 contacts with a flame for five test pieces is 25 seconds or less, and the total burning time and glowing time after the second contact with a flame is 30 seconds or less; more preferably, in the UL94 vertical flame test, the burning time of each test piece after both the first and second contact with a flame is 0 seconds, the total burning time after 10 contacts with a flame for five test pieces is 0 seconds, and the total burning time and glowing time after the second contact with a flame is 0 seconds.

[0039] The flame-retardant nonwoven fabric has excellent sound absorption properties, and the normal incident sound absorption coefficient measured in accordance with JIS A 1405-2:2007 is preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, even more preferably 85% or more, and even more preferably 90% or more in a thickness range of 20 to 30 mm and a frequency range of 2500 to 6500 Hz. A sound absorption coefficient of 70% or more in the frequency range of 2500 to 6500 Hz can reduce noise in the frequency range of 2500 to 6500 Hz, and a sound absorption coefficient of 80% or more means that noise in the frequency range of 2500 to 6500 Hz is hardly perceived. The flame-retardant nonwoven fabric also has excellent sound absorption properties, and the normal incident sound absorption coefficient measured in accordance with JIS A 1405-2:2007 is preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, even more preferably 85% or more, and even more preferably 90% or more in a thickness range of 20 to 30 mm and at frequencies of 2500 Hz, 3500 Hz, 4500 Hz, 5500 Hz, and 6500 Hz.

[0040] In one or more embodiments of the present invention, the flame-retardant nonwoven fabric can be used as a covering material for interior materials such as seats, ceilings, and floors of vehicles such as aircraft, automobiles, railroad vehicles, and ships, or as an accent material for doors, and is particularly suitable for use as a covering material for vehicle interior materials such as automobiles and railroad vehicles. In particular, the flame-retardant nonwoven fabric has excellent flame retardancy and sound absorption properties, and is therefore particularly suitable for use as a flame-retardant soundproofing material or flame-retardant sound-absorbing material for vehicles such as automobiles and railroad vehicles. More specifically, for example, the flame-retardant nonwoven fabric may be disposed as a covering material on the surface of a foam such as urethane, and used as a flame-retardant soundproofing material or flame-retardant sound-absorbing material for vehicles.

[0041] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0042] The measurement and evaluation methods used in the examples and comparative examples are as follows.

[0043] (Silica Content) 5 g of silica-containing fiber (raw cotton) was analyzed using SEM-EDS analysis (tabletop scanning electron microscope and energy dispersive X-ray analyzer JCM-6000PLUS, manufactured by JEOL Ltd.) under the following conditions, and the silica content was determined from the approximate mass of elements. Measurement conditions: Acceleration voltage: 15.0 kV, PHA mode: T3, Energy range: 0 to 20 keV

[0044] (Average Particle Diameter) The average particle diameter (D50) of the compound was measured by a laser diffraction / scattering method.

[0045] (Static electricity when passing through a card) In the production of a nonwoven fabric, the amount of static electricity generated in the fibers when passing through a card was measured using a static electricity measuring device (manufactured by Simco Japan Co., Ltd., model number "FMX-003").

[0046] (Basis Weight) A sample cut into a 10 cm square from the nonwoven fabric was used, and the mass of the sample was measured using a weighing scale (personal top-pan electronic balance EX-120G, manufactured by A&D Co., Ltd.), and the basis weight (g / m) was calculated based on the mass and area of ​​the sample. 2 ) was calculated.

[0047] (Thickness) The thickness of the nonwoven fabric was measured with a vernier caliper (M-shaped standard vernier caliper, manufactured by Mitutoyo Corporation).

[0048] (Bulk density) Based on the basis weight and thickness of the nonwoven fabric, the bulk density (g / cm 3 ) was calculated.

[0049] (Flame Retardancy) A UL94 vertical flame resistance test was carried out, and the flame retardancy was evaluated based on the criteria shown in the following Table 1. The number of test pieces for each nonwoven fabric was five.

[0050] (Sound absorption coefficient) The normal incidence sound absorption coefficient was measured in accordance with JIS A 1405-2:2007 "Measurement of sound absorption coefficient and impedance using an acoustic tube - Part 2: Transfer function method." Four circular test pieces with a diameter of 29 mm were taken from the nonwoven fabric and stacked in the thickness direction to form the measurement sample. The test equipment used was a normal incidence sound absorption coefficient measuring instrument (model DS-2000 series) manufactured by Ono Sokki Co., Ltd. The measurement was started after the measurement sample was placed in a holder with a sample thickness of 20 mm. The sound absorption coefficient can be measured every 10 Hz. Of the obtained sound absorption coefficients, the values ​​at frequencies of 2500 Hz, 3500 Hz, 4500 Hz, 5500 Hz, and 6500 Hz, as well as the minimum and maximum values ​​in the range of 2500 to 6500 Hz, were used.

[0051]

[0052] (Production Example 1) A modacrylic polymer consisting of 49.5% by mass of structural units derived from acrylonitrile, 49.5% by mass of structural units derived from vinyl chloride, and 1.0% by mass of structural units derived from sodium p-styrenesulfonate was dissolved in acetone to a resin concentration of 30% by mass. A magnesium hydroxide dispersion (concentration: 30% by mass) was added to the resulting modacrylic polymer solution to a ratio of 5 parts by mass of magnesium hydroxide per 100 parts by mass of the modacrylic polymer to obtain a spinning solution. The magnesium hydroxide dispersion was prepared by adding magnesium hydroxide (manufactured by Kyowa Chemical Industry Co., Ltd., product name "Kisuma (registered trademark) 5P") to acetone and uniformly dispersing it. The magnesium hydroxide dispersion had an average particle size of 2.0 μm. The obtained spinning solution was extruded into an aqueous acetone solution (concentration: 50% by mass) using a nozzle (hole shape: circular) to coagulate, then washed with water and dried at 120°C. After drying, the fiber was stretched three times, further heat-treated at 145°C for 5 minutes, and cut to obtain a modacrylic fiber. The obtained modacrylic fiber had a single fiber fineness of 2.2 dtex and a cut length of 51 mm.

[0053] (Production Example 2) A modacrylic fiber was obtained in the same manner as in Production Example 1, except that a spinning solution obtained by adding a dispersion of magnesium hydroxide (concentration: 30% by mass) to a modacrylic polymer solution so that the magnesium hydroxide was 10 parts by mass per 100 parts by mass of the modacrylic polymer was used. The obtained modacrylic fiber had a single fiber fineness of 1.7 dtex and a cut length of 51 mm.

[0054] (Production Example 3) A modacrylic fiber was obtained in the same manner as in Production Example 1, except that a spinning solution obtained by adding a magnesium hydroxide dispersion (concentration: 30% by mass) to a modacrylic polymer solution so that the magnesium hydroxide was 20 parts by mass per 100 parts by mass of the modacrylic polymer was used. The obtained modacrylic fiber had a single fiber fineness of 1.7 dtex and a cut length of 51 mm.

[0055] (Production Example 4) A modacrylic fiber was obtained in the same manner as in Production Example 1, except that a dispersion of magnesium oxide (manufactured by Kyowa Chemical Industry Co., Ltd., product name "500-04R") (average particle size of magnesium oxide: 2.0 μm) was used instead of the dispersion of magnesium hydroxide. The obtained modacrylic fiber had a single fiber fineness of 1.7 dtex and a cut length of 51 mm.

[0056] (Production Example 5) A modacrylic fiber was obtained in the same manner as in Production Example 1, except that a spinning solution obtained by adding a magnesium hydroxide dispersion (concentration: 30% by mass) to a modacrylic polymer solution so that the magnesium hydroxide was 3 parts by mass per 100 parts by mass of the modacrylic polymer was used. The obtained modacrylic fiber had a single fiber fineness of 1.7 dtex and a cut length of 51 mm.

[0057] (Production Example 6) Except for using a dispersion of magnesium hydroxide having an average particle size of 0.5 μm, a modacrylic fiber was obtained in the same manner as in Production Example 1. The obtained modacrylic fiber had a single fiber fineness of 1.7 dtex and a cut length of 51 mm.

[0058] (Production Example 7) A modacrylic fiber was obtained in the same manner as in Production Example 1, except that a spinning solution was used in which a dispersion of antimony trioxide having an average particle size of 2.0 μm was added to a modacrylic polymer solution instead of the dispersion of magnesium hydroxide, so that the antimony trioxide was 26 parts by mass per 100 parts by mass of the modacrylic polymer. The obtained modacrylic fiber had a single fiber fineness of 2.2 dtex and a cut length of 38 mm.

[0059] (Production Example 8) A modacrylic polymer consisting of 51.1 mass% of structural units derived from acrylonitrile, 47.9 mass% of structural units derived from vinylidene chloride, and 1.1 mass% of structural units derived from sodium p-styrenesulfonate was used as the modacrylic polymer, and a dispersion of antimony trioxide having an average particle size of 1.0 μm was used, but modacrylic fiber was obtained in the same manner as in Production Example 7. The obtained modacrylic fiber had a single fiber fineness of 2.2 dtex and a cut length of 38 mm.

[0060] In the examples and comparative examples, the following fibers were also used: Silica-containing rayon fiber: "FR CORONA (registered trademark)" manufactured by Daiwabo Rayon Co., Ltd., single fiber fineness 1.7 dtex, fiber length 51 mm, silica content 17.2 mass% Flame-retardant rayon fiber: "Lenzing FR" manufactured by Lenzing, containing 0.5 to 0.8 mass% phosphorus-based flame retardant, single fiber fineness 2.2 dtex, fiber length 51 mm Polyester fiber: "Tetoron" manufactured by Toray Industries, Inc., single fiber fineness 1.6 dtex, fiber length 51 mm Flame-retardant polyester fiber: "ESLON" manufactured by Toray Chemical Co., Ltd., single fiber fineness 1.4 dtex, fiber length 51 mm

[0061] (Examples 1 to 10, Comparative Examples 1 to 5, 9, and 10) Modacrylic fibers and silica-containing rayon fibers shown in Table 2 below were mixed in the amounts shown in Table 2 below, and the mixture was opened by carding, followed by needle punching to produce nonwoven fabrics having the basis weights shown in Table 2 below.

[0062] (Comparative Example 6) Modacrylic fiber and flame-retardant rayon fiber shown in Table 2 below were mixed in the blending amounts shown in Table 2 below, and the mixture was opened by carding, followed by needle punching to produce a nonwoven fabric having the basis weight shown in Table 2 below.

[0063] (Comparative Example 7) Modacrylic fiber and polyester fiber shown in Table 2 below were mixed in the blending amounts shown in Table 2 below, and the mixture was opened by carding, and then needle-punched to produce a nonwoven fabric having the basis weight shown in Table 2 below.

[0064] (Comparative Example 8) Modacrylic fiber and flame-retardant polyester fiber shown in Table 2 below were mixed in the blending amounts shown in Table 2 below, and the mixture was opened by carding, followed by needle punching to produce a nonwoven fabric having the basis weight shown in Table 2 below.

[0065] In Examples 1 to 10 and Comparative Examples 1 to 10, the amount of static electricity when the card was passed was measured as described above, and the results are shown in Table 2 below. The flame retardancy and sound absorption coefficient of the nonwoven fabrics obtained in Examples 1 to 10 and Comparative Examples 1 to 10 were measured as described above, and the results are shown in Tables 3 and 4 below.

[0066]

[0067]

[0068]

[0069] As can be seen from the data in Tables 2 and 3 above, the nonwoven fabrics of the Examples have high flame retardancy, meeting the highest level of V-0 in the UL94 vertical flame test. Furthermore, as can be seen from the data in Table 4 above, the nonwoven fabrics of the Examples have sound absorption coefficients of 80% or more in the thickness range of 20 to 30 mm and the frequency range of 2500 to 6500 Hz, and can be suitably used as flame-retardant soundproofing or flame-retardant sound absorbing materials for vehicles such as automobiles and railway cars.

[0070] On the other hand, the basis weight is 80 g / m 2 The nonwoven fabrics of Comparative Example 1, in which the content of silica-containing rayon fiber is less than 55% by mass, Comparative Example 2, in which the content of magnesium compound in the nonwoven fabric is less than 0.75% by mass, Comparative Examples 3 and 5, in which the content of magnesium compound in the nonwoven fabric is less than 0.75% by mass, and Comparative Example 4, in which the content of magnesium-containing modacrylic fiber is less than 15% by mass, do not even meet the V-2 standard in the UL94 vertical flame test, and have poor flame retardancy. Furthermore, the nonwoven fabric of Comparative Example 6, in which flame-retardant rayon fiber containing a phosphorus-based flame retardant is used as the regenerated cellulose fiber, also does not meet the V-2 standard in the UL94 vertical flame test, and has poor flame retardancy. Comparative Example 7, in which magnesium compound-containing modacrylic fiber is used in combination with polyester fiber, and Comparative Example 8, in which magnesium compound-containing modacrylic fiber is used in combination with flame-retardant polyester fiber, both do not meet the V-2 standard in the UL94 vertical flame test, and have poor flame retardancy. The nonwoven fabrics of Comparative Examples 9 and 10, which used modacrylic fiber containing antimony trioxide as the modacrylic fiber, met the V-0 standard in the UL94 vertical flame test and had excellent flame retardancy, but there were concerns about the impact of antimony trioxide elution and emission on the environment and human body.From the above, it can be seen that, unlike the case where magnesium compound-containing modacrylic fiber is used in combination with other flame-retardant fibers, by using magnesium compound-containing modacrylic fiber and silica-containing regenerated cellulose fiber in combination in a specified ratio and adjusting the magnesium content in the nonwoven fabric to a specified amount, a unique effect is exerted and the flame retardancy of the nonwoven fabric is improved.

[0071] Furthermore, the fabrics of the Examples, which used a combination of magnesium compound-containing modacrylic fiber and silica-containing rayon fiber, had a better feel than the nonwoven fabrics of Comparative Examples 7 and 8, which used a combination of magnesium compound-containing modacrylic fiber and polyester fiber or flame-retardant polyester fiber.

[0072] Furthermore, as can be seen from a comparison between Examples 4 to 6 and Example 7, when the content of the magnesium compound derived from modacrylic fiber in the nonwoven fabric exceeds 6.5 mass%, the amount of static electricity in the fibers when passing through the card is high, and mass productivity is poor.

[0073] The present invention is not particularly limited, but preferably includes the following embodiments: [1] A flame-retardant nonwoven fabric comprising modacrylic fiber A and regenerated cellulose fiber B, wherein the modacrylic fiber A contains a magnesium compound, and the regenerated cellulose fiber B contains silica, the flame-retardant nonwoven fabric contains 15 to 45 mass% of the modacrylic fiber A and 55 to 85 mass% of the regenerated cellulose fiber B, the flame-retardant nonwoven fabric contains 0.75 mass% or more of the magnesium compound derived from the modacrylic fiber A, and the basis weight of the flame-retardant nonwoven fabric is 80 g / m 2The flame-retardant nonwoven fabric satisfies the V-0 standard of the UL94 vertical flame test. [2] The flame-retardant nonwoven fabric according to [1], wherein the regenerated cellulose fiber B contains silica-containing rayon fiber. [3] The flame-retardant nonwoven fabric according to [1] or [2], wherein the flame-retardant nonwoven fabric is substantially free of antimony compounds. [4] The flame-retardant nonwoven fabric according to any one of [1] to [3], wherein the flame-retardant nonwoven fabric contains 5% by mass or less of a magnesium compound derived from modacrylic fiber A. [5] The flame-retardant nonwoven fabric according to any one of [1] to [4], wherein the magnesium compound contains one or more selected from the group consisting of magnesium hydroxide and magnesium oxide. [6] The flame-retardant nonwoven fabric according to any one of [1] to [5], wherein the flame-retardant nonwoven fabric contains 7.5 to 20% by mass of silica derived from regenerated cellulose fiber B. [7] The flame-retardant nonwoven fabric according to any one of [1] to [6], wherein the modacrylic polymer constituting the modacrylic fiber A contains 30 to 85% by mass of structural units derived from acrylonitrile, 15 to 70% by mass of structural units derived from one or more halogen-containing monomers selected from the group consisting of halogen-containing vinyl monomers and halogen-containing vinylidene monomers, and 0 to 3% by mass of structural units derived from a sulfonic acid group-containing vinyl monomer. [8] The flame-retardant nonwoven fabric according to [7], wherein the modacrylic fiber A contains 3 to 25 parts by mass of a magnesium compound per 100 parts by mass of the modacrylic polymer. [9] The flame-retardant nonwoven fabric according to any one of [1] to [8], wherein the regenerated cellulose fiber B contains 10 to 30% by mass of silica.

[10] The flame-retardant nonwoven fabric according to any one of [1] to [9], wherein the modacrylic fiber A has a single fiber fineness of 0.5 to 5 dtex.

[11] The flame-retardant nonwoven fabric according to any one of [1] to

[10] , wherein the flame-retardant nonwoven fabric has a normal incident sound absorption coefficient of 80% or more in a thickness range of 20 to 30 mm and a frequency range of 2500 to 6500 Hz, as measured in accordance with JIS A 1405-2:2007.

[12] A vehicle interior material comprising the flame-retardant nonwoven fabric according to any one of [1] to

[11] .

[13] The vehicle interior material according to

[12] , which is a flame-retardant soundproofing material.

Claims

1. A flame-retardant nonwoven fabric comprising modacrylic fiber A and regenerated cellulose fiber B, wherein the modacrylic fiber A contains a magnesium compound, and the regenerated cellulose fiber B contains silica. The flame-retardant nonwoven fabric comprises 15 to 45 mass% of modacrylic fiber A and 55 to 85 mass% of regenerated cellulose fiber B. The flame-retardant nonwoven fabric comprises 0.75 mass% or more of a magnesium compound derived from the modacrylic fiber A, and the weight of the flame-retardant nonwoven fabric is 80 g / m. 2 The above flame-retardant nonwoven fabric satisfies the V-0 standard of the UL94 vertical flame test.

2. The flame-retardant nonwoven fabric according to claim 1, wherein the regenerated cellulose fiber B comprises a silica-containing rayon fiber.

3. The flame-retardant nonwoven fabric according to claim 1, which is substantially free of antimony compounds.

4. The flame-retardant nonwoven fabric according to claim 1, which contains 5% by mass or less of a magnesium compound derived from modacrylic fiber A.

5. The flame-retardant nonwoven fabric according to claim 1, wherein the magnesium compound comprises at least one compound selected from the group consisting of magnesium hydroxide and magnesium oxide.

6. The flame-retardant nonwoven fabric according to claim 1, which contains 7.5 to 20 mass % of silica derived from regenerated cellulose fiber B.

7. The flame-retardant nonwoven fabric according to claim 1, wherein the modacrylic polymer constituting the modacrylic fiber A contains 30 to 85 mass% of structural units derived from acrylonitrile, 15 to 70 mass% of structural units derived from one or more halogen-containing monomers selected from the group consisting of halogen-containing vinyl monomers and halogen-containing vinylidene monomers, and 0 to 3 mass% of structural units derived from a sulfonic acid group-containing vinyl monomer.

8. The flame-retardant nonwoven fabric according to claim 7, wherein the modacrylic fiber A contains 3 to 25 parts by mass of a magnesium compound per 100 parts by mass of the modacrylic polymer.

9. The flame-retardant nonwoven fabric according to claim 1, wherein the regenerated cellulose fiber B contains 10 to 30 mass % silica.

10. The flame-retardant nonwoven fabric according to claim 1, wherein the single fiber fineness of the modacrylic fiber A is 0.5 to 5 dtex.

11. The flame-retardant nonwoven fabric according to claim 1, wherein the flame-retardant nonwoven fabric has a normal incidence sound absorption coefficient, measured in accordance with JIS A 1405-2:2007, of 80% or more in a thickness range of 20 to 30 mm and a frequency range of 2,500 to 6,500 Hz.

12. A vehicle interior material comprising the flame-retardant nonwoven fabric according to any one of claims 1 to 11.

13. The vehicle interior material according to claim 12, which is a flame-retardant soundproofing material.

Citation Information

Patent Citations

  • Flame-retardant nonwoven fabric

    JP2009299199A

  • Elastic Fire Blocking Materials

    US20070178788A1

  • Flame-retardant synthetic fiber, flame-retardant fiber assembly, processes for production of both, and textile goods

    WO2010010815A1

  • Flame-retardant fiber composite and flame-retardant working clothes

    WO2021049200A1

  • Flame-resistant acrylic fibers, flame-resistant fiber composite, and flame-resistant mattress

    WO2022181337A1