Catalyst composition , ammonia synthesis method, ammonia decomposition method, and method for producing perovskite-type acid hydride
The use of a perovskite-type oxyhydride catalyst composition with rare earth elements and transition metals addresses the inefficiencies of the Haber-Bosch method by enabling ammonia synthesis and decomposition at lower temperatures and pressures, enhancing catalytic performance and stability.
Patent Information
- Application Number
- PCT/JP2024/011019
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-03-21
- Publication Date
- 2024-12-05
AI Technical Summary
The Haber-Bosch method for ammonia synthesis requires high-temperature and high-pressure conditions, leading to equipment and cost challenges, and existing supported metal catalysts lack sufficient performance for practical use, especially under lower temperature and pressure conditions.
A catalyst composition featuring a perovskite-type oxyhydride, represented by BaREO2H, where RE is a rare earth element, supported with transition metals like Ru, Co, Fe, or Mn, which enables ammonia synthesis and decomposition reactions at lower temperatures and pressures through a mechanochemical method.
The catalyst composition achieves sufficient reaction activity under low temperature and low pressure conditions, improving catalytic performance and stability, and is suitable for long-term ammonia synthesis and decomposition processes.
Smart Images

Figure JP2024011019_05122024_PF_FP_ABST
Abstract
Description
Catalyst composition, ammonia synthesis method, ammonia decomposition method, and method for producing perovskite-type oxyhydride
[0001] The present invention relates to a catalyst composition, an ammonia synthesis method, an ammonia decomposition method, and a method for producing a perovskite-type oxyhydride. This application claims priority to Japanese Patent Application No. 2023-086677, filed May 26, 2023, the contents of which are incorporated herein by reference.
[0002] Ammonia is an important compound as a raw material for various chemical products. For example, the Haber-Bosch process, a typical method for synthesizing ammonia, uses Fe 3 O 4 A few mass % of Al 2 O 3 and K. 2 This method uses a doubly promoted iron catalyst containing O and directly reacts a mixed gas of nitrogen and hydrogen with this catalyst under high temperature and pressure conditions to produce ammonia. This technology is still used industrially today with the manufacturing process remaining almost unchanged since its completion.
[0003] Meanwhile, methods for synthesizing ammonia at temperatures lower than the reaction temperature of the Haber-Bosch process have been studied. Catalysts capable of synthesizing ammonia by contacting nitrogen and hydrogen have been studied, and transition metals have been studied as catalytically active components. Among these, a method in which ruthenium (Ru) is supported on various carriers as the catalytically active component and used as a catalyst for the ammonia synthesis reaction has been proposed as an efficient method (see, for example, Patent Document 1).
[0004] Japanese Patent Application Laid-Open No. 2006-231229
[0005] Ammonia synthesis by the Haber-Bosch process, which mainly uses a doubly promoted iron catalyst, has been put to practical use, but the high temperature and high pressure conditions required pose problems in terms of equipment and cost. The supported metal catalysts described in Patent Document 1 typically use a carbonaceous support such as activated carbon or an inorganic oxide support. However, these supported metal catalysts do not always have sufficient performance for practical use. In other words, there is a demand for ammonia synthesis catalysts with superior catalytic activity, such as those that maintain sufficient reaction activity even under lower temperature and pressure conditions than those used under the Haber-Bosch process.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a catalyst composition having sufficient reaction activity even under low-temperature and low-pressure conditions, an ammonia synthesis method, an ammonia decomposition method, and a method for producing a perovskite-type oxyhydride.
[0007] In order to solve the above problems, the present invention proposes the following means. <1> A catalyst composition according to aspect 1 of the present invention contains a perovskite-type oxyhydride represented by the following formula (1): BaREO 2 H m... (1) (In formula (1), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and m represents a number in the range of 0.5 to 1.0.) <2> Aspect 2 of the present invention relates to the catalyst composition of Aspect 1, wherein RE may be a rare earth element selected from the group consisting of Y, Sc, Tb, Dy, Ho, Er, Yb, and Lu. <3> Aspect 3 of the present invention relates to the catalyst composition of Aspect 1, wherein RE may be Y or Sc. <4> Aspect 4 of the present invention relates to the catalyst composition of Aspect 1, wherein the catalyst composition is for an ammonia synthesis reaction or an ammonia decomposition reaction. <5> Aspect 5 of the present invention relates to the catalyst composition of any one of Aspects 1 to 4, wherein the perovskite-type oxyhydride may support one or more transition metals selected from the group consisting of Ru, Co, Fe, Cr, and Mn. <6> A method for synthesizing ammonia according to aspect 6 of the present invention comprises a step of reacting nitrogen with hydrogen in the presence of the catalyst composition according to any one of aspects 1 to 5. <7> A method for decomposing ammonia according to aspect 7 of the present invention comprises a step of decomposing ammonia into hydrogen and nitrogen in the presence of the catalyst composition according to any one of aspects 1 to 6. <8> A method for producing a perovskite-type oxyhydride according to aspect 8 of the present invention comprises a step of reacting ammonia with a compound represented by the following formula (1): BaREO 2 H m ...(1) (in formula (1), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and m represents a number in the range of 0.5 to 1.0), the method for producing a perovskite-type oxyhydride represented by the following formula (1) comprises: BaO; BaH 2 and the following formula (2) RE 2 O 3...(2) (In formula (2), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu), and a compound represented by the formula: (2) (In formula (2), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.) and <12> Aspect 12 of the present invention is the method for producing a perovskite-type oxyhydride according to Aspect 8, wherein a planetary ball mill or a tumbling ball mill may be used in the mechanochemical method. <13> Aspect 13 of the present invention is the method for producing a perovskite-type oxyhydride according to Aspect 8, wherein the pressing and pulverization may be carried out at 300°C or less. <14> Aspect 14 of the present invention is the method for producing a perovskite-type oxyhydride according to Aspect 8, wherein the specific surface area of the particles of the finely divided and homogenized synthesis reaction product is 5.0 m 2 / g or less. <15> Aspect 15 of the present invention can be obtained by the method for producing a perovskite-type oxyhydride according to aspect 8. <16> Aspect 16 of the present invention may be the perovskite-type oxyhydride according to aspect 15, wherein RE is Y.
[0008] According to the above-described aspects of the present invention, it is possible to provide a catalyst composition, an ammonia synthesis method, an ammonia decomposition method, and a method for producing a perovskite-type oxyhydride, which have sufficient reaction activity even under low-temperature and low-pressure conditions.
[0009] 1 is a flowchart of a method for producing a catalyst composition according to one embodiment of the present invention. 2 H, before sintering treatment) and the perovskite-type oxyhydride of Example 2 (BaYO 21H is an XRD pattern of the perovskite-type oxyhydride of Example 3 (perovskite-type oxyhydride (BaScO 2 H, before sintering treatment) after three reaction cycles and after four reaction cycles, and the XRD patterns of the perovskite-type oxyhydride (BaScO 2 1 shows the XRD pattern of the perovskite-type oxyhydride (BaYO) of Example 2 (H, after sintering treatment). 2 H, after sintering treatment) and the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO 2 1 shows the results of TDS measurement for the perovskite-type oxyhydride (BaScO H, after sintering treatment) of Example 3. 2 H, after sintering treatment) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 1 shows the results of TDS measurement for the perovskite-type oxyhydride (BaYO) of Example 1 (H, after sintering treatment). 2 1 shows the results of XRD measurements of perovskite-type oxyhydrides obtained after heat treatment of the sintered sintered body (pre-sintered body) in a hydrogen atmosphere at various temperatures for 72 hours. 2 and N 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) was exposed to a mixed gas flow of 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering) and the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO 2 H (after sintering treatment)) 2 and N 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) was exposed to a mixed gas flow of 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering) and the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO2 H (after sintering treatment)). 2 and N 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) was exposed to a mixed gas flow of 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering) and the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO 2 H (after sintering treatment)) at 0.9 MPa and 300°C. 2 and N 2 The catalyst composition of Example 1 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) was exposed to a mixed gas flow of 2 H, before sintering) and the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO 2 1 shows the change over time in the ammonia synthesis rate for the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)). 2 H, after sintering) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 H (after sintering treatment)) 2 and N 2 Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO) 2 H, after sintering), Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering), Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO 2 1 shows the ammonia synthesis rates for the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) and the catalyst compositions of Comparative Examples 1 to 8 when exposed to ammonia at 0.1 MPa. 21 shows the temperature dependence of ammonia conversion for the catalyst composition of Example 7 (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 1H is an XRD pattern of the perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 1 shows the results of TDS measurement for the catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H, after sintering treatment) 2 and N 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) was exposed to a mixed gas flow of 2 H, after sintering) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 H, after sintering) and the catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H (after sintering treatment)) 2 and N 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) was exposed to a mixed gas flow of2 H, after sintering) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 H, after sintering) and the catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H) is the ammonia synthesis rate for the sintered product.
[0010] Hereinafter, a catalyst composition, an ammonia synthesis method, an ammonia decomposition method, and a method for producing a perovskite-type oxyhydride according to one embodiment of the present invention will be described.
[0011] (Catalyst Composition) The catalyst composition according to the embodiment of the present invention contains a perovskite-type oxyhydride. Here, the perovskite-type oxyhydride is a perovskite-type oxide ABO 3 Oxygen anion O 2ー Part of the hydrogen anion H - The catalyst composition according to this embodiment is preferably a catalyst composition for an ammonia synthesis reaction or a catalyst composition for an ammonia decomposition reaction.
[0012] "Perovskite-type oxyhydride" The perovskite-type oxyhydride according to this embodiment is a perovskite-type oxyhydride represented by the following formula (1). In the following formula (1), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and m represents a number in the range of 0.5 to 1.0. When the catalyst composition according to this embodiment contains the perovskite-type oxyhydride represented by the following formula (1), it becomes possible to relatively easily form hydrogen vacancies on the surface of the catalyst. This can further improve the catalytic performance of the catalyst composition.
[0013] Bareo 2 H m ...(1)
[0014] The catalyst composition according to the embodiment of the present invention may be, for example, BaYO 2 H m1 (0.5≦m1≦1.0), BaScO 2 H m2 (0.5≦m2≦1.0), BaGdO 2 H m3 (0.5≦m3≦1.0), BaTbO 2 H m4 (0.5≦m4≦1.0), BaDyO 2 H m5 (0.5≦m5≦1.0), BaHoO 2 H m6 (0.5≦m6≦1.0), BaErO 2 H m7 (0.5≦m7≦1.0), BaYbO 2 H m8 (0.5≦m8≦1.0), BaLuO 2 H m9 (0.5≦m9≦1.0).
[0015] In the catalyst composition according to this embodiment, RE in the formula (1) is preferably at least one rare earth element selected from the group consisting of Y, Sc, Tb, Dy, Ho, Er, Yb, and Lu, and is more preferably Y or Sc. By using Y or Sc, the catalytic performance can be further improved. Examples of the catalyst composition according to this embodiment in which RE is Y or Sc include BaYO 2 H m1 (0.5≦m1≦1.0), BaScO 2 H m2 (0.5≦m2≦1.0) Examples of the catalyst composition according to this embodiment include BaYO 2 H and BaScO 2 H is preferred. 2 H is BaScO 2 The raw material cost is lower than that of H, and the stability is high when used for ammonia synthesis over a long period of time. Therefore, the catalyst composition according to this embodiment is preferably BaYO. 2 H is more preferred.
[0016] The perovskite-type oxyhydride according to this embodiment may be characterized by a single method or a combination of methods commonly used in the art, such as Rietveld analysis of an X-ray diffraction (XRD) pattern, Thermal Desorption Spectrometry (TDS) measurement, Fourier Transform Infrared Spectroscopy (FT-IR) measurement, or nitrogen adsorption measurement.
[0017] The perovskite-type oxyhydride according to this embodiment forms cubic crystals. The cubic perovskite structure is the most densely packed of the perovskite structures based on close packing, and is easily stabilized in synthesis methods that generate high pressures, such as mechanochemical methods. The cubic crystal structure of the perovskite-type oxyhydride can be confirmed by measuring it using X-ray diffraction (XRD) and performing Rietveld analysis of the obtained XRD pattern.
[0018] The perovskite-type oxyhydride according to this embodiment is preferably in the form of particles. The particle diameter of the perovskite-type oxyhydride according to this embodiment is preferably 1 nm or more and 10 μm or less. The particle diameter of the perovskite-type oxyhydride is preferably 1 nm or more and 1 μm or less, more preferably 1 nm or more and 100 nm or less, and particularly preferably 1 nm or more and 50 nm or less.
[0019] Incidentally, the composition ratio of cations in the perovskite-type oxyhydride can be measured using, for example, an electron probe microanalyzer (EPMA).
[0020] The specific surface area (BET specific surface area) of the perovskite-type oxyhydride according to this embodiment is 5.0 m 2 The specific surface area of the perovskite-type oxyhydride according to this embodiment is preferably 1.0 m / g. 2 The specific surface area of the perovskite-type oxyhydride according to this embodiment may be 2.0 m 2 / g or more is preferred.
[0021] "Supported Metal" In the catalyst composition, it is preferable that the perovskite-type oxyhydride supports a metal (sometimes referred to as a supported metal). The supported metal has catalytic activity. The supported metal is not particularly limited as long as it promotes the ammonia synthesis reaction or the ammonia decomposition reaction. Examples of supported metals include Ru, Co, Fe, Ni, Mo, Rh, Re, Cr, and Mn. It is preferable that the perovskite-type oxyhydride according to this embodiment supports one or more transition metals selected from the group consisting of Ru, Co, Fe, Cr, and Mn (hereinafter sometimes referred to as a supported transition metal). It is more preferable that the perovskite-type oxyhydride according to this embodiment supports Ru. The perovskite-type oxyhydride according to this embodiment preferably supports one or more transition metals selected from the group consisting of Ru, Co, Fe, Cr, and Mn, because this further promotes hydrogen diffusion and reversible hydrogen exchange on the surface of the perovskite-type oxyhydride, thereby further improving catalytic performance.
[0022] Each element of the supported metal may be used alone or in combination of two or more. Compounds of these elements, such as Co 3 Mo 3 N, Fe 3 Mo 3 N, Ni 2 Mo 3 N, Mo 2 N or the like may be used as the supported metal.
[0023] The loading rate of the supported transition metal on the perovskite-type oxyhydride according to this embodiment is preferably 1 wt % or more and 10 wt % or less, based on the total mass of the catalyst composition. More preferably, the loading rate of the supported transition metal is 1 wt % or more and 8 wt % or less, based on the total mass of the catalyst composition. Even more preferably, the loading rate is 3 wt % or more and 5 wt % or less.
[0024] (Method for producing catalyst composition) Next, a method for producing a catalyst composition according to this embodiment will be described. FIG. 1 is a flowchart of a method for producing a catalyst composition according to one embodiment of the present invention. As shown in FIG. 1, the catalyst composition includes a first step S1 of producing a perovskite-type oxyhydride, which serves as a support, and a second step S2 of supporting a transition metal on the perovskite-type oxyhydride produced in the first step S1.
[0025] First, the first step S1, which is a method for producing a perovskite-type oxyhydride, will be described. The perovskite-type oxyhydride represented by the following formula (1) is produced by mixing BaO and BaH 2 and a compound represented by the following formula (2) are repeatedly compressed and pulverized by a mechanochemical method in an inert gas atmosphere until finely divided and homogenized particles of a synthetic reaction product are formed. The formed finely divided and homogenized particles of a synthetic reaction product are a perovskite-type oxyhydride.
[0026] "Raw Materials" In the first step S1, BaO and BaH 2 and a compound represented by the following formula (2): In the following formula (1), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and m represents a number in the range of 0.5 to 1.0. In the following formula (2), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. In formula (2), RE is preferably Y or Sc.
[0027] Bareo 2 H m ... (1) RE 2 O 3 ... (2)
[0028] Examples of the compound represented by the formula (2) include Y 2 O 3 , Sc 2 O 3 , Gd 2 O 3 , Tb 2 O 3 , Dy2 O 3 , Ho 2 O 3 , Er 2 O 3 , Tm 2 O 3 , Yb 2 O 3 , Lu 2 O 3 The compounds represented by the above formula (2) include Y 2 O 3 or Sc 2 O 3 The compound represented by the formula (2) is preferably Y 2 O 3 is more preferable.
[0029] BaO and BaH 2 and the compound represented by the following formula (2), based on the amount of substance (hereinafter, sometimes referred to as the molar ratio of the compound) (BaO:BaH 2 The ratio of BaO to BaH is, for example, 1.0:0.90-1.10:0.90-1.10. 2 The molar ratio of the compound represented by formula (2) to the raw materials for synthesis reaction used to form the particles of the synthesis reaction product by a mechanochemical method may be obtained by adding the raw materials at the molar ratio described above, or may be obtained by premixing the raw materials at the molar ratio described above.
[0030] (Compression and Pulverization) The above-mentioned raw materials are placed in an inert gas atmosphere and repeatedly compressed and pulverized using a mechanochemical method until finely divided and homogenized particles of the synthetic reaction product are formed. The mechanochemical method is a method in which mechanical energy is used to cause chemical changes with surrounding substances. By applying mechanical energy (for example, by colliding balls with each other), the raw materials are compressed together. Further collisions of the balls pulverize the compressed material. By repeating this compression and pulverization, the raw materials react and become finely divided and homogenized, forming particles of the synthetic reaction product.
[0031] In the mechanochemical method, it is preferable to use a planetary ball mill or a tumbling ball mill. By using a planetary ball mill or a tumbling ball mill, the raw materials can be efficiently compressed and pulverized. The materials of the balls and container used in the ball mill are not particularly limited, but for example, ZrO 2 , WC, etc. The diameter of the balls used in the ball mill is, for example, 10 mm to 20 mm.
[0032] The rotation speed of the ball mill is not particularly limited as long as it is capable of producing finely divided and homogenized particles of the synthesis reaction product, and is, for example, 600 rpm to 900 rpm.
[0033] It is preferable to alternately repeat the pressing and crushing (hereinafter sometimes referred to as mechanochemical reaction) and cooling until finely divided and homogenized particles of the synthesis reaction product are formed. By alternately performing the mechanochemical reaction and cooling, finely divided and homogenized particles of the synthesis reaction product can be formed more efficiently. After cooling, the reaction product mass resulting from the reaction of the raw materials may be powdered in a mortar or the like.
[0034] The processing time for each cycle of compression and pulverization (reaction time for the mechanochemical reaction) is not particularly limited, but is, for example, 1 to 10 minutes. In this mechanochemical reaction, compression and pulverization of the raw material are repeatedly performed.
[0035] The pressing and crushing are preferably carried out at a temperature of 300° C. or less. By carrying out the mechanochemical reaction at a temperature of 300° C. or less, it is possible to suppress desorption of hydrogen.
[0036] After the mechanochemical reaction, the mixture is preferably cooled to room temperature. The cooling method is not particularly limited, but may be, for example, by dissipating heat after the mechanochemical reaction.
[0037] The formation of finely divided and homogenized synthetic reaction product particles can be confirmed by the following method. First, X-ray diffraction (XRD) measurement of the sample is performed. If no diffraction lines originating from the raw materials are observed in the obtained XRD pattern, it is determined that a homogenized synthetic reaction product has been formed. Similarly, if there is no change in the XRD pattern before and after the mechanochemical reaction, it is also determined that a homogenized synthetic reaction product has been formed.
[0038] Next, the sample confirmed to be a homogenized synthetic reaction product is observed with a scanning electron microscope (SEM). If perovskite-type oxyhydride particles with a particle size of 10 μm or less are confirmed by SEM observation, it is determined that finely divided and homogenized synthetic reaction product particles have been formed. The presence or absence of perovskite-type oxyhydride particles can be determined using an EDX (energy dispersive X-ray fluorescence analyzer) attached to the SEM. Of course, the above-mentioned finely divided and homogenized synthesis may be confirmed in the reverse manner, by first confirming the formation of a finely divided synthetic reaction product, and then confirming the formation of finely divided and homogenized synthetic reaction product particles in the sample confirmed to be a finely divided synthetic reaction product.
[0039] In the first step, the particles of the synthesis reaction product that have been refined and homogenized may be further sintered. Sintering can promote crystallization. The sintering temperature is preferably 450°C or higher and lower than 600°C. A more preferred sintering temperature is 500°C or higher and 550°C or lower. The sintering time is not particularly limited, but is 1 hour (1 h) or longer. For example, the sintering time may be 72 hours or shorter. The sintering treatment is preferably carried out in a vacuum atmosphere or a hydrogen atmosphere. Preferably, the sintering treatment is carried out in a vacuum atmosphere (e.g., 10°C), since surface modification such as hydration is less likely to occur. --3 The sintering is preferably carried out under a vacuum of about 100 Pa or less. The vacuum atmosphere may be formed by using, for example, a turbo molecular pump. Before sintering, the particles of the synthesis reaction product may be sintered with NH 4 The remaining BaH 2 and BaO may be removed.
[0040] (Ammonia synthesis method) Next, an ammonia synthesis method will be described. In the ammonia synthesis method according to this embodiment, hydrogen (H 2 ) and nitrogen (N 2 ) and hydrogen (H 2 ) and nitrogen (N 2 ) can be reacted to obtain ammonia.
[0041] The method for reacting nitrogen and hydrogen in the presence of the catalyst composition according to the present embodiment is not particularly limited. For example, hydrogen and nitrogen may be introduced into a vessel filled with the catalyst to react the nitrogen and hydrogen.
[0042] The method for producing the mixed gas is not particularly limited. For example, hydrogen (H 2 ) and nitrogen (N 2 ) may be flowed into the container separately, or a mixed gas of a predetermined ratio may be flowed into the container. 2 ) and nitrogen (N 2 ) is preferably 3:1 molar ratio.
[0043] The pressure inside the vessel during ammonia synthesis is not particularly limited, but is, for example, 0.1 MPa to 0.9 MPa. Higher pressure is preferable because the reaction proceeds more rapidly.
[0044] The reaction temperature during ammonia synthesis is preferably 300°C or higher. The higher the reaction temperature, the faster the ammonia synthesis rate, but at 600°C or higher, there is a risk of the catalyst decomposing. Therefore, the temperature during ammonia synthesis is preferably less than 600°C. A more preferred reaction temperature is 550°C or lower. The reaction temperature is the temperature within the reaction system, and may be considered to be the same as the surface temperature of the catalyst.
[0045] (Ammonia decomposition method) Next, the ammonia decomposition method according to this embodiment will be described. The ammonia decomposition method according to this embodiment includes a step of decomposing ammonia into hydrogen and nitrogen in the presence of the catalyst composition according to this embodiment.
[0046] The method for decomposing ammonia into hydrogen and nitrogen in the presence of the catalyst composition according to this embodiment is not particularly limited. For example, ammonia may be decomposed into nitrogen and hydrogen by flowing it into a container filled with a catalyst.
[0047] The pressure inside the vessel during ammonia decomposition is not particularly limited, but is, for example, 0.1 MPa to 0.9 MPa. Higher pressure is preferable because the reaction proceeds more rapidly.
[0048] The reaction temperature during ammonia decomposition is preferably 300°C or higher. The higher the reaction temperature, the faster the ammonia decomposition rate, but at 600°C or higher, there is a risk of the catalyst decomposing. Therefore, the temperature during ammonia synthesis is preferably less than 600°C. A more preferred reaction temperature is 550°C or lower. The reaction temperature is the temperature within the reaction system, and may be considered to be the same as the surface temperature of the catalyst.
[0049] The catalyst composition, ammonia synthesis method, ammonia decomposition method, and perovskite-type oxyhydride production method according to this embodiment have been described above. The catalyst composition according to this embodiment has sufficient reaction activity even under low-temperature and low-pressure conditions. Furthermore, by using the catalyst composition according to this embodiment, ammonia synthesis and ammonia decomposition can be performed even under low-temperature and low-pressure conditions.
[0050] The technical scope of the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention. In addition, the components in the above-described embodiments can be replaced with well-known components as appropriate, and the above-described modifications can be combined as appropriate, without departing from the spirit of the present invention.
[0051] (BaH 2 ) BaH 2 was synthesized by heating Ba (dendritic pieces, 99.99%, Aldrich) in hydrogen at 600° C. for 12 hours.
[0052] (Example 1) Perovskite-type oxyhydride (BaYO 2 H, before sintering) and Ru-supported perovskite-type oxyhydride (BaYO2 All mechanochemical method operations were carried out in a glove box filled with Ar. A planetary ball mill (Pulverisette 7 Premium Line, Fritsch) was used as the apparatus for the mechanochemical method. A 20 mL container made of WC (Fritsch) was used as the grinding container, and grinding was carried out using ten balls with a diameter of 10 mm made of the same material as the grinding container. BaO (99.99%, Aldrich), BaH 2 and Y 2 O 3 (>99.9%, High Purity Chemicals) were weighed out to a total weight of approximately 2 g at a molar ratio (1:1:1), placed in a milling container together with the balls, and sealed with a silicone gasket. The container lid was then closed and placed in a ball mill. A dummy container of the same weight was placed in the other container's place to maintain weight balance. The revolution speed of the milling container was set at 800 rpm to maximize the reaction without contamination. One mechanochemical reaction cycle (hereinafter sometimes referred to as a reaction cycle) consisted of 30 cycles of rotation (reaction) for 2 minutes followed by rotation stop (heat dissipation). After each reaction cycle, the sample adhering to the container wall was peeled off and pre-ground using an agate mortar and pestle. The reaction was terminated when the X-ray diffraction (XRD) pattern of the sample showed no diffraction lines originating from the raw materials, or when the XRD pattern no longer changed, indicating that a homogenized synthetic reaction product had been formed. If not, the above reaction cycle was repeated until the above conditions were met. After the completion of the mechanochemical reaction, the synthesis reaction product was observed with a scanning electron microscope (SEM) to confirm that it was a perovskite-type oxyhydride particle having a particle size of 10 μm or less. Then, the perovskite-type oxyhydride BaYO of Example 1 was obtained. 2 In the reaction cycle, the heat dissipation operation described above was carried out to suppress a continuous temperature rise of the sample during the mechanochemical reaction, and the reaction was carried out at a temperature of 300° C. or less.
[0053] In a glove box filled with Ar, the perovskite-type oxyhydride of Example 1 and Ru3 (CO) 12 (99%, Aldrich) was weighed to achieve a Ru loading of 2 wt% (42.2 mg per gram of the perovskite-type oxyhydride of Example 1) and mixed for approximately 5 minutes using a well-dried agate pestle and mortar. After mixing, the sample was filled into a quartz glass tube with one end closed and a balloon attached to the other end. The tube was then removed from the glove box and vacuum-sealed. The vacuum-sealed sample was then placed in an electric furnace capable of rotary stirring and gradually heated while rotating and stirring at 100 rpm. Specifically, the sample was held at 40°C for 0.04 hours, then heated from 40°C to 70°C at an average heating rate of 60°C / h and held for 1 hour. Next, the sample was heated from 70°C to 120°C at an average heating rate of 25°C / h and held for 1 hour. Next, the temperature was increased from 120°C to 250°C at an average temperature increasing rate of 52°C / h, and the temperature was maintained at 250°C for 2 hours, followed by cooling to room temperature. In this manner, the catalyst composition of Example 1 supporting Ru (i.e., Ru (2 wt%)-supported perovskite-type oxyhydride (BaYO) 2 H) before sintering treatment) was obtained.
[0054] (Example 2) Perovskite-type oxyhydride (BaYO 2 H, after sintering) and Ru-supported perovskite-type oxyhydride (BaYO 2 The perovskite-type oxyhydride of Example 1 was filled into a die with a diameter of 10 mm and uniaxially pressed under a pressure of 20 to 30 MPa to form a pellet. The formed sample was then placed in a quartz glass tube, removed from the glove box to avoid exposure to the atmosphere, vacuum sealed, and placed in an electric furnace for heating. The temperature program during sintering involved increasing the temperature at 100°C / h, holding at 500°C for 72 hours, and then cooling to room temperature, followed by sintering. In this way, the perovskite-type oxyhydride of Example 2 (BaYO 2 H, after sintering treatment).
[0055] In a glove box filled with Ar, the perovskite-type oxyhydride of Example 2 and Ru 3 (CO) 12(99%, Aldrich) was weighed to achieve a Ru loading of 2 wt% (42.2 mg per gram of the perovskite-type oxyhydride of Example 2) and mixed for approximately 5 minutes using a well-dried agate pestle and mortar. After mixing, the sample was filled into a quartz glass tube with one end closed and a balloon attached to the other end. The tube was then removed from the glove box and vacuum-sealed. The vacuum-sealed sample was then placed in an electric furnace capable of rotary stirring and gradually heated while rotating and stirring at 100 rpm. Specifically, the sample was held at 40°C for 0.04 hours, then heated from 40°C to 70°C at an average heating rate of 60°C / h and held for 1 hour. Next, the sample was heated from 70°C to 120°C at an average heating rate of 25°C / h and held for 1 hour. Next, the temperature was increased from 120°C to 250°C at an average temperature increasing rate of 52°C / h, and the temperature was maintained at 250°C for 2 hours, followed by cooling to room temperature. In this manner, the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) in which 2 wt% of Ru was supported was obtained. 2 H, after sintering treatment) was obtained. The particle size of the obtained Ru-supported perovskite-type oxyhydride was 8.6 nm, calculated by CO chemisorption method (CO:Ru=1:1).
[0056] (Example 3) Perovskite-type oxyhydride (BaScO 2 H, before sintering) and perovskite-type oxyhydride (BaScO 2 H, after sintering) and Ru-supported perovskite-type oxyhydride (BaScO 2 All mechanochemical method operations were carried out in a glove box filled with Ar. A planetary ball mill (Pulverisette 7 Premium Line, Fritsch) was used as the apparatus for the mechanochemical method. A 20 mL container made of WC (Fritsch) was used as the grinding container, and grinding was carried out using ten balls with a diameter of 10 mm made of the same material as the grinding container. BaO (99.99%, Aldrich), BaH 2 and Sc 2 O 3(>99.9%, High Purity Chemicals) were weighed out to a total weight of approximately 2 g at a molar ratio of 1:1:1, and placed in a grinding container together with the balls. The container was then sealed with a silicone gasket, the lid was closed, and the container was placed in a ball mill. A dummy container with the same weight was placed in the other container's place to maintain balance. The revolution speed of the grinding container was set to 800 rpm to promote the reaction to its maximum extent without contamination. After one reaction cycle, the sample stuck to the container wall was peeled off and pre-ground using an agate mortar and pestle. The XRD pattern of the sample that had undergone three mechanochemical reaction cycles revealed that the target BaScO 2 The diffraction lines originating from H were observed as the main diffraction lines. 2 O 3 Since a slight diffraction line due to the addition of BaScO was observed, the reaction was repeated. The XRD pattern of the sample after the additional reaction showed almost no change compared to the XRD pattern of the sample before the additional reaction. Therefore, it was determined that the reaction would not proceed any further, and the mechanochemical method was terminated. In this way, the perovskite-type oxyhydride (BaScO) of Example 3 before the sintering treatment was obtained. 2 H, before sintering treatment) was obtained.
[0057] The perovskite-type oxyhydride of Example 3 before the sintering treatment was filled into a die with a diameter of 10 mm and uniaxially pressed under a pressure of 20 to 30 MPa to form a pellet. The formed sample was then placed in a quartz glass tube, removed from the glove box to avoid exposure to the atmosphere, vacuum sealed, and placed in an electric furnace for heating. The temperature program during sintering involved increasing the temperature at 100°C / h, holding at 500°C for 72 hours, and then allowing to cool to room temperature. In this way, the perovskite-type oxyhydride of Example 3 after the sintering treatment (BaScO 2 H, after sintering treatment).
[0058] The perovskite-type oxyhydride of Example 3 and Ru were sintered in a glove box filled with Ar. 3 (CO) 12(99%, Aldrich) was weighed to achieve a Ru loading of 2 wt% (42.2 mg per gram of the perovskite-type oxyhydride of Example 3) and mixed for approximately 5 minutes using a well-dried agate pestle and mortar. After mixing, the sample was filled into a quartz glass tube with one end closed and a balloon attached to the other end. The tube was then removed from the glove box and vacuum-sealed. The vacuum-sealed sample was then placed in an electric furnace capable of rotary stirring and gradually heated while rotating and stirring at 100 rpm. Specifically, the sample was held at 40°C for 0.04 hours, then heated from 40°C to 70°C at an average heating rate of 60°C / h and held for 1 hour. Next, the sample was heated from 70°C to 120°C at an average heating rate of 25°C / h and held for 1 hour. Next, the temperature was increased from 120°C to 250°C at an average temperature increasing rate of 52°C / h, and the temperature was maintained at 250°C for 2 hours, followed by cooling to room temperature. In this manner, the catalyst composition of Example 3 supporting Ru (i.e., Ru (2 wt%)-supported perovskite-type oxyhydride (BaScO 2 H, after sintering treatment) was obtained. The particle size of the obtained Ru-supported perovskite-type oxyhydride was 6.3 nm, calculated by CO chemisorption method (CO:Ru=1:1).
[0059] (Example 4) Co-supported perovskite-type oxyhydride (BaYO 2 The perovskite-type oxyhydride (BaYO) was sintered in the same manner as in Example 2 in a glove box filled with Ar. 2 H, after sintering) and Co 2 (CO) 8 (>95%, TCI) was weighed out so that the Co loading rate was 2 wt% (BaYO 2 Co per 1g of H 2 (CO) 8The samples were mixed for approximately 10 minutes using a well-dried agate pestle and mortar. After mixing, a glass reaction tube was filled with quartz wool and sealed at one end, and the sample was then loaded into the tube. Both ends were sealed with parafilm, and the tube was removed from the glove box and quickly connected to a hydrogen flow furnace that had been purged with hydrogen in advance. After connection, the tube was heated from room temperature to 250°C at an average heating rate of 220°C / h while flowing hydrogen (Co: 3 mL / min), and then maintained at 250°C for 1.5 hours, after which it was cooled to room temperature. In this way, the catalyst composition of Example 4 (i.e., Co (2 wt%)-supported perovskite-type oxyhydride (BaYO) 2 H, after sintering treatment) was obtained.
[0060] (Example 5) Fe-supported perovskite-type oxyhydride (BaYO 2 The perovskite-type oxyhydride (BaYO) was sintered in the same manner as in Example 2 in a glove box filled with Ar. 2 H, after sintering) and Fe 2 (CO) 9 (99%, Thermo Fisher Scientific) was weighed out so that the Fe loading rate was 2 wt% (BaYO 2 Fe per 1g of H 2 (CO) 9 The mixture was mixed for approximately 10 minutes using a well-dried agate pestle and mortar. After mixing, the sample was loaded into a glass reaction tube, one end of which was sealed with quartz wool, and both ends were sealed with parafilm. The tube was then removed from the glove box and quickly connected to a hydrogen flow furnace that had been pre-purged with hydrogen. After connection, the tube was heated to 200°C at an average heating rate of 85°C / min while flowing hydrogen (Fe: 5 mL / min) and held at 200°C for 1 hour. The tube was then heated from 200°C to 400°C at an average heating rate of 200°C / h, held at 400°C for 2 hours, and then cooled to room temperature. In this way, the catalyst composition of Example 5 (i.e., Fe (1 wt%)-supported perovskite-type oxyhydride (BaYO) 2 H, after sintering treatment) was obtained.
[0061] (Comparative Example 1) CeO 2The dehydrated CeO was obtained by vacuum heating at 600°C to remove water adsorbed on the surface. 2 and Ba(NH 2 ) 2 The above was mixed in an Ar glove box using an agate pestle and mortar. At this time, the molar ratio of Ce to Ba was 1:1. The obtained powder was dissolved in NH 3 The mixture was then heat-treated in an air stream at 600°C for 6 hours. 3-x N y H z A powder was obtained.
[0062] Powdered BaCeO 3-x N y H z 0.50 g and Ru 3 (CO) 12 (Aldrich, 99%) 0.056 g (BaCeO 3-x N y H z The powdered BaCeO 3-x N y H z Ru on the surface of 3 (CO) 12 The resulting product was finally heated at 250°C for 2 hours to deposit Ru. 3 (CO) 12 By thermally decomposing BaCeO 3-x N y H z The catalyst composition of Comparative Example 1 in which Ru was fixed to BaCeO (Ru (5 wt%) 3-x N y H z ) was obtained.
[0063] (Comparative Example 2) Powdered BaCeO 3-x N y H z 95 mg and Co 2 (CO) 8 14.5 mg (BaCeO 3-x N y H zThe resulting mixture (corresponding to 5% by mass of supported metal Co relative to the total mass of the catalyst) was placed in a quartz glass reaction tube, and nitrogen gas was passed through the reaction tube at 15 mL / min and hydrogen gas at 45 mL / min (total 60 mL / min). The reaction tube was heated to 400°C over 2 hours and maintained at this temperature for 5 hours to obtain BaCeO 3-x N y H z The catalyst composition of Comparative Example 2 in which Co was fixed to the catalyst (Co (5 wt%) BaCeO 3-x N y H z ) was obtained.
[0064] (Comparative Example 3) Powdered BaCeO 3-x N y H z 95 mg and Fe 2 (CO) 9 16.3 mg (BaCeO 3-x N y H z The mixture was placed in a quartz glass reaction tube, and nitrogen gas was passed through the reaction tube at 15 mL / min and hydrogen gas at 45 mL / min (total 60 mL / min). The reaction tube was heated to 400°C over 2 hours and maintained at this temperature for 5 hours to obtain BaCeO. 3-x N y H z The catalyst composition of Comparative Example 3 in which Fe was fixed to the catalyst (Fe (5 wt%) BaCeO 3-x N y H z ) was obtained.
[0065] Comparative Example 4: 5.23 g (0.02 mol) of barium nitrate, 8.68 g (0.02 mol) of cerium nitrate hexahydrate, and 38.4 g (0.2 mol) of citric acid were dissolved in water, and 42.4 g (0.4 mol) of diethylene glycol was added to the resulting solution to obtain a mixture. The resulting mixture was stirred for one hour and then heated at 120°C for four hours to cause gelation. The gelled mixture was then heated at 450°C for five hours to cause carbonization. The carbonized mixture was heated at 900°C for six hours to obtain powdered BaCeO. 3 obtained.
[0066] By using the same method as in Comparative Example 1, metal Ru was converted into BaCeO3 The catalyst composition of Comparative Example 4 (Ru(5 wt%)BaCeO 3 ) was obtained.
[0067] (Comparative Example 5) BaCeO of Comparative Example 1 3-x N y H z A catalyst composition of Comparative Example 5 (Ru (5 wt %)-Cs / MgO (Cs / Ru element ratio=1)) was obtained by the same method as in Comparative Example 1, except that MgO to which Cs had been added (referred to as Cs / MgO) was used instead of Ru.
[0068] (Comparative Example 6) BaCeO of Comparative Example 1 3-x N y H z Instead of CeO 2 The catalyst composition of Comparative Example 6 (Ru (5 wt%) / CeO 2 ) was obtained.
[0069] (Comparative Example 7) The catalyst composition of Comparative Example 7 (Ru (5 wt%) / Ca 2 N) was obtained.
[0070] Comparative Example 8 A catalyst composition of Comparative Example 8 (Ru (2 wt %) / C12A7:e-) was obtained in the same manner as described in WO 2012 / 0077658.
[0071] (Comparative Example 9) Ru / Ba 3 Y 4 O 9 was obtained by the following method. Barium carbonate (>99%, Kojundo Chemical) and yttrium oxide (>99.9%, Kojundo Chemical) were mixed in the air using an agate pestle and mortar. At this time, the molar ratio of barium carbonate to yttrium oxide was 3:2. The obtained powder was heat-treated in the air at 1300°C for 5 hours. In this way, Ba 3 Y 4 O 9 Then, the BaCeO powder of Comparative Example 1 was obtained. 3-x N y H z Ba obtained instead of3 Y 4 O 9 The catalyst composition of Comparative Example 9 (Ru (2 wt%) / Ba 3 Y 4 O 9 ) was obtained.
[0072] (X-ray Diffraction Method (XRD)) An X-ray diffractometer (MiniFlex600, Rigaku) was used, and Cu-Kα radiation (λ = 0.15418 nm) was used as the X-ray source. Measurements were performed over a measurement range of 10 to 80°, at a measurement interval of 0.02°, and at a scan speed of 1 to 2° / min. Since the sample decomposes in the atmosphere, the measurement was performed after storing it in a sealed holder for air-stable samples in a glove box filled with Ar. The sample was subjected to Rietveld analysis of the XRD pattern using TOPAS (Bruker AXS) to identify the crystalline phase.
[0073] (Thermal Desorption Spectroscopy (TDS)) A high-vacuum thermal property measurement device (TDS1400TV, ESCO) equipped with a quadrupole mass spectrometer (PrismaPlus QMG220, Pfeiffer Vacuum) was used, and the vacuum degree was 10 -4 ~10 ー7 The measurement was carried out under the following conditions: 1 Pa, the heat source was infrared, the temperature rise rate was 60°C / min, the holding temperature was 1200°C, and the SEM voltage was 1200 V. The sample was taken in a glove box filled with Ar and approximately 1 to 3 mg of SiO 2 The sample was placed on a holder and transported to the equipment using a dedicated transfer vessel. To confirm that it was a hydride and to investigate its hydrogen release characteristics, the hydrogen-derived fragment with a mass ratio of 2 in the obtained TDS spectrum was focused on, and the presence and amount of hydrogen contained therein were investigated based on the desorption temperature and desorption amount. Furthermore, since hydrides are often hydroxylated by water in the atmosphere, the presence or absence of hydroxylation was confirmed by focusing on the water-derived fragment with a mass ratio of 18. The TDS spectrum was analyzed using TDS Data Viewer (ESCO).
[0074] (Nitrogen Adsorption Measurement) Measurements were performed using a specific surface area measurement device (BELSORP mini, MicrotracBEL) at a relative pressure range of 0 to 0.4. Approximately 0.1 g of the sample was filled into a sealed sample tube in a glove box filled with Ar, and then connected to the device so as not to expose it to the atmosphere. Nitrogen adsorption measurements were performed, and the BET specific surface area was calculated using the Brunauer-Emmett-Teller (BET) equation shown in the following equation (3). Here, Va is the adsorption amount at equilibrium pressure, Vm is the monoatomic layer adsorption amount, p0 is the saturated vapor pressure, p is the equilibrium pressure, and C is a parameter related to the difference in heat of adsorption between first-layer adsorption and second-layer or subsequent adsorption. Specifically, plots were made based on the Brunauer-Emmett-Teller (BET) equation so that the relative pressure at which the BET equation holds well was in the range of 0.05 to 0.35, and C in the BET equation was approximately 50 to 300, which is the recommended value at liquid nitrogen temperature, and the specific surface area of each sample was calculated. The BET specific surface area of the perovskite-type oxyhydride of Example 1 was 2.60 m 2 The BET specific surface area of the perovskite-type oxyhydride of Example 2 was 2.17 m 2 The BET specific surface area of the perovskite-type oxyhydride of Example 3 was 4.38 m 2 / g.
[0075]
[0076] (Heat Resistance Evaluation Test) The perovskite-type oxyhydride of Example 1, which was a sample, was subjected to a heat treatment in a hydrogen atmosphere to examine the heat resistance of the sample. Specifically, the perovskite-type oxyhydride of Example 1 was placed in an alumina Tammann tube, which was then loaded into a vessel equipped with a needle valve. The tube was then removed from the glove box to avoid exposure to the atmosphere and attached to a hydrogen furnace. The vessel was then purged with hydrogen and heated at various temperatures (500°C, 550°C, 600°C, 700°C, or 800°C). After being held for 72 hours and allowed to cool to room temperature, the removed sample was subjected to XRD measurement.
[0077] (Ammonia synthesis) In the ammonia synthesis test, nitrogen gas and hydrogen gas were passed at flow rates of 15 mL / min and 45 mL / min, respectively, so that the flow rate ratio was 1:3, and the catalyst loading was standardized to 0.1 g. The reaction time was 0 to 80 hours, the temperature was 200 to 400°C, and the pressure was 0.1 to 0.9 MPa. The gas that had passed through the catalyst was passed through 5 mM dilute sulfuric acid to trap ammonia as ammonium ions. The gas was sampled at regular intervals and measured by ion chromatography (Prominence, Shimadzu) to qualitatively and quantitatively analyze ammonia. The ammonia synthesis rate was then calculated from the slope of a plot of the amount of ammonium ions produced versus sampling time.
[0078] (Ammonia decomposition) In the ammonia decomposition test, ammonia was circulated at a flow rate of 25 mL / min, and the catalyst loading was standardized to 0.1 g. The test was conducted for a reaction time of 0 to 80 hours, at a temperature of 220 to 520°C, and at a pressure of 0.1 MPa. The gas that passed through the catalyst was measured by gas chromatography (GC-14A, Shimadzu) to determine the ammonia conversion rate. The ammonia conversion rate was calculated by dividing the denominator "NH 3 Amount" and numerator "(NH 3 Amount) - (Remaining NH after decomposition and distribution 3 The percentage of the ratio is the amount of
[0079] FIG. 2 shows the perovskite-type oxyhydride (BaYO) of Example 1. 2 H, before sintering treatment) and the perovskite-type oxyhydride of Example 2 (BaYO 2 2 shows the XRD patterns of the BaYO powder (H, after sintering treatment). The horizontal axis of FIG. 2 is 2θ (°), and the vertical axis is diffraction intensity (au (arbitrary unit)). As shown in FIG. 2, in both Examples 1 and 2, BaYO powder 2 Diffraction lines thought to be derived from H and a slight Y 2 O 3 Diffraction lines originating from the observed Y 2 O 3 Regarding the diffraction lines originating from Y 2 O 3Since no diffraction lines of raw materials other than BaYO were confirmed, it is assumed that they are residual materials. The perovskite-type oxyhydride of Example 2 was subjected to Rietveld analysis. 2 H is BaScO, a cubic perovskite-type oxyhydride whose synthesis has already been reported. 2 It is assumed that BaScO has a similar crystal structure to H. 2 Using a structure created by substituting Y for Sc using the structure of H as a template, parameters such as lattice constant were optimized. As a result, it was confirmed that the XRD pattern of the perovskite-type oxyhydride of Example 2 showed good agreement with the pattern calculated from the structure with optimized parameters. From the obtained results, it was confirmed that the perovskite-type oxyhydride of Example 1 and the perovskite-type oxyhydride of Example 2 were BaYO 2 It was confirmed that the crystal structure was H (cubic crystal).
[0080] FIG. 3 shows the perovskite-type oxyhydride (BaScO 2 H, before sintering treatment) after three reaction cycles and after four reaction cycles, and the XRD patterns of the perovskite-type oxyhydride (BaScO 2 3 shows the XRD patterns of BaScO (H, after sintering treatment). The horizontal axis of FIG. 3 is 2θ (°), and the vertical axis is diffraction intensity (au (arbitrary unit)). As shown in FIG. 3, 2 The diffraction lines are thought to be due to H and a small amount of Sc 2 O 3 Diffraction lines due to Sc were observed in the third and fourth reaction cycles. 2 O 3 Since no change was observed in the diffraction lines originating from the observed Sc 2 O 3 The diffraction lines originating from BaScO are presumed to be the residual fraction. 2 The results show good agreement with the pattern calculated from the crystal structure of H. From the obtained results, it is clear that the perovskite-type oxyhydride of Example 3 is BaScO 2It was confirmed that the crystal structure was H (cubic crystal).
[0081] FIG. 4 shows the perovskite-type oxyhydride (BaYO) of Example 2. 2 H, after sintering treatment) and the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO 2 The results of TDS measurements for both the perovskite-type oxyhydride (after H, sintering treatment) and the perovskite-type oxyhydride (after H, sintering treatment) are shown. The horizontal axis represents temperature (°C) and the vertical axis represents ion current (μA). In the perovskite-type oxyhydride of Example 2, strong hydrogen desorption was observed between 50 and 250°C and above 350°C. On the other hand, 2 The fragment with a mass ratio of 18 derived from O was hardly observed. From the integral value of this fragment, H 2 and H 2 When O and H are quantified, 2 is a value on the same scale as the ideal value, and H 2 O is H 2 Since it was about 2% of 2 This suggests that H is a pure hydride that has not undergone hydroxylation. Furthermore, hydrogen desorption was confirmed even at low temperatures below 200°C, demonstrating the possibility of reversible hydrogen exchange under on-site ammonia conditions (below 400°C), confirming its suitability as a catalyst support for the ammonia synthesis reaction.
[0082] It was confirmed that the hydrogen desorption peak in the low temperature range (50 to 200°C) shifted to the higher temperature side, and the hydrogen desorption peak in the high temperature range (350°C or higher) shifted to the lower temperature side for the catalyst composition of Example 2. It is known that in the low temperature range of 400°C or lower, the Ru surface has such strong hydrogen adsorption that dissociated and adsorbed hydrogen atoms cover the Ru surface, causing hydrogen poisoning, which inhibits nitrogen adsorption. Therefore, the peak shift in the low temperature range is due to the fact that the form of hydrogen desorption is BaYO. 2It is presumed that the hydrogen desorption pattern changed from a direct desorption from the H surface to a reverse spillover of hydrogen from the surface of the perovskite-type oxyhydride onto the supported Ru. Here, reverse spillover refers to the phenomenon in which atoms or ions adsorbed on the support or the like in a catalyst consisting of a metal and a support migrate to the supported metal surface by diffusion, recombine, and are desorbed into the gas phase as molecules. On the other hand, the peak shift in the high temperature region indicates that hydrogen diffusion from the bulk to the surface has become easier, and it is presumed that hydrogen diffusion in the bulk is also promoted along with the promotion of hydrogen diffusion near the surface due to the support of Ru. Furthermore, since the spectral shape changed to show uniform hydrogen desorption overall throughout the entire temperature range above 150°C, it is possible to say that the catalyst exhibits catalytic activity in the temperature range above 150°C and that BaYO 2 It was suggested that activity may improve with increasing temperature unless H decomposes.
[0083] FIG. 5 shows the perovskite-type oxyhydride (BaScO 2 H, after sintering treatment) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 The results of TDS measurements for both the perovskite-type oxyhydride (after H, sintering treatment) and the perovskite-type oxyhydride (after H, sintering treatment) are shown. The horizontal axis represents temperature (°C) and the vertical axis represents ion current (μA). For the perovskite-type oxyhydride of Example 3, strong hydrogen desorption was observed at 100 to 200°C and above 350°C. On the other hand, for the perovskite-type oxyhydride of Example 3, strong hydrogen desorption was observed at 100 to 200°C and above 350°C. 2 The fragment with a mass ratio of 18 derived from O was hardly observed. From the integral value of this fragment, H 2 and H 2 When O and H are quantified, 2 O is H 2 Since the value was less than 1% of BaScO 2 This suggests that H is a pure hydride that has not undergone hydroxylation. Furthermore, hydrogen desorption was confirmed even at low temperatures below 200°C, demonstrating the possibility of reversible hydrogen exchange under on-site ammonia conditions (below 400°C), confirming its suitability as a catalyst support for the ammonia synthesis reaction.
[0084] For the catalyst composition of Example 3, as in Example 2, it was confirmed that the hydrogen desorption peak in the low temperature range (50 to 200°C) was shifted to the higher temperature side, and the hydrogen desorption peak in the high temperature range (350°C and above) was shifted to the lower temperature side. As a whole, the spectral shape changed to show uniform hydrogen desorption over the entire temperature range from 150°C onwards, and therefore the catalyst composition of Example 3 exhibited catalytic activity in the temperature range of 150°C and above, and the hydrogen desorption peak in the high temperature range (350°C and above) was shifted to the lower temperature side. 2 It was suggested that activity may improve with increasing temperature unless H decomposes.
[0085] (Heat Resistance Test) FIG. 6 shows the perovskite-type oxyhydride (BaYO) of Example 1. 2 The graph shows the results of XRD measurements of the perovskite-type oxyhydrides obtained after heat treatment of BaY (H, before sintering) in a hydrogen atmosphere at various temperatures for 72 hours. The horizontal axis of FIG. 6 represents 2θ (°), and the vertical axis of FIG. 6 represents the diffraction intensity (au (arbitrary unit)). 2 O 4 , BaO, BaH 2 and Y 2 O 3 It was confirmed that BaYO was precipitated. 2 It was suggested that H was decomposed. 2 The diffraction lines thought to be derived from H showed a decrease in half-width as the temperature increased, confirming that the crystallinity improved, and that the lattice expanded as hydrogen defects were filled.
[0086] Figure 7 shows the results of H at 0.9 MPa and 300°C. 2 and N 2 Under the flow of a mixture of 2 :N 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) when exposed to a 3:1 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering) and the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO 2 H, after sintering treatment) 3 ) synthesis rate (mmolg-1 h -1 7 shows the change over time in the ammonia synthesis rate (mmol g). -1 h -1 ) In the case of the catalyst composition of Example 2, the ammonia synthesis rate increased until 20 hours and then showed stable behavior. On the other hand, in the case of the catalyst composition of Example 4 and the catalyst composition of Example 5, the ammonia synthesis rate decreased until 20 hours and then showed stable behavior. In addition, the catalyst composition of Example 2 had the highest ammonia synthesis rate, and the catalyst composition with the next highest ammonia synthesis rate was the catalyst composition of Example 4. The ammonia synthesis rate of the catalyst composition of Example 5 was the lowest.
[0087] Figure 8 shows the H 2 and N 2 Under the flow of a mixture of 2 :N 2 The catalytic composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) when exposed to a 3:1 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering) and the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO 2 H, after sintering treatment) 3 ) synthesis rate (mmolg -1 h -1 8 shows the pressure dependence of the ammonia synthesis rate (mmol / g). -1 h -1 8, for the catalyst composition of Example 2, the catalyst composition of Example 4, and the catalyst composition of Example 5, the ammonia synthesis rate increased with increasing pressure. In particular, for the catalyst composition of Example 4 and the catalyst composition of Example 5, the ammonia synthesis rate increased threefold by increasing the pressure from 0.1 MPa to 0.9 MPa.
[0088] Figure 9 shows the H 2 and N2 Under the flow of a mixture of 2 :N 2 The catalytic composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) when exposed to a 3:1 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering) and the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO 2 H, after sintering treatment) 3 ) synthesis rate (mmolg -1 h -1 9 shows the temperature dependence of ammonia synthesis rate (mmol g -1 h -1 The ammonia synthesis rate for the catalyst composition of Example 2, the catalyst composition of Example 4, and the catalyst composition of Example 5 increased with increasing temperature.
[0089] FIG. 10 shows the results of H 2 and N 2 Under the flow of a mixture of 2 :N 2 The catalytic composition of Example 1 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) when exposed to a 3:1 2 H, before sintering) and the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO 2 The horizontal axis of FIG. 10 represents time (h), and the vertical axis represents the ammonia synthesis rate (mmol g -1 h -1 ) It was confirmed that the catalyst composition of Example 1 and the catalyst composition of Example 2 exhibited similar behavior regardless of whether sintering was performed or not. In addition, the ammonia synthesis rate for the catalyst composition of Example 2 was higher than the ammonia synthesis rate for the catalyst composition of Example 1.
[0090] FIG. 11 shows the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO) 2H, after sintering) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 11 shows the change over time in the ammonia synthesis rate for the sintered product (H, after sintering treatment). The horizontal axis of FIG. 11 is the reaction time (h), and the vertical axis is the ammonia synthesis rate (mmol g -1 h -1 ) In the catalyst composition of Example 3, the ammonia synthesis rate increased slightly over time from the value measured immediately after the target temperature was reached, and then decreased gradually after 20 hours had passed. On the other hand, in the catalyst composition of Example 2, the behavior of the ammonia synthesis rate until 20 hours had passed was similar to that of the catalyst composition of Example 3, but after 20 hours had passed, the ammonia synthesis rate remained constant. Therefore, it was found that the catalyst composition of Example 2 is effective when synthesizing ammonia for a longer period of time.
[0091] Figure 12 shows the results of H 2 and N 2 Under the flow of a mixture of 2 :N 2 The catalytic composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) when exposed to a 3:1 2 H, after sintering), the catalyst composition of Example 4 (i.e., Co-supported perovskite-type oxyhydride (BaYO 2 H, after sintering), the catalyst composition of Example 5 (i.e., Fe-supported perovskite-type oxyhydride (BaYO) 2 1 shows the ammonia synthesis rates for the catalyst compositions of Example 2 (after sintering) and Comparative Examples 1 to 8. Comparative Examples 1 to 8 are existing catalyst compositions. The ammonia synthesis rate value for the catalyst composition of Example 2 was higher than the ammonia synthesis rate values for Comparative Examples 2 to 8, which supported the same Ru. Furthermore, although the Ru loading rate in the catalyst composition of Example 2 was less than half that of the catalyst composition of Comparative Example 1, the ammonia synthesis rates were comparable. From the above, it was confirmed that the catalyst composition of the present disclosure is suitable for the ammonia synthesis reaction.
[0092] FIG. 13 shows the catalytic activity of the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO)) when exposed to ammonia at 0.1 MPa. 2 1 shows the temperature dependence of ammonia conversion for the catalyst composition of Example 2 (after sintering) and Comparative Example 9. For both the catalyst composition of Example 2 and the catalyst composition of Comparative Example 9, the ammonia conversion increased with increasing temperature. Furthermore, the catalyst composition of Example 2 showed a higher conversion rate. From the above, it was confirmed that the catalyst composition of the present disclosure is suitable for ammonia decomposition reactions.
[0093] (Example 6) Perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H, before sintering process) 2 O 3 Instead of Tb, 2 O 3 , Dy 2 O 3 , Ho 2 O 3 , Er 2 O 3 , Yb 2 O 3 , and Lu 2 O 3 Each perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, and BaLuO 2 H, before sintering treatment) was obtained.
[0094] (Example 7) Perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO2 H, after sintering treatment) Production of the perovskite-type oxyhydride (BaYO) of Example 1 2 Instead of the perovskite-type oxyhydrides (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 Each of the perovskite-type oxyhydrides (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H, after sintering treatment). 2 The results are shown in Figures 14 and 15.
[0095] (Example 8) Ru-supported perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H, after sintering treatment) Production of perovskite-type oxyhydride (BaYO) of Example 2 2 Instead of the perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 Each catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2H, BaYbO 2 H, BaLuO 2 The catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO) 2 The TDS, time-dependent changes in ammonia synthesis rate, and catalytic activity were measured in the same manner as in (H, after sintering). The results are shown in Figures 16, 17, and 18 and Table 1.
[0096]
[0097] In Table 1, the "Ru loading rate" was determined by X-ray fluorescence (XRF) analysis. The XRF measurement was carried out using a wavelength dispersive X-ray fluorescence analyzer S8 TIGER (manufactured by Bruker) under the following conditions.
[0098] XRF measurement conditions: Apparatus used: Bruker wavelength dispersive X-ray fluorescence analyzer S8 TIGER; X-ray source: Rh-La line; Diffraction crystal: LiF(200); Atmosphere: Vacuum; Collimator mask (X-ray irradiation range): Circle with a diameter of 5 mm; Elements to be measured: Ba, RE, Ru; Quantitative method: Fundamental parameter (FP) method (i.e., a method of estimating the composition so that it matches the actually measured fluorescent X-ray intensity, utilizing the fact that the fluorescent X-ray intensity can be theoretically calculated from both the type and amount of the constituent elements).
[0099] Since the ratio of Ru / Ba or Ru / RE is obtained by weight from the XRF measurement, the content of Ba or RE per unit weight of the carrier (BaREO 2 If the weight of each element contained in the raw materials when synthesizing H is known, the Ru support rate wt % (100 × Ru [g] / (Ru [g] + carrier [g])) can be calculated. In Table 1, the Ru support rate is calculated from the weight ratio of RE and Ru, which have high fluorescent X-ray intensity and are little affected by intensity changes due to the matrix.
[0100] (Example) When Ru / Y = 0.0541 and Y content per 1 g of carrier = 0.343 g, the weight of Ru per 1 g of carrier = 0.0541 x 0.343 = 0.0186 g. Ru loading rate = 100 x 0.0186 / (0.0186 + 1) = 1.8 wt%
[0101] In Table 1, the "Ru particle size" was estimated by CO chemisorption measurement (CO:Ru = 1:1). The CO chemisorption amount was measured using a BELCAT-A device (manufactured by Microtrac BEL) under the following conditions.
[0102] ・Device used: Microtrac-Bell catalyst analyzer BELCAT-A ・Measurement temperature: 50°C ・Carrier gas: He (30 mL / min) ・Adsorption gas: CO / He (9.51%) ・Pulse volume: 0.031 mL ・Sample amount: Approximately 0.15-0.2 g ・Pretreatment: Heat at 400°C in a hydrogen atmosphere for 2 hours. Then, switch the gas to He and heat at 400°C for 30 minutes. (Ru 3 (CO) 12 Because Ru was supported using the precursor, CO was already adsorbed on the Ru surface before measurement, making it impossible to measure the amount of CO adsorption in this state. Therefore, the adsorbed CO was removed by heating under a hydrogen flow. Furthermore, because hydrogen adsorption to Ru is strong, hydrogen adsorption on Ru is left behind when hydrogen is only passed through, so the adsorbed hydrogen was removed by passing He through. By performing these pretreatments, a clean Ru surface free of adsorbed species was obtained. In actual measurements, the amount of CO adsorption was obtained as an actual measured value, and the particle size and dispersion of Ru were determined from both the sample loading amount and the input value of the Ru support rate (automatically calculated within the Chem Master software).
[0103] (Discussion) From the results in Table 1, the actual Ru loading rate was in the range of 1.5 to 2.0 wt% for all catalyst compositions. Furthermore, the Ru particle size was smallest when the RE was Sc, and a tendency for the Ru particle size to increase as the ionic radius of the RE increased was confirmed, reaching its largest when the RE was Tb. Since no correlation was observed between the Ru loading rate and the Ru particle size, it is possible that this tendency was due to differences in the surface properties of the support or the interaction between the support and Ru (specific surface area, surface roughness, Ru adsorption energy, etc.).
[0104] FIG. 14 shows the perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2H, BaErO 2 H, BaYbO 2 H, BaLuO 2 14 shows the XRD patterns of the perovskite-type oxyhydrides of Example 7 (H, after sintering). The horizontal axis of FIG. 14 is 2θ (°), and the vertical axis is diffraction intensity (au (arbitrary unit)). As shown in FIG. 14, each of the perovskite-type oxyhydrides of Example 7 is BaTbO 2 H (cubic), BaDyO 2 H (cubic crystal), BaHoO 2 H (cubic), BaErO 2 H (cubic crystal), BaYbO 2 H (cubic crystal), BaLuO 2 It was confirmed that the lattice constant of the RE is H (cubic crystal). It was also confirmed that diffraction lines derived from the cubic perovskite structure were obtained in all samples, and it was confirmed that as the atomic number of RE increases from Tb to Lu, the diffraction peak of the RE shifts to the higher angle side and the lattice constant decreases. This is a result of reflecting the decrease in ionic radius due to lanthanide contraction.
[0105] FIG. 15 shows the perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 Figure 15 shows the TDS measurement results for the samples (H, after sintering). The horizontal axis represents temperature (°C), and the vertical axis represents the ion current (μA / mg) normalized by the sample weight. The results in Figure 15 confirm that only hydrogen desorption was observed in all samples, confirming that the samples were pure hydrides containing no hydroxyl groups (OH-). Furthermore, all samples exhibited similar spectral shapes indicating hydrogen desorption in the temperature ranges of 100°C to 200°C and 350°C and above. Therefore, it is believed that there is no significant difference in the hydrogen desorption capacity between different materials.
[0106] FIG. 16 shows the catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO 2 H,BaDyO 2 H, BaHoO 2H, BaErO 2 H, BaYbO 2 H, BaLuO 2 The results of TDS measurements of the catalyst (H, after sintering) are shown in Fig. 16. The horizontal axis represents temperature (°C), and the vertical axis represents ion current (µA / mg) normalized by sample weight. The results of Fig. 16 suggest that the addition of Ru changed the spectral shape to show uniform hydrogen desorption over the entire temperature range of 100°C or higher, suggesting that the catalyst exhibits catalytic activity over the temperature range of 100°C or higher and that the activity may improve with increasing temperature unless the support is decomposed.
[0107] Figure 17 shows the results of H 2 and N 2 Under the flow of a mixture of 2 :N 2 The catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO)) when exposed to a 3:1 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H, after sintering treatment) 3 ) synthesis rate (mmolg -1 h -1 ) over time. The horizontal axis of FIG. 17 represents the reaction time (h), and the vertical axis represents the ammonia synthesis rate (mmol g -1 h -1 17. From the results of FIG. 17, in the case of the catalyst composition of Example 8, although there is a slight difference in the behavior of the change in the ammonia synthesis rate over time, it is clear that the Ru / BaTbO 2 H, Ru / BaDyO 2 H, Ru / BaHoO 2 H, BaErO 2 H, BaYbO 2 H, Ru / BaLuO 2 In H, a constant ammonia synthesis rate was observed after 40 hours had passed since the start of the reaction. This confirmed that the above catalyst composition is also suitable for long-term ammonia synthesis.
[0108] Figure 18 shows the results of H 2 and N 2 Under the flow of a mixture of 2 :N 2 The catalyst composition of Example 8 (i.e., Ru-supported perovskite-type oxyhydride (BaTbO)) when exposed to a 3:1 2 H,BaDyO 2 H, BaHoO 2 H, BaErO 2 H, BaYbO 2 H, BaLuO 2 H, after sintering), the catalyst composition of Example 2 (i.e., Ru-supported perovskite-type oxyhydride (BaYO) 2 H, after sintering) and the catalyst composition of Example 3 (i.e., Ru-supported perovskite-type oxyhydride (BaScO 2 18 shows the ammonia synthesis rate for the samples (H, after sintering treatment). The results in FIG. 18 confirmed that all samples exhibited a high ammonia synthesis rate. In particular, the ammonia synthesis rate was significantly higher when RE was Sc. From the results in Table 1, the particle size of Ru when RE was Sc was about 3 / 4 of that when Y was used, and about 1 / 2 to 1 / 3 of that of the lanthanides from Tb to Lu. Therefore, it is expected that when RE was Sc, the number of catalytic reaction active sites was greater than that of the other catalyst compositions, and this is thought to be why a significantly higher ammonia synthesis rate was achieved.
[0109] S1 1st process, S2 2nd process
Claims
1. A catalyst composition comprising a perovskite-type oxyhydride represented by the following formula (1): BaREO 2 H m ... (1) (In formula (1), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and m represents a number included in the range of 0.5 to 1.0.) 2. The catalyst composition according to claim 1, wherein said RE is at least one rare earth element selected from the group consisting of Y, Sc, Tb, Dy, Ho, Er, Yb and Lu.
3. The catalyst composition according to claim 1, wherein said RE is Y or Sc.
4. The catalyst composition according to claim 1, which is used for an ammonia synthesis reaction or an ammonia decomposition reaction.
5. The catalyst composition according to claim 1, wherein the perovskite-type oxyhydride supports one or more transition metals selected from the group consisting of Ru, Co, Fe, Cr and Mn.
6. A method for synthesizing ammonia, comprising the step of reacting nitrogen with hydrogen in the presence of the catalyst composition according to any one of claims 1 to 5.
7. A method for decomposing ammonia, comprising the step of decomposing ammonia into hydrogen and nitrogen in the presence of the catalyst composition according to any one of claims 1 to 5.
8. BaREO according to the following formula (1) 2 H m (1) (in formula (1), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and m represents a number included in the range of 0.5 to 1.0), the method for producing a perovskite-type oxyhydride represented by the following formula (1) is provided, the method comprising: 2 and the following formula (2) RE 2 O 3 ...(2): (in formula (2), RE represents a rare earth element selected from the group consisting of Y, Sc, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu), and 9. The method for producing a perovskite-type oxyhydride according to claim 8, wherein said RE is at least one rare earth element selected from the group consisting of Y, Sc, Tb, Dy, Ho, Er, Yb and Lu.
10. The method for producing a perovskite-type hydride according to claim 8, wherein said RE is Y or Sc.
11. The method for producing a perovskite-type oxyhydride according to claim 8, wherein said RE is Y.
12. The method for producing a perovskite-type oxyhydride according to claim 7, characterized in that a planetary ball mill or a tumbling ball mill is used in the mechanochemical method.
13. The method for producing a perovskite-type oxyhydride according to claim 8, wherein the pressing and crushing are carried out at a temperature of 300° C. or less.
14. The specific surface area of the particles of the finely divided and homogenized synthetic reaction product is 5.0 m 2 9. The method for producing a perovskite-type oxyhydride according to claim 8, wherein the Mo content is 0.1 to 1.0 wt %.
15. A perovskite-type oxyhydride obtainable by the method for producing a perovskite-type oxyhydride according to claim 8.
16. The perovskite-type oxyhydride according to claim 15, wherein said RE is Y.
Citation Information
Patent Citations
Perovskite type composite oxide
JP2008100902A
Hydride ion conductor and production method thereof
JP2017098067A
Oxynitride hydride, metal carrier containing oxynitride hydride, and catalyst for ammonia synthesis
WO2020175558A1
Metal oxyhydride production method, metal oxyhydride, and ammonia synthesis method using same
WO2021006136A1