Zn-al-mg-si-based plated steel sheet

The Zn-Al-Mg-Si plated steel sheet addresses the challenges of chemical conversion and corrosion resistance by controlling Si alloy phase formation, resulting in improved chemical conversion treatment and blistering suppression, and enhanced corrosion resistance at dissimilar joints with aluminum alloys.

WO2024247426A1PCT designated stage expired Publication Date: 2024-12-05JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008337
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-03-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing Zn-Al-Mg-based plated steel sheets face challenges in chemical conversion treatment properties and corrosion resistance, particularly at dissimilar joints with aluminum alloy parts, and suffer from blistering issues due to the formation of Si alloy phases on the surface.

Method used

A Zn-Al-Mg-Si plated steel sheet is developed with a specific composition and manufacturing process that suppresses the formation of Si alloy phases on the surface, forming SiO2 oxide phases instead, which enhances chemical conversion treatment and corrosion resistance, and controls the Si alloy phase inside the plating layer to prevent blistering.

Benefits of technology

The Zn-Al-Mg-Si plated steel sheet exhibits excellent chemical conversion treatment properties, effectively suppresses blistering under the coating film, and demonstrates superior corrosion resistance at dissimilar joints with aluminum alloy parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008337_05122024_PF_FP_ABST
    Figure JP2024008337_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a Zn-Al-Mg-Si-based plated steel sheet that exhibits excellent chemical conversion treatment properties, suppression of downward bulging of a coating film, and corrosion resistance at a boundary between members of different types. A Zn-Al-Mg-Si-based plated steel sheet according to the present invention is characterized by having a foundation steel sheet and a plating layer formed on at least one surface of the foundation steel sheet, and is characterized in that: the plating layer has a composition containing, in mass%, 0.50-3.00% of Mg, 0.10-3.00% of Al, 0.010-0.20% of Si, and 0.30% or less of Fe, the remaining portion being Zn and unavoidable impurities, and has a Zn-Al-MgZn2 three-component eutectic structure; and, on the three-component eutectic structure, a needle-shaped Mg2Si alloy phase exists at a number density of less than 100000 pieces / mm2 in a backscattered electron image acquired by a scanning electron microscope at a magnification of 5000 times at an acceleration voltage of 7.0 kV, and, at an acceleration voltage of 15.0 kV with the same condition, the needle-shaped Mg2Si alloy phase exists at a number density of 500 pieces / mm2 or more and a needle-shaped SiO2 oxide phase exists at a number density of 100000 pieces / mm2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Zn-Al-Mg-Si plated steel sheet

[0001] The present invention relates to a Zn-Al-Mg-Si plated steel sheet.

[0002] Zinc plating, which inhibits iron corrosion through sacrificial corrosion protection, is excellent in rust prevention performance and economy, and is widely used to manufacture steel materials with high corrosion resistance. In particular, hot-dip galvanized steel materials, in which a plating layer is formed by immersing steel materials in molten zinc, have a simpler manufacturing process and are cheaper than electrogalvanized steel materials, and therefore demand for hot-dip galvanized steel materials is increasing across industries such as automobiles, home appliances, and building materials. However, due to the worsening of air pollution and corrosive environments associated with industrial advancement and the depletion of zinc resources due to a significant increase in zinc use, there has been a demand for plated steel materials that are more corrosion-resistant than conventional zinc plating and that also require less zinc.

[0003] Patent Document 1 discloses a Zn-Al-Mg plated steel material in which elements such as aluminum (Al) and magnesium (Mg) are added to zinc (Zn) to improve the corrosion resistance of the steel material. Patent Document 2 reports that adding silicon (Si) to a Zn-Al-Mg plated layer improves the corrosion resistance of the plated steel material at the flat and edge portions compared to conventional Zn-Al-Mg plated steel sheets. Patent Document 3 reports that adding Si to the plated layer of a Zn-Al-Mg plated steel sheet and concentrating Si at the interface between the plated layer and the base steel sheet imparts fracture toughness to the plated layer and improves corrosion resistance after processing. Patent Document 4 also reports that adding fine silica (SiO 2 It has been reported that forming a resin film containing Zn—Al—Mg on the surface of the plating layer of a Zn—Al—Mg-plated steel sheet strengthens the film and improves the workability and corrosion resistance of the processed part.

[0004] Japanese Patent Laid-Open No. 4-147955 Japanese Patent Laid-Open No. 2005-82834 Japanese Patent Laid-Open No. 2021-508771 Japanese Patent Laid-Open No. 2004-338397

[0005] However, further improvements were needed in the chemical conversion treatability of plated steel sheets and in the suppression of under-paint blistering from the edges.In addition, as the use of aluminum alloy sheets and aluminum die-castings in automobile bodies increases in order to drastically reduce the weight of automobiles, corrosion resistance at dissimilar joints between plated steel sheet members and aluminum alloy members has become a new required property, and corrosion resistance at dissimilar joints with aluminum alloy members has been desired.

[0006] In view of the above problems, an object of the present invention is to provide a Zn-Al-Mg-Si plated steel sheet that has excellent chemical conversion treatability, sufficiently suppresses under-coat blistering from the edges, and has excellent corrosion resistance at dissimilar joints where the processed steel sheet comes into contact with an aluminum alloy.

[0007] As a result of intensive research to solve the above problems, the present inventors have found the following: 2 By suppressing the formation of a Si alloy phase in the surface layer of the plating layer, excellent chemical conversion treatability can be obtained. 2 The formation of the oxide phase can improve the corrosion resistance of the dissimilar joint at the contact area between the processed part and the aluminum alloy. 2 The formation of the Si alloy phase inside the coating layer can suppress the undercoat blistering from the sheared edge after coating. In a method for producing such a coated steel sheet, a salt water application step is carried out after coating the base steel sheet, thereby reducing the Mg content of the surface layer of the coating layer. 2 Reduce the Si alloy phase and replace it with SiO 2 An oxide phase can be formed.

[0008] That is, the gist and configuration of the present invention are as follows.

[0009] [1] A steel sheet having a base steel sheet and a coating layer formed on at least one surface of the base steel sheet, wherein the coating layer contains, in mass%, Mg: 0.50 to 3.00%, Al: 0.10 to 3.00%, Si: 0.010 to 0.20%, and Fe: 0.30% or less, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn 2and a ternary eutectic structure, wherein the Zn—Al—MgZn ternary eutectic structure is found in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope. 2 On the ternary eutectic structure, needle-shaped Mg 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 Less than (0 pieces / mm 2 In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn—Al—MgZn 2 On the ternary eutectic structure, needle-shaped Mg 2 The number density of the Si alloy phase is 500 / mm 2 or more, and in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn—Al—MgZn 2 On the ternary eutectic structure, needle-shaped SiO 2 The oxide phase has a number density of 100,000 pieces / mm 2 Zn-Al-Mg-Si based plated steel sheet characterized by the presence of the above.

[0010] The present invention can provide a Zn-Al-Mg-Si plated steel sheet that has excellent chemical conversion treatability, sufficiently suppresses under-coat blistering from the edges, and has excellent corrosion resistance at dissimilar joints where the processed steel sheet comes into contact with an aluminum alloy.

[0011] (a) is a backscattered electron image at 5000x magnification obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV in one example of the present invention, (b) to (e) are Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, obtained by composition analysis using EDS. (a) is a backscattered electron image at 5000x magnification obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV in one example of the present invention, and (b) to (f) are Mg distribution, Si distribution, Al distribution, Zn distribution, and O distribution, respectively, obtained by composition analysis using EDS.

[0012] Hereinafter, an embodiment of the Zn-Al-Mg-Si plated steel sheet according to the present invention will be described. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.

[0013] A Zn-Al-Mg-Si based plated steel sheet according to one embodiment of the present invention comprises a base steel sheet and a plating layer formed on at least one surface of the base steel sheet. The plating layer contains, by mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities. 2 Furthermore, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, the Zn—Al—MgZn ternary eutectic structure is 2 On the ternary eutectic structure, needle-shaped Mg 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 Less than (0 pieces / mm 2 In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn—Al—MgZn 2 On the ternary eutectic structure, needle-shaped Mg 2 The number density of the Si alloy phase is 500 pieces / mm 2 or more, and in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn—Al—MgZn 2 On the ternary eutectic structure, needle-shaped SiO 2 The oxide phase has a density of 100,000 particles / mm 2 The presence of more than one

[0014] The type of substrate steel sheet used in the present invention is not particularly limited, and for example, a hot-rolled steel sheet or hot-rolled steel strip that has been pickled and descaled, or a cold-rolled steel sheet or cold-rolled steel strip obtained by cold rolling such a hot-rolled steel sheet or hot-rolled steel strip, can be used. There is also no particular limit to the thickness of the substrate steel sheet, but it is preferably 0.7 to 2.0 mm.

[0015] Next, the composition of the Zn-Al-Mg-Si based plating layer in the present invention will be described.

[0016] When the Mg content in the plating layer is less than 0.50 mass%, a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using the scanning electron microscope shows that the Mg content is 2 Si alloy phase and SiO 2 The number density of the oxide phase is not sufficient, and the effect of suppressing under-coating blistering from the edge and improving the corrosion resistance of dissimilar joints at the contact area between the processed part and the aluminum alloy is insufficient. Therefore, the Mg content in the plating layer is set to 0.50 mass% or more, and preferably 1.00 mass% or more. On the other hand, if the Mg content in the plating layer exceeds 3.00 mass%, brittle lumpy MgZn 2 A phase is formed, which makes the plating layer brittle and reduces adhesion, and there is a risk of deterioration in workability and corrosion resistance of the processed part. Therefore, the Mg content in the plating layer is set to 3.00 mass% or less, and preferably 2.50 mass% or less.

[0017] When the content of Al in the plating layer is less than 0.10 mass%, the plating layer contains Zn—Al—MgZn. 2 Ternary eutectic structure is not formed, and Mg 2 Since the Si alloy phase is not sufficiently formed, the effect of suppressing blistering under the coating from the edges is reduced. Therefore, the Al content in the plating layer is set to 0.10 mass% or more, and preferably 0.50 mass% or more. On the other hand, if the Al content in the plating layer exceeds 3.00 mass%, coating peeling occurs from the sheared edges of the plated steel sheet, and suppression of blistering under the coating is insufficient. Therefore, the Al content in the plating layer is set to 3.00 mass% or less, and preferably 2.00 mass% or less.

[0018] When the content of Si in the plating layer is 0.010 mass% or more, Mg is contained in the plating layer together with Mg. 2 The formation of a Si alloy phase contributes to improving the corrosion resistance of the coating layer. This is thought to be due to the following action: 2 Because the Si alloy phase is active, it reacts with water in a corrosive environment and decomposes, forming the Zn-Al-MgZn alloy described below. 2 In the ternary eutectic coating structure, Zn phase, Al phase and MgZn 2 The coating layer sacrificially protects the metal structure containing one or more of the alloy phases. At the same time, the resulting Mg corrosion product forms a protective film, suppressing further corrosion. Under the coating film, the progression of galvanic corrosion with Fe occurring at the sheared edges of the plated steel sheet is suppressed, thereby suppressing blistering that occurs at the sheared edges and becomes apparent on the painted surface. To achieve the above effect, the Si content in the coating layer is set to 0.010% by mass or more, and preferably 0.050% by mass or more. Note that if the Si content is less than 0.010% by mass, the coating layer will contain Mg. 2 On the other hand, if the Si content in the coating layer exceeds 0.20 mass%, a large amount of Mg is distributed even in the surface layer portion of the coating layer. 2 Si alloy phase is formed. Mg 2 The Si alloy phase is easily oxidized to form an oxide layer, which tends to block or inhibit the adhesion of the chemical conversion treatment agent, and therefore there is a concern that the chemical conversion treatability may be reduced. Therefore, the Si content in the plating layer is set to 0.20 mass% or less, and preferably 0.15 mass% or less.

[0019] If the Fe content in the coating layer exceeds 0.30 mass%, the growth of an alloy layer formed at the interface between the base steel sheet and the coating layer increases, resulting in a decrease in workability. Therefore, the Fe content in the coating layer is set to 0.30 mass% or less, and preferably 0.20 mass% or less. On the other hand, the lower limit of the Fe content in the coating layer is not particularly limited, and may be 0.00 mass%.

[0020] The remainder of the composition of the plating layer other than those mentioned above consists of Zn and unavoidable impurities.

[0021] Next, the structure of the Zn-Al-Mg-Si based plating layer will be described. 2 It has a ternary eutectic coating structure, and Mg 2 The coating structure further contains a Zn phase, an Al phase, or an MgZn phase. 2 An alloy phase may be included.

[0022] Mg in Zn-Al-Mg-Si based plating layer 2 If a large amount of Si alloy phase exists in the surface layer of the coating layer, there is a concern that the chemical conversion treatability may be reduced. 2 It is preferable that the Si alloy phase is not formed in the surface layer of the plating layer. 2 When the Si alloy phase is formed inside the coating layer, it suppresses corrosion of the coating that occurs at the sheared edge after painting, suppresses the progress of corrosion under the coating film, and suppresses blistering under the coating film that occurs at the sheared edge. 2 It is preferable that the Si alloy phase is not formed on the surface of the plating layer, but is formed inside the plating layer.

[0023] In the present invention, Mg 2 The phrase "the Si alloy phase is not formed in the surface layer of the plating layer" means that the surface of the plating layer is irradiated with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, and in a backscattered electron image at a magnification of 5000 times, a Zn-Al-MgZn 2 On the ternary eutectic structure, needle-shaped Mg 2 This means that no Si alloy phase is observed. 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 If the content is more than this, there is a concern that the chemical conversion treatability may be reduced. 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 Less than 0 pieces / mm 2 It is more preferable that:

[0024] In the present invention, Mg 2The phrase "the Si alloy phase is formed inside the plating layer" means that a backscattered electron image of Zn-Al-MgZn is obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope and magnifying it at 5000 times. 2 On the ternary eutectic structure, needle-shaped Mg 2 This means that a Si alloy phase is observed. 2 The number density of the Si alloy phase is 500 pieces / mm 2 When the thickness is more than 100 μm, the effect of suppressing the undercoat blister from the sheared end after coating can be obtained. 2 The number density of the Si alloy phase is 500 pieces / mm 2 or more, 1200 pieces / mm 2 On the other hand, Mg formed inside the plating layer 2 The upper limit of the number density of the Si alloy phase is not particularly limited, but the number density is generally 2500 pieces / mm 2 The following is the result.

[0025] Furthermore, inside the plating layer, Mg 2 When the Si alloy phase is corroded, SiO 2 Formation of an oxide phase. SiO formed inside the plating layer 2 When the oxide phase is present together with Zn in a corrosive environment, it promotes the production of basic zinc chloride, which has a strong protective effect, and contributes to improving corrosion resistance. 2 The oxide phase strengthens the plating layer, suppresses the occurrence of cracks when subjected to external stress, and the progression of corrosion after the cracks occur, thereby improving the corrosion resistance of the processed part. 2 It is preferred that an oxide phase is formed.

[0026] In the present invention, SiO 2 The oxide phase is "formed inside the plating layer" when, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the oxide phase is found to be Zn-Al-MgZn. 2 On the ternary eutectic structure, needle-shaped SiO 2This means that an oxide phase is observed. SiO formed inside the plating layer 2 The number density of the oxide phase is 100,000 pieces / mm 2 If the thickness is more than 1000 nm, corrosion resistance of the processed portion can be obtained. 2 The density of the oxide phase is 100,000 pieces / mm 2 or more, 150,000 pieces / mm 2 On the other hand, the SiO formed inside the plating layer is preferably 2 The upper limit of the number density of the oxide phase is not particularly limited, but the number density is generally 380,000 pieces / mm 2 The following is the result.

[0027] SiO 2 The formation of the oxide phase requires the control of the Si content in the plating bath components and the control of the reducibility (O 2 If such control or post-treatment process is insufficient, Mg 2 If the Si alloy phase is present in the surface layer of the coating, the chemical conversion treatment property may be reduced, or if Mg is present inside the coating, 2 If the Si alloy phase is too small and swelling from the sheared end after painting cannot be suppressed, or if SiO 2 The oxide phase may not be sufficiently formed, resulting in a decrease in corrosion resistance of the processed area.

[0028] 1(a) to (e) show backscattered electron images (5000x magnification) and EDS analysis results observed when the surface of the plating layer of a Zn-Al-Mg-Si-plated steel sheet manufactured in one embodiment of the present invention was irradiated with an electron beam using a scanning electron microscope at an accelerating voltage of 7.0 kV. FIG. 1(a) is a backscattered electron image of the Zn-Al-Mg-Si-plated layer, and (b) to (e) are Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, obtained by composition analysis using EDS. As shown in FIGS. 1(a) to (e), Mg 2 The Si alloy phase has a needle-like shape where the distributions of Mg and Si overlap, and the Zn-Al-MgZn 2 It can be seen that it is in a ternary eutectic structure.

[0029] 2(a) to 2(f) show backscattered electron images (5000x magnification) and EDS analysis results observed when the surface of the plating layer of a Zn-Al-Mg-Si-plated steel sheet manufactured in one example of the present invention was irradiated with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope. Fig. 2(a) is a backscattered electron image of the Zn-Al-Mg-Si-plated layer, and 2(b) to 2(f) are the Mg distribution, Si distribution, Al distribution, Zn distribution, and O distribution, respectively, obtained by composition analysis using EDS. As shown in Figs. 2(a) to 2(f), the Si distribution has a needle-like shape, and the O distribution overlaps with the distributions of Mg, Si, and Al. SiO 2 The oxide phase has a needle-like shape where the distributions of Si and O overlap, and the Zn-Al-MgZn 2 It can be seen that it is in a ternary eutectic structure.

[0030] [Method for Manufacturing Zn-Al-Mg-Si Coated Steel Sheet] Next, a method for manufacturing a Zn-Al-Mg-Si coated steel sheet according to one embodiment of the present invention will be described. The method for manufacturing a Zn-Al-Mg-Si coated steel sheet according to one embodiment of the present invention includes the steps of: immersing a substrate steel sheet in a coating bath containing, by mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance consisting of Zn and unavoidable impurities, thereby coating the substrate steel sheet; gas wiping the substrate steel sheet after the coating to adjust the coating weight of the coating layer formed on the substrate steel sheet; and applying salt water to the surface of the coated steel sheet after the gas wiping. The cooling method for the coated steel sheet after gas wiping and before the salt water coating is not particularly limited, and various methods such as air cooling, air-water cooling, and water cooling can be used.

[0031] By carrying out a salt water application process on the surface of the plated steel sheet, the plating layer is etched and the Mg present inside the plating layer is removed. 2 The Si alloy phase is oxidized. 2 When the Si alloy phase is oxidized, Mg, which has a lower natural potential in a saltwater environment, is selectively dissolved and eluted from the plating layer. As a result, the remaining Si is oxidized and becomes an oxide, SiO 2The oxide phase is formed inside the plating layer. 2 When the oxide phase is present together with Zn in a corrosive environment, it promotes the production of basic zinc chloride, which has a strong protective effect, and contributes to improving corrosion resistance.

[0032] In the method for producing a Zn-Al-Mg-Si plated steel sheet according to the present invention, the base steel sheet to be plated is the same as that described above for the base steel sheet.

[0033] When annealing heat treatment is performed on the base steel sheet before plating treatment, H in the furnace atmosphere during annealing 2 When the concentration is 1% by volume or more, oxides on the surface of the base steel sheet can be suitably reduced. 2 The concentration is preferably 1% by volume or more. 2 When the concentration is 10% by volume or less, the manufacturing cost can be suitably reduced. 2 The concentration is preferably 10% by volume or less. 2 and the remainder is N 2 The temperature of the annealing heat treatment is not particularly limited, but is preferably 600 to 850° C. The time of the annealing heat treatment is also not particularly limited, but is preferably 10 to 60 seconds.

[0034] The coating bath used in the production of the Zn-Al-Mg-Si coated steel sheet according to the present invention has a composition containing, by mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance consisting of Zn and unavoidable impurities. The explanation of each component in the coating bath is the same as the explanation of each component of the coating layer described above. The component composition of the coating bath is equivalent to the component composition of the applied coating layer.

[0035] The coating weight of the plating layer in the plating process is set to 15 g / m from the viewpoint of corrosion resistance. 2 It is preferable that the content is 30 g / m or more. 2 On the other hand, the coating weight of the plating layer is more preferably 100 g / m or more.2 When the coating weight of the plating layer is 100 g / m or less, the manufacturing cost can be suitably reduced. 2 It is preferable that the temperature of the plating bath during plating treatment is 430 to 540°C. If the plating bath temperature is less than 430°C, the fluidity of the plating bath will decrease, which may hinder uniform plating deposition. Therefore, the temperature of the plating bath is preferably 430°C or higher. On the other hand, if the temperature of the plating bath exceeds 540°C, there is a risk of an increase in oxides on the surface of the plating bath due to oxidation of Mg in the plating bath, and erosion of the refractory material in the plating bath by Al and Mg. Therefore, the temperature of the plating bath is preferably 540°C or lower, more preferably 530°C or lower.

[0036] Mg 2 In order to prevent the Si alloy phase from being formed in the surface layer of the plating layer and to form a large amount of it inside the plating layer, it is effective to reduce the reducing property of the gas used in gas wiping. 2 The reduction is very high when the above H 2 When the concentration is 1% by volume or more, if the amount of Si in the plating bath is low, even if the salt water treatment step is performed, the Mg in the plating layer is 2 Si is difficult to oxidize, and a sufficient amount of SiO 2 As a result of extensive research into this point, the inventors of the present invention have found that the O phase during gas wiping is not formed and the desired corrosion resistance of the processed part is not obtained. 2 The higher the concentration, the lower the reducing ability of the gas, and the more Mg is present in the surface layer of the plating layer. 2 As a result, it was found that the SiO of the surface layer of the plating layer is easily formed during corrosion in the salt water treatment process. 2 Reduces oxide phase and SiO inside the plating layer 2 Therefore, the gas species used in gas wiping is O 2 and N 2 It is preferable to use a mixed gas containing the above or air. It is preferable that the atmosphere during gas wiping is atmospheric air.

[0037] The gas used in gas wiping is O 2 and N 2 When the mixed gas contains O 2 When the concentration is 3% by volume or more, even if the Si content in the plating bath is low, Mg is present inside the plating layer. 2 The Si alloy phase is suitably formed, and the effect of contributing to the improvement of corrosion resistance is suitably obtained. 2 The concentration is preferably 3% by volume or more. 2 When the concentration is 15% by volume or less, the manufacturing cost can be suitably reduced. 2 The concentration is preferably 15% by volume or less. 2 The mixed gas used for gas wiping may contain H 2 When the concentration is 7% by volume or more, the Mg in the surface layer of the plating layer 2 The formation of Si alloy phase is suitably suppressed, and Mg 2 The Si alloy phase is formed, and SiO 2 The formation of the oxide phase is favorably promoted.

[0038] Gas wiping may be performed using air. In this case, even if the amount of Si in the plating bath is low, Mg is not easily introduced into the plating layer. 2 During the salt water application process after gas wiping with air, SiO 2 The formation of the oxide phase is suitably promoted, and the effect of contributing to the improvement of corrosion resistance is suitably obtained.

[0039] The method for applying saltwater to the surface of the plated steel sheet after adjusting the coating weight is not particularly limited. For example, saltwater may be applied to the surface of the plated steel sheet, left for a predetermined period of time, and then washed and dried to corrode and oxidize the plating layer of the plated steel sheet. The saltwater used in the saltwater application treatment is not particularly limited, but a sodium chloride (NaCl) aqueous solution is preferred from the viewpoint of production costs. The saltwater concentration is also not particularly limited, but is preferably 0.5 mass% or more and 5.0 mass% or less from the viewpoint of production costs. The leaving time for the saltwater application treatment is preferably 0.5 hours or more from the viewpoint of sufficient oxidation of the plating layer. On the other hand, leaving the saltwater for more than two hours may result in excessive corrosion of the plating layer, reducing the coating weight and potentially deteriorating corrosion resistance. Therefore, the leaving time for the saltwater application treatment is preferably 2 hours or less, and more preferably 1 hour or less.

[0040] For steps and conditions not described in the present invention, conventional methods can be used.

[0041] All Zn-Al-Mg-Si plated steel sheets were produced as samples using a 0.8 mm thick ultra-low carbon cold rolled steel sheet as the base steel sheet using hot dip plating equipment. Each sample was plated using variously changed plating bath compositions, and the plating bath temperature was set to 450°C, which is 30°C higher than the solidification start temperature estimated from the Zn-Al-Mg-Si quaternary equilibrium phase diagram. The base steel sheet was then plated using H 2 (5% by volume) + N 2 The steel sheet was heated in an atmosphere, and the temperature of the base steel sheet when immersed in the coating bath was set to the same temperature as the coating bath temperature, and hot-dip coating was performed in the coating bath for 1 second. Thereafter, the thickness of the coating layer was reduced to 7 μm (50 g / m) by adjusting the flow rate of the wiping gas. 2 The temperature was controlled to a value equivalent to 100°C (equivalent to 100°C). Some samples were further subjected to a saltwater treatment by immersing them in an aqueous solution of 0.5 wt % NaCl for 1 hour, followed by rinsing and drying. Table 1 shows the plating bath composition, the wiping gas composition, and the plating layer composition. In addition, for the salt for saltwater treatment in Table 1, those that underwent water treatment are marked "Yes" and those that did not undergo saltwater treatment are marked "No." The wiping was performed in an air atmosphere.

[0042]

[0043] Each sample of the obtained Zn—Al—Mg—Si plated steel sheet was sheared to a size of 10 × 20 mm. The plating layer of the sheared sample was observed from the surface of the plated steel sheet using a scanning electron microscope to determine the Zn—Al—MgZn 2 The presence or absence of a ternary eutectic structure was confirmed. During the observation, composition analysis by EDS revealed Zn phase, Al phase, MgZn 2 The structure is composed of three phases of the alloy phase, and when the same surface is analyzed by XRD, Zn phase, Al phase, and MgZn phase are found. 2 If alloy phase is confirmed, it is Zn-Al-MgZn 2 "Yes" indicates the presence of a ternary eutectic structure, and "Zn phase, Al phase, and MgZn phase" indicates the presence of a ternary eutectic structure. 2 The structure does not consist of three phases of the alloy phase, and when the same surface is analyzed by XRD, the Zn phase, Al phase, and MgZn phase are not observed. 2 If any of the alloy phases is not confirmed, Zn-Al-MgZn 2 The absence of a crystal structure is indicated as "none" in Table 1.

[0044] The plating layer of the sheared sample was observed from the surface of the plated steel sheet using a scanning electron microscope to determine whether Mg existed in the surface and interior of the plating layer. 2 The state of the Si alloy phase was observed and the number density was evaluated. 2 The number density of the Si alloy phase was evaluated from a backscattered electron image (5000x magnification) observed when irradiating an electron beam at an acceleration voltage of 7.0 kV. 2 The number density of the Si alloy phase was evaluated from a backscattered electron image (5000x magnification) observed when irradiating an electron beam at an accelerating voltage of 15.0 kV.

[0045] After shearing, the plating layer of the sample was observed from the surface of the plated steel sheet using a scanning electron microscope, and the SiO present inside the plating layer was 2 The state of the oxide phase was observed and the number density was evaluated. 2The oxide phase was evaluated by a backscattered electron image (5000x magnification) observed when irradiating with an electron beam at an accelerating voltage of 15.0 kV.

[0046] [Chemical conversion treatability] Next, the chemical conversion treatability of the resulting Zn-Al-Mg-Si plated steel sheets was evaluated. Each sample was sheared to a size of 30 × 30 mm and then phosphate-treated for 90 seconds under the same conditions. The phosphate crystal smearing (the degree of exposure of the plated surface under chemical conversion) was observed from the surface direction of the plated steel sheet using a scanning electron microscope (800x magnification). The secondary electron images were observed from the surface direction of the plated steel sheet, and the state of phosphate crystal smearing (the degree of exposure of the plated surface under chemical conversion) was observed and rated as follows. The results are shown in Table 1 as follows: "◎" for no phosphate crystal smearing and no exposed plated steel sheet surface; "◯" for very slight phosphate crystal smearing and very slight exposed plated steel sheet surface; "△" for very slight phosphate crystal smearing and very slight exposed plated steel sheet surface; and "×" for phosphate crystal smearing and exposed plated surface. A rating of ◎ or ◯ was considered a pass, and a rating of △ or × was considered a fail.

[0047] [Undercoat blistering from sheared edges after painting] Next, the suppression of undercoat blistering from sheared edges on painted Zn-Al-Mg-Si-plated steel sheets was evaluated. Each sample was sheared to a size of 80 × 80 mm, phosphate-treated under the same conditions, and electrocoated (with a constant coating thickness of 15 μm). It was then sheared to a size of 50 × 50 mm to prepare a sheared edge. The samples were then subjected to 45 cycles of corrosion testing according to JASO M609-91, after which the maximum undercoat blister width from the sheared edge was evaluated. The results are shown in Table 1, with a blister width of less than 1.0 mm indicated by "◎", a blister width of 1.0 mm or greater but less than 1.5 mm indicated by "◯", a blister width of 1.5 mm or greater but less than 2.0 mm indicated by "△", and a blister width of 2.0 mm or greater indicated by "×". A blister width of ◎ or ◯ was considered a pass, and a △ or × was considered a fail.

[0048] [Corrosion Resistance of Processed Dissimilar Joints] Next, the corrosion resistance of processed dissimilar joints of Zn-Al-Mg-Si plated steel sheets was evaluated. Each sample was sheared to a size of 70 × 120 mm and mechanically joined at two points to an Al alloy sheared to a size of 40 × 90 mm using mechanical clinching (5 mmφ) to create a processed section, producing a processed dissimilar joint sample of Zn-Al-Mg-Si plated steel sheet and Al alloy. In this case, the surfaces other than the joint surface were phosphate treated under the same conditions, and then electrocoated (with a constant coating thickness of 15 μm) to coat the surfaces. The processed dissimilar joint samples were then subjected to a corrosion test using the N-VDA test. The corrosion amount of the Al alloy after 12 weeks of corrosion testing was evaluated. The amount of Al corrosion was determined in accordance with ISO 8407:2021 by immersing a dissimilar processed sample in a 60 mass% aqueous nitric acid solution at room temperature to remove corrosion products mainly composed of aluminum, and then calculating the difference between the weight before the test and the weight after the corrosion products were removed. 2 If it is less than 5g / m, mark it as "◎" 2 10g / m or more 2 If it is less than 10 g / m, it is marked as "○" 2 15g / m or more 2 If it is less than 15g / m, it is marked as "△" 2 The above cases are indicated as "x" in Table 1. The evaluation of ⊚ or ◯ was considered to be pass, and the evaluation of △ or x was considered to be fail.

[0049] As shown in Table 1, the plating composition defined in the present invention is Mg 2 The number density of the Si alloy phase is 100,000 particles / mm when observed at an accelerating voltage of 7.0 kV. 2 Less than 500 particles / mm when observed at an accelerating voltage of 15.0 kV 2 The above-mentioned invention examples were excellent in chemical conversion treatability, sufficiently suppressed blistering under the coating film from the sheared edge, and had excellent corrosion resistance at the processed and dissimilar joints. 2 It was found that the presence of a small amount of Si alloy phase in the surface layer of the plating layer and a large amount in the interior of the plating layer is advantageous for chemical conversion treatment properties, suppression of undercoat blistering from the sheared edge, and corrosion resistance of the processed and dissimilar joints. In particular, when observed at an accelerating voltage of 15.0 kV, the SiO 2 The density of the particles is 150,000 pieces / mm 2 or more, that is, SiO2 In contrast, the comparative examples, which are outside the scope of the present invention, were inferior to the inventive examples in any of the following: chemical conversion treatability, suppression of undercoat blistering from the sheared edge, and corrosion resistance of the processed and dissimilar joints.

[0050] According to the present invention, it is possible to provide a Zn-Al-Mg-Si plated steel sheet that has excellent chemical conversion treatability, sufficiently suppresses under-coat blistering from the edge, and has excellent corrosion resistance at dissimilar joints where the processed steel sheet comes into contact with an aluminum alloy.

Claims

1. A steel sheet having a base steel sheet and a plating layer formed on at least one side of the base steel sheet, the plating layer containing, in mass%, Mg: 0.50 to 3.00%, Al: 0.10 to 3.00%, Si: 0.010 to 0.20%, Fe: 0.30% or less, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn 2 and a ternary eutectic structure, wherein the Zn-Al-MgZn ternary eutectic structure is obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope and observing a backscattered electron image at a magnification of 5000 times. 2 On the ternary eutectic structure, needle-like Mg with a long side length of 0.5 μm or more is 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 Less than (0 pieces / mm 2 In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 On the ternary eutectic structure, needle-like Mg with a long side length of 0.5 μm or more is 2 The number density of the Si alloy phase is 500 pieces / mm 2 or more, and in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 On the ternary eutectic structure, needle-like SiO having a long side length of 0.5 μm or more is 2 The oxide phase has a density of 100,000 particles / mm 2 The Zn-Al-Mg-Si plated steel sheet is characterized in that the above-mentioned components are present.

Citation Information

Patent Citations

  • Production of hot-dip zn-mg-al coated steel sheet

    JP1992147955A

  • Non-removable coating type lubricated plated steel sheet excellent in workability

    JP2004338397A

  • Highly corrosion-resistant hot-dip plating steel sheet and manufacturing method therefor

    JP2005082834A

  • Zinc alloy plated steel material with excellent corrosion resistance after processing and its manufacturing method

    JP2021508771A

  • Plated steel

    WO2018139619A1