Propylene-based resin composition
Incorporating di-tert-butylphenol into propylene-based resin compositions addresses the static electricity challenges, enhancing antistatic performance and reducing dust adhesion on molded products.
Patent Information
- Application Number
- PCT/JP2024/019162
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Propylene-based resin compositions exhibit low conductivity, leading to static electricity issues during molding, causing dirt and dust to adhere to molded products, which affects their performance and quality.
Incorporating di-tert-butylphenol into the propylene-based resin composition at specific concentrations (10 to 1800 ppm) enhances antistatic performance by improving the dissipation of static electricity.
The addition of di-tert-butylphenol effectively addresses the static electricity issues, resulting in propylene resin compositions with excellent antistatic properties and improved cleanliness of molded articles.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Propylene-based resin composition
[0001] The present invention relates to a propylene-based resin composition and a molded article thereof.
[0002] A propylene-based resin composition containing a propylene-based polymer has good mechanical properties and can be used in various applications, such as automobile interior components.
[0003] Japanese Patent Application Laid-Open No. 2001-019825
[0004] However, since propylene-based resin compositions have low electrical conductivity, static electricity generated during molding or other processes does not easily dissipate, and as a result, dust and dirt may adhere to the resulting molded product. The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a propylene-based resin composition and the like having excellent antistatic properties.
[0005] The present inventors have conducted extensive research to solve the above problems and have found that the above problems can be solved by adding an appropriate amount of di-tert-butylphenol to a propylene-based resin composition, thereby completing the present invention.
[0006] [1] A propylene-based resin composition containing a propylene-based polymer and di-tert-butylphenol, wherein the content of di-tert-butylphenol is 10 to 1,800 ppm by mass, based on 100 parts by mass of the total mass of the propylene-based resin composition. [2] The propylene-based resin composition according to [1], wherein the content of the propylene-based polymer is 50 parts by mass or more, based on 100 parts by mass of the total mass of the propylene-based resin composition. [3] The propylene-based resin composition according to [1] or [2], further containing an ethylene-α-olefin copolymer. [4] The propylene-based resin composition according to [3], wherein the content of the ethylene-α-olefin copolymer is 1 to 40 parts by mass, based on 100 parts by mass of the total mass of the propylene-based resin composition. [5] The propylene-based resin composition according to any one of [1] to [4], further containing an inorganic filler. [6] The propylene-based resin composition according to [5], wherein the content of the inorganic filler is 1 to 40 parts by mass, relative to 100 parts by mass of the total mass of the propylene-based resin composition. [7] The propylene-based resin composition according to any one of [1] to [6], further comprising an ethylene-α-olefin copolymer and an inorganic filler. [8] A molded article comprising the propylene-based resin composition according to any one of [1] to [7].
[0007] According to the present invention, it is possible to provide a propylene-based resin composition having excellent antistatic properties and a molded article of the propylene-based resin composition.
[0008] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the specific embodiments shown below.
[0009] Explanation of Terms Before describing the embodiments of the present invention, commonly used terms will be explained.
[0010] In this specification, the term "monomer unit" refers to a structural unit (residue) derived from a monomer contained in a polymer obtained by polymerizing a monomer.
[0011] As used herein, the term "α-olefin" refers to an olefin containing a carbon atom chain of three or more carbon atoms having a terminal (α-position) carbon-carbon double bond.
[0012] In this specification, the "intrinsic viscosity (unit: dL / g)" is a value measured at a temperature of 135°C using tetralin as a solvent by the following method.
[0013] Specifically, the intrinsic viscosity can be determined by an "extrapolation method" in which reduced viscosities are measured at a plurality of concentrations using an Ubbelohde viscometer, the reduced viscosities are plotted against the concentrations, and the concentrations are extrapolated to zero. More specifically, the intrinsic viscosity can be determined by the method described on page 491 of "Polymer Solutions, Polymer Experiments 11" (published by Kyoritsu Shuppan Co., Ltd. in 1982), in which reduced viscosities are measured at three concentrations of 0.1 g / dL, 0.2 g / dL, and 0.5 g / dL, the reduced viscosities are plotted against the concentrations, and the concentrations are extrapolated to zero.
[0014] In this specification, "melt flow rate (MFR)" means "melt mass flow rate" and is a melt flow rate measured in accordance with JIS K7210-1:2014 and K7210-2:2014 under conditions of a temperature of 230°C and a load of 2.16 kgf.
[0015] In this specification, unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass".
[0016] (Propylene-Based Resin Composition) The propylene-based resin composition according to an embodiment of the present invention is a propylene-based resin composition containing a propylene polymer (A) and di-tert-butylphenol (B), wherein the content of di-tert-butylphenol (B) is 10 to 1800 ppm by mass when the total mass of the propylene-based resin composition is 100 parts by mass.
[0017] The propylene-based resin composition of this embodiment has excellent antistatic properties.
[0018] Components that may be contained in the propylene-based resin composition of this embodiment will be described below.
[0019] Propylene-Based Polymer (A) A propylene-based polymer is a polymer containing propylene units in an amount of more than 50% by mass relative to all constituent units (100% by mass). The propylene units in a propylene-based polymer are usually 100% by mass or less.
[0020] Examples of propylene-based polymers include propylene homopolymers and copolymers obtained by polymerizing propylene and one or more other monomers copolymerizable with propylene in any combination in any ratio. The copolymers may be random copolymers or block copolymers.
[0021] Examples of other monomers copolymerizable with propylene include olefins other than propylene (e.g., ethylene, olefins having 4 or more carbon atoms). The olefin may have 12 or less carbon atoms.
[0022] The olefin having 4 or more carbon atoms may be a linear olefin or a branched olefin. The olefin having 4 or more carbon atoms may be an olefin having a cyclic structure, such as an α-olefin having a cyclic structure such as vinylcyclopropane or vinylcyclobutane.
[0023] Examples of olefins other than propylene that can be copolymerized with propylene include α-olefins other than propylene (e.g., ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene). The olefins other than propylene that can be copolymerized with propylene are preferably ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and more preferably ethylene, propylene, 1-butene, 1-hexene, and 1-octene.
[0024] (Propylene-Based Random Copolymer) Examples of the propylene-based random copolymer include a random copolymer containing propylene units and ethylene units (hereinafter also referred to as random polymer (1)); a random copolymer containing propylene units and α-olefin units having 4 or more carbon atoms (hereinafter also referred to as random polymer (2)); and a random copolymer containing propylene units, ethylene units, and α-olefin units having 4 or more carbon atoms (hereinafter also referred to as random polymer (3)).
[0025] The α-olefin having 4 or more carbon atoms that can constitute the propylene-based random copolymer is preferably an α-olefin having 4 to 10 carbon atoms. Examples of the α-olefin having 4 to 10 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and preferably 1-butene, 1-hexene, and 1-octene.
[0026] Examples of the random copolymer (2) include propylene-1-butene random copolymer, propylene-1-hexene random copolymer, propylene-1-octene random copolymer, and propylene-1-decene random copolymer.
[0027] Examples of the random copolymer (3) include propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, and propylene-ethylene-1-decene copolymer.
[0028] The content of ethylene units in the random copolymer (1) is preferably 0.1 to 40% by mass.
[0029] The content of α-olefin units having 4 or more carbon atoms in the random copolymer (2) is preferably 0.1 to 40 mass%, more preferably 0.1 to 30 mass%, and even more preferably 2 to 15 mass%.
[0030] The total content of ethylene units and α-olefin units having 4 or more carbon atoms in the random copolymer (3) is preferably 0.1 to 40 mass%, more preferably 0.1 to 30 mass%, and even more preferably 2 to 15 mass%.
[0031] The content of propylene units in each of these random copolymers (1) to (3) is preferably 60 to 99.9% by mass.
[0032] The propylene polymer (A) can be produced, for example, by the following polymerization method using a polymerization catalyst.
[0033] Examples of polymerization catalysts include Ziegler-type catalyst systems; Ziegler-Natta-type catalyst systems; catalyst systems containing a Group 4 transition metal compound having a cyclopentadienyl ring and an alkylaluminoxane; catalyst systems containing a Group 4 transition metal compound having a cyclopentadienyl ring, a compound that reacts with the metal compound to form an ionic complex, and an organoaluminum compound; and catalyst systems in which catalyst components (e.g., a Group 4 transition metal compound having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) are supported on inorganic particles (e.g., silica, clay minerals, etc.) and modified. Prepolymerization catalysts prepared by prepolymerizing monomers such as ethylene and α-olefins in the presence of such catalyst systems may also be used. Examples of Ziegler-Natta-type catalyst systems include catalyst systems that use a combination of a titanium-containing solid transition metal component and an organometallic component.
[0034] Examples of such catalyst systems include those described in JP-A-61-218606, JP-A-5-194685, JP-A-7-216017, JP-A-9-316147, JP-A-10-212319, and for heterophasic propylene polymer materials, JP-A-2004-182981.
[0035] Examples of polymerization methods include bulk polymerization, solution polymerization, and gas-phase polymerization. Here, bulk polymerization refers to a method in which polymerization is carried out using an olefin that is liquid at the polymerization temperature as a medium. Solution polymerization refers to a method in which polymerization is carried out in an inert hydrocarbon solvent such as propane, butane, isobutane, pentane, hexane, heptane, or octane. Gas-phase polymerization refers to a method in which gaseous monomers are used as a medium and the gaseous monomers are polymerized in that medium.
[0036] Examples of the polymerization method include a batch system, a continuous system, and a combination thereof. The polymerization method may be a multi-stage system using a plurality of polymerization reactors connected in series.
[0037] Various conditions in the polymerization method (polymerization temperature, polymerization pressure, monomer concentration, catalyst input amount, polymerization time, etc.) can be appropriately determined depending on the desired propylene-based polymer.
[0038] In the production of a propylene polymer, the resulting propylene polymer may be maintained at a temperature at which impurities such as residual solvent and oligomers can volatilize and which is lower than the temperature at which the propylene polymer melts, thereby removing residual solvent contained in the resulting propylene polymer and ultralow molecular weight oligomers by-produced during the production. Examples of methods for removing impurities such as residual solvent and oligomers include the methods described in JP-A-55-75410 and JP-A-2565753.
[0039] From the viewpoint of improving the fluidity of the propylene-based resin composition when melted and the toughness of a molded article obtained by molding the propylene-based resin composition, the propylene homopolymer preferably has an intrinsic viscosity [η] of 0.1 to 5 dL / g, more preferably 0.5 to 4 dL / g, and even more preferably 0.6 to 3 dL / g.
[0040] Furthermore, from the viewpoint of improving the fluidity of the propylene-based resin composition when melted and the toughness of a molded article containing the resin composition, the propylene homopolymer preferably has a molecular weight distribution Mw / Mn of 2 or more but less than 10, more preferably 3 to 8, and even more preferably 3 to 6. Here, Mw represents the weight-average molecular weight, and Mn represents the number-average molecular weight. The molecular weight distribution can be measured by gel permeation chromatography (GPC).
[0041] The propylene resin composition of the present embodiment may contain two or more types of propylene polymers as the propylene polymer (A).
[0042] Examples of combinations of two or more propylene polymers when two or more propylene-based polymers are contained include combinations of two or more propylene homopolymers having different weight average molecular weights, and heterophasic propylene polymer materials.
[0043] Here, the term "heterophasic propylene polymer material" refers to a material containing two or more types of propylene polymers, in which the two or more types of propylene polymers are not compatible with each other and form separate phases.
[0044] Examples of heterophasic propylene polymer materials include materials containing a combination of polymer (I) and polymer (II) below.
[0045] Here, polymer (I) is a polymer having propylene units in an amount of more than 80% by mass and not more than 100% by mass relative to the amount of all structural units. Polymer (I) may be a propylene homopolymer or a copolymer of propylene and other monomers. The total content of monomer units other than propylene units in polymer (I) is usually 0% by mass or more and less than 20% by mass, and may be 0% by mass or more, or may be 0.01% by mass or more, when the mass of polymer (I) is taken as 100% by mass.
[0046] Examples of monomer units other than propylene units that may be contained in the polymer (I) include ethylene units and α-olefin units having 4 or more carbon atoms.
[0047] The α-olefin having 4 or more carbon atoms that can constitute the polymer (I) is preferably an α-olefin having 4 to 10 carbon atoms, more preferably 1-butene, 1-hexene, and 1-octene, and even more preferably 1-butene.
[0048] Examples of polymer (I) include propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, and propylene-ethylene-1-octene copolymer.
[0049] Among these, as the polymer (I), a propylene homopolymer, a propylene-ethylene copolymer, a propylene-1-butene copolymer, and a propylene-ethylene-1-butene copolymer are preferred, and from the viewpoint of improving the rigidity of a molded article obtained by molding the propylene-based resin composition, a propylene homopolymer is more preferred.
[0050] Furthermore, polymer (II) is a copolymer of propylene units and at least one monomer unit selected from the group consisting of ethylene units and α-olefin units having 4 or more carbon atoms. Polymer (II) is preferably a polymer containing propylene units in an amount of more than 0 mass% and not more than 90 mass%, more preferably more than 0 mass% and not more than 80 mass%, based on the amount of all structural units. Polymer (II) may be a random copolymer or a block copolymer.
[0051] The total content of ethylene units and α-olefin units having 4 or more carbon atoms in polymer (II) is preferably 20 to 80 mass%, and more preferably 20 to 60 mass%, when the mass of polymer (II) is taken as 100 mass%.
[0052] The α-olefin having 4 or more carbon atoms that can constitute polymer (II) is preferably an α-olefin having 4 to 10 carbon atoms, and examples thereof include the same as the examples of α-olefins that can constitute polymer (I) already described above.
[0053] Examples of polymer (II) include propylene-ethylene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, propylene-ethylene-1-decene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, and propylene-1-decene copolymer. Polymer (II) is preferably a propylene-ethylene copolymer, a propylene-1-butene copolymer, or a propylene-ethylene-1-butene copolymer, and more preferably a propylene-ethylene copolymer.
[0054] The content of polymer (II) in the heterophasic propylene polymer material is preferably 1 to 50 mass%, more preferably 1 to 45 mass%, even more preferably 5 to 40 mass%, and particularly preferably 7 to 35 mass%, when the total mass of polymer (I) and polymer (II) is 100 mass%.
[0055] The polymer (I) and the polymer (II) may each consist of only one type of polymer, or may contain two or more types of polymers.
[0056] Examples of heterophasic propylene polymer materials include those in which polymer (I) is a propylene homopolymer, a combination of a propylene homopolymer and a (propylene-ethylene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-hexene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-octene) copolymer, a combination of a propylene homopolymer and a (propylene-1-butene) copolymer, a combination of a propylene homopolymer and a (propylene-1-hexene) copolymer, a combination of a propylene homopolymer and a (propylene-1-octene) copolymer, and a combination of a propylene homopolymer and a (propylene-1-decene) copolymer.
[0057] The heterophasic propylene polymer material may also be a combination in which the polymer (I) is a polymer containing propylene units and monomer units other than propylene units. If the type of polymer (I) is listed first and the type of polymer (II) is listed second, specific examples of such heterophasic propylene polymer materials include a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-hexene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-decene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene ... a combination of a (propylene-1-decene) copolymer and a (propylene-1-decene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-hexene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-octene) copolymer, a combination of a (propylene-ethylene-1-butene) copolymer and a (propylene-ethylene-1-decene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-butene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-decene) copolymer,Examples of the copolymer include a combination of a (propylene-1-hexene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-1-hexene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-1-hexene) copolymer and a (propylene-1-decene) copolymer, a combination of a (propylene-1-octene) copolymer and a (propylene-1-octene) copolymer, and a combination of a (propylene-1-octene) copolymer and a (propylene-1-decene) copolymer.
[0058] Preferred heterophasic propylene polymer materials that can be contained in the propylene-based resin composition of the present embodiment include a combination of a propylene homopolymer and a (propylene-ethylene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-butene) copolymer, and a combination of a (propylene-1-butene) copolymer and a (propylene-1-butene) copolymer, with a combination of a propylene homopolymer and a (propylene-ethylene) copolymer being more preferred.
[0059] The heterophasic propylene polymer material can be produced by multi-stage polymerization including a first polymerization step of producing polymer (I) and a second polymerization step of producing polymer (II) in the presence of polymer (I) produced in the first step. The polymerization can be carried out using the catalyst system exemplified above as a catalyst usable for producing the propylene polymer.
[0060] The propylene polymer (A) preferably contains at least one selected from the group consisting of propylene homopolymers and heterophasic propylene polymer materials.
[0061] The propylene polymer (A) is 13The isotactic pentad fraction (also referred to as the [mmmm] fraction) measured by C-NMR is preferably 0.97 or more, more preferably 0.98 or more. The closer the isotactic pentad fraction of the propylene polymer is to 1, the higher the stereoregularity of the molecular structure of the propylene polymer and the higher the crystallinity of the propylene polymer. When the propylene polymer is a copolymer, the isotactic pentad fraction can be measured for the chain of propylene units in the copolymer.
[0062] From the viewpoint of improving the processability in molding of the propylene-based resin composition, the propylene polymer (A) preferably has a melt flow rate (MFR) measured under conditions of a temperature of 230°C and a load of 2.16 kgf of 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, and preferably 500 g / 10 min or less, more preferably 400 g / 10 min or less, and preferably 0.1 g / 10 min to 500 g / 10 min.
[0063] From the viewpoint of improving the fluidity and processability of the propylene-based resin composition, the intrinsic viscosity of the propylene-based polymer (A) of the present embodiment is usually less than 5 dL / g, 0.1 dL / g or more, preferably 0.5 dL / g or more, more preferably 0.7 dL / g or more and less than 4 dL / g, and even more preferably 0.8 dL / g or more and less than 3 dL / g.
[0064] In the present embodiment, the polystyrene-equivalent weight average molecular weight of the propylene polymer (A) is usually 100,000 to 1,000,000, and preferably 500,000 to 1,000,000, from the viewpoint of improving the appearance and elongation properties of the molded article.
[0065] The propylene polymer (A) may have a molecular weight distribution (Mw / Mn) of usually 10 or less, preferably 3-8, from the viewpoint of improving moldability and mechanical properties.
[0066] Here, Mw represents the weight average molecular weight, and Mn represents the number average molecular weight. The weight average molecular weight, number average molecular weight, and molecular weight distribution can be measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.
[0067] When the propylene-based polymer is a polymer material composed of a polymer (I) and a polymer (II) formed by multistage polymerization, a part of the polymer (I) prepared in the first polymerization stage is extracted from the polymerization reactor to determine its intrinsic viscosity, and the intrinsic viscosity (hereinafter referred to as ([η] Total)) of the propylene-based polymer finally obtained by the multistage polymerization is determined, and the intrinsic viscosity of the polymer formed in the second polymerization stage can be calculated using these intrinsic viscosity values and the content of each polymer.
[0068] Furthermore, when a polymer material consisting of polymer (I) and polymer (II) is a material produced by a method in which polymer (I) is obtained in an earlier polymerization step and polymer (II) is obtained in a later polymerization step, the procedures for measuring and calculating the contents and intrinsic viscosities ([η] Total, [η] I, and [η] II) of polymer (I) and polymer (II) are as follows.
[0069] The intrinsic viscosity [η]II of polymer (II) can be calculated by the following formula from the intrinsic viscosity ([η]I) of polymer (I) obtained in the previous polymerization step, the intrinsic viscosity ([η]Total) of the final polymer after the subsequent polymerization step (i.e., a polymer composed of polymer (I) and polymer (II)) measured by the above-mentioned method, and the content of polymer (II) contained in the final polymer.
[0070] [η]II = ([η]Total - [η]I × XI) / XII [η]Total: intrinsic viscosity of the final polymer (unit: dL / g) [η]I: intrinsic viscosity of polymer (I) (unit: dL / g) XI: mass ratio of polymer (I) to the final polymer XII: mass ratio of polymer (II) to the final polymer Note that XI and XII can be determined from the mass balance during polymerization.
[0071] The intrinsic viscosity (hereinafter referred to as [η]I) of the polymer (I) is preferably 0.1 to 5 dL / g, more preferably 0.5 to 4 dL / g, and even more preferably 0.6 to 3 dL / g.
[0072] The intrinsic viscosity (hereinafter referred to as [η]II) of the polymer (II) is preferably 1 to 10 dL / g, more preferably 1.5 to 9 dL / g, and even more preferably 2 to 8 dL / g.
[0073] The ratio of [η]II to [η]I ([η]II / [η]I) is preferably 1-20, more preferably 1-10.
[0074] The mass ratio XII of polymer (II) to the final polymer may be calculated from the following formula using the heat of crystalline fusion of each of polymer (I) and the final polymer: XII=1-(ΔHf)T / (ΔHf)P, where (ΔHf)T: heat of fusion of the final polymer (polymer (I) and polymer (II)) (unit: cal / g) (ΔHf)P: heat of fusion of polymer (I) (unit: cal / g).
[0075] The molecular weight distribution (Mw / Mn) of the polymer (I) measured by GPC is preferably 1 or more and less than 10, more preferably 2 or more and less than 7, and even more preferably 3 or more and less than 5.
[0076] The content of the propylene polymer (A) in the propylene resin composition of the present embodiment is preferably 50 parts by mass or more, may be 60 parts by mass or more, may be 70 parts by mass or more, may be 80 parts by mass or more, may be 90 parts by mass or more, and may be 99 parts by mass or less, may be 50 to 95 parts by mass, or may be 60 to 95 parts by mass, relative to 100 parts by mass of the total mass of the propylene resin composition.
[0077] Di-tert-butylphenol (B) The propylene-based resin composition of this embodiment contains di-tert-butylphenol. Specific examples of "di-tert-butylphenol" include 2,4-di-tert-butylphenol, 2,6-di-tert-butylphenol, and 3,5-di-tert-butylphenol. The structural formula of 2,4-di-tert-butylphenol is shown below.
[0078] In the present embodiment, the content of di-tert-butylphenol is, from the viewpoint of exhibiting antistatic performance, 10 ppm by mass or more, optionally 20 ppm by mass or more, optionally 50 ppm by mass or more, optionally 70 ppm by mass or more, optionally 100 ppm by mass or more, optionally 200 ppm by mass or more, optionally 250 ppm by mass or more, optionally 300 ppm by mass or more, or optionally 400 ppm by mass or more, relative to 100 parts by mass of the total mass of the propylene-based resin composition. From the same viewpoint, the content of di-tert-butylphenol is 1800 ppm by mass or less, optionally 1600 ppm by mass or less, optionally 1400 ppm by mass or less, optionally 1200 ppm by mass or less, optionally 1000 ppm by mass or less, optionally 900 ppm by mass or less, optionally 800 ppm by mass or less, optionally 700 ppm by mass or less, or optionally 600 ppm by mass or less, when the total mass of the propylene-based resin composition is 100 parts by mass.
[0079] In the present embodiment, the content of di-tert-butylphenol is calculated based on the amount of raw materials charged in the production of the propylene-based resin composition. However, when the amount of raw materials charged is unknown, the content may be measured from the propylene-based resin composition, for example, pellets or a molded product.
[0080] Specifically, when measuring the content of di-tert-butylphenol in a resin composition, the amount of di-tert-butylphenol generated when a molded article obtained by molding a propylene-based resin composition under the following injection molding conditions is heated at 100°C for 15 minutes can be used as the content: Injection molding conditions: cylinder temperature; 200°C, mold temperature; 40°C, filling pressure; 15 MPa, dwell pressure; 4.3 MPa, dwell time; 40 seconds
[0081] More specifically, for example, the propylene-based resin composition of the present embodiment is injection-molded using any suitable conventional injection molding machine under the above-mentioned injection molding conditions to form 2 g of cuttings of a molded article, and the cuttings are heated at 100°C for 15 minutes to generate di-tert-butylphenol, which can be quantified by gas chromatography measurement using any suitable conventional gas chromatography measurement device.
[0082] If the content of di-tert-butylphenol in the propylene-based resin composition is as described above, the antistatic properties can be improved.
[0083] Ethylene-α-olefin copolymer (C) The propylene-based resin composition of the present embodiment may contain an ethylene-α-olefin copolymer.
[0084] In the ethylene-α-olefin copolymer (C), when the total mass of the ethylene-α-olefin copolymer is taken as 100 mass%, the sum of the content of the monomer units derived from ethylene and the content of the monomer units derived from an α-olefin having 4 or more carbon atoms may be 100 mass%.
[0085] Examples of α-olefins having 4 or more carbon atoms include α-olefins having 4 to 12 carbon atoms. Examples of α-olefins having 4 to 12 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene. Of the α-olefins having 4 or more carbon atoms, 1-butene, 1-hexene, and 1-octene are preferred. The α-olefin may also be an α-olefin having a cyclic structure, such as vinylcyclopropane or vinylcyclobutane.
[0086] Examples of the ethylene-α-olefin copolymer (C) include an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, an ethylene-1-decene copolymer, an ethylene-(3-methyl-1-butene) copolymer, and a copolymer of ethylene and an α-olefin having a cyclic structure.
[0087] In the ethylene-α-olefin copolymer (C), the content of the monomer units derived from an α-olefin having 4 or more carbon atoms is preferably 1 to 49 mass%, more preferably 5 to 49 mass%, and even more preferably 24 to 49 mass%, based on the total mass of the ethylene-α-olefin copolymer (100 mass%).
[0088] The ethylene-α-olefin copolymer (C) preferably has an MFR (measured at 190°C under a load of 2.16 kgf) of 0.1 g / 10 min or more and 100 g / 10 min or less, more preferably 0.5 g / 10 min or more and 70 g / 10 min or less.
[0089] The density of the ethylene-α-olefin copolymer (C) is 0.850 to 0.890 g / cm from the viewpoint of improving the impact resistance of the molded article. 3 is preferably 0.850 to 0.880 g / cm 3 More preferably, it is 0.855 to 0.870 g / cm 3 It is more preferable that:
[0090] The ethylene-α-olefin copolymer (C) can be produced by polymerizing ethylene and an α-olefin having 4 or more carbon atoms using a polymerization catalyst.
[0091] Examples of the polymerization catalyst used for the production include homogeneous catalysts such as metallocene catalysts, and Ziegler-Natta catalysts.
[0092] Examples of homogeneous catalysts include a catalyst comprising a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane; a catalyst comprising a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that reacts with the transition metal compound to form an ionic complex, and an organoaluminum compound; and a modified catalyst obtained by supporting a catalyst component (a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) on inorganic particles (silica, clay mineral, etc.).
[0093] Examples of Ziegler-Natta catalysts include catalysts that combine a titanium-containing solid transition metal component with an organometallic component.
[0094] The ethylene-α-olefin copolymer component (C) may be a commercially available product. Examples of commercially available ethylene-α-olefin copolymers (C) include ENGAGE (registered trademark) manufactured by Dow Chemical Japan, TAFMER (registered trademark) manufactured by Mitsui Chemicals, Inc., NEOZEX (registered trademark) and ULTOZEX (registered trademark) manufactured by Prime Polymer Co., Ltd., and EXCELLEN FX (registered trademark), SUMIKACENE (registered trademark), and ESPRENE SPO (registered trademark) manufactured by Sumitomo Chemical Co., Ltd.
[0095] The content of the ethylene-α-olefin copolymer (C) in the propylene-based resin composition is usually 1 mass% or more and 40 mass% or less, preferably 5 mass% or more and 35 mass% or less, and more preferably 5 mass% or more and 30 mass% or less, based on 100 mass% of the total amount of the propylene-based resin composition.
[0096] Inorganic Filler (D) The propylene-based resin composition according to this embodiment may further contain an inorganic filler (D) from the viewpoint of improving mechanical properties, dimensional stability, and the like.
[0097] Examples of the inorganic filler (D) include (i) a fibrous inorganic filler and (ii) a non-fibrous inorganic filler. In this embodiment, two or more types of inorganic fillers (D) may be used in combination. Specific examples are described below.
[0098] (i) Fibrous Inorganic Filler In the present embodiment, the fibrous inorganic filler preferably has an average fiber diameter of 0.2 μm to 20 μm, an average fiber length of 5 μm to 200 μm, and an aspect ratio of 10 to 30. From the viewpoint of improving the rigidity of the molded body and improving the appearance of the molded body, it is more preferable that the average fiber diameter is 0.3 μm to 10 μm, the average fiber length is 7 μm to 150 μm, and the aspect ratio is 12 to 25.
[0099] The average fiber diameter and average fiber length of the fibrous inorganic filler are, for example, the average values of the fiber diameter and fiber length measured by randomly selecting 50 or more fibers from an image of the fibrous inorganic filler obtained by an electron microscope, and the aspect ratio can be calculated using these average values.
[0100] Examples of fibrous inorganic fillers include fibrous magnesium oxysulfate, potassium titanate fiber, magnesium hydroxide fiber, aluminum borate fiber, calcium silicate fiber, calcium carbonate fiber, carbon fiber, glass fiber, and metal fiber. Of these, fibrous magnesium oxysulfate and calcium silicate fiber are preferred.
[0101] The fibrous inorganic filler can be used as it is. From the viewpoint of improving the interfacial adhesion and further improving the dispersibility, the fibrous inorganic filler may be further surface-treated with, for example, a silane coupling agent or a metal salt of a higher fatty acid before use.
[0102] Examples of higher fatty acid metal salts that can be used for the surface treatment include calcium stearate, magnesium stearate, and zinc stearate.
[0103] In this embodiment, examples of the form of the fibrous inorganic filler include powder, flake, and granule. In this embodiment, any of the above-mentioned forms of the fibrous inorganic filler may be used. Because of its good handleability, it is preferable to use a fibrous inorganic filler in the form of granules.
[0104] (ii) Non-fibrous inorganic filler Examples of non-fibrous inorganic fillers include talc, mica, calcium carbonate, barium sulfate, magnesium carbonate, clay, alumina, calcium sulfate, silica sand, carbon black, titanium oxide, magnesium hydroxide, molybdenum, diatomaceous earth, sericite, shirasu, calcium hydroxide, calcium sulfite, sodium sulfate, bentonite, graphite, etc. From the viewpoints of improving the impact strength and improving the appearance of the molded body, it is preferable to use talc.
[0105] The average particle size of the non-fibrous inorganic filler is preferably 15 μm or less, more preferably 10 μm or less. Here, the average particle size of the non-fibrous inorganic filler is determined based on volume-based particle size distribution measurement data measured by laser diffraction according to the method specified in JIS R1629, and means the particle size when the cumulative number of particles from the smallest particle size reaches 50% (50% equivalent particle size) in the particle size distribution measurement data. The particle size defined in this way is generally referred to as "50% equivalent particle size" and is expressed as "D50".
[0106] The non-fibrous inorganic filler can be used as it is. From the viewpoint of improving interfacial adhesion and dispersibility, the non-fibrous inorganic filler may be surface-treated with a silane coupling agent, a titanium coupling agent, or a surfactant before use.
[0107] Examples of surfactants that can be used for the surface treatment include higher fatty acids, higher fatty acid esters, higher fatty acid amides, and higher fatty acid salts.
[0108] The fibrous inorganic filler may be used as it is, or may be surface-treated with a silane coupling agent or a metal salt of a higher fatty acid in order to improve interfacial adhesion and dispersibility.
[0109] The content of the inorganic filler in the polyolefin-based resin composition is usually 1 part by mass or more and 40 parts by mass or less, preferably 5 parts by mass or more and 35 parts by mass or less, and more preferably 5 parts by mass or more and 30 parts by mass or less, when the total amount of the propylene-based resin composition is 100 parts by mass.
[0110] Other Additives (E) The propylene-based resin composition of the present embodiment may contain various other additives (E) as further optional components in addition to the components already described above.
[0111] Examples of such optional additives include antioxidants, neutralizing agents, ultraviolet absorbers, light stabilizers, lubricants, antistatic agents, colorants (e.g., inorganic pigments, organic pigments), flame retardants, elastomers, antiblocking agents, processing aids, organic peroxides, pigment dispersants, foaming agents, foam nucleating agents, plasticizers, crosslinking agents, crosslinking aids, brightness enhancers, antibacterial agents, light diffusing agents, and molecular weight modifiers.
[0112] The propylene-based resin composition of the present embodiment may contain one kind of these additives alone, or may contain two or more kinds of optional components in any combination at any ratio.
[0113] Among the additives (E), antioxidants, neutralizing agents, ultraviolet absorbers, light stabilizers, and colorants are preferably used. These will be described in detail below. The propylene-based resin composition of the present embodiment preferably includes, in addition to the above components, one or more selected from the group consisting of organic peroxides, neutralizing agents, antioxidants, ultraviolet absorbers, light stabilizers, and colorants.
[0114] The propylene-based resin composition may contain other additives such as resins and rubbers in addition to the additives already described.
[0115] Other additives include, for example, polystyrenes (e.g., polystyrene, poly(p-methylstyrene), poly(α-methylstyrene), AS (acrylonitrile / styrene copolymer) resin), ABS (acrylonitrile / butadiene / styrene copolymer) resin, AAS (special acrylic rubber / acrylonitrile / styrene copolymer) resin, ACS (acrylonitrile / chlorinated polyethylene / styrene copolymer) resin, polychloroprene, chlorinated rubber, polyvinyl chloride, polyvinylidene chloride, acrylic resin, ethylene / vinyl alcohol copolymer resin, fluororesin, polyacetal, grafted polyphenylene ether resin, and polyphenylene sulfide resin, Examples of suitable resins include thermoplastic resins such as polyurethane, polyamide, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate), polycarbonate, polysulfone, polyether ether ketone, polyether sulfone, and aromatic polyester resin; epoxy resin, diallyl phthalate prepolymer, silicone resin, silicone rubber, polybutadiene, 1,2-polybutadiene, polyisoprene, styrene / butadiene copolymer, butadiene / acrylonitrile copolymer, epichlorohydrin rubber, acrylic rubber, and natural rubber; and PLA resin (polylactic acid) produced by polymerizing plant-derived monomers extracted from biomaterials.
[0116] (Method for Producing Propylene-Based Resin Composition) The propylene-based resin composition of this embodiment can be produced by melt-kneading the components described above. The temperature during melt-kneading may be 180°C or higher, 180 to 300°C, or 180 to 250°C.
[0117] Examples of melt-kneading devices used in melt-kneading for producing the propylene-based resin composition of the present embodiment include any suitable conventionally known Banbury mixer, single-screw extruder, twin-screw co-rotating extruder, and twin-screw counter-rotating extruder.
[0118] Specific examples of the melt kneading apparatus include ZSK (registered trademark) manufactured by Coperion, TEM (registered trademark) manufactured by Toshiba Machine Co., Ltd., TEX (registered trademark) manufactured by The Japan Steel Works, Ltd., KZW (registered trademark) manufactured by Technovel Co., Ltd., CMP (registered trademark) and TEX (registered trademark) manufactured by The Japan Steel Works, Ltd., and FCM (registered trademark), NCM (registered trademark), and LCM (registered trademark) manufactured by Kobe Steel, Ltd.
[0119] The order of kneading the raw materials is not particularly limited. For example, all the raw materials may be kneaded by being charged into a production apparatus at once, or some of the selected components may be kneaded and then the resulting kneaded mixture may be kneaded with other components.
[0120] Alternatively, a propylene-based resin composition may be produced by melt-kneading an intermediate composition α containing at least two components with other raw materials. For example, an intermediate composition α containing a propylene-based polymer (A1) and di-tert-butylphenol may be melt-kneaded with a propylene-based polymer (A2) not containing di-tert-butylphenol. Here, the propylene-based polymer (A1) and the propylene-based polymer (A2) may be the same or different. The intermediate composition α may further contain at least one of an ethylene-α-olefin copolymer and an inorganic filler.
[0121] The intermediate composition α contains a propylene polymer (A) and di-tert-butylphenol, and the content of di-tert-butylphenol may be more than 1,800 ppm by mass when the total mass of the intermediate composition is 100 parts by mass. Such a material can be used as a masterbatch. Furthermore, at least one of the various components, such as the propylene polymer, ethylene-α-olefin copolymer, and inorganic filler, used as raw materials in the production of the propylene resin composition may be recycled.
[0122] The properties of the propylene-based resin composition of this embodiment are not particularly limited. The propylene-based resin composition of this embodiment can be in the form of, for example, a strand (filament), a sheet, a plate, or a pellet. The pellet shape can be produced, for example, by preparing a strand-shaped propylene-based resin composition and then cutting it to an appropriate length.
[0123] (Molded Article) The present invention also relates to a molded article obtained by molding the propylene-based resin composition. That is, the propylene-based resin composition of this embodiment can be suitably used as a material for forming a molded article. The molded article can be obtained by molding the propylene-based resin composition by various molding methods. The shape, size, etc. of the molded article may be determined appropriately.
[0124] The propylene-based resin composition of the present embodiment can be used as a material for molded articles such as automotive materials, home appliance materials, monitor materials, office equipment materials, medical materials, drain pans, toiletry materials, food packaging containers, bottles, containers, sheets, films, etc. The propylene-based resin composition of the present embodiment is difficult to be charged and can suppress, for example, the adhesion of dust and the like, and therefore can be preferably applied to materials for vehicle-related members, home appliance materials, and food packaging containers such as retort pouches and pouches that can be heated in a microwave oven.
[0125] The propylene-based resin composition of the present embodiment is particularly preferably used as a material for injection molding.
[0126] An example of using the propylene-based resin composition of this embodiment as an injection molding material to produce an injection-molded article will be described below.
[0127] The injection-molded article is an article molded from the propylene-based resin composition of the present embodiment. Injection-molded articles generally have excellent dimensional stability.
[0128] The injection-molded article can be produced by any suitable conventional injection molding method, such as injection foam molding, supercritical injection foam molding, ultra-high speed injection molding, injection compression molding, gas-assisted injection molding, sandwich molding, sandwich foam molding, and insert-outsert molding.
[0129] The molded article (injection molded article) of this embodiment can be produced by the above method in any suitable shape and dimensions depending on the application.
[0130] Examples of material applications for vehicle-related members that are injection molded articles include interior parts such as door trims, pillars, instrument panels, consoles, rocker panels, armrests, door panels, and spare tire covers; exterior parts such as bumpers, spoilers, fenders, and side steps; and other parts such as air intake ducts, coolant reserve tanks, fender liners, fans, and under-deflectors, as well as integrally molded parts such as front end panels.
[0131] Examples of home appliance materials include materials for washing machines (outer tubs, inner tubs, lids, pulsators, balancers, etc.), materials for dryers, materials for vacuum cleaners, materials for rice cookers, materials for pots, materials for warmers, materials for dishwashers, and materials for air purifiers.
[0132] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0133] In the examples and comparative examples, the following raw materials were used.
[0134] Propylene-Based Polymer (A) The following heterophasic propylene polymer material was prepared as the propylene-based polymer (A).
[0135] Heteropharmacologically stable propylene polymer material (A-1) was produced by gas phase polymerization in the presence of a polymerization catalyst obtained by the method described in Example 1 of JP-A-2004-182981. The physical properties of the obtained polymer material are as follows:
[0136] Melt flow rate (MFR) (230°C, 2.16 kgf): 32.4 g / 10 min Polymer (I): Propylene homopolymer component (P part) Intrinsic viscosity: 1.00 dL / g Polymer (II): Propylene-ethylene random copolymer component (EP part) Intrinsic viscosity: 5.0 dL / g Amount of propylene-ethylene random copolymer component: 16 wt% Content of structural units derived from ethylene in polymer (II) (content of monomer units derived from ethylene based on the total weight of polymer (II)): 43.0 wt%
[0137] Content of structural units derived from ethylene in polymer (II) The content of structural units derived from ethylene in polymer (II) was determined from a 13C-NMR spectrum measured under the following conditions, based on the report by Kakugo et al. (Macromolecules, 15, 1150-1152 (1982)). The 13C-NMR spectrum was measured under the following conditions using a sample prepared by uniformly dissolving about 200 mg of heterophasic propylene polymerization material in 3 mL of ortho-dichlorobenzene in a test tube with a diameter of 10 mm. Measurement temperature: 135°C Pulse repetition time: 10 seconds Pulse width: 45° Number of accumulations: 2500
[0138] Intrinsic viscosity (unit: dL / g) The intrinsic viscosity is a value measured at a temperature of 135°C using tetralin as a solvent by the following method.
[0139] Using an Ubbelohde viscometer, the reduced viscosity is measured at three concentrations: 0.1 g / dL, 0.2 g / dL, and 0.5 g / dL. The reduced viscosity is plotted against the concentration, and the intrinsic viscosity is calculated by extrapolation, where the concentration is extrapolated to zero. The method for calculating the intrinsic viscosity by extrapolation is described, for example, on page 491 of "Polymer Solutions, Polymer Experiments 11" (published by Kyoritsu Shuppan Co., Ltd. in 1982).
[0140] Di-tert-butylphenol (B) 2,4-di-tert-butylphenol (B-1) manufactured by Kanto Chemical Co., Inc. was prepared.
[0141] Di-tert-butylphenol (B) 2,6-di-tert-butylphenol (B-2) manufactured by Kanto Chemical Co., Inc. was prepared.
[0142] Ethylene-α-olefin copolymer (C) The following ethylene-1-octene random copolymer (C-1) was prepared: "EG8200" manufactured by The Dow Chemical Company, density: 0.870 g / cm 3 MFR (measured at 190°C and 2.16 kgf load): 5.0 g / 10 min
[0143] Inorganic filler (D) The following inorganic filler was prepared: Talc (D-1) "MW UPN TT-H" manufactured by Hayashi Kasei Average particle diameter D50 [L] (laser diffraction method, 50% equivalent particle diameter): 4.90 μm
[0144] Here, the average particle diameter D50 [L] of talc was measured using a Microtrac particle size analyzer MT-3300EXII manufactured by Nikkiso Co., Ltd., after dispersing the particles under the following conditions according to the method specified in JIS R1629.
[0145] Dispersion treatment of particles Dispersion medium: Ethanol Equipment: Homogenizer Output: 40 W Treatment time: 10 minutes
[0146] Additive (E) The following additives (F-1), (F-2) and (F-3) were prepared.
[0147] Additive (F-1) "Calcium stearate" manufactured by Sakai Chemical Industry Co., Ltd.
[0148] Additive (F-2) "IRGAFOS168" manufactured by BASF (phosphorus-based antioxidant)
[0149] Additive (F-3) BASF IRGANOX 1010 (phenolic antioxidant)
[0150] (Examples A1 to A7, Comparative Examples A1 to A3, Examples B1 to B3) Production of Propylene-Based Resin Compositions Raw materials having the compositions shown in Tables 1 to 3 were melt-kneaded using a twin-screw kneader KZW-15 / 45MG (cylinder inner diameter 15.5 mm, screw outer diameter 15.0 mm, L / D=45) manufactured by Technovel Corporation to obtain pellet-shaped propylene-based resin compositions.
[0151] The melt-kneading conditions were a cylinder temperature of 200°C, a screw rotation speed of 500 rpm, two screen meshes of 100 mesh and 50 mesh stacked together, and an extrusion rate of 6 kg / hr. The evaluation results are shown in Tables 1 to 3.
[0152] Manufacture of injection-molded articles for evaluating volume resistivity The pellet-shaped propylene-based resin composition obtained by the above method was dried at 100°C for 1 hour and then injection-molded under the following conditions to manufacture a plate-shaped molded article measuring 150 mm in length, 90 mm in width, and 3.0 mm in thickness: Injection molding machine: SE130DU manufactured by Sumitomo Heavy Industries, Ltd. (clamping force 130 tons, cylinder diameter 40 mm) Cylinder temperature: 220°C Mold temperature: 50°C Injection speed: 20 mm / sec Cooling time: 30 sec
[0153] Measurement of volume resistivity (unit: Ω cm) One of the obtained flat-plate-like molded articles was placed on a large-diameter electrode for flat-plate-like molded articles (SME-8310, manufactured by DKK-TOA Corporation) in accordance with JIS-K6911, and a voltage of 500 V was applied. The resistance value after 1 minute was measured using a digital insulation meter (DSM-8103, manufactured by DKK-TOA Corporation), and the volume resistivity value was calculated based on this value. The smaller the volume resistivity value, the better the antistatic property.
[0154]
[0155]
[0156]
Claims
1. A propylene-based resin composition containing a propylene polymer and di-tert-butylphenol, wherein the content of di-tert-butylphenol is 10 to 1,800 ppm by mass when the total mass of the propylene-based resin composition is 100 parts by mass.
2. The propylene-based resin composition according to claim 1, wherein the content of the propylene-based polymer is 50 parts by mass or more when the total mass of the propylene-based resin composition is 100 parts by mass.
3. The propylene-based resin composition according to claim 1 or 2, further comprising an ethylene-α-olefin copolymer.
4. The propylene-based resin composition according to claim 3, wherein the content of the ethylene-α-olefin copolymer is 1 to 40 parts by mass per 100 parts by mass of the propylene-based resin composition.
5. The propylene-based resin composition according to any one of claims 1 to 4, further comprising an inorganic filler.
6. The propylene-based resin composition according to claim 5, wherein the content of the inorganic filler is 1 to 40 parts by mass when the total mass of the propylene-based resin composition is 100 parts by mass.
7. The propylene-based resin composition according to any one of claims 1 to 6, further comprising an ethylene-α-olefin copolymer and an inorganic filler.
8. The propylene resin composition according to any one of claims 1 to 7, wherein the di-tert-butylphenol is 2,4-di-tert-butylphenol.
9. The propylene-based resin composition according to claim 8, wherein the content of 2,4-di-tert-butylphenol is 10 to 1,200 ppm by mass when the total mass of the propylene-based resin composition is 100 parts by mass.
10. The propylene-based resin composition according to any one of claims 1 to 9, further comprising at least one member selected from the group consisting of organic peroxides, neutralizing agents, antioxidants, ultraviolet absorbers, light stabilizers and colorants.
11. A molded article comprising the propylene-based resin composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Drying method and apparatus for polyolefin
JP1980075410A
Ethylene-propylene block copolymer
JP1993194685A
Catalyst for polymerizing alpha-olefin and production of alpha-olefin polymer
JP1995216017A
Propylene / ethylene-alpha-olefin block copolymer and its production
JP1997316147A
Alpha-olefin polymerization catalyst and production of alpha-olefin polymer
JP1998212319A
Cited By
Composition comprising a phosphorous-containing methacrylate and 2,4-di(tert-butyl)-phenol
WO2026131571A1