Separator for electrochemical device having polymer binder layer, electrochemical device comprising same, and method for manufacturing same

The separator for electrochemical devices addresses adhesion and dispersibility issues by using a combination of polymer binders in the coating and adhesive layers, resulting in enhanced mechanical properties and reduced defects, thereby improving the performance and safety of the device.

WO2024248277A1PCT designated stage expired Publication Date: 2024-12-05LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/002772
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-03-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing separators for electrochemical devices face challenges in maintaining strong adhesion between the porous polymer substrate and the coating layer while ensuring the dispersibility of inorganic particles, which affects the mechanical properties and safety of the battery.

Method used

A separator design is implemented with a coating layer containing a first polymer binder and inorganic particles on a porous polymer substrate, and an adhesive layer with a second polymer binder, where the first binder is in solution form and the second binder is in particle form, optimizing the binder content and solubility to enhance adhesion and dispersibility.

Benefits of technology

This design improves the adhesion between the coating layer and the porous polymer substrate, enhances the mechanical properties of the separator, and reduces defects during manufacturing, leading to improved performance and safety of the electrochemical device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024002772_05122024_PF_FP_ABST
    Figure KR2024002772_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The separator for an electrochemical device includes: a porous polymer substrate; a coating layer which is provided on at least one surface of the porous polymer substrate and includes a first polymer binder and inorganic particles; and an adhesive layer which is provided on the coating layer and includes a second polymer binder, wherein the first polymer binder is in a solution form and, within the coating layer, one portion adjacent to the porous polymer substrate contains greater amount of the first polymer binder than the other portion spaced apart from and facing the porous polymer substrate.
Need to check novelty before this filing date? Find Prior Art

Description

A separator for an electrochemical device having a polymer binder layer, an electrochemical device including the same, and a method for manufacturing the same

[0001] This invention claims the benefit of Korean Patent Application No. 10-2023-0068198, filed with the Korean Intellectual Property Office on May 26, 2023, the entire contents of which are incorporated herein by reference. The present invention relates to a separator for an electrochemical device, an electrochemical device comprising the same, and a method for manufacturing the same, and to electrodes, separators, and secondary batteries manufactured using the same.

[0002] Among the components of electrochemical devices, the separator is a polymer substrate with a porous structure located between the anode and cathode, which isolates the anode and cathode, prevents electrical short-circuiting between the two electrodes, and allows electrolytes and ions to pass through.

[0003] Meanwhile, to improve the performance and safety of secondary batteries employing electrochemical devices, improvements are being made to the characteristics of each of the positive electrode, negative electrode, electrolyte, and separator.

[0004] The present invention provides a separator for an electrochemical device, an electrochemical device including the same, and a method for manufacturing the same, wherein a polymer binder included in a slurry for an adhesive layer is positioned at the interface between the coating layer and the porous polymer substrate to improve the adhesive strength between the coating layer and the porous polymer substrate, and improves the dispersibility of inorganic particles included in the slurry for the coating layer.

[0005] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.

[0006] According to one embodiment of the present invention, a separator for an electrochemical device is provided, comprising: a porous polymer substrate; a coating layer provided on at least one surface of the porous polymer substrate and including a first polymer binder and inorganic particles; and an adhesive layer provided on the coating layer and including a second polymer binder, wherein the first polymer binder is in solution form, and the content of the first polymer binder included in a portion of the coating layer adjacent to the porous polymer substrate is greater than the content of the first polymer binder included in another portion spaced apart from the porous polymer substrate.

[0007] According to one embodiment of the present invention, the solubility of the second polymer binder in water is less than the solubility of the first polymer binder in water.

[0008] According to one embodiment of the present invention, the first polymer binder is selected from the group consisting of polyacrylic acid, polyurethane, polyacrylonitrile, polyethylene glycol, polyacrylamide, polyvinyl alcohol, and combinations thereof.

[0009] According to one embodiment of the present invention, the second polymer binder is in particle form.

[0010] One embodiment of the present invention provides a method for manufacturing a separator for an electrochemical device, comprising: a step of applying a slurry for a coating layer comprising a first polymer binder and inorganic particles to at least one surface of a porous polymer substrate to form a coating layer; and a step of applying a slurry for an adhesive layer comprising a first polymer binder and a second polymer binder on the coating layer to form an adhesive layer, wherein the first polymer binder is in a solution form, and the solubility of the second polymer binder in water is lower than the solubility of the first polymer binder in water.

[0011] According to one embodiment of the present invention, the step of providing the coating layer and the step of providing the adhesive layer further include a drying step.

[0012] According to one embodiment of the present invention, the content of the first polymer binder dissolved in the solvent in the slurry for the coating layer is about 0.1 wt% or more and 10 wt% or less.

[0013] According to one embodiment of the present invention, the content of the second polymer binder dissolved in the solvent in the slurry for the adhesive layer is about 5 wt% or more and 40 wt% or less.

[0014] According to one embodiment of the present invention, the average particle diameter (D) of the particles included in the slurry for the coating layer 90 ) is approximately 0.01 ㎛ or more and 10.0 ㎛ or less.

[0015] One embodiment of the present invention provides an electrochemical device comprising: a positive electrode; a negative electrode; and a separator for an electrochemical device interposed between the positive electrode and the negative electrode, wherein the adhesive force between the porous polymer substrate and the coating layer is about 30 gf / 25 mm or more.

[0016] According to one embodiment of the present invention, the adhesive force between the porous polymer substrate and the coating layer is greater than the adhesive force between either the positive electrode or the negative electrode and the adhesive layer by about 5 gf / 25 mm or more.

[0017] One embodiment of the present invention provides an electrochemical device comprising: a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode, the separator comprising: a porous polymer substrate; a coating layer provided on at least one surface of the porous polymer substrate and including a first polymer binder and inorganic particles; and an adhesive layer provided on the coating layer and including a second polymer binder, wherein the second polymer binder is in solution form, and an adhesive force between the porous polymer substrate and the coating layer is greater than an adhesive force between either the positive electrode or the negative electrode and the adhesive layer.

[0018] A separator for an electrochemical device according to one embodiment of the present invention improves the adhesion between a coating layer and a porous polymer substrate.

[0019] A method for manufacturing an electrochemical device according to one embodiment of the present invention maintains the viscosity of a slurry for a coating layer low, thereby improving the dispersibility of inorganic particles and a polymer binder.

[0020] An electrochemical device according to one embodiment of the present invention improves the adhesion between a coating layer and a porous polymer substrate, and improves the adhesion between the separator and an electrode.

[0021] Figure 1 is a schematic diagram of a separator for an electrochemical device according to one embodiment of the present invention.

[0022] Figure 2 is a flowchart of a method for manufacturing a separator for an electrochemical device according to one embodiment of the present invention.

[0023] Figure 3 is a schematic diagram of an electrochemical device according to one embodiment of the present invention.

[0024] In some of the accompanying drawings, corresponding components are designated by the same reference numerals. Those skilled in the art will appreciate that the drawings illustrate elements simply and clearly and are not necessarily drawn to scale. For example, to facilitate understanding of various embodiments, the dimensions of some elements depicted in the drawings may be exaggerated relative to other elements. Furthermore, elements of known technology that are useful or essential in commercially feasible embodiments may often not be depicted so as not to obscure the spirit of various embodiments of the present invention.

[0025] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.

[0026] The terminology used herein is for the purpose of describing embodiments only and is not intended to limit the present invention, and the singular forms herein also include the plural forms unless specifically stated otherwise in the text.

[0027] In this specification, “A and / or B” means “A and B, or A or B.”

[0028] In this specification, when it is said that a component is “provided on”, this does not exclude other components being placed in between, unless otherwise specifically stated, but rather means that other components may be placed thereon.

[0029] In this specification, “%” means weight percent unless explicitly indicated otherwise.

[0030] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values ​​provided to aid understanding of the present invention.

[0031] In this specification, the characteristic of “having pores” means that the object includes a plurality of pores and that the pores are interconnected with each other, thereby allowing gaseous and / or liquid fluids to pass from one side of the object to the other side.

[0032] In this specification, the separator has a porous characteristic including a large number of pores, and acts as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the cathode and the anode in an electrochemical device.

[0033] Although the separator itself does not participate in the electrochemical reaction, its physical properties, such as wettability to the electrolyte, degree of porosity, and thermal shrinkage, affect the performance and safety of the electrochemical device.

[0034] Accordingly, in order to enhance the physical properties of the separator, a coating layer is added to a porous polymer substrate, and as an example of various methods for changing the properties of the coating layer by adding various substances to the coating layer, an inorganic substance is added to the coating layer to enhance the mechanical strength of the separator, or an inorganic substance or a hydrate is added to the coating layer to enhance the flame retardancy and heat resistance of the polymer substrate.

[0035] The separator can be bonded to the electrode through a lamination process, and a polymer binder is added to the coating layer composition of the separator to secure adhesion between the electrode and the separator.

[0036] Meanwhile, when bonding electrodes and separators in the battery manufacturing process, battery manufacturing becomes easier, battery thickness is uniformly implemented, and battery stiffness is improved, so a multilayer separator technology that forms a first coating layer and a second coating layer on the separator is being developed. The adhesive strength between the electrode and the separator is affected by the adhesion between the adhesive binder and the electrode, the adhesion between the adhesive binder and the inorganic coating layer, and the adhesion between the inorganic coating layer and the porous substrate. In the manufacturing process of a multilayer separator, if the solvent used for the first coating layer and the second coating layer is the same, there is a problem that the adhesive strength between the first coating layer and the porous polymer substrate is weakened during the manufacturing process of the second coating layer. In order to solve this problem, a solution-type binder is added to the slurry for manufacturing the first coating layer to improve the adhesive strength between the porous polymer substrate and the first coating layer, but the slurry for manufacturing the first coating layer has a problem in that the viscosity is increased due to the solution-type binder, resulting in poor dispersibility.

[0037] In order to prevent such problems, the present invention provides a separation membrane that can improve the adhesion between a porous polymer substrate and a coating layer while preventing a decrease in the dispersibility of an inorganic substance included in the coating layer.

[0038]

[0039] Hereinafter, the present invention will be described in more detail.

[0040] FIG. 1 is a schematic diagram of a separator (100) for an electrochemical device according to one embodiment of the present invention. Referring to FIG. 1, a separator (100) for an electrochemical device according to one embodiment of the present invention will be described.

[0041] One embodiment of the present invention provides an electrochemical device separator (100) comprising: a porous polymer substrate (110); a coating layer (130) provided on at least one surface of the porous polymer substrate (110) and including a first polymer binder (131) and inorganic particles (133); and an adhesive layer (150) provided on the coating layer (130) and including a second polymer binder (151), wherein the first polymer binder (131) is in a solution form, and the content of the first polymer binder (131) included in a portion of the coating layer (130) adjacent to the porous polymer substrate (110) is greater than the content of the first polymer binder (131) included in another portion spaced apart from the porous polymer substrate (110).

[0042] A separator (100) for an electrochemical device according to one embodiment of the present invention improves the adhesive strength between a coating layer (130) and a porous polymer substrate (110).

[0043] According to one embodiment of the present invention, the separator (100) for an electrochemical device includes a porous polymer substrate (110). As described above, the separator (100) for an electrochemical device includes the porous polymer substrate (110), thereby allowing lithium ions to pass through while blocking electrical contact, and implementing a shutdown function at an appropriate temperature.

[0044] According to one embodiment of the present invention, the porous polymer substrate (110) is manufactured using a polyolefin resin as a base resin. Examples of polyolefin-based resins include polyethylene, polypropylene, polypentene, and the like, and the porous membrane includes at least one of these. The porous membrane, i.e., the membrane having a large number of pores, manufactured using the polyolefin resin as a base resin provides a shutdown function at an appropriate temperature.

[0045] According to one embodiment of the present invention, the weight average molecular weight of the polyolefin resin is about 500,000 to 1.5 million. By controlling the weight average molecular weight of the polyolefin resin within the above-described range, the compression resistance of the separator is improved. Furthermore, when different types of polyolefin resins are mixed and used or the separator is formed with a multilayer structure of different types of polyolefin resins, the weight average molecular weight of the polyolefin resin is calculated by adding the weight average molecular weight according to the content ratio of each polyolefin resin.

[0046] In this specification, “weight average molecular weight (Mw)” is measured by gel permeation chromatography (GPC: gel permeation chromatography, PL GPC220, Agilent Technologies), and the measurement conditions are as follows.

[0047] - Column: PL Olexis (Polymer Laboratories)

[0048] - Solvent: TCB (Trichlorobenzene)

[0049] - Flow rate: 1.0 ml / min

[0050] - Sample concentration: 1.0 mg / ml

[0051] - Injection volume: 200 ㎕

[0052] - Column temperature: 160 ℃

[0053] - Detector: Agilent High Temperature RI detector

[0054] - Standard: Polystyrene (corrected with a cubic function)

[0055] According to one embodiment of the present invention, the porous polymer substrate (110) is manufactured by a method (wet method) in which a polyolefin resin is mixed with a plasticizer at a high temperature to form a single phase, the polymer material and the plasticizer are phase-separated during a cooling process, the plasticizer is extracted to form pores, and then stretching and heat-setting are performed. In addition, the porous polymer substrate using the polyolefin resin has a core portion made of a mixture of polyethylene and polypropylene and a polyethylene skin portion laminated on both sides of the core portion.

[0056] According to one embodiment of the present invention, the average size of the pores and the maximum size of the pores of the separation membrane (100) can be easily manufactured by a person skilled in the art by controlling the mixing ratio of the plasticizer, the stretching ratio, the heat-setting treatment temperature, etc. to conform to the scope of the present invention.

[0057] According to one embodiment of the present invention, the electrochemical device separator (100) includes a coating layer (130) provided on at least one surface of the porous polymer substrate (110). As described above, the electrochemical device separator (100) includes the coating layer (130) provided on at least one surface of the porous polymer substrate (110), thereby improving the heat resistance of the separator, improving the mechanical properties, and preventing the separator from shrinking at high temperatures and causing an electrical short circuit of the electrode.

[0058] According to one embodiment of the present invention, the coating layer (130) includes a first polymer binder (131) and inorganic particles (133). As described above, since the coating layer (130) includes the first polymer binder (131) and the inorganic particles (133), the heat resistance of the separator is improved, the mechanical properties are improved, the shrinkage of the separator at high temperatures is prevented, resulting in an electrical short circuit of the electrode, pores are formed inside the coating layer, and the adhesive force between the porous polymer substrate and the coating layer is improved.

[0059] In one embodiment of the present invention, the adhesive strength between the porous polymer substrate and the coating layer refers to the binding strength of the porous polymer substrate and the coating layer. For example, the adhesive strength between the porous polymer substrate and the coating layer is measured by measuring the peel strength when the separator and the adhesive tape are attached and then removed using a UTM (Universal Testing Machine). Alternatively, a separator specimen prepared by cutting it to 70 mm (length) x 25 mm (width) is attached and fixed to a glass plate using double-sided tape, and then the separator portion of the specimen is peeled at an angle of 180° at a speed of 150 mm / min at 25°C, and the strength at this time is measured.

[0060] According to one embodiment of the present invention, the coating layer (130) includes a plurality of pores. For example, the coating layer (130) is a porous coating layer. Alternatively, the coating layer (130) is a porous coating layer including a plurality of pores therein. As described above, by including a plurality of pores, the coating layer (130) physically blocks contact between the negative electrode and the positive electrode, while allowing lithium ions to pass through and current to flow.

[0061] According to one embodiment of the present invention, the coating layer (130) is formed by binding and integrating inorganic particles (133) by a first polymer binder (131). The pores within the coating layer (130) originate from the interstitial volume, which is the empty space between the inorganic particles.

[0062] According to one embodiment of the present invention, the first polymer binder (131) is in solution form. For example, the first polymer binder (131) is dissolved in a solvent and provided in the pores of the coating layer. For example, the first polymer binder (131) is dissolved in a solvent included in a slurry for a coating layer and / or a slurry for an adhesive layer, which will be described later, and provided in the pores of the coating layer. By selecting the first polymer binder (131) as being in solution form as described above, the adhesive strength between the porous polymer substrate and the coating layer is improved.

[0063] In one embodiment of the present invention, “solution type” means that 50 wt% or more of the substance to be dissolved is dissolved in 100 g of a solvent under room temperature (20°C) and 1 atm pressure conditions based on 100 wt% of the substance to be dissolved.

[0064] According to one embodiment of the present invention, the thickness of the coating layer (130) is formed to a thickness of about 1 μm to 20 μm on either side of the porous polymer substrate (110), but is not particularly limited thereto. The thickness can be adjusted to an appropriate range by those skilled in the art in terms of heat resistance or electrical resistance.

[0065] In one embodiment of the present invention, the thickness of the porous polymer substrate, the coating layer, and / or the adhesive layer described below is measured using a contact thickness measuring device. The contact thickness measuring device is, for example, VL-50S-B from Mitutoyo.

[0066] According to one embodiment of the present invention, the adhesive layer (150) is provided on the coating layer (130). As described above, by providing the adhesive layer (150) on the coating layer (130), the adhesive force between the electrode and the separator is improved, while at the same time improving the heat resistance of the separator.

[0067] According to one embodiment of the present invention, the adhesive layer (150) includes a second polymer binder (151). As described above, by including the second polymer binder (151) in the adhesive layer (150), the uniformity of the inorganic particles of the coating layer is improved, thereby increasing the thickness uniformity of the separator, and improving the adhesion of the separator to the electrode.

[0068] According to one embodiment of the present invention, the content of the first polymer binder (131) included in a portion adjacent to the porous polymer substrate (110) in the coating layer (130) is greater than the content of the first polymer binder (131) included in another portion spaced apart from the porous polymer substrate (110). As described above, by implementing that the content of the first polymer binder (131) included in a portion adjacent to the porous polymer substrate (110) in the coating layer (130) is greater than the content of the first polymer binder (131) included in another portion spaced apart from the porous polymer substrate (110), the first polymer binder (131) is excessively disposed in a portion adjacent to the porous polymer substrate (110) in the coating layer (130), thereby improving the adhesion between the coating layer (130) and the porous polymer substrate (110). Furthermore, by implementing the content of the first polymer binder (131) in the slurry for the coating layer described below to be relatively low, the increase in viscosity of the slurry for the coating layer can be suppressed, thereby implementing a low particle size, thereby improving the dispersibility of the inorganic particles (133) in the slurry for the coating layer.

[0069] According to one embodiment of the present invention, the solubility of the second polymer binder (151) in water is lower than the solubility of the first polymer binder (131) in water. As described above, by implementing the solubility of the second polymer binder (151) in water to be lower than the solubility of the first polymer binder (131), the second polymer binder (151) is not dissolved by the solvent of the slurry for the adhesive layer, so that the second polymer binder (151) exists in the adhesive layer (150) and improves the adhesive strength of the adhesive layer (150) with the electrode.

[0070] According to one embodiment of the present invention, the first polymer binder (131) is one selected from the group consisting of polyacrylic acid, polyurethane, polyacrylonitrile, polyethylene glycol, polyacrylamide, polyvinyl alcohol, and combinations thereof. As described above, by selecting the first polymer binder (131) as one selected from the group consisting of polyacrylic acid, polyurethane, polyacrylonitrile, polyethylene glycol, polyacrylamide, polyvinyl alcohol, and combinations thereof, the binding force of the inorganic particles (133) within the coating layer (130) is improved, and the adhesive force between the coating layer and the porous polymer substrate (110) is improved.

[0071] According to one embodiment of the present invention, the second polymer binder (151) is in solution form. For example, the second polymer binder (151) is dissolved in a solvent and provided in the pores of the coating layer (131) and / or the porous polymer substrate (110).

[0072] Alternatively, the second polymer binder (151) is dissolved in a solvent included in the slurry for the adhesive layer described below and is provided in the pores of the coating layer (130) and / or the porous polymer substrate (110). As described above, by selecting the second polymer binder (151) as being in solution form, the first polymer binder (131) improves the adhesive strength between the porous polymer substrate (110) and the coating layer (130) while selecting either the solution form or the particle form.

[0073] According to one embodiment of the present invention, the second polymer binder (151) is in particle form. By selecting the second polymer binder (151) as being in particle form as described above, the uniformity of the inorganic particles of the coating layer is improved, and the adhesive strength between the separator and the electrode is improved.

[0074] According to one embodiment of the present invention, the second polymer binder (151) is an acrylic binder, a polyvinylidene binder, or a combination thereof. By selecting the second polymer binder from the above-described ones, the adhesive strength between the electrode and the separator can be improved during the lamination process of the battery, facilitating the manufacture of the battery, and stably implementing the stacking process.

[0075] According to one embodiment of the present invention, the acrylic binder is a polymer containing a carboxylic acid ester as a repeating unit, for example, a (meth)acrylic acid ester or an acrylic-styrene copolymer.

[0076] According to one embodiment of the present invention, examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, n-amyl (meth)acrylate, i-amyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, ethylene glycol (meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, Examples thereof include trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl (meth)acrylate, and ethylene di(meth)acrylate, and at least one selected from these. Among these, at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate may be used, or methyl (meth)acrylate may be used.

[0077] According to one embodiment of the present invention, the acrylic-styrene copolymer includes an acrylic binder, and the acrylic binder is a polyacrylate. For example, the acrylic binder is at least one selected from the group consisting of styrenebutadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, and acrylate polymers, and more specifically, is a copolymer including acrylate.

[0078] According to one embodiment of the present invention, the polyvinylidene-based binder is a copolymer of polyvinylidene fluoride (PVdF) and hexafluoropropylene (HFP). By selecting a polyvinylidene-based binder as described above, the porosity of the separator can be maintained, and even if the coating layer is wetted by an electrolyte after activation of the battery, the adhesive strength can be maintained. Furthermore, the stiffness of the battery can be improved, and bending of the separator can be prevented.

[0079] According to one embodiment of the present invention, the polyvinylidene-based binder is a polyvinylidene-based binder having a hexafluoropropylene (HFP) content of about 1 wt% or more and 50 wt% or less. For example, the hexafluoropropylene (HFP) content in the polyvinylidene-based binder is about 1 wt% or more and 50 wt% or less, about 2 wt% or more and 45 wt% or less, about 3 wt% or more and 40 wt% or less, about 4 wt% or more and 35 wt% or less, about 5 wt% or more and 30 wt% or less, about 7 wt% or more and 25 wt% or less, or about 10 wt% or more and 20 wt% or less. As described above, by selecting a polyvinylidene-based binder having a content of hexafluoropropylene of about 1 wt% or more and 50 wt% or less, the porosity of the separator can be maintained, and the adhesive strength can be maintained even when the coating layer is wetted by the electrolyte after activation of the battery. In one embodiment of the present invention, the degree of substitution of the polyvinylidene-based binder means the weight ratio in which hexafluoropropylene is included.

[0080]

[0081] According to one embodiment of the present invention, the content of the first polymer binder (131) in the coating layer is about 25 parts by weight or less with respect to 100 parts by weight of the coating layer (130). For example, the total content of the first polymer binder (131) is about 0 to 25 parts by weight, about 1 to 24 parts by weight, about 2 to 23 parts by weight, about 3 to 22 parts by weight, about 4 to 21 parts by weight, about 5 to 20 parts by weight, about 6 to 19 parts by weight, about 7 to 18 parts by weight, about 8 to 17 parts by weight, about 9 to 16 parts by weight, about 10 to 15 parts by weight, about 11 to 14 parts by weight, or about 12 to 13 parts by weight, based on 100 parts by weight of the coating layer (130). By controlling the content of the first polymer binder (131) within the above-described range, the ease of assembly is improved in the process of assembling the electrode.

[0082] According to one embodiment of the present invention, the content of the inorganic particles (133) is greater than about 75 parts by weight with respect to 100 parts by weight of the coating layer (130). For example, the content of the inorganic particles (133) is about 75 parts by weight to less than 100 parts by weight, about 76 parts by weight to 99 parts by weight, about 77 parts by weight to 98 parts by weight, about 78 parts by weight to 97 parts by weight, about 79 parts by weight to 96 parts by weight, about 80 parts by weight to 95 parts by weight, about 81 parts by weight to 94 parts by weight, about 82 parts by weight to 93 parts by weight, about 83 parts by weight to 92 parts by weight, about 84 parts by weight to 91 parts by weight, about 85 parts by weight to 90 parts by weight, about 86 parts by weight to 89 parts by weight, or about 87 parts by weight to 88 parts by weight, based on 100 parts by weight of the coating layer (130). By controlling the content of the inorganic particles (133) within the above-described range, the heat resistance of the separator is improved.

[0083] According to one embodiment of the present invention, the inorganic particles (133) that can be used in the coating layer (130) are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in one embodiment of the present invention are those that can be used in the operating voltage range of the applied electrochemical device (e.g., Li / Li). + There are no particular limitations as long as no oxidation and / or reduction reaction occurs at a voltage of about 0 V to 5 V as a reference.

[0084] According to one embodiment of the present invention, non-limiting examples of the inorganic particles (133) include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3)O3-PbTiO3(PMN-PT), hafnia(HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), etc., and one or more of these are included.

[0085] According to one embodiment of the present invention, the average diameter (D) of the inorganic particles (133) 50 ) has no special limitations, but in order to form a coating layer (130) of uniform thickness and have an appropriate porosity, it is preferably in the range of about 0.3 ㎛ or more and 1 ㎛ or less. For example, when it is less than about 0.3 ㎛, the dispersibility of inorganic particles in the slurry prepared for manufacturing the coating layer is reduced, and when it exceeds about 1 ㎛, the surface of the formed coating layer becomes uneven or the thickness of the coating layer increases.

[0086] In one embodiment of the present invention, "D 50 "Particle size" means the particle size at the 50% point of the cumulative distribution of the number of particles according to the particle size. The particle size is measured using the laser diffraction method. For example, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the particle size distribution is calculated by measuring the difference in the diffraction pattern according to the particle size when the particles pass through the laser beam. By calculating the particle diameter at the point where the cumulative distribution of the number of particles according to the particle size in the measuring device becomes 50%, D 50 Measure the mouth diameter.

[0087] According to one embodiment of the present invention, the porosity of the coating layer (130) may be about 30% by volume or more. For example, the porosity of the coating layer (130) may be about 30% by volume or more and 70% by volume or less, about 32% by volume or more and 68% by volume or less, about 34% by volume or more and 66% by volume or less, about 36% by volume or more and 64% by volume or less, about 38% by volume or more and 62% by volume or less, about 40% by volume or more and 60% by volume or less, about 42% by volume or more and 58% by volume or less, about 44% by volume or more and 56% by volume or less, about 46% by volume or more and 54% by volume or about 48% by volume or more and 52% by volume. By controlling the porosity of the coating layer (130) within the above-described range, it is possible to maintain the movement of ions in the separator and prevent an increase in resistance of the separator. For example, if the porosity is less than about 70% by volume, it can secure mechanical properties that can withstand the pressing process for bonding with the electrode, and also, since the surface opening ratio is not too high, it is suitable for securing adhesive strength. On the other hand, if the porosity is more than about 30% by volume, it is advantageous from the perspective of ion permeability.

[0088] In one embodiment of the present invention, the “porosity” means the ratio of the volume occupied by pores to the total volume, and uses volume % as its unit, and can be used interchangeably with terms such as porosity and porosity.

[0089] In one embodiment of the present invention, the “porosity” corresponds to a value obtained by subtracting the volume converted into the weight and density of each component of the coating layer (130) from the volume calculated in terms of the thickness, width, and length of the coating layer (130).

[0090] In one embodiment of the present invention, the porosity and pore size of the coating layer (130) are measured by the BET 6-point method using a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Bell Japan Inc, Belsorp-II mini) through a nitrogen gas adsorption flow method. At this time, it is advantageous to use a capillary flow porometer.

[0091]

[0092] One embodiment of the present invention provides a method for manufacturing a separator (100) for an electrochemical device, comprising: a step (S10) of applying a slurry for a coating layer containing a first polymer binder (131) and inorganic particles (133) onto at least one surface of a porous polymer substrate (110) to form a coating layer (130); and a step (S30) of applying a slurry for an adhesive layer containing a first polymer binder (131) and a second polymer binder (151) onto the coating layer (130) to form an adhesive layer (150).

[0093] A method for manufacturing a separator (100) for an electrochemical device according to one embodiment of the present invention maintains the viscosity of a slurry for a coating layer low, thereby improving the dispersibility of inorganic particles and a polymer binder.

[0094] FIG. 2 is a flowchart of a method for manufacturing a separator (100) for an electrochemical device according to an embodiment of the present invention. Referring to FIG. 2, a method for manufacturing a separator (100) for an electrochemical device according to an embodiment of the present invention will be described. In the description of the method for manufacturing a separator (100) for an electrochemical device according to an embodiment of the present invention, any content that overlaps with the description of the separator for an electrochemical device will be omitted.

[0095] According to one embodiment of the present invention, prior to the step (S20) of providing the coating layer (130), a step (S10) of preparing a slurry for a coating layer including a first polymer binder (131) and inorganic particles (133) is included. As described above, in the step (S10) of preparing the slurry for a coating layer, the viscosity of the slurry for the coating layer can be implemented to be low, thereby improving the dispersibility of the inorganic particles within the slurry and improving the uniformity of the coating layer.

[0096] According to one embodiment of the present invention, a step (S20) of applying a slurry for a coating layer including a first polymer binder (131) and inorganic particles (133) to at least one surface of a porous polymer substrate (110) to form a coating layer (130) is included. As described above, by including a step (S20) of applying a slurry for a coating layer including a first polymer binder (131) and inorganic particles (133) to at least one surface of a porous polymer substrate (110) to form a coating layer (130), a coating layer (130) can be formed with a single application, and the slurry for the coating layer uniformly disperses inorganic particles, thereby improving the uniformity of the coating layer.

[0097] According to one embodiment of the present invention, a step (S40) of preparing a slurry for an adhesive layer including a first polymer binder (131) and a second polymer binder (151) is included before the step (S50) of providing the adhesive layer (150). As described above, by including a step (S40) of preparing a slurry for an adhesive layer including a first polymer binder (131) and a second polymer binder (151) before the step (S50) of providing the adhesive layer (150), the first polymer binder is included in the slurry for the coating layer at a low content (10 wt% or less), thereby lowering the viscosity of the slurry for the coating layer and improving the dispersibility of the inorganic particles within the slurry for the coating layer.

[0098] According to one embodiment of the present invention, a step (S50) of forming an adhesive layer (150) by applying a slurry for an adhesive layer including a first polymer binder (131) and a second polymer binder (151) onto the coating layer (130) is included. The adhesive layer (150) can be formed with a single application, and the first polymer binder, which is a liquid dissolved in the slurry for an adhesive layer, moves into the pores of the coating layer, thereby allowing the first polymer binder to be positioned in excess on the porous polymer substrate.

[0099] According to one embodiment of the present invention, the method of applying the slurry for the coating layer to the surface of the porous polymer substrate (110) and / or the method of applying the slurry for the adhesive layer to the surface of the coating layer (130) are not particularly limited to any one method, and conventional methods known in the art may be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, gravure, or a mixture thereof may be used.

[0100] According to one embodiment of the present invention, a drying step (S30, S60) is further included after the step (S20) of providing the coating layer (130) and the step (S50) of providing the adhesive layer (150). As described above, by further including a drying step (S30, S60) after the step (S20) of providing the coating layer (130) and the step (S50) of providing the adhesive layer (150), damage to the coating layer can be minimized, and the solvent included in the slurry can be easily removed.

[0101] Meanwhile, the order of the method for manufacturing the above-described electrochemical device separator (100) may be appropriately modified and implemented. For example, the slurry preparation step (S40) for the adhesive layer may be implemented together with the slurry preparation step (S10) for the coating layer.

[0102] According to one embodiment of the present invention, the drying process appropriately sets time conditions so as to minimize the occurrence of surface defects in the coating layer (130) and / or the adhesive layer (150). The drying may be performed using a drying auxiliary device such as a drying oven or hot air within an appropriate range.

[0103] According to one embodiment of the present invention, the first polymer binder (131) and the inorganic particles (133) are dissolved and dispersed in a solvent to prepare a slurry for a coating layer. The solvent preferably has a solubility index similar to that of the binder polymer to be used and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of solvents that can be used include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof. For example, the solvent is water. The content ratio of the inorganic particles and the polymer binder particles is as described below, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the coating layer to be finally manufactured according to one embodiment of the present invention.

[0104] According to one embodiment of the present invention, a polymer binder resin, i.e., a first polymer binder particle (131) and a second polymer binder (151), are dispersed and dissolved in an appropriate solvent to prepare a slurry for an adhesive layer. The solvent is preferably one having a solubility index similar to that of the binder polymer to be used and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of usable solvents include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof. Alternatively, the solvent is water.

[0105] According to one embodiment of the present invention, the content of the first polymer binder (131) dissolved in the solvent in the slurry for the coating layer is about 0.1 wt% or more and 10 wt% or less. For example, the content of the first polymer binder (131) dissolved in the solvent in the slurry for the coating layer is about 0.2 wt% to 9.9 wt%, about 0.3 wt% to 9.8 wt%, about 0.4 wt% to 9.7 wt%, about 0.5 wt% to 9.6 wt%, about 0.6 wt% to 9.5 wt%, about 0.7 wt% to 9.4 wt%, about 0.8 wt% to 9.3 wt%, about 0.9 wt% to 9.2 wt%, about 1.0 wt% to 9.1 wt%, about 1.1 wt% to 9.0 wt%, about 1.2 wt% to 8.9 wt%, about 1.3 wt% to 8.8 wt%, about 1.4 wt% to 8.7 wt%, about 1.5 % to 8.6 wt%, about 1.6 wt% to 8.5 wt%, about 1.7 wt% to 8.4 wt%, about 1.8 wt% to 8.3 wt%, about 1.9 wt% to 8.2 wt%, about 2.0 wt% to 8.1 wt%, about 2.1 wt% to 8.0 wt%, about 2.2 wt% to 7.9 wt%, about 2.3 wt% to 7.8 wt%, about 2.4 wt% to 7.7 wt%, about 2.5 wt% to 7.6 wt%, about 2.6 wt% to 7.5 wt%, about 2.7 wt% to 7.4 wt%, about 2.8 wt% to 7.3 wt%, about 2.9 wt% to 7.2 wt%, about 3.0 wt% or more 7.1 wt% or less, about 3.1 wt% or more and 7.0 wt% or less, about 3.2 wt% or more and 6.9 wt% or less, about 3.3 wt% or more and 6.8 wt% or less, about 3.4 wt% or more and 6.7 wt% or less, about 3.5 wt% or more and 6.6 wt% or less, about 3.6 wt% or more and 6.5 wt% or less, about 3.7 wt% or more and 6.4 wt% or less, about 3.8 wt% or more and 6.3 wt% or less, about 3.9 wt% or more and 6.2 wt% or less, about 4.0 wt% or more and 6.1 wt% or less, about 4.1 wt% or more and 6.0 wt% or less, about 5.2 wt% or more and 5.9 wt% or less, about 5.3 wt% or more and 5.8 wt% or less, about 5.4 wt% or more and 5.7 wt% or less, or about 5.5 wt% or more and 5.6 wt% or less. By controlling the content of the first polymer binder (131) dissolved in the solvent in the slurry for the coating layer within the above-described range, the bonding strength of the coating layer is improved.

[0106] According to one embodiment of the present invention, the slurry for the coating layer further comprises a dispersant. For example, the dispersant is sodium carboxymethyl cellulose. As described above, by further comprising the dispersant in the slurry for the coating layer, the degree of dispersion of the inorganic particles contained in the slurry for the coating layer is improved.

[0107] According to one embodiment of the present invention, the content of the dispersant is about 1 wt% or more and 5 wt% or less based on the total content excluding the solvent included in the slurry for the coating layer. By controlling the content of the dispersant in the slurry for the coating layer within the above-described range, the degree of dispersion of the inorganic particles included in the slurry for the coating layer is improved.

[0108] According to one embodiment of the present invention, the content of the first polymer binder (131) dissolved in the solvent in the slurry for the adhesive layer is about 5 wt% or more and 40 wt% or less. For example, the content of the first polymer binder (131) dissolved in the solvent in the slurry for the adhesive layer is about 6 wt% to 39 wt%, about 7 wt% to 38 wt%, about 9 wt% to 37 wt%, about 10 wt% to 36 wt%, about 11 wt% to 35 wt%, about 12 wt% to 34 wt%, about 13 wt% to 32 wt%, about 14 wt% to 31 wt%, about 15 wt% to 30 wt%, about 16 wt% to 29 wt%, about 17 wt% to 28 wt%, about 19 wt% to 27 wt%, about 20 wt% to 26 wt%, about 21 wt% to 25 wt%, and about 22 wt% to 24 wt%. By controlling the content of the first polymer binder (131) dissolved in the solvent in the slurry for the adhesive layer within the above-described range, the adhesive strength between the porous polymer substrate and the coating layer is improved.

[0109] According to one embodiment of the present invention, the content of the second polymer binder (151) in the slurry for the adhesive layer is about 30 wt% or more and 95 wt% or less. For example, the content of the second polymer binder (151) in the slurry for the adhesive layer is about 35 wt% or more and 90 wt% or less, about 40 wt% or more and 85 wt% or less, about 45 wt% or more and 80 wt% or less, about 50 wt% or more and 75 wt% or less, about 55 wt% or more and 70 wt% or less, or about 60 wt% or more and 65 wt% or less. By controlling the content of the second polymer binder (151) in the slurry for the adhesive layer within the above-described range, the adhesive strength between the electrode and the separator is improved.

[0110] According to one embodiment of the present invention, the viscosity of the slurry for the coating layer may be about 20 cp or more and 40 cp or less. For example, the viscosity of the slurry for the coating layer may be about 21 cp or more and 39 cp or less, about 22 cp or more and 38 cp or less, about 23 cp or more and 37 cp or less, about 24 cp or more and 36 cp or less, about 25 cp or more and 35 cp or less, about 26 cp or more and 34 cp or less, about 27 cp or more and 33 cp or less, about 28 cp or more and 32 cp or less, or about 29 cp or more and 31 cp or less. By controlling the viscosity of the slurry for the coating layer within the above-described range, the dispersibility of the inorganic particles in the slurry for the coating layer can be improved, and the uniformity of the coating layer is improved.

[0111] According to one embodiment of the present invention, the average particle diameter (D) of the particles included in the slurry for the coating layer 90 ) is about 0.01 ㎛ or more and 10.0 ㎛ or less. In the above-mentioned range, the average particle diameter (D) of the particles included in the slurry for the coating layer 90 ) can be adjusted to reduce the thickness of the coating layer, and the dispersibility of the slurry for the coating layer can be improved.

[0112] In one embodiment of the present invention, "D 90 "Particle size" means the particle size at the 90% point of the cumulative distribution of the number of particles according to the particle size. The particle size is measured using the laser diffraction method. For example, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the particle size distribution is calculated by measuring the difference in the diffraction pattern according to the particle size when the particles pass through the laser beam. By calculating the particle diameter at the point where the cumulative distribution of the number of particles according to the particle size in the measuring device becomes 90%, D 90 Measure the mouth diameter.

[0113] According to one embodiment of the present invention, the separator (100) is interposed between the cathode and the anode and is manufactured into an electrochemical device through a lamination process that applies heat and / or pressure to bond them. In one embodiment of the present invention, the lamination process is performed by a roll press device including a pair of pressure rollers. That is, the cathode, the separator, and the anode are sequentially laminated and placed between the pressure rollers to achieve interlayer bonding. At this time, the lamination process is performed by a hot press method.

[0114] FIG. 3 is a schematic diagram of an electrochemical device (1000) according to one embodiment of the present invention. Referring to FIGS. 1 and 3, the electrochemical device (1000) according to one embodiment of the present invention will be described.

[0115] One embodiment of the present invention provides an electrochemical device (1000) comprising: a positive electrode (300); a negative electrode (500); and a separator (100) for an electrochemical device interposed between the positive electrode (300) and the negative electrode (500), wherein the adhesive force between the porous polymer substrate (110) and the coating layer (130) is about 30 gf / 25 mm or more.

[0116] An electrochemical device (1000) according to one embodiment of the present invention improves the adhesive strength between a coating layer (130) and a porous polymer substrate (110), and improves the adhesive strength between the separator (100) and an electrode.

[0117]

[0118] According to one embodiment of the present invention, the electrochemical device (1000) includes an anode (300); a cathode (500); and a separator (100) for an electrochemical device interposed between the anode (300) and the cathode (500). As described above, by including the anode (300); the cathode (500); and the separator (100) for an electrochemical device interposed between the anode (300) and the cathode, the uniformity of the coating layer is improved, and the adhesion between the coating layer and the porous polymer substrate is improved.

[0119] According to one embodiment of the present invention, the adhesive force between the porous polymer substrate (110) and the coating layer (130) is about 30 gf / 25mm or more. For example, the adhesive force between the porous polymer substrate (110) and the coating layer (130) is about 30 gf / 25mm or more and 100 gf / 25mm or less, about 35 gf / 25mm or more and 95 gf / 25mm or less, about 40 gf / 25mm or more and 90 gf / 25mm or less, about 45 gf / 25mm or more and 85 gf / 25mm or less, about 50 gf / 25mm or more and 80 gf / 25mm or less, about 55 gf / 25mm or more and 75 gf / 25mm or less, or about 60 gf / 25mm or more and 70 gf / 25mm or less. Alternatively, the adhesive force refers to dry adhesive force. By controlling the adhesive strength between the porous polymer substrate (110) and the coating layer (130) within the above-described range, the ease of assembly is improved in the process of assembling the electrode.

[0120] In one embodiment of the present invention, the “adhesive force” is measured by bonding an electrode and a separator at 60° C. and 6.5 MPa to produce a half-cell to measure the electrode / separator adhesive force of the separator, and then applying force to the half-cell at 180° and a measurement speed of 300 mm / min using a UTM device to measure the force required to separate the electrode and the separator.

[0121] According to one embodiment of the present invention, the adhesive force between the porous polymer substrate (110) and the coating layer (130) is greater than the adhesive force between either the positive electrode (300) or the negative electrode (500) and the adhesive layer (150) by about 5 gf / 25 mm. For example, the adhesive strength between the porous polymer substrate (110) and the coating layer (130) is greater than the adhesive strength between either the positive electrode (300) or the negative electrode (500) and the adhesive layer (150) by about 5 gf / 25mm or more and 100 gf / 25mm or less, about 10 gf / 25mm or more and 95 gf / 25mm or less, about 15 gf / 25mm or more and 90 gf / 25mm or less, about 20 gf / 25mm or more and 85 gf / 25mm or less, about 25 gf / 25mm or more and 80 gf / 25mm or less, about 30 gf / 25mm or more and 75 gf / 25mm or less, about 35 gf / 25mm or more and 70 gf / 25mm or less, about 40 gf / 25mm or more and 65 gf / 25mm or less, or about 45 gf / 25mm or more and 60 gf / 25mm or less or about 50 gf / 25mm or more and 55 gf / 25mm or less is large. In the above-described range, the adhesive force between the porous polymer substrate (110) and the coating layer (130) is improved by controlling the difference in adhesive force between either the positive electrode (300) or the negative electrode (500) and the adhesive layer (150), thereby improving the adhesive force between the separator (100) and the electrode.

[0122] According to one embodiment of the present invention, the positive electrode (300) has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-xLithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn1-xM x A lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.

[0123] According to one embodiment of the present invention, the negative electrode (500) has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, graphite carbon, etc. as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함한다.

[0124] According to one embodiment of the present invention, the conductive material is, for example, one selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials thereof. For example, the conductive material is one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials thereof.

[0125] According to one embodiment of the present invention, the current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., etc. are used.

[0126] According to one embodiment of the present invention, the binder resin uses a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0127] According to one embodiment of the present invention, the positive electrode slurry for manufacturing the positive electrode active material layer includes a dispersant, wherein the dispersant is a pyrrolidone-based compound. Alternatively, the dispersant is N-methylpyrrolidone (ADC-01, LG Chemical).

[0128] According to one embodiment of the present invention, the content of the dispersant included in the positive electrode slurry may be about 0 part by weight or more and 0.5 part by weight or less with respect to 100 parts by weight of the positive electrode slurry. For example, the content of the dispersant included in the positive electrode slurry may be about 0.05 part by weight or more and 0.4 part by weight or less with respect to 100 parts by weight of the positive electrode slurry.

[0129] According to one embodiment of the present invention, the negative electrode slurry for manufacturing the negative electrode active material layer may include a dispersant, wherein the dispersant is a polypyrrolidone-based compound. For example, the dispersant is polyvinylpyrrolidone (Junsei, Japan).

[0130] According to one embodiment of the present invention, the content of the dispersant included in the cathode slurry is about 0 part by weight or more and 0.5 part by weight or less, based on 100 parts by weight of the cathode slurry. For example, the content of the dispersant included in the cathode slurry is about 0.05 part by weight or more and 0.4 part by weight or less, based on 100 parts by weight of the cathode slurry.

[0131] According to one embodiment of the present invention, the electrochemical device prepared as described above is placed in an appropriate case and an electrolyte is injected to manufacture a battery.

[0132] According to one embodiment of the present invention, the electrolyte is A + B - As a salt with the same structure, A + is Li + , Na + , K +B containing an ion composed of an alkali metal cation or a combination thereof; - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 - Salts containing anions such as or combinations thereof are dissolved or dissociated in organic solvents such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or mixtures thereof, but are not limited thereto.

[0133] In one embodiment of the present invention, the separator for an electrochemical device of the present invention can be similarly applied to a lithium secondary battery or a sodium secondary battery manufactured using lithium ions or sodium ions as a positive electrode active material including the separator for an electrochemical device.

[0134] In addition, unlike the lithium secondary battery described above, the lithium secondary battery according to another embodiment of the present invention is an all-solid-state battery.

[0135] One embodiment of the present invention provides a battery module including a battery including the electrochemical element as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Examples of the device include a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.

[0136] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not construed as being limited to the examples described below. The examples of the present invention are provided to more fully explain the present invention to those of ordinary skill in the art.

[0137] <Example 1>

[0138] Polyethylene resin (weight average molecular weight 900,000) was extruded and a porous polymer substrate (total thickness of approximately 9 ㎛, porosity of 40% by volume) was manufactured using a wet method.

[0139] D of 600 nm as an inorganic particle 50 Al2O3 powder having particle sizes of 0.1 to 1.5 was prepared. Polyacrylic acid (K-702, Lubrizol) was prepared as the first binder polymer, and sodium carboxymethyl cellulose (CMC-Na) (SG-L02, GL Chem) was prepared as the dispersant.

[0140] The above-prepared inorganic particles, first binder polymer, and dispersant were added to water in a weight ratio of 92:5:3, and then the inorganic particles were crushed and dispersed to prepare a slurry for a coating layer.

[0141] The slurry for the coating layer was applied to both sides of the porous polymer substrate using a doctor blade by bar coating, and dried with air at 50°C using a heat gun to form a coating layer.

[0142] A slurry for an adhesive layer (solid content: 5 wt%) was prepared by adding and dispersing polyacrylic acid (K-702, Lubrizol Co.), a polyacrylate copolymer, as a first polymer binder, and an acrylic emulsion (BM-2510M, Zeon Co.), as a second polymer binder, in a weight ratio of 90:10 in water, a solvent.

[0143] The slurry for the above adhesive layer was applied by bar coating on the above coating layer and then dried to form an adhesive layer, thereby manufacturing a separator for an electrochemical device.

[0144] The slurry for the adhesive layer was applied to both sides of the surface of the coating layer using a doctor blade by bar coating, and dried with wind at 50°C using a heat gun to form an adhesive layer, thereby manufacturing a separator for an electrochemical device.

[0145] <Comparative Example 1>

[0146] A separator was manufactured in the same manner as in Example 1, except that a slurry for a coating layer was manufactured using the inorganic particles, the first polymer binder, and the dispersant in a weight ratio of 85:12:3.

[0147] Comparative Example 2

[0148] A separator was manufactured in the same manner as in Example 1, except that a slurry for a coating layer was manufactured using the inorganic particles, the first polymer binder, and the dispersant in a weight ratio of 97:0:3.

[0149] <Comparative Example 3>

[0150] A separator was manufactured in the same manner as in Example 1, except that the slurry for the adhesive layer was manufactured using the first polymer binder and the second polymer binder in a weight ratio of 3:97 in the electrochemical device separator of Example 1.

[0151] Comparative Example 4

[0152] A separator was manufactured in the same manner as in Example 1, except that the adhesive layer was not formed in the separator for the electrochemical device of Example 1.

[0153] Comparative Example 5

[0154] A separator was manufactured in the same manner as in Example 1, except that the slurry for the adhesive layer was manufactured to include only the second polymer binder in the separator for the electrochemical device of Example 1.

[0155] Comparative Example 6

[0156] A separator was manufactured in the same manner as in Example 1, except that the slurry for the adhesive layer was manufactured to include only the first polymer binder in the separator for the electrochemical device of Example 1.

[0157]

[0158] <Manufacturing of electrochemical devices>

[0159] 1) Manufacturing of the anode

[0160] Cathode active material (LiNi) 0.8 Mn 0.1 Co 0.1 O2), a conductive agent (carbon black), a dispersant (N-methylpyrrolidone, ADC-01, LG Chemical), and a binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to manufacture a positive electrode having a positive electrode active material layer (thickness 120 μm).

[0161] 2) Manufacturing of cathode

[0162] Graphite (natural graphite and artificial graphite blend), conductive agent (carbon black), dispersant (polyvinylpyrrolidone, Junsei, Japan), and binder resin (PVDF-HFP and PVDF blend) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for an anode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of a copper thin film (thickness 10 μm) and dried to manufacture an anode having an anode active material layer (thickness 120 μm).

[0163] 3) Lamination process

[0164] The separators of the examples and comparative examples were interposed between the manufactured cathodes and anodes, and a lamination process was performed to obtain an electrode assembly. The lamination process was performed using a hot press at 60°C and 6.5 MPa for 1 second.

[0165]

[0166] <Experimental Example 1: Measurement of Adhesion Between Electrodes and Separators>

[0167] The separators of Example 1 and Comparative Examples 1 to 6 were cut into 70 mm (length) x 25 mm (width) pieces, and the prepared cathodes and separators were laminated using a press under the conditions of 60°C, 6.5 MPa, and 1 second to produce specimens. The prepared specimens were fixed by attaching them to a glass plate using double-sided tape, and at this time, the cathodes were positioned so that they faced the glass plate. The separator portion of the specimen was peeled at an angle of 180° at a speed of 150 mm / min at 25°C, and the strength at this time was measured and summarized in Table 1 below.

[0168] <Experimental Example 2: Measurement of Adhesion Between Porous Polymer Substrate and Coating Layer>

[0169] The separators of Example 1 and Comparative Examples 1 to 6 were cut into 70 mm (length) x 25 mm (width) pieces and fixed by attaching them to a glass plate using double-sided tape. The separator portion of the specimen was peeled at an angle of 180° at a speed of 150 mm / min at 25°C, and the strength at this time was measured and summarized in Table 1 below.

[0170] <Experimental Example 3: Measurement of particle size in slurry for coating layer>

[0171] The slurry for the coating layer manufactured in the membrane manufacturing process of Example 1 and Comparative Examples 1 to 6 was dispersed in a dispersion medium, and then introduced into a laser diffraction particle size measuring device (Microtrac S3500). When the particles passed through the laser beam, the difference in the diffraction pattern according to the particle size was measured to calculate the particle size distribution, which was summarized in Table 1 below.

[0172] <Experimental Example 4: Viscosity Measurement of Slurry for Coating Layer>

[0173] The viscosity of the slurry for the coating layer manufactured in the membrane manufacturing process of Example 1 and Comparative Examples 1 to 6 was measured at 25°C using a Brookfield LV DV-II + Pro Viscometer (cone-plate type), torque 90%, spindle #42, sample loading amount 1 mL) and summarized in Table 1 below.

[0174] <Experimental Example 5: Defect Count Measurement>

[0175] The membranes of Example 1 and Comparative Examples 1 to 6 were cut to 0.5 m X 0.5 m and the number of defects of 1 ㎛ or more was counted using an optical microscope. 2 After conversion, it is summarized in Table 1 below.

[0176]

[0177] Adhesion of electrode-separator (gf / 25mm) Adhesion of porous polymer substrate-coating layer (gf / 25mm) Particle size of slurry for coating layer (D90, ㎛) Viscosity of slurry for coating layer (cp) Number of defects (pieces / m) 2 ) Example 132541.1280 Comparative Example 1356115.48937 Comparative Example 215331.0250 Comparative Example 313221.1280 Comparative Example 40301.1280 Comparative Example 511191.1280 Comparative Example 60941.1280

[0178] Referring to Table 1 above, Example 1, which is an embodiment of the present invention, included an appropriate amount of the first polymer binder in the coating layer, and it was confirmed that both the adhesion of the electrode-separator and the adhesion of the porous polymer substrate-coating layer were improved and the number of defects was 0. In contrast, Comparative Example 1 confirmed that the first polymer binder was excessively included in the coating layer, and thus the number of defects rapidly increased and the viscosity of the slurry for the coating layer increased. In Comparative Example 2, it was confirmed that both the adhesion of the electrode-separator and the adhesion of the porous polymer substrate-coating layer were reduced because the first polymer binder was not included in the coating layer. In Comparative Example 3, it was confirmed that both the adhesion of the electrode-separator and the adhesion of the porous polymer substrate-coating layer were reduced because the first polymer binder was included in a small amount and the second polymer binder was excessively included in the adhesive layer. Comparative Example 4 confirmed that the adhesion of the electrode-separator was rapidly reduced because the adhesive layer was not included. Comparative Example 5 confirmed that both the adhesion of the electrode-separator and the adhesion of the porous polymer substrate-coating layer were reduced when only the second polymer binder was included in the adhesive layer. In addition, Comparative Example 6 confirmed that the adhesion of the electrode-separator was rapidly reduced when only the first polymer binder was included in the adhesive layer.

[0179] Therefore, the separator for an electrochemical device according to one embodiment of the present invention and the electrochemical device including the same reduce the number of defects by controlling the type and content of the polymer binder included in the coating layer and the adhesive layer, thereby improving both the adhesion between the electrode and the separator and the adhesion between the porous polymer substrate and the coating layer, and improve workability by lowering the viscosity of the slurry during the manufacturing process.

[0180] One embodiment of the present invention provides a separator for an electrochemical device, comprising: a porous polymer substrate; a coating layer provided on at least one surface of the porous polymer substrate and including a first polymer binder and inorganic particles; and an adhesive layer provided on the coating layer and including a second polymer binder, wherein the first polymer binder is in solution form, and the content of the first polymer binder included in a portion of the coating layer adjacent to the porous polymer substrate is greater than the content of the first polymer binder included in another portion spaced apart from the porous polymer substrate.

[0181] According to one embodiment of the present invention, the solubility of the second polymer binder in water may be lower than the solubility of the first polymer binder in water.

[0182] According to one embodiment of the present invention, the first polymer binder may be one selected from the group consisting of polyacrylic acid, polyurethane, polyacrylonitrile, polyethylene glycol, polyacrylamide, polyvinyl alcohol, and combinations thereof.

[0183] According to one embodiment of the present invention, the second polymer binder may be in particle form.

[0184] One embodiment of the present invention provides a method for manufacturing a separator for an electrochemical device, comprising: a step of applying a slurry for a coating layer containing a first polymer binder and inorganic particles to at least one surface of a porous polymer substrate to form a coating layer; and a step of applying a slurry for an adhesive layer containing a first polymer binder and a second polymer binder to form an adhesive layer on the coating layer.

[0185] According to one embodiment of the present invention, the step of providing the coating layer and the step of providing the adhesive layer may further include a drying step.

[0186] According to one embodiment of the present invention, the content of the first polymer binder dissolved in the solvent in the slurry for the coating layer may be 0.1 wt% or more and 10 wt% or less.

[0187] According to one embodiment of the present invention, the content of the second polymer binder dissolved in the solvent in the slurry for the adhesive layer may be 5 wt% or more and 40 wt% or less.

[0188] According to one embodiment of the present invention, the average particle diameter (D) of the particles included in the slurry for the coating layer 90 ) may be 0.01 ㎛ or more and 10.0 ㎛ or less.

[0189] One embodiment of the present invention provides an electrochemical device comprising: a positive electrode; a negative electrode; and a separator for an electrochemical device interposed between the positive electrode and the negative electrode, wherein the adhesive force between the porous polymer substrate and the coating layer is 30 gf / 25 mm or more.

[0190] According to one embodiment of the present invention, the adhesive force between the porous polymer substrate and the coating layer may be greater than the adhesive force between either the positive electrode or the negative electrode and the adhesive layer by about 5 gf / 25 mm or more.

[0191] While the present invention has been described above with reference to preferred embodiments, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes can be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.

[0192] [Explanation of symbols]

[0193] 100: Separator for electrochemical devices

[0194] 110: Porous polymer substrate

[0195] 130: Coating layer

[0196] 131: First polymer binder

[0197] 133: Inorganic particles

[0198] 150: Adhesive layer

[0199] 151: Second polymer binder

[0200] 300: Bipolar

[0201] 500: negative

[0202] 1000: Electrochemical devices

Claims

1. Porous polymer substrate; A coating layer provided on at least one surface of the porous polymer substrate, the coating layer including a first polymer binder and inorganic particles; and It is provided on the above coating layer and includes an adhesive layer including a second polymer binder, The above first polymer binder is in solution form, A separator for an electrochemical device, wherein the content of the first polymer binder included in a portion adjacent to the porous polymer substrate in the coating layer is greater than the content of the first polymer binder included in another portion facing away from the porous polymer substrate.

2. In claim 1, A separator for an electrochemical device, wherein the solubility of the second polymer binder in water is lower than the solubility of the first polymer binder in water.

3. In claim 1, A separator for an electrochemical device, wherein the first polymer binder is one selected from the group consisting of polyacrylic acid, polyurethane, polyacrylonitrile, polyethylene glycol, polyacrylamide, polyvinyl alcohol, and combinations thereof.

4. In claim 1, A separator for an electrochemical device, wherein the second polymer binder is in particle form.

5. In a manufacturing method for manufacturing a separator for an electrochemical device according to any one of claims 1 to 4, A step of providing a coating layer by applying a slurry for a coating layer including a first polymer binder and inorganic particles to at least one surface of a porous polymer substrate; and A method for manufacturing a separator for an electrochemical device, comprising the step of forming an adhesive layer by applying a slurry for an adhesive layer including a first polymer binder and a second polymer binder onto the coating layer.

6. In claim 5, A method for manufacturing a separator for an electrochemical device, further comprising a drying step after each of the step of providing the coating layer and the step of providing the adhesive layer.

7. In claim 5, A method for manufacturing a separator for an electrochemical device, wherein the content of the first polymer binder dissolved in a solvent in the slurry for the above coating layer is 0.1 wt% or more and 10 wt% or less.

8. In claim 5, A method for manufacturing a separator for an electrochemical device, wherein the content of the first polymer binder dissolved in a solvent in the slurry for the adhesive layer is 5 wt% or more and 40 wt% or less.

9. In claim 5, The average particle diameter (D) of the inorganic particles contained in the slurry for the coating layer 90 ) is a method for manufacturing a separator for an electrochemical device having a thickness of 0.01 ㎛ or more and 10.0 ㎛ or less.

10. A positive electrode; a negative electrode; and a separator for an electrochemical device interposed between the positive electrode and the negative electrode, comprising any one of claims 1 to 4, An electrochemical device wherein the adhesive strength between the porous polymer substrate and the coating layer is 30 gf / 25 mm or more.

11. In claim 10, An electrochemical device wherein the adhesive force between the porous polymer substrate and the coating layer is at least 5 gf / 25 mm greater than the adhesive force between either the positive electrode or the negative electrode and the adhesive layer.

Citation Information

Patent Citations

  • A sperator for an electrochemical device, an electrochemical device comprising the same and a manufacturing method thereof

    KR1020240170137A

  • Electrode assembly having separator and electrode adhesive layers, and electrochemical devices comprising the same

    KR1020140026009A

  • A separator comprising a adhesion layer for an electrochemical device and an electrode assembly comprising the same

    KR1020170113474A

  • System and method for ventilation of substation

    KR1020220081969A

  • Separator for electrochemical cell and method for its manufacture

    US20170373292A1