Semiconductor laser element and semiconductor laser device
The semiconductor laser device employs a two-layer transparent electrode structure with varying magnesium concentrations and a thin p-side cladding layer to address the trade-off between output and voltage, achieving efficient and low-voltage operation by suppressing both bulk and contact resistance.
Patent Information
- Application Number
- PCT/JP2024/017347
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-10
- Publication Date
- 2024-12-05
AI Technical Summary
Semiconductor laser devices face a trade-off between increasing output and reducing operating voltage, as thinning the p-side cladding layer increases light absorption, and using transparent electrodes with added impurities like magnesium reduces contact resistance but increases bulk resistance, necessitating a solution to suppress both bulk and contact resistance.
A semiconductor laser device with a two-layer transparent electrode structure, where the first layer has a higher magnesium concentration and the second layer has a lower concentration, is used, along with a thin p-side cladding layer, to reduce bulk and contact resistance, thereby lowering the operating voltage without increasing bulk resistance.
This configuration effectively reduces the operating voltage of the semiconductor laser device while maintaining high efficiency by managing the magnesium concentration and thickness of the transparent electrode layers, achieving a balance between reduced resistance and increased output.
Smart Images

Figure JP2024017347_05122024_PF_FP_ABST
Abstract
Description
Semiconductor laser element and semiconductor laser device
[0001] The present disclosure relates to a semiconductor laser element and a semiconductor laser device including the same.
[0002] In recent years, semiconductor laser elements have been attracting attention as light sources for a variety of applications, including as light sources for image display devices such as displays and projectors, light sources for vehicle headlamps, light sources for industrial and consumer lighting, and light sources for industrial equipment such as laser welding devices, thin film annealing devices, and laser processing devices.
[0003] As disclosed in Patent Document 1 and the like, a semiconductor laser element generally has a structure in which an emission layer that emits light is sandwiched between a first semiconductor layer (e.g., an n-side cladding layer) and a second semiconductor layer (e.g., a p-side cladding layer).
[0004] Japanese Patent Application Publication No. 9-246664
[0005] A semiconductor laser element according to one aspect of the present disclosure includes a substrate, a first semiconductor layer formed on the substrate, a light-emitting layer formed on the first semiconductor layer, a second semiconductor layer formed on the light-emitting layer, the second semiconductor layer having an upwardly protruding ridge portion, and a transparent electrode member formed above the ridge portion, wherein the transparent electrode member is in contact with the second semiconductor layer and includes a first transparent electrode member containing an added impurity at a first impurity concentration, and a second transparent electrode member containing the added impurity at a second impurity concentration lower than the first impurity concentration.
[0006] Schematic diagram for explaining a configuration of a semiconductor laser element according to an embodiment of the present disclosure Schematic diagram for explaining a configuration of a semiconductor laser element according to an embodiment of the present disclosure Schematic cross-sectional views illustrating each step in a method for manufacturing a semiconductor laser element according to the embodiment Schematic cross-sectional views illustrating each step in a method for manufacturing a semiconductor laser element according to the embodiment Schematic cross-sectional views illustrating each step in a method for manufacturing a semiconductor laser element according to the embodiment Schematic cross-sectional views illustrating each step in a method for manufacturing a semiconductor laser element according to the embodiment Schematic cross-sectional views illustrating each step in a method for manufacturing a semiconductor laser element according to the embodiment Schematic cross-sectional views illustrating each step in a method for manufacturing a semiconductor laser element according to the embodiment 6A and 6B are schematic cross-sectional views illustrating steps in a method for manufacturing a semiconductor laser element according to the present embodiment; a top view illustrating a mounting form of a semiconductor laser element according to the present embodiment; a cross-sectional view illustrating a mounting form of a semiconductor laser element according to the present embodiment; a diagram illustrating, in comparison with a comparative example, an effect obtained by configuring a transparent electrode member from a first transparent electrode member having a relatively high magnesium concentration and a second transparent electrode member having a magnesium concentration lower than that of the first transparent electrode member in the present disclosure; a diagram illustrating the results of an experiment measuring a voltage value at which a current flowing through a transparent electrode member is 0.5 mA when the film thickness of the first transparent electrode member is changed in a configuration corresponding to the present disclosure described in FIG. 6; a diagram illustrating the results of a simulation of a voltage value at which a current flowing through a transparent electrode member is 5 mA when the film thickness of the first transparent electrode member layer is changed in a configuration corresponding to the present disclosure described in FIG.FIG. 1 shows the results of a simulation calculation of the maximum film thickness of the first transparent electrode member layer at which the voltage ratio between the configuration corresponding to the present disclosure and the configuration of the comparative example is 1 or less. FIG. 2 shows the results of a simulation calculation of the waveguide loss when the film thickness of the transparent electrode member and the height of the ridge portion are changed. FIG. 3 shows the results of a simulation calculation of the waveguide loss when the film thickness of the transparent electrode member and the height of the ridge portion are changed.
[0007] There is a demand for increasing the output power of semiconductor laser devices without increasing their operating voltage, thereby achieving high efficiency. To meet this demand, the operating voltage of semiconductor laser devices can be reduced by thinning the p-side cladding layer. However, it is known that a trade-off exists: thinning the p-side cladding layer increases light absorption by the p-side electrode.
[0008] One way to resolve this trade-off is to use a transparent p-electrode, but transparent materials such as ITO (indium tin oxide) and ZnO generally have a relatively small work function, which increases the contact resistance with the p-side cladding layer.
[0009] It is known that using a material containing diffused impurities such as magnesium for the p-side electrode, which is a transparent electrode, reduces the resistance near the interface due to the impurity elements. However, adding impurities such as magnesium to the transparent electrode material increases the bulk resistance of the p-side electrode. Since an increase in the bulk resistance of the p-side electrode increases the operating voltage of the semiconductor laser device, in order to improve the efficiency of the semiconductor laser device, it is necessary to reduce the contact resistance between the p-side electrode and the p-side cladding layer without increasing the bulk resistance.
[0010] An object of the present disclosure is to provide a semiconductor laser element and a semiconductor laser device that can reduce the bulk resistance of a transparent p-side electrode and also the contact resistance between the p-side electrode and the p-side cladding layer.
[0011] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. However, more detailed explanations than necessary, such as detailed explanations of already well-known matters or redundant explanations of substantially identical configurations, may be omitted. Note that each of the embodiments described below is merely a specific example of the present disclosure, and the present disclosure is not limited to the numerical values, shapes, materials, components, and the arrangement and connection forms of the components shown in the following embodiments.
[0012] In the following embodiments, the drawings are schematic diagrams and are not necessarily strictly illustrated. Therefore, the scales and the like are not necessarily the same in the drawings. In addition, in the drawings, the same reference numerals are used for substantially the same components, and duplicated explanations are omitted or simplified.
[0013] In the following embodiments, the terms "above" and "below" do not refer to the upward direction (vertically upward) and downward direction (vertically downward) in absolute spatial recognition, but are used as terms defined by a relative positional relationship based on the stacking order in a stacked configuration. The terms "above" and "below" are used not only when two components are arranged with a gap between them and another component is present between them, but also when two components are arranged in contact with each other.
[0014] In the drawings shown in the following embodiments, the X-axis, Y-axis, and Z-axis represent three axes of a three-dimensional Cartesian coordinate system. The X-axis and Y-axis are perpendicular to each other and are also perpendicular to the Z-axis.
[0015] [Configuration of Semiconductor Laser Device] The configuration of a semiconductor laser device according to an embodiment of the present disclosure will be described with reference to FIGS. 1A and 1B. FIGS. 1A and 1B are schematic diagrams for explaining the configuration of a semiconductor laser device 1 according to an embodiment of the present disclosure. FIG. 1A shows a top view of the semiconductor laser device 1, and FIG. 1B shows a cross-sectional view of the semiconductor laser device 1. FIG. 1B shows a cross-section of the semiconductor laser device 1 taken along line IB-IB in FIG. 1A.
[0016] 1B , the semiconductor laser device 1 includes a substrate 10, a first semiconductor layer 20, a light-emitting layer 30, a second semiconductor layer 40, and a dielectric layer 60. The semiconductor laser device 1 further includes a transparent electrode member 50, a p-side electrode 70, and an n-side electrode 80.
[0017] The semiconductor laser device 1 forms a resonator having a front end face Cf and a rear end face Cr, and emits laser light from the front end face Cf.
[0018] In this embodiment, the substrate 10 is, for example, a gallium nitride (GaN) substrate. As an example, the substrate 10 is an n-type hexagonal GaN substrate whose main surface is a (0001) plane. The thickness of the substrate 10 may be set to a thickness that allows cleavage when the semiconductor laser devices 1 are separated into individual pieces, that is, for example, 50 μm or more and 130 μm or less. As an example, the thickness of the substrate 10 is 90 μm.
[0019] The first semiconductor layer 20 is a semiconductor layer of a first conductivity type disposed above the substrate 10. In this embodiment, the first semiconductor layer 20 includes a nitride semiconductor material. As an example, the first semiconductor layer 20 is an n-type AlN layer having a thickness of 3 μm. 0.03 Ga 0.97 The n-side cladding layer is made of N.
[0020] The thickness and Al composition of the first semiconductor layer 20 are not limited to the above examples. For example, the thickness of the first semiconductor layer 20 may be 0.5 μm or more and 5.0 μm or less. The first semiconductor layer 20 may be an n-type Al 0.03 Ga 0.97 It may also include an n-type semiconductor layer other than N.
[0021] The light emitting layer 30 is disposed above the first semiconductor layer 20. In this embodiment, the light emitting layer 30 contains a nitride semiconductor material. The light emitting layer 30 has a stacked structure including an n-side light guiding layer 31, an active layer 32, and a p-side light guiding layer 33.
[0022] The n-side optical guide layer 31 is made of n-type GaN with a thickness of, for example, 0.2 μm.
[0023] The active layer 32 is, for example, an In layer having a thickness of 5 nm. 0.06 Ga 0.94 The N quantum well layer is formed of 10 nm thick In 0.02 Ga 0.98 The active layer 32 has a structure in which a quantum well layer is sandwiched between N barrier layers. The active layer 32 has a structure in which, for example, two quantum well layers are sandwiched between barrier layers. The number of quantum well layers is not limited to two, but may be one, or three or more. The compositions and thicknesses of the quantum well layers and barrier layers included in the active layer 32 are not limited to the above-mentioned examples, and may be any composition and thickness that can emit light of, for example, 400 nm to 470 nm.
[0024] The p-side optical guide layer 33 is made of p-type GaN with a thickness of, for example, 0.1 μm.
[0025] The second semiconductor layer 40 is a semiconductor layer of a second conductivity type disposed above the light emitting layer 30. The second conductivity type of the second semiconductor layer 40 is a conductivity type different from the first conductivity type of the first semiconductor layer 20. In the present embodiment, the second semiconductor layer 40 contains a nitride semiconductor material. The second semiconductor layer 40 has a stacked structure including an electron barrier layer 41, a p-side cladding layer 42, and a p-side contact layer 43.
[0026] The electron barrier layer 41 is, for example, an Al layer having a thickness of 10 nm. 0.35 Ga 0.65 It is composed of N.
[0027] The p-side cladding layer 42 is, for example, a p-type Al layer having a thickness of 1.5 nm. 0.06 Ga 0.94 The p-side cladding layer 42 is a 0.20 μm-thick strained superlattice formed by stacking 66 periods of GaN and 1.5 nm-thick p-type GaN. The configuration of the p-side cladding layer 42 is not limited to this. The thickness of the p-side cladding layer 42 may be thinner than the thickness at which no light absorption occurs when a metal electrode is used as the p-side electrode, i.e., for example, 0.05 μm to 0.6 μm. By making the thickness of the p-side cladding layer 42 relatively thin, the bulk resistance of the p-side cladding layer 42 can be reduced, and the operating voltage of the semiconductor laser device 1 can be reduced.
[0028] The p-side cladding layer 42 is provided along the cavity length direction (i.e., the resonance direction of the laser light) and has a protrusion that protrudes upward. In the p-side cladding layer 42, flat portions 40b that are approximately flat are formed on both sides of the protrusion in the longitudinal direction.
[0029] The p-side contact layer 43 is made of p-type GaN and has a thickness of 0.05 μm. The p-side contact layer 43 is formed above the convex portion of the p-side cladding layer 42, but not above the flat portion 40 b. The convex portion of the p-side cladding layer 42 and the p-side contact layer 43 form a ridge-shaped ridge portion 40 a.
[0030] The width of the ridge portion 40 a is, for example, 1 μm to 100 μm, and when the semiconductor laser device 1 is operated at a high optical output (for example, in the watt class), the width of the ridge portion 40 a may be set to, for example, 10 μm to 50 μm.
[0031] The transparent electrode member 50 is disposed above the ridge portion 40a. The transparent electrode member 50 is an ohmic electrode that makes ohmic contact with the p-side contact layer 43, which is the layer above the ridge portion 40a. The width of the transparent electrode member 50 may be, for example, the same as or narrower than the ridge portion 40a. When the width of the transparent electrode member 50 is narrower than the width of the ridge portion 40a, the distribution of the current injected into the active layer 32 is adjusted, and the operating efficiency of the semiconductor laser device 1 can be improved.
[0032] The transparent electrode member 50 has a first transparent electrode member 51 and a second transparent electrode member 52. The first transparent electrode member 51 is formed in contact with the p-side contact layer 43, and the second transparent electrode member 52 is formed above the first transparent electrode member 51.
[0033] The transparent electrode member 50 is made of, for example, ITO, In 2 O 3 The first transparent electrode member 51 and the second transparent electrode member 52 may be made of the same material or different materials. In this embodiment, the first transparent electrode member 51 and the second transparent electrode member 52 are made of In 2 O 3 It is formed by
[0034] The first transparent electrode member 51 and the second transparent electrode member 52 contain magnesium as an impurity at different concentrations. For example, the magnesium concentration of the first transparent electrode member 51 is 1E19 atoms / cm 3 More than 1E21 atoms / cm 3 In order to further reduce the operating voltage of the semiconductor laser element 1, the magnesium concentration of the first transparent electrode member 51 is set to 2E19 atoms / cm 3 More than 3E20atoms / cm 3 More preferably, the magnesium concentration of the first transparent electrode member 51 may be set to 7E19 atoms / cm 3 More than 2E20atoms / cm 3 In this embodiment, the magnesium concentration of the first transparent electrode member 51 may be 9E19 atoms / cm 3 is.
[0035] The magnesium concentration of the second transparent electrode member 52 is set to be lower than the magnesium concentration of the first transparent electrode member 51. As an example, the magnesium concentration of the second transparent electrode member 52 is 1 / 10 or less of the magnesium concentration of the first transparent electrode member 51. Magnesium does not have to be added to the second transparent electrode member 52. In the present embodiment, the magnesium concentration of the second transparent electrode member 52 is 0 (no magnesium is added).
[0036] The thickness of the first transparent electrode member 51 is set to an appropriate thickness depending on the rated operating current density of the semiconductor laser device 1. The thickness of the second transparent electrode member 52 is set to an appropriate thickness in order to reduce the influence of light absorption by the p-side electrode 70. Details of the method for setting the thickness of the first transparent electrode member 51 and the method for setting the thickness of the second transparent electrode member 52 will be described later.
[0037] As described above, in the semiconductor laser device 1 according to this embodiment, the transparent electrode member 50 has a two-layer structure of the first transparent electrode member 51 and the second transparent electrode member 52, and magnesium is added to at least the first transparent electrode member 51 that is in contact with the p-side contact layer 43. The magnesium concentration of the second transparent electrode member 52 is set to be significantly lower than the magnesium concentration of the first transparent electrode member 51. The effects achieved by the semiconductor laser device 1 due to such a structure will be described in detail later.
[0038] The dielectric layer 60 is an insulating film continuously formed from the side surfaces of the ridge portion 40a and the transparent electrode member 50 to above the flat portion 40b. More specifically, the dielectric layer 60 is continuously formed around the ridge portion 40a and the transparent electrode member 50, over the side surfaces of the transparent electrode member 50, the side surfaces of the p-side contact layer 43, the side surfaces of the convex portions of the p-side cladding layer 42, and the upper surface of the p-side cladding layer 42. That is, the dielectric layer 60 is disposed to the side or above the second semiconductor layer 40. The dielectric layer 60 is formed so as to have a lower refractive index than the second semiconductor layer 40. The dielectric layer 60 confines light emitted from the light-emitting layer 30 within the ridge portion 40a and the transparent electrode member 50. In this embodiment, the dielectric layer 60 is formed of SiO2.
[0039] The shape of the dielectric layer 60 is not limited to the above example, and may be in contact with, for example, the side surfaces of the first transparent electrode member 51 and the second transparent electrode member 52 and part of the upper surface of the second transparent electrode member 52. Even with such a shape, it is possible to stably confine the light generated from the light-emitting layer 30 directly below the ridge portion 40 a.
[0040] 1A, the dielectric layer 60 is formed over the entire semiconductor laser device 1 when viewed from above. On the other hand, the p-side electrode 70 is formed inside the dielectric layer 60 when viewed from above. In other words, when viewed from above, the semiconductor laser device 1, the p-side electrode 70 is not formed on the peripheral edge of the semiconductor laser device 1. This allows the semiconductor laser device 1 to have a non-current injection region, to which no current is supplied, on the peripheral edge of the end, thereby improving the yield when the semiconductor laser device 1 is singulated.
[0041] When the semiconductor laser device 1 is operated at high power, a facet coating film such as a dielectric multilayer film may be formed on the front facet Cf shown in FIG. 1A . It is difficult to form such a facet coating film only on the facet, and the facet coating film may end up being formed on the upper surface of the semiconductor laser device 1 as well. In such a case, the p-side electrode 70 is not formed at the end of the semiconductor laser device 1 in the cavity length direction (the Y-axis direction in FIGS. 1A and 1B ). This causes the dielectric layer 60 and the facet coating film to come into contact with each other at the end of the semiconductor laser device 1 in the cavity length direction, and some of the light emitted from the light-emitting layer 30 may be lost due to the influence of the facet coating film.
[0042] To avoid this, in this embodiment, the thickness of the dielectric layer 60 is set to 100 nm or more. Note that if the thickness of the dielectric layer 60 is too thick, it becomes difficult to form the p-side electrode 70. Therefore, the thickness of the dielectric layer 60 may be set to a thickness equal to or less than the height of the ridge portion 40 a and the transparent electrode member 50.
[0043] Furthermore, as described above, the dielectric layer 60 is formed so as to cover the ridge portion 40 a and the flat portion 40 b. The ridge portion 40 a is formed, for example, by an etching process, and damage from the etching process may remain on the side surfaces of the ridge portion 40 a and on the flat portion 40 b. If etching damage remains on the ridge portion and the flat portion of a semiconductor laser element, leakage current may occur during operation of the semiconductor laser element. However, in this embodiment, the dielectric layer 60 completely covers the ridge portion 40 a and the flat portion 40 b, and therefore the occurrence of such unnecessary leakage current can be reduced.
[0044] The p-side electrode 70 is formed to be wider than the transparent electrode member 50 and is formed in contact with the dielectric layer 60. In other words, the p-side electrode 70 is formed so as to cover the transparent electrode member 50 and the dielectric layer 60. The p-side electrode 70 is formed using, for example, a metal material such as Ti, Ni, Pt, or Au. In this embodiment, the p-side electrode 70 has a three-layer structure of Ti / Pt / Au.
[0045] The n-side electrode 80 is an electrode disposed below the substrate 10. The n-side electrode 80 is an ohmic electrode that is in ohmic contact with the substrate 10. The n-side electrode 80 is, for example, a laminated film made of Ti / Pt / Au. Note that the configuration of the n-side electrode 80 is not limited thereto, and it may be, for example, a laminated film in which Ti and Au are laminated.
[0046] [Method for Manufacturing Semiconductor Laser Device 1] Next, a method for manufacturing the semiconductor laser device 1 shown in Figures 1A and 1B will be described with reference to Figures 2A to 4D. Figures 2A to 4D each show a schematic cross-sectional view illustrating each step in the method for manufacturing the semiconductor laser device 1 according to this embodiment.
[0047] First, as shown in FIG. 2A , a first semiconductor layer 20, a light-emitting layer 30, and a second semiconductor layer 40 are sequentially formed on a substrate 10, which is an n-type hexagonal GaN substrate whose main surface is a (0001) plane, by metalorganic chemical vapor deposition (MOCVD).
[0048] More specifically, the films are formed in the following order: First, an n-side cladding layer made of n-type AlGaN is grown to a thickness of 3 μm on a 400 μm-thick substrate 10 as the first semiconductor layer 20. Next, an n-side optical guide layer 31 made of n-type GaN is grown to a thickness of 0.2 μm. Next, an active layer 32 having a structure in which two periods of InGaN barrier layers and InGaN quantum well layers are stacked is grown. Next, a p-side optical guide layer 33 made of p-type GaN is grown to a thickness of 0.1 μm. Next, an electron barrier layer 41 made of AlGaN is grown to a thickness of 10 nm. Next, a p-side cladding layer 42 made of a strained superlattice structure having a thickness of approximately 0.2 μm is grown, which is composed of 66 periods of 1.5 nm-thick p-type AlGaN layers and 1.5 nm-thick GaN layers. Next, a p-side contact layer 43 made of p-type GaN is grown to a thickness of 0.01 μm.
[0049] In the growth of each layer, for example, trimethylindium (TMI) is used as an organic metal source for forming an indium film. For example, trimethylgallium (TMG) is used as an organic metal source for forming a gallium film. For example, trimethylaluminum (TMA) is used as an organic metal source for forming an aluminum film. Furthermore, ammonia (NH3) is used as a nitrogen source.
[0050] Next, as shown in FIG. 2B, a first protective film 91 is formed on the p-side contact layer 43. More specifically, a first protective film 91 is formed on the p-side contact layer 43 using silane (SiH 4 The first protective film 91 is formed by a plasma CVD (Chemical Vapor Deposition) method using a silicon oxide film (SiO 2 ) is deposited to a thickness of 300 nm. The material for forming the first protective film 91 is not limited to the above example, and may be, for example, a material such as a dielectric or a metal that has selectivity for etching the second semiconductor layer 40 described below. Furthermore, the method for forming the first protective film 91 is not limited to plasma CVD, and any known film formation method such as thermal CVD, sputtering, vacuum deposition, or pulsed laser film formation may be used.
[0051] 2C, the first protective film 91 is removed, leaving a predetermined shape. More specifically, a protective film made of photoresist is formed on the first protective film 91, and portions of the first protective film 91 are selectively removed using lithography and etching, followed by the removal of the protective film. The first protective film 91 is a film for forming the ridge portion 40a shown in FIGS. 1A and 1B, and the predetermined shape of the first protective film 91 corresponds to the shape of the ridge portion 40a.
[0052] As a lithography method for forming the first protective film 91, a photolithography method using a short wavelength light source, an electron beam lithography method for direct drawing with an electron beam, a nanoimprint method, etc. can be used. Furthermore, as an etching method for forming the first protective film 91, for example, a CF 4 Dry etching by reactive ion etching (RIE) using a fluorine-based gas such as fluorine, or wet etching using hydrofluoric acid (HF) diluted at a ratio of about 1:10 can be used. As a solvent for removing the protective film, for example, an organic solvent such as acetone can be used.
[0053] 2D , the p-side contact layer 43 and the p-side cladding layer 42 are etched using the first protective film 91 as a mask, thereby forming a ridge portion 40a and a flat portion 40b in the second semiconductor layer 40. More specifically, the regions of the p-side contact layer 43 and the p-side cladding layer 42 protected by the first protective film 91 are not etched, and the ridge portion 40a made of the p-side contact layer 43 and the p-side cladding layer 42 is formed. On the other hand, the p-side contact layer 43 and the p-side cladding layer 42 in the region where the first protective film 91 is not formed are removed by etching, thereby forming the flat portion 40b. The p-side contact layer 43 and the p-side cladding layer 42 are etched using, for example, Cl. 2 Dry etching by the RIE method using a chlorine-based gas such as HCl can be used.
[0054] Then, when the ridge portion 40a and the flat portion 40b are formed, the CF 4The first protective film 91 is removed by dry etching using reactive ion etching (RIE) with a fluorine-based gas such as fluorine-based fluoride or by wet etching with hydrofluoric acid (HF) diluted at a ratio of about 1:10.
[0055] Next, as shown in FIG. 3A, a second protective film 92 made of photoresist is formed on the p-side contact layer 43 and the flat portion 40b.
[0056] 3B, an opening is formed in the second protective film 92 above the p-side contact layer 43 by lithography. At this time, by forming the opening so that the cross section of the opening has an inverted mesa shape, the subsequent transparent electrode can be formed with high accuracy.
[0057] 3C, a first transparent electrode member 51 is formed to a thickness of 2 nm on the entire surface above the second protective film 92 and the p-side contact layer 43 by vacuum deposition or the like, and then a second transparent electrode member 52 is formed to a thickness of 200 nm. The method for forming the transparent electrode member 50 is not limited to vacuum deposition, but may also be sputtering or pulse laser deposition. The transparent electrode member 50 may be formed from a material such as ITO, In, or the like. 2 O 3 , ZnO, or the like, as long as it is in ohmic contact with the second semiconductor layer 40 (p-side contact layer 43).
[0058] When forming the transparent electrode member 50, magnesium is added to at least the first transparent electrode member 51. As a method for adding magnesium, In is used as a target material during film formation. 2 O 3 A method using a material made by sintering In and MgO is one example. 2 O 3 By controlling the ratio of In and MgO, the concentration of magnesium contained in the transparent electrode member 50 can be adjusted. 2 O 3A sintered material with a compounding ratio of 99:1 between SiO and MgO was used as a target material, and a 200 nm film was formed on a sapphire substrate for evaluation by vacuum deposition. The magnesium concentration in the film was analyzed by secondary ion mass spectrometry (SIMS), and found to be 9E19 atoms / cm 3 In having a magnesium concentration of 2 O 3 The method of adding magnesium is not limited to the above method, and for example, a transparent electrode material to which magnesium is added as an impurity element may be used.
[0059] Next, as shown in Fig. 3D, the second protective film 92 is removed using an organic solvent such as acetone. By using such a lift-off method, the transparent electrode member 50 can be formed only above the ridge portion 40a. In the example shown in Fig. 3D, the transparent electrode member 50 is formed with a width smaller than that of the ridge portion 40a, but by devising the photoresist shape in Fig. 3B, it is also possible to form a transparent electrode member 50 with the same width as the ridge portion 40a.
[0060] 4A, a dielectric layer 60 is formed on the transparent electrode member 50, the p-side contact layer 43, and the flat portion 40b. The dielectric layer 60 may be formed of, for example, silane (SiH 4 ) by the plasma CVD method using silicon oxide film (SiO 2 ) is deposited to a thickness of 300 nm.
[0061] Next, as shown in FIG. 4B, only the dielectric layer 60 on the transparent electrode member 50 is removed by, for example, photolithography and wet etching using hydrofluoric acid or the like, to expose the upper surface of the transparent electrode member 50.
[0062] 4C , a p-side electrode 70 is formed so as to cover the transparent electrode member 50 and the dielectric layer 60. More specifically, a negative resist is patterned according to the shape of the p-side electrode 70 by photolithography or the like, the p-side electrode 70 made of Ti / Pt / Au is formed on the entire surface above the substrate 10 by vacuum deposition or the like, and unnecessary portions of the electrode are removed by lift-off.
[0063] 4D , the substrate 10 is polished to adjust its thickness, and then an n-side electrode 80 is formed on the lower surface of the substrate 10 (the surface behind the main surface on which the first semiconductor layer 20 and the like are disposed). The thickness of the substrate 10 is, for example, approximately 90 μm. The n-side electrode 80 made of Ti / Pt / Au is formed by, for example, vacuum deposition. The shape of the n-side electrode 80 may be formed into a predetermined shape by patterning using photolithography, etching, or the like.
[0064] By the above manufacturing method, the semiconductor laser device 1 according to the present embodiment can be manufactured.
[0065] [Mounting of Semiconductor Laser Device 1] Next, a mounting of the semiconductor laser device 1 according to this embodiment will be described with reference to Figures 5A and 5B. Figure 5A shows a schematic top view of a semiconductor laser device 2 on which the semiconductor laser device 1 is mounted. Figure 5B shows a schematic cross-sectional view of the semiconductor laser device 2 on which the semiconductor laser device 1 is mounted. Figure 5B shows a cross-section of the semiconductor laser device 2 taken along line IIIb-IIIb in Figure 5A.
[0066] In this embodiment, the semiconductor laser device 2 includes the semiconductor laser element 1 and a submount 100, as shown in FIG. 5B.
[0067] The submount 100 includes a base 101, a first electrode 102a, a second electrode 102b, a first adhesive layer 103a, and a second adhesive layer 103b.
[0068] The base 101 is a base placed below the substrate 10 of the semiconductor laser element 1 and functions as a heat sink. The material of the base 101 is not particularly limited, but may be ceramic such as aluminum nitride (AlN) or silicon carbide (SiC), diamond (C) formed by CVD, a metal such as Cu or Al, or an alloy such as CuW. The material of the base 101 may be made of a material having the same or higher thermal conductivity as that of the semiconductor laser element 1.
[0069] 5A and 5B, the first electrode 102a is disposed on one surface of the base 101. The second electrode 102b is disposed on the other surface of the base 101. The first electrode 102a and the second electrode 102b are, for example, a laminated film made up of three metal films: a Ti film having a thickness of 0.1 μm, a Pt film having a thickness of 0.2 μm, and an Au film having a thickness of 0.2 μm.
[0070] The first adhesive layer 103a is disposed above the first electrode 102a. The second adhesive layer 103b is disposed below the second electrode 102b. The first adhesive layer 103a and the second adhesive layer 103b are, for example, eutectic solder (gold-tin solder) made of a gold-tin alloy containing 70% Au and 30% Sn, respectively.
[0071] 5B , the semiconductor laser element 1 is mounted in a manner (junction-down mounting) in which the p-side, i.e., the transparent electrode member 50 side, is connected to the submount 100. The p-side electrode 70 of the semiconductor laser element 1 is connected to the first adhesive layer 103 a of the submount 100.
[0072] When the semiconductor laser device 1 is mounted on the first adhesive layer 103a using gold-tin solder, a eutectic reaction occurs between the gold-tin solder and the gold of the p-side electrode 70 or the gold of the first electrode 102a, which may make it difficult to distinguish the boundary between the first adhesive layer 103a and the p-side electrode 70 or the first electrode 102a. In this case, the thickness of the first adhesive layer 103a may be defined as the distance from a layer (e.g., a Pt layer) that does not undergo a eutectic reaction with the gold-tin solder of the p-side electrode 70 to a layer (e.g., a Pt layer) that does not undergo a eutectic reaction with the gold-tin solder of the first electrode 102a.
[0073] A wire 110 is connected by wire bonding to the n-side electrode 80 of the semiconductor laser device 1 and the first electrode 102a of the submount 100. A current is supplied to the semiconductor laser device 1 through the wire 110.
[0074] Although not shown, the submount 100 may be mounted in a metal package such as a CAN package for the purpose of improving heat dissipation and simplifying handling. That is, the submount 100 may be adhered to the metal package by the second adhesive layer 103b. Note that the base 101 itself may function as the package. In this case, the submount 100 does not need to include the second adhesive layer 103b.
[0075] [Functions and Effects of Semiconductor Laser Device 1] As described above, in the semiconductor laser device 1 according to the embodiment of the present disclosure, the thickness of the p-side cladding layer 42 of the second semiconductor layer 40, which is the p-side semiconductor layer, is made relatively thin (for example, 0.05 μm to 0.6 μm) in order to achieve high efficiency. This reduces the bulk resistance of the p-side cladding layer 42, and allows the operating voltage of the entire semiconductor laser device 1 to be reduced.
[0076] Furthermore, in the semiconductor laser element 1 according to the embodiment of the present disclosure, by providing the transparent electrode member 50 between the p-side electrode 70 and the second semiconductor layer 40, it is possible to suppress light absorption by the p-side electrode 70 that occurs due to the reduction in the thickness of the second semiconductor layer 40.
[0077] Furthermore, in the semiconductor laser device 1 according to the embodiment of the present disclosure, the transparent electrode member 50 has at least two layers, a first transparent electrode member 51 and a second transparent electrode member 52. At least the first transparent electrode member 51 is doped with magnesium as an impurity. Magnesium may be doped in both the first transparent electrode member 51 and the second transparent electrode member 52. In this case, the magnesium concentration of the second transparent electrode member is lower than the magnesium concentration of the first transparent electrode member 51. More specifically, the magnesium concentration of the second transparent electrode member is 1 / 10 or less of the magnesium concentration of the first transparent electrode member 51. This makes it possible to suppress an increase in the bulk resistance of the transparent electrode member 50 due to the addition of magnesium, when viewed as a whole.
[0078] With this configuration, the bulk resistance of the transparent electrode member 50 can be reduced, so that the operating voltage of the entire semiconductor laser device 1 can be reduced, and thus a highly efficient semiconductor laser device 1 can be realized.
[0079] In the above-described embodiment, an example has been shown in which the transparent electrode member 50 is configured with two layers, the first transparent electrode member 51 and the second transparent electrode member 52, but the present disclosure is not limited to this. For example, the transparent electrode member may be configured with three or more transparent electrode members. In this case, the magnesium concentration contained in the bottommost transparent electrode member in contact with the p-side contact layer is set to be the highest, and the magnesium concentration contained in the transparent electrode member formed above it is set to be lower than that of the bottommost layer, thereby achieving the same effect as the above-described embodiment.
[0080] Below, the effects obtained by forming a transparent electrode member from a first transparent electrode member having a relatively high magnesium concentration and a second transparent electrode member having a lower magnesium concentration than the first transparent electrode member (or no magnesium is added) in the semiconductor laser element according to the present disclosure will be explained in more detail in comparison with a comparative example.
[0081] 6 is a diagram for explaining the effect obtained by configuring a transparent electrode member including a first transparent electrode member having a relatively high magnesium concentration and a second transparent electrode member having a lower magnesium concentration than the first transparent electrode member in the present disclosure, in comparison with a comparative example. Fig. 6 shows a graph plotting the results of measuring the voltage between a plurality of transparent electrode member patterns each having a rectangular shape in top view, which are arranged closely together on a second semiconductor layer.
[0082] 6, the circles indicate the results of measurements using a configuration corresponding to the present disclosure. The configuration corresponding to the present disclosure is a configuration in which a magnesium concentration of 9E19 atoms / cm is formed on an appropriate second semiconductor layer. 3 In 2 O 3 A 2-nm thick film of In was formed on top of it. 2 O 3The magnesium concentration is 9E19 atoms / cm 3 In 2 O 3 The layer corresponds to the first transparent electrode member of the semiconductor laser device according to the present disclosure, and is an In layer containing no magnesium. 2 O 3 The layer corresponds to the second transparent electrode member of the semiconductor laser device according to the present disclosure.
[0083] 6, the squares indicate the results of measurements using a comparative example of the present disclosure. The comparative example has a magnesium concentration of 9E19 atoms / cm 3 In 2 O 3 That is, the comparative example has a configuration consisting of only a layer of a transparent electrode member having a uniform magnesium concentration.
[0084] In the configurations used for the measurements in FIG. 6 (both the configuration corresponding to the present disclosure and the configuration of the comparative example), for simplicity, a ridge structure corresponding to the ridge portion 40 a of the semiconductor laser device 1 according to the embodiment of the present disclosure is not formed in the second semiconductor layer.
[0085] 6, in the low current region where the current value is 0.5 mA or less, the measurement results using the configuration according to the present disclosure and the measurement results using the configuration of the comparative example are almost the same voltage, whereas in the region where the current value is greater than 0.5 mA, the measurement results using the configuration according to the present disclosure are lower in voltage than the measurement results using the configuration of the comparative example. This is thought to be because the configuration according to the present disclosure has a two-layer structure consisting of a first transparent electrode member to which magnesium is added and a second transparent electrode member to which magnesium is not added, which makes it possible to keep the bulk resistance of the entire transparent electrode member lower than that of the comparative example.
[0086] From the above, it can be said that in the semiconductor laser element according to the present disclosure, the transparent electrode member has a two-layer structure of a first transparent electrode member and a second transparent electrode member, and the magnesium concentration of the second transparent electrode member is made lower than that of the first transparent electrode member, thereby realizing a reduction in the operating voltage of the entire semiconductor laser element.
[0087] [Method for Setting Thickness of First Transparent Electrode Member] As described above, in the configuration corresponding to the present disclosure in Fig. 6, the film thickness (2 nm) of the first transparent electrode member to which magnesium is added is set to be significantly thinner than the film thickness (200 nm) of the second transparent electrode member to which magnesium is not added. This is because, from the viewpoint of reducing the bulk resistance of the transparent electrode members, it is desirable to make the film thickness of the first transparent electrode member to which magnesium is added thinner.
[0088] However, if the thickness of the first transparent electrode member is too thin, the effect of reducing the contact resistance between the first transparent electrode member and the second semiconductor layer may not be sufficiently obtained. In consideration of these factors, in the semiconductor laser element according to the present disclosure, it is desirable to appropriately set the thickness of the first transparent electrode member to which magnesium is added.
[0089] Below, a description will be given of the verification carried out to appropriately set the film thickness of the first transparent electrode member in the semiconductor laser element according to the present disclosure and the results thereof.
[0090] Fig. 7 shows the results of an experiment measuring the voltage value at which the current flowing through the transparent electrode member is 0.5 mA when the film thickness of the first transparent electrode member is changed in the configuration corresponding to the present disclosure described in Fig. 6. The horizontal axis of Fig. 7 represents the film thickness of the first transparent electrode member, and the vertical axis represents the voltage value at which the current is 0.5 mA. In Fig. 7, a film thickness of 0 corresponds to a case where the layer of the second transparent electrode member and the second semiconductor layer (p-side contact layer) are in direct contact.
[0091] 7, it can be seen that increasing the film thickness of the first transparent electrode member reduces the voltage required to obtain the same current value. When the experimental results of FIG. 7 are expressed as an approximate formula Y=A×exp(−B×X)+C, A=0.16, B=0.50, and C=0.63 are obtained. According to FIG. 7, it can be said that the contact resistance can be sufficiently reduced by setting the film thickness of the first transparent electrode member containing magnesium to, for example, 1 nm or more, more preferably 5 nm or more.
[0092] Fig. 8 is a diagram showing the results of a simulation of the voltage value at which a current of 5 mA flows through the transparent electrode member when the film thickness of the first transparent electrode member layer is changed in the configuration corresponding to the present disclosure described in Fig. 6. In Fig. 8, the vertical axis shows the ratio (voltage ratio) of the voltage values required to obtain the same current value (5 mA) between the configuration corresponding to the present disclosure in Fig. 6 and the configuration of the comparative example.
[0093] 8, when the film thickness of the first transparent electrode member is 0 to 3 nm, the voltage ratio decreases as the film thickness increases. This is because the contact resistance between the first transparent electrode member and the p-side contact layer of the second semiconductor layer decreases as the film thickness increases.
[0094] 8, when the film thickness of the first transparent electrode member is 3 nm or more, the voltage ratio increases as the film thickness increases. This is thought to be because when the film thickness of the first transparent electrode member is 3 nm or more, the effect of increasing voltage due to an increase in bulk resistance becomes dominant over the effect of reducing voltage due to a decrease in contact resistance.
[0095] 8, when the film thickness of the first transparent electrode member is 0 to 9 nm, the voltage ratio is 1 or less, and it is clear that the voltage value required to obtain the same current value can be reduced compared to the comparative example configuration that does not include a transparent electrode member to which magnesium is added. On the other hand, when the film thickness of the first transparent electrode member layer is 9 nm or more, the effect of the increase in voltage due to the increase in bulk resistance of the first transparent electrode member becomes dominant.
[0096] 9 is a diagram showing the results of simulation calculations of the maximum film thickness of the first transparent electrode member layer at which the voltage ratio between the configuration according to the present disclosure and the configuration of the comparative example is 1 or less when the operating current density is changed. In FIG. 9, the horizontal axis represents the current density (kA / cm 2 ), and the vertical axis indicates the maximum film thickness at which the voltage ratio is 1 or less. The operating current of 5 mA shown in FIG. 8 corresponds to a current density of 3.2 kA / cm in FIG. 2 This corresponds to the point.
[0097] Here, if the maximum film thickness at which the voltage ratio is 1 or less is D and the operating current density is J, the calculation result in Fig. 9 is approximated by D = 29.3 × exp(-0.32 × J) (dashed line in Fig. 9). In other words, when the maximum film thickness D of the first transparent electrode member is in a range that satisfies D ≦ 29.3 × exp(-0.32 × J), it can be said that the configuration according to the present disclosure can reduce the operating voltage more than the configuration of the comparative example.
[0098] Thus, in the present disclosure, it is desirable to determine the film thickness of the first transparent electrode member according to the operating current density of the semiconductor laser element. For example, in order to operate the semiconductor laser element at a high optical output (e.g., in the watt class), the current density should be set to 3 kA / cm. 2 According to the calculation results in FIG. 9, the current density must be 3 kA / cm 2 The maximum film thickness that can be set to above this is approximately 11 nm. In order to further reduce the operating voltage, it is desirable that the film thickness of the first transparent electrode member be set to, for example, 1.5 nm or more and 5 nm or less.
[0099] [Method for Setting the Thickness of the Second Transparent Electrode Member] Next, the thickness of the second transparent electrode member having a lower magnesium concentration than the first transparent electrode member (or no magnesium added) in the semiconductor laser device according to the present disclosure will be described. The thickness of the second transparent electrode member is important for suppressing laser light absorption.
[0100] As described in the above embodiment, a p-side electrode is formed above the second transparent electrode member. In the present disclosure, by appropriately setting the thickness of the second transparent electrode member, the absorption of laser light emitted from the light-emitting layer by the p-side electrode is reduced.
[0101] 10A and 10B are diagrams for explaining the relationship between the thickness of the second transparent electrode member and the waveguide loss due to the p-side electrode. Fig. 10A is a cross-sectional view showing a simplified configuration of the second transparent electrode member and the p-side electrode periphery in a semiconductor laser element according to the present disclosure. Fig. 10A does not show the first transparent electrode member as part of the transparent electrode member.
[0102] Fig. 10B shows the results of simulation calculation of the waveguide loss α when the thickness H1 of the p-side cladding layer and the thickness H2 of the transparent electrode member are changed. Note that the thickness means the length of each member in the Z-axis direction. The waveguide loss is the attenuation rate of the optical energy when light propagates through the waveguide per unit length. In other words, I 0 Let be a constant and X be the distance from the reference point, then the light energy I(X) at any distance X is I(X) = I 0 ×exp(−α×X).
[0103] As explained below, the waveguide loss was calculated by approximating the three-dimensional ridge structure in contact with the transparent electrode member with a two-dimensional slab waveguide structure using the equivalent refractive index method. First, the light distribution in the stacking direction and the equivalent refractive index (i.e., effective refractive index) were calculated using the thickness and refractive index of each layer along the Z1-Z1 line in Figure 10A. Although details are omitted, the equivalent refractive index can be calculated by discretizing the two-dimensional scalar wave equation and solving the eigenvalue problem. Then, by expressing the refractive index as a complex number, the waveguide loss can be calculated from its imaginary part.
[0104] When the equivalent refractive index is ni and the waveguide loss is α, in the semiconductor laser device 1 according to the present embodiment described above, ni=2.493 and α=4.1 cm -1 The values of ni and α change depending on H1 and H2. Figure 10B shows the calculation results of α when H1 and H2 are changed.
[0105] 10B, the waveguide loss α increases when either H1 or H2 is small. This is thought to be because the smaller either H1 or H2 is, the greater the proportion of the light distribution that falls on the p-side electrode, and the greater the effect of light absorption by the p-side electrode.
[0106] As a result of investigation, when the semiconductor laser device according to the present disclosure is used in a high-output region where the optical output exceeds 1 watt, it is found that α is set to 10 cm -1 Less than 6cm, more preferably -1or less. According to the calculation results shown in FIG. 10B, it can be said that the waveguide loss α can be sufficiently reduced if H2 is set to 100 nm or more. More preferably, if H2 is set to 200 nm or more, the waveguide loss α can be kept at a substantially constant value, and even if the value of H2 is increased beyond this, the waveguide loss α hardly changes. This is because, if the thickness H2 of the transparent electrode member is large to a certain extent, the proportion of the light distribution that falls on the p-side electrode does not change.
[0107] Since the dependence of α on the thickness H1 of the p-side cladding layer and the thickness H2 of the transparent electrode member is complex, it is difficult to express all the calculation results in a single formula. -1 When they are in the vicinity, the relationship between α, H1, and H2 is given by the following equation (1).
[0108] α ≒ 2.5 × 10 -5 ×H1 2 -3.3 x 10 -2 ×H1+9.7×10 3 ×H2 (-1.9) +6.9 (1) Using equation (1), α = 6 cm -1 H1 and H2 that realize the above can be obtained.
[0109] In the above-described embodiment, the thickness H1 of the p-side cladding layer is set to, for example, 0.05 μm or more and 0.6 μm or less. According to the formula (1) and the calculation results shown in FIG. 10B, when H1 is 50 nm, for example, by setting H2 to 200 nm or less, the waveguide loss α≦6 cm -1 Furthermore, when H1 is 100 nm or more (for example, 200 nm), if H2 is 100 nm or more, the waveguide loss α≦6 cm -1 The following can be achieved: Since the film thickness of the transparent electrode member is adjusted by film formation, it is desirable that the tolerance for film thickness is wide.
[0110] As explained above, in the semiconductor laser device 1 according to the above-described embodiment (see, for example, FIGS. 1A and 1B ), the absorption of laser light by the p-side electrode 70 can be suitably suppressed by setting the thickness of the transparent electrode member 50 (the total thickness of the first transparent electrode member and the second transparent electrode member) to approximately 100 nm or more. When the transparent electrode member is fabricated by the lift-off method, if the film thickness is too thick, lift-off may not be possible, making patterning difficult. Considering the film thickness and shape of the resist, the total thickness of the first transparent electrode member and the second transparent electrode member may be set to 1000 nm or less, preferably 500 nm or less.
[0111] [Modifications, etc.] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments.
[0112] For example, in the above embodiment, magnesium is exemplified as an impurity to be added to the first transparent electrode member 51 and the second transparent electrode member 52. However, the present disclosure is not limited to this. For example, zinc, beryllium, or silicon may be added as an impurity to the first transparent electrode member 51 and the second transparent electrode member 52.
[0113] Furthermore, for example, in the above embodiment, the semiconductor laser element 1 is a nitride semiconductor laser element, but the semiconductor laser element according to the present disclosure is not limited to this. For example, the semiconductor laser element according to the present disclosure may be a semiconductor laser element made of a semiconductor other than a nitride semiconductor, such as a semiconductor laser element made of a gallium arsenide-based semiconductor material.
[0114] This disclosure also includes forms obtained by applying various modifications to the above-mentioned embodiments that a person skilled in the art would conceive, and forms realized by arbitrarily combining the components and functions of the above-mentioned embodiments within the scope of the present disclosure.
[0115] According to the present disclosure, the bulk resistance of the transparent p-side electrode can be reduced, and the contact resistance between the p-side electrode and the p-side cladding layer can also be reduced.
[0116] The semiconductor laser device according to the present disclosure can be used as a light source for image display devices, lighting, industrial equipment, etc., and is particularly useful as a light source for equipment requiring a relatively high optical output.
[0117] REFERENCE SIGNS LIST 1 semiconductor laser element 2 semiconductor laser device 10 substrate 20 first semiconductor layer 30 light emitting layer 31 n-side optical guide layer 32 active layer 33 p-side optical guide layer 40 second semiconductor layer 40a ridge portion 40b flat portion 41 electron barrier layer 42 p-side cladding layer 43 p-side contact layer 50 transparent electrode member 51 first transparent electrode member 52 second transparent electrode member 60 dielectric layer 70 p-side electrode 80 n-side electrode 91 first protective film 92 second protective film 100 submount 101 base 102a first electrode 102b second electrode 103a first adhesive layer 103b second adhesive layer 110 wire
Claims
1. A semiconductor laser device comprising: a substrate; a first semiconductor layer formed on the substrate; a light-emitting layer formed on the first semiconductor layer; a second semiconductor layer formed on the light-emitting layer, the second semiconductor layer having an upwardly protruding ridge portion; and a transparent electrode member formed above the ridge portion, the transparent electrode member comprising: a first transparent electrode member in contact with the second semiconductor layer and containing an added impurity at a first impurity concentration; and a second transparent electrode member containing the added impurity at a second impurity concentration lower than the first impurity concentration.
2. The semiconductor laser device according to claim 1, wherein the second impurity concentration is 1 / 10 or less of the first impurity concentration.
3. The semiconductor laser device according to claim 1, wherein the impurity is magnesium.
4. The semiconductor laser element according to claim 1, wherein the thickness of the first transparent electrode member is thinner than the thickness of the second transparent electrode member.
5. The semiconductor laser element according to claim 1, wherein the thickness D of the first transparent electrode member is expressed by the following formula (1): D≦29.3×exp(−0.32×J) (1), where J is the rated operating current density of the semiconductor laser element.
6. The semiconductor laser element according to claim 1, wherein the transparent electrode member has a film thickness of 100 nm or more.
7. The transparent electrode member is In 2 O 3 The semiconductor laser device according to claim 1 , comprising:
8. A semiconductor laser device comprising: a semiconductor laser element according to any one of claims 1 to 7; and a submount on which the semiconductor laser element is mounted.
Citation Information
Patent Citations
Semiconductor light emitting device and its manufacturing method
JP2004179365A
Reflecting electrode, and compound semiconductor light-emitting device having the same
JP2006074042A
Semiconductor laser element
JP2013038394A
Semiconductor laser element and manufacturing method of the same
JP2020126995A
Transparent Conductive Structure, Device comprising the same, and the Manufacturing Method thereof
US20140203322A1