Polypropylene-based resin foam particle molded body and polypropylene-based resin foam particle

By incorporating talc on the surface of foamed polypropylene resin particles, the charging performance and mechanical properties of polypropylene resin foam particles are enhanced, addressing the poor insulation and charging issues in conventional technologies, and enabling effective use in charging-related applications.

WO2024247858A1PCT designated stage expired Publication Date: 2024-12-05JSP CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018917
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional expanded particle molded bodies obtained by in-mold molding of expanded particles containing carbon exhibit poor insulation properties, making it difficult to develop charging performance, particularly for colored expanded particle molded bodies which struggle to exhibit sufficient charging performance compared to uncolored ones.

Method used

The introduction of talc on the surface of foamed polypropylene resin particles, with a specific amount ranging from 500 to 9000 mass ppm, ensures effective charging performance by maintaining a charged state over time and improving mechanical properties such as tensile strength and fusion rate, while also allowing for in-mold molding of polypropylene resin foam particles.

Benefits of technology

The presence of talc on the surface of the foamed particles enhances the charging voltage attenuation rate, maintains a charged state, and improves mechanical properties like tensile strength and fusion rate, enabling the use of polypropylene resin foam particles in various applications utilizing charging phenomena.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018917_05122024_PF_FP_ABST
    Figure JP2024018917_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a polypropylene-based resin foam particle molded body that exhibits sufficient charging performance despite comprising polypropylene-based resin foam particles containing a carbon material. This polypropylene-based resin foam particle molded body contains a carbon material. Talc is present at a surface section of the foam particle molded body. An initial electrification voltage V0 at an applied voltage of +10 kV and an electrification voltage V120 120 seconds after the applied voltage is stopped, which are measured on the basis of JIS L1094:2014 A, satisfy formula (1). Formula (1): (V0-V120)×100 / V0≤25(%)
Need to check novelty before this filing date? Find Prior Art

Description

Polypropylene resin expanded bead molded body and polypropylene resin expanded bead

[0001] The present invention relates to a molded article of expanded polypropylene resin beads and expanded polypropylene resin beads.

[0002] Expanded polypropylene resin beads molded by molding expanded polypropylene resin beads in a mold are used for various purposes such as packaging cushioning materials, automobile parts, building materials, etc. Depending on the application of the expanded polypropylene resin beads molded, additives such as colorants, conductivity imparting agents, antibacterial agents, antistatic agents, etc. are blended into the expanded polypropylene resin beads.

[0003] In addition, since the polypropylene resin itself is insulating, when an electric charge is generated on the surface of the molded article due to friction with other substances, the molded article maintains a statically charged state for a long time. Furthermore, even when the polypropylene resin molded article is in contact with a metal conductor, the molded article maintains a charged state if the metal conductor is insulated by being surrounded by an insulator.

[0004] Utilizing the charged state of a substance, i.e., the charging phenomenon, is widely used in industry, for example, in air filters, air purifiers, photosensitive drums of copy machines, electrets in acoustic elements, electrostatic sorting of plastics, electrostatic flocking, electrostatic painting, etc.

[0005] On the other hand, expanded bead moldings made of black or gray expanded polypropylene resin beads containing a coloring pigment such as carbon black (Patent Document 1) are known. These expanded bead moldings are expected to be used from various perspectives, such as for separation from expanded polystyrene resin beads, for improving appearance against stains, and for improving appearance when using colored recycled raw materials. Furthermore, these expanded bead moldings have excellent light-blocking properties, weather resistance, and design properties.

[0006] Japanese Patent Application Publication No. 7-300537

[0007] The present inventors have attempted to charge the colored foamed bead moldings in order to apply them to various applications that utilize the charging phenomenon, but have found that it is more difficult to make the colored foamed bead moldings exhibit charging properties than uncolored foamed bead moldings.

[0008] The present invention has been made in view of the above background, and an object of the present invention is to provide a polypropylene-based resin expanded bead molding that exhibits sufficient electrostatic charging performance despite being made of expanded polypropylene-based resin beads containing carbons. Another object of the present invention is to provide a polypropylene-based resin expanded bead molding that can be obtained by in-mold molding.

[0009] [1] A polypropylene resin foamed bead molding containing carbons, wherein talc is present on the surface of the foamed bead molding, and the initial electrification voltage V when a +10 kV voltage is applied is measured according to JIS L1094:2014 A method. 0 and the charged voltage V 120 seconds after the application was stopped 120 and a polypropylene resin expanded bead molding, characterized in that the following formula (1) is satisfied: (V 0 -V 120 ) x 100 / V 0 [2] The expanded polypropylene resin bead molding according to the above [1], wherein the amount of talc present in the surface portion of the expanded bead molding is 500 ppm by mass or more and 9000 ppm by mass or less. [3] The expanded bead molding has a molding density of 15 kg / m 3 More than 300kg / m 3

[0013] The expanded polypropylene-based resin bead molding according to [1] or [2], wherein the fusion rate of the expanded bead molding is 80% or more and the fusion rate of the expanded bead molding is 80% or more. [4] Expanded polypropylene-based resin beads containing carbons, characterized in that talc is present in the surface portion of the expanded beads, and the amount of talc present in the surface portion of the expanded beads is 600 ppm by mass or more and 10,000 ppm by mass or less. [5] The expanded polypropylene-based resin beads according to [4], wherein the expanded beads are multi-layered expanded beads having a polypropylene-based resin expanded core layer and a coating layer covering the foamed core layer, and at least the coating layer contains carbons.

[0010] According to the present invention, there is provided an expanded polypropylene resin bead molding containing carbons exhibiting good electrostatic chargeability. Furthermore, there is also provided expanded polypropylene resin beads that can be obtained by in-mold molding. The expanded polypropylene resin bead molding of the present invention is expected to be useful in a variety of applications that utilize its electrostatic chargeability.

[0011] Fig. 1 is an explanatory diagram showing the state of talc in single-layer expanded beads. Fig. 2 is an explanatory diagram showing other states of talc in single-layer expanded beads. Fig. 3 is an explanatory diagram showing other states of talc in multi-layer expanded beads. Fig. 4 is an explanatory diagram showing other states of talc in multi-layer expanded beads.

[0012] The expanded polypropylene resin bead molding of the present invention and the expanded polypropylene resin beads from which the expanded bead molding can be formed in a mold are described in detail below. In this specification, the expanded polypropylene resin beads are sometimes referred to as "expanded beads," and the expanded polypropylene resin bead molding is sometimes referred to as "molded article, expanded bead molding."

[0013] In this specification, when multiple types of numerical ranges are defined as numerical values ​​for "items defined using numerical values ​​(referred to as numerically defined items (NM)") such as numerical values ​​corresponding to specific attributes or amounts of addition, for each numerically defined item (NM), the upper limit and lower limit values ​​in the combinations defining each numerical range may be independently combined in any combination. In this specification, a combination defining a numerical range refers to a combination of an upper limit and a lower limit value. Note that a numerical range defined by any combination of an upper limit and a lower limit value includes the upper limit value, the lower limit value, and values ​​between the upper limit value and the lower limit value (i.e., the numerical range is equal to or greater than the lower limit value and equal to or less than the upper limit value). For example, when a target numerically defined item (NM) (particular When the numerical value for a specific compound (such as density or amount of a specific compound) is between MA1 and MB1, preferably between MA2 and MB2, and more preferably between MA3 and MB3, the lower limit of the target numerical specification item (NM) may be any value (selected lower limit) selected from the group consisting of MA1, MA2, and MA3 (a group refers to a collection of multiple elements (a set of numerical values, etc.)), and the upper limit of the target numerical specification item (NM) may be any value (selected upper limit) selected from the group consisting of MB1, MB2, and MB3. Furthermore, the numerical range of the target numerical specification item (NM) may be a numerical range (selected numerical range) that is between the "selected lower limit" and the "selected upper limit." Note that MA1, MA2, MA3, MB1, MB2, and MB3 represent numerical values.

[0014] Furthermore, unless otherwise specified, even when different numerically prescribed items (NM) are combined, the upper limit value of each numerically prescribed item (NM) may be individually set as the "selected upper limit value." This also applies to the lower limit value and numerical range of the numerically prescribed item (NM).

[0015] (Expanded Bead Molding) The expanded bead molding of the present invention is an in-mold molded product of expanded polypropylene resin beads containing carbons, and talc is present on the surface of the expanded bead molding. Furthermore, the expanded bead molding has an initial electrification voltage V of 10 kV applied voltage measured according to JIS L1094:2014 A method. 0and the charged voltage V 120 seconds after the application was stopped 120 The feature of the present invention is that even if the molded article is made of expanded polypropylene resin beads containing carbons, the presence of talc on the surface of the molded article gives it electrostatic properties to the extent that the following formula (1) is satisfied. (V 0 -V 120 ) x 100 / V 0 ≦ 25% (1)

[0016] The numerical value (V 0 -V 120 ) x 100 / V 0 The electrostatic voltage decay rate (value determined by the formula) is sometimes referred to as the electrostatic voltage decay rate. When the electrostatic voltage decay rate is within the above range, the foamed bead molded article has the property of maintaining a charged state for a long period of time. The electrostatic voltage decay rate is preferably 20% or less, more preferably 15% or less, even more preferably 10% or less, and most preferably 5% or less. The lower the lower limit of the electrostatic voltage decay rate, the better. The lower limit of the electrostatic voltage decay rate is approximately 1%. In other words, the electrostatic voltage decay rate is preferably approximately 1% or more. The numerical range of the electrostatic voltage decay rate of the foamed bead molded article can be, for example, a range (a numerical range not less than the lower limit and not more than the upper limit) having a lower limit of any one value from the group (numerical group) consisting of 0% and 1% and an upper limit of any one value from the group (numerical group) consisting of 20%, 15%, 10%, and 5%.

[0017] (Molded body density) The density of the molded body in the foamed bead mold (molded body density) is 15 kg / m 3 More than 500kg / m 3 The density of the compact is preferably 15 kg / m or less. 3 More than 500kg / m 3 From the viewpoint of improving the effect of achieving an excellent balance between the rigidity and the weight of the molded body, the density of the molded body is set to 15 kg / m or less. 3 More than 300kg / m 3 More preferably, it is 20 kg / m or less. 3More than 150kg / m 3 The density of the compact is calculated by dividing the mass of the compact by the volume calculated based on the dimensions of the compact. The range of the density of the compact is, for example, 15 kg / m or less. 3 , and 20 kg / m 3 and 300 kg / m 3 , and 150 kg / m 3 The range can be any one of the values ​​in the group consisting of the above as the upper limit (a numerical range not less than the lower limit and not more than the upper limit).

[0018] (Tensile Strength of Molded Article) The tensile strength of the expanded bead molding of the present invention is preferably 150 kPa or more, more preferably 200 kPa or more, and even more preferably 250 kPa or more. If the tensile strength is within the above range, the expanded bead molding will have excellent fusion properties despite the presence of talc on the surface of the expanded beads, resulting in a molding with excellent mechanical properties. The upper limit of the tensile strength of the expanded bead molding is approximately 6000 kPa. The numerical range of the tensile strength of the expanded bead molding can be, for example, a range in which the lower limit is any one of the values ​​in the group consisting of 150 kPa, 200 kPa, and 250 kPa, and the upper limit is 6000 kPa (a numerical range not less than the lower limit and not more than the upper limit).

[0019] The tensile strength (kPa) of an expanded bead molding is measured in accordance with JIS K6767:1999. Specifically, a vertical slicer is used to cut a piece 120 mm long x 25 mm wide x 10 mm thick from the expanded bead molding so that all surfaces are cut out, and a dumbbell-shaped No. 1 test piece is prepared from the cut piece using a jigsaw. The test piece is subjected to a tensile test at a tensile speed of 500 mm / min to determine the tensile strength (kPa). The maximum value (kPa) measured during the tensile test is defined as the tensile strength of the expanded bead molding.

[0020] (Tensile strength of molded article / density of molded article) In the present invention, the ratio of tensile strength of the expanded bead molded article to density of the molded article (kPa / (kg / m 3)) value (value obtained by dividing the tensile strength of the expanded bead molding by the molding density) is 5 kPa / (kg / m 3 ) or more, and 3 ) or more, and 9 kPa / (kg / m 3 If the ratio is within the above range, the expanded bead molding will have excellent fusion properties despite the presence of talc on the surface of the expanded beads, resulting in a molding with excellent mechanical properties. The upper limit of the ratio is approximately 20 kPa / (kg / m 3 The numerical range of the ratio of tensile strength to density of the expanded bead molding is, for example, 5 kPa / (kg / m 3 ), 7kPa / (kg / m 3 ), and 9 kPa / (kg / m 3 ) as the lower limit, and 20 kPa / (kg / m 3 ) as the upper limit (a numerical range not less than the lower limit and not more than the upper limit).

[0021] (Fusion rate of the expanded bead molding) The expanded bead molding of the present invention is obtained by fusing a plurality of expanded beads. The fusion rate of the expanded bead molding is preferably 80% or more, and more preferably 90% or more. Expanded bead moldings with a fusion rate within the above range exhibit excellent fusion properties and excellent mechanical properties, despite the presence of minerals such as talc at the interfaces originating from the plurality of expanded beads in the expanded bead molding.

[0022] The fusion rate can be determined based on the ratio of foamed beads exposed on the fracture surface when the foamed bead molding is broken to the number of foamed beads that have undergone material destruction. Specifically, first, unprocessed test pieces (150 mm long x 75 mm wide x 25 mm thick) are cut from the center of the thickness direction of the foamed bead molding. Then, each unprocessed test piece is cut with a cutter knife to a depth of approximately 2 mm in the thickness direction, perpendicular to the length and passing through the center, to prepare a test piece. Next, using the test piece, a three-point bending test is performed in accordance with JIS K7221-2 (2006) under conditions of a support distance of 70 mm and a pressure wedge speed of 200 mm / min. In this test, the test piece is pressed until it breaks. Next, the number (n) of expanded beads present on the fracture surface of the expanded bead molding and the number (b) of expanded beads that have been destroyed are measured, and the ratio (b / n) of (b) to (n) expressed as a percentage is defined as the fusion rate (%).

[0023] (Amount of talc present in the surface portion of the expanded bead molding) Talc is present in the surface portion of the expanded bead molding, and the amount of talc present is preferably 600 mass ppm or more and 9000 mass ppm or less. If the amount of talc present is within this range, the expanded bead molding will have good electrostatic charge characteristics. Note that the surface portion of the expanded bead molding is generally assumed to be the portion within a range of 20 μm inside from the surface.

[0024] (Expanded Polypropylene Resin Beads) The expanded polypropylene resin beads of the present invention can be used to produce expanded bead molded articles. The expanded bead molded articles can be obtained by in-mold molding using the expanded polypropylene resin beads of the present invention. Specifically, a molded article can be produced by filling a large number of expanded beads into a mold and carrying out a molding step in which a heating medium such as steam is supplied to fuse the expanded beads to each other. That is, an expanded bead molded article can be obtained by in-mold molding of the expanded beads. Talc is present on the surface of the expanded bead molded article of the present invention, and such a molded article can be obtained by in-mold molding using expanded beads having talc present on the surface, as described below.

[0025] The expanded beads of the present invention can be described using previously known descriptions of expanded beads. The expanded beads of the present invention may have a single-layer structure or a multi-layer structure. In the expanded beads having the single-layer structure (sometimes referred to as single-layer expanded beads), the single foam layer may be made of a polypropylene-based resin as described below. In the expanded beads having the multi-layer structure (sometimes referred to as multi-layer expanded beads), the core layer may be made of a polypropylene-based resin as described below.

[0026] (Foam Layer) When the expanded polypropylene resin beads of the present invention are single-layer expanded beads, the base resin of the single-layer expanded beads is composed of a polypropylene resin. When the expanded beads of the present invention are multi-layer expanded beads, the base resin of the core layer of the expanded beads is composed of a polypropylene resin. Examples of these polypropylene resins include propylene homopolymers and propylene copolymers containing 50% by mass or more of structural units derived from propylene. Examples of polypropylene copolymers include copolymers of propylene with ethylene or α-olefins having 4 or more carbon atoms, such as propylene-ethylene copolymers, propylene-butene copolymers, and propylene-ethylene-butene copolymers, as well as propylene-maleic anhydride copolymers. These copolymers may be block copolymers, random copolymers, or graft copolymers. While the polymers may be crosslinked, non-crosslinked copolymers are preferred. In this specification, the term "base resin" of a specific structure refers to the polymer component among the components constituting the structure. Examples of the "certain specific structure" include the foam layer constituting the single-layer expanded beads, the core layer constituting the multi-layer expanded beads, and the coating layer constituting the multi-layer expanded beads.

[0027] The base resin constituting the core layer of the single-layer expanded beads or multi-layer expanded beads may contain, in addition to a polypropylene-based resin, other resin materials such as other resins and elastomers, as long as the intended effects of the present invention are achieved. Examples of other resin materials include thermoplastic resins and / or elastomers other than polypropylene-based resins. Examples of thermoplastic resins other than polypropylene-based resins include at least one resin selected from polyethylene-based resins, polystyrene-based resins, polyamide-based resins, polyester-based resins, etc. Examples of elastomers that can be used include olefin-based thermoplastic elastomers and / or styrene-based thermoplastic elastomers.

[0028] The proportion of polypropylene-based resin in the base resin is 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and it is particularly preferable that the resin component in the base resin is composed of polypropylene-based resin.

[0029] The melting point Tmc of the polypropylene resin constituting the core layer of the single-layer or multi-layer expanded beads is preferably 120°C or higher and 160°C or lower. In this case, it is possible to stably obtain expanded bead molded articles having excellent mechanical properties while improving the in-mold moldability of the expanded beads (moldability during in-mold molding). From the viewpoint of improving the in-mold moldability of the expanded beads and the mechanical properties of the resulting molded articles, the melting point Tmc of the polypropylene resin constituting the core layer of the single-layer or multi-layer expanded beads is preferably 130°C or higher, more preferably 135°C or higher. Furthermore, from the viewpoint of improving in-mold moldability under low molding pressure conditions, the melting point Tmc of the polypropylene resin constituting the core layer of the single-layer or multi-layer expanded beads is preferably 155°C or lower, more preferably 153°C or lower, and even more preferably 150°C or lower. The numerical range of the melting point Tmc of the polypropylene-based resin can be, for example, a range having a lower limit of any one value in the group consisting of 120°C, 130°C, and 135°C and an upper limit of any one value in the group consisting of 155°C, 153°C, and 150°C (a numerical range not less than the lower limit and not more than the upper limit).

[0030] In this specification, the melting point of a polypropylene-based resin is determined based on JIS K7121:1987. Specifically, the conditioning is performed in the manner of "(2) Measuring the melting temperature after a certain heat treatment," and a test piece of the conditioned polypropylene-based resin is heated from 30°C to 200°C at a heating rate of 10°C / min to obtain a DSC curve, and the apex temperature of the melting peak is taken as the melting point. When multiple melting peaks appear in the DSC curve, the apex temperature of the melting peak with the largest area is taken as the melting point.

[0031] (Multilayer Expanded Beads) When the expanded polypropylene resin beads of the present invention are multilayer expanded beads, the multilayer expanded beads have an expanded core layer (expanded core layer) and a coating layer, and the coating layer is a layer that covers all or part of the expanded core layer. Examples of multilayer expanded beads include those having a so-called sheath-core structure. The coating layer is preferably a layer that enables in-mold molding of a multilayer expanded bead molding equivalent to a good single-layer expanded bead molding at a steam pressure lower than the minimum steam pressure required to obtain an expanded bead molding in which the single-layer expanded beads are well fused together (i.e., a good single-layer expanded bead molding) when expanded beads consisting of a single foam layer without a coating layer (i.e., single-layer expanded beads) are molded in a mold. Note that an expanded bead molding in which the expanded beads are well fused together means that the fusion rate of the molding is 80% or more, preferably 85% or more, and more preferably 90% or more. The method for measuring the fusion rate of the molding is as described above. The covering layer is preferably made of a resin that can be fused to the foamed core layer at a lower temperature (specifically, at a lower steam pressure) than the resin that constitutes the foamed core layer. Examples of the resin that constitutes the covering layer include a resin that has a lower melting point or a lower softening point than the resin that constitutes the core layer.

[0032] (Coating Layer) Examples of the base resin of the coating layer include polyolefin-based resins. Examples of polyolefin-based resins include polyethylene-based resins such as linear low-density polyethylene, low-density polyethylene, and high-density polyethylene; polypropylene-based resins such as propylene-ethylene copolymer, propylene-butene copolymer, and propylene-ethylene-butene copolymer; and mixtures thereof. From the viewpoint of excellent adhesion to the foamed core layer, the polyolefin-based resin of the coating layer is preferably a polypropylene-based resin and / or a polyethylene-based resin, and more preferably a polypropylene-based resin. When the base resin constituting the coating layer is a polypropylene resin, it is more preferably at least one selected from a propylene-ethylene copolymer, a propylene-butene copolymer, and a propylene-ethylene-butene copolymer. Furthermore, a coating layer made of a polypropylene-based resin and / or a polyethylene-based resin further improves adhesion between the foamed core layer and the coating layer, and enables the stable production of molded articles with good mechanical properties. The base resin composed of at least one selected from the group consisting of a propylene-ethylene copolymer, a propylene-butene copolymer, and a propylene-ethylene-butene copolymer may be composed of a single copolymer or a mixture of multiple copolymers. Furthermore, from the viewpoint of the fusibility, adhesiveness, etc., it is preferable that the base resin be obtained using a metallocene polymerization catalyst.

[0033] When the base resin constituting the coating layer is a polyolefin-based resin, the melting point Tms (°C) of the polyolefin-based resin is preferably lower than, for example, the melting point Tmc (°C) of the polypropylene-based resin constituting the foamed core layer. That is, it is preferable that Tms < Tmc. In this case, the fusion property between the expanded beads during molding is improved, and a molded article with excellent fusion property can be produced at a low temperature (specifically, low steam pressure) during in-mold molding. From the viewpoint of further improving this effect, it is preferable that Tmc - Tms ≧ 1 (°C), more preferably Tmc - Tms ≧ 3 (°C), and even more preferably Tmc - Tms ≧ 5 (°C). From the viewpoint of further suppressing peeling between the foamed core layer and the coating layer and adhesion of the resin to the molding die during in-mold molding, it is preferable that Tmc - Tms ≦ 30 (°C), more preferably Tmc - Tms ≦ 25 (°C), and even more preferably Tmc - Tms ≦ 20 (°C). The numerical range of Tmc-Tms can be, for example, a range having a lower limit of any one value from the group consisting of 1 (°C), 3 (°C), and 5 (°C) and an upper limit of any one value from the group consisting of 30 (°C), 25 (°C), and 20 (°C) (a numerical range not less than the lower limit and not more than the upper limit).

[0034] From the viewpoint of preventing the resin from adhering to the molding die during in-mold molding, the melting point Tms of the polyolefin resin constituting the coating layer is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher. On the other hand, from the viewpoint of improving the fusion properties of the expanded beads during molding, the melting point Tms of the polyolefin resin constituting the coating layer is preferably 150°C or lower, more preferably 145°C or lower, and even more preferably 140°C or lower. The melting point of the polyolefin resin constituting the coating layer is determined in accordance with JIS K7121:1987. Specifically, it is determined under the same conditions and by the same method as for the polypropylene resin constituting the foamed core layer described below. The numerical range of the melting point Tms of the polyolefin resin constituting the coating layer can be, for example, a range having a lower limit of any one value from the group consisting of 100°C, 110°C, and 120°C, and an upper limit of any one value from the group consisting of 150°C, 145°C, and 140°C (a numerical range not less than the lower limit and not more than the upper limit).

[0035] When the expanded beads of the present invention are multi-layer expanded beads, the proportion of the coating layer in the expanded beads is preferably 0.5% by mass or more and 15% by mass or less. In this case, the in-mold moldability (moldability during in-mold molding) of the expanded beads can be improved, while an expanded bead molded article with excellent mechanical properties can be stably obtained. From the viewpoint of improving the effect of excellent balance between in-mold moldability and mechanical properties, the mass proportion of the coating layer in the expanded beads is more preferably 1% by mass or more and 10% by mass or less, and even more preferably 2% by mass or more and 8% by mass or less. The numerical range representing the proportion of the coating layer in the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 0.5%, 1%, and 2% by mass and an upper limit of any one of the group consisting of 15%, 10%, and 8% by mass (a numerical range at least the lower limit and at most the upper limit).

[0036] When the expanded beads of the present invention are multi-layer expanded beads, the expanded core layer is made of an expanded polypropylene-based resin, and the coating layer is made of an expanded or non-expanded polyolefin-based resin. The coating layer is preferably in a substantially non-expanded state. "Substantially non-expanded" means that there is almost no cellular structure.

[0037] (Carbons) The expanded beads of the present invention contain carbons. Carbons are used to color the expanded beads gray, black, or a mottled pattern thereof, or to impart functionality to the expanded beads. When the expanded beads are single-layer expanded beads, the content of carbons in the expanded beads is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 4% by mass, and even more preferably 1% by mass to 3% by mass. When the expanded beads are single-layer expanded beads, the numerical range representing the content of carbons in the expanded beads can be, for example, a range with a lower limit of any one of the groups consisting of 0.1% by mass, 0.5% by mass, and 1% by mass and an upper limit of any one of the groups consisting of 5% by mass, 4% by mass, and 3% by mass (a numerical range equal to or greater than the lower limit and equal to or less than the upper limit). On the other hand, when the expanded beads are multi-layer expanded beads, it is preferable that at least the coating layer contains carbons. The coexistence of carbons and talc on the surface of the multi-layer expanded beads makes it easier to obtain molded articles that combine electrostatic charging properties and good appearance. In this case, the carbon content in the coating layer is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.5% by mass or more and 4% by mass or less, and even more preferably 1% by mass or more and 3% by mass or less. When the expanded beads are multi-layer expanded beads, the numerical range indicating the carbon content in the coating layer can be, for example, a range with a lower limit of any one value from the group consisting of 0.1% by mass, 0.5% by mass, and 1% by mass, and an upper limit of any one value from the group consisting of 5% by mass, 4% by mass, and 3% by mass (a numerical range equal to or greater than the lower limit and equal to or less than the upper limit). Furthermore, carbons can also be contained in the foamed core layer. In this case, the carbon content in the foamed core layer is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.5% by mass or more and 4% by mass or less, and even more preferably 1% by mass or more and 3% by mass or less. Furthermore, the numerical range indicating the content of carbons in the foamed core layer can be, for example, a range having a lower limit of any one value from the group consisting of 0.1 mass%, 0.5 mass%, and 1 mass%, and an upper limit of any one value from the group consisting of 5 mass%, 4 mass%, and 3 mass% (a numerical range not less than the lower limit and not more than the upper limit).The carbon content in the single-layer expanded beads and in the core layer and coating layer of the multi-layer expanded beads is roughly the same as the amount of carbon added to the single-layer resin particles and the core layer and coating layer of the multi-layer resin particles during the production of the resin particles to be expanded.

[0038] The carbon content of expanded beads and their molded articles can be quantified by TG-DTA. Specifically, a sample cut from the expanded beads or molded articles is used as the measurement sample (measurement sample), and the weighed sample is heated from 40°C to 600°C in a nitrogen atmosphere. The heating temperature of the sample is then lowered to 400°C, the atmospheric gas is changed from nitrogen to air, and the sample is heated to 800°C. The weight loss of the sample when heated to 600°C in a nitrogen atmosphere is taken as the organic matter content, and the weight loss of the sample when heated to 800°C in an air atmosphere is taken as the carbon content. When measuring the content of the coating layer, a sample of the target portion can be scraped off and measured in the same manner.

[0039] Examples of the carbons include at least one type of carbon powder selected from carbon black, carbon nanotubes, graphite, graphene, carbon nanofibers, carbon microfibers, carbon microcoils, and carbon nanocoils, and examples of usable carbons include channel black, roller black, furnace black, thermal black, acetylene black, SWCNT (single-walled carbon nanotube), MWCNT (multi-walled carbon nanotube), branched MWCNT, etc. Among these, furnace black is preferred as the carbon to be used for the expanded beads because it has an excellent balance between dispersibility in polypropylene-based resins and material costs.

[0040] The conventional foamed bead moldings obtained by molding foamed beads containing carbons in a mold have poor insulating properties, making it difficult to exhibit electrostatic charging performance, and the present inventors have solved this problem by adding a specific amount of talc to the surface of the foamed beads.

[0041] (Talc) Talc is present on the surface of the expanded bead molding of the present invention. Furthermore, by molding expanded beads configured so that talc is present on the surface of the expanded beads into a molded article, the expanded bead molding can exhibit desired electrostatic charge characteristics while exhibiting favorable physical properties as a molded article. The talc preferably contains a magnesium silicate component, and its content is preferably 20% or more, more preferably 50% or more, and even more preferably 80% or more. The content can be calculated, for example, by performing various compositional analyses. When talc is present on the surface of the expanded beads, the number-average particle diameter of the talc, determined using the maximum length on a micrograph as the representative diameter, is preferably 0.01 μm to 30 μm, particularly 0.01 μm to 10 μm. Furthermore, the layer charge of the talc is preferably 0±0.5, more preferably 0.

[0042] (Presence of Talc) In the expanded beads, talc may be present on the surface of the expanded beads in various ways, including an embodiment in which talc is attached to the surface of the expanded beads, an embodiment in which talc is contained at least on the surface side of the expanded beads, and an embodiment in which talc is both attached and contained. Specific examples are shown in FIGS. 1 to 4. However, the present invention is not limited to these embodiments. FIGS. 1 and 2 are cross-sectional views of typical single-layer expanded beads, and FIGS. 3 and 4 are cross-sectional views of multi-layer expanded beads. The single-layer expanded beads 1A shown in FIGS. 1 and 2 have an expanded layer 4 and talc 5. In FIG. 1, talc 5 is attached to the surface of the single-layer expanded beads 1A. In FIG. 2, talc 5 is contained in the surface side of the single-layer expanded beads 1A. The multi-layer expanded beads 1B shown in FIGS. 3 and 4 have an expanded core layer 2 and a coating layer 3, and the coating layer 3 coats the core layer 2. The multi-layer expanded beads 1B also contain talc 5. In Figure 3, talc 5 is attached to the surface of multi-layer expanded beads 1B. In Figure 2, talc 5 is contained in the coating layer 3 of single-layer expanded beads 1B. The expanded core layer of the expanded beads is appropriately referred to as the "expanded core layer." The shapes of the expanded beads in Figures 1 to 4 are, for example, cylindrical or spherical. The term "cylindrical" includes those that are somewhat rounded, and the term "sphere" includes not only those whose cross section is a perfect circle but also those that are elliptical, circular, or close to an ellipse. Furthermore, the expanded beads of the present invention also include those having a cylindrical or concave outer shape with a hollow portion.

[0043] As described above, for both single-layer and multi-layer expanded beads, the forms in which talc is present on the surface of the expanded beads include, specifically, (1) a form in which talc is attached to the expanded beads (FIGS. 1 and 3) and (2) a form in which talc is contained on the surface side of the expanded beads (FIGS. 2 and 4), as described above with reference to Figures 1 to 4. Furthermore, the forms (1) and (2) may coexist.

[0044] (1) Adhesion In the case of single-layer expanded beads, talc is preferably attached to the surface of the expanded beads ( FIG. 1 ) to ensure that talc is present on the surface of the expanded beads. In the case of multi-layer expanded beads, talc is preferably attached to the surface of the multi-layer expanded beads, i.e., the surface of the coating layer ( FIG. 3 ). The amount of talc attached to the surface of the single-layer expanded beads shown in FIG. 1 and the amount of talc attached to the surface of the multi-layer expanded beads shown in FIG. 3 can both be adjusted as described in the Examples of the present specification. That is, the amount of talc present on the surface of the expanded beads can be adjusted as described in the Examples of the present specification. Specifically, based on the positive correlation between the amount of talc added to the dispersion medium in a sealed container and the amount of talc attached to the surface of the resulting expanded beads, the amount of talc can be adjusted by conducting several experiments. A rough guideline for the amount of talc added is in the range of 0.05 to 15 parts by mass per 100 parts by mass of resin particles added to the dispersion medium in the sealed container. Well-known dispersants or surfactants may be used in combination when adding talc to the dispersion medium.

[0045] The amount of talc attached to the surface of the expanded beads is preferably 600 to 10,000 ppm by mass, more preferably 700 to 8,000 ppm by mass, and even more preferably 900 to 7,000 ppm by mass. The numerical range of the amount of talc attached to the surface of the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 600 ppm by mass, 700 ppm by mass, and 900 ppm by mass, and an upper limit of any one of the group consisting of 10,000 ppm by mass, 8,000 ppm by mass, and 7,000 ppm by mass (a numerical range from the lower limit to the upper limit).

[0046] (2) Content In the case of single-layer expanded beads, talc is preferably kneaded into the base resin of the expanded beads and incorporated at least on the surface side ( FIG. 2 ). In the case of multi-layer expanded beads, talc is preferably kneaded into at least the base resin constituting the coating layer and incorporated into the coating layer of the expanded beads ( FIG. 4 ). The extent of the surface portion in FIG. 2 is determined appropriately depending on the type and amount of talc present, the desired electrostatic performance, etc., and the extent of the surface portion may be assumed to be approximately a range extending from the surface of the expanded beads to a position 20 μm inward. The talc content of both the surface portion of the single-layer expanded beads shown in FIG. 2 and the talc content of the coating layer of the multi-layer expanded beads shown in FIG. 4 generally coincides with the amount of talc blended into the base resin during the production of the resin beads to be expanded. That is, the amount of talc present in the surface portion of the expanded beads generally coincides with the amount of talc blended into the base resin during the production of the resin beads to be expanded.

[0047] (Talc Content) The talc content in the surface portion of the expanded beads is preferably 600 ppm by mass or more and 10,000 ppm by mass or less, more preferably 700 ppm by mass or more and 9,000 ppm by mass or less, and even more preferably 900 ppm by mass or more and 8,000 ppm by mass or less. By having the talc content within the above range, the amount of talc present in the surface portion of the expanded beads can be adjusted to a preferred range. Furthermore, sufficient electrostatic charging performance can be exhibited in expanded bead moldings obtained from expanded beads containing carbons. Furthermore, by adjusting the amount of talc present in the surface portion of the expanded beads to a preferred range, the fusion properties of the expanded beads to each other can be sufficiently maintained even during in-mold molding of the expanded beads. The numerical range of the talc content in the surface portion of the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 600 ppm by mass, 700 ppm by mass, and 900 ppm by mass, and an upper limit of any one of the group consisting of 10,000 ppm by mass, 8,000 ppm by mass, and 7,000 ppm by mass (a numerical range not less than the lower limit and not more than the upper limit).

[0048] (Measurement of the Amount of Talc Present on the Surface Portion of Expanded Beads) The amount of talc present on the surface portion of expanded beads in the present invention can be measured as follows: For example, a calibration curve for talc is measured in advance using attenuated total reflection spectroscopy (ATR), and the amount of talc present on the surface of expanded beads can be measured based on this calibration curve.

[0049] For example, the content of talc present in the surface portion of the expanded beads can be measured by the following method. First, a resin test piece with a known talc content is prepared. Next, the surface portion of the resin test piece is measured by total internal reflection spectroscopy (ATR method) using an infrared spectrophotometer to obtain an infrared light absorption spectrum of the resin test piece. Next, the peak wavelength attributable to talc is confirmed from the infrared light absorption spectrum of the resin test piece, and the absorption intensity of the peak wavelength is obtained. Specifically, the peak wavelength attributable to talc is 1000 cm -1 , 650 cm -1 A calibration curve is prepared from the relationship between the talc content in the resin test piece and the absorption intensity at the peak wavelength attributable to talc, allowing the amount of talc present on the surface of the expanded beads to be calculated.

[0050] Separately, a sample of expanded beads to be measured is cut into two equal parts. The cut surface of the expanded beads (i.e., the interior of the expanded beads) is used as the measurement target, and measurement is similarly performed by the ATR method to obtain an infrared absorption spectrum of the cut surface. Based on the infrared absorption spectrum of the cut surface, the absorption intensity at the same wavelength as the peak wavelength (the wavelength identified from the infrared absorption spectrum of the resin test piece as the peak wavelength derived from talc) is then obtained.

[0051] Next, the surface of the expanded beads is measured by attenuated total reflection spectroscopy (ATR) to obtain an infrared absorption spectrum of the surface of the expanded beads, and the absorption intensity of the peak wavelength derived from talc is measured based on the infrared absorption spectrum of the surface of the expanded beads.

[0052] The difference between the absorption intensity based on the infrared absorption spectrum of the surface portion of the expanded beads and the absorption intensity based on the infrared absorption spectrum of the cut surface is calculated.

[0053] The amount of talc present on the surface of the expanded beads can be calculated from the relationship between the calculated difference value and the calibration curve. If inorganic powder other than talc is attached to the surface of the expanded beads, this can be removed before measuring the talc content.

[0054] The difference value may be determined based on the difference spectrum (difference spectrum) between the infrared absorption spectrum of the surface portion of the expanded beads and the infrared absorption spectrum of the cut surface. That is, after obtaining the difference spectrum, the absorption intensity at the same wavelength as the wavelength determined from the infrared absorption spectrum of the resin test piece as the peak wavelength attributable to talc may be read based on the difference spectrum, and the read absorption intensity may be used as the difference value.

[0055] Although the method for determining the amount of talc present on the surface of expanded beads (abundance of talc) has been described here, this method can also be applied to determining the amount of talc present on the surface of a molded article molded from expanded beads. That is, the expanded beads to be measured used in the method for determining the amount of talc present on the surface of expanded beads (abundance of talc) can be replaced with a molded article to be measured.

[0056] (Amount of Talc) The amount of talc present in the surface portion of the expanded beads is a value calculated as the sum of the amount of talc attached and the total amount, and is preferably 600 to 10,000 ppm by mass, more preferably 650 to 9,000 ppm by mass, and even more preferably 700 to 8,000 ppm by mass. The numerical range representing the amount of talc present in the surface portion of the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 600 ppm by mass, 650 ppm by mass, and 700 ppm by mass, and an upper limit of any one of the group consisting of 10,000 ppm by mass, 9,000 ppm by mass, and 8,000 ppm by mass (a numerical range not less than the lower limit and not more than the upper limit). In addition, when talc is attached to and contained in the expanded beads (or when it is unclear whether talc is attached or contained), the amount present can be measured as the sum of the attached amount and the contained amount by employing the above-mentioned content measurement method without performing an operation to remove the attached talc. Regarding the analysis to determine whether the attached or contained component is talc, for example, shape observation and composition analysis can be separately performed using an appropriate combination of scanning electron microscope observation, infrared spectroscopy, X-ray fluorescence analysis, etc., to determine whether the attached or contained component is talc. Furthermore, when components other than talc are present, the attached amount and the contained amount can be calculated by subtracting the components other than talc.

[0057] (Method for measuring the amount of talc present in an expanded bead molding) The amount of talc present in the surface portion of an expanded bead molding (the surface portion refers to the area extending 20 μm inward from the surface) can also be quantified using the method using an infrared spectrophotometer, etc., in the same manner as the method for measuring talc in expanded beads described above. For example, when talc is attached to and / or contained on the surface of an expanded bead molding, the amount of talc present in the molding can be measured as the sum of the amount of talc attached and the amount of talc contained.

[0058] (Ratio of Talc to Carbons) In order to further improve the electrostatic performance of the expanded beads of the present invention, the mass ratio (CB / talc amount) of the amount of talc present on the expanded bead surface (talc amount) to the carbon content (CB) in the expanded beads is preferably 2.5 to 100, more preferably 3 to 50. The numerical range of the mass ratio of the amount of talc present on the expanded bead surface (talc amount) to the carbon content (CB) in the expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 2.5 and 3 and an upper limit of any one value from the group consisting of 100 and 50 (a numerical range not less than the lower limit and not more than the upper limit).

[0059] (Other Additives) The expanded beads of the present invention may contain additives. Specific examples of additives include flame retardants, flame retardant auxiliaries, cell regulators, antioxidants, weathering agents, and crystal nucleating agents. The additives may be contained in the entire expanded beads or only in a portion of the expanded beads. Specifically, the additives may be contained in the entire single-layer expanded beads, the entire multi-layer expanded beads, or only in the coating layer of the multi-layer expanded beads.

[0060] (Bulk density of expanded particles) The bulk density of the expanded particles is 10 kg / m 3 More than 500kg / m 3 When the bulk density is in this range, the rigidity of the molded article can be increased while reducing the weight of the molded article. From the viewpoint of improving the effect of achieving an excellent balance between rigidity and lightweight, the bulk density of the expanded beads is preferably 15 kg / m or less. 3 More than 100kg / m 3 More preferably, it is 18 kg / m or less. 3 More than 50kg / m 3 It is more preferable that the bulk density of the expanded beads is 10 kg / m or less. 3 , 15 kg / m 3 and 18 kg / m 3 and 500 kg / m 3 , 100 kg / m 3 and 50 kg / m 3The range can be any one of the values ​​in the group consisting of the above as the upper limit (a numerical range not less than the lower limit and not more than the upper limit).

[0061] The bulk density of expanded beads is measured by the following method. First, a plurality of expanded beads (expanded beads) to be measured are left for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. Then, a mass W (unit: g) of expanded beads is filled into a measuring cylinder, and the bottom of the measuring cylinder is lightly tapped against the floor several times to stabilize the filling height of the expanded beads in the measuring cylinder. The bulk volume V (unit: L) of the expanded beads indicated by the graduated scale on the measuring cylinder is read, and the mass W of the expanded beads is divided by the bulk volume V of the expanded beads (i.e., W / V). The value obtained in this way is kg / m 3 The bulk density of the expanded particles (unit: kg / m 3 ) can be obtained.

[0062] (High-Temperature Peak) The expanded beads preferably have a crystalline structure in which a melting peak specific to the polypropylene resin (i.e., the resin-specific peak) and one or more melting peaks (i.e., high-temperature peaks) appear on the higher temperature side of the DSC curve obtained when heated from 23°C to 200°C at a heating rate of 10°C / min. The DSC curve is obtained by performing differential scanning calorimetry (DSC) in accordance with JIS K7121:1987 using 1 to 3 mg of expanded beads as a test sample. The resin-specific peak is an endothermic peak due to the melting of crystals specific to the polypropylene resin constituting the expanded beads, and is thought to be due to the endothermic heat generated when crystals typically melt in polypropylene resins. On the other hand, the endothermic peak on the higher temperature side of the resin-specific peak (i.e., the high-temperature peak) is an endothermic peak that appears on the higher temperature side of the resin-specific peak on the DSC curve. When this high-temperature peak appears, it is estimated that a high-melting point secondary crystalline component is present in the resin. In the DSC curve obtained by heating from 23°C to 200°C at a heating rate of 10°C / min (i.e., first heating), followed by cooling from 200°C to 23°C at a cooling rate of 10°C / min, and then again heating from 23°C to 200°C at a heating rate of 10°C / min (i.e., second heating), only an endothermic peak due to melting of crystals specific to the polypropylene resin constituting the expanded beads is observed, making it possible to distinguish between the resin-specific peak and the high-temperature peak. The apex temperature of this resin-specific peak may differ slightly between the first and second heatings, but the difference is usually within 5°C.

[0063] From the viewpoint of further improving the moldability of the expanded beads and obtaining molded articles with superior rigidity, the heat of fusion of the high-temperature peak of the expanded beads is preferably 5 J / g to 40 J / g, more preferably 7 J / g to 30 J / g, and even more preferably 10 J / g to 20 J / g. The total heat of fusion of the expanded beads is preferably 25 J / g to 150 J / g, more preferably 35 J / g to 100 J / g, and even more preferably 50 J / g to 90 J / g. The range of the heat of fusion of the high-temperature peak of the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 5 J / g, 7 J / g, and 10 J / g, and an upper limit of any one of the group consisting of 40 J / g, 30 J / g, and 20 J / g (a numerical range not less than the lower limit and not more than the upper limit). The numerical range indicating the total heat of fusion of the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 25 J / g, 35 J / g, and 50 J / g and an upper limit of any one of the group consisting of 150 J / g, 100 J / g, and 90 J / g (a numerical range not less than the lower limit and not more than the upper limit).

[0064] (Method for Measuring High-Temperature Peaks) The heat of fusion of each peak in the DSC curve of expanded beads is determined as follows. First, approximately 2 to 4 mg of expanded beads are sampled from a dried group of expanded beads. Using these expanded beads as test specimens, a DSC curve is obtained by heating the test specimen from 23°C to 200°C at a heating rate of 10°C / min using a differential scanning calorimeter. Note that multiple expanded beads may be used as test specimens. The DSC curve exhibits a resin-specific peak ΔH1 and a high-temperature peak ΔH2, which peaks at a higher temperature than the peak of the resin-specific peak ΔH1. Next, a line L1 is obtained by connecting point α at a temperature of 80°C on the DSC curve with point β at the melting end temperature T of the expanded beads. Next, a line L2 parallel to the vertical axis of the graph is drawn from point γ on the DSC curve, which corresponds to the valley between the resin-specific peak ΔH1 and the high-temperature peak ΔH2, and the point where lines L1 and L2 intersect is designated δ. The point γ can also be said to be a maximum point existing between the resin-specific peak ΔH1 and the high-temperature peak ΔH2. The area of ​​the resin-specific peak ΔH1 is the area of ​​the portion surrounded by the curve of the resin-specific peak ΔH1 portion of the DSC curve, the line segment α-δ, and the line segment γ-δ, and this is the heat of fusion of the resin-specific peak. The area of ​​the high-temperature peak ΔH2 is the area of ​​the portion surrounded by the curve of the high-temperature peak ΔH2 portion of the DSC curve, the line segment δ-β, and the line segment γ-δ, and this is the heat of fusion of the high-temperature peak (i.e., the high-temperature peak heat quantity). The area of ​​the total melting peak is the area of ​​the portion surrounded by the curve of the resin-specific peak ΔH1 portion of the DSC curve, the curve of the high-temperature peak ΔH2 portion, and the line segment α-β (i.e., the straight line L1), and this is the heat of fusion of the total melting peak (total heat of fusion).

[0065] (Method for producing expanded beads) Next, an example of a method for producing expanded beads will be described. Expanded beads can be produced by a process including a resin bead production process, a dispersion process, a blowing agent impregnation process, and a foaming process. In the dispersion process, polypropylene-based resin particles are dispersed in an aqueous medium in a container. In the foaming agent impregnation process, the polypropylene-based resin particles are impregnated with a foaming agent in the container. In the foaming process, the polypropylene-based resin particles containing the foaming agent (i.e., expandable resin particles) are released from the container together with the aqueous medium and foamed. Hereinafter, an embodiment of the production method will be specifically described.

[0066] (Production of Resin Particles) The production of single-layer resin particles is well known, while the production of multilayer resin particles is carried out, for example, as follows. Two extruders, an extruder for forming a core layer and an extruder for forming a coating layer, are connected to a co-extrusion die. The extruder for forming the core layer melts and kneads a polypropylene resin for forming the core layer with additives as needed to produce a melt of the resin composition for forming the core layer. Meanwhile, the extruder for forming the coating layer melts and kneads a polyolefin resin for forming the coating layer with carbons, talc as needed, and other additives as needed to produce a melt of the resin composition for forming the coating layer. The melts are then extruded and merged in the die to form a sheath-core composite by co-extrusion, consisting of a non-foamed core layer and a non-foamed coating layer covering the outer surface of the core layer. In the composite, the core layer is composed of the resin composition for forming the core layer, and the coating layer is composed of the resin composition for forming the coating layer. The composite is then extruded from the extruder and pelletized by various cutting methods using a pelletizer or the like. The cutting method can be selected from strand cutting, hot cutting, underwater cutting, etc. In this manner, multilayer resin particles consisting of a core layer and a coating layer that coats this core layer can be obtained. When talc is to be contained in the expanded resin particles, in the resin particle manufacturing process, talc is preferably added to the resin used to form the expanded resin particles in the case of single-layer resin particles, and to the resin used to form the coating layer in the case of multilayer resin particles.

[0067] (Resin Particles) The particle diameter of the single-layer or multilayer resin particles is preferably 0.1 mm to 3.0 mm, more preferably 0.3 mm to 1.5 mm. The length / outer diameter ratio of the resin particles is preferably 0.5 to 5.0, more preferably 1.0 to 3.0. The average mass per single-layer or multilayer resin particle (determined from the masses of 200 randomly selected particles) is preferably 0.1 mg to 20 mg, more preferably 0.2 mg to 10 mg, even more preferably 0.3 mg to 5 mg, and particularly preferably 0.4 mg to 2 mg. The mass ratio of the core layer to the coating layer in the multilayer resin particles (specifically, the mass (parts by mass) of the core layer:the mass (parts by mass) of the coating layer) is preferably 99.5:0.5 to 90:10, more preferably 99:1 to 92:8, and even more preferably 98:2 to 94:6. The sum of the masses of the core layer and the coating layer is taken as 100. Therefore, the numerical range representing the particle diameter of the single-layer resin particle or the multilayer resin particle can be, for example, a range having a lower limit of any one of the values ​​in the group consisting of 0.1 mm and 0.3 mm and an upper limit of any one of the values ​​in the group consisting of 3.0 mm and 1.5 mm (a numerical range not less than the lower limit and not more than the upper limit). The numerical range representing the length / outer diameter ratio of the resin particle can be, for example, a range having a lower limit of any one of the values ​​in the group consisting of 0.5 and 1.0 and an upper limit of any one of the values ​​in the group consisting of 5.0 and 3.0 (a numerical range not less than the lower limit and not more than the upper limit). The numerical range representing the average mass per single-layer resin particle or the multilayer resin particle can be, for example, a range having a lower limit of any one of the values ​​in the group consisting of 0.1 mg, 0.2 mg, 0.3 mg, and 0.4 mg and an upper limit of any one of the values ​​in the group consisting of 20 mg, 10 mg, 5 mg, and 2 mg (a numerical range not less than the lower limit and not more than the upper limit). Regarding the mass ratio of the core layer to the coating layer in the multilayer resin particle (specifically, the mass (parts by mass) of the core layer: the mass (parts by mass) of the coating layer), the numerical range indicating the mass (parts by mass) of the coating layer can be, for example, a range in which the lower limit is any one value from the group consisting of 0.5, 1, and 2, and the upper limit is any one value from the group consisting of 10, 8, and 6 (a numerical range not less than the lower limit and not more than the upper limit).The total mass of the core layer and the coating layer is 100.

[0068] The particle size and average mass of the multilayer resin particles can be adjusted, for example, by cutting the molten resin by appropriately changing the extrusion speed, take-up speed, cutter speed, etc. when extruding the molten resin from the extruder.

[0069] (Irregular Shaped Expanded Beads, Cylindrical Hole Shape, etc.) The expanded beads of the present invention may have the aforementioned typical cylindrical or spherical shape, as well as shapes with hollows or concave portions. By molding expanded beads having such hollows or concave portions in a mold, it is possible to obtain the expanded bead moldings described, for example, in JP-A-7-137063 and JP-A-2006-307177. The expanded bead moldings obtained by molding expanded beads having hollows or concave portions in a mold have the advantage of improving the electrostatic properties of the expanded bead moldings due to the relatively high specific surface area of ​​the expanded beads used for molding, although the reason for this is not entirely clear. From the perspective of such advantages, it is preferable to use expanded beads having hollows or concave portions as the shape of the expanded beads of the present invention. Note that expanded beads having hollows refer to shapes such as bottomed cylindrical or through-hole cylindrical expanded beads. Expanded beads having a recessed outer periphery literally mean expanded beads having an external recess (visually visible) on the surface thereof, such as expanded beads having a shape typified by a bottomed cylindrical shape or a C-shaped cross section (portion) in which the side of a penetrating cylindrical shape is missing. The shape, pore diameter, and width of the missing lateral surface portion of the hollow or recessed outer periphery include those described in JP-A-7-137063 and JP-A-2006-307177. Additionally, the shape, pore diameter, and width of the missing lateral surface portion of the hollow or recessed outer periphery can be appropriately designed according to technical concepts such as increasing the specific surface area, forming interconnected voids in the resulting expanded bead molding, and reducing the molding pressure during in-mold molding.

[0070] (Dispersion step) The dispersion step is a step of dispersing polypropylene-based resin particles in an aqueous medium. As the polypropylene-based resin particles, well-known resin particles (single-layer resin particles) or multi-layer resin particles having a core layer and a coating layer that coats the core layer are used. In this specification, polypropylene-based resin particles having a core layer and a coating layer are appropriately referred to as "multi-layer resin particles."

[0071] (Dispersion medium) An aqueous medium is used as a dispersion medium (specifically, a liquid) for dispersing the single-layer or multi-layer resin particles in a sealed container. The aqueous medium is a dispersion medium (specifically, a liquid) containing water as a main component. The proportion of water in the aqueous medium is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. Examples of dispersion media other than water in the aqueous medium include ethylene glycol, glycerin, methanol, and ethanol. Water is particularly preferred as the aqueous medium.

[0072] (Talc Adhesion) When talc is to be attached to the expanded beads, it is preferable to add talc to an aqueous medium so that the amount of talc is 0.1 to 15 parts by mass per 100 parts by mass of resin particles, and then disperse the talc in the aqueous medium. The talc dispersed in the aqueous medium not only acts as an inorganic dispersant but also remains on the surface of the expanded beads in the expansion step described below, thereby obtaining expanded beads with talc uniformly attached to the surface of the expanded beads. Note that when the resin particles contain talc and it is not necessary to attach talc to the expanded beads, it is not necessary to use talc as an inorganic dispersant.

[0073] (Dispersion) In the dispersion step, in addition to talc as described above, other inorganic dispersants can be added to the aqueous medium. Furthermore, other inorganic dispersants other than talc and other additives may be appropriately added to the aqueous medium. Examples of other inorganic dispersants that can be used include inorganic fine particles such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, and zinc oxide. These inorganic fine particles may be used alone, or two or more types of inorganic fine particles may be used in combination. Additives other than the inorganic dispersant include dispersing aids and surfactants. Examples of dispersing aids include aluminum sulfate. Examples of surfactants include anionic surfactants such as sodium alkylbenzenesulfonate, sodium dodecylbenzenesulfonate, and sodium alkanesulfonate. Surfactants may be used alone, or two or more types of surfactants may be used in combination.

[0074] (Foaming Agent Impregnation Step) The foaming agent impregnation step is a step of impregnating resin particles with a foaming agent. The foaming agent impregnation step may be performed after the dispersion step described above, or a part or all of the step may be performed overlapping with the dispersion step.

[0075] In the blowing agent impregnation step, for example, a container containing resin particles is sealed, and a blowing agent is added to the sealed container to impregnate the resin particles with the blowing agent. This allows for the production of expandable resin particles containing the blowing agent in the resin particles. Examples of the blowing agent include physical blowing agents. The physical blowing agent can be added to the sealed container at any time before the resin particles are expanded. The blowing agent may be added to the aqueous medium together with the resin particles during the dispersion step, and then the resin particles may be impregnated with the blowing agent by heating or other means. Alternatively, the blowing agent may be introduced into the sealed container concurrently with the dispersion step or after completion of the dispersion step to impregnate the multilayer resin particles with the blowing agent. For example, when carbon dioxide is used as a physical blowing agent, a solid blowing agent (specifically, in the form of dry ice) may be added to the aqueous medium together with the multilayer resin particles during the dispersion step, or gaseous carbon dioxide may be introduced by pressurizing the gaseous carbon dioxide into the sealed container during or after completion of the dispersion step. When the resin particles are impregnated with the blowing agent, the impregnation of the resin particles with the blowing agent can be promoted by heating and / or pressurizing the inside of the closed container.

[0076] (Maintenance Step) In order to adjust the crystalline state of the expanded beads, the heating rate of the sealed container may be adjusted in the dispersion step and / or the blowing agent impregnation step, or the temperature and / or time for maintaining the sealed container at a predetermined temperature may be adjusted. For example, the crystalline state of the expanded beads can be adjusted so that an endothermic peak (i.e., a high-temperature peak) appears at a higher temperature than the endothermic peak (i.e., the resin-specific peak) of the main component of the base resin constituting the core layer of the expanded beads in a DSC curve obtained by heat flux differential scanning calorimetry. Expanded beads exhibiting a high-temperature peak are preferred from the viewpoint of broadening the range of molding conditions (specifically, molding temperature and molding pressure) under which a good molded product can be obtained. The adjustment to obtain the high-temperature peak is performed, for example, with reference to the method described in Japanese Patent No. 4077745.

[0077] (Blowing Agent) The blowing agent may be appropriately selected from among common blowing agents used to obtain expanded particles. As the blowing agent, a physical blowing agent is preferred. As the physical blowing agent, an inorganic physical blowing agent and / or an organic physical blowing agent can be used. Examples of inorganic physical blowing agents include carbon dioxide, air, nitrogen, helium, argon, water, etc. Examples of organic physical blowing agents include aliphatic hydrocarbons such as propane, butane, and hexane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; and halogenated hydrocarbons such as 2,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, and trans-1-chloro-3,3,3-trifluoropropene.

[0078] These physical blowing agents may be used alone, or two or more types of physical blowing agents may be used in combination. Among these blowing agents, preferably, blowing agents containing an inorganic physical blowing agent such as carbon dioxide, nitrogen, or air as the main component are used, and more preferably, carbon dioxide is used. In this specification, "containing an inorganic physical blowing agent as the main component" means that the physical blowing agent contains 50 mol% or more of the inorganic physical blowing agent. Preferably, the physical blowing agent contains 70 mol% or more, more preferably 90 mol% or more of the inorganic physical blowing agent, and even more preferably, the physical blowing agent consists solely of the inorganic physical blowing agent.

[0079] The amount of physical foaming agent added is determined appropriately depending on the type of base resin constituting the resin particles, the type of foaming agent, the desired bulk density of the expanded particles, etc. In particular, the amount of physical foaming agent added is preferably determined depending on the desired bulk density. For example, when carbon dioxide is used as the physical foaming agent, the amount of carbon dioxide added is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the multilayer resin particles. The amount of carbon dioxide added as a physical foaming agent (per 100 parts by mass of the multilayer resin particles) can be, for example, a range in which the lower limit is any one of the values ​​in the group consisting of 0.1 parts by mass, 0.5 parts by mass, and 1 part by mass, and the upper limit is any one of the values ​​in the group consisting of 30 parts by mass, 15 parts by mass, and 10 parts by mass (a numerical range not less than the lower limit and not more than the upper limit).

[0080] (Expansion Process) The expansion process is a process in which resin particles containing a blowing agent (i.e., expandable resin particles) are released from a container together with an aqueous medium and expanded to obtain expanded particles. More specifically, the expandable resin particles are expanded by releasing the expandable resin particles together with the aqueous medium under a pressure lower than the internal pressure of the container (specifically, a sealed container). This expansion method makes it possible to easily obtain expanded particles with a low bulk density.

[0081] The bulk density of expanded beads can be adjusted by, for example, appropriately changing the expansion conditions, such as the temperature and pressure, inside the sealed container when releasing the contents of the sealed container during the expansion process. To produce expanded beads with a lower bulk density, a multi-stage expansion process, such as the two-stage expansion process described below, can be performed. In the two-stage expansion process, the expanded beads obtained as described above are first stored in a pressurizable sealed container, and a gas such as air is injected into the sealed container to increase the pressure inside the cells of the expanded beads (i.e., the internal pressure). The expanded beads with increased internal pressure are then removed from the sealed container and heated with steam or hot air to expand the expanded beads, thereby completing the two-stage expansion process. The two-stage expansion process can produce expanded beads with a lower bulk density (two-stage expanded beads). Furthermore, compared to a method of obtaining expanded beads with a low bulk density through a single expansion process, the method of obtaining expanded beads with a low bulk density through the two-stage expansion process makes it easier to increase the cell diameter of the final expanded beads. The expanded bead molding produced using the expanded beads obtained by the two-stage expansion process can further suppress the occurrence of uneven color tone, so that the two-stage expansion process is preferably carried out when producing expanded beads containing a colorant.

[0082] The expanded beads are used, for example, to produce a molded article, which is produced, for example, by molding the expanded beads in a mold.

[0083] Specifically, expanded beads are first filled into a mold having a cavity corresponding to the shape of the molded article to be produced. The expanded beads filled in the mold are then heated using a heating medium such as steam. The expanded beads in the cavity further expand and fuse together due to the heating. This allows the expanded beads to integrate with each other, resulting in a molded article corresponding to the shape of the cavity. Molded articles produced using the expanded beads have excellent fusion properties. Therefore, the mechanical properties inherently required of expanded bead molded articles are exhibited, and expanded bead molded articles are suitable for a variety of applications, such as packaging materials, automotive components, and building materials, which require electrostatic properties.

[0084] The expanded beads of the present invention may be produced by any method other than the above, as long as talc can be attached to and / or incorporated into the surface of the expanded beads. For example, when talc is incorporated into the surface of the expanded beads, the expanded beads may be produced by an extrusion foaming method using an extruder different from that used in the above-described expanded bead production method.

[0085] The expanded beads of the present invention and their molded articles can be used in a wide variety of applications that utilize the electrification phenomenon of the expanded beads or expanded bead molded articles, such as air filters consisting of expanded bead molded articles having interconnected voids obtained by molding the expanded beads of the present invention into a cylindrical shape having a hollow portion in a mold, and expanded bead molded articles that have been subjected to an electrostatic flocking treatment by utilizing the electrostatic charging properties of the expanded bead molded articles of the present invention.

[0086] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to these examples.

[0087] The polypropylene resins used in the examples and comparative examples are as follows: In Tables 1 to 3, the polypropylene resins used in each example and comparative example are designated by the abbreviations PP1 to PP4.

[0088] (Polypropylene Resins) - Abbreviation PP1: Ethylene-propylene random copolymer (melting point 139°C, melt flow rate (230°C, load 2.16 kg) 7.0 g / 10 min, flexural modulus 850 MPa, ethylene content 3.1% by mass) - Abbreviation PP2: Ethylene-propylene random copolymer (melting point 127°C, melt flow rate (230°C, load 2.16 kg) 24 g / 10 min, flexural modulus 700 MPa, ethylene content 4.4% by mass) - Abbreviation PP3: Ethylene-propylene random copolymer (melting point 153°C, melt flow rate (230°C, load 2.16 kg) 8.0 g / 10 min, flexural modulus 1300 MPa, ethylene content 1.4% by mass) PP4: propylene-ethylene-butene random copolymer (melting point 135°C, ethylene component content, melt flow rate (230°C, load 2.16 kg) 5.0 g / 10 min, flexural modulus 750 MPa, ethylene component content 3.8% by mass, butene component content 3.8% by mass)

[0089] The melt mass-flow rates of the polypropylene-based resins indicated by the abbreviations PP1 to PP4 are values ​​measured at 230°C and a load of 2.16 kg in accordance with JIS K7210-1:2014. The flexural modulus of the polypropylene-based resins is a value measured in accordance with JIS K7171:2008.

[0090] The ethylene content or butene content of the polypropylene resins (specifically, ethylene-propylene copolymer and ethylene-propylene-butene copolymer) designated by the abbreviations PP1 to PP4 above is a value determined by a known method using IR spectroscopy. Specifically, the ethylene content or butene content is determined by the method described in "Polymer Analysis Handbook" (edited by the Polymer Analysis Research Forum of the Japan Society for Analytical Chemistry, published in January 1995, published by Kinokuniya Shoten, pages 615-616, "II.2.3 2.3.4 Propylene / ethylene copolymer," and pages 618-619, "II.2.3 2.3.5 Propylene / butene copolymer"), in which the ethylene content or butene content is determined by a quantitative determination method based on the relationship between the absorbance of ethylene and butene corrected by a predetermined coefficient and the thickness of a film-like test piece, etc.

[0091] (Inorganic compounds) Talc: average particle size 2.6 μm Kaolin: average particle size 3 μm

[0092] Example 1 (Production of Multilayer Resin Particles) A ​​production apparatus was used, which included a twin-screw extruder for forming a core layer with an inner diameter of 26 mm, a die for forming a multilayer strand attached downstream of the extruder for forming the core layer, and a single-screw extruder for forming a coating layer with an inner diameter of 25 mm. The production apparatus had a configuration in which the downstream portion of the extruder for forming the coating layer was connected to the die for forming the multilayer strand, and was capable of laminating melts for forming each layer within the die and of co-extrusion. A propylene-ethylene random copolymer listed in Table 1 was used as the base resin constituting the core layer.

[0093] Core layer forming materials (specifically, a base resin (types shown in Table 1), a cell control agent, and carbon black) for forming the core layer were supplied to the extruder for forming the core layer and melt-kneaded. This produced a molten core layer forming resin composition blended with 0.1 mass % of the cell control agent (specifically, zinc borate) and 2.6 mass % of carbon black (specifically, furnace black).

[0094] Materials for forming a coating layer (specifically, a base resin (type shown in Table 1), carbon black (specifically, 2.6% by mass of furnace black), and talc (amounts shown in Table 1)) were supplied to the extruder for forming a coating layer and melt-kneaded. This produced a melt of a resin composition for forming a coating layer, in which the additive concentrations were blended in the amounts shown in Table 1. The base resins used to form the coating layer were those shown in Table 1.

[0095] The extrusion rates of each extruder were adjusted so that the melts for forming each layer were such that the core layer:coating layer ratio was 95:5. The melts were introduced into a multilayer strand-forming die and merged within the die. A composite (specifically, a multilayer strand) having a hollow two-layer structure (a sheath-core structure consisting of a coating layer and a core layer) was extruded through the holes in a die attached downstream of the die. The extruded strand was water-cooled and cut with a pelletizer to obtain multilayer resin particles with an average mass of 1.0 mg per particle. The multilayer resin particles obtained in Example 1 were multilayer hollow resin particles.

[0096] (Production of Expanded Beads) 1 kg of multilayer hollow resin particles was charged into a sealed container with a capacity of 5 L together with 3 L of water as an aqueous medium. Furthermore, 0.004 parts by mass (amount as an active ingredient) of an inorganic dispersant and a surfactant (trade name: NEOGEN S-20F, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) of the type and amount shown in Table 1 were added to the sealed container per 100 parts by mass of the multilayer resin particles. When talc was used as the inorganic dispersant, the talc used as the inorganic dispersant adhered to the surface of the expanded beads.

[0097] Next, carbon dioxide as a blowing agent was injected into the sealed container at room temperature, and the pressure was increased to 1.0 MPa (G) in gauge pressure. In this specification, pressures marked with (G) refer to gauge pressures, i.e., pressure values ​​based on atmospheric pressure. The contents of the sealed container were then heated to the foaming temperature (specifically, 147°C) at a rate of 2°C / min while stirring, and carbon dioxide was injected, and the pressure was increased to 2.0 MPa (G) in gauge pressure, and the container was maintained at that temperature for 15 minutes. This adjusted the crystalline state of the expanded beads so that the expanded beads would have a high-temperature peak in the endothermic curve measured by DSC.

[0098] Thereafter, the contents of the sealed container (specifically, resin particles and water) were released under atmospheric pressure to obtain expanded particles (specifically, first-stage expanded particles).

[0099] The first-stage expanded beads obtained as described above were left to cure for 24 hours in an environment of 60°C, 50% relative humidity, and 1 atm. The cured first-stage expanded beads were then loaded into a pressurizable sealed container, and the pressure inside the sealed container was increased from atmospheric pressure to pressurize the expanded beads. While maintaining the pressurized state of the expanded beads, the pressure inside the cells of the expanded beads was increased, and the first-stage expanded beads were removed from the sealed container to obtain first-stage expanded beads with an internal cell pressure of 0.5 MPa (G). The first-stage expanded beads were then fed into a second-stage expansion device. Steam was supplied into the device to expand the first-stage expanded beads, and the resulting second-stage expanded beads were dried at 40°C for 12 hours to obtain second-stage expanded beads. The expanded beads obtained by second-stage expansion were used for the following measurements and for the production of expanded bead moldings. The physical properties of the resulting expanded beads are shown in Table 1.

[0100] (Production of Molded Article) Expanded beads (specifically, two-stage expanded beads) were filled into a pressurizable sealed container, and the pressure inside the sealed container was increased from normal pressure to pressurize the expanded beads. The pressurized state of the expanded beads was maintained for 24 hours to increase the pressure inside the cells of the expanded beads. The expanded beads were then removed from the sealed container, and expanded beads with an internal cell pressure of 0.1 MPa (G) were obtained. These expanded beads were filled into a mold (specifically, a die) having a molding cavity capable of molding a plate-shaped molded article measuring 200 mm long x 250 mm wide x 50 mm high, and molding was performed using the following heating method. Steam was supplied to the mold with drain valves on both sides open to perform preheating (exhaust process). Steam was then supplied from one side of the mold to heat it, and then steam was further supplied from the other side to heat it. Subsequently, steam was supplied from both sides of the mold to heat it at the molding pressure (molding heating steam pressure) listed in Table 1. After heating, the pressure was released and the molded product was water-cooled until the surface pressure due to the foaming force of the molded product reached 0.04 MPa (G), after which the mold was opened and the molded product was removed. This molded product was cured in an oven at 80°C for 12 hours and then slowly cooled to room temperature to obtain a box-shaped molded product with an open top. The physical properties of the obtained molded product are shown in Table 1.

[0101] In Examples 2 and 3, the preparation was carried out in the same manner as in Example 1, except that the amount of talc added to the coating layer was changed. The conditions for Examples 2 and 3, and the physical properties of the expanded beads and molded articles obtained in Examples 2 and 3 are shown in Table 1.

[0102] Examples 4 and 5 were prepared in the same manner as in Example 1, except that the base resin of the core layer or the coating layer was changed as shown in Table 1. The conditions for Examples 4 and 5, and the physical properties of the expanded beads and molded articles obtained in Examples 4 and 5 are shown in Table 1.

[0103] Example 6 was produced in the same manner as Example 1, except that the expanded beads were cylindrical. The conditions for Example 6 and the physical properties of the expanded beads and molded article obtained in Example 6 are shown in Table 1.

[0104] In the following Examples 7 and 8 to 12, no talc was contained in the coating layer, and talc was attached to the surface of the multi-layer expanded beads.

[0105] Example 7 (Production of Multilayer Resin Particles) A ​​production apparatus was prepared, including a twin-screw extruder for forming a core layer with an inner diameter of 26 mm, a die for forming a multilayer strand attached downstream of the extruder for forming a core layer, and a single-screw extruder for forming a coating layer with an inner diameter of 25 mm. The production apparatus had a configuration in which the downstream portion of the extruder for forming a coating layer was connected to the die for forming a multilayer strand, and was configured to enable lamination of melts for forming each layer within the die and to enable co-extrusion. A propylene-ethylene random copolymer listed in Table 2 was used as the base resin constituting the core layer.

[0106] The core layer forming materials (specifically, base resin: Table 2, cell control agent, 2.6% by mass of carbon black) for forming the core layer were fed into the extruder for forming the core layer and melt-kneaded. This produced a melt of the resin composition for forming the core layer, blended with 0.1% by mass of the cell control agent (specifically, zinc borate) and 2.6% by mass of carbon black (specifically, furnace black). The melt of the resin composition for forming the coating layer was produced using the same method as in Example 1, except that the addition of talc was omitted. Based on each melt, resin particles were obtained using the same conditions and method as in Example 1.

[0107] (Production of Expanded Beads) 1 kg of resin particles was supplied to a sealed container having a capacity of 5 L together with 3 L of water as an aqueous medium. Furthermore, talc (inorganic dispersant) and 0.004 parts by mass of a surfactant (trade name: NEOGEN S-20F, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., sodium dodecylbenzenesulfonate) in the amounts shown in Table 1 were added to the sealed container relative to 100 parts by mass of the resin particles, to prepare a dispersion system in which the contents were dispersed in the dispersion medium.

[0108] Next, carbon dioxide as a blowing agent was injected into the sealed container at room temperature, and the pressure was increased to 1.0 MPa (G) in gauge pressure. In this specification, pressures marked with (G) refer to gauge pressures, i.e., pressure values ​​based on atmospheric pressure. The sealed container was then heated at a rate of 2°C / min while stirring to the foaming temperature (specifically, 147°C). Carbon dioxide was then injected into the sealed container to increase the pressure in the sealed container to 2.0 MPa (G) in gauge pressure, and the pressure and foaming temperature were maintained for 15 minutes. By maintaining the pressure and temperature in the sealed container, the crystalline state of the expanded beads was adjusted so that the expanded beads had a high-temperature peak in the endothermic curve measured by DSC.

[0109] Thereafter, the contents of the sealed container (specifically, resin particles and water) were released under atmospheric pressure to obtain expanded particles (specifically, first-stage expanded particles).

[0110] The steps after the formation of the first-stage expanded beads were the same as in Example 1 to obtain expanded beads and a molded article made from expanded beads. The conditions for Example 7 and the physical properties of the expanded beads and molded article obtained in Example 7 are shown in Table 2.

[0111] Examples 8 to 12 In Examples 8 and 9, expanded beads and expanded bead molded articles were obtained by carrying out the same steps as in Example 7, except that various conditions were changed as shown in Table 2. In Examples 10 and 11, expanded beads and expanded bead molded articles were obtained by carrying out the same steps as in Example 7, except that the base resin of the core layer or coating layer was changed as shown in Table 2. In Example 12, expanded beads and expanded bead molded articles were obtained by carrying out the same steps as in Example 7, except that the shape of the expanded beads was changed to a cylindrical shape. Table 2 shows the conditions for each of Examples 8 to 12, and the physical properties of the expanded beads and molded articles obtained in each Example.

[0112] The bulk density, total heat of fusion, high-temperature peak heat, and average cell diameter of the expanded beads obtained in each of the Examples and Comparative Examples were measured as follows.

[0113] (Measurement of Bulk Density of Expanded Beads) First, a plurality of expanded beads (expanded beads) to be measured were left for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. Thereafter, a mass W (unit: g) of expanded beads was filled into a measuring cylinder, and the bottom of the measuring cylinder was lightly tapped against the floor several times to stabilize the filling height of the expanded beads in the measuring cylinder. The bulk volume V (unit: L) of the expanded beads indicated on the measuring cylinder was read, and the value obtained by dividing the mass W of the expanded beads by the bulk volume V of the expanded beads (i.e., W / V) was calculated. The obtained value was converted into units to determine the bulk density (unit: kg / m) of the expanded beads. 3 ) was obtained.

[0114] (Measurement of total heat of fusion and high-temperature peak heat quantity) Approximately 2 mg of expanded beads were collected from the expanded beads after curing or drying. These expanded beads were used as test pieces, and a DSC curve was obtained by heating the test piece from 23°C to 200°C at a heating rate of 10°C / min using a differential scanning calorimeter (specifically, a DSC7020 manufactured by Hitachi High-Technologies Corporation). The area of ​​all melting peaks in the DSC curve was determined, and this was taken as the total heat of fusion. In addition, the area of ​​the high-temperature peak in the DSC curve was determined, and this was taken as the high-temperature peak heat quantity. The above measurements were performed on five expanded beads, and the arithmetic average values ​​were used as the measurement results for the total heat of fusion and the high-temperature peak heat quantity.

[0115] (Average Cell Diameter) An expanded bead was roughly divided into two parts passing through the center of the expanded bead, and a photograph of the cut surface (cross-sectional photograph) was taken using a scanning electron microscope. In the obtained cross-sectional photograph, four line segments were drawn at equal angles from the outermost surface of the expanded bead through the center to the outermost surface on the opposite side. The number of cells intersecting each line segment was counted, and the total length of the four line segments was divided by the total number of cells intersecting the lines to obtain the average cell diameter of one expanded bead. This operation was performed on 10 randomly selected expanded beads, and the arithmetic mean of the values ​​obtained for each expanded bead was used as the average cell diameter of the expanded beads in this specification.

[0116] The apparent density, fusion property, and withstand voltage attenuation rate of the molded bodies obtained in each of the Examples and Comparative Examples were measured as follows: The tensile strength of the molded bodies and the tensile strength / density of the molded bodies were measured using the methods described above.

[0117] (Measurement of green body density) The density (apparent density (unit: kg / m)) was determined by dividing the mass of the green body by the volume calculated based on the green body dimensions. 3 ) was calculated.

[0118] (Evaluation of fusion property) When the molded body was broken, the number of foamed beads (A) present on the fracture surface due to material destruction was divided by the total number of foamed beads (B) present on the fracture surface (see formula (2) below), and the result was expressed as a percentage to determine the fusion rate. A value of 80% or more was considered acceptable and indicated as ◯ in Table 1, and a value of less than 80% was considered unacceptable and indicated as × in Table 1. Fusion rate = A / B × 100% (2)

[0119] (Measurement of Electrostatic Discharge Decay) A test piece having dimensions of 45 mm length x 45 mm width x 5 mm thickness was cut out from the surface of the produced molded body. One of the two faces of the cut-out test piece, which is defined as 45 mm length x 45 mm width, has the skin derived from the surface of the molded body remaining. Using the cut-out test piece, an applied voltage of +10 kV was measured in accordance with JIS L1094:2014 Method A, and the initial electrostatic discharge voltage (0 seconds) V 0 (kV) and the charged voltage V 120 seconds after the application was stopped 120 The electrostatic voltage decay rate was calculated based on the electrostatic potential (kV) and the following formula (3) (note that no treatment was performed to remove the inorganic dispersant adhering to the test piece sample). 0 -V 120 ) x 100 / V 0 ...(3)

[0120] The surface talc amount (abundance) of the expanded beads and molded articles obtained in each Example and Comparative Example was determined using the method described below in "Measurement of the amount of talc present in multilayer expanded beads and in expanded bead molded articles."

[0121] (Measurement of the Amount of Talc Present in Multilayer Expanded Beads and in Expanded Bead Molded Products) (1) Examples 1 to 6 and Comparative Example 2 (Procedure 1) Preparation of a Calibration Curve A calibration curve defining the relationship between the amount of talc present and the absorption intensity described below was established as follows. First, to prepare the calibration curve, a solid sheet (a sheet of polypropylene resin with a known talc content) (50 μm thick) was prepared by kneading a predetermined amount of talc into polypropylene resin. An MC-15HT kneader manufactured by Xplore was used to prepare the solid sheet. Talc and polypropylene resin were kneaded using the kneader at 200°C, 50 rpm, and for 3 minutes to obtain polypropylene pellets. The polypropylene pellets were then formed into a solid sheet at 200°C using a heat press, and the solid sheet was then cooled to room temperature to prepare a sheet approximately 50 μm thick. The sheet surface of this "solid sheet in which talc is kneaded into a polypropylene-based resin" was brought into close contact with a prism and measured by the ATR method using an infrared spectrophotometer, and the infrared absorption spectrum of the solid sheet was obtained. Based on the infrared absorption spectrum of the solid sheet, a peak attributable to talc was observed at a wavelength of 1000 cm -1 A peak recognized around the wavelength of 650 cm (referred to as the first absorption peak) -1 A peak recognized near the first absorption peak (referred to as the second absorption peak) was identified. Based on the infrared absorption spectrum of the solid sheet, two types of calibration curves were created that define the relationship between the absorption intensity (absorbance value) at these absorption peaks and the amount of talc added to the solid sheet (amount of talc present). The two types of calibration curves define the relationship between the absorption intensity at the first absorption peak and the amount of talc present (wavelength 1000 cm). -1 The first calibration curve is based on an absorption peak near the wavelength of 650 cm. The second calibration curve defines the relationship between the absorption intensity at the second absorption peak and the amount of talc present. -1(Step 2) Measurement of Samples The expanded beads produced in each of Examples 1 to 6 and Comparative Example 2 were held with tweezers and their surfaces were rubbed with a Kimtowel 10 times to remove the inorganic dispersant adhering to the surface, thereby producing expanded beads from which the adhering kaolin had been removed. The surfaces of these expanded beads were used as measurement samples. Then, the expanded bead surfaces of the measurement samples were subjected to a pressure of 340 kg / cm under the following measurement conditions. 2 The expanded beads were pressed tightly against a prism with a pressing force of 1000 Hz, infrared light was incident, and the totally reflected light was measured to obtain an infrared absorption spectrum (without ATR correction). Separately, the expanded beads produced in each of Examples 1 to 6 and Comparative Example 2 were cut into approximately two equal parts passing through their centers so that the volumes were roughly equal, to obtain measurement samples. The cut surfaces of the measurement samples were pressed tightly against a prism, infrared light was incident in the same manner as above, and the totally reflected light was measured to obtain an infrared absorption spectrum (without ATR correction). The infrared absorption spectrum corresponding to the talc present in the coating layer of the expanded beads was obtained as the difference spectrum between the two spectra. (Procedure 3) Calculation of the amount of talc present on the surface of the expanded beads The amount of talc present on the surface of the expanded beads was calculated using the 1000 cm wavelength talc as the calibration curve prepared in Procedure 1. -1 The first calibration curve was created using a peak near the wavelength of 650 cm. -1 The amount of talc present on the surface of the expanded beads was calculated from the difference spectrum measured in step 2, i.e., the absorption intensity of the peak corresponding to talc present in the coating layer of the expanded beads, using the second calibration curve prepared by employing the peak around the wavelength of 1000 cm mentioned above. -1 The amount of talc present on the surface of the expanded beads was calculated using the first calibration curve created by using a peak in the vicinity of the wavelength of 1000 cm. -1 If an accurate difference spectrum around 650 cm cannot be determined, -1 The amount of talc present on the surface of the expanded beads was calculated using a second calibration curve prepared using a peak in the vicinity of the wavelength of 1000 cm. -1 When an accurate difference spectrum cannot be determined in the vicinity of the wavelength of 1000 cm, for example, when determining the infrared absorption spectrum (difference spectrum) of the surface portion of the expanded beads measured in (Procedure 2), -1Examples of such cases include when the absorption intensity of a peak near the expanded bead is equal to or exceeds the upper limit of detectability in infrared spectrophotometer measurements. Since it is unlikely that talc other than the talc present in the expanded bead is mixed in during the manufacturing process (talc contamination during the manufacturing process), talc is present only in the coating layer of the expanded bead. The amount of talc present on the surface of the expanded bead is the amount of talc calculated based on the infrared absorption spectrum measured by the above-described method and the calibration curve (the "amount of talc present on the surface"). (2) Examples 7 to 12 and Comparative Examples 1, 3, and 4: Calibration curves defining the relationship between the amount of talc present and the absorption intensity described below were established using the same method as in "Procedure 1" of (1) Examples 1 to 6 and Comparative Example 2. Difference spectra were measured using the expanded beads produced in Examples 7 to 12 and Comparative Examples 1, 3, and 4. Talc adhered to the surface of the expanded beads in Examples 7 to 12 and Comparative Examples 1, 3, and 4. Therefore, the surface portion of the expanded beads was used as the measurement sample. Specifically, the procedure of "holding the expanded beads with tweezers and rubbing their surfaces with a Kimtowel 10 times to remove the inorganic dispersant adhering to the surface" was omitted, and the surface portion of the expanded beads was used as the measurement sample. A difference spectrum was measured based on the measurement sample using the surface portion of the expanded beads. The difference spectrum was obtained using the same method as in "Procedure 2" of (1) Examples 1 to 6 and Comparative Example 2 described above. For each of Examples 7 to 12 and Comparative Examples 1, 3, and 4, the amount of talc present in the surface portion of the expanded beads was calculated using the same method as in "Procedure 3" of (1) Examples 1 to 6 and Comparative Example 2 described above. That is, the amount of talc present in the surface portion of the expanded beads was calculated based on the calibration curve and difference spectrum. Since talc contamination during the manufacturing process is unlikely, talc adheres only to the surface of the expanded beads, and the amount of talc present in the surface portion of the expanded beads is the amount of talc present calculated based on the calibration curve and difference spectrum. <Measurement conditions> Prism: zinc selenide Incident angle of infrared light: 45° Number of accumulations: 512 times Resolution: 4 cm -1 Detector: TGS (Triglycine sulfate) Measurement wave number range: 600 to 4000 cm-1 Number of reflections: 1 Measurement area: Area up to 20 μm from the surface Apparatus: FT / IR-4600 type A (ATR PRO450-S type) manufactured by JASCO Corporation

[0122] (3) Amount of Talc Present in Expanded Bead Molded Articles The amount of talc present in the expanded bead molded articles produced in each of Examples 1 to 12 and Comparative Examples 1 to 4 was also measured by applying the same method as described in "Procedure 1" to "Procedure 3" in (1) Examples 1 to 6 and Comparative Example 2, except that the measurement target was changed from expanded beads to expanded bead molded articles. The measurement results are shown in the column for surface talc amount (abundance) in the molded article evaluation column in Tables 1, 2, and 3.

[0123] Tables 1, 2, and 3 show the value of the amount of CB (wt%) / surface talc (wt%) present. The surface talc (wt%) is determined based on the measured amount of talc present described above. CB (wt%) is the carbon content in the expanded beads, and in Examples 1 to 12 and Comparative Examples 1 to 4, it is the carbon black content.

[0124] Comparative Example 1: Expanded beads and a molded article were prepared in the same manner as in Example 1, except that talc was not added to the coating layer. Table 3 shows the various conditions and the physical properties of the resulting expanded beads and molded article. Comparative Example 1 had a higher electrostatic decay rate compared to Example 1, etc. Comparative Example 2: Expanded beads and a molded article were prepared in the same manner as in Example 1, except that the amount of talc added to the coating layer was below the lower limit of the claimed range. Table 3 shows the resin beads and expansion process conditions, as well as the physical properties of the resulting expanded beads and molded article. Comparative Example 2 had a higher electrostatic decay rate compared to Example 1, etc. Comparative Example 3: Expanded beads were prepared in the same manner as in Example 4, except that the amount of talc added as an inorganic dispersant during the production of expanded beads was reduced. The dispersibility in the furnace during the production of expanded beads was low, and stable production of expanded beads was not possible. Table 3 shows the resin beads and expansion process conditions, as well as the physical properties of the resulting expanded beads. In Comparative Example 3, the amount of expanded beads obtained was small, so a molded article could not be obtained, and the physical properties of the molded article could not be measured. Comparative Example 4 Expanded beads were produced in the same manner as in Example 4, except that the amount of talc added as an inorganic dispersant during the production of expanded beads was increased. The resin beads, the expansion process conditions, and the physical properties of the expanded beads are shown in Table 3. In Comparative Example 4, the fusion properties of the expanded beads were low, and stable production of an expanded bead molded article was not possible. The physical properties of the molded article could not be measured because a molded article could not be obtained.

[0125]

[0126]

[0127]

[0128] 1A Single-layer expanded particle 1B Multi-layer expanded particle 2 Core layer 3 Coating layer 4 Expanded layer 5 Talc

Claims

1. A polypropylene resin foamed bead molding containing carbons, in which talc is present on the surface of the foamed bead molding, and the initial charging voltage V when a voltage of +10 kV is applied is measured based on JIS L1094:2014 A method. 0 and the charged voltage V 120 seconds after the application was stopped 120 and a polypropylene resin foamed bead molding, characterized in that the following formula (1) is satisfied. 0 -V 120 ) x 100 / V 0 ≦ 25 ... (1) 2. The expanded polypropylene resin bead molding according to claim 1, wherein the amount of talc present in the surface portion of the expanded bead molding is 500 ppm by mass or more and 9,000 ppm by mass or less.

3. The density of the foamed bead molding is 15 kg / m 3 More than 300kg / m 3 3. The expanded polypropylene resin bead molding according to claim 1, wherein the fusion rate of the expanded polypropylene resin bead molding is 80% or more.

4. A polypropylene-based resin expanded particle containing carbons, characterized in that talc is present on the surface portion of the expanded particle, and the amount of talc present on the surface portion of the expanded particle is 600 ppm by mass or more and 10,000 ppm by mass or less.

5. The polypropylene-based resin expanded beads according to claim 4, which are multi-layered expanded beads having a polypropylene-based resin expanded core layer and a coating layer covering the expanded core layer, and at least the coating layer contains carbons.

Citation Information

Patent Citations

  • Molded body of foamed polymer chips having gap

    JP1995137063A

  • Foamed colored polypropylene resin particle and colored molded polypropylene resin foam produced therefrom

    JP1995300537A

  • Polyproylene based resin foam particle, process for production of polyproylene based resin foam particle molded propduct and polyproylene based resin foam particle molded product

    JP2006307177A

  • Polyolefin resin in-mold foam molding

    JP4077745B2

  • Expansion molding granular polyolefin material

    JP1985067543A