Polarizing film and method for manufacturing same

The integration of a boron-containing compound and boric acid in the cured material layer of polarizing films addresses the issue of humidification reliability, enhancing adhesion and preventing swelling, thus ensuring effective polarization performance in harsh conditions.

WO2024247412A1PCT designated stage expired Publication Date: 2024-12-05NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007312
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-02-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current polarizing films face challenges in maintaining humidification reliability, particularly under severe water resistance tests, with existing adhesives failing to provide adequate performance in high-temperature and humid environments.

Method used

Incorporating a specific boron-containing compound and boric acid in the cured material layer of the polarizing film, which enhances interfacial adhesion and suppresses swelling, thereby improving the film's durability in humid conditions.

Benefits of technology

The use of a boron-containing compound and boric acid in the cured material layer significantly improves the polarizing film's humidification reliability, allowing it to maintain polarization properties effectively in high-temperature and humid environments by increasing interfacial adhesion and suppressing polarizer swelling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a polarizing film in which a cured product layer is provided on at least one surface of a polarizer, wherein the cured product layer is a layer of a cured product of a curable resin composition containing a specific boron-containing compound and boric acid. The mass ratio of the specific boron-containing compound and boric acid in the curable resin composition is preferably 1:0.1 to 1:30.0. Preferably, the content of a compound represented by general formula (1) in the curable resin composition is 0.05-5 mass%, and the content of boric acid is 0.1-2 mass%. The polarizer preferably contains 10-22 mass% of boric acid. It is preferable that A:B = 1:0.001 to 1:0.1, where A mass% is the ratio at which the polarizer contains boric acid, and B mass% is the ratio at which the curable resin composition contains boric acid.
Need to check novelty before this filing date? Find Prior Art

Description

Polarizing film and method for producing the same

[0001] The present invention relates to a polarizing film having a cured product layer on at least one surface of a polarizer, particularly a polarizing film having a transparent protective film laminated via an adhesive layer on at least one surface of a polarizer, and a method for producing the same. The polarizing film can be used alone or as an optical film laminated with the polarizing film to form image displays such as liquid crystal displays (LCDs), organic EL displays, CRTs, and PDPs.

[0002] Liquid crystal display devices (LCDs) are rapidly expanding into the market for watches, mobile phones, PDAs, laptops, PC monitors, DVD players, TVs, and more. Liquid crystal display devices visualize the polarization state through the switching of liquid crystals, and polarizers are used for this display principle. In particular, applications such as TVs require increasingly higher brightness, contrast, and a wider viewing angle, which in turn requires increasingly higher transmittance, polarization degree, and color reproducibility in polarizing films.

[0003] The most commonly used polarizers are iodine-based polarizers, which have a structure in which iodine is adsorbed into polyvinyl alcohol (hereinafter also simply referred to as "PVA") and stretched, due to their high transmittance and polarization degree. A typical polarizing film is one in which transparent protective films are bonded to both sides of a polarizer using a so-called aqueous adhesive in which a polyvinyl alcohol-based material is dissolved in water (see Patent Document 1 below). Examples of transparent protective films that can be used include triacetyl cellulose, which has high moisture permeability. When using the aqueous adhesive (so-called wet lamination), a drying process is required after bonding the polarizer and the transparent protective film together.

[0004] Meanwhile, active energy ray-curable adhesives have been proposed as an alternative to the water-based adhesives. When a polarized film is produced using an active energy ray-curable adhesive, a drying step is not required, and therefore productivity of the polarized film can be improved. For example, the present inventors have proposed a radical polymerization type active energy ray-curable adhesive that uses an N-substituted amide monomer as a curable component (see Patent Document 2 below).

[0005] JP 2001-296427 A JP 2012-052000 A

[0006] An adhesive layer formed using the active energy ray-curable adhesive described in Patent Document 2 can fully pass a water resistance test, which evaluates the presence or absence of color loss and peeling after immersion in 60°C hot water for six hours. However, in recent years, water resistance tests have been conducted under more severe conditions, and there has been a demand to maintain and improve the humidification reliability of the polarization properties of polarizing films. Therefore, the reality is that there is room for further improvement in the adhesives for polarizing films reported to date, including the active energy ray-curable adhesive described in Patent Document 2, particularly in terms of the humidification reliability of the polarization properties.

[0007] The present invention has been developed in view of the above circumstances, and an object of the present invention is to provide a polarizing film having excellent humidification reliability of polarization characteristics, and a method for producing the same.

[0008] Further objects of the present invention are to provide an optical film using the polarizing film, and to provide an image display device using the polarizing film or the optical film.

[0009] As a result of extensive research to solve the above problems, the inventors have discovered that the above object can be achieved by causing a specific boron-containing compound and boric acid to coexist in a cured material layer provided on at least one surface of a polarizer, thereby solving the problem of the present invention.

[0010] That is, the present invention provides a polarizing film having a cured material layer on at least one surface of a polarizer, wherein the cured material layer is represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 and each independently represent a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group, each of which may have a substituent, and boric acid.

[0011] In the polarizing film (1), a polarizing film (2) is preferred in which the mass ratio of the compound represented by the general formula (1) to the boric acid in the curable resin composition is 1:0.1 to 1:30.0.

[0012] In the polarizing film (1) or (2), the curable resin composition further comprises a compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 The polarizing film (3) preferably contains a compound (which may form a cyclic heterocycle).

[0013] In any one of the polarizing films (1) to (3), a polarizing film (4) is preferred in which the content of the compound represented by the general formula (1) in the curable resin composition is 0.05 to 5 mass % and the content of the boric acid is 0.1 to 2 mass %.

[0014] In any one of the polarizing films (1) to (4), the polarizer is preferably a polarizing film (5) containing 10 to 22% by mass of boric acid.

[0015] In the polarizing films (1) to (5), when the content of boric acid in the polarizer is A% by mass and the content of boric acid in the curable resin composition is B% by mass, a polarizing film (6) is preferred in which A:B=1:0.001 to 1:0.1.

[0016] In any one of the polarizing films (1) to (6), a polarizing film (7) in which the thickness of the cured product layer is 1 μm or more and 2 μm or less is preferred.

[0017] In any of the above polarizing films (1) to (7), a polarizing film (8) is preferred, which is a polarizing film in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, and the adhesive layer is the cured product layer.

[0018] In the polarizing film (8), a polarizing film (9) is preferred in which the transparent protective film is a triacetyl cellulose-based resin film.

[0019] In the polarizing film (8) or (9), a polarizing film (10) is preferred which has a compatible layer between the transparent protective film and the adhesive layer, in which the transparent protective film and the adhesive layer are compatible with each other.

[0020] The present invention also relates to an optical film (11) comprising at least one laminate of any one of the polarizing films (1) to (10).The present invention further relates to an image display device (12) comprising any one of the polarizing films (1) to (10) or the optical film (11).

[0021] The present invention also provides a method for producing a polarizing film, in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, the adhesive layer being a cured product layer of a curable resin composition including at least a first composition and a second composition, the first composition comprising at least a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group, which may have a substituent), and boric acid, and the second composition contains at least a compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6may form a cyclic heterocycle), and the method for producing a polarizing film includes: a first coating step of coating a first composition on an attachment surface of the polarizer; a second coating step of coating a second composition on an attachment surface of the transparent protective film; a laminating step of laminating the polarizer and the transparent protective film together; and an adhering step of adhering the polarizer and the transparent protective film together via the adhesive layer obtained by curing the curable resin composition by irradiating the polarizer surface side or the transparent protective film surface side with active energy rays.

[0022] In the method (13) for producing a polarizing film, a method (14) for producing a polarizing film is preferred, in which the mass ratio of the compound represented by general formula (1) to the boric acid in the first composition is 1:0.1 to 1:30.0.

[0023] In the polarizing film production method (13) or (14), a polarizing film production method (15) is preferred, in which the content of the compound represented by general formula (1) in the curable resin composition is 0.05 to 5 mass %, and the content of boric acid in the curable resin composition is 0.1 to 2 mass %.

[0024] In any one of the above polarizing film manufacturing methods (13) to (15), the polarizer is preferably a polarizer containing 10 to 22 mass % of boric acid (16).

[0025] In any of the above polarizing film production methods (13) to (16), a polarizing film production method (17) is preferred, in which, when the content of boric acid in the polarizer is A% by mass and the content of boric acid in the curable resin composition is B% by mass, A:B=1:0.001 to 1:0.1.

[0026] In any one of the above polarizing film manufacturing methods (13) to (17), a polarizing film manufacturing method (18) is preferred, in which the first composition after the first coating step has a coating thickness before drying of 0.6 to 2.0 μm and a coating thickness after drying of 0.3 to 1.0 μm.

[0027] In any one of the above polarizing film manufacturing methods (13) to (18), a polarizing film manufacturing method (19) is preferred, in which the thickness of the adhesive layer is 1 μm or more and 2 μm or less.

[0028] The polarizing film according to the present invention has a cured layer on at least one surface of a polarizer, and the cured layer is a cured layer of a curable resin composition containing a specific boron-containing compound represented by general formula (1) and boric acid, and therefore has excellent humidification reliability of polarization characteristics. The reason for this effect is not clear, but can be assumed as follows.

[0029] The cured material layer provided on at least one surface of the polarizer is formed from a curable resin composition, and the curable resin composition contains a specific boron-containing compound represented by general formula (1). The specific boron-containing compound represented by general formula (1) contains a boric acid group (or a borate ester group) and a reactive group X, and the boric acid group (or the borate ester group) can form a covalent bond with a functional group, such as a hydroxyl group, present on the polarizer surface. The reactive group X can also react with other curable components contained in the curable resin composition to form a covalent bond. Therefore, in order to improve the interfacial adhesion between the polarizer and the cured material layer and suppress swelling of the polarizer, it is extremely important to enhance the reactivity of the specific boron-containing compound represented by general formula (1). As a result of extensive research by the present inventors, it was found that by having the specific boron-containing compound represented by general formula (1) and boric acid coexist in the curable resin composition used as the raw material for the cured material layer, boric acid can significantly improve the reactivity of the specific boron-containing compound represented by general formula (1). In other words, the coexistence of the specific boron-containing compound represented by general formula (1) and boric acid dramatically increases the interfacial adhesion between the cured layer and the polarizer, thereby suppressing swelling of the polarizer even when the polarizing film is exposed to a high-temperature, humid environment. As a result, it is presumed that the humidification reliability of the polarization properties of the polarizing film is significantly improved. In addition, when boric acid is present in the curable resin composition that is the raw material for the cured layer, the boric acid can also contribute to a crosslinking reaction within the polarizer. Therefore, even when the polarizing film is exposed to a high-temperature, humid environment, the crosslinking reaction within the polarizer caused by boric acid suppresses swelling of the polarizer. In other words, it is presumed that the crosslinking reaction within the polarizer caused by boric acid also significantly improves the humidification reliability of the polarization properties of the polarizing film.

[0030] The present invention also relates to a method for producing a polarizing film in which a transparent protective film is laminated to at least one surface of a polarizer via an adhesive layer. The adhesive layer is a cured layer of a curable resin composition composed of at least a first composition and a second composition. When the first composition contains a specific boron-containing compound represented by general formula (1) and boric acid, the resulting polarizing film exhibits significantly improved humidification reliability of its polarization properties. The reason for this effect is unclear, but can be assumed as follows.

[0031] The specific boron-containing compound represented by general formula (1) contains a boric acid group (or a borate ester group) and a reactive group X. The boric acid group (or a borate ester group) forms a covalent bond with a functional group, such as a hydroxyl group, present on the polarizer surface, and the reactive group X reacts with another curable component contained in the curable resin composition to also form a covalent bond. Therefore, in order to improve the interfacial adhesion between the polarizer and the cured material layer and to suppress swelling of the polarizer, it is extremely important to enhance the reactivity of the specific boron-containing compound represented by general formula (1). As a result of extensive research by the present inventors, it has been found that by having the specific boron-containing compound represented by general formula (1) and boric acid coexist in the curable resin composition that is the raw material for the cured material layer, boric acid can significantly improve the reactivity of the specific boron-containing compound represented by general formula (1). In other words, the coexistence of the specific boron-containing compound represented by general formula (1) and boric acid dramatically increases the interfacial adhesion between the cured layer and the polarizer, thereby suppressing swelling of the polarizer even when the polarizing film is exposed to a high-temperature, humid environment. As a result, it is presumed that the humidification reliability of the polarization properties of the polarizing film is significantly improved. Additionally, when boric acid is present in the curable resin composition that is the raw material for the cured layer, the boric acid can contribute to a crosslinking reaction within the polarizer. Therefore, even when the polarizing film is exposed to a high-temperature, humid environment, swelling of the polarizer is suppressed due to the crosslinking reaction within the polarizer caused by the boric acid. In other words, it is presumed that the humidification reliability of the polarization properties of the polarizing film is also significantly improved due to the crosslinking reaction within the polarizer caused by the boric acid. In particular, in the method for producing a polarizing film according to the present invention, a first composition containing the specific boron-containing compound represented by general formula (1) and boric acid is applied to the bonding surface of the polarizer, so that the specific boron-containing compound represented by general formula (1) and boric acid are present at high concentrations on the surface of the polarizer. Therefore, the specific boron-containing compound represented by general formula (1) reacts with the polarizer quickly and efficiently, and the crosslinking reaction in the polarizer caused by boric acid also proceeds quickly and efficiently. Therefore, the method for producing a polarizing film according to the present invention can produce a polarizing film with significantly improved humidification reliability of its polarization properties.

[0032] The polarizing film according to the present invention is a polarizing film having a cured material layer on at least one surface of a polarizer. The cured material layer is a polarizing film having a structure represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 and each independently represent a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group, each of which may have a substituent, and boric acid. Examples of the aliphatic hydrocarbon group include a linear or branched alkyl group having 1 to 20 carbon atoms, which may have a substituent, a cyclic alkyl group having 3 to 20 carbon atoms, which may have a substituent, and an alkenyl group having 2 to 20 carbon atoms. Examples of the aryl group include a phenyl group having 6 to 20 carbon atoms, which may have a substituent, and a naphthyl group having 10 to 20 carbon atoms, which may have a substituent. Examples of the heterocyclic group include a 5- or 6-membered ring group containing at least one heteroatom, which may have a substituent. These may be linked together to form a ring. In general formula (1), R 1 and R 2 is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, and most preferably a hydrogen atom.

[0033] X in the compound represented by general formula (1) is a reactive group, which is a functional group that can react with a curable component that constitutes the cured product layer, particularly the adhesive layer, and examples thereof include a hydroxyl group, an amino group, an aldehyde group, a carboxyl group, a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, an α,β-unsaturated carbonyl group, a mercapto group, and a halogen group. When the curable resin composition constituting the cured product layer, particularly the adhesive layer, is active energy ray-curable, the reactive group X is preferably at least one reactive group selected from the group consisting of vinyl groups, (meth)acrylic groups, styryl groups, (meth)acrylamide groups, vinyl ether groups, epoxy groups, oxetane groups, and mercapto groups. When the curable resin composition constituting the cured product layer, particularly the adhesive layer, is radically polymerizable, the reactive group X is preferably at least one reactive group selected from the group consisting of (meth)acrylic groups, styryl groups, and (meth)acrylamide groups. When the compound represented by general formula (1) has a (meth)acrylamide group, this is more preferred because it has high reactivity and increases the copolymerization rate with the curable component in the cured product layer, particularly the adhesive layer. Furthermore, this is also preferred because the (meth)acrylamide group has high polarity and excellent adhesiveness, allowing the effects of the present invention to be efficiently obtained. When the curable resin composition constituting the cured product layer, particularly the adhesive layer, is cationic polymerizable, the reactive group X preferably has at least one functional group selected from a hydroxyl group, an amino group, an aldehyde, a carboxyl group, a vinyl ether group, an epoxy group, an oxetane group, and a mercapto group. In particular, when the reactive group X has an epoxy group, this is preferred because the resulting cured product layer, particularly the adhesive layer, has excellent adhesion to the adherend, and when the reactive group X has a vinyl ether group, this is preferred because the curability of the curable resin composition is excellent.

[0034] Preferred specific examples of the compound represented by general formula (1) include the following compounds (1a) to (1d). 3 is a hydrogen atom or a methyl group.

[0035] In addition to the compounds exemplified above, examples of the compound represented by general formula (1) include esters of (meth)acrylates and boric acid, such as esters of hydroxyethyl acrylamide and boric acid, esters of methylolacrylamide and boric acid, esters of hydroxyethyl acrylate and boric acid, and esters of hydroxybutyl acrylate and boric acid.

[0036] The polarizing film according to the present invention includes a cured product layer, particularly an adhesive layer, on at least one surface of a polarizer. The cured product layer, particularly the adhesive layer, is formed using a curable resin composition as a raw material. The curable resin composition may be composed of a single composition or two or more compositions, for example, a first composition and a second composition. When the curable resin composition is composed of a single composition, the cured product layer, particularly the adhesive layer, may be formed by coating the curable resin composition on the bonding surface of the polarizer or on the bonding surface of another adherend, such as a transparent protective film. When the curable resin composition is composed of two or more compositions, for example, a first composition and a second composition, the first composition may be coated on the bonding surface of the polarizer and the second composition may be coated on the bonding surface of another adherend, such as a transparent protective film. In this case, it is preferable to blend a compound represented by general formula (1) and boric acid into the first composition. The first composition containing the compound represented by general formula (1) and boric acid may also contain a curable component or a solvent such as water. However, when a solvent such as water is blended, it is necessary to remove the solvent such as water from the first composition coated on the bonding surface of the polarizer, for example, by applying the first composition to the bonding surface of the polarizer and then providing a drying step, etc. Therefore, when calculating the blending amount in the curable resin composition in the present invention, the calculation excludes the solvent such as water.

[0037] From the viewpoint of improving the humidification reliability of the polarization properties of the polarizing film, the amount of the compound represented by general formula (1) in the curable resin composition constituting the cured product layer, particularly the adhesive layer, is preferably 0.05 to 5 mass%, and more preferably 1.0 to 3.0 mass%. Similarly, the amount of boric acid in the curable resin composition is preferably 0.1 to 2 mass%, and more preferably 0.2 to 1.0 mass%.

[0038] Furthermore, from the viewpoint of improving the humidification reliability of the polarization properties of the polarizing film, the mass ratio of the compound represented by general formula (1) to boric acid in the curable resin composition constituting the cured product layer, particularly the adhesive layer, is preferably 1:0.10 to 1:30.0, and more preferably 1:0.15 to 1:5 from the viewpoint of the effect of suppressing edge discoloration.

[0039] In addition to the compound represented by the general formula (1) and boric acid, the curable resin composition can contain curable components and other components. The curable resin composition used in the present invention is preferably an active energy ray-curable resin composition. Active energy ray-curable resin compositions can be classified into radical polymerization-curable resin compositions and cationic polymerization-curable resin compositions. In the present invention, active energy rays in the wavelength range of 10 nm to less than 380 nm are referred to as ultraviolet rays, and active energy rays in the wavelength range of 380 nm to 800 nm are referred to as visible light.

[0040] Examples of the curable component constituting the radical polymerization curable resin composition include compounds represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 The number of carbon atoms in the alkyl moiety of the alkyl group, hydroxyalkyl group, and / or alkoxyalkyl group is not particularly limited, but examples include those having 1 to 4 carbon atoms. 5 and R 6 Examples of the cyclic heterocycle that may be formed include N-acryloylmorpholine.

[0041] Specific examples of the compound represented by general formula (2) include N-alkyl group-containing (meth)acrylamide derivatives such as N-methyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and N-hexyl(meth)acrylamide; N-hydroxyalkyl group-containing (meth)acrylamide derivatives such as N-methylol(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and N-methylol-N-propane(meth)acrylamide; and N-alkoxy group-containing (meth)acrylamide derivatives such as N-methoxymethylacrylamide and N-ethoxymethylacrylamide. Examples of the cyclic ether group-containing (meth)acrylamide derivative include heterocycle-containing (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocycle, such as N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine, etc. Among these, N-hydroxyethylacrylamide and N-acryloylmorpholine are preferred because of their excellent reactivity, ability to produce a cured product with a high elastic modulus, and excellent adhesion to polarizers.

[0042] When the curable resin composition is composed of two compositions, for example, a first composition and a second composition, the compound represented by general formula (2) may be blended only in the second composition, or may be blended in both the first composition and the second composition.

[0043] From the viewpoint of improving the adhesion and water resistance between the polarizer and the adhesive layer, particularly improving the adhesion and water resistance when the polarizer and the transparent protective film are bonded via an adhesive layer, the content of the compound represented by general formula (2) in the curable resin composition is preferably 20 to 80 mass %, and more preferably 40 to 70 mass %.

[0044] The curable resin composition used in the present invention may contain, as a curable component, other monofunctional radical polymerizable compounds in addition to the compound represented by general formula (2). Examples of the monofunctional radical polymerizable compounds include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Specific examples include (meth)acrylic acid (C1-20) alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.

[0045] Examples of the (meth)acrylic acid derivatives include cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxy Examples of suitable (meth)acrylates include polycyclic (meth)acrylates such as ethyl (meth)acrylate and dicyclopentanyl (meth)acrylate; and alkoxy or phenoxy group-containing (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxy polyethylene glycol (meth)acrylate. Among these, dicyclopentenyloxyethyl acrylate and phenoxyethyl acrylate are preferred because of their excellent adhesion to various protective films.

[0046] In addition, examples of the (meth)acrylic acid derivatives include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. hydroxyl group-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether; 2,2,2-trifluoroethyl (meth)acrylate, 2,2,2-trifluoroethylethyl (meth)acrylate; Halogen-containing (meth)acrylates such as acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; 3-oxetanylmethyl (meth)acrylate, 3-methyl-oxetanylmethyl (meth)acrylate; oxetane group-containing (meth)acrylates such as acrylate, 3-ethyl-oxetanylmethyl (meth)acrylate, 3-butyl-oxetanylmethyl (meth)acrylate, and 3-hexyl-oxetanylmethyl (meth)acrylate; (meth)acrylates having a heterocycle such as tetrahydrofurfuryl (meth)acrylate and butyrolactone (meth)acrylate; hydroxypivalic acid neopentyl glycol (meth)acrylic acid adduct; and p-phenylphenol (meth)acrylate. Among these, 2-hydroxy-3-phenoxypropyl acrylate is preferred because of its excellent adhesion to various protective films.

[0047] Furthermore, examples of the monofunctional radically polymerizable compound include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.

[0048] Examples of the monofunctional radically polymerizable compound include lactam vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; and vinyl monomers having a nitrogen-containing heterocycle such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, and vinylmorpholine.

[0049] Furthermore, as the monofunctional radical polymerizable compound, a radical polymerizable compound having an active methylene group can be used. The radical polymerizable compound having an active methylene group is a compound having an active double bond group such as a (meth)acrylic group at the end or in the molecule, and also having an active methylene group. Examples of the active methylene group include an acetoacetyl group, an alkoxymalonyl group, and a cyanoacetyl group. It is preferable that the active methylene group is an acetoacetyl group. Specific examples of radically polymerizable compounds having an active methylene group include acetoacetoxyalkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, and 2-acetoacetoxy-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxymethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radically polymerizable compound having an active methylene group is preferably an acetoacetoxyalkyl (meth)acrylate.

[0050] A bifunctional or higher polyfunctional radically polymerizable compound can be blended as a curable component constituting the radical polymerization curable resin composition. Examples of the polyfunctional radically polymerizable compound include polyfunctional (meth)acrylamide derivatives such as N,N'-methylenebis(meth)acrylamide, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, and bisphenol A diglycidyl ether di(meth)acrylate. esters of (meth)acrylic acid with polyhydric alcohols such as acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal(meth)acrylate, dioxane glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerin tetra(meth)acrylate; and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples include Aronix M-220 (manufactured by Toagosei Co., Ltd.), Light Acrylate 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer Co., Ltd.), and CD-536 (manufactured by Sartomer Co., Ltd.), etc. Furthermore, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, and various (meth)acrylate monomers may be used as needed.It is preferable to include a polyfunctional (meth)acrylamide derivative in the curable resin composition because it has a high polymerization rate, excellent productivity, and excellent crosslinkability when the resin composition is cured.

[0051] From the viewpoint of achieving both adhesion to polarizers and various transparent protective films and optical durability under harsh environments, it is preferable to use a monofunctional radically polymerizable compound and a polyfunctional radically polymerizable compound in combination. The amount of the monofunctional radically polymerizable compound in the curable resin composition is preferably 30 to 90% by mass, more preferably 50 to 80% by mass. The amount of the polyfunctional radically polymerizable compound in the curable resin composition is preferably 10 to 70% by mass, more preferably 20 to 50% by mass.

[0052] <Embodiments of Radical Polymerization Curable Resin Composition> The curable resin composition used in the present invention can be used as an active energy ray-curable resin composition when the curable component is used as an active energy ray-curable component. When an electron beam or the like is used as the active energy ray, the active energy ray-curable resin composition does not need to contain a photopolymerization initiator, but when ultraviolet light or visible light is used as the active energy ray, it is preferable that the active energy ray-curable resin composition contains a photopolymerization initiator.

[0053] The photopolymerization initiator is appropriately selected depending on the active energy ray. When curing is performed with ultraviolet light or visible light, a photopolymerization initiator that is cleaved by ultraviolet light or visible light is used. Examples of the photopolymerization initiator include benzophenone-based compounds such as benzil, benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and α-hydroxycyclohexylphenyl ketone; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin methyl ether. aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates.

[0054] The amount of the photopolymerization initiator to be blended is preferably 0.5 to 5 parts by mass, and more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the total amount of the active energy ray-curable resin composition.

[0055] When the active energy ray-curable resin composition is used as a visible light-curable type, it is preferable to use a photopolymerization initiator that is particularly sensitive to light of 380 nm or more. Photopolymerization initiators that are highly sensitive to light of 380 nm or more will be described later.

[0056] The photopolymerization initiator may be a compound represented by the following general formula (3): (In the formula, R 7 and R 8 -H, -CH 2 CH 3 , -iPr or Cl, R 7 and R 8 It is preferable to use a compound represented by general formula (3) alone, or to use a compound represented by general formula (3) in combination with a photopolymerization initiator highly sensitive to light of 380 nm or longer, which will be described later. When a compound represented by general formula (3) is used, the adhesiveness is superior to when a photopolymerization initiator highly sensitive to light of 380 nm or longer is used alone. Among the compounds represented by general formula (3), R 7 and R 8 Ga-CH 2 CH 3 The amount of the compound represented by general formula (3) in the active energy ray-curable resin composition is preferably 0.1 to 4 mass%, and more preferably 0.5 to 3 mass%, when the total amount of the curable resin composition is 100 mass%.

[0057] It is also preferable to add a polymerization initiation aid as necessary. Examples of the polymerization initiation aid include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, and isoamyl 4-dimethylaminobenzoate, with ethyl 4-dimethylaminobenzoate being particularly preferred. When a polymerization initiation aid is used, the amount added is preferably 0.1 to 3 parts by mass, and more preferably 0.3 to 1 part by mass, relative to 100 parts by mass of the total amount of the active energy ray-curable resin composition.

[0058] In addition, a known photopolymerization initiator can be used in combination as needed. Since the optical functional layer and the base film having UV absorption ability do not transmit light of 380 nm or less, it is preferable to use a photopolymerization initiator that is highly sensitive to light of 380 nm or more. Specific examples include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, and the like.

[0059] In the present invention, the curable resin composition preferably contains an acrylic oligomer obtained by polymerizing a (meth)acrylic monomer. By containing an acrylic oligomer in the curable resin composition, it is possible to reduce cure shrinkage when the composition is irradiated with active energy rays and cured, and to reduce interfacial stress between the adhesive layer and the adherend, such as the optical functional layer and the substrate film. As a result, it is possible to suppress a decrease in adhesion between the adhesive layer and the adherend.

[0060] Considering workability and uniformity during application, it is preferable that the active energy ray-curable resin composition has a low viscosity, and therefore it is preferable that the acrylic oligomer obtained by polymerizing a (meth)acrylic monomer also has a low viscosity. As an acrylic oligomer that has a low viscosity and can prevent cure shrinkage of the adhesive layer, one having a weight average molecular weight (Mw) of preferably 15,000 or less, more preferably 10,000 or less, and particularly preferably 5,000 or less. On the other hand, in order to sufficiently suppress cure shrinkage of the cured product layer (adhesive layer), the weight average molecular weight (Mw) of the acrylic oligomer is preferably 500 or more, more preferably 1,000 or more, and particularly preferably 1,500 or more. Specific examples of the (meth)acrylic monomer constituting the acrylic oligomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,(Meth)acrylic acid (C1-20) alkyl esters such as 2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and N-octadecyl (meth)acrylate; further, for example, cycloalkyl (meth)acrylates (for example, cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, etc.), aralkyl (meth)acrylates (for example, benzyl (meth)acrylate, etc.), polycyclic (meth)acrylates (for example, 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and 4-methyl-2-propylpentyl (meth)acrylate; (meth)acrylate, etc.), hydroxyl group-containing (meth)acrylic acid esters (for example, hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropylmethyl-butyl (meth)methacrylate, etc.), alkoxy group- or phenoxy group-containing (meth)acrylic acid esters (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), epoxy group-containing (meth)acrylic acid esters (for example, glycidyl (meth)acrylate, etc.), halogen-containing (meth)acrylic acid esters (for example, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,Examples of the acrylic oligomer (E) include 2-trifluoroethylethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, etc., and alkylaminoalkyl (meth)acrylates (for example, dimethylaminoethyl (meth)acrylate, etc.). These (meth)acrylates can be used alone or in combination of two or more. Specific examples of the acrylic oligomer (E) include "ARUFON" manufactured by Toagosei Co., Ltd., "Actflow" manufactured by Soken Chemical & Engineering Co., Ltd., and "JONCRYL" manufactured by BASF Japan Ltd.

[0061] The amount of the acrylic oligomer in the curable resin composition is preferably 3 to 40% by mass, and more preferably 5 to 20% by mass.

[0062] The curable resin composition used in the present invention may contain a silane coupling agent. Specific examples of the silane coupling agent include active energy ray-curable compounds such as vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane.

[0063] Preferred are 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0064] Specific examples of non-active energy ray-curable silane coupling agents other than those mentioned above include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazole silane.

[0065] The curable resin composition used in the present invention may be a cationic polymerization curable resin composition. Cationic polymerizable compounds used in cationic polymerization curable resin compositions are classified into monofunctional cationic polymerizable compounds having one cationic polymerizable functional group in the molecule and polyfunctional cationic polymerizable compounds having two or more cationic polymerizable functional groups in the molecule. Monofunctional cationic polymerizable compounds have relatively low liquid viscosity, and their inclusion in a cationic polymerization curable resin composition can reduce the liquid viscosity. Furthermore, monofunctional cationic polymerizable compounds often have functional groups that impart various functions. By incorporating them into a cationic polymerization curable resin composition, various functions can be imparted to the cationic polymerization curable resin composition and / or the cured product of the cationic polymerization curable resin composition. Polyfunctional cationic polymerizable compounds can three-dimensionally crosslink the cured product of the cationic polymerization curable resin composition, and are therefore preferably incorporated into a cationic polymerization curable resin composition. The ratio of the monofunctional cationic polymerizable compound to the polyfunctional cationic polymerizable compound is preferably in the range of 10 to 1,000 parts by mass of the polyfunctional cationic polymerizable compound per 100 parts by mass of the monofunctional cationic polymerizable compound. Examples of the cationically polymerizable functional group include an epoxy group, an oxetanyl group, and a vinyl ether group. Examples of compounds having an epoxy group include an aliphatic epoxy compound, an alicyclic epoxy compound, and an aromatic epoxy compound. The cationically polymerizable resin composition of the present invention particularly preferably contains an alicyclic epoxy compound because of its excellent curability and adhesiveness. Examples of the alicyclic epoxy compound include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, caprolactone-modified products, trimethylcaprolactone-modified products, and valerolactone-modified products of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and specific examples thereof include Celloxide 2021, Celloxide 2021A, Celloxide 2021P, Celloxide 2081, Celloxide 2083, and Celloxide 2085 (all manufactured by Daicel Chemical Industries, Ltd.), and Cyracure UVR-6105, Cyracure UVR-6107, Cyracure 30, and R-6110 (all manufactured by Dow Chemical Japan Ltd.).Compounds having an oxetanyl group are preferably contained because they have the effect of improving the curability of the cationically polymerizable resin composition and reducing the liquid viscosity of the composition. Examples of compounds having an oxetanyl group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetanyl)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and phenol novolac oxetane. Commercially available compounds include Aronoxetane OXT-101, Aronoxetane OXT-121, Aronoxetane OXT-211, Aronoxetane OXT-221, and Aronoxetane OXT-212 (all manufactured by Toagosei Co., Ltd.). A compound having a vinyl ether group is preferably contained because it has the effect of improving the curability of the cationically polymerizable resin composition and reducing the liquid viscosity of the composition. Examples of the compound having a vinyl ether group include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol divinyl ether, cyclohexanedimethanol divinyl ether, cyclohexanedimethanol monovinyl ether, tricyclodecane vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, and pentaerythritol tetravinyl ether.

[0066] The cationic polymerization curable resin composition contains at least one compound selected from the group consisting of the epoxy group-containing compound, the oxetanyl group-containing compound, and the vinyl ether group-containing compound described above as a curable component. Since all of these compounds cure by cationic polymerization, a photocationic polymerization initiator is incorporated into the composition. This photocationic polymerization initiator generates cationic species or a Lewis acid upon irradiation with active energy rays such as visible light, ultraviolet light, X-rays, or electron beams, thereby initiating the polymerization reaction of the epoxy group or the oxetanyl group. The photoacid generator described below is preferably used as the photocationic polymerization initiator. Furthermore, when the cationic polymerization resin composition is used as a visible light curable resin, it is preferable to use a photocationic polymerization initiator that is particularly sensitive to light of 380 nm or longer. However, since photocationic polymerization initiators are generally compounds that exhibit a maximum absorption in the wavelength range around 300 nm or shorter, incorporating a photosensitizer that exhibits a maximum absorption in the longer wavelength range, specifically, light of wavelengths longer than 380 nm, can be used to stimulate the generation of cationic species or acids from the photocationic polymerization initiator. Examples of photosensitizers include anthracene compounds, pyrene compounds, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, and photoreducible dyes, and two or more of these may be used in combination. Anthracene compounds are particularly preferred because of their excellent photosensitizing effect, and specific examples include Anthracure UVS-1331 and Anthracure UVS-1221 (manufactured by Kawasaki Chemical Industries, Ltd.). The content of the photosensitizer is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass.

[0067] In the present invention, the active energy ray-curable resin composition may contain a photoacid generator. When the active energy ray-curable resin composition contains a photoacid generator, the water resistance and durability of the adhesive layer can be dramatically improved compared to when the active energy ray-curable resin composition does not contain a photoacid generator. The photoacid generator can be represented by the following general formula (3):

[0068] General formula (4) (However, L +represents any onium cation. - is PF6 6 - , SbF 6 - , AsF 6 - , SbCl 6 - , BiCl 5 - , SnCl 6 - , ClO 4 - , a dithiocarbamate anion, and a counter anion selected from the group consisting of SCN-.

[0069] Next, the counter anion X in the general formula (4) - This article explains:

[0070] Counter anion X in general formula (4) - Although there is no particular limitation in principle, a non-nucleophilic anion is preferred. - When PF is a non-nucleophilic anion, nucleophilic reactions are unlikely to occur with cations coexisting in the molecule or with various materials used in combination, and as a result, it is possible to improve the stability over time of the photoacid generator represented by general formula (4) itself and compositions using it. The non-nucleophilic anion here refers to an anion with a low ability to cause a nucleophilic reaction. Examples of such anions include PF 6 - , SbF 6 - , AsF 6 - , SbCl 6 - , BiCl 5 - , SnCl 6 - , ClO 4 - , B(C 6 H 5 ) 4 - , dithiocarbamate anion, SCN - Examples include:

[0071] Specifically, "Cyracure UVI-6992" and "Cyracure UVI-6974" (both manufactured by Dow Chemical Japan Co., Ltd.), "ADEKAOPTOMER SP150", "ADEKAOPTOMER SP152", "ADEKAOPTOMER SP170", and "ADEKAOPTOMER SP172" (all manufactured by ADEKA Corporation), and "Omnicat250" (IGM Resins B.V.), "CI-5102", "CI-2855" (all manufactured by Nippon Soda Co., Ltd.), "SAN-AID SI-60L", "SAN-AID SI-80L", "SAN-AID SI-100L", "SAN-AID SI-110L", "SAN-AID SI-180L" (all manufactured by Sanshin Chemical Industry Co., Ltd.), "IK-1", "CPI-100P", "CPI-101A", "CPI-110P", "CPI-200K", "CPI-210S", "CPI Specific preferred examples of the photoacid generator of the present invention include "WPI-310B", "CPI-410B", and "CPI-410S" (all manufactured by San-Apro Ltd.), "WPI-069", "WPI-113", "WPI-116", "WPI-041", "WPI-044", "WPI-054", "WPI-055", "WPAG-281", "WPAG-567", and "WPAG-596" (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).

[0072] The polarizing film according to the present invention is a polarizing film having a cured layer on at least one surface of a polarizer, and is preferably a polarizing film in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, and the adhesive layer is a cured layer.

[0073] The thickness of the cured product layer (adhesive layer) is preferably 1 μm or more and 2 μm or less from the viewpoint of improving the humidification reliability of the polarization properties of the polarizing film.

[0074] When the polarizing film according to the present invention is a polarizing film in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, it is preferable to provide a compatible layer between the transparent protective film and the adhesive layer, in which the two are compatible with each other, from the viewpoint of improving the humidification reliability of the polarization properties of the polarizing film. A method for confirming the formation of the compatible layer will be described later.

[0075] In the present invention, the polarizer is not particularly limited, and various polarizers can be used. Examples of polarizers include those obtained by uniaxially stretching a hydrophilic polymer film, such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or a partially saponified ethylene-vinyl acetate copolymer film, after iodine has been adsorbed thereon. The thickness of the polarizer can be, for example, 3 to 20 μm.

[0076] However, in the present invention, from the viewpoint of improving humidification reliability in a severe environment of high temperature and high humidity, it is preferable to use a thin polarizer having a thickness of 3 μm or more and 15 μm or less as the polarizer. A thickness of 12 μm or less is particularly preferable, and a thickness of 10 μm or less, particularly 8 μm or less, is further preferable. Such a thin polarizer has little thickness unevenness, excellent visibility, and is excellent in durability against thermal shock due to little dimensional change.

[0077] A polarizer obtained by dyeing a polyvinyl alcohol-based film with iodine and uniaxially stretching it can be produced, for example, by immersing the polyvinyl alcohol in an iodine aqueous solution to dye it and then stretching it to 3 to 7 times its original length. If necessary, the polyvinyl alcohol-based film may contain boric acid, zinc sulfate, zinc chloride, or the like, or may be immersed in an aqueous solution of potassium iodide or the like. Furthermore, if necessary, the polyvinyl alcohol-based film may be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water not only removes dirt and antiblocking agents from the polyvinyl alcohol-based film surface, but also swells the polyvinyl alcohol-based film, thereby preventing unevenness such as uneven dyeing. Stretching may be performed after dyeing with iodine, or the film may be stretched while dyeing, or the film may be dyed with iodine after stretching. Stretching may also be performed in an aqueous solution of boric acid, potassium iodide, or the like, or in a water bath.

[0078] The polarizer preferably contains boric acid from the viewpoints of stretching stability and humidification reliability. Furthermore, the content of boric acid in the polarizer is preferably 22% by mass or less, and more preferably 20% by mass or less, of the total amount of the polarizer, from the viewpoint of suppressing the occurrence of through cracks. From the viewpoints of stretching stability and humidification reliability, the content of boric acid in the polarizer is preferably 10% by mass or more, and more preferably 12% by mass or more, of the total amount of the polarizer.

[0079] From the viewpoint of improving the humidification reliability of the polarization properties of the polarizing film, in the polarizing film according to the present invention, when the proportion of boric acid contained in the polarizer is A mass %, and the proportion of boric acid contained in the curable resin composition is B mass %, A:B is preferably 1:0.001 to 1:0.1, and more preferably 1:0.01 to 1:0.05.

[0080] Representative examples of the thin polarizer include the thin polarizers described in Japanese Patent No. 4751486, Japanese Patent No. 4751481, Japanese Patent No. 4815544, Japanese Patent No. 5048120, WO 2014 / 077599, and WO 2014 / 077636, and the like, as well as thin polarizers obtained by the manufacturing methods described therein.

[0081] Among the thin polarizers obtained by manufacturing methods including a stretching step and a dyeing step in a laminated state, those obtained by a manufacturing method including a stretching step in a boric acid aqueous solution as described in Japanese Patent Nos. 4751486, 4751481, and 4815544 are preferred because they can be stretched at a high magnification and have improved polarization performance. In particular, those obtained by a manufacturing method including a supplementary in-air stretching step before stretching in a boric acid aqueous solution as described in Japanese Patent Nos. 4751481 and 4815544 are preferred. These thin polarizers can be obtained by a manufacturing method including a stretching step and a dyeing step of a polyvinyl alcohol-based resin (hereinafter also referred to as PVA-based resin) layer and a stretching resin substrate in a laminated state. With this manufacturing method, even if the PVA-based resin layer is thin, it can be stretched without problems such as breakage due to stretching because it is supported by the stretching resin substrate.

[0082] The transparent protective film is made of a thermoplastic resin that exhibits excellent transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose-based resin films, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The transparent protective film may contain one or more suitable additives. Examples of additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, even more preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the thermoplastic resin in the transparent protective film is 50% by weight or less, the inherent high transparency of the thermoplastic resin may not be fully exhibited.

[0083] The material for forming the transparent protective film is preferably one that is excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc., and in particular, a moisture permeability of 150 g / m 2 / 24h or less is more preferable, and 140g / m 2 / 24h or less is particularly preferred, and 120g / m 2 / 24 hours or less is even more preferable.

[0084] The surface of the transparent protective film to which the polarizer is not bonded can be provided with a functional layer such as a hard coat layer, an antireflection layer, an antisticking layer, a diffusion layer, an antiglare layer, etc. The functional layer such as the hard coat layer, the antireflection layer, the antisticking layer, the diffusion layer, or the antiglare layer can be provided on the transparent protective film itself, or can be provided separately from the transparent protective film.

[0085] The thickness of the transparent protective film can be determined as appropriate, but is generally about 1 to 500 μm, preferably 1 to 300 μm, more preferably 5 to 200 μm, further preferably 10 to 200 μm, and more preferably 20 to 80 μm, from the viewpoints of workability such as strength and handleability, thinness, etc.

[0086] As the transparent protective film, a retardation film having a front retardation of 40 nm or more and / or a thickness direction retardation of 80 nm or more can be used. The front retardation is usually controlled in the range of 40 to 200 nm, and the thickness direction retardation is usually controlled in the range of 80 to 300 nm. When a retardation film is used as the transparent protective film, the retardation film also functions as the transparent protective film, thereby enabling a thinner film to be achieved.

[0087] Examples of the retardation film include a birefringent film obtained by uniaxially or biaxially stretching a polymer material, an oriented film of a liquid crystal polymer, an oriented layer of a liquid crystal polymer supported by a film, etc. The thickness of the retardation film is not particularly limited, but is generally about 20 to 150 μm.

[0088] The retardation film may be a film satisfying the following formulas (1) to (3): 0.70<Re

[450] / Re

[550] <0.97 (1) 1.5×10 -3 < Δn < 6 × 10 -3 ... (2) 1.13<NZ<1.50 ... (3) (wherein Re

[450] and Re

[550] are in-plane retardation values ​​of the retardation film measured at 23°C with light of wavelengths of 450 nm and 550 nm, respectively; Δn is in-plane birefringence, which is nx-ny, where nx and ny are the refractive indices in the slow axis direction and the fast axis direction of the retardation film, respectively; and NZ is the ratio of nx-nz, which is the birefringence in the thickness direction, to nx-ny, which is the in-plane birefringence, where nz is the refractive index in the thickness direction of the retardation film).

[0089] The polarizing film according to the present invention may be provided with a retardation layer. The retardation layer may be a single layer or multiple layers, and the retardation layer may also serve as a protective layer for the polarizer.

[0090] A liquid crystalline compound is preferably used to form the retardation layer, and a solvent containing the liquid crystalline compound can be applied using, for example, a wire bar, a gap coater, a comma coater, a gravure coater, a slot die, or the like. In this case, the applied liquid crystalline solution may be dried naturally or by heating. It is preferable that the liquid crystalline solution be applied at a concentration lower than the isotropic phase-liquid crystal phase transition concentration, i.e., in an isotropic phase state. In this case, stable alignment can be achieved by methods such as rubbing treatment or photoalignment.

[0091] When the polarizing film according to the present invention is a polarizing film in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, it can be preferably produced by the following production method.

[0092] A method for producing a polarizing film in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, the adhesive layer being a cured layer of a curable resin composition constituted by at least a first composition and a second composition, the first composition containing at least a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group, which may have a substituent, and boric acid, and the second composition contains at least a compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 may form a cyclic heterocycle), and the method for producing a polarizing film includes: a first coating step of coating a first composition on the bonding surface of a polarizer; a second coating step of coating a second composition on the bonding surface of a transparent protective film; a bonding step of bonding the polarizer and the transparent protective film together; and an adhesion step of bonding the polarizer and the transparent protective film together via an adhesive layer obtained by curing the curable resin composition by irradiating the polarizer surface or the transparent protective film surface with active energy rays. Each step will be described below.

[0093] In the above-described manufacturing method, the curable resin composition is composed of a first composition and a second composition. However, in the polarized film according to the present invention, the adhesive layer may be composed of a cured product layer of a single curable resin composition. The first composition contains at least a compound represented by general formula (1) and boric acid. If necessary, the first composition may also contain a curable component such as a compound represented by general formula (2).

[0094] The first composition may contain a solvent and an additive. A solvent capable of stabilizing and dissolving or dispersing the compound represented by general formula (1) is preferred. Such a solvent may be an organic solvent, water, or a mixture thereof. Examples of the solvent include esters such as ethyl acetate, butyl acetate, and 2-hydroxyethyl acetate; ketones such as methyl ethyl ketone, acetone, cyclohexanone, methyl isobutyl ketone, diethyl ketone, methyl n-propyl ketone, and acetylacetone; cyclic ethers such as tetrahydrofuran (THF) and dioxane; aliphatic or alicyclic hydrocarbons such as n-hexane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic alcohols such as methanol, ethanol, n-propanol, isopropanol, and cyclohexanol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and diethylene glycol monoethyl ether; and glycol ether acetates such as diethylene glycol monomethyl ether acetate and diethylene glycol monoethyl ether acetate. Examples of additives include binder resins, surfactants, plasticizers, tackifiers, low-molecular-weight polymers, polymerizable monomers, surface lubricants, leveling agents, antioxidants, corrosion inhibitors, light stabilizers, ultraviolet absorbers, polymerization inhibitors, silane coupling agents, titanium coupling agents, inorganic or organic fillers, metal powders, particles, foil-like materials, etc. The binder resin may be transparent, and examples thereof include polymers such as acrylic resins, styrene resins, polyvinyl alcohol resins, urethane resins, polyester resins, polypropylene resins, polyethylene resins, epoxy resins, and polycarbonate resins.

[0095] In the above-described production method, the curable resin composition is composed of a first composition and a second composition, and when the first composition contains a solvent such as water, the content of the compound represented by general formula (1) in the curable resin composition containing the first composition is preferably 0.05 to 5 mass%, and more preferably 1.0 to 3.0 mass%, excluding the content of the solvent. Similarly, the content of boric acid in the curable resin composition is preferably 0.1 to 2 mass%, and more preferably 0.2 to 1.0 mass%.

[0096] From the viewpoint of improving the humidification reliability of the polarization properties of the polarized film to be produced, the polarizer used in the above production method preferably contains 10 to 22 mass % of boric acid. Furthermore, when the proportion of boric acid contained in the polarizer is A mass % and the proportion of boric acid contained in the curable resin composition is B mass %, A:B is preferably 1:0.001 to 1:0.1, and more preferably A:B is 1:0.01 to 1:0.05.

[0097] The second composition contains at least the compound represented by the general formula (2). If necessary, the second composition may contain the compound represented by the general formula (1) and / or boric acid.

[0098] In the above-described polarizing film manufacturing method, a first composition is applied to the bonding surface of a polarizer in a first coating step, and a second composition is applied to a transparent protective film in a second coating step. The method for applying the curable resin composition alone or the first composition and the second composition together is appropriately selected depending on the viscosity of the composition and the desired thickness, and examples thereof include a reverse coater, a gravure coater (direct, reverse, or offset), a bar reverse coater, a roll coater, a die coater, a bar coater, and a rod coater. The viscosity of the curable resin composition alone or the first composition and the second composition is preferably 3 to 100 mPa·s, more preferably 5 to 50 mPa·s, and most preferably 10 to 30 mPa·s. High viscosity compositions are undesirable because they result in poor surface smoothness and poor appearance after coating. Therefore, each composition can be heated or cooled to adjust the viscosity to a preferred range before application. If the first composition contains water as a solvent, a drying step may be performed after the first coating step.

[0099] From the viewpoint of improving the humidification reliability of the polarization properties of the polarizing film, the thickness before drying after the first coating step is preferably 0.6 to 2.0 μm, and the thickness after drying is preferably 0.3 to 1.0 μm. The coating thickness in the second coating step may be appropriately adjusted so as to obtain the desired adhesive layer thickness.

[0100] The polarizer and / or transparent protective film may be subjected to a surface modification treatment before the coating process. It is particularly preferable to perform a surface modification treatment on the polarizer. Examples of surface modification treatments include corona treatment, plasma treatment, and Itro treatment, with corona treatment being particularly preferable. Corona treatment generates reactive functional groups such as carbonyl groups and amino groups on the polarizer surface, improving adhesion to the adhesive layer. Furthermore, the ashing effect removes foreign matter from the surface and reduces surface irregularities, allowing the production of a polarized film with excellent appearance characteristics.

[0101] The polarizer and the transparent protective film are bonded together via the curable resin compositions (first composition + second composition) applied as described above using a roll laminator or the like (bonding step).

[0102] After the polarizer and the transparent protective film are bonded together, the curable resin composition is cured by irradiation with active energy rays (electron beams, ultraviolet rays, visible light, etc.) to form an adhesive layer. The active energy rays (electron beams, ultraviolet rays, visible light, etc.) can be irradiated from any appropriate direction.

[0103] When irradiating with electron beams, any suitable irradiation conditions can be used as long as they are sufficient to cure the curable resin composition. For example, the acceleration voltage for electron beam irradiation is preferably 5 kV to 300 kV, more preferably 10 kV to 250 kV. If the acceleration voltage is less than 5 kV, the electron beam may not reach the adhesive, resulting in insufficient curing. If the acceleration voltage is greater than 300 kV, the penetration power through the sample may be too strong, potentially damaging the polarizer and transparent protective film. The irradiation dose is 5 to 100 kGy, more preferably 10 to 75 kGy. If the irradiation dose is less than 5 kGy, the adhesive may not be sufficiently cured. If the irradiation dose is greater than 100 kGy, the optical functional layer and substrate film may be damaged, resulting in reduced mechanical strength and yellowing, and the desired optical properties may not be achieved.

[0104] Electron beam irradiation is usually performed in an inert gas atmosphere, but if necessary, it may be performed in the atmosphere or with a small amount of oxygen introduced. Depending on the materials of the polarizer and the transparent protective film, by appropriately introducing oxygen, oxygen inhibition is intentionally caused on the optical functional layer and the substrate film surface that are first hit by the electron beam, which prevents damage to the polarizer and the transparent protective film and allows the electron beam to be efficiently irradiated only on the adhesive.

[0105] When producing the polarized film of the present invention, it is preferable to use active energy rays that include visible light in the wavelength range of 380 nm to 450 nm, and particularly active energy rays that have the highest exposure dose of visible light in the wavelength range of 380 nm to 450 nm. When using ultraviolet light and visible light, if a transparent protective film with ultraviolet absorption ability (an ultraviolet-opaque transparent protective film) is used, light with wavelengths shorter than approximately 380 nm is absorbed, and therefore light with wavelengths shorter than 380 nm does not reach the curable resin composition and does not contribute to the polymerization reaction. Furthermore, light with wavelengths shorter than 380 nm absorbed by the polarizer or transparent protective film is converted into heat, which generates heat in the polarizer or transparent protective film itself, causing defects such as curling and wrinkling in the polarized film. Therefore, when ultraviolet light or visible light is used in the present invention, it is preferable to use an active energy ray generator that does not emit light with a wavelength shorter than 380 nm. More specifically, the ratio of the integrated illuminance in the wavelength range of 380 to 440 nm to the integrated illuminance in the wavelength range of 250 to 370 nm is preferably 100:0 to 100:50, and more preferably 100:0 to 100:40. When producing the polarized film of the present invention, active energy rays are preferably emitted from a gallium-encapsulated metal halide lamp or an LED light source emitting light in the wavelength range of 380 to 440 nm. Alternatively, light sources that emit ultraviolet and visible light, such as low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, incandescent lamps, xenon lamps, halogen lamps, carbon arc lamps, metal halide lamps, fluorescent lamps, tungsten lamps, gallium lamps, excimer lasers, or sunlight, can also be used. A bandpass filter can also be used to block ultraviolet light with a wavelength shorter than 380 nm. In order to prevent curling of the polarizing film while improving the adhesive performance of the adhesive layer between the polarizer and the transparent protective film, it is preferable to use active energy rays obtained by using a gallium-encapsulated metal halide lamp and passing through a bandpass filter capable of blocking light with wavelengths shorter than 380 nm, or active energy rays with a wavelength of 405 nm obtained by using an LED light source.

[0106] When the polarizing film according to the present invention is produced on a continuous line, the line speed depends on the curing time of the curable resin composition, but is preferably 1 to 500 m / min, more preferably 5 to 300 m / min, and even more preferably 10 to 100 m / min. If the line speed is too slow, productivity will be poor or the damage to the optical polarizer or transparent protective film will be too great, making it impossible to produce a polarizing film that can withstand durability tests and the like. If the line speed is too high, the curing of the curable resin composition will be insufficient, and the desired adhesiveness may not be achieved.

[0107] The polarizing film described above or an optical film laminated with at least one polarizing film may also be provided with an adhesive layer for adhering to other components such as a liquid crystal cell. The adhesive for forming the adhesive layer is not particularly limited, and may be appropriately selected and used, for example, from an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, or a rubber-based polymer. In particular, adhesives that have excellent optical transparency, adequate adhesive properties such as wettability, cohesion, and adhesiveness, and excellent weather resistance and heat resistance, such as acrylic adhesives, are preferably used.

[0108] The adhesive layer can be provided on one or both sides of the polarizing film or optical film as a superimposed layer of layers with different compositions or types. When provided on both sides, the adhesive layers on the front and back of the polarizing film or optical film can have different compositions, types, thicknesses, etc. The thickness of the adhesive layer can be determined appropriately depending on the intended use, adhesive strength, etc., and is generally 1 to 500 μm, preferably 1 to 200 μm, and particularly preferably 1 to 100 μm.

[0109] The exposed surface of the adhesive layer is covered with a temporary separator to prevent contamination until the adhesive layer is put into practical use. This prevents contact with the adhesive layer during normal handling. As the separator, apart from the thickness requirements described above, any suitable conventional separator can be used, such as a suitable thin sheet such as a plastic film, rubber sheet, paper, cloth, nonwoven fabric, net, foam sheet, metal foil, or a laminate thereof, optionally coated with a suitable release agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based release agent.

[0110] The polarizing film or optical film of the present invention can be preferably used to form various devices such as liquid crystal displays. The formation of a liquid crystal display can be carried out in a conventional manner. That is, a liquid crystal display is generally formed by appropriately assembling a liquid crystal cell, a polarizing film or optical film, and, if necessary, components such as an illumination system, and incorporating a drive circuit. However, in the present invention, there are no particular limitations except for the use of the polarizing film or optical film of the present invention, and the method can be carried out in a conventional manner. Any type of liquid crystal cell, such as a TN type, STN type, or π type, can be used.

[0111] Appropriate liquid crystal display devices can be formed, such as those in which an optical laminate is disposed on one or both sides of a liquid crystal cell, or those in which a backlight or reflector is used in the illumination system. In such cases, the optical laminate according to the present invention can be disposed on one or both sides of the liquid crystal cell. When optical laminates are disposed on both sides, they may be the same or different. Furthermore, when forming a liquid crystal display device, appropriate components such as a diffuser, anti-glare layer, anti-reflection film, protective plate, prism array, lens array sheet, light diffuser, backlight, etc. can be disposed in one or more layers at appropriate positions.

[0112] Examples of the present invention will be described below, but the embodiments of the present invention are not limited to these.

[0113] <Polarizer> A laminate formed by forming a 9 μm-thick PVA layer on an amorphous PET substrate was subjected to in-air auxiliary stretching at a stretching temperature of 130°C to form a stretched laminate. The stretched laminate was then dyed to form a dyed laminate. The dyed laminate was then stretched in a boric acid solution at a stretching temperature of 65°C to form an optical film laminate including a 5 μm-thick PVA layer, in which the dyed laminate was stretched together with the amorphous PET substrate to a total stretch ratio of 5.94. This two-stage stretching process resulted in highly oriented PVA molecules in the PVA layer formed on the amorphous PET substrate, and iodine adsorbed by dyeing was highly oriented in one direction as a polyiodine ion complex, forming a thin polarizer. Polarizers with different boric acid contents were produced by appropriately varying the boric acid concentration in the bath during the above-mentioned stretching in boric acid solution.

[0114] <Transparent protective film> Transparent protective film 1: triacetyl cellulose-based resin film (product name "TJ25", manufactured by Fujifilm Corporation)

[0115] <Active energy rays> Visible light (gallium-filled metal halide lamp) was used as the active energy rays. Irradiation device: Light HAMMER10 manufactured by Fusion UV Systems, Inc. Bulb: V bulb Peak irradiance: 1600 mW / cm 2 , cumulative irradiation dose 1000 / mJ / cm 2 The illuminance of visible light was measured using a Sola-Check system manufactured by Solatell.

[0116] (Preparation of Curable Resin Composition) The first composition and the second composition constituting the curable resin compositions of Examples 1 and 2 and Comparative Examples 1 to 3 were prepared according to the formulations in Table 1. The values ​​in the table indicate the weight percentages when the total amount of each composition is taken as 100 mass %. Note that, because the water blended into the first composition is removed in the drying step after the first coating step, water was omitted from the calculation of the composition of the curable resin composition (total of the first composition and the second composition).

[0117] The materials constituting the curable resin composition are as follows: (Curable components) N-Acryloylmorpholine (compound represented by general formula (2)): trade name "ACMO", manufactured by Kojin Co., Ltd. 1,9-Nonanediol diacrylate: trade name "Light Acrylate 1.9ND-A", manufactured by Kyoeisha Chemical Co., Ltd. Phenoxydiethylene glycol acrylate: trade name "Light Acrylate P2H-A", manufactured by Kyoeisha Chemical Co., Ltd. (Acrylic oligomers) Acrylic oligomer obtained by polymerizing (meth)acrylic monomers: trade name "ARUFON UP-1190", manufactured by Toagosei Co., Ltd. (Initiators) 2-Methyl-4'-methylthio-2-morpholinopropiophenone: trade name "Omnirad 907", manufactured by IGM Resins B.V. Diethylthioxanthone: trade name "KAYACURE DETX-S (referred to as "DETX-S" in Table 1)" manufactured by Nippon Kayaku Co., Ltd. (leveling agent) Trade name "BYK-UV3505" manufactured by BYK Corporation (compound represented by general formula (1)) 3-methacrylamidophenylboronic acid: trade name "MAPBA" manufactured by Junsei Chemical Co., Ltd. (boric acid) (surface conditioner) Trade name "EXP.4200" manufactured by Nissin Chemical Industry Co., Ltd.

[0118] (Production of Polarized Film) Example 1 Using an MCD coater (manufactured by Fuji Machinery Co., Ltd.) (cell shape: honeycomb, gravure roll ruling: 1000 rolls / inch, rotation speed 140% / relative to line speed), the second composition was coated to a coating thickness of 1.0 μm on the bonding surface of the transparent protective film 1 (second coating step). The first composition was coated on the thin polarizer surface side of the optical film laminate to a coating thickness of 0.8 to 1.2 μm before drying (first coating step), and then water contained in the first composition was removed using a blower (drying step). The coating thickness after drying was 0.4 to 0.6 μm. Next, the transparent protective film 1 and the optical film laminate including the thin polarizer were bonded together from the coated side using a roller (bonding step). The thin polarizer and the transparent protective film were then bonded together via an adhesive layer obtained by irradiating the laminate with visible light from an active energy ray irradiation device from the side of the laminated transparent protective film, thereby curing the curable resin composition composed of the first composition and the second composition. Next, the amorphous PET substrate of the optical film laminate was peeled off.

[0119] Example 2 and Comparative Examples 1 to 3 Polarized films were produced in the same manner as in Example 1, except that the contents and presence or absence of the compound represented by general formula (1) and boric acid in the first composition used in Example 1, and the boric acid content of the polarizer, etc. were changed to those shown in Table 1.

[0120] <Evaluation of Humidity Reliability of Polarizing Properties of Polarizing Film> A polarizing film (sample for evaluating humidity durability test) was prepared by bonding a polarizing film to one side of a 0.7 mm thick non-alkali glass sheet via an adhesive layer (thickness: 20 μm).

[0121] The obtained polarized film was exposed to an environment of 60°C and 95% humidity for 240 hours, and the degree of polarization before and after exposure was measured using a spectrophotometer with an integrating sphere (V7100 manufactured by JASCO Corporation), and the change in the degree of polarization ΔPz (%) = |(degree of polarization before exposure (%)) - (degree of polarization after exposure (%))| was calculated. It was determined that the smaller the change in the degree of polarization ΔPz (%), the more excellent the humidification reliability of the polarization characteristics in a severe humidified environment.

[0122] <Evaluation of Edge Discoloration of Polarizing Properties of Polarizing Film> Using the same samples as those for the humidification reliability described above, the discoloration length (from the start of discoloration to the edge of the sample) on all four sides was measured using an electron microscope, and it was determined that the smaller the value, the better the edge discoloration resistance under severe humidification environments.

[0123] <Measurement of Thickness of Compatible Layer in Adhesive Layer of Polarizing Film> The cross section of the polarizing plate was observed and measured using an SEM (SU8200 manufactured by Hitachi High-Technologies Corporation).

[0124]

Claims

1. A polarizing film having a cured material layer on at least one surface of a polarizer, the cured material layer being represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and boric acid.

2. The polarizing film according to claim 1, wherein the mass ratio of the compound represented by general formula (1) to the boric acid in the curable resin composition is 1:0.1 to 1:30.

0.

3. The curable resin composition further comprises a compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 The polarizing film according to claim 1 , wherein R 1 is a cyclic heterocycle.

4. The polarized film according to claim 1, wherein the content of the compound represented by general formula (1) in the curable resin composition is 0.05 to 5 mass %, and the content of the boric acid is 0.1 to 2 mass %.

5. The polarizing film according to claim 1, wherein the polarizer contains 10 to 22% by mass of boric acid.

6. The polarized film according to claim 1, wherein the proportion of boric acid contained in the polarizer is A% by mass, and the proportion of boric acid contained in the curable resin composition is B% by mass, such that A:B=1:0.001 to 1:0.

1.

7. The polarizing film according to claim 1, wherein the thickness of the cured layer is 1 μm or more and 2 μm or less.

8. The polarizing film according to claim 1, which comprises a polarizing element and a transparent protective film laminated on at least one surface thereof via an adhesive layer, the adhesive layer being the cured material layer.

9. The polarizing film according to claim 8, wherein the transparent protective film is a triacetyl cellulose-based resin film.

10. The polarizing film according to claim 8, further comprising a compatible layer between said transparent protective film and said adhesive layer, said compatible layer being compatible with said transparent protective film and said adhesive layer.

11. An optical film comprising at least one laminate of the polarizing film according to claim 1.

12. An image display device comprising the polarizing film according to claim 1 or the optical film according to claim 11.

13. A method for producing a polarizing film in which a transparent protective film is laminated on at least one surface of a polarizer via an adhesive layer, the adhesive layer being a cured layer of a curable resin composition composed of at least a first composition and a second composition, the first composition being at least a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and boric acid, A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6a first coating step of coating a first composition on a bonding surface of the polarizer, a second coating step of coating a second composition on a bonding surface of the transparent protective film, a bonding step of bonding the polarizer and the transparent protective film together, and a bonding step of bonding the polarizer and the transparent protective film together via the adhesive layer obtained by irradiating the polarizer surface side or the transparent protective film surface side with active energy rays to cure the curable resin composition.

14. The method for producing a polarized film according to claim 13, wherein the mass ratio of the compound represented by general formula (1) to the boric acid in the first composition is 1:0.1 to 1:30.

0.

15. The method for producing a polarized film according to claim 13, wherein the content of the compound represented by general formula (1) in the curable resin composition is 0.05 to 5 mass %, and the content of the boric acid is 0.1 to 2 mass %.

16. The method for producing a polarizing film according to claim 13, wherein the polarizer contains 10 to 22% by mass of boric acid.

17. The method for producing a polarized film according to claim 13, wherein the proportion of boric acid contained in the polarizer is A% by mass, and the proportion of boric acid contained in the curable resin composition is B% by mass, such that A:B=1:0.001 to 1:0.

1.

18. The method for producing a polarized film according to claim 13, wherein the first composition after the first coating step has a coating thickness before drying of 0.6 to 2.0 μm and a coating thickness after drying of 0.3 to 1.0 μm.

19. The method for producing a polarizing film according to claim 13, wherein the thickness of the adhesive layer is 1 μm or more and 2 μm or less.

Citation Information

Patent Citations

  • Active energy ray-polymerizable resin composition and laminate

    JP2016172801A

  • Manufacturing method for polarizing film

    JP2021039269A

  • Polarizing plate and liquid crystal display having the same

    US20140125924A1

  • Adhesive agent composition, adhesive agent composition for polarizing plate, adhesive agent for polarizing plate, and polarizing plate manufactured using said adhesive agent

    WO2015022825A1

  • Polarizing film, method for manufacturing same, optical film, and image display device

    WO2019163749A1