Semiconductor device

The semiconductor device design with a high-Curie-point buffer plate and porosity-controlled buffer bonding material addresses thermal stress and deformation issues, enhancing lifespan at high temperatures by reducing thermal deformation and stress in the main electrode.

WO2024247875A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018981
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Semiconductor devices face internal breakdown and reduced lifespan at high operating temperatures due to thermal deformation and stress, leading to increased electrical and thermal series resistance, particularly during power cycle tests.

Method used

A semiconductor device design featuring a buffer plate made of laminated or alloy material with a Curie point of 300°C or higher, combined with a sintered body buffer bonding material having a porosity of 5% to 40%, which reduces thermal stress and deformation of the main electrode, thereby enhancing lifespan at high temperatures.

Benefits of technology

The solution effectively suppresses thermal deformation and stress in the main electrode, leading to improved lifespan and reduced risk of internal breakdown, even at high operating temperatures, as demonstrated by extended power cycle test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018981_05122024_PF_FP_ABST
    Figure JP2024018981_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This semiconductor device comprises: a semiconductor chip which comprises a semiconductor substrate and a main electrode that is provided on the semiconductor substrate; a buffer plate; and a buffer bonding material which is provided between the main electrode and the buffer plate. The buffer plate is a multilayer material or an alloy material having a Curie point of 300°C or higher. The multilayer material has a first copper layer that is in contact with the buffer bonding material, an alloy layer that is provided on the first copper layer and has a Curie point of 300°C or higher, and a second copper layer that is provided on the alloy layer.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor Devices

[0001] The present disclosure relates to semiconductor devices.

[0002] This application claims priority based on Japanese Application No. 2023-089063 filed on May 30, 2023, and incorporates by reference all of the contents of the aforementioned Japanese application.

[0003] As an example of a semiconductor device suitable for a power module, a semiconductor device has been proposed in which a buffer plate is bonded to a main electrode of a semiconductor chip and bonding wires are bonded to the buffer plate.

[0004] Japanese Patent Publication No. 2018-186220 Japanese Patent Publication No. 2017-005037 Japanese Patent Publication No. 2019-057663

[0005] The semiconductor device disclosed herein comprises a semiconductor chip having a semiconductor substrate and a main electrode provided on the semiconductor substrate, a buffer plate, and a buffer bonding material provided between the main electrode and the buffer plate, wherein the buffer plate is a laminate material or an alloy material having a Curie point of 300°C or higher, and the laminate material has a first copper layer in contact with the buffer bonding material, an alloy layer having a Curie point of 300°C or higher provided on the first copper layer, and a second copper layer provided on the alloy layer.

[0006] Fig. 1 is a top view showing a semiconductor device according to a first embodiment. Fig. 2 is a cross-sectional view showing the semiconductor device according to the first embodiment. Fig. 3 is a top view showing a semiconductor device according to a second embodiment. Fig. 4 is a cross-sectional view showing the semiconductor device according to the second embodiment. Fig. 5 is a diagram showing an example of the results of a power cycle test.

[0007] [Problem to be Solved by the Present Disclosure] In recent years, there has been an increasing demand for semiconductor devices that can be used at higher temperatures, and therefore, a long service life at higher temperatures is desired.

[0008] An object of the present disclosure is to provide a semiconductor device that has a good life even at high operating temperatures.

[0009] [Advantages of the Present Disclosure] According to the present disclosure, a good lifespan can be obtained even at high operating temperatures.

[0010] The embodiments for carrying out the invention are described below.

[0011] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. In the following description, the same or corresponding elements will be denoted by the same reference numerals, and the same description will not be repeated.

[0012] [1] A semiconductor device according to one aspect of the present disclosure includes a semiconductor chip including a semiconductor substrate and a main electrode provided on the semiconductor substrate, a buffer plate, and a buffer bonding material provided between the main electrode and the buffer plate, wherein the buffer plate is a laminate material or an alloy material having a Curie point of 300°C or higher, and the laminate material includes a first copper layer in contact with the buffer bonding material, an alloy layer provided on the first copper layer and having a Curie point of 300°C or higher, and a second copper layer provided on the alloy layer.

[0013] In ferromagnetic materials, thermal expansion is small at temperatures below the Curie point because volume changes due to magnetostriction and thermal expansion due to normal lattice vibration cancel each other out. Because the buffer plate is made of an alloy material with a Curie point of 300°C or higher or a laminated material having an alloy layer with a Curie point of 300°C or higher, thermal expansion of the buffer plate is small at temperatures below 300°C. This also suppresses thermal deformation of the main electrode bonded to the buffer plate by the buffer bonding material. Therefore, even when used at high temperatures, internal breakdown of the main electrode is suppressed, ensuring a long service life.

[0014] Internal breakdown of the main electrode occurs when grain boundary sliding and cracks occurring at the grain boundaries of the crystals that make up the main electrode accumulate due to repeated thermal deformation. Internal breakdown of the main electrode is confirmed, for example, as a decrease in the density of the main electrode or an increase in the thickness of the main electrode. Furthermore, when internal breakdown occurs in the main electrode, the effective bonding area between the main electrode and the components sandwiching it decreases. Therefore, internal breakdown can also be confirmed as an increase in electrical or thermal series resistance.

[0015] Internal breakdown of the main electrode can also occur during a power cycle test. In other words, during a power cycle test, repeated temperature increases and decreases can cause grain boundary sliding and cracks to occur, resulting in internal breakdown. For example, in the later stages of a power cycle test, internal breakdown of the main electrode can be observed as breakage or peeling of the main electrode, a sudden increase in electrical resistance or disconnection, or a sudden increase in thermal resistance or thermal runaway. These phenomena become particularly noticeable just before the end of life.

[0016] [2] In [1], the buffer bonding material may have a sintered body with a porosity of 5% to 40%. By having the buffer bonding material have a sintered body with a porosity of 5% to 40%, thermal stress acting on the buffer bonding material is reduced, and thermal deformation of the main electrode is suppressed. Therefore, a good life is easily obtained.

[0017] [3] In [1] or [2], the alloy material and the alloy layer may contain iron and nickel, and the proportion of nickel in the alloy material and the alloy layer may be 40 mass % or more. In this case, the alloy material and the alloy layer are likely to have a Curie point of 300° C. or more.

[0018] [4] In [1] or [2], the alloy material and the alloy layer may contain iron, nickel, and cobalt, and the total proportion of nickel and cobalt in the alloy material and the alloy layer may be 40 mass % or more. In this case, the alloy material and the alloy layer are likely to have a Curie point of 300° C. or more.

[0019] [5] A semiconductor device according to another aspect of the present disclosure includes a semiconductor chip including a semiconductor substrate and a main electrode provided on the semiconductor substrate, a buffer plate, and a buffer bonding material provided between the main electrode and the buffer plate, wherein the buffer bonding material has a sintered body with a porosity of 5% or more and 40% or less.

[0020] The buffer bonding material has a sintered body with a porosity of 5% to 40%, which reduces the thermal stress acting on the buffer bonding material and suppresses thermal deformation of the main electrode. Therefore, even when used at high temperatures, internal destruction of the main electrode is suppressed and a long life is achieved.

[0021] [6] In any one of [1] to [5], the main electrode may include an aluminum layer or an aluminum alloy layer, which makes it easier to obtain good electrical conductivity in the main electrode.

[0022] [7] In [6], the first linear expansion coefficient of the semiconductor substrate and the second linear expansion coefficient of the buffer plate may be smaller than the third linear expansion coefficient of the main electrode, and the second linear expansion coefficient may be smaller than the first linear expansion coefficient. In this case, because the third linear expansion coefficient is larger than the first linear expansion coefficient, the main electrode tends to thermally deform more than the semiconductor substrate. However, because the second linear expansion coefficient is smaller than the first linear expansion coefficient, the thermal deformation of the main electrode can be effectively suppressed by the buffer bonding material. Therefore, thermal stress generated in the main electrode due to thermal deformation can be suppressed, and internal destruction of the aluminum layer or aluminum alloy layer included in the main electrode can be suppressed.

[0023] Generally, aluminum or aluminum alloy layers are weaker than other metal components of semiconductor devices in terms of strength and heat resistance. The grain boundary sliding that causes internal destruction of the main electrode is called creep, and the creep onset temperature can be determined by using a temperature 0.4 times the melting point (Tm). This index indicates that creep begins at a lower temperature in aluminum or aluminum alloy layers than in other components. For example, the values ​​of "Tm x 0.4" for aluminum, copper, and nickel are 100°C, 270°C, and 418°C, respectively.

[0024] In particular, when the aluminum or aluminum alloy layer included in the main electrode is formed by sputtering, the grain size of the crystals constituting the aluminum or aluminum alloy layer is small, on the order of a few micrometers, and therefore, when thermal strain occurs between the layers sandwiching the main electrode due to temperature rise and fall cycles during a power cycle test, grain boundary sliding is likely to occur.

[0025] In contrast, when the second linear expansion coefficient is smaller than the first linear expansion coefficient, the buffer bonding material can effectively suppress thermal deformation of the main electrode, thereby suppressing internal destruction of the aluminum layer or aluminum alloy layer contained in the main electrode.

[0026] [Details of Embodiments of the Present Disclosure] Embodiments of the present disclosure will be described in detail below, but the present embodiments are not limited thereto. Note that, in this specification and drawings, components having substantially the same functional configurations may be denoted by the same reference numerals to avoid redundant description. In this specification and drawings, the X1-X2 direction, the Y1-Y2 direction, and the Z1-Z2 direction are defined as mutually orthogonal directions. The plane including the X1-X2 direction and the Y1-Y2 direction is defined as the XY plane, the plane including the Y1-Y2 direction and the Z1-Z2 direction is defined as the YZ plane, and the plane including the Z1-Z2 direction and the X1-X2 direction is defined as the ZX plane. For convenience, the Z1 direction is defined as the upward direction, and the Z2 direction is defined as the downward direction. Furthermore, in this disclosure, planar view refers to viewing an object from the Z1 side.

[0027] (First Embodiment) A first embodiment will be described. The first embodiment relates to a semiconductor device. FIG. 1 is a top view showing the semiconductor device according to the first embodiment. FIG. 2 is a cross-sectional view showing the semiconductor device according to the first embodiment. FIG. 2 corresponds to a cross-sectional view taken along line II-II in FIG. 1.

[0028] As shown in Figures 1 and 2, the semiconductor device 1 according to the first embodiment mainly includes a heat sink 120, a substrate 110, a terminal 102, a terminal 103, a case 190, a diode 300, and a buffer plate 500.

[0029] The heat sink 120 is, for example, a rectangular plate-like body with a uniform thickness in a plan view. The material of the heat sink 120 is a metal with high thermal conductivity, such as copper (Cu), a copper alloy, aluminum (Al), or an aluminum-silicon-carbon alloy (Al-Si-C alloy). The heat sink 120 is fixed to a cooler or the like using a thermal interface material (TIM) or the like.

[0030] The case 190 is formed, for example, in a frame shape in a plan view, and the outer shape of the case 190 is the same as the outer shape of the heat sink 120. The case 190 is made of an insulating material such as resin. The case 190 has a pair of side walls 191 and 192 facing each other and a pair of end walls 193 and 194 connecting both ends of the side walls 191 and 192. The side walls 191 and 192 are arranged parallel to the ZX plane, and the end walls 193 and 194 are arranged parallel to the YZ plane. The side wall 191 is arranged on the Y1 side of the side wall 192, and the end wall 193 is arranged on the X2 side of the end wall 194.

[0031] Terminal 102 is disposed on the upper surface (surface on the Z1 side) of end wall portion 193, and terminal 103 is disposed on the upper surface (surface on the Z1 side) of end wall portion 194. Terminal 102 and terminal 103 are each made of a metal plate.

[0032] Inside the case 190, the substrate 110 is disposed on the Z1 side of the heat sink 120. The substrate 110 has an insulating substrate 119, a second conductive pattern 112, a third conductive pattern 113, and a conductive layer 115. The first conductive pattern 111, the second conductive pattern 112, the third conductive pattern 113, the fourth conductive pattern 114, and the conductive layer 115 are made of Cu.

[0033] The second conductive pattern 112 and the third conductive pattern 113 are provided on the Z1 side surface of the insulating substrate 119. The conductive layer 115 is provided on the Z2 side surface of the insulating substrate 119. The conductive layer 115 is bonded to the heat sink 120 by a bonding material 131. The bonding material 131 may be a solder material or a sintered bonding material. When the bonding material 131 is a sintered bonding material, operation at a higher temperature, near the melting point of the solder or higher, is possible.

[0034] As shown in FIG. 2 , the diode 300 mainly includes a silicon carbide substrate 310 , an anode electrode 332 , and a cathode electrode 333 .

[0035] The silicon carbide substrate 310 has a main surface 310A and a main surface 310B opposite to the main surface 310A. The main surface 310A is on the Z1 side of the main surface 310B. The silicon carbide substrate 310 has, for example, a rectangular parallelepiped shape. The main surfaces 310A and 310B are parallel to the XY plane. The anode electrode 332 is provided on the main surface 310A, and the cathode electrode 333 is provided on the main surface 310B. The diode 300 is provided on the third conductive pattern 113. The anode electrode 332 includes, for example, an aluminum layer. The anode electrode 332 may include an aluminum alloy layer such as an aluminum-silicon alloy (Al—Si alloy) or an Al—Si—Cu alloy instead of the aluminum layer. The cathode electrode 333 has an ohmic layer and a bonding layer provided on the ohmic layer. The ohmic layer includes, for example, nickel or a nickel alloy. Nickel or a nickel alloy has good contact resistance with silicon carbide. The bonding layer includes a nickel layer. The bonding layer may further include a gold layer or a silver layer provided on the nickel layer. When the cathode electrode 333 includes a bonding layer, good bonding is obtained between the cathode electrode 333 and the third conductive pattern 113. The cathode electrode 333 is bonded to the third conductive pattern 113 using a bonding material 133 such as a silver sintered body or a copper sintered body. The diode 300 is an example of a semiconductor chip. The silicon carbide substrate 310 is an example of a semiconductor substrate. The anode electrode 332 is an example of a main electrode.

[0036] The buffer plate 500 is, for example, a laminated material having a first copper layer 510, an alloy layer 520, and a second copper layer 530. The alloy layer 520 is provided on the Z1 side of the first copper layer 510, and the second copper layer 530 is provided on the Z1 side of the alloy layer 520. That is, the alloy layer 520 is provided on the first copper layer 510, and the second copper layer 530 is provided on the alloy layer 520. The alloy layer 520 is an alloy material having a Curie point of 300°C or higher. The alloy layer 520 may, for example, contain iron (Fe) and nickel (Ni), with the proportion of Ni in the alloy layer 520 being 40% by mass or higher. The alloy layer 520 may, for example, contain Fe, Ni, and cobalt (Co), with the total proportion of Ni and Co in the alloy layer 520 being 40% by mass or higher. The alloy layer 520 may also contain 29% by mass of Ni and 17% by mass of Co. In either case, the alloy layer 520 may contain Fe at a rate of 45% by mass or more, or 48% by mass or more. The alloy layer 520 may also contain approximately 0.7% by mass of manganese. The material of the alloy layer 520 may be Kovar (registered trademark). The thickness T2 of the buffer plate 500 is, for example, 0.05 mm or more and 0.5 mm or less. The thickness T2 of the buffer plate 500 may be 0.05 mm or more and 0.25 mm or less. For example, the thickness T2 of the buffer plate 500 is smaller than the thickness T1 of the diode 300. The buffer plate 500 is disposed on the anode electrode 332. The first copper layer 510 is bonded to the anode electrode 332 using a buffer bonding material 135 such as a silver sintered body or a copper sintered body. The buffer bonding material 135 has a sintered body with a porosity of 5% to 40%.

[0037] The silicon carbide substrate 310 has a first linear expansion coefficient ρ1, the buffer plate 500 has a second linear expansion coefficient ρ2, and the anode electrode 332 has a third linear expansion coefficient ρ3. Unless otherwise specified, the linear expansion coefficient in this disclosure refers to the linear expansion coefficient in a direction parallel to the main surface 310A at 25°C. Furthermore, unless otherwise specified, the linear expansion coefficient in this disclosure refers to the linear expansion coefficient when the silicon carbide substrate 310, the buffer plate 500, and the anode electrode 332 are unbonded and the silicon carbide substrate 310, the buffer plate 500, and the anode electrode 332 are separated into a single body. The first linear expansion coefficient ρ1 and the second linear expansion coefficient ρ2 are smaller than the third linear expansion coefficient ρ3. The second linear expansion coefficient ρ2 may be larger or smaller than the first linear expansion coefficient ρ1, but when the difference between the first linear expansion coefficient ρ1 and the second linear expansion coefficient ρ2 is small, thermal stress acting on the anode electrode 332 is easily suppressed. When the second linear expansion coefficient ρ2 is smaller than the first linear expansion coefficient ρ1, the life is more likely to be extended than when the second linear expansion coefficient ρ2 is larger than the first linear expansion coefficient ρ1. For example, when the first linear expansion coefficient ρ1 is 4.0×10 -6 / °C, whereas the second linear expansion coefficient ρ2 is 1.2 × 10 -6 / ℃ or more 3.9 x 10 -6 / °C or less. In this case, the value of "ρ2 - ρ1" is -2.8 × 10 -6 / ℃ or more -0.1 x 10 -6 / °C or less, and a longer life is likely to be obtained than when the value of "ρ2 - ρ1" is positive. The linear expansion coefficient of iron-nickel alloy is 1.2 × 10 -6 / °C, and the linear expansion coefficient of copper is 16.5 × 10 -6 / °C, and the linear expansion coefficient of aluminum is 23.1 × 10 -6 / °C. When the anode electrode 332 is made of aluminum, the third linear expansion coefficient ρ3 is about 23.1×10 -6 / ℃.

[0038] The semiconductor device 1 further includes wires 162, 165, and 166. The number of each of the wires 162, 165, and 166 is not limited, and may be one, or two or more.

[0039] Wire 162 connects second copper layer 530 of buffer plate 500 to second conductive pattern 112. Wire 165 connects second conductive pattern 112 to terminal 102. Wire 166 connects third conductive pattern 113 to terminal 103. Wires 162, 165, and 166 are, for example, copper wires. Each of wires 162, 165, and 166 has a diameter of, for example, 100 μm or more and 400 μm or less. Wires 162, 165, and 166 are bonded by, for example, ultrasonic bonding.

[0040] Generally, the lifetime of a semiconductor device used in a power module at its operating temperature is evaluated by a power cycle test. In the power cycle test, a semiconductor device sample is repeatedly energized and deenergized. The maximum junction temperature (Tjmax) is set as the operating temperature at which the lifetime is to be evaluated. Based on the difference (ΔT) between the maximum junction temperature (Tjmax) and the minimum junction temperature (Tjmin), the sample is determined to have reached the end of its lifetime when the junction temperature (Tj) reaches Tjmax + ΔT × 20%.

[0041] For example, if the maximum bonding temperature (Tjmax) is 250°C and the minimum bonding temperature (Tjmin) is 65°C, the difference (ΔT) is 185°C, so it is determined that the sample has reached the end of its life when the bonding temperature (Tj) reaches 287°C. Also, if the maximum bonding temperature (Tjmax) is 250°C and the minimum bonding temperature (Tjmin) is 25°C, the difference (ΔT) is 225°C, so it is determined that the sample has reached the end of its life when the bonding temperature (Tj) reaches 295°C.

[0042] Furthermore, in ferromagnetic materials such as Invar (registered trademark) and Kovar, thermal expansion is small at temperatures below the Curie point because volume changes due to magnetostriction and thermal expansion due to normal lattice vibration cancel each other out. As described above, in this embodiment, the alloy layer 520 is an alloy material with a Curie point of 300°C or higher. In other words, thermal expansion of the alloy layer 520 is small at temperatures below 300°C. Therefore, in this embodiment, thermal deformation of the alloy layer 520 and the buffer plate 500 is suppressed in a power cycle test with a maximum junction temperature (Tjmax) of 250°C.

[0043] Furthermore, because thermal deformation of the buffer plate 500 is suppressed, thermal deformation of the anode electrode 332 joined to the buffer plate 400 by the buffer bonding material 135 is also suppressed. Therefore, according to this embodiment, even when used at high temperatures, thermal stress generated in the anode electrode 332 due to thermal deformation can be suppressed, and internal destruction of the anode electrode 332 can be suppressed.

[0044] In this embodiment, the buffer bonding material 135 has a sintered body with a porosity of 5% or more and 40% or less. The higher the porosity, the lower the thermal stress acting on the buffer bonding material 135 during heating, which results in suppressing thermal stress in the anode electrode 332. According to stress analysis using the finite element method, when the temperature of the buffer bonding material 135 made of a copper sintered body is 200°C, the thermal stress in the anode electrode 332 is 54 MPa when the porosity is 0%, 36 MPa when the porosity is 5%, and 10 MPa when the porosity is 30%. In other words, when the porosity is 5%, the thermal stress is 34% lower than when the porosity is 0%, and the thermal stress is 72% lower when the porosity is 30% than when the porosity is 5%. Furthermore, stress analysis using the finite element method has confirmed that even when the temperature of the buffer bonding material 135 made of sintered copper is 250°C, the thermal stress generated in the anode electrode 332 is reduced when the porosity is 5% or more and 40% or less.

[0045] The effect of reducing thermal stress due to the increase in the porosity of the sintered body becomes more pronounced when the sintered body is used at high temperatures. This is because, in the case of bulk Cu, the Young's modulus obtained from the stress-strain curve does not usually have temperature dependence. On the other hand, the stress-strain curve of a Cu sintered body does have temperature dependence, and the Young's modulus from the stress-strain curve becomes smaller in the high temperature range. The fact that this phenomenon acts in a direction advantageous for suppressing thermal deformation of the anode electrode 332 has also been confirmed by stress analysis using the above-mentioned finite element method. Furthermore, a similar temperature dependence has been confirmed not only for Cu sintered bodies but also for Ag sintered bodies.

[0046] If the porosity is less than 5%, it is difficult to reduce the thermal stress generated in the anode electrode 332. If the porosity is more than 40%, the buffer bonding material 135 is likely to become brittle. The porosity of the sintered body included in the buffer bonding material 135 may be 5% or more and 30% or less, or may be 5% or more and 20% or less.

[0047] In this manner, in this embodiment, the thermal stress acting on the buffer bonding material 135 is reduced, thereby suppressing thermal deformation of the anode electrode 332. Therefore, according to this embodiment, even when used at high temperatures, the thermal stress generated in the anode electrode 332 due to thermal deformation can be suppressed, and internal destruction of the anode electrode 332 can be suppressed.

[0048] According to this embodiment, the effect of the alloy layer 520 being an alloy material having a Curie point of 300°C or higher and the effect of the buffer bonding material 135 being a sintered body having a porosity of 5% or more and 40% or less can be obtained, but the effect of combining these can also be obtained as described below.

[0049] Two main factors are considered to be the causes of thermal stress occurring in the anode electrode 332. The first factor is thermal strain due to the difference between the second linear expansion coefficient ρ2 of the buffer plate 500 and the first linear expansion coefficient ρ1 of the silicon carbide substrate 310. The second factor is the temperature dependence of the Young's modulus of the buffer bonding material 135. Regarding the first factor, by reducing the difference between the second linear expansion coefficient ρ2 and the first linear expansion coefficient ρ1, thermal strain can be suppressed over a wide temperature range from the minimum bonding temperature to the maximum bonding temperature, which are the operating temperatures. Regarding the second factor, the Young's modulus of the buffer bonding material 135 decreases with increasing temperature, so the effect of suppressing thermal strain can be maintained over a wide temperature range. In contrast, if a bonding material made of a copper bulk material is used instead of the buffer bonding material 135, the effect of suppressing thermal strain may be reduced because the copper bulk material does not have a temperature-dependent Young's modulus.

[0050] Because the anode electrode 332 includes an aluminum layer or an aluminum alloy layer, good electrical conductivity is easily achieved in the anode electrode 332. Meanwhile, the first linear expansion coefficient ρ1 of the silicon carbide substrate 310 and the second linear expansion coefficient ρ2 of the buffer plate 500 are smaller than the third linear expansion coefficient ρ3 of the anode electrode 332, and the second linear expansion coefficient ρ2 is smaller than the first linear expansion coefficient ρ1. In this case, the anode electrode 332 tends to thermally deform to a greater extent than the silicon carbide substrate 310. However, because the second linear expansion coefficient ρ2 is smaller than the first linear expansion coefficient ρ1, the thermal deformation of the anode electrode 332 can be effectively suppressed by the buffer bonding material 135. Therefore, thermal stress generated in the anode electrode 332 due to thermal deformation can be suppressed, and internal destruction of the anode electrode 332 can be suppressed.

[0051] In this embodiment, by bonding the wire 162 to the buffer plate 500, the wire 162 can be electrically connected to the anode electrode 332 via the buffer plate 500. Therefore, even if ultrasonic bonding is used to bond the wire 162, damage to the diode 300 can be suppressed. If the wire 162 is a copper wire, it is easy to bond the wire 162 to the second copper layer 530 of the buffer plate 500, and it is also easy to obtain low electrical resistance for the wire 162.

[0052] The buffer plate 500 does not have to include the first copper layer 510 and the second copper layer 530. In other words, the buffer plate 500 may be made of an alloy layer 520 such as Kovar, whose Curie point is 300° C. or higher.

[0053] When alloy layer 520 contains Fe and Ni and the proportion of Ni in alloy layer 520 is 40 mass % or more, it is easy to obtain a Curie point of 300° C. or higher in alloy layer 520. When alloy layer 520 contains Fe, Ni, and Co and the total proportion of Ni and Co in alloy layer 520 is 40 mass % or more, it is also easy to obtain a Curie point of 300° C. or higher in alloy layer 520.

[0054] If the Curie point of the alloy layer 520 is 300° C. or higher, the porosity of the sintered body included in the buffer bonding material 135 does not have to be 5% or higher and 40% or lower. Also, if the porosity of the sintered body included in the buffer bonding material 135 is 5% or higher and 40% or lower, the Curie point of the alloy layer 520 does not have to be 300° C. or higher.

[0055] A plurality of diodes 300 may be provided on the third conductive pattern 113. In this case, the plurality of diodes 300 are electrically connected in parallel to one another.

[0056] Second Embodiment Next, a second embodiment will be described. The second embodiment differs from the first embodiment mainly in that a transistor is included. FIG. 3 is a top view showing a semiconductor device according to the second embodiment. FIG. 4 is a cross-sectional view showing the semiconductor device according to the second embodiment. FIG. 4 corresponds to a cross-sectional view taken along line IV-IV in FIG. 3.

[0057] As shown in Figures 3 and 4, the semiconductor device 2 of the second embodiment mainly has a heat sink 120, a substrate 110, terminals 101, 102, 103, a case 190, a transistor 200, a diode 300, a buffer plate 400, and a buffer plate 500.

[0058] Terminals 101 and 102 are arranged on the upper surface (surface on the Z1 side) of end wall portion 193, and terminal 103 is arranged on the upper surface (surface on the Z1 side) of end wall portion 194. For example, terminal 102 is arranged on the Y2 side of terminal 101. Terminals 101, 102, and 103 are each made of a metal plate.

[0059] The substrate 110 has an insulating substrate 119, a first conductive pattern 111, a second conductive pattern 112, a third conductive pattern 113, a fourth conductive pattern 114, and a conductive layer 115. The first conductive pattern 111, the second conductive pattern 112, the third conductive pattern 113, the fourth conductive pattern 114, and the conductive layer 115 are made of Cu.

[0060] The first conductive pattern 111, the second conductive pattern 112, the third conductive pattern 113, and the fourth conductive pattern 114 are provided on the Z1 side surface of the insulating substrate 119. The conductive layer 115 is provided on the Z2 side surface of the insulating substrate 119.

[0061] As shown in FIG. 4 , the transistor 200 mainly includes a silicon carbide substrate 210 , a gate electrode 231 , a source electrode 232 , and a drain electrode 233 .

[0062] The silicon carbide substrate 210 has a principal surface 210A and a principal surface 210B opposite to the principal surface 210A. The principal surface 210A is on the Z1 side of the principal surface 210B. The silicon carbide substrate 210 has, for example, a rectangular parallelepiped shape. The principal surfaces 210A and 210B are parallel to the XY plane. The gate electrode 231 and the source electrode 232 are provided on the principal surface 210A, and the drain electrode 233 is provided on the principal surface 210B. The transistor 200 is provided on the fourth conductive pattern 114. The gate electrode 231 and the source electrode 232 include, for example, an aluminum layer. The gate electrode 231 and the source electrode 232 may include an aluminum alloy layer such as an Al—Si alloy or an Al—Si—Cu alloy instead of the aluminum layer. The drain electrode 233 has an ohmic layer and a bonding layer provided on the ohmic layer. The ohmic layer includes, for example, nickel or a nickel alloy. Nickel or a nickel alloy has good contact resistance with silicon carbide. The bonding layer includes a nickel layer. The bonding layer may further include a gold layer or a silver layer provided on the nickel layer. When the drain electrode 233 includes a bonding layer, good bonding properties are obtained between the drain electrode 233 and the fourth conductive pattern 114. The drain electrode 233 is bonded to the fourth conductive pattern 114 using a bonding material 132 such as a silver sintered body or a copper sintered body. The transistor 200 is an example of a semiconductor chip. The silicon carbide substrate 210 is an example of a semiconductor substrate. The source electrode 232 is an example of a main electrode.

[0063] The buffer plate 400 is, for example, a laminated material having a first copper layer 410, an alloy layer 420, and a second copper layer 430. The alloy layer 420 is provided on the Z1 side of the first copper layer 410, and the second copper layer 430 is provided on the Z1 side of the alloy layer 420. That is, the alloy layer 420 is provided on the first copper layer 410, and the second copper layer 430 is provided on the alloy layer 420. The alloy layer 420 is an alloy material having a Curie point of 300°C or higher. The alloy layer 420 may, for example, contain Fe and Ni, with the proportion of Ni in the alloy layer 420 being 40% by mass or higher. The alloy layer 420 may, for example, contain Fe, Ni, and Co, with the total proportion of Ni and Co in the alloy layer 420 being 40% by mass or higher. The alloy layer 420 may also contain 29% by mass of Ni and 17% by mass of Co. In either case, the alloy layer 420 may contain Fe at a rate of 45% by mass or more, or 48% by mass or more. The alloy layer 420 may also contain approximately 0.7% by mass of manganese. The material of the alloy layer 420 may be Kovar. The thickness T4 of the buffer plate 400 is, for example, 0.05 mm or more and 0.5 mm or less. The thickness T4 of the buffer plate 400 may be 0.05 mm or more and 0.25 mm or less. For example, the thickness T4 of the buffer plate 400 is smaller than the thickness T3 of the transistor 200. The buffer plate 400 is disposed on the source electrode 232. The first copper layer 410 is bonded to the source electrode 232 using a buffer bonding material 134 such as a silver sintered body or a copper sintered body. The buffer bonding material 134 has a sintered body with a porosity of 5% to 40%.

[0064] The silicon carbide substrate 210 has a first linear expansion coefficient ρ1', the buffer plate 400 has a second linear expansion coefficient ρ2', and the source electrode 232 has a third linear expansion coefficient ρ3'. Unless otherwise specified, the linear expansion coefficient in this disclosure refers to the linear expansion coefficient in a direction parallel to the main surface 210A at 25°C. Furthermore, unless otherwise specified, the linear expansion coefficient in this disclosure refers to the linear expansion coefficient when the silicon carbide substrate 210, the buffer plate 400, and the source electrode 232 are released from their bonded state and are taken as a single unit. The first linear expansion coefficient ρ1' and the second linear expansion coefficient ρ2' are smaller than the third linear expansion coefficient ρ3', and the second linear expansion coefficient ρ2' is smaller than the first linear expansion coefficient ρ1'. For example, when the first linear expansion coefficient ρ1' is 4.0×10 -6 / °C, while the second linear expansion coefficient ρ2' is 1.2 × 10 -6 / ℃ or more 3.9 x 10 -6 / °C or less. In this case, the value of "ρ2' - ρ1'" is -2.8 × 10 -6 / ℃ or more -0.1 x 10 -6 / °C or less. When the source electrode 232 is made of aluminum, the third linear expansion coefficient ρ3' is 23.1 × 10 -6 / ℃.

[0065] The semiconductor device 2 further includes wires 161, 162, 163, 164, 165, and 166. The number of each of the wires 161, 162, 163, 164, 165, and 166 is not limited, and may be one, or two or more.

[0066] Wire 161 connects gate electrode 231 of transistor 200 to first conductive pattern 111. Wire 162 connects second copper layer 430 of buffer plate 400 to second conductive pattern 112. Wire 163 connects third conductive pattern 113 to fourth conductive pattern 114. Wire 164 connects first conductive pattern 111 to terminal 101. Wire 165 connects second conductive pattern 112 to terminal 102. Wire 166 connects anode electrode 332 of diode 300 to terminal 103. Wires 161, 162, 163, 164, 165, and 166 are, for example, copper wires. Each of wires 161, 162, 163, 164, 165, and 166 has a diameter of, for example, 100 μm or more and 400 μm or less. The wires 161, 162, 163, 164, 165 and 166 are bonded together by, for example, ultrasonic bonding.

[0067] Other configurations of the second embodiment, such as the configurations of the diode 300 and the buffer plate 500, are the same as those of the first embodiment.

[0068] As described above, in this embodiment, the alloy layer 420 is made of an alloy material having a Curie point of 300° C. or higher. In other words, the thermal expansion of the alloy layer 420 is small at temperatures below 300° C. Therefore, in this embodiment, thermal deformation of the alloy layer 420 and the buffer plate 400 is suppressed in a power cycle test in which the maximum bonding temperature (Tjmax) is set to 250° C.

[0069] Furthermore, since thermal deformation of the buffer plate 400 is suppressed, thermal deformation of the source electrode 232 joined to the buffer plate 400 by the buffer bonding material 134 is also suppressed. Therefore, according to this embodiment, even when used at high temperatures, thermal stress occurring in the source electrode 232 due to thermal deformation can be suppressed, and internal destruction of the source electrode 232 can be suppressed.

[0070] Furthermore, in this embodiment, the buffer bonding material 134 has a sintered body with a porosity of 5% to 40%. Therefore, as with the diode 300, the thermal stress acting on the buffer bonding material 134 is reduced, thereby suppressing thermal deformation of the source electrode 232. Therefore, according to this embodiment, even when used at high temperatures, the thermal stress generated in the source electrode 232 due to thermal deformation can be suppressed, and internal destruction of the source electrode 232 can be suppressed. The porosity of the sintered body included in the buffer bonding material 134 may be 5% to 30% or 5% to 20%.

[0071] Because the source electrode 232 includes an aluminum layer or an aluminum alloy layer, good conductivity is easily achieved in the source electrode 232. Meanwhile, the first linear expansion coefficient ρ1' of the silicon carbide substrate 210 and the second linear expansion coefficient ρ2' of the buffer plate 400 are smaller than the third linear expansion coefficient ρ3' of the source electrode 232, and the second linear expansion coefficient ρ2' is smaller than the first linear expansion coefficient ρ1'. In this case, the source electrode 232 tends to thermally deform to a greater extent than the silicon carbide substrate 210. However, because the second linear expansion coefficient ρ2' is smaller than the first linear expansion coefficient ρ1', the thermal deformation of the source electrode 232 can be effectively suppressed by the buffer bonding material 134. Therefore, thermal stress generated in the source electrode 232 due to thermal deformation can be suppressed, and internal destruction of the source electrode 232 can be suppressed.

[0072] In this embodiment, by bonding the wire 162 to the buffer plate 400, the wire 162 can be electrically connected to the source electrode 232 via the buffer plate 400. Therefore, even if ultrasonic bonding is used to bond the wire 162, damage to the transistor 200 can be suppressed. If the wire 162 is a copper wire, it is easy to bond the wire 162 to the second copper layer 430 of the buffer plate 400, and it is also easy to obtain low electrical resistance for the wire 162.

[0073] The buffer plate 400 may not include the first copper layer 410 and the second copper layer 430. In other words, the buffer plate 400 may be made of an alloy layer 420 such as Kovar, whose Curie point is 300° C. or higher.

[0074] When alloy layer 420 contains Fe and Ni and the proportion of Ni in alloy layer 420 is 40 mass% or more, it is easy to obtain a Curie point of 300° C. or higher in alloy layer 420. When alloy layer 420 contains Fe, Ni, and Co and the total proportion of Ni and Co in alloy layer 420 is 40 mass% or more, it is also easy to obtain a Curie point of 300° C. or higher in alloy layer 420.

[0075] If the Curie point of the alloy layer 420 is 300° C. or higher, the porosity of the buffer bonding material 134 does not have to be 5% or higher and 40% or lower. Also, if the porosity of the buffer bonding material 134 is 5% or higher and 40% or lower, the Curie point of the alloy layer 420 does not have to be 300° C. or higher.

[0076] A plurality of transistors 200 may be provided on the fourth conductive pattern 114. In this case, the plurality of transistors 200 are electrically connected in parallel to one another.

[0077] (Characteristics Test) Next, an example of the results of a power cycle test on the semiconductor device according to the embodiment of the present disclosure will be described. The power cycle test is performed in accordance with IEC 60749 as follows.

[0078] In the power cycle test, the temperature of the sample was raised from room temperature (25°C) to 65°C, and then a current of 125 A was repeatedly applied and cut off. The current application time was 1 second, and the cut-off time was 13 seconds. The maximum junction temperature (Tjmax), which is the maximum value of the junction temperature (Tj) in each cycle, was 250°C, and the difference (ΔT) between the maximum junction temperature and the minimum junction temperature (65°C) in each cycle was 185°C.

[0079] The current initiation voltage when a low current of about 100 mA is passed through the sample corresponds to the junction temperature (Tj) of the sample. Therefore, by passing a low current of 100 mA, which is sufficiently smaller than the current passed immediately after current is passed through the sample, through each power-on and power-off cycle and measuring the current initiation voltage at this time, the current initiation temperature for each cycle can be converted into the maximum junction temperature (Tjmax). As the power cycle test progresses, the sample gradually deteriorates and the maximum junction temperature (Tjmax) gradually increases. Therefore, the life in this test is defined as the point at which the difference (ΔT) from the start of current application increases by 20%. As mentioned above, if the minimum junction temperature is 65°C and the maximum junction temperature is 250°C, the difference (ΔT) is 185°C, so the life is defined as the point at which the maximum junction temperature (Tjmax) reaches 287°C. This test is conducted in accordance with the IEC 60749 inspection standard established by the International Organization for Standardization, so the lifespans of power module samples with different structures and manufacturing methods can be compared using the same standards.

[0080] Figure 5 shows an example of the results of a power cycle test. Figure 5 shows the results of a power cycle test for a total of four types of samples (Samples No. 1, No. 2, No. 3, and No. 4). In this power cycle test, diodes were used as samples. The horizontal axis of Figure 5 represents the number of cycles of current application and interruption, and the vertical axis represents the maximum junction temperature (Tjmax). The buffer plate and buffer bonding material configurations were different among the four types of samples, while the other conditions were the same. Table 1 shows an overview of the buffer plate and buffer bonding material for the four types of samples. Table 1 also shows the proportions of Ni and Co that make up the alloy layer. Table 1 also shows the number of cycles at which the difference (ΔT) increased by 20% (life).

[0081]

[0082] As shown in Fig. 5 and Table 1, in sample No. 1, the material of the alloy layer was Invar, the Curie point was 280°C, the porosity of the sintered body included in the buffer bonding material was 3%, and the life was 19,700 cycles.

[0083] In sample No. 2, the material of the alloy layer was Kovar, the Curie point was 435°C, and the porosity of the sintered body included in the buffer bonding material was 3%. The lifespan of sample No. 2 was 45,400 cycles. The lifespan of sample No. 2 was 2.3 times longer than that of sample No. 1.

[0084] In sample No. 3, the alloy layer was made of Invar, the Curie point was 280°C, and the porosity of the sintered body included in the buffer bonding material was 30%. The lifespan of sample No. 3 was 49,900 cycles. The lifespan of sample No. 3 was 2.5 times longer than that of sample No. 1.

[0085] In sample No. 4, the material of the alloy layer was Kovar, the Curie point was 435°C, and the porosity of the sintered body included in the buffer bonding material was 30%. The lifespan of sample No. 4 was 135,100 cycles. The lifespan of sample No. 4 was 6.8 times longer than that of sample No. 1.

[0086] Thus, in Samples No. 2, No. 3, and No. 4, which satisfy at least one of the conditions that the Curie point of the alloy layer is 300°C or higher or the sintered body contained in the buffer bonding material is 5% to 40%, excellent life was obtained even under the condition of a high operating temperature of 250°C.

[0087] Furthermore, the lifespan of Sample No. 2 was 2.3 times that of Sample No. 1, and the lifespan of Sample No. 3 was 2.5 times that of Sample No. 1. Multiplying these results, it can be inferred that the lifespan of Sample No. 4 would be 5.75 times that of Sample No. 1, but in reality it was 6.8 times longer. This demonstrates that the combination of an alloy layer having a Curie point of 300°C or higher and a sintered body having a porosity of 5% to 40% can produce a greater effect than the combination of the respective effects.

[0088] In the present disclosure, the Curie point of the alloy layer or alloy material may be 350°C or higher, or 400°C or higher.

[0089] The porosity of a sintered body is determined by observing the cross section of the buffer plate under an electron microscope and calculating the ratio of the total area of ​​pores to the area of ​​the cross section. When observing the cross section, the sample is usually mechanically polished, with careful attention paid to not blocking the pores. After mechanical polishing, surface damage can be removed by sputtering, or the accelerating voltage of the electron beam can be increased during electron microscopy to eliminate the influence of the surface layer, making it easier to determine the porosity more accurately.

[0090] The porosity of the sintered body can be adjusted depending on the pressure applied during the heat treatment in hydrogen gas to form the buffer bonding material. For example, when the pressure is 20 MPa, the porosity is about 3%, and when the pressure is 3 MPa, the porosity is about 30%.

[0091] In the present disclosure, an aluminum alloy layer may be used in place of an aluminum layer for the main electrode. Furthermore, the material used for the buffer bonding material is not limited. For example, the buffer bonding material may be made of a sintered body of an intermetallic compound containing copper, silver, nickel, or copper and tin. The sintered body of the intermetallic compound containing copper and tin can be obtained, for example, by transient liquid phase sintering.

[0092] In the present disclosure, the semiconductor chip may be a silicon carbide chip. Silicon carbide chips have excellent high-temperature resistance and are less likely to break down even when used at high temperatures. Silicon carbide chips also have high mechanical properties. Furthermore, internal breakdown of the main electrode is suppressed, making it easier for the semiconductor device as a whole to have a long life even at high temperatures.

[0093] Although the embodiments have been described in detail above, the present disclosure is not limited to the specific embodiments, and various modifications and changes are possible within the scope of the claims.

[0094] 1, 2 Semiconductor device 101, 102, 103 Terminal 110 Substrate 111 First conductive pattern 112 Second conductive pattern 113 Third conductive pattern 114 Fourth conductive pattern 115 Conductive layer 119 Insulating substrate 120 Heat sink 131, 132, 133 Bonding material 134, 135 Buffer bonding material 161, 162, 163, 164, 165, 166: Wire 190 Case 191, 192 Side wall portion 193, 194 End wall portion 200 Transistor (semiconductor chip) 210 Silicon carbide substrate (semiconductor substrate) 210A, 210B Main surface 231 Gate electrode 232 Source electrode (main electrode) 233 Drain electrode 300 Diode (semiconductor chip) 310 Silicon carbide substrate (semiconductor substrate) 310A, 310B: Main surface 332: Anode electrode (main electrode) 333: Cathode electrode 400, 500: Buffer plate 410, 510: First copper layer 420, 520: Alloy layer 430, 530: Second copper layer

Claims

1. A semiconductor device comprising: a semiconductor chip having a semiconductor substrate and a main electrode provided on the semiconductor substrate; a buffer plate; and a buffer bonding material provided between the main electrode and the buffer plate, wherein the buffer plate is a laminate material or an alloy material having a Curie point of 300°C or higher, and the laminate material has: a first copper layer in contact with the buffer bonding material; an alloy layer having a Curie point of 300°C or higher provided on the first copper layer; and a second copper layer provided on the alloy layer.

2. The semiconductor device according to claim 1, wherein the buffer bonding material has a sintered body with a porosity of 5% or more and 40% or less.

3. The semiconductor device according to claim 1 or 2, wherein the alloy material and the alloy layer contain iron and nickel, and the proportion of nickel in the alloy material and the alloy layer is 40 mass % or more.

4. The semiconductor device according to claim 1 or 2, wherein said alloy material and said alloy layer contain iron, nickel and cobalt, and the total proportion of nickel and cobalt in said alloy material and said alloy layer is 40 mass % or more.

5. A semiconductor device comprising: a semiconductor chip having a semiconductor substrate and a main electrode provided on the semiconductor substrate; a buffer plate; and a buffer bonding material provided between the main electrode and the buffer plate, the buffer bonding material having a sintered body with a porosity of 5% or more and 40% or less.

6. The semiconductor device according to claim 1, wherein the main electrode includes an aluminum layer or an aluminum alloy layer.

7. The semiconductor device according to claim 6, wherein a first linear expansion coefficient of said semiconductor substrate and a second linear expansion coefficient of said buffer plate are smaller than a third linear expansion coefficient of said main electrode, and said second linear expansion coefficient is smaller than said first linear expansion coefficient.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method thereof

    JP2013098266A