Glass material and magneto-optic element
The glass material composition addresses thermal lens issues in magneto-optical devices by optimizing Tb2O3 and other oxides, reducing thermal lens effects and maintaining high light transmittance, thereby improving processing quality in magneto-optical elements.
Patent Information
- Application Number
- PCT/JP2024/018650
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
Magneto-optical devices experience deteriorated processing quality due to thermal lens effects caused by increased laser output, leading to changes in beam diameter and power density, which are not effectively mitigated by existing glass materials.
A glass material composition with specific ranges of Tb2O3, B2O3, Al2O3, SiO2, P2O5, FeO, and CeO2 is developed to minimize thermal lens effects, optimizing the Verdet constant and light transmittance, and incorporating FeO and Fe2O3 to reduce absorption and heat generation.
The glass material significantly reduces thermal lens effects, maintaining high light transmittance and stabilizing beam diameter, enhancing the performance of magneto-optical elements in devices like optical isolators and sensors.
Smart Images

Figure JP2024018650_05122024_PF_FP_ABST
Abstract
Description
Glass material and magneto-optical element
[0001] The present invention relates to a glass material and a magneto-optical element.
[0002] Paramagnetic glass materials are known to exhibit the Faraday effect, a magneto-optical effect. The Faraday effect rotates linearly polarized light passing through a material placed in a magnetic field. Magneto-optical elements utilizing this effect (e.g., Faraday rotators) are used in magneto-optical devices such as optical isolators.
[0003] Examples of paramagnetic glass materials include SiO 2 -B 2 O 3 -Al 2 O 3 -Tb 2 O 3 system (Patent Document 1), P 2 O 5 -B 2 O 3 -Tb 2 O 3 A system (Patent Document 2) is known.
[0004] Special Publication No. 51-46524 Publication No. 52-32881
[0005] In recent years, the output power of laser light irradiating magneto-optical devices has been increasing. This increase in laser output power raises the temperature of magneto-optical elements, which can easily cause changes in the laser beam diameter due to the thermal lens effect. Such beam diameter changes result in changes in power density, which can degrade the processing quality when used for processing, for example.
[0006] In view of the above, an object of the present invention is to provide a glass material and a magneto-optical element with reduced thermal lens effect.
[0007] Various aspects of the glass material and magneto-optical element that solve the above problems will be described below.
[0008] The glass material of embodiment 1 contains, in mol %, Tb 2 O 3 10% to 58%, B 2 O 3 +Al 2 O 3+SiO 2 +P 2 O 5 1% to 89%, FeO+Fe 2 O 3 Contains 0.01 ppm to 100 ppm, and CeO 2 It is characterized by containing more than 1% to 20%.
[0009] The glass material of embodiment 2 is the same as embodiment 1 except that, in mol %, B 2 O 3 0% to 70%, Al 2 O 3 0% to 70%, SiO 2 0% to 70%, P 2 O 5 It is preferable that the content is 0% to 20%.
[0010] The glass material of embodiment 3 is the same as embodiment 1 or embodiment 2, except that, in mol %, B 2 O 3 More than 12% to 40%, Al 2 O 3 1% to 20%, SiO 2 0% to 40%, P 2 O 5 It is preferable that the content is 0% to 5%.
[0011] The glass material of Aspect 4 is any one of Aspects 1 to 3, further comprising, in mol %, Pr 2 O 3 Less than 5%, Dy 2 O 3 It is preferable that it contains less than 5%.
[0012] The glass material of Aspect 5 is the glass material of any one of Aspects 1 to 4, wherein the ratio of Tb to total Tb is 3+ It is preferable that the ratio of is 55% or more.
[0013] The glass material of Aspect 6 is any one of Aspects 1 to 5, and preferably has a light transmittance of 80% or more at a wavelength of 1064 nm.
[0014] The magneto-optical element of the seventh aspect is characterized by using the glass material of any one of the first to sixth aspects.
[0015] According to the present invention, it is possible to provide a glass material and a magneto-optical element with a reduced thermal lens effect.
[0016] 1 is a schematic cross-sectional view showing one embodiment of an apparatus for producing a glass material of the present invention.
[0017] The glass material of the present invention contains, in mol %, Tb 2 O 3 10% to 58%, B 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 1% to 89%, FeO+Fe 2 O 3 Contains 0.01 ppm to 100 ppm, and further contains CeO 2 The present invention is characterized in that the content of CeO is more than 1% to 20%. 2 "Containing more than 1% to 20%" means, in mol%, CeO 2 CeO relative to the total content of the components other than 100% 2 is more than 1% to 20% (that is, the total amount is more than 101% to 120% in mole %).
[0018] The reasons for specifying the glass composition as described above and the content of each component are explained below. In the following explanation, "%" means "mol %" unless otherwise specified. Furthermore, in the following explanation, the "visible to near-infrared wavelength range" refers to the wavelength range used for visible to near-infrared lasers, and unless otherwise specified, refers to a wavelength range of 300 nm to 2000 nm, particularly 300 nm to 1100 nm.
[0019] Tb 2 O 3 is a component that increases the absolute value of the Verdet constant and enhances the Faraday effect. 2 O 3 The content of Tb is preferably 10% to 58%. 2 O 3The content of Tb is preferably 10% or more, 12% or more, 15% or more, 16% or more, 18% or more, 20% or more, 21% or more, 22% or more, 25% or more, and particularly preferably 26% or more, and is preferably 58% or less, 55% or less, 52% or less, 50% or less, 49% or less, 46% or less, 45% or less, 44% or less, 43% or less, 41% or less, and particularly preferably 40% or less. 2 O 3 If the content of Tb is too small, it becomes difficult to obtain the above-mentioned effects. 2 O 3 If the content is too high, vitrification becomes difficult. In addition, the light transmittance of the glass material is likely to decrease, and the beam diameter is likely to change due to the thermal lens effect. Note that Tb exists in the glass in a trivalent or tetravalent state, but in the present invention, all of these are considered to be Tb 2 O 3 It is expressed as:
[0020] Tb to total Tb 3+ The ratio of Tb to total Tb is preferably 55% or more, 60% or more, 70% or more, 80% or more, and particularly preferably 90% or more. 4+ The ratio of Tb can be reduced. 4+ has absorption in the wavelength range of 300 nm to 1100 nm, and the light transmittance of the glass material is likely to decrease. 3+ By setting the ratio of Tb to the above value, absorption of laser light in the visible to near-infrared wavelength range can be suppressed, and heat generation in the glass material can be easily suppressed. Therefore, the thermal lens effect can be easily suppressed. 3+ The upper limit of the ratio may be, for example, 100% or less.
[0021] FeO and Fe 2 O 3 is a component that reduces light transmittance in the visible to near-infrared wavelength range and is prone to cause a thermal lens effect. 2+ ) has a broad absorption peak at a wavelength of around 1200 nm. Therefore, the glass material absorbs laser light in the visible to near-infrared wavelength range, generating heat and easily causing a thermal lens effect. 2 O 3 (Fe 3+) does not cause the above absorption, and therefore can improve the light transmittance. 2 O 3 (Fe 3+ ) may be reduced to FeO during the melting process. Therefore, the glass material of the present invention is 2 O 3 Content of (FeO and Fe 2 O 3 The total amount of FeO and Fe is preferably 0.01 ppm to 100 ppm. 2 O 3 The content of FeO+Fe is preferably 0.01 ppm or more, 0.05 ppm or more, 0.1 ppm or more, 0.2 ppm or more, 0.3 ppm or more, 0.4 ppm or more, 0.5 ppm or more, particularly 1 ppm or more, and is preferably 100 ppm or less, 50 ppm or less, 30 ppm or less, 20 ppm or less, 15 ppm or less, 14 ppm or less, 13 ppm or less, 11 ppm or less, 10 ppm or less, 9 ppm or less, 8 ppm or less, particularly 5 ppm or less. 2 O 3 If the content is too low, the production cost tends to increase.
[0022] CeO 2 is also a component that suppresses changes in beam diameter due to the thermal lens effect. 2 The content (addition amount) of CeO is preferably more than 1% to 20% in terms of mole percent. 2 The content (addition amount) of CeO is preferably more than 1%, 1.1% or more, 1.2% or more, 1.5% or more, particularly 2% or more, and is preferably 20% or less, 19% or less, 15% or less, particularly 10% or less. 2 If the amount of CeO added is too small, it becomes difficult to obtain the above-mentioned effects. 2 If the amount of added is too large, the light transmittance of the glass material is likely to decrease.
[0023] As described above, the glass material of the present invention contains FeO and Fe, which tend to reduce light transmittance and cause the thermal lens effect. 2 O 3 Even if it contains CeO 2As a result of containing as an essential component, the decrease in light transmittance of the glass material in the visible to near-infrared wavelength range can be suppressed, and laser light absorption can be reduced. As a result, the glass material of the present invention can reduce the thermal lens effect.
[0024] B 2 O 3 , Al 2 O 3 , SiO 2 , P 2 O 5 is a component that forms the glass framework, widens the vitrification range, and stabilizes vitrification. 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 The content of (B 2 O 3 , Al 2 O 3 , SiO 2 , P 2 O 5 The total amount of B is preferably 1% to 89%. 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 The content of is preferably 1% or more, 5% or more, 10% or more, 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, particularly 48% or more, and is preferably 89% or less, 85% or less, 80% or less, 75% or less, particularly 70% or less. 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 If the content is too low, vitrification becomes difficult. 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5If the content of each component is too high, it becomes difficult to obtain a sufficient Faraday effect. The preferred ranges of each component are as follows:
[0025] B 2 O 3 The content of B is preferably 0% to 70%. 2 O 3 The content of is preferably 0% or more, 1% or more, 5% or more, 10% or more, particularly preferably more than 12%, and is preferably 70% or less, 67% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, particularly preferably 40% or less.
[0026] Al 2 O 3 The content of Al is preferably 0% to 70%. 2 O 3 The content is preferably 0% or more, 1% or more, particularly preferably 2% or more, and is preferably 70% or less, 67% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, particularly preferably 20% or less.
[0027] SiO 2 The content of is preferably 0% to 70%. More specifically, SiO 2 The content is preferably 0% or more, 1% or more, 5% or more, particularly preferably 10% or more, and is preferably 70% or less, 67% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, particularly preferably 40% or less.
[0028] P 2 O 5 The content of P is preferably 0% to 20%. 2 O 5 The content is preferably 0% or more, 1% or more, particularly preferably 2% or more, and is preferably 20% or less, 15% or less, 10% or less, particularly preferably 5% or less.
[0029] In addition to the above components, the glass material of the present invention may contain the following components.
[0030] GeO 2is a component that forms a glass skeleton, widens the vitrification range, and stabilizes vitrification. 2 The content of is preferably 0% to 60%. More specifically, GeO 2 The content of GeO is preferably 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, and particularly preferably 35% or less. 2 If the content is too high, it becomes difficult to obtain a sufficient Faraday effect. 2 The lower limit of the content may be, for example, 0% or more, particularly 1% or more.
[0031] ZnO is a component that stabilizes vitrification. The ZnO content is preferably 0% to 20%. More specifically, the ZnO content is preferably 20% or less, 15% or less, 13% or less, 10% or less, 8% or less, and particularly preferably 5% or less. If the ZnO content is too high, devitrification tends to occur. Furthermore, it becomes difficult to obtain a sufficient Faraday effect. From the viewpoint of stabilizing vitrification, the ZnO content may be 0% or more, particularly 1% or more.
[0032] La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 is a component that stabilizes vitrification. 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 The contents of La and La are preferably 10% or less, 7% or less, 5% or less, 4% or less, 2% or less, and particularly preferably 1% or less. If the contents of these components are too high, vitrification becomes more difficult. 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3The lower limit of the content of each of may be, for example, 0% or more, particularly 0.1% or more.
[0033] Pr 2 O 3 and Dy 2 O 3 has optical absorption in the visible to near-infrared wavelength range. 2 O 3 and Dy 2 O 3 The contents of these components are preferably less than 5%, 4% or less, 3% or less, 2% or less, 1% or less, 500 ppm or less, and particularly preferably 100 ppm or less. If the contents of these components are too high, the light transmittance in the visible to near-infrared wavelength range tends to decrease. Note that Pr and Dy exist in the glass in a trivalent or tetravalent state, but in the present invention, these are referred to as Pr 2 O 3 or Dy 2 O 3 It is expressed as: Pr 2 O 3 and Dy 2 O 3 The lower limit of the content of each of these may be, for example, 0% or more, particularly 0.001 ppm or more.
[0034] EU 2 O 3 and Sm 2 O 3 has optical absorption in the visible to near-infrared wavelength range. 2 O 3 and Sm 2 O 3 The content of each of these components is preferably less than 5%, 3% or less, 2% or less, 1% or less, 500 ppm or less, and particularly preferably 100 ppm or less. If the content of these components is too high, the light transmittance in the visible to near-infrared wavelength range tends to decrease. Note that Eu and Sm exist in the glass in a divalent or trivalent state, but in the present invention, these are respectively referred to as Eu and Sm. 2 O 3 or Sm 2 O 3 It is expressed as: Eu 2 O 3 and Sm 2 O 3The lower limit of the content of each of may be, for example, 0.001 ppm or more.
[0035] MgO, CaO, SrO, and BaO are components that stabilize vitrification and tend to increase chemical durability. The contents of MgO, CaO, SrO, and BaO are each preferably 10% or less, particularly 5% or less. If the contents of these components are too high, it becomes difficult to obtain a sufficient Faraday effect. The lower limits of the contents of MgO, CaO, SrO, and BaO may be, for example, 0% or more, particularly 1% or more.
[0036] Ga 2 O 3 is a component that stabilizes vitrification and also easily widens the vitrification range. 2 O 3 The content of is preferably 0% to 6%. More specifically, Ga 2 O 3 The content of Ga is preferably 6% or less, 5% or less, 4% or less, particularly preferably 2% or less. 2 O 3 If the content of Ga is too high, devitrification tends to occur. In addition, it becomes difficult to obtain a sufficient Faraday effect. 2 O 3 The lower limit of the content may be, for example, 0% or more, particularly 1% or more.
[0037] Fluorine is a component that enhances glass-forming ability and easily widens the vitrification range. 2 The fluorine content (calculated as 0% to 10%) is preferably 0% to 10%. More specifically, the fluorine content is preferably 10% or less, 7% or less, 5% or less, 3% or less, 2% or less, and particularly preferably 1% or less. If the fluorine content is too high, the components may volatilize during melting, which may adversely affect vitrification. Also, striae may be more likely to occur. The lower limit of the fluorine content may be, for example, 0% or more, particularly 0.1% or more.
[0038] The glass material preferably has a light transmittance of 80% or more, 82% or more, particularly 83% or more at a wavelength of 1064 nm. Furthermore, at a wavelength of 633 nm, the light transmittance is preferably 60% or more, 65% or more, 70% or more, particularly 75% or more. Furthermore, at a wavelength of 532 nm, the light transmittance is preferably 30% or more, 50% or more, 60% or more, particularly 70% or more. High light transmittance in the above wavelength ranges suppresses heat generation in the magneto-optical element due to light absorption and makes it easier to suppress changes in beam diameter due to the thermal lens effect. The above light transmittances are values when the glass material has a thickness of 1 mm. Furthermore, the upper limit of the light transmittance at each of the above wavelengths may be, for example, 100% or less, particularly 99% or less.
[0039] The glass material of the present invention, having the above-described configuration, can increase light transmittance and suppress beam diameter change. For example, the beam diameter change rate can be suppressed to 30% or less, 25% or less, 20% or less, and particularly 15% or less. The beam diameter change rate can be measured, for example, as follows. First, a glass sample processed to a thickness of 3 mm is irradiated with laser light having a wavelength of 1064 nm and an output of 50 W, with a beam diameter of φ1 mm, and the size of the beam diameter at a position 300 mm from the sample is measured. The beam diameter can be, for example, 1 / e 2 Next, the beam diameter change rate when the output is increased to 50 W can be calculated using the beam diameter at an output of 10 mW as a reference. If the beam diameter changes due to the thermal lens effect of the collimator lens even when there is no sample, the beam diameter change rate can be calculated by subtracting the beam diameter change rate when there is no sample from the measured beam diameter change rate.
[0040] The Verdet constant of the glass material of the present invention at a wavelength of 1064 nm is preferably 0.01 min / Oe cm or more, particularly 0.02 min / Oe cm or more. Glass materials having the above Verdet constant are suitable for use in magneto-optical elements. The upper limit of the Verdet constant at a wavelength of 1064 nm may be, for example, less than 0.5 min / Oe cm, 0.4 min / Oe cm or less, particularly 0.3 min / Oe cm or less. The Verdet constant refers to a value measured using a rotating analyzer method.
[0041] The glass material of the present invention can be suitably used for magneto-optical elements (for example, Faraday rotators) that constitute magnetic devices such as optical isolators, optical circulators, and magnetic sensors.
[0042] The glass material of the present invention can be produced, for example, by a containerless levitation method. Figure 1 is a schematic cross-sectional view showing one embodiment of an apparatus for producing the glass material of the present invention. Hereinafter, the method for producing the glass material of the present invention will be described with reference to Figure 1.
[0043] The glass material manufacturing apparatus 1 has a molding die 10. The molding die 10 also serves as a melting container. The molding die 10 has a molding surface 10a and a plurality of gas ejection holes 10b opening in the molding surface 10a. The gas ejection holes 10b are connected to a gas supply mechanism 11 such as a gas cylinder. Gas is supplied from the gas supply mechanism 11 to the molding surface 10a via the gas ejection holes 10b. The type of gas is not particularly limited, and may be, for example, air or oxygen, or a reducing gas containing nitrogen gas, argon gas, helium gas, carbon monoxide gas, carbon dioxide gas, or hydrogen. Among these, it is preferable to use an inert gas from the viewpoint of suppressing oxidation of the glass material and from the viewpoint of safety.
[0044] A glass material can be manufactured using the glass material manufacturing apparatus 1 as follows. First, glass raw material lump 12 is placed on the molding surface 10a. Examples of the glass raw material lump 12 include a lump obtained by integrating raw material powders by press molding or the like, a sintered body obtained by integrating raw material powders by press molding or the like and then sintering, and an aggregate of crystals having a composition equivalent to a target glass composition.
[0045] Next, gas is ejected from the gas ejection holes 10b to levitate the frit lump 12 above the molding surface 10a. That is, the frit lump 12 is held in a state where it is not in contact with the molding surface 10a. In this state, a laser beam is irradiated onto the frit lump 12 from the laser beam irradiation device 13. This heats and melts the frit lump 12, vitrifying it to obtain molten glass. The molten glass is then cooled to obtain a glass material. At this time, the molten glass and the glass material are cooled until the temperatures thereof are at least below their softening points. During the process of heating and melting the frit lump 12 and the process of cooling the molten glass and the glass material until the temperatures thereof are at least below their softening points, it is preferable to continue ejecting gas at least to prevent contact between the frit lump 12, the molten glass, and even the glass material and the molding surface 10a. The frit lump 12 may also be levitated above the molding surface 10a by utilizing magnetic force generated by applying a magnetic field. In addition to the method of irradiating laser beams, the frit lump 12 may also be heated and melted by radiant heating or the like.
[0046] The method for producing the glass material of the present invention is not limited to the containerless levitation method described above. For example, the glass material of the present invention may be produced by crucible melting. In the case of crucible melting, a large amount of raw material powder can be melted at once, making it easier to obtain a large glass material. The large glass material can be suitably used for high-power laser applications, etc.
[0047] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0048] Tables 1 to 3 show Examples 1 to 17 of the present invention and Comparative Examples 1 and 2.
[0049]
[0050]
[0051]
[0052] Each sample was prepared as follows: First, raw materials were mixed to obtain the glass compositions shown in Tables 1 to 3, and then press-molded. The press-molded raw materials were sintered at 800°C for 5 hours to prepare glass raw material blocks.
[0053] Next, the glass raw material lump was roughly crushed in a mortar to obtain small pieces of 1 g. Next, using the small pieces of the glass raw material lump and an apparatus similar to that shown in Figure 1, a glass material (diameter: approximately 9 mm) was produced by a containerless levitation method. The heat source was a 100 W CO 2 A laser oscillator was used. Nitrogen gas was used as the gas for suspending the glass raw material mass in the air, and the supply flow rate was set to 1 to 30 L / min. The obtained glass material was 4%-H 2 / N 2 After annealing at 770°C for 6 hours in a sintered atmosphere, the following measurements were carried out. The results are shown in Tables 1 to 3. In Examples 1 to 17, CeO 2 When the total amount of all components including Tb is converted to 100 mol%, the 2 O 3 12.6% to 51%, B 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 47.1% to 71.4%, CeO 2 1.1% to 16.7%, FeO+Fe 2 O 3 A glass material containing 0.1 ppm to 4.9 ppm of B was obtained. 2 O 3 , Al 2 O 3 , SiO 2 and P 2 O 5 The content of each is B 2 O 3 0%~58.3%, Al 2 O 3 0% to 60.2%, SiO 2 0% to 61.8%, P 2 O 5 It ranged from 0% to 9.2%.
[0054] The Verdet constant was measured using a rotating analyzer method. Specifically, the glass material was polished to a thickness of 1 mm, and the Faraday rotation angle was measured in a wavelength range of 500 nm to 1100 nm in a magnetic field of 10 kOe, and the Verdet constant at a wavelength of 1064 nm was calculated.
[0055] The light transmittance was measured using a spectrophotometer (V-670 manufactured by JASCO Corporation). Specifically, the obtained glass material was polished to a thickness of 1 mm, and the light transmittance at a wavelength of 1064 nm was read from the light transmittance curve. The light transmittance is the external transmittance including reflection.
[0056] Tb to total Tb 3+ The ratio of Tb to total Tb was measured by X-ray absorption fine structure (XAFS). Specifically, a spectrum of X-ray absorption near edge structure (XANES) was obtained, and the ratio of Tb to total Tb was calculated from the shift of the peak position of each Tb ion. 3+ The ratio (mol %) of
[0057] The beam diameter change rate was measured as follows. First, a laser beam with a wavelength of 1064 nm and an output of 50 W was irradiated onto a glass sample processed to a thickness of 3 mm with a beam diameter of 1 mm, and the size of the beam diameter was measured at a position 300 mm from the sample. The beam diameter was 1 / e 2 Next, the beam diameter change rate when the output was increased to 50 W was calculated based on the beam diameter at an output of 10 mW. Note that even when there was no sample, a change in the beam diameter was observed due to the thermal lens effect of the collimator lens, so the value obtained by subtracting the amount of change in the beam diameter when there was no sample from the measured beam diameter change rate was used as the beam diameter change rate.
[0058] As shown in Tables 1 to 3, the glass materials of Examples 1 to 17 had absolute values of the Verdet constant ranging from 0.027 to 0.215 at a wavelength of 1064 nm. Furthermore, the light transmittance at a wavelength of 1064 nm was 82.2% or more, and the beam diameter change rate was low, at 15% or less.
[0059] On the other hand, the glass materials of Comparative Examples 1 and 2 had a light transmittance of 79.5% or less and a beam diameter change rate of 33% or more.
[0060] The glass material of the present invention can be suitably used for magneto-optical elements (for example, Faraday rotators) that constitute magnetic devices such as optical isolators, optical circulators, and magnetic sensors.
[0061] REFERENCE SIGNS LIST 1 Glass material manufacturing apparatus 10 Mold 10a Mold surface 10b Gas ejection hole 11 Gas supply mechanism 12 Glass raw material lump 13 Laser light irradiation device
Claims
1. Tb in mole percent 2 O 3 10% to 58%, B 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 1% to 89%, FeO+Fe 2 O 3 Contains 0.01 ppm to 100 ppm, and further contains CeO 2 A glass material containing more than 1% to 20%.
2. B in mole percent 2 O 3 0% to 70%, Al 2 O 3 0% to 70%, SiO 2 0% to 70%, P 2 O 5 The glass material according to claim 1, containing 0% to 20%.
3. B in mole percent 2 O 3 More than 12% to 40%, Al 2 O 3 1% to 20%, SiO 2 0% to 40%, P 2 O 5 The glass material according to claim 1, containing 0% to 5%.
4. Pr in mole percent 2 O 3 Less than 5%, Dy 2 O 3 The glass material according to any one of claims 1 to 3, containing less than 5%.
5. Tb to total Tb 3+ The glass material according to any one of claims 1 to 3, wherein the proportion of 6. The glass material according to any one of claims 1 to 3, which has a light transmittance of 80% or more at a wavelength of 1064 nm.
7. A magneto-optical element using the glass material according to any one of claims 1 to 3.
Citation Information
Patent Citations
Imonozunanoshiwakesochi
JP1976046524A
Continuous crystallization equipment
JP1977032881A
Single mode optical fiber having faraday rotation effect
JP1987158135A
Method for manufacturing glass material
JP2022100192A
Faraday rotator and magneto-optic element
WO2019239684A1