Marine biodegradable polymer compound having aliphatic unsaturated carbon-carbon bond and method for producing same
The marine biodegradable polymer compound with aliphatic unsaturated bonds and anionic groups addresses the challenge of biodegradability in low-microorganism environments by decomposing in seawater, enhancing the biodegradation of resin materials and reducing oceanic pollution while maintaining physical properties.
Patent Information
- Application Number
- PCT/JP2024/016244
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-04-25
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional biodegradable resins exhibit high biodegradability in environments with abundant microorganisms but fail to decompose in low-microorganism environments like the ocean, and starch-based resins have inferior physical properties and reduced biodegradability when mixed with polyester resins.
A marine biodegradable polymer compound with aliphatic unsaturated carbon-carbon bonds and anionic groups, which decomposes in seawater through ion exchange with metal cations, promoting biodegradation by increasing the specific surface area and facilitating the breakdown of resin materials.
The polymer compound enhances biodegradability in seawater, accelerating the decomposition of resin materials and reducing environmental pollution, while maintaining physical properties, thus addressing the limitations of existing biodegradable resins in oceanic environments.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Marine biodegradable polymer compound having aliphatic unsaturated carbon-carbon bond and method for producing same
[0001] The present invention relates to marine biodegradable polymer compounds having aliphatic unsaturated carbon-carbon bonds and a method for producing the same.
[0002] In recent years, environmental pollution (marine pollution) and adverse effects on ecosystems caused by microplastics have become a problem, and various efforts have been launched to reduce the environmental burden. Among these efforts, the development and widespread use of biodegradable resins has been attracting attention.
[0003] On the other hand, while general biodegradable resins exhibit high biodegradability in environments such as soil and sludge where there are many microorganisms responsible for decomposition, they have the disadvantage of being difficult to decompose in environments with extremely low microbial concentrations, such as the ocean (Non-Patent Document 1). Furthermore, even for resins that have been reported to be biodegradable in the ocean, such as polycaprolactone (PCL) and polyhydroxyalkanoic acid (PHA), it has been found that the decomposition rate varies significantly depending on the type of seawater, and it has been reported that this is influenced by various factors, such as the presence or absence of decomposing bacteria in the seawater, the number of bacteria, salt concentration, pH, water temperature, dissolved oxygen concentration, and amount of dissolved organic carbon (Non-Patent Document 2).
[0004] Furthermore, starch-based resins have also been put to practical use as biodegradable resins and are on the market, but because the physical properties of starch alone are significantly inferior, most of them are mixed with polyester-based resins such as polybutylene adipate / terephthalate (PBAT) and polylactic acid (PLA), which are difficult to biodegrade in the ocean. As a result, even starch-based resins tend to have significantly reduced biodegradability in the ocean.
[0005] Under these circumstances, there is a need to develop materials that can be reliably decomposed in any type of seawater while maintaining their physical properties, as well as materials that can act as decomposition accelerators for resins that are difficult to biodegrade in seawater, while also reducing the environmental impact.
[0006] Hideshige Takada, "Current Status of Microplastic Pollution, International Trends and Countermeasures," Journal of the Japanese Society of Material Cycles and Waste Management, Vol. 29, No. 4, pp. 261-269, 2018; Akira Ebisui and four others, "Decomposition of Biodegradable Plastics in Seawater," Journal of Fisheries Engineering, Vol. 40, No. 2, pp. 143-149, 2003
[0007] The present invention has been made in view of the above circumstances, and provides a polymer compound that induces biodegradability in the ocean, and a marine biodegradable resin composition using the same.
[0008] As a result of extensive research into solving the above problems, the present inventors have found that a polymerizable compound having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond in the main chain, and has one or more -COO - R + , -SO3 - R + , —O—SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) We have found that marine biodegradable polymer compounds having a substituent selected from the group consisting of a hydrogen ion, a monovalent metal cation, and a monovalent organic cation in a side chain exhibit high marine biodegradability. In particular, we have found that polymer compounds in which prepolymer compounds having anionic groups contained in the marine biodegradable polymer compound are bonded via divalent or higher metal cations have high strength because the side chains are bonded via the metal cations, and that in seawater, the molecules of the polymer compound are cleaved by ion exchange with monovalent cations such as sodium and potassium, thereby accelerating marine biodegradation.
[0009] Furthermore, the inventors discovered that by using this material in combination with a resin, particularly a biodegradable resin, the material undergoes primary decomposition in seawater first, resulting in (1) the formation of pores in the resin material, which increases the specific surface area of the resin and promotes the growth of microorganisms responsible for decomposition, and (2) the primary decomposition promotes secondary decomposition, i.e., biodegradation by microorganisms, thereby ultimately promoting the biodegradation of resin materials in the ocean, thereby completing the present invention.
[0010] That is, the present invention provides the following marine biodegradable polymer compound and a method for producing the same: 1. A polymer compound containing a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, having an aliphatic unsaturated carbon-carbon bond in the main chain, and having one or more -COO - R + , -SO3 - R + , —O—SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation. 2. The marine biodegradable polymer compound of 1 having two or more acidic groups in the side chain. 3. The marine biodegradable polymer compound of 1 or 2, wherein the repeating unit contains an ester bond. 4. Any of 1 to 3, wherein the number average molecular weight is 300 to 100,000. 5. The marine biodegradable polymer compound of 1 or 2, wherein the number average molecular weight is 300 to 100,000. 6. The marine biodegradable polymer compound of 1 or 2, wherein the number average molecular weight is 300 to 100,000. 7. The marine biodegradable polymer compound of 1 or 2, wherein the number average molecular weight is 300 to 100,000. - R + , -SO3 - R + , —O—SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R +is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation. 6. Any of the marine biodegradable polymer compounds of 1 to 5, having a substituent selected from the group consisting of: -COO, -COO- ... - R + 9. The marine biodegradable polymer compound of any one of 1 to 8, which has maleic acid residues in the main chain. 10. R + is a monovalent metal cation or a monovalent organic cation. 11. A marine biodegradable polymer compound in which a polymeric polyvalent anion derived from the marine biodegradable polymer compound in any one of 1 to 10 is bonded via a divalent or higher metal cation. 12. A marine biodegradable polymer compound in which the content of the metal cation is 1 to 100 eq / 10 5g. 13. The marine biodegradable polymer compound of 11 or 12, wherein the divalent or higher metal cation is calcium ion, magnesium ion, or aluminum. 14. A marine biodegradation promoter comprising the marine biodegradable polymer compound of any of 1 to 13. 15. A marine biodegradable resin composition comprising the marine biodegradation promoter of 14 and a resin. 16. The marine biodegradable resin composition of 15, wherein the resin is a biodegradable resin. 17. The marine biodegradable resin composition of 16, wherein the content of the marine biodegradation promoter is 1 to 50 mass % and the content of the biodegradable resin is 50 to 99 mass %. 18. A molded article obtained from the marine biodegradable resin composition of any of 15 to 17. 19. 19. A method for producing a marine biodegradable polymer compound, comprising a step of reacting a polymer compound having an aliphatic unsaturated carbon-carbon bond in its main chain, and comprising repeating units containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, with a compound having a reactive group reactive with an aliphatic unsaturated carbon-carbon bond and a substituent selected from -COOH, -S03H, -O-S03H, and -P(=O)(OH)-OH. 20. A method for producing a marine biodegradable polymer compound, comprising a step of neutralizing, with a monovalent base, the substituent of a marine biodegradable polymer compound having repeating units containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, and having an aliphatic unsaturated carbon-carbon bond in its main chain and one or more substituents selected from -COOH, -S03H, -O-S03H, and -P(=O)(OH)-OH in its side chain. 21. 21. A method for producing a marine biodegradable polymer compound according to claim 20, wherein the base is lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, or potassium hydrogen carbonate. 22. A method for producing a marine biodegradable polymer compound according to claim 20, wherein the base is lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, or potassium hydrogen carbonate. - R + , -SO3 - R + , —O—SO3 - R+ and -P(=O)(OH)-O - R + (In the formula, R + 22. A method for producing a marine biodegradable polymer compound, the method comprising the step of crosslinking a marine biodegradable polymer compound having, in a side chain, a substituent selected from the group consisting of a hydrogen ion, a monovalent metal cation, and a monovalent organic cation, using a polyvalent metal salt. 23. A method for producing a marine biodegradable polymer compound according to claim 22, wherein the polyvalent metal salt is a calcium salt, a magnesium salt, or an aluminum salt.
[0011] The marine biodegradable polymer compound of the present invention has marine biodegradability and exhibits characteristic physical properties derived from the substituents and unsaturated bonds in the side chains. Furthermore, the marine biodegradable polymer compound gradually dissolves in seawater upon contact with seawater or exhibits hydrophilicity, so that resin compositions and molded articles containing the same exhibit accelerated biodegradation in the ocean and are useful for combating marine pollution. The marine biodegradable polymer compound has marine biodegradability, so that compositions and molded articles containing the same exhibit accelerated biodegradation in the ocean and are useful for combating marine pollution. Environmentally friendly compositions and molded articles can be obtained by using a marine biodegradation promoter made from the marine biodegradable polymer compound of the present invention.
[0012] [Marine biodegradable polymer compound A] A first embodiment of the marine biodegradable polymer compound of the present invention comprises a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond (hereinafter simply referred to as an aliphatic unsaturated bond) in the main chain, and has one or more -COO - R + , -SO3 - R + , —O—SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R +is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) The aliphatic unsaturated bond may be a double bond or a triple bond, but a double bond is preferred in consideration of the stability and reactivity of the structure.
[0013] The marine biodegradable polymer compound A may have two or more of the above-mentioned substituents on the side chain. When the polymer compound A has two or more of the above-mentioned substituents, the respective substituents may be the same as or different from each other.
[0014] From the viewpoint of mechanical properties and biodegradability, the repeating units constituting the marine biodegradable polymer compound A preferably contain an ester bond or an amide bond, more preferably contain an ester bond, and most preferably contain an ester bond formed by polycondensation of a dicarboxylic acid and a diol in the repeating unit.
[0015] The marine biodegradable polymer compound A preferably has a molecular weight of 300 to 100,000, and in consideration of biodegradability in seawater and mechanical properties, it is more preferably 300 to 10,000, even more preferably 500 to 5,000, even more preferably 700 to 4,000, and most preferably 900 to 3,000. Molecular weights within the above ranges are preferred because they provide good biodegradability and mechanical properties. In the present invention, the molecular weight refers to the number average molecular weight determined by the terminal group quantitative method.
[0016] The marine biodegradable polymer compound A must have the above-mentioned substituents on the side chains, but may also have the above-mentioned substituents at the ends of the main chain. In this case, the substituents may be present at both ends or only at one end, which can be adjusted depending on the desired physical properties, biodegradability, and water solubility. The substituents at the ends of the main chain may be the same as or different from the substituents on the side chains.
[0017] In the marine biodegradable polymer compound A, it is preferable that the number of the substituents is an appropriate number of acidic groups relative to the number average molecular weight, taking into consideration the physical properties, biodegradability, and water solubility. Specifically, the value obtained by dividing the number average molecular weight by the average number of acidic groups per molecule is preferably 100 to 10,000, more preferably 200 to 5,000, even more preferably 300 to 5,000, and most preferably 500 to 1,000.
[0018] The marine biodegradable polymer compound A has aliphatic unsaturated carbon-carbon bonds in the main chain, and the number of aliphatic unsaturated carbon-carbon bonds per molecule is preferably 0.1 to 50 on average, more preferably 0.5 to 25, and even more preferably 1 to 10, so as to achieve both strength and biodegradability.
[0019] The substituents on the side chains may be bonded directly to the main chain or via a linking group; however, in consideration of mechanical properties, the substituents are preferably bonded via a linking group having 1 to 50 atoms, more preferably via a linking group having 2 to 30 atoms, and even more preferably via a linking group having 5 to 25 atoms. The structure of the linking group may be linear, branched, or cyclic, but is preferably linear or branched, and more preferably linear. Furthermore, the atoms constituting the linking group are not particularly limited, but the linking group preferably contains at least one atom selected from carbon, oxygen, nitrogen, boron, sulfur, phosphorus, and silicon atoms, and more preferably contains at least one atom selected from carbon, oxygen, nitrogen, and sulfur atoms.
[0020] Considering the environmental impact and ease of handling, the substituent is preferably —COO - R + , -SO3 - R + Preferably, -COO - R + It is particularly preferred that:
[0021] The aliphatic unsaturated bond in the marine biodegradable polymer compound A may be derived from any monomer, but considering the ease of introduction, cost, and risk of side reactions, it is preferable that the aliphatic unsaturated bond is derived from a polyol compound having an aliphatic unsaturated bond or a polycarboxylic acid compound having an aliphatic unsaturated bond, and it is more preferable that the aliphatic unsaturated bond is derived from a dicarboxylic acid compound having an aliphatic unsaturated bond.
[0022] Specific examples of the polyol compound having an aliphatic unsaturated bond are preferably diol compounds having an aliphatic unsaturated bond such as 2-butene-1,4-diol, 3-hexene-1,6-diol, 4-hydroxy-2-(hydroxymethyl)-2-cyclopenten-1-one, etc. The polyol compound having an aliphatic unsaturated bond may be a commercially available product or a synthesized product.
[0023] Specific examples of the polycarboxylic acid compound having an aliphatic unsaturated bond include dicarboxylic acids having an aliphatic unsaturated bond such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, 2-pentenedioic acid, methylenesuccinic acid, allylmalonic acid, isopropylidenesuccinic acid, 2,4-hexadienedioic acid, and acetylenedicarboxylic acid, but in consideration of reactivity, solubility, and physical properties of the product, fumaric acid and maleic acid are preferred, and maleic acid is more preferred. The polycarboxylic acid compound having an aliphatic unsaturated bond may be a commercially available product or a synthesized product.
[0024] The marine biodegradable polymer compound A preferably has a relative cellulose biodegradability of 40% or more. In the present invention, the relative cellulose biodegradability refers to the degree of decomposition of cellulose 60 days after immersion in seawater. The marine biodegradable polymer compound A more preferably has a relative cellulose biodegradability of 50% or more, even more preferably 60% or more, and most preferably 80% or more. The relative cellulose biodegradability can be measured according to ASTM D6691, known marine biodegradation test methods, or BOD modified with reference to these methods.
[0025] The marine biodegradable polymer compound A preferably has a softening point or melting point suitable for the melting temperature of the resin. The polymer compound is solid or liquid at room temperature. More specifically, the lower limit of the softening point or melting point is preferably 0°C or higher, 25°C or higher, 40°C or higher, 80°C or higher, or 100°C or higher, in that order, and the upper limit is preferably 180°C or lower, 150°C or lower, or 120°C or lower, in that order. In consideration of handleability, the softening point or melting point is preferably within the range of 0 to 180°C, more preferably 25 to 120°C.
[0026] [Method for producing marine biodegradable polymer compound A] In the marine biodegradable polymer compound A, + is a hydrogen ion (i.e., a polymer having a substituent selected from —COOH, —SOH, —O—SOH, and —P(═O)(OH)—OH (hereinafter also referred to as marine biodegradable polymer compound A1) can be produced by a method including a step of reacting a polymer compound (hereinafter also referred to as polymer compound P) that contains repeating units containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, and that has an aliphatic unsaturated carbon-carbon bond in the main chain, with a compound (hereinafter also referred to as compound Q) that has a reactive group reactive with an aliphatic unsaturated carbon-carbon bond and a substituent selected from —COOH, —SOH, —O—SOH, and —P(═O)(OH)—OH (hereinafter these are collectively referred to as acidic group A).
[0027] Examples of the polymer compound P include an unsaturated polyester compound, an unsaturated polyamide compound, an unsaturated polycarbonate compound, an unsaturated polyurethane compound, and an unsaturated polyurea compound. An unsaturated polyester compound or an unsaturated polyamide compound is preferred, and an unsaturated polyester compound is more preferred.
[0028] The unsaturated polyester compound can be produced, for example, by polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond with a polyol compound containing a polyol compound having no aliphatic unsaturated bond, polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having no aliphatic unsaturated bond with a polyol compound containing a polyol compound having an aliphatic unsaturated bond, or polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond with a polyol compound containing a polyol compound having an aliphatic unsaturated bond. When producing unsaturated polyesters, known polyester polymerization methods can be used, such as the method described in Sen to Kogyo (Senbi to Kogyo), Vol. 40, No. 4.5, pp. 259-261, 1984. Commercially available unsaturated polyester compounds may also be used.
[0029] Specific examples of the polycarboxylic acid compound having an aliphatic unsaturated bond and the polyol compound having an aliphatic unsaturated bond include those mentioned above.
[0030] Specific examples of the polyol compound having no aliphatic unsaturated bonds include saturated diol compounds such as ethylene glycol, 1,3-propanediol, and 1,4-butanediol, with 1,4-butanediol being preferred in terms of reactivity, solubility, and physical properties of the product. The polyol compound having no aliphatic unsaturated bonds may be a commercially available product or a synthesized product.
[0031] Specific examples of the polycarboxylic acid compound having no aliphatic unsaturated bond include saturated polycarboxylic acids and aromatic polycarboxylic acids such as succinic acid, glutaric acid, adipic acid, sebacic acid, terephthalic acid, isophthalic acid, trimellitic acid, pyromellitic acid, etc. The polycarboxylic acid compound having no aliphatic unsaturated bond may be a commercially available product or a synthesized product.
[0032] The unsaturated polyester compound is preferably produced by polycondensation of a polycarboxylic acid compound containing a dicarboxylic acid compound having an aliphatic unsaturated bond and a polyol compound containing a diol compound having no aliphatic unsaturated bond.
[0033] In this case, the polycarboxylic acid compound used as the raw material may contain a polycarboxylic acid compound having no aliphatic unsaturated bond in addition to the dicarboxylic acid compound having an aliphatic unsaturated bond. Specific examples of the polycarboxylic acid compound having no aliphatic unsaturated bond include succinic acid, glutaric acid, adipic acid, sebacic acid, terephthalic acid, isophthalic acid, trimellitic acid, and pyromellitic acid. However, in consideration of reactivity, solubility, and physical properties of the product, succinic acid or adipic acid is preferred, and succinic acid is more preferred. The content of the polycarboxylic acid compound having no aliphatic unsaturated bond in the carboxylic acid compound used as the raw material is preferably 0 to 80 mol%, more preferably 10 to 40 mol%, and most preferably 30 to 60 mol%.
[0034] Furthermore, the polyol compound as a raw material may contain a polyol compound of triol or higher in addition to the diol compound. Specific examples of the polyol compound include monosaccharides such as glycerin, trimethylolpropane, pentaerythritol, and glucose, but in consideration of reactivity, solubility, and physical properties of the product, glycerin or trimethylolpropane is preferred, and glycerin is more preferred. The content of the polyol compound of triol or higher in the polyol compound as a raw material is preferably 0.01 to 5 mol%, more preferably 0.05 to 3 mol%, and most preferably 0.1 to 1 mol%.
[0035] In the polymerization reaction of the unsaturated polyester compound, polycondensation catalysts such as antimony trioxide, germanium catalysts, and titanium catalysts; or catalysts generally used in transesterification such as magnesium acetate and manganese acetate, may be used as needed to promote the reaction. Considering the environmental impact, metal-free catalysts are preferred. The amount of the catalyst used is preferably about 0.01 to 5 parts by mass per 100 parts by mass of the raw material compound.
[0036] The unsaturated polyamide compound can be produced, for example, by polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond with a polyamine compound containing a polyamine compound having no aliphatic unsaturated bonds, polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having no aliphatic unsaturated bonds with a polyamine compound containing a polyamine compound having an aliphatic unsaturated bond, or polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond with a polyamine compound containing a polyamine compound having an aliphatic unsaturated bond. The polycarboxylic acid can be the aforementioned compound, and the polyamine having an aliphatic unsaturated bond can be a diamine compound having an aliphatic unsaturated bond, such as 2-butene-1,4-diamine or 3-hexene-1,6-diamine. When producing a polyamide having an aliphatic unsaturated bond, known polyamide polymerization methods can be used, such as those described in JP-B-52-12233 and JP-B-5-71056. Moreover, as the polyamide compound having an aliphatic unsaturated bond, commercially available products may be used.
[0037] In the polymerization reaction of the unsaturated polyamide, a polycondensation catalyst such as a metal salt, ammonium salt, or ester of phosphoric acid, phosphorous acid, or hypophosphorous acid may be used as needed to promote the reaction. The amount of the catalyst used is preferably about 0.01 to 5.0 parts by mass per 100 parts by mass of the raw material compound.
[0038] The unsaturated polycarbonate compound can be produced, for example, by polycondensing a carbonate ester such as diphenyl carbonate or phosgene, or a carbonate chloride, with a polyol compound having an aliphatic unsaturated bond. Examples of polyol compounds having an aliphatic unsaturated bond that can be used include diol compounds having an aliphatic unsaturated bond, such as 2-butene-1,4-diol and 3-hexene-1,6-diol. When producing the unsaturated polycarbonate compound, known polycarbonate polymerization methods can be used, such as the methods described in JP-A-2013-010948 and JP-A-2016-94589. Furthermore, commercially available products may also be used as the unsaturated polycarbonate compound.
[0039] In the polymerization reaction of the unsaturated polycarbonate, for the purpose of promoting the reaction, a polycondensation catalyst such as antimony trioxide, a germanium catalyst, a titanium catalyst, etc.; or a catalyst generally used in transesterification such as magnesium acetate, manganese acetate, etc. The amount of the catalyst used is preferably about 0.01 to 1.0 part by mass per 100 parts by mass of the raw material compound.
[0040] The unsaturated polyurethane compound can be produced, for example, by polyaddition of a polyisocyanate such as hexamethylene diisocyanate or diphenylmethane diisocyanate with a polyol compound including a diol compound having an aliphatic unsaturated bond, an unsaturated polyester compound having a hydroxy group prepared using the method described above, or an unsaturated polycarbonate compound having a hydroxy group; polyaddition of a polyisocyanate containing a polyisocyanate having an aliphatic unsaturated bond such as 2-butene-1,4-diisocyanate or 3-hexene-1,6-diisocyanate with a polyol compound; or polyaddition of a polyisocyanate containing a polyisocyanate having an aliphatic unsaturated bond with a diol compound having an aliphatic unsaturated bond or a polyol including a polyol compound having an aliphatic unsaturated bond described above. When producing the unsaturated polyurethane compound, known polyurethane polymerization methods can be used, for example, the methods described in JP-B-52-12233 and JP-B-5-71056 can be used.
[0041] The reaction between a polyol compound having an aliphatic unsaturated bond and a polyisocyanate may be carried out using an amine catalyst such as 1,4-diazabicyclo[2.2.2]octane (DABCO) or 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) or a tin catalyst such as dibutyltin dilaurate, in order to improve reactivity and thereby shorten the reaction time and lower the reaction temperature. Zinc complexes, iron complexes, bismuth complexes, and zirconium complexes similar to the tin complexes are also useful as catalysts. The amount of the catalyst used is preferably about 0.01 to 5 parts by mass per 100 parts by mass of the raw material compound.
[0042] The unsaturated polyurea compound can be produced, for example, by polycondensation of the polyisocyanate with a polyamine compound containing the polyamine compound having an aliphatic unsaturated bond or a polyamine containing an unsaturated polyamide compound having an amino group prepared by the method described above, polycondensation of a polyisocyanate containing a polyisocyanate with a polyamine compound, or polycondensation of a polyisocyanate containing a polyisocyanate with a polyamine compound containing the polyamine compound having an aliphatic unsaturated bond or a polyamine compound containing an unsaturated polyamide compound having an amino group prepared by the method described above. When producing the unsaturated polyurea compound, known polyurea polymerization methods can be used as reference, for example, the method described in JP 2004-27148 A can be used as reference.
[0043] In the polymerization reaction of the unsaturated polyurea compound, a catalyst such as a salt of a metal, such as lithium, sodium, magnesium, aluminum, potassium, titanium, cobalt, germanium, zinc, rubidium, strontium, tin, antimony, cesium, barium, or lead, an alkoxide, or an organometallic compound may be used, if necessary, for the purpose of promoting the reaction. The amount of the catalyst used is preferably about 0.0001 to 1 part by mass per 100 parts by mass of the raw material compound.
[0044] In the reaction between polymer compound P and compound Q, the amount of compound Q used is preferably 5 to 200 mol % relative to the aliphatic unsaturated bonds in the unsaturated polyester compound. At 5 to 20 mol %, the physical properties derived from the double bonds are strongly exhibited, while at more than 20 mol % but not more than 200 mol %, the physical properties derived from the side chain acidic group A are strongly exhibited. Therefore, the amount may be adjusted depending on the purpose.
[0045] The reaction between polymer compound P and compound Q is not particularly limited, and may be, for example, a conjugate addition reaction, a radical reaction, a Diels-Alder reaction, or a photocycloaddition reaction. However, in consideration of reactivity, selectivity, and the physical properties of the product, a conjugate addition reaction is preferred. Particularly preferred examples of the reaction include the addition reaction of mercaptocarboxylic acid, amino acid, malonic acid derivative, or the like to an aliphatic unsaturated bond of a polyester compound having a maleic acid residue.
[0046] In the reaction between polymer compound P and compound Q, a commonly used catalyst may be used as necessary. Examples of such a catalyst include base catalysts such as DBU and TEA in conjugate addition reactions, transition metal catalysts such as organoruthenium complexes and organotitanium complexes in radical reactions, Lewis acid catalysts such as ytterbium triflate and scandium triflate in Diels-Alder reactions, and photosensitizers such as thiophene and benzophenone in photocycloaddition reactions.
[0047] Compound Q can be appropriately selected depending on the target reaction. For example, in the case of a conjugate addition reaction, examples of compound Q include nucleophilic organic acids and derivatives thereof, such as mercaptocarboxylic acids such as 3-mercaptopropionic acid, amino acids such as 5-aminovaleric acid and 6-aminohexanoic acid, aminosulfonic acids such as 2-aminoethanesulfonic acid, aminophosphoric acids such as ethanolamine phosphate, malonic acid, and organocopper ate complexes. In the case of a radical reaction, examples include carboxylic acids and sulfonic acids having an unsaturated bond, such as acrylic acid, 3-pentenoic acid, carboxystyrene, and styrenesulfonic acid. In the case of a Diels-Alder reaction, examples include pyrrole carboxylic acids such as 1-methyl-2-pyrrolecarboxylic acid. In the case of a photocycloaddition reaction, examples include carboxylic acids having an unsaturated bond, such as acrylic acid and 3-pentenoic acid. Considering reactivity, selectivity, physical properties of the product, and safety, it is preferable to use 3-mercaptopropionic acid, 5-aminovaleric acid, 6-aminohexanoic acid, or a malonic acid derivative in the conjugate addition reaction, and it is most preferable to use 3-mercaptopropionic acid in the conjugate addition reaction. The compound Q may be a commercially available product or a synthesized product.
[0048] The compound Q may be used as it is with the acidic group A, or the acidic group A may be protected by esterification or the like as necessary, and then deprotected to form the acidic group A after the reaction between the polymer compound P and the compound Q.
[0049] In the marine biodegradable polymer compound A, the R + A marine biodegradable polymer compound A2, in which some or all of the acidic groups A in the marine biodegradable polymer compound A1 are monovalent metal cations or monovalent organic cations, can be synthesized by neutralizing some or all of the acidic groups A in the marine biodegradable polymer compound A1.
[0050] In the marine biodegradable polymer compound A2, the substituent R + As the cation, a lithium ion, a sodium ion, a potassium ion, a rubidium ion, a cesium ion, a francium ion, an ammonium ion, a methylammonium ion, an ethylammonium ion, an anilinium ion, a pyridinium ion, a dimethylammonium ion, a diethylammonium ion, a trimethylammonium ion, a triethylammonium ion, and the like are preferred, and from the viewpoints of safety, environmental load, and operability, sodium ions, potassium ions, and ammonium ions are more preferred, and sodium ions and potassium ions are even more preferred.
[0051] The neutralization reaction is not particularly limited and can be carried out using, for example, an inorganic base and / or an organic base capable of reacting with an acidic group. Examples of the base include lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, trisodium phosphate, tripotassium phosphate, lithium methoxide, sodium methoxide, potassium methoxide, lithium tert-butoxide, sodium tert-butoxide, potassium tert-butoxide, ammonia, methylamine, ethylamine, TEA, and DBU. Among these, lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, or potassium bicarbonate is preferred, and in consideration of safety and environmental impact, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, or potassium bicarbonate is particularly preferred.
[0052] [Marine biodegradable polymer compound B] A second aspect of the marine biodegradable polymer compound of the present invention is a marine biodegradable polymer compound (hereinafter also referred to as marine biodegradable polymer compound B) obtained by crosslinking marine biodegradable polymer compound A with a divalent or higher metal cation. That is, marine biodegradable polymer compound B contains a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond in the main chain, and has one or more -COO - , -SO3 - , —O—SO3 - and -P(=O)(OH)-O - The polymer has a structure in which an anionic polymer compound having a monovalent anionic substituent selected from the group consisting of the following at its side chain is bonded by an ionic bond with a divalent or higher metal cation.
[0053] The divalent or higher metal cation is not particularly limited, but examples thereof include calcium ions, beryllium ions, magnesium ions, strontium ions, barium ions, zinc ions, aluminum ions, iron ions, copper ions, platinum ions, gold ions, titanium ions, nickel ions, cobalt ions, manganese ions, zirconium ions, ruthenium ions, rhodium ions, palladium ions, scandium ions, gallium ions, indium ions, and radium ions. Among these, calcium ions, beryllium ions, magnesium ions, strontium ions, barium ions, zinc ions, and aluminum ions are preferred, with calcium ions, magnesium ions, and aluminum ions being more preferred. The divalent or higher metal cation may be used alone or in combination.
[0054] The metal ion equivalent in the marine biodegradable polymer compound is 1 to 100 eq / 10 5 g is preferable, but considering biodegradability in seawater and mechanical properties, 2 to 80 eq / 10 5 g is more preferable, and 10 to 50 eq / 10 5 It is more preferable that the metal ion equivalent is in the above range, since the biodegradability is good and the mechanical properties are not impaired. The metal ion equivalent is a value measured by inductively coupled plasma mass spectrometry (ICP-MS).
[0055] The marine biodegradable polymer compound B is formed by bonding at least two marine biodegradable polymer compounds A2 via a metal cation, and may contain only one type of marine biodegradable polymer compound A2, or may contain multiple different types of marine biodegradable polymer compound A2, or may further contain other anionic compounds simultaneously. Examples of such anionic compounds include carboxylate anions, sulfonate anions, and polymer compounds having anionic groups at their terminals and a number average molecular weight of 500 to 10,000.
[0056] The marine biodegradable polymer compound B can have a linear, branched, crosslinked network, or other structure. When the polymer compound B is linear or branched, its molecular weight is preferably 600 to 1,000,000, more preferably 1,000 to 500,000, even more preferably 5,000 to 300,000, and most preferably 10,000 to 100,000. While typical biodegradable resins, as described below, exhibit high biodegradability in environments where decomposition microorganisms are abundant, such as soil and sludge, they have the disadvantage of being difficult to decompose in environments with extremely low microbial concentrations, such as the ocean. The inventors focused on metal ions abundant in seawater and the stable salt concentration in the ocean. They speculate that the marine biodegradable polymer compound B decomposes by ion exchange in seawater (reducing molecules by cleavage) and chemically reduces molecules, allowing efficient degradation even in environments with few biodegrading microorganisms. By setting the molecular weight of the marine biodegradable polymer compound B within the above range, biodegradability in the ocean can be promoted more efficiently, while the resin composition used during normal use is also physically useful.
[0057] The marine biodegradable polymer compound B preferably has a softening point or melting point suitable for the melting temperature of the resin. The polymer compound is solid at room temperature, and more specifically, the lower limit of the softening point or melting point is preferably 40°C or higher, 50°C or higher, and 60°C or higher, in that order, and the upper limit is preferably 250°C or lower, 180°C or lower, 160°C or lower, and 140°C or lower, in that order. When the resin is a biodegradable resin, it preferably has a softening point or melting point within the range of 40 to 200°C, more preferably 50 to 160°C, and even more preferably 60 to 140°C.
[0058] The marine biodegradable polymer compound B preferably has a relative cellulose biodegradability of 40% or more. In the present invention, the relative cellulose biodegradability refers to the degree of decomposition of cellulose 60 days after immersion in seawater. The marine biodegradable polymer compound B more preferably has a relative cellulose biodegradability of 50% or more, even more preferably 60% or more, and most preferably 80% or more. The relative cellulose biodegradability can be measured according to ASTM D6691, known marine biodegradation test methods, or BOD modified with reference to these methods.
[0059] [Method for Producing Marine Biodegradable Polymer Compound B] The marine biodegradable polymer compound B can be produced by a method including a step of crosslinking the marine biodegradable polymer compound A with a polyvalent metal salt.
[0060] Examples of the crosslinking treatment method include a method in which a powder or solution of a polyvalent metal salt is dropped into a medium in which the marine biodegradable polymer compound A is dissolved, and precipitation or precipitating takes place while a bonding treatment is being carried out; a method in which a powder or solution of a polyvalent metal salt is dropped into a molten liquid of the marine biodegradable polymer compound A, and a bonding treatment is carried out; and a method in which a solution in which the marine biodegradable polymer compound A is dissolved is dropped into a powder of a polyvalent metal salt or a solution in which the polyvalent metal salt is dissolved, and precipitation or precipitating takes place while a bonding treatment is being carried out.
[0061] In a preferred example, a solution of the marine biodegradable polymer compound A2 is prepared in water, an organic solvent, or a mixed solvent thereof, or a melt of the marine biodegradable polymer compound A2 is heated to dissolve the polymer. Heating may be performed as necessary to improve solubility or reduce the viscosity of the melt. A solution containing a divalent or higher metal salt is then added to the resulting solution or melt, followed by stirring. Alternatively, a solution of the marine biodegradable polymer compound A2 may be added to a solution containing a divalent or higher metal salt, followed by stirring.
[0062] Examples of the polyvalent metal salt include calcium salt, strontium salt, magnesium salt, barium salt, radium salt, lead salt, zinc salt, nickel salt, iron salt, copper salt, cadmium salt, cobalt salt, manganese salt, aluminum salt, gallium salt, indium salt, and thallium salt. However, calcium salt, magnesium salt, and aluminum salt are preferred from the viewpoints of being metals contained in seawater, environmental aspects, safety, and versatility, and calcium salt and magnesium salt are more preferred in consideration of the seawater environment. Specific examples of the polyvalent metal salt include calcium chloride, calcium sulfate, calcium carbonate, calcium hydroxide, calcium oxide, magnesium chloride, magnesium sulfate, magnesium carbonate, magnesium hydroxide, magnesium oxide, aluminum sulfate, sodium aluminum sulfate (sodium alum), and potassium aluminum sulfate (potassium alum). However, calcium chloride, magnesium chloride, and aluminum sulfate are preferred from the viewpoints of water solubility, handling, cost, and the like.
[0063] Furthermore, neutralization and bonding via a divalent or higher metal cation can be carried out simultaneously by neutralizing the acidic group A of the marine biodegradable polymer compound A1 with a base containing a divalent or higher metal.
[0064] In a preferred example, a solution of the marine biodegradable polymer compound A1 is prepared in water, an organic solvent, or a mixed solvent thereof, or a melt of the marine biodegradable polymer compound A1 is heated to dissolve the polymer. Heating may be performed as necessary to improve solubility or reduce the viscosity of the melt. Next, a solution of a base containing a divalent or higher metal is added to the resulting solution or melt and stirred. Alternatively, a solution of the marine biodegradable polymer compound A1 may be added to a solution of a base containing a divalent or higher metal and stirred.
[0065] Examples of the base containing a divalent or higher metal include magnesium hydride, strontium hydride, calcium hydride, barium hydride, magnesium methoxide, calcium methoxide, strontium methoxide, barium methoxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium oxide, strontium oxide, calcium oxide, barium oxide, magnesium carbonate, strontium carbonate, calcium carbonate, barium carbonate, magnesium hydrogencarbonate, strontium hydrogencarbonate, calcium hydrogencarbonate, and barium hydrogencarbonate. From the viewpoints of solubility in water, reactivity, cost, and the like, calcium hydride, calcium methoxide, calcium hydroxide, and barium hydroxide are preferred, and calcium hydroxide is more preferred.
[0066] The concentration of the polyvalent metal salt in the solution containing the polyvalent metal salt or the concentration of the base in the solution containing a base containing a divalent or higher metal is preferably 1 to 40% by mass, more preferably 10 to 30% by mass. The solvent for the solution is preferably water, a lower alcohol solvent such as methanol, ethanol, 1-propanol, or 2-propanol, an amphipathic solvent such as acetone, acetonitrile, THF, DMF, DMSO, or NMP, or a mixed solvent thereof. However, a mixed solvent with other organic solvents may also be used as long as it can dissolve the salt to the desired concentration without dissolving the particles.
[0067] Furthermore, if the polyvalent metal salt or the base containing a divalent or higher metal has good reactivity and reacts even in a solid state, it may be used in a powder form without using a medium, or may be used by dispersing it in a small amount of medium.
[0068] In this way, the marine biodegradable polymer compound A can be bound via the metal cation, and the target marine biodegradable polymer compound B, which gradually becomes insoluble, is obtained as a precipitate, sediment, or bulk. The treatment time is preferably 0.5 to 24 hours, and more preferably 1 to 12 hours.
[0069] At this time, in order to control the particle size and shape (e.g., spherical) of the precipitate or sediment, a surfactant or a polymer stabilizer may be dissolved in at least one of the solution in which the marine biodegradable polymer compound A1 or A2 is dissolved and the solution containing a base containing a divalent or higher metal or a polyvalent metal salt.
[0070] Heating may be carried out when precipitating or precipitating the target marine biodegradable polymer compound B. Heating may be carried out when mixing the solution in which the marine biodegradable polymer compound A1 or A2 is dissolved or the molten liquid of the marine biodegradable polymer compound A1 or A2 with the solution containing the polyvalent metal salt or the base containing a divalent or higher metal, or when stirring after mixing, or both. The heating temperature is preferably 15 to 150°C, more preferably 20 to 100°C, and more preferably 40 to 80°C.
[0071] After the treatment, the particles can be washed and dried as needed to obtain the marine biodegradable polymer compound B. Washing can be carried out by a conventional method, for example, removing the solvent after the binding treatment, adding water, and then centrifuging. Drying can be carried out by a conventional method, for example, spray drying, vacuum drying, freeze drying, or the like. The obtained marine biodegradable polymer compound B may be subjected to a surface treatment or a pulverization treatment using known equipment to adjust the particle size, as needed.
[0072] The marine biodegradable polymer compound B may be one in which at least one end of the anionic polymer compound that is not bonded to itself via a divalent metal cation is blocked with a blocking segment group.
[0073] By selecting the capping segment group, it is possible to incorporate multiple effects in a single material and a composite material (marine biodegradable resin composition) using this material, such as adjustment of melting temperature and melt viscosity, adjustment of crystallinity, adjustment of microbial adhesion and biodegradability, adjustment of physical properties such as resin tensile strength, flexural strength, and elasticity, improvement of compatibility with resin, adjustment of hydrophobicity, adjustment of water repellency, adjustment of adhesion, and adjustment of plasticity, thereby improving both the biodegradability and physical properties of the marine biodegradable resin composition. Since the organic anion that forms the capping segment is desirably a structure that is biodegradable in the marine environment, it is desirable to select a capping segment group that is marine biodegradable and has a molecular weight of 5,000 or less. For example, when emphasis is placed on the rate of biodegradation in the marine environment and the maintenance of average physical properties, a molecular weight of 2,500 or less is preferred, and a molecular weight of 1,000 or less is more preferred.
[0074] Specifically, the blocking segment group preferably has a monovalent hydrocarbon group having 3 or more carbon atoms, more preferably has a monovalent hydrocarbon group having 6 or more carbon atoms, even more preferably has a monovalent hydrocarbon group having 10 or more carbon atoms, and most preferably has a monovalent hydrocarbon group having 12 or more carbon atoms. There are no particular limitations on the upper limit of the number of carbon atoms in the monovalent hydrocarbon group, but it is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.
[0075] The capping segment group is preferably a monovalent organic anion selected from a carboxylate anion having a monovalent hydrocarbon group of 3 or more carbon atoms, a sulfonate anion having a monovalent hydrocarbon group of 3 or more carbon atoms, a sulfate ester anion having a monovalent hydrocarbon group of 3 or more carbon atoms, and a phosphate ester anion having a monovalent hydrocarbon group of 3 or more carbon atoms. Of these, a monovalent organic anion derived from a carboxylic acid having a monovalent hydrocarbon group of 3 or more carbon atoms is preferred, and a monovalent organic anion derived from a fatty acid having a monovalent hydrocarbon group of 3 or more carbon atoms or an amino acid derivative having a monovalent hydrocarbon group of 3 or more carbon atoms is more preferred.
[0076] Terminal blocking can be carried out using at least one terminal blocking agent selected from a carboxylic acid having a monovalent hydrocarbon group of 3 or more carbon atoms, a salt of the carboxylic acid, a sulfonic acid having a monovalent hydrocarbon group of 3 or more carbon atoms, a salt of the sulfonic acid, a sulfate ester having a monovalent hydrocarbon group of 3 or more carbon atoms, a salt of the sulfate ester, a phosphate ester having a monovalent hydrocarbon group of 3 or more carbon atoms, and a salt of the phosphate ester. Terminal blocking can be carried out by adding the terminal blocking agent to a solution containing polymer compound A or B, followed by bonding treatment with a polyvalent metal ion.
[0077] As the terminal blocking agent, the acid compounds or salt compounds described in paragraphs
[0029] to
[0044] of JP-A-2021-191810 are preferred.
[0078] [Marine Biodegradable Resin Composition] The marine biodegradable resin composition of the present invention contains the marine biodegradable polymer compound.
[0079] The marine biodegradable polymer compound may be used as a main raw material, or may be used in combination with other resins as additives. The other resins are not particularly limited, but are preferably biodegradable resins. When used in combination with other resins as additives, the marine biodegradable polymer compound functions as a marine biodegradation promoter. In this case, the composite resin becomes a resin composition in which biodegradation in the ocean is promoted. Furthermore, in order to adjust the physical properties and handleability of the resin composition, multiple types of resins may be used in combination as the other resins.
[0080] Examples of the other resins include polyethylene, polyester, polypropylene, polyethylene terephthalate, polystyrene, polyurethane, epoxy resin, chlorinated polyethylene resin, chlorinated polypropylene resin, modified nylon resin, phenolic resin, silicone resin, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, styrene-maleic acid resin, styrene-butadiene resin, butadiene resin, acrylonitrile-butadiene resin, poly(meth)acrylonitrile resin, (meth)acrylamide resin, bio-PET, bio-polyamide, bio-polycarbonate, bio-polyurethane, polyvinyl alcohol, polybutylene adipate / terephthalate, polyethylene terephthalate succinate, bio-polybutylene succinate, polylactic acid blend, starch-blend polyester resin, polybutylene terephthalate succinate, polylactic acid, and polyhydroxyalkanoic acid. However, in consideration of reducing the burden on the environment and promoting marine biodegradability, highly biodegradable resins are particularly preferred.
[0081] Examples of the biodegradable resin include polycaprolactone, poly(caprolactone / butylene succinate), polybutylene succinate (PBS), poly(butylene succinate / adipate) (PBSA), poly(butylene adipate / terephthalate) (PBAT), poly(butylene succinate / carbonate), polyethylene terephthalate copolymer, poly(ethylene terephthalate / succinate), poly(tetramethylene adipate / terephthalate), polyethylene succinate Resins derived from petroleum, such as esters, polyvinyl alcohol, polyglycolic acid, glycolic acid / caprolactone copolymers, and glycolic acid / trimethylene carbonate copolymers; (polylactic acid / polybutylene succinate-based) block copolymers, (polylactic acid / polycaprolactone) copolymers, (polylactic acid / polyether) copolymers, polylactic acid blends (PBAT), lactic acid / glycolic acid copolymers, bio-polybutylene succinate, poly(butylene succinate / adipate), and starch blends. Examples of such resins include resins partially derived from biomass as raw materials, such as polyester resins and poly(butylene terephthalate succinate); resins 100% derived from biomass as raw materials, such as polyhydroxyalkanoates such as polyhydroxybutyrate, polyhydroxyvalerate, polyhydroxycaprylic acid, poly(hydroxybutyrate / hydroxyhexanoate) (PHBH), poly(3-hydroxybutyrate / 4-hydroxybutyrate) (P3HB4HB), and poly(hydroxybutyrate / hydroxyvalerate) (PHBV), and polylactic acid (PLA); and resins derived from natural polymers, such as cellulose, cellulose acetate, cellulose ester resins, starch, esterified starch, and chitosan.
[0082] Among these, it is preferable to combine the marine biodegradable polymer compound with a biodegradable resin selected from resins that are biodegradable in soil or compost but poorly biodegradable in the ocean, such as polycaprolactone, (bio)PBS, PBSA, PBAT, poly(tetramethylene adipate / terephthalate), poly(butylene succinate / carbonate), polyhydroxyalkanoates such as PHBH and PHBV, PLA, cellulose, starch, chitosan, etc. As the biodegradable resin, resins derived from PBSA, PBS, PBAT, PLA, and starch are particularly preferred.
[0083] Furthermore, in consideration of reducing the environmental load, the raw material for the resin to be combined is preferably derived from biomass, and most preferably from 100% biomass-derived raw material.
[0084] The marine biodegradable resin composition of the present invention may contain a solvent. The solvent may dissolve the resin matrix while leaving the marine biodegradable polymer compound as particles, or may dissolve both the resin and the marine biodegradable polymer compound. By adjusting the solvent appropriately, the composition can be used as a molded body formed into a film by casting or the like, or as a paint, ink, surface treatment agent, etc. Preferred solvents include, for example, water, formic acid, hexane, heptane, acetonitrile, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dimethyl sulfone, acetone, methyl ethyl ketone, diethyl ketone, acetophenone, dimethyl ether, dipropyl ether, tetrahydrofuran, chloroform, methylene chloride, trichloroethylene, ethylene dichloride, tetrachloroethane, chlorobenzene, methanol, ethanol, n-propanol, isopropanol, butanol, pentanol, hexafluoroisopropanol, methyl glycol, methyl triglycol, hexyl glycol, phenyl glycol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, benzene, toluene, xylene, etc. These may be used alone or in combination of two or more.
[0085] When a solvent is used, the total concentration of the resin and the marine biodegradable polymer compound in the resin composition is preferably 0.5 to 90% by mass, more preferably 1 to 80% by mass, even more preferably 5 to 60% by mass, and most preferably 10 to 50% by mass. The ratio of the marine biodegradable polymer compound to the resin is preferably 99:1 to 10:90 by mass, more preferably 97:3 to 40:60, even more preferably 95:5 to 50:50, and most preferably 90:10 to 60:40.
[0086] The marine biodegradable resin composition of the present invention may not contain a solvent. In this case, the resin may be thermally melted and then an insoluble marine biodegradable polymer compound may be added and mixed thereto, or the resin and the marine biodegradable polymer compound may be melted and mixed together.
[0087] In the marine biodegradable resin composition of the present invention, the content of the marine biodegradable polymer compound is preferably 1 to 50% by mass, more preferably 3 to 50% by mass, even more preferably 5 to 45% by mass, even more preferably 7 to 40% by mass, and most preferably 10 to 35% by mass. Meanwhile, the content of the resin is preferably 50 to 99% by mass, more preferably 50 to 97% by mass, even more preferably 55 to 95% by mass, even more preferably 60 to 93% by mass, and most preferably 65 to 90% by mass. By including the marine biodegradable polymer compound in the above range, the composition can be utilized as a marine biodegradation promoter that promotes the progress of biodegradation in seawater while maintaining the physical properties of the biodegradable resin. The marine biodegradable polymer compound may be used alone or in combination of two or more types.
[0088] The marine biodegradable resin composition of the present invention may contain additives, as needed, such as antioxidants, release agents, peeling agents, surface modifiers, hydrophobizing agents, water repellent agents, hydrophilizing agents, dyes / pigments, colorants, heat stabilizers, light stabilizers, weather resistance improvers, antistatic agents, antifogging agents, lubricants, antiblocking agents, hardeners, softeners, compatibilizers, flame retardants, flow improvers, plasticizers, dispersants, antibacterial agents, fillers, metal deactivators, etc. The content of these additives is not particularly limited as long as it does not impair the effects of the present invention, but is preferably about 0.1 to 50 parts by mass per 100 parts by mass of the resin.
[0089] When the marine biodegradable resin composition contains a solvent, it can be prepared, for example, by adding the resin, the marine biodegradable polymer compound, and, if necessary, the additives to a solvent simultaneously or in any order and mixing them. When the marine biodegradable resin composition does not contain a solvent, for example, the resin can be melted, and the marine biodegradable polymer compound and, if necessary, the additives can be added thereto simultaneously or in any order and mixed, or the resin and marine biodegradable polymer compound can be heated to melt and mix them together, and the additives can be added and mixed as necessary.
[0090] [Molded Article] By molding the resin composition, a molded article can be obtained in which the marine biodegradable polymer compound is dispersed or dissolved in the resin. When the resin composition contains a solvent, the resin composition can be used as is for molding. When the resin composition does not contain a solvent, the resin in the resin composition, or the resin and the marine biodegradable polymer compound, can be melted by heat and then molded.
[0091] The shape of the molded product may be, for example, a film, a fiber, a plate, a foam molded product, or any other shape depending on the intended use. The molding method is not particularly limited, and various conventionally known molding methods can be used. Specific examples thereof include blow molding, injection molding, extrusion molding, compression molding, melt extrusion molding, solution casting molding, and calendar molding.
[0092] The marine biodegradable resin composition of the present invention can be used as a raw material for plastic molded products, and as various additives for molded products such as liquids, coatings, films, plates, paper, etc. When used as a raw material for plastic molded products, it can be used as a raw material for general-purpose applications such as films, packaging, containers, trays, laminates, adhesives, coating materials, medical and clothing fibers, shoes, belts, tires, tubes, shock absorbers, fishing lines, fishing nets, etc., and for marine applications, etc., and is particularly suitable for use as a raw material for marine applications, etc. In addition, when used as an additive, for example, light scattering agents and optical filter materials, colorants, cosmetics, absorbents, adsorbents, inks, adhesives, electromagnetic wave shielding materials, fluorescent sensors, biomarkers, recording materials, recording elements, polarizing materials, drug carriers for drug delivery systems (DDS), biosensors, DNA chips, test agents, baked voided moldings, antiblocking agents, screen printing, offset printing, process printing, gravure printing, pad printing, coater, inkjet and the like additives for printing inks used, for marking pens, ballpoint pens, fountain pens, brush pens, markers and other writing instrument ink additives, crayons, paints, erasers and other stationery additives, brush coating, spray coating, electrostatic coating, electrodeposition coating, flow coating, roller coating, dip coating and the like additives for paints used in marine applications, particularly hull paints and the like It can be widely used as an additive.
[0093] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0094] In the following examples and comparative examples, the metal ion equivalent was measured by heating and decomposing the target substance with nitric acid or aqua regia, followed by emission spectrometry using an ICP-MS (ICPE-9820, manufactured by Shimadzu Corporation). The melting temperature was measured using a differential scanning calorimeter (DSC6200, manufactured by Seiko Instruments Inc.). Specifically, 5 mg of the measurement sample was precisely weighed, placed in an aluminum pan, and heated at a rate of 10°C / min at room temperature and humidity within a measurement temperature range of 20 to 300°C, using an empty aluminum pan as a reference. The melting temperature was calculated from the endothermic (melting) peak point of the obtained curve.
[0095] [1] Synthesis of marine biodegradable polymer compound A [Example 1-1] Synthesis of marine biodegradable polymer compound A-1 43.2 g of 1,4-butanediol and 53.7 g of maleic acid were added to a 300 mL recovery flask and stirred at 160°C for 6 hours under a nitrogen atmosphere, after which 2.26 g of 3-mercaptopropionic acid, 1.33 g of triethylamine and 100 g of acetonitrile were added and stirred at 70°C for 3 hours to obtain marine biodegradable polymer compound A-1. Marine biodegradable polymer compound A-1 was obtained by: 1 It was confirmed by H-NMR measurement that the number average molecular weight was 2100, the polymer had an average of 8 aliphatic unsaturated bonds, and an average of 2 acidic groups.
[0096] [Example 1-2] Synthesis of marine biodegradable polymer compound A-2 41.6 g of 1,4-butanediol, 50.8 g of dimethyl maleate, 16.8 g of dimethyl terephthalate, and 0.96 g of titanium tetraisopropoxide were added to a 300 mL recovery flask and stirred at 160°C for 5 hours under a nitrogen atmosphere, after which 37.1 g of 3-mercaptopropionic acid and 18.2 g of acetonitrile were added and stirred at 130°C for 4 hours to obtain marine biodegradable polymer compound A-2. Marine biodegradable polymer compound A-2 was obtained by: 1It was confirmed by H-NMR measurement that the number average molecular weight was 2000, that the copolymer had an average of three aliphatic unsaturated bonds, and an average of four acidic groups.
[0097] [Example 1-3] Synthesis of marine biodegradable polymer compound A-3 39.7 g of 1,4-butanediol, 25.2 g of succinic acid, and 25.0 g of maleic acid were added to a 300 mL recovery flask and stirred at 160°C for 6 hours under a nitrogen atmosphere, after which 25.7 g of 3-mercaptopropionic acid and 11.4 g of acetonitrile were added and stirred at 130°C for 3 hours to obtain marine biodegradable polymer compound A-3. Marine biodegradable polymer compound A-3 was obtained by: 1 It was confirmed by H-NMR measurement that the number average molecular weight was 1800, that the copolymer had an average of two aliphatic unsaturated bonds, and an average of two acidic groups.
[0098] [Example 1-4] Synthesis of marine biodegradable polymer compound A-4 43.5 g of 1,4-butanediol, 52.9 g of maleic acid, and 0.53 g of fumaric acid were added to a 300 mL recovery flask and stirred at 160°C for 6 hours under a nitrogen atmosphere, after which 1.25 g of 5-aminovaleric acid was added and stirred at 160°C for 3 hours under a nitrogen atmosphere to obtain marine biodegradable polymer compound A-4. Marine biodegradable polymer compound A-4 was obtained by: 1 It was confirmed by H-NMR measurement that the number average molecular weight was 1900, the polymer had an average of 7 aliphatic unsaturated bonds, and an average of 2 acidic groups.
[0099] [Example 1-5] Synthesis of marine biodegradable polymer compound A-5 46.9 g of 1,4-butanediol, 39.5 g of adipic acid, and 31.3 g of maleic acid were added to a 500 mL recovery flask and stirred at 160°C for 6 hours under a nitrogen atmosphere, after which 8.45 g of di-tert-butyl malonate, 4.00 g of potassium carbonate, and 100 g of acetonitrile were added and stirred at 70°C for 3 hours. 174 mL of 3N hydrochloric acid was then added and stirred for 1 hour. Subsequently, an aqueous sodium hydroxide solution was added to adjust the pH to 7, and the mixture was extracted with ethyl acetate and dried under reduced pressure to obtain marine biodegradable polymer compound A-5. Marine biodegradable polymer compound A-5 was obtained by: 1It was confirmed by H-NMR measurement that the number average molecular weight was 3,600, the polymer had an average of 8 aliphatic unsaturated bonds, and an average of 3 acidic groups.
[0100] Comparative Example 1-1 Sodium polyacrylate (degree of polymerization: 2700 to 7500) (Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the comparative polymer compound AX-1.
[0101] Table 1 below shows the marine biodegradable polymer compounds A-1 to A-5 and polymer compound AX-1.
[0102] [2] Synthesis of marine biodegradable polymer compound B [Example 2-1] Synthesis of marine biodegradable polymer compound B-1 60.0 g of marine biodegradable polymer compound A-1 and 21.1 g of a 10% by mass aqueous solution of sodium bicarbonate were added to a 300 mL recovery flask and stirred, and then 20.1 g of a 30% by mass aqueous solution of calcium chloride was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-1. The melting point of marine biodegradable polymer compound B-1 was 51°C.
[0103] Example 2-2 Synthesis of Marine Biodegradable Polymer Compound B-2 59.8 g of marine biodegradable polymer compound A-2 and 40.8 g of a 10% by mass aqueous solution of potassium bicarbonate were added to a 300 mL recovery flask and stirred, followed by the addition of 39.9 g of a 30% by mass aqueous solution of magnesium chloride and stirring. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-2. The melting point of marine biodegradable polymer compound B-2 was 107°C.
[0104] Example 2-3 Synthesis of Marine Biodegradable Polymer Compound B-3 30.4 g of marine biodegradable polymer compound A-3 and 78.2 g of a 10% by mass aqueous potassium bicarbonate solution were added to a 300 mL recovery flask and stirred, followed by addition of 25.1 g of a 30% by mass aqueous calcium chloride solution and stirring. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-3. The melting point of marine biodegradable polymer compound B-3 was 95°C.
[0105] Example 2-4 Synthesis of Marine Biodegradable Polymer Compound B-4 61.1 g of marine biodegradable polymer compound A-4 and 50.0 g of 2.5% by mass aqueous sodium hydroxide solution were added to a 300 mL recovery flask and stirred, followed by the addition of 15.2 g of 30% by mass aqueous aluminum sulfate solution and stirring. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-4. The melting point of marine biodegradable polymer compound B-4 was 58°C.
[0106] Example 2-5 Synthesis of Marine Biodegradable Polymer Compound B-5 60 g of marine biodegradable polymer compound A-5 and 35.1 g of a 2% by mass aqueous solution of sodium hydroxide were added to a 300 mL recovery flask and stirred, followed by the addition of 12.0 g of a 30% by mass aqueous solution of calcium chloride and 2.6 g of a 30% aqueous solution of magnesium chloride, followed by stirring. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-5. The melting point of marine biodegradable polymer compound B-5 was 61°C.
[0107] Comparative Example 2-1 Synthesis of Ion-Crosslinked Polymer Compound BX-1 30.0 g of sodium polyacrylate (degree of polymerization 2500-7500) (FUJIFILM Wako Pure Chemical Industries, Ltd.) and 100 g of ion-exchanged water were added to a 300 mL recovery flask and stirred, and then 35.1 g of a 30 mass % aqueous calcium chloride solution was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain ion-crosslinked polymer compound BX-1. Polymer compound BX-1 did not melt due to heat.
[0108] Table 2 below shows the marine biodegradable polymer compounds B-1 to B-5 and the ionically cross-linked polymer compound BX-1.
[0109] [3] Biodegradability Test of Compounds and Powders [Examples 3-1 to 3-10, Comparative Examples 3-1 to 3-2] Marine biodegradable polymer compounds A-1 to A-5, marine biodegradable polymer compounds B-1 to B-5, compound AX-1, and polymer compound BX-1 were subjected to seawater biodegradation tests using the following method. Microcrystalline cellulose (Sigma-Aldrich Avicel PH-101) was used as a control material, and the relative biodegradability of cellulose was evaluated. The results are shown in Table 3.
[0110] <Test method and conditions> Biodegradability measurement method: Measurement of oxygen consumption using a closed respirometer (reference ASTM D6691) Test equipment: OxiTop IDS (WTW) Incubation temperature: 30±1°C, dark place Biodegradability (%) = (BOD O -BOD B ) / ThOD x 100 BOD O : Biochemical oxygen demand (measured value: mg) for testing or inoculum activity confirmation B : Average biochemical oxygen demand of blank test (measured value: mg) ThOD: Theoretical oxygen demand required when test material or control material is completely oxidized (calculated value: mg) Relative cellulose biodegradability (%) = (Maximum biodegradability of test particles / Maximum cellulose biodegradability) x 100 Seawater (collected from Tokyo Bay [Chiba Prefecture: Chiba Port])] The collected seawater was aerated at room temperature of 25°C after removing foreign matter with a 10 μm filter. In addition, ammonium chloride and potassium dihydrogen phosphate were added as inorganic nutrients to the solution at 0.05 g / L and 0.1 g / L, respectively.
[0111]
[0112] From the results shown in Table 3, it can be seen that the particles of the present invention had biodegradability almost equivalent to that of cellulose within a culture period of 60 days.
[0113] [4] Preparation of Marine Biodegradable Resin Compositions and Confirmation Tests in Seawater - 1 (1) Surface Changes [Examples 4-1 to 4-5, Comparative Examples 4-1 to 4-2] Biodegradable resin PBSA (FD-92 manufactured by Mitsubishi Chemical Corporation) was crushed using a crusher (Wonder Blender WB-1 manufactured by Osaka Chemical Co., Ltd.) and sieved through a stainless steel sieve (26 μm mesh). Marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 were mixed at 140 ° C to a concentration of 20% by mass, and then press-molded at 150 ° C to produce a 200 μ m thick film (Examples 4-1 to 4-5, Comparative Example 4-1). PBSA itself (not containing the marine biodegradable polymer compounds) was also press-molded at 150 ° C to produce a 200 μ m thick film (Comparative Example 4-2). The resulting films were cut into 10 mm square pieces and placed in 200 mL of ion-exchanged water and 200 mL of seawater (collected from Tokyo Bay (Chiba Port, Chiba Prefecture)), and left to stand at 25°C for 7 and 30 days, respectively. The films were then removed and their surfaces and appearances were observed using a scanning electron microscope. The results are shown in Table 4.
[0114]
[0115] From the results shown in Table 4, it is believed that biodegradability is promoted by the presence of microorganisms in seawater as well as by the breakdown caused by seawater.
[0116] (2) Weight Loss of Composite Resin [Examples 5-1 to 5-5, Comparative Examples 5-1 to 5-2] Using the same method as in (1), films were prepared by adding marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 to PBSA, and films of PBSA alone. The obtained films were processed into 20 mm squares, sandwiched between stainless steel nets, and immersed in seawater (collected from Tokyo Bay [Chiba Prefecture: Chiba Port]) in a 15 L tank. The progress of weight loss after immersion was observed after 30, 60, and 90 days. The results are shown in Table 5.
[0117]
[0118] (3) Tensile Strength Measurement [Examples 6-1 to 6-5, Comparative Example 6-1] Using the same method as in (1), films were prepared by adding marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 to PBSA at concentrations of 10 mass%, 20 mass%, or 30 mass%, respectively, and films of PBSA alone. According to JIS K 7139-A22, dumbbells were prepared from various films, and the tensile stress (yield point) was measured using a universal testing machine (MCT-2150, manufactured by A&D Co., Ltd.). Five measurements were taken for each sample, and the average value was used as the tensile stress. The results are shown in Table 6.
[0119]
[0120] [5] Preparation of Marine Biodegradable Resin Compositions and Confirmation Tests in Seawater - 2 (1) Surface Changes [Examples 7-1 to 7-5, Comparative Examples 7-1 to 7-2] A starch-based resin (Mater-Bi EF05B, manufactured by Novamont) was crushed using a crusher (Wonder Blender WB-1 manufactured by Osaka Chemical Co., Ltd.) and sieved through a stainless steel sieve (26 μm mesh). The resulting mixture was kneaded at 140 ° C to a concentration of 20% by mass with the marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1. The mixture was then press-molded at 150 ° C to produce a 200 μm thick film (Examples 7-1 to 7-5, Comparative Example 7-1). The starch-based resin itself (without particles) was also press-molded at 150 ° C to produce a 200 μm thick film (Comparative Example 7-2). The resulting films were cut into 10 mm square pieces and placed in 200 mL of ion-exchanged water and 200 mL of seawater (collected from Tokyo Bay (Chiba Port, Chiba Prefecture)), respectively, and left to stand at 25°C for 7 and 30 days, respectively. The films were then removed and their surfaces and appearances were observed using a scanning electron microscope. The results are shown in Table 7.
[0121]
[0122] From the results shown in Table 5, it is believed that biodegradability is promoted by the presence of microorganisms in seawater as well as by the disintegration caused by seawater.
[0123] (2) Weight loss of composite resin [Examples 8-1 to 8-5, Comparative Examples 8-1 to 8-2] In the same manner as in (1), films were prepared by adding marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 to starch-based resin, and films of starch-based resin alone. The obtained films were processed into 20 mm squares and sandwiched between stainless steel nets. They were then immersed in seawater (collected from Tokyo Bay [Chiba Prefecture: Chiba Port]) in a 15 L tank, and the progress of weight loss after immersion was observed after 30, 60, and 90 days. The results are shown in Table 8.
[0124]
[0125] (3) Tensile Strength Measurement [Examples 9-1 to 9-5, Comparative Example 9-1] Using the same method as in (1), films were prepared by adding marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 to starch-based resins at concentrations of 10 mass%, 20 mass%, or 30 mass%, respectively, and films of starch-based resins alone. According to JIS K 7139-A22, dumbbells were prepared from various films, and the tensile stress (yield point) was measured using a universal testing machine (MCT-2150, manufactured by A&D Co., Ltd.). Five measurements were made for each sample, and the average value was taken as the tensile stress. The results are shown in Table 9.
[0126]
[0127] From the above results, the marine biodegradable polymer compound of the present invention is biodegraded in seawater before the biodegradable resin, and is broken down into smaller molecules or salt-substituted, which makes it more likely to dissolve or become hydrophilic. Therefore, by adding a marine biodegradation promoter consisting of the marine biodegradable polymer compound of the present invention to a resin composition that is biodegradable in soil or compost or a resin composition that is poorly biodegradable in the ocean, it becomes possible to create irregularities in seawater, which helps microbial adhesion and promotes biodegradation, thereby ultimately improving overall marine biodegradability and reducing the environmental burden. By combining the marine biodegradation promoter made of the marine biodegradable polymer compound of the present invention with a resin that is biodegradable in soil or compost, it is possible to improve seawater biodegradability, and by appropriately modifying the structure of the organic anion, it is possible to incorporate multiple effects, such as adjusting the melting temperature and viscosity, adjusting the degree of crystallinity, adjusting the adhesion and biodegradability of microorganisms, adjusting physical properties such as the resin tensile strength, flexural strength, and elasticity, improving compatibility with the resin, adjusting the degree of hydrophobicity, adjusting the hydrophobicity, and adjusting the adhesion and plasticity, and it is possible to improve both the biodegradability and physical properties of the marine biodegradable resin composition.
Claims
1. A polymer having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, an aliphatic unsaturated carbon-carbon bond in the main chain, and one or more -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation or a monovalent organic cation.
2. The marine biodegradable polymer compound according to claim 1, having two or more acidic groups in the side chain.
3. The marine biodegradable polymer compound according to claim 1, wherein the repeating unit contains an ester bond.
4. The marine biodegradable polymer compound according to claim 1, which has a number average molecular weight of 300 to 100,000.
5. In addition, -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + The marine biodegradable polymer compound according to claim 1, which has a substituent selected from the group consisting of hydrogen ions, monovalent metal cations and monovalent organic cations.
6. The marine biodegradable polymer compound according to claim 1, wherein the number of aliphatic unsaturated carbon-carbon bonds in one molecule is 0.1 to 50 on the average.
7. The marine biodegradable polymer compound according to claim 1, wherein the substituent is bonded to the main chain via a linking group having 1 to 50 atoms.
8. The substituent is —COO - R + 2. The marine biodegradable polymer compound according to claim 1, 9. The marine biodegradable polymer compound according to claim 1, which has maleic acid residues in its main chain.
10. R + The marine biodegradable polymer compound according to claim 1, wherein is a monovalent metal cation or a monovalent organic cation.
11. A marine biodegradable polymer compound in which a polymeric polyvalent anion derived from the marine biodegradable polymer compound according to claim 1 is bonded via a divalent or higher metal cation.
12. The content of the metal cation is 1 to 100 eq / 10 5 The marine biodegradable polymer compound according to claim 11, wherein 13. The marine biodegradable polymer compound according to claim 11, wherein the divalent or higher metal cation is a calcium ion, a magnesium ion or an aluminum ion.
14. A marine biodegradation promoter comprising the marine biodegradable polymer compound according to any one of claims 1 to 13.
15. A marine biodegradable resin composition comprising the marine biodegradation promoter according to claim 14 and a resin.
16. The marine biodegradable resin composition according to claim 15, wherein the resin is a biodegradable resin.
17. The marine biodegradable resin composition according to claim 16, wherein the content of the marine biodegradation promoter is 1 to 50 mass %, and the content of the biodegradable resin is 50 to 99 mass %.
18. A molded article obtained from the marine biodegradable resin composition according to claim 15.
19. A method for producing a marine biodegradable polymer compound, comprising a step of reacting a polymer compound having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, and having an aliphatic unsaturated carbon-carbon bond in the main chain, with a compound having a reactive group reactive to an aliphatic unsaturated carbon-carbon bond and a substituent selected from -COOH, -SOH, -O-SOH, and -P(=O)(OH)-OH.
20. A method for producing a marine biodegradable polymer compound, the method comprising the step of neutralizing, with a monovalent base, a substituent of a marine biodegradable polymer compound, the substituent comprising a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, an aliphatic unsaturated carbon-carbon bond in the main chain, and one or more substituents selected from -COOH, -SOH, -O-SOH, and -P(=O)(OH)-OH in a side chain.
21. The method for producing a marine biodegradable polymer compound according to claim 20, wherein the base is lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate or potassium bicarbonate.
22. A polymer having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, an aliphatic unsaturated carbon-carbon bond in the main chain, and one or more -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) A method for producing a marine biodegradable polymer compound, comprising a step of crosslinking a marine biodegradable polymer compound having a substituent selected from the group consisting of a hydrogen ion, a monovalent metal cation, and a monovalent organic cation, at a side chain thereof, using a polyvalent metal salt.
23. The method for producing a marine biodegradable polymer compound according to claim 22, wherein the polyvalent metal salt is a calcium salt, a magnesium salt or an aluminum salt.
Citation Information
Patent Citations
Compound of mortar
JP1977012233A
Production of nonwoven fabric
JP1993071056A
Polyurea resin composition, curing agent for polyurea resin and composition set for forming polyurea resin
JP2004027148A
Method for producing polycarbonate polyol, and polyurethane using the polycarbonate polyol
JP2013010948A
Polycarbonate polyol
JP2016094589A
Cited By
Marine biodegradable resin composition
WO2026221033A1
Biodegradation promotor
WO2026221034A1