Regenerated cellulose fiber for resin reinforcement, method for producing discoloration-inhibited regenerated cellulose fiber, resin composition, pellet and method for producing same, and molded article

By adding glycerin and boric acid to regenerated cellulose fibers, the thermal stability and color retention are enhanced, addressing the issue of discoloration in resin compositions and molded articles, resulting in improved performance and appearance.

WO2024247871A1PCT designated stage expired Publication Date: 2024-12-05DAICEL CORP +1

Patent Information

Application Number
PCT/JP2024/018975
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Regenerated cellulose fibers used for resin reinforcement have low thermal stability, leading to discoloration and performance deterioration when heated, resulting in poor appearance in resin compositions and molded articles.

Method used

Incorporating a compound such as glycerin and boric acid into regenerated cellulose fibers to enhance thermal stability, preventing coloration during heating processes, and using these fibers in conjunction with thermoplastic or thermosetting resins to create a resin composition that maintains appearance integrity.

Benefits of technology

The treated regenerated cellulose fibers and resin compositions exhibit suppressed coloration and improved thermal stability, reducing the likelihood of appearance defects in molded products, making them suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018975_05122024_PF_FP_ABST
    Figure JP2024018975_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A first problem is to provide a discoloration-inhibited regenerated cellulose fiber for resin reinforcement. A second problem is to provide, inter alia, a regenerated cellulose fiber-containing resin composition that is resistant to the heat-induced generation of a poor appearance. A third problem is to provide a method for producing a discoloration-inhibited regenerated cellulose fiber. The first problem can be solved by a regenerated cellulose fiber for resin reinforcement, that contains at least one compound (A) selected from weak acids and monohydric and higher hydric alcohols. The second problem can be solved by a resin composition comprising: a regenerated cellulose fiber containing at least one compound (A) selected from weak acids and monohydric and higher hydric alcohols; and a thermoplastic resin or a thermosetting resin. The third problem can be solved by a method for producing a regenerated cellulose fiber, the method comprising heating the aforementioned regenerated cellulose fiber at 200-300°C.
Need to check novelty before this filing date? Find Prior Art

Description

Regenerated cellulose fiber for resin reinforcement, method for producing regenerated cellulose fiber with suppressed coloration, resin composition, pellets and method for producing the same, and molded product

[0001] The present invention relates to regenerated cellulose fibers for resin reinforcement, a method for producing regenerated cellulose fibers with reduced discoloration, a resin composition, pellets and a method for producing the same, and a molded article.

[0002] Cellulose fibers are fibers containing cellulose, the main component of wood, and are classified into plant fibers, regenerated fibers (regenerated cellulose fibers), semi-synthetic fibers, cellulose nanofibers, etc. Such cellulose fibers are not limited to applications such as clothing, but are also widely used as industrial raw materials for food, cosmetics, functional paper, etc.

[0003] Regenerated cellulose fibers can be produced by various methods, such as the viscose method, the cuprammonium method, the solvent method, etc. In recent years, in response to growing environmental awareness, regenerated cellulose fibers made from cellulose, a biomass-derived material, have been used as modifiers and reinforcing materials for resins (see, for example, Patent Document 1, etc.).

[0004] When regenerated cellulose fibers are used as a reinforcing material for resins, methods such as blending short regenerated cellulose fibers into a resin to obtain a regenerated cellulose fiber-reinforced resin composition and impregnating continuous regenerated cellulose fibers with a resin and then cutting them to a desired length to obtain a resin material reinforced with regenerated cellulose fibers (resin-impregnated long fiber bundles) are known. On the other hand, regenerated cellulose fibers have low thermal stability, and heating can cause deformation and discoloration of the appearance, resulting in performance degradation. Therefore, for example, in resin compositions containing regenerated cellulose fibers, heating during the preparation of the resin composition and / or during the production of molded articles from the resin composition can cause discoloration of the regenerated cellulose fibers, resulting in poor appearance.

[0005] JP 2017-95831 A

[0006] The first object of the present invention is to provide regenerated cellulose fibers for resin reinforcement that are suppressed in discoloration. The second object is to provide a resin composition containing regenerated cellulose fibers that is less likely to suffer from poor appearance due to heating, pellets of the resin composition, a method for producing the pellets, and molded articles. The third object is to provide a method for producing regenerated cellulose fibers that are suppressed in discoloration.

[0007] That is, the present invention has the following aspects. [1] Regenerated cellulose fibers for resin reinforcement, comprising at least one compound (A) selected from a monohydric or higher alcohol and a weak acid. [2] Regenerated cellulose fibers according to [1], wherein the proportion of the compound (A) per 100 parts by mass of the regenerated cellulose fibers is 0.01 to 20 parts by mass. [3] Regenerated cellulose fibers according to [1] or [2], wherein the alcohol comprises glycerin and the weak acid comprises boric acid. [4] Resin composition comprising regenerated cellulose fibers comprising at least one compound (A) selected from a monohydric or higher alcohol and a weak acid, and a thermoplastic resin. [5] Resin composition comprising regenerated cellulose fibers comprising at least one compound (A) selected from a monohydric or higher alcohol and a weak acid, and a thermosetting resin. [6] Resin composition according to [4] or [5], wherein the proportion of the compound (A) per 100 parts by mass of the regenerated cellulose fibers is 0.01 to 20 parts by mass. [7] The resin composition according to any one of [4] to [6], wherein the alcohol comprises glycerin and the weak acid comprises boric acid. [8] Pellets of the resin composition according to [4], [6], or [7]. [9] A molded product of the resin composition according to any one of [4] to [7].

[10] A method for producing regenerated cellulose fibers with reduced discoloration, comprising heating the regenerated cellulose fibers according to any one of [1] to [3] at 200 to 300°C.

[11] A method for producing the regenerated cellulose fibers according to

[10] , wherein the heating comprises applying a heat load of 200 to 300°C to at least the surface of the regenerated cellulose fibers.

[12] A method for producing pellets according to [8], comprising impregnating the regenerated cellulose fibers with the molten thermoplastic resin, or melt-kneading the regenerated cellulose fibers with the thermoplastic resin.

[13] The method for producing pellets according to

[12] , wherein the temperature of the molten thermoplastic resin or the melt-kneading temperature is 200 to 300°C.

[14] The method for producing pellets described in

[12] or

[13] , wherein the impregnation with the molten thermoplastic resin or the melt-kneading includes reacting the regenerated cellulose fiber with the compound (A).

[0008] The present invention can solve the first to third problems described above. Specifically, it can provide regenerated cellulose fibers for resin reinforcement that are suppressed in discoloration. It can also provide a resin composition containing regenerated cellulose fibers that are less likely to suffer from poor appearance due to heating, pellets of the resin composition, a method for producing the pellets, and molded articles. It can also provide a method for producing regenerated cellulose fibers that are suppressed in discoloration.

[0009] 1 is a photograph of the regenerated cellulose fibers of Example 2 and Comparative Example 2 after heating, 2 is a photograph of the pellets of Example 3 and Comparative Example 3 before heating, and 3 is a photograph of the pellets of Example 3 and Comparative Example 3 after heating.

[0010] An embodiment of the present disclosure will be described in detail below. However, the scope of the present disclosure is not limited to the embodiment described herein, and various modifications can be made without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Furthermore, when multiple upper and lower limit values ​​are described for a specific parameter, any of these upper and lower limit values ​​can be combined to form a suitable numerical range. Furthermore, the lower and / or upper limit values ​​of a numerical range described in this disclosure are numerical values ​​within that range and may be replaced with numerical values ​​shown in the examples. The expression "X to Y" indicating a numerical range means "X or greater and Y or less." If a specific description described for one embodiment also applies to other embodiments, that description may be omitted in other embodiments. Each configuration and combination thereof in each embodiment is merely an example, and additions, omissions, substitutions, and other modifications of configurations are possible as appropriate within the spirit of the present disclosure. The present disclosure is not limited by the embodiments. Each feature disclosed herein may be combined with any other feature disclosed herein.

[0011] A first embodiment of the present invention relates to regenerated cellulose fibers for resin reinforcement.

[0012] [Regenerated cellulose fiber for resin reinforcement] The first embodiment relates to a regenerated cellulose fiber for resin reinforcement, which contains at least one compound (A) selected from monohydric or higher alcohols and weak acids. The regenerated cellulose fiber according to the first embodiment is less likely to discolor when heated than conventional regenerated cellulose fibers. Therefore, when blended into a resin as a resin reinforcing material, discoloration is less likely to occur when heated during preparation of the resin composition or molding of the resin composition.

[0013] <Compound (A)> The regenerated cellulose according to the first embodiment contains at least one compound (A) selected from monohydric or higher alcohols and weak acids. Examples of the monohydric or higher alcohol include alcohols having 1 to 20 carbon atoms. Specific examples include monohydric alcohols such as methanol, ethanol, propanol, isopropanol, butanol, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, benzyl alcohol, and phenethyl alcohol; linear polyhydric alcohols such as mannitol, glycerin, erythritol, pentaerythritol, xylitol, glucitol, and ethylene glycol; and phenols such as phenol, para-cresol, meta-cresol, ortho-cresol, ethylphenol, guaiacol, and catechol. These compounds may be used alone or in combination. Among these compounds, glycerin, mannitol, methanol, erythritol, or ethylene glycol is preferred, and glycerin, mannitol, or erythritol is more preferred, from the viewpoint of easily suppressing coloration of the fibers during heating.

[0014] Examples of weak acids include acetic acid, boric acid, boric acid compounds, etc. Among these, it is more preferable to contain boric acid or a boric acid compound, and it is even more preferable to contain boric acid.

[0015] Examples of the boric acid compound include borate salts such as alkali metal salts, alkaline earth metal salts, and metal salts; metaboric acid and its salts; polyboric acid and its salts; etc. These boric acid compounds may be used alone or in combination of two or more.

[0016] In one embodiment, the regenerated cellulose fibers preferably contain at least one selected from glycerin and boric acid as compound (A), more preferably glycerin or boric acid. In one embodiment, the compound (A) may contain at least one selected from boric acid, glycerin, pentaerythritol, and mannitol.

[0017] In one embodiment, the ratio of compound (A) to 100 parts by mass of regenerated cellulose fibers is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and even more preferably 0.5 to 15 parts by mass. If the ratio of compound (A) is within this range, when compound (A) is blended into a resin as a resin reinforcing material, the fibers are less likely to be discolored by heating during preparation of the resin composition and / or molding of the resin composition. In one embodiment, the ratio of compound (A) to 100 parts by mass of regenerated cellulose fibers may be in the range of 0.01 to 20 parts by mass, 0.03 to 15 parts by mass, or 0.05 to 10 parts by mass.

[0018] In one embodiment, the regenerated cellulose fibers may be continuous fibers, short fibers, or spun fibers formed by twisting short fibers into a long thread. The method for producing the regenerated cellulose fibers is not particularly limited, and may be continuous fibers obtained from solvent-process regenerated cellulose such as viscose rayon, cupra, lyocell, or ionic liquid.

[0019] The average fiber diameter of the regenerated cellulose fibers is not particularly limited. From the viewpoint of use as a resin reinforcing material, it may be 5 to 50 μm or 7 to 30 μm. The average fiber diameter of the regenerated cellulose fibers can be the average value of the major axes of the fiber cross sections measured under a microscope.

[0020] In the regenerated cellulose fibers according to the first embodiment, the compound (A) is preferably attached to at least a portion of the surface of the regenerated cellulose fibers. Furthermore, a portion of the compound (A) may react with the reducing terminal or hydroxyl groups of the regenerated cellulose fibers. For example, when the compound (A) contains glycerin, all of the glycerin contained in the regenerated cellulose fibers may be attached (coated) to at least a portion of the fiber surface, or a portion of the glycerin may react with the reducing terminal of the regenerated cellulose, with the remaining glycerin attached to at least a portion of the fiber surface. Furthermore, when a weak acid (preferably boric acid) is contained, all of the weak acid may be attached (coated) to at least a portion of the fiber surface, or a portion of the weak acid may react with the hydroxyl groups of the regenerated cellulose, with the remaining weak acid attached to at least a portion of the fiber surface.

[0021] It is believed that the regenerated cellulose fibers according to the first embodiment contain compound (A), and when heated in a resin composition, compound (A) reacts with the reducing end or hydroxyl group of the regenerated cellulose, resulting in improved thermal stability. That is, when a resin composition containing such regenerated cellulose fibers is heated (for example, during melt-kneading to prepare a resin composition or heat treatment to obtain a molded product), compound (A) reacts with the reducing end or hydroxyl group of the regenerated cellulose fibers at the temperature, thereby suppressing the coloring of the fibers during heating. Such regenerated cellulose fibers can be suitably used as a resin reinforcing material.

[0022] <Method for producing regenerated cellulose fibers for resin reinforcement> As a method for producing regenerated cellulose fibers according to the first embodiment, from the viewpoint of effectively incorporating compound (A) into the regenerated cellulose fibers (preferably attaching compound (A) to at least a portion of the fiber surface), a method comprising immersing regenerated cellulose fibers (raw fiber) in compound (A) or an aqueous medium containing compound (A) and then drying the fibers, or alternatively, dropping (including spraying) compound (A) alone or an aqueous medium containing compound (A) onto the raw fiber and then drying the fibers is preferred. Hereinafter, one embodiment of the method for producing regenerated cellulose fibers according to the first embodiment will be described.

[0023] When producing regenerated cellulose fibers containing a monohydric or higher alcohol, preferably glycerin, as compound (A), it is preferable to immerse the raw fiber in compound (A) or to add compound (A) alone dropwise to the raw fiber, and then dry the raw fiber.

[0024] When producing regenerated cellulose fibers containing a weak acid, preferably boric acid, as compound (A), it is preferable to immerse the raw fiber in an aqueous medium containing compound (A) or to add the aqueous medium containing compound (A) dropwise to the raw fiber, and then dry the raw fiber.

[0025] When an aqueous medium containing compound (A) is used, the aqueous medium may be an aqueous solution of compound (A) or an emulsion (dispersion) in which compound (A) is dispersed. The water component contained in the aqueous medium may be pure water, ion-exchanged water, tap water, industrial water, or a mixture thereof. From the viewpoint of cost, the water component is preferably tap water or industrial water. The aqueous medium may also contain optional components other than the water component and compound (A).

[0026] In one embodiment, the proportion of compound (A) relative to the total mass of the aqueous medium is preferably 0.1 to 50% by mass, more preferably 0.3 to 15% by mass, and particularly preferably 0.3 to 10% by mass. By using an aqueous medium having a compound (A) concentration within the above range, it becomes easier to control the proportion of compound (A) relative to 100 parts by mass of the finally obtained regenerated cellulose fibers to the range of 0.01 to 20 parts by mass.

[0027] The temperature of the aqueous medium is not particularly limited and can be set depending on the solubility of the compound (A) in the water component. For example, when the compound (A) contains boric acid, the saturated aqueous solution concentration of boric acid at 20°C is less than 5% by mass. Therefore, for example, when preparing a 9% by mass aqueous solution of boric acid, it is preferable to set the temperature of the aqueous medium to 50°C or higher.

[0028] When raw fibers are immersed in an aqueous medium containing compound (A) or when the aqueous medium is dripped onto the raw fibers, it is preferable to adjust the amount of aqueous medium absorbed by the raw fibers and the amount of aqueous medium coexisting around the raw fibers. Specifically, it is more preferable to adjust the "ratio of aqueous medium to the total mass of raw fibers before immersion in the aqueous medium or before dripping the aqueous medium" (hereinafter referred to as the "aqueous medium ratio") to 200% by mass or less. By adjusting the aqueous medium ratio to 200% by mass or less and then drying, the drying efficiency is likely to be improved and the discoloration suppression effect of the finally obtained regenerated cellulose fibers is likely to be improved.

[0029] In one embodiment, the aqueous medium ratio may be adjusted to 150% by mass or less, or 100% by mass or less. The lower limit is preferably 10% by mass or more. That is, the aqueous medium ratio may be adjusted to 10 to 200% by mass, 10 to 150% by mass, or 10 to 100% by mass.

[0030] The method for adjusting the aqueous medium ratio is not particularly limited, and it is preferable to dehydrate the raw material fibers by, for example, compression dehydration, centrifugal dehydration, vibration dehydration, or the like.

[0031] After the above steps, the raw fiber is dried to obtain the regenerated cellulose fiber according to the first embodiment. The drying temperature is preferably from room temperature (about 15 to 25°C) to 300°C, and more preferably from 20 to 260°C.

[0032] Another aspect of the regenerated cellulose fiber according to the first embodiment is the use of the regenerated cellulose fiber containing at least one compound (A) selected from monohydric or higher alcohols and weak acids as a resin reinforcing material, or a method for using the same. The method for using the regenerated cellulose fiber according to the first embodiment as a resin reinforcing material includes mixing the regenerated cellulose fiber according to the first embodiment with at least one resin selected from a thermoplastic resin and a thermosetting resin. Details of the method for using the regenerated cellulose fiber according to the first embodiment will be described in the method for producing a resin composition according to the second embodiment.

[0033] Next, details of the second embodiment will be described. The second embodiment relates to a resin composition containing regenerated cellulose fibers, pellets of the resin composition, a method for producing the pellets, and a molded article.

[0034] [Resin composition containing regenerated cellulose fibers] The second embodiment relates to a resin composition containing regenerated cellulose fibers containing at least one compound (A) selected from monohydric or higher alcohols and weak acids, and a thermoplastic resin. The second embodiment also relates to a resin composition containing regenerated cellulose fibers containing at least one compound (A) selected from monohydric or higher alcohols and weak acids, and a thermosetting resin. Hereinafter, a resin composition containing a thermoplastic resin will be referred to as "resin composition (I)." A resin composition containing a thermosetting resin will be referred to as "resin composition (II)."

[0035] <Resin composition (I)> The resin composition (I) according to the second embodiment comprises a regenerated cellulose fiber containing at least one compound (A) selected from a monohydric or higher alcohol and a weak acid, and a thermoplastic resin. The resin composition (I) is less likely to suffer from poor appearance due to heating when preparing the resin composition (I) or when obtaining a molded article from the resin composition (I).

[0036] <Resin Composition (II)> The resin composition (II) according to the second embodiment comprises regenerated cellulose fibers containing at least one compound (A) selected from a monohydric or higher alcohol and a weak acid, and a thermosetting resin. The resin composition (II) is less likely to suffer from poor appearance due to heating when a molded article is obtained from the resin composition (II). In the present disclosure, the phrase "poor appearance due to heating" refers to a situation in which, when the resin composition (I) or (II) is heated at a certain temperature (200 to 300°C), the resin composition (I) or (II) yellows more than before heating, or the regenerated cellulose fibers contained in the resin composition (I) or (II) become discolored, resulting in uneven coloring throughout the resin composition.

[0037] (Regenerated Cellulose Fibers) The regenerated cellulose fibers contained in the resin compositions (I) and (II) can preferably be those described in the first embodiment, and the preferred embodiments are also the same. Specifically, glycerin is preferred as the monohydric or higher alcohol, and boric acid is preferred as the weak acid. The proportion of compound (A) contained in the regenerated cellulose fibers is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and even more preferably 0.5 to 15 parts by mass, per 100 parts by mass of the regenerated cellulose fibers. By including regenerated cellulose fibers with a proportion of compound (A) within the above range, poor appearance due to heating is less likely to occur. Furthermore, the weight loss rate due to thermal decomposition is also likely to be low. In one embodiment, the proportion of compound (A) per 100 parts by mass of the regenerated cellulose fibers may be in the range of 0.01 to 20 parts by mass, 0.03 to 15 parts by mass, or 0.05 to 10 parts by mass.

[0038] (Thermoplastic resin) Examples of thermoplastic resins include styrene-based resins, acrylic-based resins, aliphatic or aromatic polycarbonate-based resins, aliphatic or aromatic polyester-based resins (polyethylene terephthalate, polylactic acid, etc.), linear polyolefin-based resins, cyclic olefin-based resins, aliphatic or aromatic polyamide-based resins, polyphenylene ether-based resins, polyvinyl alcohol-based resins, polyoxyalkylene-based resins, polyphenylene sulfide-based resins, thermoplastic polyimide-based resins, polyacetal-based resins, polysulfone-based resins, amorphous fluorine-based resins, and epoxy-based resins. These thermoplastic resins may be used alone or in combination of two or more. The thermoplastic resin may be a biodegradable resin. When a biodegradable resin is contained as the thermoplastic resin, the biodegradability of the resin composition (I) is increased, making it more likely to become an environmentally friendly resin composition. Examples of biodegradable resins include cellulose esters, starch polyesters, polylactic acid (PLA), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH), polylactic acid / polycaprolactone copolymers, polyglycolic acid (PGA), polylactic acid / polyether copolymers, butanediol / long-chain dicarboxylic acid copolymers, polybutylene adipate / terephthalate (PBAT), polytetramethylene adipate-co-terephthalate, polyethylene terephthalate succinate (PETS), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polyvinyl alcohol (PVA), etc. These biodegradable resins may be used alone or in combination of two or more.

[0039] More preferred examples of the thermoplastic resin include one or more selected from the group consisting of polyolefins (polyethylene, polypropylene, etc.), polyesters (polyethylene terephthalate, polylactic acid, etc.), polyamides (PA6, PA66, PA4, PA12, aromatic polyamides, etc.), polyacrylonitrile, polymethyl methacrylate, polystyrene, polyvinyl alcohol, polyphenylene ether, polyoxymethylene, and polyphenylene sulfide.

[0040] In one embodiment, when the thermoplastic resin is crystalline, its melting point may be 80 to 300° C., 90 to 300° C., 100 to 300° C., 150 to 280° C., or 150 to 260° C. In the present disclosure, the melting point refers to the peak top temperature of the endothermic peak (the highest peak when two or more peaks are present) that appears when the temperature is increased at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC).

[0041] (Thermosetting Resin) Examples of the thermosetting resin include phenolic resin, urea resin, melamine resin, benzoguanamine resin, alkyd resin, unsaturated polyester resin, vinyl ester resin, diallyl (tere)phthalate resin, epoxy resin, silicone resin, urethane resin, furan resin, ketone resin, xylene resin, thermosetting polyimide resin, etc. These may be used alone or in combination of two or more.

[0042] The proportion of regenerated cellulose fibers in resin composition (I) or (II) can be set arbitrarily depending on the desired physical properties, but in one embodiment, it may be 1 to 50% by mass, or 5 to 40% by mass, relative to the total mass of resin composition (I) or (II).

[0043] The resin compositions (I) and (II) according to the second embodiment may contain known additives as needed. Examples of the additives include stabilizers (antioxidants such as hindered phenol antioxidants, shrinkage inhibitors, antistatic agents, UV absorbers, heat stabilizers, weather stabilizers, etc.), lubricants, release agents, lubricants, impact modifiers, colorants (dyes, pigments, etc.), plasticizers, dispersants, flame retardants, antibacterial agents, preservatives, mildew inhibitors, insect repellents, deodorizers, crystallization accelerators, crystal nucleating agents, and foaming agents. These may be used alone or in combination of two or more.

[0044] <Method for producing resin composition (I)> The resin composition (I) can be produced by mixing regenerated cellulose fibers and a thermoplastic resin by a conventionally known method.

[0045] <Pellets and manufacturing method thereof> The resin composition (I) may be in the form of pellets. The manufacturing method of the pellets preferably includes impregnating regenerated cellulose fibers with a molten thermoplastic resin or melt-kneading regenerated cellulose fibers with a thermoplastic resin.

[0046] When a manufacturing method including impregnating regenerated cellulose fibers with a molten thermoplastic resin (melt impregnation) is employed, it is preferable to melt-impregnate a continuous fiber bundle of regenerated cellulose with the thermoplastic resin and then cut it to the desired length to obtain pellets. In one embodiment, the temperature of the molten thermoplastic resin is preferably 200 to 300°C, more preferably 200 to 280°C. It is also more preferable to react the regenerated cellulose fibers with the compound (A) by impregnating them with the molten thermoplastic resin.

[0047] When a production method including melt-kneading regenerated cellulose fibers and a thermoplastic resin is adopted, it is preferable to feed the regenerated cellulose fibers and the thermoplastic resin into an extruder, melt-knead them at 200 to 300°C, and then cut the strand-like material into pellets by a pelletizing method or the like. The melt-kneading temperature is more preferably 200 to 280°C. It is also more preferable to react the regenerated cellulose fibers with the compound (A) by melt-kneading.

[0048] <Method for producing resin composition (II)> The resin composition (II) can be produced by mixing regenerated cellulose fibers and the above-mentioned thermosetting resin by a conventionally known method.

[0049] <Molded Article> The molded article according to the second embodiment is obtained by molding the resin composition (I) or (II) described above by a known resin molding method such as injection molding. The molded article according to the second embodiment is less likely to suffer from poor appearance due to heating during molding. Therefore, such molded articles can be suitably used in various fields such as automobiles, electrical and electronic products, office automation, home appliances, and miscellaneous goods.

[0050] The molded article according to the second embodiment also has the characteristic of better fiber dispersion than molded articles containing regenerated cellulose fibers other than those of the first embodiment. When a long-fiber-containing resin composition is injection molded, the long fibers tend to entangle within the molded article, and the entangled fibers are compressed and pressed within the molded article. When the molded article is heated and the matrix resin softens, the pressed, entangled fibers expand. That is, the entangled fibers expand like a spring that has been pressed down (under load) being released from the load and stretches up. This expansion causes the molded article itself to expand. Surprisingly, it was found that the resin composition according to the second embodiment has improved fiber dispersion. Even more surprisingly, it was found that molded articles made from this resin composition have better fiber dispersion and reduced entanglement than molded articles made from a resin composition containing regenerated cellulose fibers that does not contain compound (A), and therefore tend to have a very small coefficient of thermal expansion when heated.

[0051] Next, details of the third embodiment will be described. The third embodiment relates to a method for producing regenerated cellulose fibers with reduced coloration.

[0052] [Method for producing regenerated cellulose with reduced discoloration] The third embodiment relates to a method for producing regenerated cellulose fibers, which includes heating the regenerated cellulose fibers of the first embodiment at 200 to 300° C. The regenerated cellulose fibers obtained by the production method of the third embodiment are fibers with reduced discoloration compared to conventional regenerated cellulose fibers.

[0053] In the third embodiment, the method for heating the regenerated cellulose fibers is not particularly limited, and the regenerated cellulose fibers may be heated using a heating device such as an oven, or the regenerated cellulose fibers may be impregnated with molten resin at 200 to 300°C, or the regenerated cellulose fibers may be melt-kneaded with a thermoplastic resin at 200 to 300°C, etc.

[0054] In one embodiment, the heating preferably includes applying a heat load of 200 to 300°C to at least the surface of the regenerated cellulose fibers. Here, "applying a heat load" includes not only heating the regenerated cellulose fibers themselves in an oven or the like, but also heating the fiber surface or the interior of the fibers by contacting the regenerated cellulose fibers with a molten resin. It is presumed that this process causes the reducing terminals or hydroxyl groups of the regenerated cellulose fibers to react with compound (A), thereby suppressing discoloration of the regenerated cellulose fibers.

[0055] The present disclosure will be explained in more detail below by showing examples, but interpretation of the present disclosure is not limited to these examples.

[0056] [Example 1 and Comparative Example 1] 0.4 g of regenerated cellulose fiber (raw fiber) (regenerated cellulose fiber (lyocell) obtained by a solvent method; average fiber diameter: 11 μm, 552 tex, 2700 filaments) was immersed in 10 g of glycerin and then heated and dried at 230°C for 60 minutes. After cooling, the fiber was washed with water and dried under reduced pressure to obtain regenerated cellulose fiber containing glycerin. The ratio of glycerin to 100 parts by mass of regenerated cellulose fiber was 0.7 parts by mass. The obtained regenerated cellulose fiber of Example 1 and the raw fiber (Comparative Example 1) were heated in an oven at 270°C for an additional 10 minutes. The discoloration level of the regenerated cellulose fiber after heating was evaluated according to the following criteria. The discoloration level was compared, with the color of Blank 1 (raw fiber) being assigned Level 1 and the color of Comparative Example 1 (raw fiber heated at 270°C for 10 minutes) being assigned Level 4. The results are shown in Table 1. (Discoloration Level) Level 1: The color is similar to that of Blank 1. Level 2: Slightly more colored than Blank 1. Level 3: Slightly more colored than Level 2. Level 4: The entire fiber is colored to the same extent as Comparative Example 1.

[0057]

[0058] Example 2 and Comparative Example 2: 100 parts by mass (W1: approximately 0.8 g) of regenerated cellulose fibers (raw fiber) (regenerated cellulose fibers (lyocell) obtained by a solvent method; average fiber diameter: 11 μm, 552 tex, 2700 filaments) whose weight (W1) had been measured in advance were immersed for 5 seconds in an aqueous medium containing boric acid (5.0% by mass boric acid aqueous solution, aqueous medium temperature: 60°C) to absorb at least 200 parts by mass of the aqueous medium. The fibers were then sandwiched between paper towels and compressed for dehydration to remove the aqueous medium. The weight (W2) was then measured, and the aqueous medium ratio was calculated using the following formula (1). The aqueous medium ratio was found to be 74% by mass. Aqueous medium ratio = (W2 - W1) / W1 × 100 (1). The regenerated cellulose fibers containing the aqueous medium were then dried at 23°C for 240 hours to obtain regenerated cellulose fibers containing boric acid. The amount of boric acid per 100 parts by mass of the regenerated cellulose fibers was 3.7 parts by mass. The regenerated cellulose fiber of Example 2 and the raw fiber (Comparative Example 2) were heated in an oven at 240°C for 15 minutes. The color level of the regenerated cellulose fiber after heating was evaluated according to the same criteria as in Example 1. The color level was compared by assigning the color of Blank 1 (raw fiber) as level 1 and the color of Comparative Example 2 (raw fiber heated at 240°C for 15 minutes) as level 4. The results are shown in Table 2.

[0059]

[0060] 1 shows photographs of the regenerated cellulose fibers of Example 2 and Comparative Example 2 after heating. As shown in FIG. 1 and Tables 1 and 2, the regenerated cellulose fibers containing compound (A) according to the first embodiment (Examples 1 and 2) showed less discoloration due to heating than the raw fiber of Comparative Examples 1 and 2.

[0061] [Example 3 and Comparative Example 3] Regenerated cellulose fibers containing boric acid obtained by the same process as in Example 2 were cut to lengths of 1 to 2 cm. Next, 10% by mass of the regenerated cellulose fibers were blended with 90% by mass of polypropylene resin (homopolypropylene resin, manufactured by SunAllomer Co., Ltd., product name "PMB02A") and melt-kneaded using a small kneader (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name "Laboplastomill (registered trademark)") at a kneading temperature of 200°C, a rotation speed of 100 rpm, and a kneading time of 3 minutes to prepare pellets of the resin composition of Example 3. Furthermore, pellets of the resin composition of Comparative Example 3 were prepared under the same conditions as Example 3, except that raw fiber was used as the regenerated cellulose fiber. Next, small pieces of approximately 0.07 g were cut from the pellets of Example 3 and Comparative Example 3 and heated in an oven at 240°C for 15 minutes. The coloration level of the heated pellets was evaluated according to the following evaluation criteria. The discoloration levels were compared by assigning the color of Blank 1 (pellets before heating) to Level 1 and the color of a small piece of the pellets of Comparative Example 3 when heated at 240°C for 15 minutes to Level 4. The results are shown in Table 3. (Discoloration Level) Level 1: The color is about the same as Blank 1. Level 2: Slightly more discolored than Blank 1. Level 3: Slightly more discolored than Level 2. Level 4: The entire piece is discolored to the same extent as Comparative Example 3.

[0062]

[0063] Figure 2 shows photographs of small pieces of pellets from Example 3 and Comparative Example 3 before heating. As shown in Figure 2, there was no significant difference in appearance between the pellets (before heating) obtained in Example 3 and Comparative Example 3, and both were a light ivory color. Figure 3 also shows photographs of the pellets from Example 3 and Comparative Example 3 after heating. As shown in Figure 3 and Table 3, it was found that the pellets of the resin composition (I) according to the second embodiment had fewer appearance defects due to heating than the pellets of the resin composition of Comparative Example 3.

[0064] [Example 4 and Comparative Example 4] Continuous regenerated cellulose fibers (raw continuous fibers) were immersed in an aqueous medium containing boric acid (boric acid concentration 3.8% by mass, aqueous medium temperature 25°C) to allow the aqueous medium to be absorbed into the continuous regenerated cellulose fibers. The aqueous medium was then dehydrated (the aqueous medium ratio calculated from the above formula (1) after dehydration was 36%), and non-contact drying (drying temperature: 180°C) and contact drying (drying temperature: 180°C) were performed to obtain the continuous regenerated cellulose fibers of Example 4 (continuous regenerated cellulose fibers containing boric acid). The amount of boric acid per 100 parts by mass of the continuous regenerated cellulose fibers of Example 4 was 1.4 parts by mass. The above series of steps were carried out using an apparatus (Minisizer, manufactured by Kaji Seisakusho Co., Ltd., product name "DCC001P") equipped with a storage section for storing raw continuous fibers, an immersion section equipped with a container for storing an aqueous medium, a drying section equipped with a non-contact drying device and a contact drying device, and a recovery section for recovering the treated continuous fibers, while winding the continuous fibers toward the recovery section (winding speed: 20 m / min).

[0065] Next, 67.9% by mass of polypropylene resin (homopolypropylene resin, manufactured by SunAllomer Co., Ltd., product name "PMB02A") and 2.1% by mass of maleic anhydride-modified polypropylene resin (manufactured by SK Functional Polymer, product name "OREVAC CA100") were mixed and charged into a twin-screw extruder (manufactured by The Japan Steel Works, Ltd., product name "TEX30α"), and the mixture was melt-kneaded at a cylinder temperature of 280 ° C. The molten mixture was then impregnated into the regenerated cellulose continuous fiber containing boric acid, which had been passed through a crosshead die, so that the continuous fiber was 30% by mass. The mixture was then shaped using a shaping nozzle at the exit of the crosshead die, shaped using a shaping roll, and cut to a length of 7 mm using a pelletizer to obtain pellets of a resin composition containing regenerated cellulose fiber containing boric acid and polypropylene. Furthermore, as Comparative Example 4, pellets of a resin composition containing raw continuous fiber were obtained under the same conditions as above.

[0066] Next, the resin compositions (pellets) of Example 4 and Comparative Example 4 were injection molded under the following conditions to obtain molded articles (ISO multipurpose test pieces). For the obtained molded articles, various mechanical properties were measured under the following conditions. The thermal expansion coefficient was also measured under the following conditions. The results are shown in Table 4. (Molding conditions) Molding machine: FUNAC Corporation, product name "α-S150iA". Test piece: ISO multipurpose test piece. Molding temperature: 200°C. Mold temperature: 60°C.

[0067] <Measurement of Tensile Strength> Using the obtained ISO multipurpose test specimen, the tensile strength was measured in accordance with ISO 527-1 and 2. Specifically, using a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph (registered trademark) AG-20kNXDplus"), the measurement was performed under the conditions of a temperature of 23°C, a test speed of 5 mm / min, and a chuck distance (span) of 115 mm.

[0068] <Measurement of Charpy impact strength> Using the obtained ISO multipurpose test specimen, measurement was performed in accordance with ISO 179 / 1eA. Specifically, measurement was performed using a digital impact tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd., product name "Impact Tester No. 258-L IMPACT TESTER") under the following conditions: test temperature: 23°C, measurement mode: V-notched, hammer capacity: 4J.

[0069] <Measurement of flexural strength and flexural modulus> Using the obtained ISO multipurpose test piece, measurements were made in accordance with ISO 178. Specifically, measurements were made using a tensile tester (manufactured by Toyo Seiki Seisaku-sho, product name "Bendograph II") under the conditions of a temperature of 23°C, a test speed of 2 mm / min, and a chuck distance (span) of 64 mm.

[0070] <Measurement of Thermal Expansion Coefficient> A molded article was cut out from the obtained ISO multipurpose test piece at a position 5 cm from the gate side, and the thermal expansion coefficients (240°C x 5 minutes, 260°C x 3 minutes, 260°C x 5 minutes, 280°C x 2 minutes) of the molded article were measured.

[0071]

[0072] As shown in Table 4, the molded article of the resin composition containing the continuous fibers of regenerated cellulose according to the first embodiment (the molded article according to the second embodiment) had a very low coefficient of thermal expansion while maintaining mechanical properties comparable to those of the molded article made from the raw continuous fibers. Therefore, the resin composition according to the second embodiment can suppress the springback phenomenon during profile extrusion (the phenomenon in which the resin expands in the thickness and width directions the moment it leaves the extrusion die), and is expected to be applied to profile extrusion molded articles.

[0073] When the regenerated cellulose fiber according to the first embodiment is blended into a resin as a resin reinforcing material, discoloration due to heating during preparation of the resin composition or molding of the resin composition is unlikely to occur. The regenerated cellulose fiber has industrial applicability as a reinforcing material that can produce molded products with little discoloration. The resin composition according to the second embodiment is unlikely to suffer from poor appearance due to heating during molding. Therefore, molded products of the resin composition according to the second embodiment can be suitably used in various fields such as automobiles, electrical and electronics, office automation, home appliances, and miscellaneous goods.

Claims

1. Regenerated cellulose fibers for resin reinforcement, comprising at least one compound (A) selected from monohydric or higher alcohols and weak acids.

2. Regenerated cellulose fibers according to claim 1, wherein the ratio of said compound (A) to 100 parts by mass of said regenerated cellulose fibers is 0.01 to 20 parts by mass.

3. The regenerated cellulose fibers of claim 1 or 2, wherein the alcohol comprises glycerin and the weak acid comprises boric acid.

4. A resin composition comprising regenerated cellulose fibers containing at least one compound (A) selected from monohydric or higher alcohols and weak acids, and a thermoplastic resin.

5. A resin composition comprising regenerated cellulose fibers containing at least one compound (A) selected from monohydric or higher alcohols and weak acids, and a thermosetting resin.

6. A resin composition according to claim 4 or 5, wherein the ratio of the compound (A) to 100 parts by mass of the regenerated cellulose fibers is 0.01 to 20 parts by mass.

7. The resin composition according to claim 4 or 5, wherein the alcohol comprises glycerin and the weak acid comprises boric acid.

8. Pellets of the resin composition according to claim 4.

9. A molded article made from the resin composition according to claim 4 or 5.

10. A method for producing regenerated cellulose fibers with suppressed discoloration, comprising heating the regenerated cellulose fibers according to claim 1 or 2 at 200 to 300°C.

11. The method for producing regenerated cellulose fibers according to claim 10, wherein the heating step includes applying a heat load of 200 to 300° C. to at least the surface of the regenerated cellulose fibers.

12. A method for producing pellets as described in claim 8, comprising: impregnating the regenerated cellulose fibers with the molten thermoplastic resin; or melt-kneading the regenerated cellulose fibers with the thermoplastic resin.

13. The method for producing pellets according to claim 12, wherein the temperature of the molten thermoplastic resin or the temperature of the melt-kneading is 200 to 300°C.

14. The method for producing pellets according to claim 12, wherein the impregnation with the molten thermoplastic resin or the melt-kneading includes reacting the regenerated cellulose fibers with the compound (A).

Citation Information

Patent Citations

  • Sheet containing cellulose fiber layer

    JP2017095831A

  • Preparation method of functional fabric

    CN112626673A

  • Treatment goods for ophthalmology

    JP1990168958A

  • Dust collection bag and filter for electric vacuum cleaner

    JP2001120477A

  • Cellulose resin composition

    JP2021066789A

Cited By

  • Resin composition and method for producing same

    WO2026116329A1