Laser processing method and wafer manufacturing method

The laser processing method addresses variations in modified layer depth by moving the irradiation position in an arc-shaped pattern, ensuring consistent peeling layer formation and improved wafer manufacturing efficiency.

WO2024247650A1PCT designated stage expired Publication Date: 2024-12-05DENSO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017304
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-09
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Variations in the formation depth of the modified layer during laser slicing of semiconductor wafers lead to peeling defects and increased machining allowances, resulting in poor manufacturing efficiency.

Method used

A laser processing method where the irradiation position of a transparent laser beam is moved along an arc-shaped scanning line with discrete points, forming an array of irradiation marks, and subsequent beams are directed to these marks to control the formation of a peeling layer with reduced depth variations.

Benefits of technology

This method reduces variations in the modified layer depth, minimizing material loss and enhancing manufacturing efficiency by maintaining a consistent peeling surface, thus improving the wafer production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017304_05122024_PF_FP_ABST
    Figure JP2024017304_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a laser processing method for irradiating an object (2) to be processed made of a semiconductor material with a laser beam (B), the method including modified layer formation. During the modified layer formation, a surface (21) of the object to be processed is irradiated with a laser beam which is penetrative thereto, to form a modified layer (RA) at a predetermined depth from the surface. During the modified layer formation, an irradiation position (PR) of the laser beam on the surface is moved along an arc-shaped scanning line (Sc) so that arc-shaped irradiation trajectory lines (Ls) comprising an irradiation mark of the laser beam are formed arrayed at a predetermined line pitch (pL) with respect to a radial direction (Dr) of the scanning line. The irradiation positions are provided discretely along the scanning line at multiple points, and an irradiation mark formed by irradiation with a preceding laser beam is irradiated with a subsequent laser beam.
Need to check novelty before this filing date? Find Prior Art

Description

Laser processing method and wafer manufacturing method CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application is based on Japanese Patent Application No. 2023-87817, filed on May 29, 2023, the contents of which are incorporated herein by reference.

[0002] The present disclosure relates to a laser processing method for a processing object made of a semiconductor material, and a wafer manufacturing method using the same.

[0003] Laser slicing is a known method for producing wafers from semiconductor ingots. Laser slicing involves scanning the interior of the ingot with a focal point of a laser beam to form a modified layer, which is then used as the delamination surface. Known scanning methods include, for example, the one described in Patent Document 1. The method described in Patent Document 1 involves moving the focal point in a spiral pattern from the center toward the edge.

[0004] JP 2013-49161 A

[0005] In the wafer production method described in Patent Document 1, variations in the depth of the modified layer may occur. Variations in the depth of the modified layer may result in steps on the separation surface, increasing the amount of grinding or polishing required, or causing separation defects, resulting in poor manufacturing efficiency. The present disclosure has been made in consideration of the circumstances exemplified above. That is, the present disclosure provides a technique for suppressing variations in the depth of the modified layer or separation layer, for example.

[0006] According to one aspect of the present disclosure, a laser processing method is a method of irradiating a laser beam onto an object to be processed made of a semiconductor material, and includes modified layer formation, in which a modified layer is formed at a predetermined depth from the surface by irradiating the surface of the object with the laser beam that is transparent to the surface of the object to be processed, and the modified layer formation is performed by moving the irradiation position of the laser beam on the surface along an arc-shaped scanning line, thereby forming an arc-shaped irradiation trajectory line consisting of the irradiation marks of the laser beam in an array at a predetermined line pitch in the radial direction of the scanning line, and the irradiation positions are provided discretely along the scanning line to form multiple points, and the subsequent laser beam is irradiated onto the irradiation marks formed by irradiation of the preceding laser beam. According to another aspect of the present disclosure, a wafer manufacturing method is a method for obtaining a wafer from an ingot, comprising: irradiating a surface of one end of the ingot in a height direction with a transparent laser beam to form a delamination layer from the surface to a depth corresponding to the thickness of the wafer; The delamination layer formation comprises: moving the irradiation position of the laser beam on the surface along an arc-shaped scanning line to form an arc-shaped irradiation locus line consisting of irradiation marks of the laser beam at a predetermined line pitch in the radial direction of the scanning line; The irradiation positions are discretely arranged along the scanning line to form multiple points, and a subsequent laser beam is irradiated onto the irradiation marks formed by irradiation of a preceding laser beam. Note that in each section of the application documents, each element may be assigned a reference number in parentheses. In this case, the reference number merely indicates an example of the correspondence between the element and the specific configuration described in the embodiment described below. Therefore, the present disclosure is not limited in any way by the reference numbers.

[0007] 3A and 3B are side views showing an outline of a wafer manufacturing method according to an embodiment of the present disclosure; FIG. 4 is a process diagram showing an outline of the wafer manufacturing method; FIG. 5 is a side view showing an outline of a separation layer formation step shown in FIG. 2, i.e., a laser processing method according to an embodiment of the present disclosure; FIG. 6 is a plan view showing a schematic configuration of an ingot that has undergone the separation layer formation step shown in FIGS. 2 and 3; FIG. 7 is an enlarged plan view showing an example of a two-dimensional scanning pattern of a laser beam in the laser processing method and the wafer manufacturing method according to an embodiment of the present disclosure; FIG. 8 is a diagram showing a state of formation of an irradiation mark when the laser beam is scanned in a direction perpendicular to the off-angle direction in a wafer manufacturing method of a comparative example; FIG. 9 is a diagram showing a state of formation of an irradiation mark when the laser beam is scanned in a direction perpendicular to the off-angle direction in a wafer manufacturing method of a comparative example; FIG. 10 is a diagram showing a state of formation of an irradiation mark when the laser beam is scanned in the off-angle direction in a wafer manufacturing method of another comparative example; FIG. 11 is a diagram showing a state of formation of an irradiation mark when the laser beam is scanned in the off-angle direction in a wafer manufacturing method of another comparative example; 12 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 13 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 14 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 15 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 16 is an enlarged plan view showing another example of a two-dimensional scanning pattern of a laser beam in a laser processing method and a wafer manufacturing method according to another embodiment of the present disclosure. FIG. 17 is a process diagram showing an outline of a wafer manufacturing method according to yet another embodiment of the present disclosure. FIG. 18 is a plan view showing an example of how measurement positions are set in the wafer optical measurement process shown in FIG. 10. FIG. 19 is a graph showing how an absorption coefficient calculated from the transmittance measured at the measurement positions shown in FIG. 12 changes depending on the measurement position. FIG. 19 is a side cross-sectional view showing the difference in transmittance at the modified layer generation position in the laser slicing process, i.e., the peeling layer formation process, shown in FIG. 10.16 is a side cross-sectional view showing the difference in transmittance at the modified layer generation position in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 10. FIG. 17 is a side cross-sectional view showing the difference in transmittance at the modified layer generation position in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 10. FIG. 18 is a side cross-sectional view for explaining an example of a method for setting the laser beam irradiation conditions in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 10. FIG. 19 is a plan view for explaining a method for deriving the amount of change in absorption coefficient shown in equation (2). FIG. 19 is a graph showing the change in absorption coefficient in the depth direction of the ingot at the in-plane center position shown in FIG. 16. FIG. 19 is a graph showing the change in absorption coefficient in the depth direction of the ingot at the first end position shown in FIG. 16. FIG. 19 is a graph showing the change in absorption coefficient in the depth direction of the ingot at the second end position shown in FIG. 16. FIG. 19 is a graph for explaining an example of a method for deriving the absorption coefficient. FIG. 19 is a side view showing a first product and a second product generated for setting the laser beam irradiation conditions in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 10. FIG. 20 is a graph showing a region where the measurement pitch is finer in the wafer optical measurement process shown in FIG. 10.

[0008] (Embodiments) Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. It should be noted that if various modified examples applicable to one embodiment are introduced in the middle of a series of explanations related to the embodiment, it may hinder understanding of the embodiment. Therefore, the modified examples will not be introduced in the middle of a series of explanations related to the embodiment, but will be explained together after the series of explanations.

[0009] 1, a wafer 1 manufactured by the wafer manufacturing method according to this embodiment is obtained by slicing an ingot 2 that is substantially cylindrical in side view along a plane substantially perpendicular to the height direction, and is formed into a thin plate that is substantially circular in plan view. Note that, in order to simplify the illustration and description, so-called orientation flats that are normally provided on the wafer 1 and ingot 2 are not shown or described in this specification as appropriate.

[0010] 1, for ease of explanation, the wafer 1 and the ingot 2 are illustrated as being arranged coaxially along a central axis L that is parallel to the thickness direction of the wafer 1 and the height direction of the ingot 2. That is, the wafer 1 has an end face that is approximately cylindrical and surrounds the central axis L. Similarly, the ingot 2 has a side face that is approximately cylindrical and surrounds the central axis L. The central axis L is a virtual straight line that is parallel to the approximately cylindrical side or end face of the wafer 1 or the ingot 2 and passes through the axial center of the wafer 1 or the ingot 2.

[0011] In this embodiment, the ingot 2 is a single-crystal SiC ingot having a c-axis Lc and a (0001) plane Pc that are orthogonal to each other, and has an off-angle θ exceeding 0 degrees. The c-axis Lc is a crystal axis indicated by a direction index as

[0001] . The (0001) plane Pc is a crystal plane that is orthogonal to the c-axis Lc and is called a "C-plane" in the strict sense of crystallography. The off-angle θ is the angle between the central axis L of the wafer 1 or ingot 2 and the c-axis Lc, and is, for example, approximately 1 to 4 degrees. That is, the c-axis Lc of the wafer 1 and the ingot 2 is tilted at an off-angle θ exceeding 0 degrees toward the off-angle direction Dθ. The off-angle direction Dθ is the direction of movement of a point on the central axis L located on the laser-irradiated surface when the central axis L is rotated toward the c-axis Lc around the intersection of the central axis L and the c-axis Lc. The laser irradiated surface is the upper surface or top surface of the wafer 1 or ingot 2 in the drawing.

[0012] For simplicity of explanation, a right-handed XYZ coordinate system is set as shown in FIG. 1 . In this right-handed XYZ coordinate system, the off-angle direction Dθ and the positive X-axis direction are assumed to be the same direction. The X-axis and Y-axis are assumed to be parallel to the main surfaces of wafer 1 and ingot 2. The "main surface" is a surface perpendicular to the thickness direction of a plate-like object, and may also be referred to as the "top surface," "bottom surface," or "plate surface." Alternatively, the "main surface" is a surface perpendicular to the height direction of a columnar object such as ingot 2, and may also be referred to as the "top surface" or "bottom surface." Furthermore, the thickness direction of wafer 1 and the height direction of ingot 2 are assumed to be parallel to the Z-axis. Any direction perpendicular to the Z-axis may hereinafter be referred to as the "in-plane direction." The right-handed XYZ coordinate system shown in FIG. 1 is assumed to be consistent with the right-handed XYZ coordinate systems shown in other figures, unless otherwise specified.

[0013] The wafer 1 has a pair of main surfaces, a wafer C-face 11 and a wafer Si-face 12. In this embodiment, the wafer 1 is formed so that the wafer C-face 11, which is the top surface, is inclined at an off angle θ with respect to the (0001) plane Pc. Similarly, the ingot 2 has a pair of main surfaces, an ingot C-face 21 and an ingot Si-face 22. The ingot 2 is formed so that the ingot C-face 21, which is the top surface, is inclined at an off angle θ with respect to the (0001) plane Pc. Note that in FIG. 1 , the direction in which the wafer C-face 11 and the ingot C-face 21 face is shown as the positive direction of the Z axis.

[0014] (Outline of Wafer Manufacturing Method) The wafer manufacturing method according to this embodiment is a method for obtaining a wafer 1 from an ingot 2 using laser processing. FIG. 2 is a process diagram showing a typical example of a wafer manufacturing method according to this embodiment. Below, an outline of each process in this wafer manufacturing method will be described. Note that the term "process" can also be referred to as a "procedure" or "treatment." Furthermore, the term "process" does not only refer to an independent process, but also includes cases where it is difficult or impossible to clearly distinguish from other processes once the intended purpose of the process has been achieved. The same applies to the terms "treatment" and "procedure."

[0015] (1) Separation Layer Formation Step As shown in Figure 3, a laser beam B having a predetermined degree of transparency for the ingot 2 is irradiated onto an ingot C-face 21, which is the main surface at one end in the height direction of the ingot 2. As a result, a separation layer 23 is formed from the ingot C-face 21 to a depth corresponding to the thickness of the wafer 1. Here, the "predetermined degree of transparency" refers to a degree of transparency that allows a focal point BP of the laser beam B to be formed inside the ingot 2 at a depth corresponding to the thickness of the wafer 1. The "depth corresponding to the thickness of the wafer 1" is a dimension obtained by adding a thickness corresponding to a predetermined processing allowance in a wafer flattening step or the like, which will be described later, to the target thickness of the wafer 1 as a finished product, and may also be referred to as the "depth corresponding to the thickness of the wafer 1."

[0016] (2) Wafer Peeling Process The wafer precursor 24, which is the portion between the ingot C-face 21 (laser irradiated surface) and the peeling layer 23, is peeled from the ingot 2 at the peeling layer 23. As in the expression "wafer peeling process" above, the plate-like object obtained by peeling the wafer precursor 24 from the ingot 2 may be commonly referred to as a "wafer." However, to distinguish it from the wafer 1 as a finished product having an epi-ready mirror-finished main surface, such a plate-like object will hereinafter be referred to as a "peeled body 30."

[0017] The peeled body 30 has a pair of main surfaces, a non-peeled surface 31 and a peeled surface 32. The non-peeled surface 31 is the surface on the side that did not form the peeled layer 23 before the wafer peeling process, and corresponds to the ingot C-face 21 before the peeled layer forming process and the wafer peeling process. The peeled surface 32 formed the peeled layer 23 before the wafer peeling process, and is a surface that was newly formed by the wafer peeling process. The peeled surface 32 has rough irregularities that require grinding or polishing due to variations in the depth of the peeled layer 23 and peeling during the wafer peeling process.

[0018] (3) Wafer Planarization Process At least the peeled surface 32 of the non-peeled surface 31 and the peeled surface 32, which are the main surfaces of the peeler 30, is planarized to obtain the wafer 1 as a finished product. In the wafer planarization process, in addition to general grinding stone polishing and CMP, ECMG and ECMP can be used. Note that CMP is an abbreviation for Chemical Mechanical Polishing. ECMG is an abbreviation for Electro-Chemical Mechanical Grinding. ECMP is an abbreviation for Electro-Chemical Mechanical Polishing. The wafer planarization process can be performed by using these multiple types of planarization processes alone or in appropriate combination.

[0019] (4) Ingot Planarization Process The top surface of the ingot 2 newly formed by peeling off the wafer precursor 24 at the peeling layer 23 is planarized, i.e., mirror-finished, so that it can be reused in the peeling layer formation process. In the ingot planarization process, in addition to general grinding stone polishing and CMP, ECMG and ECMP can also be used. The ingot planarization process can also be performed by using these multiple types of planarization processes alone or in appropriate combination.

[0020] 2, the peeled body 30 peeled from the ingot 2 through the peeling layer forming step and the wafer peeling step is finished into an epi-ready wafer 1 through the following steps: Rough grinding of the peeled surface 32 that will become the wafer Si surface 12; ECMG grinding of the peeled surface 32 after rough grinding; ECMP polishing of the peeled surface 32 after ECMG grinding; and Cleaning.

[0021] Furthermore, the ingot 2 remaining after the peeled body 30 has been peeled off from the ingot 2 through the peeling layer forming step and the wafer peeling step can be subjected to the peeling layer forming step again through the following steps: Rough grinding of the ingot C-face 21 newly generated by the wafer peeling step; Finish grinding of the ingot C-face 21 after rough grinding; and Cleaning.

[0022] (Details of the Separation Layer Formation Step) Hereinafter, details of the separation layer formation step corresponding to the laser processing method of the present disclosure will be described with reference to FIG. 3 in addition to FIG. 1 and FIG. 2 . As shown in FIG. 3 , the separation layer formation step is a step of forming a separation layer 23 inside an ingot 2, which is a processing target made of a semiconductor material, by irradiating the ingot 2 with a transparent laser beam B. The separation layer 23 is formed by leaving a large number of irradiation marks RM of the laser beam B in the in-plane direction. The irradiation marks RM are formed by a modified layer RA and cracks C. The modified layer RA is a modified region formed by separating SiC into silicon and carbon at or near the focal point BP by irradiation with the laser beam B. Therefore, the separation layer formation step can also be referred to as a modified layer formation step.

[0023] In the peeling layer formation process, the irradiation position PR of the laser beam B is moved two-dimensionally on the ingot C surface 21 to form a peeling layer 23 consisting of a modified layer RA and cracks C at a depth from the ingot C surface 21 corresponding to the thickness of the wafer 1. Here, the "irradiation position PR" refers to the center position of the laser beam B on the ingot C surface 21. Note that the "irradiation position PR" includes not only the position on the ingot C surface 21 where the laser beam B is actually irradiated, but also positions where the laser beam B is scheduled to be irradiated and positions that have been irradiated in the past. In addition, in this embodiment, the pulsed laser beam B is intermittently irradiated at discrete irradiation positions PR, thereby forming irradiation marks RM at each of the multiple irradiation positions PR. As a result, the multiple irradiation positions PR are arranged discretely, i.e., in a dotted line, on the irradiation trajectory line Ls. Therefore, moving the irradiation position PR means moving the position of the intermittently irradiated laser beam B on the ingot C surface 21 in an almost discontinuous or discrete manner. In Figure 3 and other figures, the moving direction of the irradiation position PR is shown as the scanning direction Ds.

[0024] In this embodiment, the peeling layer forming step irradiates the ingot C-face 21 with the laser beam B while moving the irradiation position PR so as to trace a concentric or spiral trajectory. As a result, as shown in Fig. 4, arc-shaped irradiation locus lines Ls, which are the loci of irradiation marks RM formed by the movement of the irradiation position PR, are formed at a predetermined pitch in the radial direction of the ingot C-face 21. In other words, the peeling layer 23 is formed by the concentric or spiral irradiation locus lines Ls.

[0025] Specifically, in the peeling layer formation process, as shown in FIG. 5 , the irradiation position PR is moved along an arc-shaped scanning line Sc. That is, the scanning line Sc has a substantially arc-shaped shape centered on the center point in the in-plane direction of the ingot C-face 21. Therefore, the scanning direction Ds is a substantially circumferential direction along the scanning line Sc. As a result, a plurality of arc-shaped irradiation loci Ls are formed in an array at a predetermined line pitch pL in the radial direction of the scanning line Sc. The line pitch pL is the distance between adjacent scanning lines Sc or irradiation loci Ls in the radial direction Dr. The radial direction Dr is a direction extending radially in the in-plane direction from the center point in the in-plane direction of the ingot C-face 21, i.e., the intersection point between the central axis L shown in FIG. 1 and the ingot C-face 21. In other words, the radial direction Dr is the radial direction of the ingot C-face 21, the scanning line Sc, or the irradiation loci Ls. The line pitch can be set to about one to several times the irradiation pitch, which is the distance between adjacent irradiation marks RM included in one irradiation locus line Ls.

[0026] For the sake of simplicity in the following description, in the example of Fig. 5, the multiple scanning lines Sc are shown concentrically around the center point of the in-plane direction of the ingot C-face 21. Therefore, the scanning direction Ds is the circumferential direction around the center point of the ingot C-face 21 along the movement trajectory of the irradiation position PR. Here, in Fig. 5, the multiple scanning lines Sc are shown with ordinal numbers assigned, such as Sc1, Sc2, Sc3, ... Scm, Scn, ..., in order from the outside in the radial direction Dr. m and n are used to simplify the illustration, and it is assumed that n = m + 1.

[0027] In this embodiment, for a plurality of concentric scanning lines Sc, one circular scan is performed along one scanning line Sc, and then the irradiation position PR is offset by a predetermined amount in the radial direction Dr, and the next circular scan is performed along the next scanning line Sc. Here, "circular scanning" refers to scanning the laser beam B around one rotation, i.e., approximately 360 degrees, along one scanning line Sc. As shown in FIG. 5 , the scanning directions Ds of the circular scans of adjacent scanning lines Sc in the radial direction Dr are opposite to each other. That is, for example, the scanning direction Ds of odd-numbered scanning lines Sc, i.e., Sc1, Sc3, Sc5, ..., is clockwise. On the other hand, the scanning direction Ds of even-numbered scanning lines Sc, i.e., Sc2, Sc4, Sc6, ..., is counterclockwise. Specifically, for example, clockwise circular scanning is first performed along the outermost scanning line Sc, i.e., Sc1. Thereafter, the irradiation position PR is moved in the radial direction Dr by the line pitch pL, and a counterclockwise circular scan is performed along the adjacent scanning line Sc on the inside, i.e., Sc2. Furthermore, the irradiation position PR is moved in the radial direction Dr by the line pitch pL, and a clockwise circular scan is performed along the adjacent scanning line Sc on the inside, i.e., Sc3. In this manner, circular scans are performed while reversing the scanning direction Ds in the order of Sc1, Sc2, Sc3, Sc4, ... from the outside of the scanning line Sc in the radial direction Dr. This can be achieved by reversing the direction of relative movement between the ingot 2 to be processed and the laser beam B, for example, the rotation direction of the ingot 2.

[0028] In this embodiment, as shown in FIGS. 3 and 5 , the irradiation positions PR are discretely arranged along the scanning direction Ds or the scanning line Sc to form multiple points, and the trailing laser beam B is irradiated onto the irradiation mark RM formed by the irradiation of the leading laser beam B. That is, multiple laser beams B spaced apart from each other in the scanning direction Ds can be simultaneously irradiated and scanned in the scanning direction Ds. FIG. 5 shows an example in which two laser beams B are scanned while being spaced apart by a predetermined beam pitch pB in the circumferential direction along the scanning line Sc, i.e., in the scanning direction Ds. The beam pitch pB is N times the irradiation pitch, where N is a positive integer and N≧2. Hereinafter, of the two laser beams B, the leading laser beam B in the scanning direction Ds will be referred to as the leading beam B1, and the trailing laser beam B will be referred to as the trailing beam B2. The irradiation position PR corresponding to the leading beam B1 is referred to as a leading irradiation position PR1, and the irradiation position PR corresponding to the trailing beam B2 is referred to as a trailing irradiation position PR2.

[0029] (Effects) The effects achieved by this embodiment will be described below while comparing it with comparative examples as appropriate.

[0030] In the peeling layer formation process, the laser beam B is scanned over almost the entire surface of the ingot C-face 21, forming multiple, approximately circular irradiation trajectories Ls in the radial direction Dr. As described above, the laser beam B has a predetermined degree of transparency with respect to the ingot 2. Therefore, the focal point BP is formed at a predetermined depth from the ingot C-face 21, which is the laser irradiation surface. As a result, a peeling layer 23 consisting of a modified layer RA and cracks C is formed at a predetermined depth from the ingot C-face 21. Then, a wafer precursor 24, which will eventually become the wafer 1, is formed closer to the ingot C-face 21 than the peeling layer 23. At this time, as the modified layer RA is formed, cracks C originate from the modified layer RA and propagate along the (0001) plane Pc. That is, the propagation direction of the cracks C is inclined by an off-angle θ with respect to the in-plane direction parallel to the ingot C-face 21.

[0031] 6A and 6B show the formation of irradiation marks RM by a comparative wafer manufacturing method corresponding to the technology disclosed in Japanese Patent Application Laid-Open No. 2016-111143. In this comparative example, linear scanning of a laser beam B in a first direction, which is an in-plane direction perpendicular to the off-angle direction Dθ, is performed multiple times while changing the position in a second direction, which is an in-plane direction perpendicular to the first direction. According to this comparative example, between adjacent scans in the second direction, i.e., the off-angle direction Dθ, cracks C significantly propagate along the off-angle direction Dθ. As a result, as shown in FIG. 6B , the processing allowance region W, which is the width in the depth direction of the irradiation marks RM, increases. The processing allowance region W corresponds to the thickness of the peeling layer 23 shown in FIG. 3 and constitutes the processing allowance in the wafer flattening process and the ingot flattening process after the wafer peeling process. In other words, in the wafer flattening process and the ingot flattening process, the material portion removed and discarded from the peeled body 30 or the ingot 2 by grinding or polishing is at least equal to or larger than the processing allowance region W. Therefore, in this comparative example, a large amount of material was lost.

[0032] On the other hand, Figures 7A to 7D show the formation of irradiation marks RM according to another comparative example, in which the linear scanning direction of the laser beam B is simply changed to an in-plane direction parallel to the off-angle direction Dθ in order to address the above-mentioned issues. The scanning direction of the laser beam B is indicated by a dashed arrow in the figure. When the laser beam B is scanned in a direction parallel to the off-angle direction Dθ, as shown in Figures 7A and 7B, the next irradiation mark RM is formed before the progression of the crack C in the previously formed irradiation mark RM along the off-angle direction Dθ becomes sufficiently large. In other words, the progression of the crack C in the previously formed irradiation mark RM is suppressed by the subsequently formed irradiation mark RM. Therefore, the progression of the crack C along the off-angle direction Dθ in each of the multiple irradiation marks RM arranged in the scanning direction of the laser beam B can be suppressed more than in the cases of Figures 6A and 6B.

[0033] Here, let us assume a situation in which no irradiation mark RM exists around the irradiation position PR in the in-plane direction. In such a situation, irradiation of the laser beam B tends to cause the irradiation mark RM at a depth near the focal point BP. However, in reality, the laser beam B moves along the scanning direction of the laser beam B while generating irradiation marks RM one after another. Therefore, the situation described above mainly occurs when forming the irradiation mark RM corresponding to the starting point of one scan. Therefore, in most situations, a situation occurs in which the irradiation mark RM exists around the irradiation position PR in the in-plane direction.

[0034] That is, as shown in Figures 7B and 7C, at least a crack C in the previously formed irradiation mark RM is usually present at the in-plane position corresponding to the current irradiation position PR. This increases the absorption rate of the laser beam B in the irradiation mark RM. Furthermore, the crack C is formed along the (0001) plane Pc. Therefore, as shown in Figure 7C, the formation positions of the modified layer RA and the irradiation mark RM tend to progress along the (0001) plane Pc as the laser scans.

[0035] As the irradiation mark RM progresses along the (0001) plane Pc, it is formed at increasingly deeper positions, gradually moving away from the depth of the original focal point BP. This results in a situation where, at the depth corresponding to the previously formed irradiation mark RM, the applied energy density of the laser beam B irradiated this time cannot be increased to a level sufficient to generate a new modified layer RA. When this situation occurs, as shown in FIG. 7D , the newly formed modified layer RA is formed at a depth near the focal point BP of the currently irradiated laser beam B. This results in a step between the previously formed irradiation mark RM and the currently formed irradiation mark RM. Therefore, the processing allowance region W, which is the width of the irradiation mark RM in the depth direction, becomes larger. Therefore, even with this comparative example, a large amount of material loss occurs.

[0036] Furthermore, as described above, if the scanning direction of the laser beam B is linear, the moving speed must be set to zero at the end of the movement of the irradiation position PR, resulting in an acceleration / deceleration region, which lengthens the processing time. In this regard, the example of moving the focal point BP in a spiral pattern, as described in Patent Document 1, can effectively solve this problem. However, even in this case, the relationship between the scanning direction of the laser beam B, i.e., the moving direction, and the off-angle direction Dθ changes from moment to moment depending on the position in the circumferential direction. That is, during one rotation, a state in which the scanning direction of the laser beam B is perpendicular to the off-angle direction Dθ, as shown in FIGS. 6A and 6B, and a state in which the scanning direction of the laser beam B is parallel to the off-angle direction Dθ, as shown in FIGS. 7A to 7D, alternately occur. This causes variations in the formation depth of the modified layer RA, resulting in steps in the peeled layer 23, i.e., the peeled surface 32. Depending on the position in the in-plane direction, the cracks C may no longer connect in the radial direction of the ingot 2, preventing peeling. Furthermore, excessive growth of the crack C increases the processing allowance area W, resulting in a large loss of material.

[0037] Therefore, in this embodiment, the irradiation positions PR are discretely arranged along the arc-shaped scanning line Sc to form multiple points, and the trailing laser beam B is irradiated onto the irradiation mark RM formed by the irradiation of the preceding laser beam B. That is, multiple laser beams B spaced apart from each other in the scanning direction Ds can be simultaneously irradiated and scanned in the scanning direction Ds. Then, the trailing laser beam B is irradiated onto the irradiation mark RM formed by the irradiation of the preceding laser beam B in the scanning direction Ds, i.e., the traveling direction of the laser beam B. Specifically, the leading laser beam B forms a small modified layer RA, and the trailing laser beam B irradiates the modified layer RA to enlarge it. Laser scanning in this embodiment will be described in more detail below using Figures 8A to 8D.

[0038] First, as shown in FIG. 8A , the advance beam B1 forms an irradiation mark RM at a position corresponding to the advance irradiation position PR1. The advance beam B1 is output with lower energy, i.e., pulse energy, than when a laser beam B is irradiated once at one irradiation position PR as in the comparative examples. Note that the "single irradiation" in this case may include multiple pulsed irradiations. Thus, the modified layer RA formed by the irradiation of the relatively low-energy advance beam B1 and the amount of crack C propagation from such modified layer RA are smaller than in the comparative examples. Therefore, as shown in FIG. 8B , the focal point BP of the next advance beam B1 can be formed at a position where the irradiation mark RM formed immediately before it does not interfere. This allows the modified layer RA formed by the advance beam B1 to be formed at approximately the same depth. Therefore, as shown in FIGS. 8B and 8C , the multiple modified layers RA formed by the advance beam B1 do not propagate along the (0001) plane Pc, but rather along the same plane substantially parallel to the ingot C-face 21.

[0039] As shown in FIG. 8C , the trailing beam B2 is irradiated onto the modified layer RA formed by irradiation with the leading beam B1. As a result, the modified layer RA thickens and cracks C propagate in the radial direction Dr. Like the leading beam B1, the trailing beam B2 is output with lower energy than when a laser beam B is irradiated once at one irradiation position PR as in each comparative example. The output energy of the leading beam B1 and the trailing beam B2 may be the same or different. Specifically, for example, the output energies of the leading beam B1 and the trailing beam B2 can be appropriately adjusted depending on the transmittance of the laser beam B through the ingot 2, etc.

[0040] According to this embodiment, as shown in FIG. 8D , by sequentially irradiating the trailing beam B2 onto multiple modified layers RA formed at approximately the same depth by the leading beam B1, the irradiation marks RM progress along the same plane approximately parallel to the ingot C-face 21. This effectively suppresses variations in the depths of the modified layers RA and the irradiation marks RM, regardless of the relationship between the scanning direction Ds and the off-angle direction Dθ. That is, it is possible to form the peeling layer 23 as thin as possible. Therefore, the processing allowance region W, which results in material loss, is effectively reduced, and the process time can be shortened as much as possible. Therefore, this embodiment makes it possible to provide a wafer manufacturing method with higher manufacturing efficiency than conventional methods.

[0041] Second Embodiment A second embodiment will be described below. In the description of this embodiment, differences from the first embodiment will be mainly described. In addition, the same reference numerals are used for identical or equivalent parts between the first embodiment and this embodiment. Therefore, in the following description of this embodiment, for components having the same reference numerals as those in the first embodiment, the description of the first embodiment may be used as appropriate unless there is a technical contradiction or a special additional explanation. The same applies to the third and subsequent embodiments.

[0042] 5, the first embodiment is an example in which circular scanning is performed while reversing the scanning direction Ds in the order of Sc1, Sc2, Sc3, Sc4, ..., starting from the outside of the scanning line Sc in the radial direction Dr. Note that this order can also be reversed. In contrast, this embodiment forms a new irradiation locus line Ls by irradiating the laser beam B between existing irradiation locus lines Ls adjacent in the radial direction Dr. Specifically, in this embodiment, for example, circular scanning along the outermost even-numbered scanning line Sc, i.e., Sc2, is performed after the irradiation locus line Ls is formed by the scanning lines Sc on both sides of it in the radial direction Dr, i.e., Sc1 and Sc3. Similarly, in this embodiment, for example, circular scanning along the second outermost even-numbered scanning line Sc, i.e., Sc4, is performed after the irradiation locus line Ls is formed by the scanning lines Sc on both sides of it in the radial direction Dr, i.e., Sc3 and Sc5.

[0043] As described above, the crack C propagates along the (0001) plane Pc upon irradiation with the laser beam B. Here, the propagation in the scanning direction Ds can be limited to approximately the irradiation pitch due to the formation of a modified layer RA by the leading beam B1 prior to the irradiation of the trailing beam B2. On the other hand, the propagation in the radial direction Dr is not particularly limited unless a preceding irradiation locus Ls is formed. Therefore, in the scanning mode shown in FIG. 5 , particularly when a small line pitch pL is set, a situation may arise in which the crack C extending from the previously formed irradiation locus Ls reaches the current irradiation position PR. If this situation occurs, the laser beam B will be irradiated onto the area where the crack C exists, and as described above, the absorption rate will increase at the location where the crack C occurs, which may result in fluctuations in the depth of the modified layer RA. Alternatively, the crack C may reflect the laser beam B, causing the focal point BP to occur at a shallower depth than expected, resulting in the modified layer RA occurring at a shallower position than usual. Therefore, if the above situation occurs, the processing allowance area W will become larger, and there is a concern that material loss will increase.

[0044] Therefore, in the scanning mode according to this embodiment, the current circular scan is performed between adjacent existing irradiation locus lines Ls spaced apart by twice the line pitch pL in the radial direction Dr. According to this scanning mode, when the current circular scan is performed, it is easy to achieve a situation in which the crack C extending from the previously formed irradiation locus line Ls does not reach the corresponding scan line Sc. Therefore, during the current circular scan, the laser beam B is not interfered with by the crack C, and the modified layer RA can be formed to a substantially uniform depth across the entire width of the ingot 2 in the scanning direction Ds. Therefore, according to this scanning mode, material loss due to variations in the depth of the modified layer RA can be effectively suppressed.

[0045] There is no particular limitation on the order in which circular scanning is performed for each of the multiple scanning lines Sc. That is, for example, circular scanning for odd-numbered scanning lines Sc may be completed first, and then circular scanning for even-numbered scanning lines Sc may be performed. Alternatively, conversely, circular scanning for even-numbered scanning lines Sc may be completed first, and then circular scanning for odd-numbered scanning lines Sc may be performed. Alternatively, circular scanning for the outermost pair of odd-numbered scanning lines Sc may be performed first, for example, Sc1, Sc3, Sc2, Sc5, Sc4, ..., and then circular scanning for the even-numbered scanning lines Sc and the odd-numbered scanning lines Sc may be performed alternately. Furthermore, circular scanning may be performed from the inside in the radial direction Dr, rather than from the outside as in the above example.

[0046] (Third Embodiment) A third embodiment will be described below. This embodiment is a partial modification of the second embodiment. That is, in this embodiment, a new irradiation locus line Ls is formed by irradiating a laser beam B between existing irradiation locus lines Ls adjacent to each other in the radial direction Dr. Furthermore, in this embodiment, irradiation locus lines Ls are simultaneously formed for multiple scanning lines Sc in a single circular scan. Specifically, multiple laser beams B having different irradiation positions PR in at least the radial direction Dr are irradiated onto the ingot C surface 21, thereby simultaneously forming multiple irradiation locus lines Ls. FIG. 9 shows an example in which a total of six laser beams B, two in the scanning direction Ds and three in the radial direction Dr, are scanned in the scanning direction Ds in a single laser scan.

[0047] More specifically, in the example of FIG. 9 , for example, odd-numbered scanning lines Sc are scanned three at a time. Then, even-numbered scanning lines Sc are scanned three at a time. This makes it possible to achieve the same effects as those of the first and second embodiments described above, but with a shorter cycle time. Note that the positions of the three laser beams B or irradiation positions PR arranged in the radial direction Dr in the scanning direction Ds may be substantially the same as shown in FIG. 9 . That is, the three laser beams B or irradiation positions PR may be located on an imaginary line extending radially from the center point of the ingot C-face 21. Alternatively, the arrangement direction of the three laser beams B or irradiation positions PR may intersect with this imaginary line.

[0048] (Fourth Embodiment) A fourth embodiment will be described below. This embodiment is different from the first to third embodiments in that the irradiation conditions of the laser beam B are controlled according to the position in the in-plane direction. Specifically, with reference to FIGS. 5 and 9, this embodiment changes the output of the laser beam B according to the circumferential position of the irradiation position PR on the scan line Sc. Hereinafter, in FIG. 5 and other figures, the right-handed XYZ coordinate system is set so that the off-angle direction Dθ is the positive X-axis direction and the ingot C-face 21 faces the positive Z-axis direction, and the substantially circular shape of the ingot C-face 21 is likened to a clock so that the positive Y-axis direction is the 12 o'clock direction and the positive X-axis direction is the 3 o'clock direction.

[0049] In the first type of region where the irradiation position PR is located at the 6 o'clock and 12 o'clock azimuths, the scanning direction Ds is parallel to the off-angle direction Dθ. In such regions, cracks C are unlikely to propagate in the radial direction Dr, which is the direction of the line pitch pL. Therefore, in such regions, the output is increased to promote the propagation of cracks C. In contrast, in the second type of region where the irradiation position PR is located at the 3 o'clock and 9 o'clock azimuths, the scanning direction Ds is perpendicular to the off-angle direction Dθ. In such regions, cracks C are likely to propagate in the radial direction Dr, which is the direction of the line pitch pL, and there is a concern that the propagation of cracks C to adjacent scanning lines Sc may cause fluctuations in the depth of the modified layer RA. Therefore, in such regions, the output is reduced to suppress the propagation of cracks C. In regions intermediate between the first type of region and the second type of region in the circumferential direction, the output is set to an intermediate value and is varied according to changes in circumferential position. In this way, by adjusting the output according to the circumferential position, it is possible to effectively stabilize the propagation amount of cracks C.

[0050] Fifth Embodiment A fifth embodiment will now be described. As with the fourth embodiment, this embodiment also controls the irradiation conditions of the laser beam B according to the position in the in-plane direction. However, in this embodiment, the irradiation conditions of the laser beam B are controlled based on the measurement results of the transmittance of the laser beam B through the semiconductor material constituting the ingot 2. Specifically, in this embodiment, the optical characteristics, i.e., the transmittance and refractive index, of the obtained wafer 1 or peeled body 30 are measured at multiple positions in the in-plane direction, and the irradiation conditions of the next laser beam B are controlled based on the measurement results. The irradiation conditions include, for example, the output, i.e., the irradiation energy and the irradiation distance.

[0051] FIG. 10 shows an outline of the wafer manufacturing method according to this embodiment. In FIG. 10 , "Loading / Unloading" refers to the loading and unloading steps of the workpiece, i.e., the peeled body 30 or the ingot 2. "Laser Slicing" refers to the peeled layer formation step. "Rough Grinding" refers to the rough grinding step of the main surface of the ingot 2 or the peeled body 30. For example, a grinding material with a grit size of about #800 can be used for rough grinding. "Finish Grinding" refers to the finish grinding step of the surface. For example, a grinding material with a grit size of about #30000 can be used for finish grinding. "Wafer Beveling" refers to the chamfering of the corners of the outer edge of the peeled body 30 in the radial direction. The "radial direction" here refers to the direction extending radially from the center of the peeled body 30 in the in-plane direction. "Wafer Optical Measurement" refers to the process of measuring the optical properties of the peeled body 30 after finish grinding at multiple positions in the in-plane direction. "Ingot cleaning" refers to a process of cleaning the ingot 2 after finish grinding. The arrows on the left side of the blocks indicating each process indicate the processing flow of the ingot 2. The arrows on the right side of the blocks indicating each process indicate the processing flow of the wafer 1 or the peeled body 30, which may be commonly referred to as a "wafer."

[0052] Referring to FIG. 10 , first, an ingot 2 is loaded into a wafer manufacturing apparatus. Next, the loaded ingot 2 is subjected to a separation layer forming process by laser slicing, i.e., irradiation with a laser beam B. Subsequently, in a wafer separation process, a separation body 30 is separated from the ingot 2 that has undergone the separation layer forming process. The top surface of the ingot 2 newly generated after the wafer separation process is flattened by rough grinding and finish grinding. Thereafter, the ingot 2 is cleaned and then subjected to the separation layer forming process again. Note that the ingot 2 that has undergone the separation layer forming process or the ingot cleaning process is ejected from the wafer manufacturing apparatus if its height falls below a predetermined value.

[0053] The peeled body 30 peeled from the ingot 2 in the wafer peeling process is subjected to beveling, rough grinding, and finish grinding, and then optical measurement. The measurement results are used to determine the irradiation conditions of the laser beam B in the next peeling layer formation process. That is, based on the optical measurement results for each location in the in-plane direction of the wafer 1, the irradiation conditions for each location in the in-plane direction of the ingot C-face 21 in the next peeling layer formation process are controlled. This enables fine-tuned changes to the irradiation conditions to accommodate variations in optical properties from location to location in the in-plane direction, thereby reducing material loss. Note that only one of the transmittance and refractive index may be measured. Alternatively, the transmittance and refractive index may be measured on the finally obtained epi-ready wafer 1. Depending on the rough grinding conditions, finish grinding may not be necessary. That is, rough grinding and finish grinding may be integrated.

[0054] FIG. 11 shows an example of how optical measurement positions are set in a generator 100. The generator 100 is the target of optical measurement and corresponds to a wafer 1 or a separated body 30 whose surface has been flattened to a predetermined degree after being separated from an ingot 2. In this example, the optical measurement positions are set at a constant measurement pitch in each of the X-axis direction and the Y-axis direction. The measurement pitch is, for example, about 1 mm. The X-axis direction is, for example, parallel to the off-angle direction Dθ shown in FIG. 1 and the like.

[0055] FIG. 13 shows how the absorption coefficient of laser beam B changes with the change in measurement position when optical measurements are performed at multiple measurement positions on the measurement line Lx, as shown in FIG. 12. The measurement line Lx is a virtual line that passes through the center of the generator 100 in the in-plane direction and is parallel to the X-axis. In FIG. 13, the horizontal axis indicates the measurement position, measured in mm, when the center of the generator 100 in the in-plane direction is set as the origin, i.e., "0." As shown in FIG. 13, the absorption coefficient is not constant in the in-plane direction but changes with the change in measurement position. The absorption coefficient is obtained, i.e., calculated, using the following equation (1). In the following equation (1), α represents the absorption coefficient, D represents the workpiece thickness, i.e., the thickness of the generator 100, and T represents the transmittance.

[0056] This embodiment is particularly effective when the wafer 1 or ingot 2 has a facet region RF as shown in FIGS. 11 and 12 . The facet region RF may also be referred to as a "facet portion." Regions other than the facet region RF are hereinafter referred to as non-facet regions RN. The non-facet region RN may also be referred to as a "non-facet portion." It is known that the intensity of the laser beam B reaching the focal point BP is stronger in the non-facet region RN than in the facet region RF. Specifically, the region with a high absorption coefficient on the right side in FIG. 13 corresponds to the facet region RF. Furthermore, as shown in FIG. 13 , even the non-facet region RN, which has a lower absorption coefficient than the facet region RF, may have a distribution in the in-plane direction, i.e., the radial direction. The "radial direction" refers to the direction extending radially from the center of the in-plane direction of the generative body 100 along the in-plane direction.

[0057] 14A to 14C show how the location where the modified layer RA occurs changes with changes in transmittance, i.e., absorption coefficient. In the figures, the density of the hatching on the ingot 2 corresponds to the transmittance or absorption coefficient. That is, the darker the hatching, the lower the transmittance and, therefore, the higher the absorption coefficient. The location where the modified layer RA occurs is the position where the laser beam B is focused, and can be indicated by the dimension in the depth direction of the ingot 2 from the ingot C-face 21, which is the laser irradiation surface. Here, the depth direction of the ingot 2 is a direction parallel to the height direction of the ingot 2, and more specifically, the direction from the ingot C-face 21 toward the ingot Si-face 22. In the figures, the circle drawn with a dashed line next to the modified layer RA indicates the focused state, i.e., the beam diameter, of the laser beam B at the location where the modified layer RA occurs.

[0058] First, referring to FIG. 14A , as the laser beam B travels through the ingot 2 in the depth direction, it is focused while attenuating according to the absorption coefficient. When the energy density increases to a predetermined level due to the focusing, it reaches the processing threshold, and a modified layer RA is formed. Here, when the transmittance is low, i.e., when the absorption coefficient is high, the amount of attenuation is large. As a result, the energy density corresponding to the processing threshold is reached at a deep position where the focusing cross-sectional area is smaller, as shown in FIG. 14B, and the modified layer RA is generated. On the other hand, when the transmittance is high, the amount of attenuation is small. As shown in FIG. 14C, the energy density corresponding to the processing threshold is reached even at a shallow position where the focusing cross-sectional area is larger, and the modified layer RA is generated. Thus, if the position where the modified layer RA is generated varies due to differences in transmittance, i.e., absorption coefficient, the surface of the product 100 after peeling becomes rough, and the amount of processing required for grinding and polishing, i.e., material loss, increases.

[0059] Therefore, in this embodiment, the transmittance is measured at multiple positions in the in-plane direction, and the irradiation conditions of the laser beam B at each of the multiple positions in the in-plane direction are controlled based on the measurement results. Specifically, this embodiment acquires, i.e., calculates, the absorption coefficient based on the transmittance measured for the product 100 generated in the past, including the previous generation. Then, this embodiment acquires the trend of change in the absorption coefficient in the height direction, i.e., the depth direction, of the ingot 2 for each different position in the plane, and determines the irradiation energy of the laser beam B based on this. That is, for example, the lower the transmittance, the higher the irradiation energy.

[0060] A specific example of controlling the irradiation conditions of the next laser beam B from the optical measurement results of the product 100 obtained previously will be described below. First, the transmittance, etc. of the product 100 obtained previously is measured using a transmittance meter. At this time, the workpiece thickness, which is the thickness of the product 100, is also measured. The absorption coefficient is calculated based on the measured transmittance, workpiece thickness, and the above formula (1). Then, the input energy, which is the irradiation energy of the laser beam B, is derived using the following formula (2). In the following formula (2) and FIG. 15, I 0indicates the input energy, I indicates the processing threshold, i.e., the minimum applied energy required for modification, z indicates the depth, and k indicates the amount of change in the absorption coefficient in the depth direction, i.e., the change tendency of the absorption coefficient in the depth direction of the ingot 2.

[0061] A method for deriving the amount of change in the absorption coefficient will be described below. As shown in Figure 16, the central position of the ingot 2 in the in-plane direction is defined as the in-plane central position Ma. Furthermore, the position on a measurement line Lx that passes through the in-plane central position Ma and is parallel to the X-axis and is an end position of the ingot 2 located within the facet region RF is defined as the first end position Mb. Furthermore, the position on this measurement line Lx that is opposite to the first end position Mb is defined as the second end position Mc. The second end position Mc is a position that is approximately symmetrical to the first end position Mb with respect to the in-plane central position Ma.

[0062] Figure 17A shows how the absorption coefficient changes in the depth direction of the ingot 2 at the in-plane center position Ma. Figure 17B shows how the absorption coefficient changes in the depth direction of the ingot 2 at the first end position Mb. Figure 17C shows how the absorption coefficient changes in the depth direction of the ingot 2 at the second end position Mc. As shown in Figures 17A to 17C, it can be seen that the change in the absorption coefficient in the depth direction of the ingot 2 has a certain tendency and differs for each in-plane position. Based on this tendency of change in the absorption coefficient in the depth direction for each in-plane position, the amount of change in the absorption coefficient can be derived, and this value can be added to or multiplied by the absorption coefficient obtained previously and used to determine the input energy for the next processing.

[0063] For example, as shown in FIG. 18, the previously obtained absorption coefficient α n-1 and the absorption coefficient α obtained two times previously n-2 Based on the amount of change in the absorption coefficient, the estimated value α n Specifically, for example, the previously acquired absorption coefficient α n-1 and the absorption coefficient α obtained two times previously n-2 The difference between the previous absorption coefficient α n-1The absorption coefficient estimate α n Then, the absorption coefficient estimate α n Based on this, it is possible to determine the irradiation energy of the laser beam B. When calculating the amount of change in the absorption coefficient, statistical processing using a so-called "smoothing filter" or the like may be performed.

[0064] 19, a first product 101 and a second product 102 are produced. The first product 101 is a product 100 obtained from one end of the ingot 2 in the height direction, i.e., the ingot C-face 21 side. The second product 102 is a product 100 obtained from the other end of the ingot 2 in the height direction, i.e., the ingot Si-face 22 side. Next, a first absorption coefficient, which is the absorption coefficient in the first product 101, and a second absorption coefficient, which is the absorption coefficient in the second product 102, are obtained. The higher of the first and second absorption coefficients can then be used as the upper limit of the absorption coefficient to determine the irradiation conditions for the laser beam B, i.e., the irradiation energy. In other words, the absorption coefficient obtained from the product 100 with the higher absorption coefficient, i.e., the wafer 1, can be used as the upper limit, and the coefficient setting can be used to prevent any further change.

[0065] The measurement pitch for optical measurement may be uniform as shown in FIG. 11 , but can be changed as appropriate. That is, for example, different pitches may be used in the X-axis direction and the Y-axis direction. Alternatively, the measurement pitch may be finer in a region where the change in absorption coefficient is greater than in other regions, such as the region surrounded by the dashed-dotted rectangle in FIG. 20 . Specifically, such a region is, for example, the boundary between the non-facet region RN and the facet region RF. That is, the measurement pitch may be finer in such a boundary region than in other regions. The region where the measurement pitch is finer may include the entire facet region RF. More specifically, referring to FIG. 20 , for example, the measurement pitch may be finer in a region to the right of the measurement position 40 mm than in a region to the left of the measurement position 40 mm. In other words, the measurement pitch may be finer in a predetermined region formed by the non-facet region RN and the boundary between the non-facet region RN and the facet region RF than in a region outside such a predetermined region.

[0066] (Modifications) The present disclosure is not limited to the above-described embodiment. Therefore, the above-described embodiment can be modified as appropriate. Representative modifications will be described below. In the following description of the modifications, differences from the above-described embodiment will be mainly described. Furthermore, the same reference numerals are used for parts that are identical or equivalent to each other in the above-described embodiment and the modifications. Therefore, in the following description of the modifications, the description of the above-described embodiment can be used as appropriate for components that have the same reference numerals as the above-described embodiment, unless there is a technical contradiction or special additional explanation.

[0067] The present disclosure is not limited to the specific configurations shown in the above embodiments. That is, for example, there are no particular limitations on the outer diameter or planar shape (e.g., the presence or absence of a so-called orientation flat) of the wafer 1, i.e., the ingot 2. There are also no particular limitations on the magnitude of the off-angle θ. Furthermore, in the above embodiments, the wafer C-plane 11 and the ingot C-plane 21 do not coincide with the C-plane in the strict crystallographic sense, i.e., the (0001) plane Pc. However, even in such cases, the term "C-plane" is used because it is generally accepted. However, the present disclosure is not limited to such an embodiment. That is, the wafer C-plane 11 and the ingot C-plane 21 may coincide with the C-plane in the strict crystallographic sense, i.e., the (0001) plane Pc. In other words, the off-angle θ may be 0 degrees.

[0068] In the above embodiment, the peeling layer 23 is formed on the ingot C-face 21 side by "C-face side irradiation" in which the laser beam B is irradiated onto the ingot C-face 21. However, the present disclosure is not limited to this embodiment. That is, the present disclosure is also applicable to "Si-face side irradiation" in which the laser beam B is irradiated onto the ingot Si-face 22 to form the peeling layer 23 on the ingot Si-face 22 side.

[0069] Depending on the irradiation conditions and scanning conditions of the laser beam B, the peeled surface 32 may have a surface condition that allows it to be satisfactorily ground or polished even if it is subjected to the ECMG process as is. Therefore, the rough grinding process of the peeled surface 32 shown in Fig. 2 may be omitted. The same applies to the rough grinding of the top surface of the ingot 2 after the wafer peeling process.

[0070] In the above embodiment, the scanning direction Ds is the circumferential direction along the arc-shaped scanning line Sc, but the present disclosure is not limited to this. That is, for example, the scanning direction Ds may be defined as the tangential direction of the arc-shaped scanning line Sc at the irradiation position PR. Furthermore, there is no particular limitation on the number of laser beams B arranged in the scanning direction Ds that are scanned in one circular scan. That is, in the above embodiment, two laser beams B, the leading beam B1 and the trailing beam B2, are arranged in the scanning direction Ds, but three or more laser beams may be arranged. In other words, the irradiation mark RM, i.e., the modified layer RA, may be gradually enlarged by irradiating one irradiation position PR with the laser beam B three or more times. The number of laser beams B arranged in the radial direction Dr that are scanned in one circular scan and the arrangement in the scanning direction Ds may also be appropriately changed from the specific example shown in the above embodiment.

[0071] Referring to FIG. 5 , in the second embodiment, the multiple scanning lines Sc are divided into two types, odd-numbered and even-numbered, for scanning. However, the present disclosure is not limited to this configuration. That is, for example, the multiple scanning lines Sc may be divided into three types, a first group of 3kth, a second group of 3k−1th, and a third group of 3k−2th, for scanning. k is an integer greater than or equal to 1. Similarly, for example, the multiple scanning lines Sc may be divided into four types, a first group of 4kth, a second group of 4k−1th, a third group of 4k−2th, and a fourth group of 4k−3th, for scanning. Furthermore, the present disclosure is not limited to a configuration in which multiple circular scanning lines Sc are arranged concentrically. That is, for example, referring to FIG. 5 , odd-numbered scanning lines Sc1, Sc3, Sc5, ... may be part of one spiral scanning line Sc extending from the outside to the inside, and even-numbered scanning lines Sc2, Sc4, Sc6, ... may be part of another spiral scanning line Sc extending from the inside to the outside. In this case, these two alternately arranged spiral scanning lines Sc may be connected at the center in the in-plane direction of the ingot C-plane 21.

[0072] It goes without saying that the elements constituting the above-described embodiments are not necessarily essential unless expressly stated as essential or clearly considered essential in principle. Furthermore, when numerical values ​​such as the number, amount, and range of components are mentioned, the present disclosure is not limited to those specific numerical values ​​unless expressly stated as essential or clearly limited to specific numerical values ​​in principle. Similarly, when the shape, direction, positional relationship, etc. of components are mentioned, the present disclosure is not limited to those shapes, directions, positional relationships, etc., unless expressly stated as essential or clearly limited to specific shapes, directions, positional relationships, etc. in principle.

[0073] The modified examples are not limited to the above examples. For example, other than those exemplified above, multiple embodiments may be combined with each other as long as there is no technical contradiction. Similarly, multiple modified examples may be combined with each other as long as there is no technical contradiction.

[0074] (Viewpoints of the Present Disclosure) As is clear from the description of the above-described embodiments and modified examples, the above-described present disclosure can be understood from the following viewpoints, for example. [First Viewpoint] A laser processing method for irradiating a workpiece (2) made of a semiconductor material with a laser beam (B), comprising modified layer formation, in which the laser beam, which is transparent to a surface (21) of the workpiece, is irradiated to form a modified layer (RA) at a predetermined depth from the surface, the modified layer formation being performed by moving an irradiation position (PR) of the laser beam on the surface along an arc-shaped scanning line (Sc) to form an array of arc-shaped irradiation locus lines (Ls) made of irradiation marks of the laser beam at a predetermined line pitch (pL) in a radial direction (Dr) of the scanning line, the irradiation positions being discretely provided along the scanning line to form multiple points, and a subsequent laser beam is irradiated onto the irradiation marks formed by irradiation of a preceding laser beam. [Second Aspect] The laser processing method according to the first aspect, wherein a new irradiation locus line is formed by irradiating the laser beam between the existing irradiation locus lines that are adjacent in the radial direction. [Third Aspect] The laser processing method according to the first or second aspect, wherein the directions of relative movement between the object to be processed and the laser beam are opposite in the scanning lines that are adjacent in the radial direction. [Fourth Aspect] The laser processing method according to any one of the first to third aspects, wherein a plurality of irradiation locus lines are simultaneously formed by irradiating the surface with a plurality of the laser beams that have different irradiation positions in at least the radial direction. [Fifth Aspect] The laser processing method according to any one of the first to fourth aspects, wherein irradiation conditions of the laser beam are controlled in accordance with an in-plane position along the surface. [Sixth Aspect] The laser processing method according to the fifth aspect, wherein the irradiation conditions are controlled based on a measurement result of the transmittance of the laser beam at the in-plane position.[Seventh Aspect] The laser processing method according to the sixth aspect, wherein a change trend in the absorption coefficient of the laser beam in the semiconductor material in the depth direction is obtained based on the measurement results, and the irradiation conditions are determined based on the obtained change trend. [Eighth Aspect] The laser processing method according to the sixth or seventh aspect, wherein a measurement pitch of the transmittance is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions. [Ninth Aspect] The laser processing method according to any one of the first to eighth aspects, wherein the object to be processed is a single crystal SiC ingot. [Tenth Aspect] A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising: irradiating a surface (21) at one end in a height direction of the ingot with a transparent laser beam (B) to form a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer, wherein the peeling layer formation comprises: moving an irradiation position (PR) of the laser beam on the surface along an arc-shaped scanning line (Sc) to form an array of arc-shaped irradiation loci (Ls) consisting of irradiation marks of the laser beam at a predetermined line pitch (pL) in a radial direction (Dr) of the scanning line, wherein the irradiation positions are discretely provided along the scanning line to form multiple points, and a subsequent laser beam is irradiated onto the irradiation marks formed by irradiation of a previous laser beam. [Eleventh Aspect] The wafer manufacturing method according to the tenth aspect, wherein the laser beam is irradiated between existing irradiation loci adjacent to each other in the radial direction to form a new irradiation loci. [Twelfth Aspect] The wafer manufacturing method according to the tenth or eleventh aspect, wherein directions of relative movement between the ingot and the laser beam are opposite in adjacent scanning lines in the radial direction. [Thirteenth Aspect] The wafer manufacturing method according to any one of the tenth to twelfth aspects, wherein a plurality of the irradiation locus lines are simultaneously formed by irradiating the surface with a plurality of the laser beams having different irradiation positions at least in the radial direction.[14th Aspect] A wafer manufacturing method according to any one of the 10th to 13th aspects, wherein irradiation conditions of the laser beam are controlled in accordance with an in-plane position along the surface. [15th Aspect] A wafer manufacturing method according to the 14th aspect, wherein the irradiation conditions are controlled based on a measurement result of the transmittance of the laser beam at the in-plane position. [16th Aspect] A wafer manufacturing method according to the 15th aspect, wherein a change trend in the height direction of the absorption coefficient of the laser beam in the ingot is obtained based on the measurement result, and the irradiation conditions are determined based on the obtained change trend. [17th Aspect] A wafer manufacturing method according to the 15th or 16th aspect, wherein a measurement pitch of the transmittance is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions.

Claims

1. A laser processing method for irradiating a laser beam (B) onto a processing object (2) made of a semiconductor material, the method including modified layer formation, in which the laser beam, which is transparent to a surface (21) of the processing object, is used to form a modified layer (RA) at a predetermined depth from the surface, the modified layer formation being performed by moving the irradiation position (PR) of the laser beam on the surface along an arc-shaped scanning line (Sc) to form an arc-shaped irradiation locus line (Ls) consisting of the irradiation marks of the laser beam at a predetermined line pitch (pL) in the radial direction (Dr) of the scanning line, the irradiation positions being discretely provided along the scanning line to form multiple points, and the subsequent laser beam is irradiated onto the irradiation marks formed by irradiation of the preceding laser beam.

2. The laser processing method according to claim 1, wherein a new irradiation trajectory line is formed by irradiating the laser beam between existing irradiation trajectory lines adjacent in the radial direction.

3. The laser processing method according to claim 1, wherein directions of relative movement between the object to be processed and the laser beam in adjacent scanning lines in the radial direction are opposite to each other.

4. The laser processing method according to claim 1, wherein a plurality of the irradiation trajectories are formed simultaneously by irradiating the surface with a plurality of the laser beams having different irradiation positions at least in the radial direction.

5. The laser processing method according to claim 1, further comprising controlling irradiation conditions of the laser beam in accordance with an in-plane position along the surface.

6. The laser processing method according to claim 5, wherein the irradiation conditions are controlled based on a measurement result of the transmittance of the laser beam at the in-plane position.

7. The laser processing method according to claim 6, further comprising the steps of: obtaining a change trend in the absorption coefficient of the laser beam in the semiconductor material in the depth direction based on the measurement results; and determining the irradiation conditions based on the obtained change trend.

8. The laser processing method according to claim 6, wherein the measurement pitch of the transmittance is narrower in a boundary portion between the facet region (RF) and the non-facet region (RN) than in other portions.

9. The laser processing method according to claim 1, wherein the object to be processed is a single crystal SiC ingot.

10. A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising forming a peeling layer (23) from a surface (21) on one end side in a height direction of the ingot with a transparent laser beam (B) to form a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer, the peeling layer formation being performed by moving an irradiation position (PR) of the laser beam on the surface along an arc-shaped scanning line (Sc) to form an arc-shaped irradiation locus line (Ls) consisting of irradiation marks of the laser beam at a predetermined line pitch (pL) in a radial direction (Dr) of the scanning line, the irradiation positions being discretely provided along the scanning line to form multiple points, and the subsequent laser beam being irradiated onto the irradiation marks formed by irradiation of the preceding laser beam.

11. The wafer manufacturing method according to claim 10, further comprising the step of: forming a new irradiation locus line by irradiating the laser beam between existing irradiation locus lines adjacent in the radial direction.

12. The wafer manufacturing method according to claim 10, wherein directions of relative movement between the ingot and the laser beam in adjacent scanning lines in the radial direction are opposite to each other.

13. The wafer manufacturing method according to claim 10, wherein a plurality of the irradiation trajectories are simultaneously formed by irradiating the surface with a plurality of the laser beams having different irradiation positions at least in the radial direction.

14. The wafer manufacturing method according to claim 10, further comprising controlling irradiation conditions of the laser beam in accordance with an in-plane position along the surface.

15. The wafer manufacturing method according to claim 14, further comprising controlling the irradiation conditions based on a measurement result of a transmittance of the laser beam at the in-plane position.

16. The wafer manufacturing method according to claim 15, further comprising: obtaining a trend of change in the absorption coefficient of the laser beam in the ingot in the height direction based on the measurement results; and determining the irradiation conditions based on the obtained trend of change.

17. A wafer manufacturing method according to claim 15, further comprising the step of narrowing the measurement pitch of the transmittance in a boundary portion between a facet region (RF) and a non-facet region (RN) compared to other portions.

Citation Information

Patent Citations

  • Substrate processing device and substrate processing method

    JP2015123466A

  • Cutting method of processing object material

    JP2018050066A

  • Laser machining device

    JP2020102522A

  • Method for detecting facet area, method for producing wafer, detection device, and laser processing device

    JP2023003693A