Biodegradable resin composition and biodegradable molded product comprising same

The biodegradable resin composition, combining a biodegradable resin with light-shielding particles and an inorganic filler, addresses the limitations of conventional polymers by providing strong, UV-resistant, and easily decomposable biodegradable molded articles.

WO2024248352A1PCT designated stage expired Publication Date: 2024-12-05SK LEAVEO CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006188
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-08
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional petroleum-based polymer materials are not biodegradable, leading to environmental issues due to slow decomposition and emission of harmful substances, while biodegradable alternatives like PLA and PBAT lack flexibility and mechanical strength, and PBAT has poor resistance to ultraviolet rays.

Method used

A biodegradable resin composition comprising a biodegradable resin, light-shielding particles, and an inorganic filler, which provides excellent mechanical properties and resistance to ultraviolet rays, with an elongation retention rate of 20% or more, allowing for the production of biodegradable molded articles that maintain mechanical strength and can be easily decomposed.

Benefits of technology

The biodegradable resin composition ensures high biodegradability, improved water resistance, and maintained mechanical strength, enabling the creation of eco-friendly products with enhanced durability and disposability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024006188-APPB-IMG-000001
    Figure PCTKR2024006188-APPB-IMG-000001
  • Figure PCTKR2024006188-APPB-IMG-000002
    Figure PCTKR2024006188-APPB-IMG-000002
  • Figure PCTKR2024006188-APPB-IMG-000003
    Figure PCTKR2024006188-APPB-IMG-000003
Patent Text Reader

Abstract

The present invention provides: a biodegradable resin composition comprising a biodegradable resin, light-shielding particles, and an inorganic filler, and having an elongation retention rate (△E) of 20% or more as measured by a predetermined measurement method; and a biodegradable molded product comprising the biodegradable resin composition. In addition, the content of the biodegradable resin may be 30-90 wt% based on the total weight of the biodegradable resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Biodegradable resin composition and biodegradable molded article comprising the same

[0001] The present invention relates to a biodegradable resin composition and a biodegradable molded article comprising the same.

[0002]

[0003] With growing concerns about environmental issues, solutions are being sought for the disposal of various household goods, especially disposable products. Specifically, petroleum-based polymer materials are widely used in the manufacture of various products such as films, fibers, packaging materials, bottles, and containers due to their low cost and excellent processability. However, when incinerated at the end of their useful life, they emit hazardous substances, and depending on the type, they can take hundreds of years to completely decompose naturally.

[0004] To overcome the limitations of these petroleum-based polymer materials, active research is being conducted on biodegradable resins that decompose in a relatively short period of time. Biodegradable resins such as polylactic acid (PLA), polybutyleneadipate terephthalate (PBAT), and polybutylene succinate (PBS) are being introduced as alternatives.

[0005] However, PLA lacks flexibility, and PBAT has poor mechanical properties, limiting its use. To address these issues, U.S. Patent No. 9,096,758 described a biodegradable resin composition using PBAT mixed with inorganic fillers. However, its poor mechanical properties and UV resistance still limit its ability to replace conventional petroleum-based polymer materials.

[0006]

[0007] The present invention provides a biodegradable resin composition having excellent mechanical properties and resistance to ultraviolet rays, and a biodegradable molded product comprising the same.

[0008]

[0009] A biodegradable resin composition according to the present invention comprises a biodegradable resin, light-shielding particles, and an inorganic filler, and has an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method.

[0010] [measurement method]

[0011] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C.

[0012] 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm.

[0013] 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine).

[0014] 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine).

[0015] 6) Calculate the elongation retention rate (ΔE) using Equation 1 below.

[0016] [Formula 1]

[0017] ΔE(%) = (E1 / E0) X 100

[0018] In one embodiment of the present invention, the content of the biodegradable resin may be 30 wt% to 90 wt% based on the total weight of the biodegradable resin composition.

[0019] In one embodiment of the present invention, the content of the light-blocking particles may be 0.1 wt% to 10.0 wt% based on the total weight of the biodegradable resin composition.

[0020] In one embodiment of the present invention, the average diameter of the light-shielding particles may be from 10 nm to 500 nm.

[0021] In one embodiment of the present invention, the BET specific surface area of ​​the light-shielding particles is 100 m 2 / g to 700 m 2 / g may be.

[0022] In one embodiment of the present invention, the light-shielding particles may have a moisture absorption rate of 0.01% to 2.00% at a temperature of 25°C, a relative humidity of 90%, and after 120 hours.

[0023] In one embodiment of the present invention, the content of the inorganic filler may be 10 wt% to 90 wt% based on the total weight of the biodegradable resin composition.

[0024] In one embodiment of the present invention, the inorganic filler may include calcium carbonate surface-treated with an organic acid.

[0025] In one embodiment of the present invention, the first elongation of the biodegradable resin composition may be 150% to 400%.

[0026] In one embodiment of the present invention, the second elongation of the biodegradable resin composition may be 100% to 300%.

[0027] In one embodiment of the present invention, the biodegradable resin composition may further include a plasticizer.

[0028] A biodegradable molded article according to the present invention comprises a biodegradable resin composition comprising a biodegradable resin, light-shielding particles, and an inorganic filler, and having an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method.

[0029] [measurement method]

[0030] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C.

[0031] 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm.

[0032] 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine).

[0033] 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine).

[0034] 6) Calculate the elongation retention rate (ΔE) using Equation 1 below.

[0035] [Formula 1]

[0036] ΔE(%) = (E1 / E0) X 100

[0037] In one embodiment of the present invention, the biodegradable molded product may be a nonwoven fabric, a vacuum-formed sheet, a blown molded product, or an injection-molded product.

[0038]

[0039] The biodegradable resin composition according to the present invention has a high degree of biodegradability, so that a biodegradable molded product including the biodegradable resin composition can be easily decomposed when discarded.

[0040] In addition, the biodegradable resin composition according to the present invention exhibits excellent resistance to ultraviolet rays and thus exhibits high elongation retention. That is, biodegradable films and biodegradable molded articles comprising the biodegradable resin composition can appropriately maintain mechanical strength over a typical period of use.

[0041] In addition, the biodegradable resin composition according to the present invention exhibits high biodegradability and improved water resistance while minimizing the decrease in mechanical strength, thereby enabling the user to maintain a certain degree of mechanical strength and chemical properties during a typical period of use.

[0042]

[0043] The structural or functional descriptions of the embodiments disclosed in this specification or application are merely illustrative for the purpose of explaining embodiments according to the technical idea of ​​the present invention, and the embodiments according to the technical idea of ​​the present invention can be implemented in various forms other than the embodiments disclosed in this specification or application, and the technical idea of ​​the present invention is not construed as being limited to the embodiments described in this specification or application.

[0044] Additionally, when a component is referred to as "including" in this specification or application, unless otherwise specifically stated, this does not exclude other components, but rather implies the inclusion of additional components. Furthermore, all numerical ranges indicating physical property values, dimensions, etc. of the components described in this specification or application should be understood to be modified by the term "about" in all cases, unless otherwise specified.

[0045]

[0046] Hereinafter, a biodegradable resin composition according to the present invention and a biodegradable molded product comprising the same will be described.

[0047]

[0048] <Biodegradable resin composition>

[0049] A biodegradable resin composition according to the present invention comprises a biodegradable resin, light-shielding particles, and an inorganic filler, and has an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method.

[0050] [measurement method]

[0051] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C.

[0052] 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm.

[0053] 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine).

[0054] 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine).

[0055] 6) Calculate the elongation retention rate (ΔE) using Equation 1 below.

[0056] [Formula 1]

[0057] ΔE(%) = (E1 / E0) X 100

[0058]

[0059] The above biodegradable resin composition comprises a biodegradable resin.

[0060] The biodegradable resin may include a diol component and a dicarboxylic acid component. Specifically, the biodegradable resin may include a first repeating unit and a second repeating unit, wherein the first repeating unit may include a diol component and an aromatic dicarboxylic acid component, and the second repeating unit may include a diol component and an aliphatic dicarboxylic acid component.

[0061] The above diol component may include 1,4-butanediol or a derivative thereof. The diol component may include 95 mol% or more, 97 mol% or more, 98 mol% or more, 99 mol% or more, or 100 mol% of 1,4-butanediol or a derivative thereof, based on the total mole number of the diol component. By including 1,4-butanediol or a derivative thereof, the diol component can improve biodegradability, flexibility, and strength, and when the diol component is composed solely of 1,4-butanediol, the effects of improving biodegradability and strength can be maximized.

[0062] The above diol component may further include a second diol different from the first diol, which is 1,4-butanediol or a derivative thereof. The second diol may be at least one selected from the group consisting of propanediol, hexanediol, cyclohexanedimethanol, and ethylene glycol. Specifically, the second diol may be at least one selected from the group consisting of 1,3-propanediol, 1,2-propanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,6-hexanediol, 2,3-hexanediol, 2,4-hexanediol, 2,5-hexanediol, 2,6-hexanediol, 3,4-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, and ethylene glycol. The diol component may include the second diol in an amount of 5 mol% or less, 3 mol% or less, 2 mol% or less, or 1 mol% or less, based on the total mole number of the diol component.

[0063] The aromatic dicarboxylic acid component may be at least one selected from the group consisting of terephthalic acid, dimethylterephthalic acid, and derivatives thereof. Specifically, the aromatic dicarboxylic acid component may be terephthalic acid or dimethylterephthalic acid. The dicarboxylic acid component may contain the aromatic dicarboxylic acid component in an amount of 15 mol% or more, 30 mol% or more, 45 mol% or more, 50 mol% or more, or 75 mol% or more, based on the total mole number of the dicarboxylic acid component, and may contain 30 mol% to 90 mol%, 35 mol% to 80 mol%, 40 mol% to 75 mol%, 45 mol% to 65 mol%, or 45 mol% to 55 mol%.

[0064] The aliphatic dicarboxylic acid component may be at least one selected from the group consisting of adipic acid, succinic acid, and derivatives thereof. Specifically, the aliphatic dicarboxylic acid component may be adipic acid or succinic acid. The dicarboxylic acid component may comprise the aliphatic dicarboxylic acid component in an amount of 15 mol% or more, 30 mol% or more, 45 mol% or more, 50 mol% or more, or 75 mol% or more, based on the total mole number of the dicarboxylic acid component, and may comprise 30 mol% to 90 mol%, 35 mol% to 80 mol%, 40 mol% to 75 mol%, 45 mol% to 65 mol%, or 45 mol% to 55 mol%.

[0065] The molar ratio of the aromatic dicarboxylic acid component and the aliphatic dicarboxylic acid component may be 0.5 to 1.5:1, 0.6 to 1.5:1, 0.6 to 1.4:1, 0.7 to 1.4:1, 0.7 to 1.3:1, or 0.8 to 1.2:1.

[0066] The molar ratio of the above diol component and the above dicarboxylic acid component may be 0.5 to 2:1, 0.5 to 1.9:1, 0.5 to 1.8:1, 0.5 to 1.7:1, 0.6 to 1.7:1, 0.6 to 1.6:1, 0.7 to 1.5:1, or 0.9 to 1.2:1. When the above range is satisfied, the biodegradable resin composition can have improved biodegradability, strength, and processability without discoloration such as yellowing.

[0067] The biodegradable resin may include polybutylene adipate terephthalate (PBAT), wherein the first repeating unit may include a diol component and an aromatic dicarboxylic acid component, and the second repeating unit may include a diol component and an aliphatic dicarboxylic acid component.

[0068] Specifically, the polybutylene adipate terephthalate may include a unit represented by the following chemical formula 1.

[0069] [Chemical Formula 1]

[0070]

[0071] In the above chemical formula 1, m may be 1 to 20, and n may be 1 to 20.

[0072] The biodegradable resin composition may include a heterogeneous biodegradable resin other than the polybutylene adipate terephthalate. For example, the heterogeneous biodegradable resin may include at least one selected from the group consisting of polybutylene azelate terephthalate (PBAzT), polybutylene sebacate terephthalate (PBSeT), polybutylene succinate terephthalate (PBST), polyhydroxyalkanoate (PHA), and polylactic acid (PLA). The heterogeneous biodegradable resin may complement the mechanical properties of the polybutylene adipate terephthalate.

[0073] The above polylactic acid may be a high-melting-point polylactic acid having a stereocomplex crystal structure. In addition, the polylactic acid may be formed by solution mixing or melt mixing of poly L-lactic acid and poly D-lactic acid.

[0074] Specifically, the polylactic acid may include a unit represented by the following chemical formula 2.

[0075] [Chemical Formula 2]

[0076]

[0077] The polylactic acid may be a polymer comprising L-lactic acid units and / or D-lactic acid units. The polylactic acid may comprise poly L-lactic acid and / or poly D-lactic acid.

[0078] The poly L-lactic acid may be a polymer mainly comprising L-lactic acid units. The poly L-lactic acid may comprise L-lactic acid units in an amount of about 90 mol% to about 100 mol%, about 91 mol% to about 100 mol%, about 92 mol% to about 100 mol%, about 93 mol% to about 100 mol%, about 94 mol% to about 100 mol%, about 95 mol% to about 100 mol%, about 96 mol% to about 100 mol%, or about 97 mol% to about 100 mol%. The poly L-lactic acid may comprise D-lactic acid units and / or units other than lactic acid. The poly L-lactic acid may contain the D-lactic acid unit and / or units other than lactic acid in an amount of about 0 mol% to about 10 mol%, about 0 mol% to about 9 mol%, about 0 mol% to about 8 mol%, about 0 mol% to about 7 mol%, about 0 mol% to about 6 mol%, about 0 mol% to about 5 mol%, or about 0 mol% to about 3 mol%.

[0079] The poly D-lactic acid may be a polymer mainly comprising D-lactic acid units. The poly D-lactic acid may comprise the D-lactic acid units in an amount of about 90 mol% to about 100 mol%, about 91 mol% to about 100 mol%, about 92 mol% to about 100 mol%, about 93 mol% to about 100 mol%, about 94 mol% to about 100 mol%, about 95 mol% to about 100 mol%, or about 97 mol% to about 100 mol%. The poly D-lactic acid may comprise the L-lactic acid units and / or units other than lactic acid. The poly D-lactic acid may contain the L-lactic acid unit and / or units other than lactic acid in an amount of about 0 mol% to about 10 mol%, about 0 mol% to about 9 mol%, about 0 mol% to about 8 mol%, about 0 mol% to about 7 mol%, about 0 mol% to about 6 mol%, about 0 mol% to about 5 mol%, or about 0 mol% to about 3 mol%.

[0080] Units other than the above lactic acid may be units derived from dicarboxylic acids, polyhydric alcohols, hydroxycarboxylic acids, lactones, etc. having functional groups capable of forming two or more ester bonds, and units derived from various polyesters, various polyethers, various polycarbonates, etc. composed of various components of these.

[0081] Examples of the above dicarboxylic acids include succinic acid, adipic acid, azelaic acid, sebacic acid, terephthalic acid, and isophthalic acid. Examples of the above polyhydric alcohols include aliphatic polyhydric alcohols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, glycerin, sorbitan, neopentyl glycol, diethylene glycol, triethylene glycol, polyethylene glycol, and polypropylene glycol, or aromatic polyhydric alcohols such as bisphenol with ethylene oxide added thereto.

[0082] Examples of the above hydroxycarboxylic acids include glycolic acid, hydroxybutyric acid, etc. Examples of the lactones include glycolide, ε-caprolactone glycolide, ε-caprolactone, β-propiolactone, δ-butyrolactone, β- or γ-butyrolactone, pivalolactone, δ-valerolactone, etc.

[0083] The polylactic acid may be commercially available from Biomer, Inc. under the name BIOMER™ L9000. The polylactic acid may also be commercially available from Natureworks LLC (NATUREWORKS®) or Mitsui Chemical (LACEA™). The polylactic acid may also be described in U.S. Patent Nos. 4,797,468, 5,470,944, 5,770,682, 5,821,327, 5,880,254, and 6,326,458, the entire contents of which are incorporated herein by reference for all purposes.

[0084] The above polyhydroxyalkanoate may include a unit represented by the following chemical formula 3.

[0085] [Chemical Formula 3]

[0086]

[0087] In the above chemical formula 3, R is independently selected from the group consisting of a hydrogen atom, a hydrocarbon group, a heteroatom, and a combination thereof, n is the number of repeating units of 1 to 35,000, and x can represent an integer of 1 to 5.

[0088] The above polyhydroxyalkanoate may be a homopolymer or copolymer composed of at least one moiety selected from the group consisting of 3-hydroxypropionate, 3-hydroxybutyrate, 3-hydroxyvalerate, 3-hydroxyhexanoate, 3-hydroxyheptanoate, 3-hydroxyoctanoate, 3-hydroxynonanoate, 3-hydroxydecanoate, 3-hydroxyundecanoate, 3-hydroxydodecanoate, and combinations thereof. In addition, the at least one moiety may have the same or different numbers of repeating units.

[0089] The above polyhydroxyalkanoate may be a copolymer comprising 3-hydroxybutyrate units and 3-hydroxyhexanoate units as main constituent units.

[0090] The above polyhydroxyalkanoate may contain 3-hydroxybutyrate units in an amount of 80 mol% or more as a constituent component. The above polyhydroxyalkanoate may contain 3-hydroxybutyrate units in an amount of about 85 mol% or more.

[0091] The above polyhydroxyalkanoate may be a poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin or a poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) copolymer resin.

[0092] The above polyhydroxyalkanoate can be produced by a microorganism such as, for example, Alcaligenes eutrophus AC 32 strain, which has a PHA synthase gene derived from Aeromonas caviae introduced into Alcaligenes eutrophus (international deposit under the Budapest Treaty, international depositary authority: National Institute of Advanced Industrial Science and Technology, Patent Organism Depositary Center (Central 6, 1-1 Higashi 1-chome, Tsukuba-shi, Ibaraki Prefecture, Japan), original deposit date: August 12, 1996, transferred on August 7, 1997, deposit number FERM BP-6038 (transferred from original deposit FERM P-15786)) (J. Bacteriol., 179, 4821 (1997)).

[0093] The above polyhydroxyalkanoate can be obtained as a commercial product. Commercial products of the above polyhydroxyalkanoate include Danimer's "NODAX", Tianan biopolymer's "ENMAT", CJ CheilJedang's "PHACT", Kaneka's "Aonilex (registered trademark) X131N", "Aonilex (registered trademark) X131A", "Aonilex (registered trademark) 151A", "Aonilex (registered trademark) 151C", "PHBH (registered trademark) X331N", "PHBH (registered trademark) X131A", "PHBH (registered trademark) 151A", or "PHBH (registered trademark) 151C".

[0094] The content of the biodegradable resin may be 90 wt% or less, 89 wt% or less, 88 wt% or less, 87 wt% or less, 86 wt% or less, 85 wt% or less, 80 wt% or less, 70 wt% or less, 10 wt% or more to 90 wt% or less, 20 wt% or more to 90 wt% or less, 30 wt% or more to 90 wt% or less, 40 wt% or more to 80 wt% or less, 40 wt% or more to 70 wt% or less, or 45 wt% or more to 70 wt% or less, based on the total weight of the biodegradable resin composition. When the above range is satisfied, water resistance can be significantly improved without deterioration of mechanical properties.

[0095]

[0096] The biodegradable resin composition includes light-blocking particles. The light-blocking particles may include carbon black. The light-blocking particles can block ultraviolet rays and function as a peroxide decomposition and radical quencher.

[0097] The content of the above-mentioned light-blocking particles may be 0.1 wt% to 10.0 wt%, 0.1 wt% to 8.0 wt%, 0.1 wt% to 6.0 wt%, 0.1 wt% to 5.0 wt%, or 0.1 wt% to 4.0 wt%, based on the total weight of the biodegradable resin composition. When the above range is satisfied, the decrease in tensile strength and elongation due to the influence of ultraviolet rays can be minimized without decreasing biodegradability.

[0098] The average diameter of the above light-shielding particles may be 10 nm to 500 nm, 20 nm to 500 nm, 20 nm to 400 nm, 20 nm to 300 nm, 20 nm to 250 nm, or 20 nm to 200 nm. The above light-shielding particles may have a pH of 3 to 10, 3.5 to 10, 4 to 10, 4.5 to 10, 4.5 to 9.5, 5 to 9.5, or 5 to 9 at a temperature of 25°C. When the above range is satisfied, the dispersing power within the biodegradable resin composition is excellent, thereby minimizing deterioration of mechanical properties due to the influence of ultraviolet rays.

[0099] The BET surface area of ​​the above-mentioned light-shielding particles is 100 m 2 / g to 700 m 2 / g, 150 m 2 / g to 700 m 2 / g, 200 m 2 / g to 700 m 2 / g, 250 m 2 / g to 700 m 2 / g, or 250 m 2 / g to 650 m 2 / g. The specific gravity of the above light-shielding particles may be 1.0 to 2.5, 1.3 to 2.5, 1.5 to 2.5, 1.5 to 2.3, 1.5 to 2.1, or 1.7 to 2.1. When the above range is satisfied, the dispersing power within the biodegradable resin composition is good, and the smoothness of the biodegradable molded product manufactured from the biodegradable resin composition can be improved.

[0100] The above-mentioned light-shielding particles may have a moisture absorption rate of 0.01% to 2.00%, 0.01% to 1.80%, 0.01% to 1.60%, 0.01% to 1.40%, 0.01% to 1.20%, or 0.01% to 1.00% at a temperature of 25°C, a relative humidity of 90%, and after 120 hours. The moisture absorption rate may be measured according to the following calculation formula 1 by measuring the initial weight of carbon black, storing the carbon black for 120 hours under conditions of a temperature of 25°C and a relative humidity of 90%, and measuring the weight increase of the carbon black.

[0101] [Calculation Formula 1]

[0102] Moisture absorption rate (%) = [Weight increase of the carbon black (based on 25°C temperature, 90% relative humidity, and 120 hours) / Initial weight of the carbon black] × 100

[0103] When the above range is satisfied, ultraviolet rays can be blocked while water resistance can be improved.

[0104] The surface of the above-described light-shielding particle may be modified. The surface of the above-described light-shielding particle may be imparted with hydrophobic properties by a surface modifier. The surface modifier may include an amine compound having 5 to 20 carbon atoms. The light-shielding particle with the modified surface may have an increased repulsive force with respect to water, thereby reducing moisture absorption, and thus the biodegradable resin composition including the light-shielding particle may have improved water resistance.

[0105]

[0106] The above biodegradable resin composition comprises an inorganic filler.

[0107] The content of the inorganic filler is 10 wt% or more, 20 wt% or more, 30 wt% or more, 35 wt% or more, 40 wt% or more, 45 wt% or more, 50 wt% or more, 55 wt% or more, 60 wt% or more, 65 wt% or more, 70 wt% or more, 75 wt% or more, 80 wt% or more, 10 wt% or more to 90 wt% or less, 20 wt% or more to 90 wt% or less, 30 wt% or more to 90 wt% or less, 30 wt% or more to 85 wt% or less, 30 wt% or more to 80 wt% or less, 30 wt% or more to 75 wt% or less, 30 wt% or more to 70 wt% or less, 35 wt% or more to 85 wt% or less, 35 wt% or more to 80 wt% or less, or 35 wt% or more to It can be 75 wt% or less. When the above range is satisfied, production costs can be reduced, biodegradability and water resistance can be improved by increasing the biodegradation starting point, and the physical properties of the molded product can be improved by preventing the dispersibility of inorganic fillers from decreasing. In addition, since the specific gravity of the biodegradable molded product does not increase significantly, it can be used in a wider variety of products, and the product's elongation and strength can be maintained, ensuring product reliability.

[0108] The specific surface area of ​​the above inorganic filler is 0.1 m 2 / g to 10.0 m 2 / g, 0.1 m 2 / g to 9.0 m 2 / g, 0.1 m 2 / g to 8.0 m 2 / g, 0.1 m 2 / g to 7.0 m 2 / g, 0.1 m 2 / g to 6.0 m 2 / g, 0.1 m 2 / g to 5.0 m 2 / g, 0.1 m 2 / g to 4.0 m 2 / g, or 0.1 m 2 / g to 3.0 m 2 / g. The above specific surface area can be measured by a nitrogen gas adsorption method. When the above range is satisfied, it can be easily dispersed in a biodegradable resin, thereby promoting the biodegradability of the biodegradable resin and improving processability.

[0109] The average particle diameter of the above-mentioned inorganic filler may be 0.1 ㎛ to 10.0 ㎛, 0.1 ㎛ to 9.0 ㎛, 0.1 ㎛ to 8.0 ㎛, 0.1 ㎛ to 7.0 ㎛, 0.1 ㎛ to 6.0 ㎛, 0.1 ㎛ to 5.0 ㎛, 0.1 ㎛ to 4.0 ㎛, 0.1 ㎛ to 3.0 ㎛, 1.0 ㎛ to 5.0 ㎛, 1.0 ㎛ to 4.0 ㎛, or 1.0 ㎛ to 3.0 ㎛. The above-mentioned average particle diameter can be calculated from the measurement results of the specific surface area by the air permeation method using a specific surface area measuring device. When the above range is satisfied, an increase in viscosity may not occur when mixing the biodegradable resin and the inorganic filler, and the uniformity of the particle size may be improved.

[0110] The sphericity of the above-mentioned inorganic filler may be 0.30 to 0.95, 0.30 to 0.93, 0.30 to 0.90, 0.50 to 0.95, 0.50 to 0.93, 0.50 to 0.90, 0.60 to 0.95, 0.60 to 0.93, or 0.60 to 0.90. When the above range is satisfied, a large number of fine pores generated at the interface between the biodegradable resin and the inorganic filler may be included, thereby improving biodegradability and increasing the strength and molding processability of the molded product.

[0111] The above-mentioned inorganic filler may include calcium carbonate (CaCO3). Generally, molded articles manufactured from biodegradable resin compositions may generate acid components during biodegradation. The acid components may react with the calcium carbonate to generate CO2 and H2O, thereby further enhancing the biodegradation rate of the molded article at the molecular level. Furthermore, the calcium carbonate can neutralize the acid components, thereby reducing environmental impact and preventing soil acidification.

[0112] The above calcium carbonate may be heavy calcium carbonate obtained by mechanically crushing or classifying natural calcium carbonate containing CaCO3 as its main component, such as limestone, chalk, marble, shells, and coral.

[0113] The above calcium carbonate may be surface-treated with an organic acid. By surface-treating the calcium carbonate with the organic acid, the dispersibility within the biodegradable resin composition may be increased, and the reactivity with the biodegradable resin may be improved. The surface treatment may be performed by a physical method such as plasma treatment or corona treatment, or a chemical method such as a silane coupling agent, a titanium coupling agent, or a surfactant. The organic acid may include a higher fatty acid, a higher fatty acid ester, a higher fatty acid amide, a higher fatty acid, and the like, and may be, for example, calcium stearate.

[0114] The above surface-treated calcium carbonate can be manufactured by the following method.

[0115] First, calcium carbonate powder can be produced through a grinding process. Thereafter, the calcium carbonate powder can be classified to obtain calcium carbonate having a desired particle size.

[0116] Thereafter, the calcium carbonate can be heat treated at about 200°C to about 800°C by a heating device selected from a kiln, an electric furnace, or a microwave. The heat treatment time can be about 5 minutes to about 30 minutes, about 7 minutes to about 15 minutes, or about 7 minutes to about 14 minutes. The heat treatment temperature can be about 250°C to about 700°C or about 300°C to about 600°C. By heat treating the calcium carbonate under the above conditions, moisture within the calcium carbonate can be easily removed, the organic acid can be easily bound to the surface of the calcium carbonate, and agglomeration of the calcium carbonate can be minimized.

[0117] Thereafter, an organic acid may be added to the heat-treated calcium carbonate to perform a process of treating the surface of the calcium carbonate. The process temperature may be 70°C to about 130°C. The amount of the organic acid added may be about 0.5 parts by weight to about 5 parts by weight, about 0.5 parts by weight to about 4 parts by weight, about 0.5 parts by weight to about 3 parts by weight, about 0.5 parts by weight to about 2 parts by weight, about 0.6 parts by weight to about 5 parts by weight, about 0.6 parts by weight to about 4 parts by weight, about 0.6 parts by weight to about 3 parts by weight, about 0.6 parts by weight to about 2 parts by weight, about 0.7 parts by weight to about 5 parts by weight, about 0.7 parts by weight to about 4 parts by weight, about 0.7 parts by weight to about 3 parts by weight, or about 0.7 parts by weight to about 2 parts by weight, based on 100 parts by weight of the calcium carbonate. The process time may be from about 1 minute to about 60 minutes, from about 10 minutes to about 30 minutes, or from about 5 minutes to about 20 minutes.

[0118] Thereafter, the surface-treated calcium carbonate may undergo an additional process of crushing and classifying the aggregates aggregated in the surface treatment process. In the surface-treated calcium carbonate, the content of the organic acid may be about 0.1 wt% to about 3 wt%, about 0.1 wt% to about 2 wt%, about 0.1 wt% to about 1 wt%, about 0.2 wt% to about 3 wt%, about 0.2 wt% to about 2 wt%, about 0.2 wt% to about 1 wt%, about 0.3 wt% to about 3 wt%, about 0.3 wt% to about 2 wt%, or about 0.3 wt% to about 1 wt%, based on the total weight.

[0119] The above-mentioned calcium carbonate surface-treated with an organic acid may be partially oxidized. The above-mentioned surface-treated calcium carbonate may partially include calcium oxide (CaO). The proportion of the calcium oxide may be 5% by volume or less, 4% by volume or less, 3% by volume or less, 2% by volume or less, 1% by volume or less, 0.01% by volume or more to 5% by volume or less, 0.01% by volume or more to 4% by volume or less, 0.01% by volume or more to 3% by volume or less, 0.01% by volume or more to 2% by volume or less, or 0.01% by volume or more to 1% by volume, based on 100% by volume of the surface-treated calcium carbonate particles. The proportion of the calcium oxide may be measured by the EDTA (Ethylene diamine tetra acetic acid) titration method according to JIS R 9011. When the above range is satisfied, the uniformity of the surface of the calcium carbonate can be improved, and the phenomenon of organic acid being eluted from the surface of the calcium carbonate can be minimized, so that the water resistance can be improved.

[0120]

[0121] The biodegradable resin composition may further comprise a reinforcing material. The reinforcing material may be a fiber derived from biomass. The reinforcing material may comprise nanocellulose. The nanocellulose may be a natural material nanocellulose in the form of a gel or dry powder, and the dispersion stability, strength, and processability of the biodegradable resin comprising the nanocellulose may all be improved.

[0122] The diameter of the nanocellulose may be 1 nm to 100 nm, 1 nm to 95 nm, 5 nm to 90 nm, 10 nm to 80 nm, 5 nm to 60 nm, or 15 nm to 60 nm. The length of the nanocellulose may be 5 nm to 5 ㎛, 5 nm to 1 ㎛, 10 nm to 700 nm, 20 nm to 500 nm, 60 nm to 300 nm, 80 nm to 200 nm, or 100 nm to 250 nm. When the above ranges are satisfied, the strength and tear strength of the biodegradable resin composition may be further improved.

[0123] The nanocellulose may be in the form of a dry powder or gel having aggregated secondary particles rather than single particles, and the size of the secondary particles may be 1 μm to 50 μm, 2 μm to 45 μm, or 5 μm to 50 μm. The nanocellulose may be in the form of a freeze-dried powder to reduce the volume for easy storage and transportation.

[0124] The average particle size of the above nanocellulose may be 200 nm or less, 190 nm or less, or 185 nm or less, and the particle size deviation may be 20% or less, 18% or less, or 16% or less. When the above ranges are satisfied, the dispersibility and durability of the nanocellulose may be improved.

[0125] The above nanocellulose can perform a crystal nucleating function, thereby improving the crystallization speed of the biodegradable resin composition and increasing the crystallization temperature of the biodegradable resin composition. The nanocellulose may be at least one selected from the group consisting of cellulose nanocrystals, cellulose nanofibers, and microfibrillated cellulose. In terms of strength and thermal properties, the cellulose nanocrystals or the cellulose nanofibers are preferable.

[0126] The above nanocellulose can perform UV resistance function, thereby providing the biodegradable resin with appropriate UV resistance properties, biodegradation rate, and hydrolysis rate. The above nanocellulose may be at least one selected from the group consisting of hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropylmethyl cellulose, cellulose acetate, methyl cellulose, ethyl cellulose, propyl cellulose, butyl cellulose, pentyl cellulose, hexyl cellulose, and cyclohexyl cellulose.

[0127] The above nanocellulose may be bead mill pretreated or ultrasonically pretreated. The above nanocellulose may be water-dispersed nanocellulose that has been bead mill pretreated or ultrasonically pretreated.

[0128] The above nanocellulose may be obtained by dispersing cellulose nanocrystals in a dry powder or gel form having a particle size of 1 μm to 50 μm in water and then pretreating them with a bead mill or ultrasonic pretreatment. If the above nanocellulose dispersed in water is pretreated with a bead mill or ultrasonic pretreatment, the number of nanocellulose particles may increase and dispersibility may be maximized.

[0129] The above nanocellulose may be pretreated with a silane coupling agent in an amount of 0.01 to 10 wt%, 0.05 to 8 wt%, 0.1 to 8 wt%, 0.5 to 6 wt%, or 0.7 to 6 wt% based on the total weight of the nanocellulose. When the above range is satisfied, interfacial adhesion, dispersibility, and compatibility can be maximized, and thus the mechanical properties, durability, and hydrolysis resistance of the biodegradable resin composition including the same can be further improved.

[0130] The biodegradable resin may contain the nanocellulose in an amount of 0.01 to 3 wt%, 0.01 to 2.5 wt%, 0.05 to 2 wt%, 0.07 to 1.8 wt%, 0.1 to 1.2 wt%, 0.1 to 1 wt%, or 0.15 to 0.7 wt% based on the total weight of the biodegradable resin. When the above range is satisfied, the biodegradability and strength of the biodegradable resin composition may be further improved.

[0131]

[0132] The biodegradable resin composition may include an oligomer. The weight average molecular weight of the oligomer may be from about 400 g / mol to about 1,300 g / mol. The oligomer may be included in the biodegradable resin composition in an amount of from about 3,000 ppm to about 30,000 ppm, from about 5,000 ppm to about 20,000 ppm, or from about 5,000 ppm to about 15,000 ppm, based on the weight of the biodegradable resin. The oligomer may be a reaction product of at least two of the diol, the aromatic dicarboxylic acid, and the aliphatic dicarboxylic acid. The oligomer may be a reaction product of 1,4-butanediol, terephthalic acid, and adipic acid.

[0133]

[0134] The biodegradable resin composition may further include a plasticizer. The plasticizer may impart processability or flexibility to a molded article to be manufactured. The plasticizer may be glycerol, acrylate, glycerin, glycerol monostearate (GMS), sorbitol, or a mixture thereof. The plasticizer may be present in an amount of 0.1 wt% to 15 wt%, 0.1 wt% to 14 wt%, 0.1 wt% to 13 wt%, 0.1 wt% to 12 wt%, 0.1 wt% to 11 wt%, 0.1 wt% to 10 wt%, 0.1 wt% to 9 wt%, 0.1 wt% to 8 wt%, 0.1 wt% to 7 wt%, 0.1 wt% to 6 wt%, or 0.1 wt% to 5 wt%, based on the total weight of the biodegradable resin composition. When the above range is satisfied, the elongation and tearing strength of a molded product manufactured from the biodegradable resin composition can be improved.

[0135]

[0136] The biodegradable resin composition may further include an antioxidant. The antioxidant may include at least one selected from the group consisting of a phosphorus-based antioxidant, a phenol-based antioxidant, and a pentaerythritol-based antioxidant.

[0137] The above-mentioned phosphorus antioxidant may be at least one selected from the group consisting of triesters, diesters, monoesters of phosphorous acid, such as triphenyl phosphite, trisnonylphenyl phosphite, and tris(2,4-di-t-butylphenyl)phosphite, trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresyl phosphate, tris(nonylphenyl)phosphate, and 2-ethylphenyl diphenyl phosphate.

[0138] The above phenolic antioxidants are α-tocopherol, butylhydroxytoluene, sinapyl alcohol, vitamin E, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 2,6-di-t-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-t-butyl-4-hydroxybenzyl phosphonate diethyl ester, 2,2-bis(((3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoyl)oxy)methyl)propane-1,3-diyl It may be at least one selected from the group consisting of bis(3-(3,5-di-tert)-butyl-4-hydroxyphenyl)propanoate), pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxymethyl]methane.

[0139] The above antioxidant may further include at least one selected from the group consisting of BHT, ascorbic acid, catechin, quercetin, dodecyl gallate, TBHQ, Ralox, Irganox 1135, Irganox 1076, nordihydroguaiaretic acid, epicatechin gallate, epigallocatechin gallate, epigallocatein, propyl gallate, 2,3,5-trihydroxybutyrophenone, butylated hydroxyanisole, 4-hydroxymethyl-2,6-di-tert-butylphenol, α-tocopherol, resveratrol, rutin, astaxanthin, lycopene, beta-carotene, and melatonin.

[0140] The content of the antioxidant may be 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, 1.5 wt% or less, 1 wt% or less, 0.5 wt% or less, 0.3 wt% or less, 0 to 5 wt%, 0.01 to 4 wt%, 0.1 to 3 wt%, 1 to 3 wt%, 1 to 2 wt%, 0.01 to 0.3 wt%, 0.05 to 0.3 wt%, 0.15 to 0.3 wt%, or 0.2 to 0.3 wt%, based on the total weight of the biodegradable resin composition.

[0141] The above antioxidant may include both the phosphorus-based antioxidant and the phenol-based antioxidant. When the above antioxidant includes both the phosphorus-based antioxidant and the phenol-based antioxidant, the weight ratio of the phosphorus-based antioxidant and the phenol-based antioxidant may be 1:10 to 10:1, 1:5 to 5:1, 1:1 to 5:1, 2:1 to 4:1, 2.5:1 to 3.5:1, 1:5 to 1:1, 1:2 to 1:4, or 1:2.5 to 1:3.5. When the above range is satisfied, there is an effect of delaying the oxidation phenomenon of the biodegradable resin composition in various temperature ranges.

[0142]

[0143] The above biodegradable resin composition may include a heat stabilizer.

[0144] The heat stabilizer may be a phosphorus heat stabilizer. The heat stabilizer may include at least one selected from the group consisting of an amine-based high-temperature heat stabilizer such as tetraethylenepentaamine, triethylphosphonoacetate, phosphoric acid, phosphorous acid, polyphosphoric acid, trimethyl phosphate, triethyl phosphate, trimethylphosphine, and triphenylphosphine. The heat stabilizer may be an antioxidant having an antioxidant function. The content of the heat stabilizer may be 3,000 ppm or less, 10 ppm to 3,000 ppm, 20 ppm to 2,000 ppm, 20 ppm to 1,500 ppm, or 20 ppm to 1,000 ppm based on the total weight of the biodegradable resin.

[0145]

[0146] The above biodegradable resin composition may include an active agent.

[0147] The above-mentioned lubricant may include at least one selected from the group consisting of a fatty acid-based lubricant including stearic acid, an aliphatic alcohol-based lubricant, an aliphatic amide-based lubricant including stearamide, an aliphatic ester-based lubricant such as n-butyl stearate, methyl hydroxystearate, polyhydric alcohol fatty acid ester, saturated fatty acid ester, ester wax, and the like, and a fatty acid metal soap-based lubricant. Specifically, the lubricant may be a stearate-based lubricant, and may include at least one selected from the group consisting of calcium stearate, zinc stearate, barium stearate, magnesium stearate, glycerin stearate, and butyl stearate. The stearate-based lubricant reduces heat generation due to friction during mixing, melting, and processing of raw materials, has an excellent dispersing effect for biodegradable resins in terms of cost, and has an excellent lubricating effect, thereby improving manufacturing efficiency.

[0148] The content of the above-mentioned active agent may be 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, less than 1 wt%, 0.9 wt% or less, 0.8 wt% or less, 0.7 wt% or less, 0.5 wt% or less, 0.3 wt% or less, or 0.1 wt% or less, based on the total weight of the biodegradable resin composition. When the above range is satisfied, the manufacturing efficiency can be improved without deteriorating the physical properties of the biodegradable resin composition.

[0149]

[0150] The biodegradable resin composition may include a flame retardant. The flame retardant may include at least one selected from the group consisting of halogen-based flame retardants, phosphorus-based flame retardants, and non-phosphorus halogen-based flame retardants such as metal hydrates.

[0151] The above halogen-based flame retardant may include at least one selected from the group consisting of halogenated bisphenol-based compounds such as halogenated bisphenyl alkanes, halogenated bisphenyl ethers, halogenated bisphenyl thioethers, and halogenated bisphenyl sulfones, and bisphenol-bis(alkylether)-based compounds such as brominated bisphenol A, brominated bisphenol S, chlorinated bisphenol A, and chlorinated bisphenol S.

[0152] The above-mentioned phosphorus flame retardant may include at least one selected from the group consisting of tris(diethyl phosphinic acid)aluminum, bisphenol A bis(diphenyl phosphate), triaryl isopropyl phosphate, cresyl di-2,6-xylenyl phosphate, and aromatic condensed phosphate esters.

[0153] The metal hydrate may include aluminum trihydrate, magnesium dihydrate, or a combination thereof.

[0154] The above flame retardant may include at least one selected from the group consisting of antimony oxide, such as antimony trioxide or antimony pentoxide, zinc oxide, iron oxide, aluminum oxide, molybdenum oxide, titanium oxide, calcium oxide, and magnesium oxide, as a flame retardant additive to improve the flame retardant effect.

[0155]

[0156] The biodegradable resin composition may include a foaming agent. The foaming agent may be mixed into the molten biodegradable resin composition or injected under pressure, and may be a substance that changes phase from solid to gas, liquid to gas, or gas itself, and may be used to control the foaming ratio (foaming density) of the foam sheet.

[0157] The above-mentioned foaming agent may include at least one selected from the group consisting of aliphatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, inorganic gases, and water.

[0158]

[0159] The biodegradable resin composition may include a dispersant. The dispersant may improve the dispersibility of solvents and solutes. The dispersant may include at least one selected from the group consisting of aliphatic polyester, polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoate.

[0160] The dispersant may be included in an amount of 1 to 20 wt%, 1 to 15 wt%, 1 to 13 wt%, 1 to 11 wt%, 2 to 10 wt%, 5 to 15 wt%, 7 to 12 wt%, 2 to 8 wt%, 5 to 8 wt%, or 2 to 5 wt% based on the total weight of the biodegradable resin composition.

[0161]

[0162] The biodegradable resin composition may include a chain extender. The chain extender may include at least one selected from the group consisting of aromatic diisocyanates, aliphatic diisocyanates, isocyanurates, bisoxazolines, carboxylic anhydrides, and epoxides.

[0163] The above aromatic diisocyanate may include at least one selected from the group consisting of tolylene 2,4-diisocyanate, tolylene 2,6-diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, naphthylene 1,5-diisocyanate, and xylylene diisocyanate.

[0164] The above aliphatic diisocyanate may include at least one selected from the group consisting of 1,6-hexamethylene diisocyanate, isophorone diisocyanate, and methylenebis(4-isocyanatocyclohexane).

[0165] The above isocyanurate may include isophorone diisocyanate or methylenebis(4-isocyanatocyclohexane).

[0166] The above bisoxazoline may include at least one selected from the group consisting of 2,2'-bis(2-oxazoline), bis(2-oxazolinyl)methane, 1,2-bis(2-oxazolinyl)ethane, 1,3-bis(2-oxazolinyl)propane, and 1,4-bis(2-oxazolinyl)butane.

[0167] The above epoxide means an epoxy-containing copolymer based on at least one of styrene, acrylic acid ester and methacrylic acid ester, and a copolymer having a copolymer content of more than 20, more than 30, or more than 50 wt% having glycidyl (meth)acrylate is preferred.

[0168] The chain extender may be 1.5 wt% or less, 1.4 wt% or less, 1.3 wt% or less, 1.2 wt% or less, 1.1 wt% or less, 1 wt% or less, 0.9 wt% or less, 0.8 wt% or less, 0.7 wt% or less, 0.6 wt% or less, 0.5 wt% or less, 0.4 wt% or less, 0.3 wt% or less, and may be 0 wt% to 1.5 wt%, 0.01 wt% to 1.5 wt%, 0.1 wt% to 1.5 wt%, 0.1 wt% to 1.0 wt%, 0.1 wt% to 0.9 wt%, 0.1 wt% to 0.8 wt%, 0.1 wt% to 0.7 wt%, 0.1 wt% to 0.6 wt%, or 0.1 wt% to 0.5 It can be a weight %.

[0169]

[0170] The above biodegradable resin composition has an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method.

[0171] [measurement method]

[0172] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C.

[0173] 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm.

[0174] 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine).

[0175] 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine).

[0176] 6) Calculate the elongation retention rate (ΔE) using Equation 1 below.

[0177] [Formula 1]

[0178] ΔE(%) = (E1 / E0) X 100

[0179] The above elongation retention rate may be an indicator of the resistance of the biodegradable resin composition to ultraviolet rays. For example, the mechanical properties of the biodegradable resin composition may be deteriorated by ultraviolet rays. In particular, as the amount of exposure of the biodegradable resin composition to ultraviolet rays increases, the elongation may be significantly reduced. That is, as the elongation retention rate (ΔE), which is calculated as the ratio of the second elongation (E1) to the first elongation (E0), decreases, it may mean that the resistance of the biodegradable resin composition to ultraviolet rays decreases.

[0180] Preferably, the biodegradable resin composition may have an elongation retention rate measured by the above measurement method of 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, 50% or more, 20% to 95% or less, or 20% to 90% or less. Conventionally, biodegradable resin compositions with high biodegradability have been used to manufacture eco-friendly products, but their low resistance to ultraviolet rays has made it difficult to apply them to product fields requiring long-term durability. Accordingly, the present invention provides a biodegradable resin composition having a high biodegradability and improved resistance to ultraviolet rays when the elongation retention rate measured by the above measurement method satisfies the above range, so that the manufactured biodegradable molded product can be easily decomposed when discarded, and can also appropriately maintain mechanical strength during a general use period.

[0181] The first elongation of the biodegradable resin composition may be 150% to 400%, 160% to 400%, 160% to 380%, 160% to 360%, or 190% to 345%. The second elongation of the biodegradable resin composition may be 100% to 300%, 110% to 300%, 120% to 300%, 150% to 300%, or 150% to 250%. When the above ranges are satisfied, the ultraviolet resistance, mechanical properties, and water resistance of the biodegradable resin composition may be improved.

[0182]

[0183] The biodegradable resin composition may include a hydrolysis inhibitor. The hydrolysis inhibitor may be two types of hydrolysis inhibitors having different weight average molecular weights. When the weight average molecular weight (Mw) of the hydrolysis inhibitor is large, volatility may be low and hydrolysis resistance may be improved. When the weight average molecular weight (Mw) of the hydrolysis inhibitor is small, compatibility with the biodegradable resin may be increased.

[0184] In order to increase compatibility with a biodegradable resin, one hydrolysis inhibitor having a weight average molecular weight (Mw) of 10,000 g / mol or less, 9,000 g / mol or less, 8,000 g / mol or less, 7,000 g / mol or less, 6,000 g / mol or less, or 5,000 g / mol or less can be used, and in order to lower volatility and improve hydrolysis resistance, one hydrolysis inhibitor having a weight average molecular weight of 10,000 g / mol or more, 20,000 g / mol or more, 30,000 g / mol or more, 40,000 g / mol or more, or 50,000 g / mol or more can be used. The weight average molecular weight can be measured as a relative value to a standard PS (standard polystyrene) sample through GPC using THF as an eluent. When the above range is satisfied, the mechanical properties and hydrolysis resistance of the biodegradable resin composition can be improved.

[0185] The above hydrolysis inhibitor may include a carbodiimide-based compound. The carbodiimide-based compound may be a monomer or a polymer. The carbodiimide-based compound may react with moisture and acid to convert into a urea structure, thereby reducing the reactivity between moisture and acid and the ester group contained in the biodegradable resin. As a result, the phenomenon of the biodegradable resin being hydrolyzed by moisture and acid may be reduced, and consequently, the hydrolysis resistance of the biodegradable resin composition may be improved.

[0186] The above carbodiimide compound may include a compound represented by the following chemical formula 4.

[0187] [Chemical Formula 4]

[0188]

[0189] In the above chemical formula 4, n is an integer from 1 to 20.

[0190] The above carbodiimide compounds are N,N'-di-o-tolylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-dioctyldecylcarbodiimide, N,N'-di-2,6-diketylphenylcarbodiimide, N-tolyl-N'cyclohexylcarbodiimide, N,N'-di-2,6-diisopropylphenylcarbodiimide, N,N'-di-2,6-di-tert-butylphenylcarbodiimide, N-tolyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, It may be at least one selected from the group consisting of N,N'-di-p-tolylcarbodiimide, p-phenylene-bis-di-o-tolylcarbodiimide, p-phenylene-bisdicyclohexylcarbodiimide, hexamethylene-bisdicyclohexylcarbodiimide, ethylene-bisdiphenylcarbodiimide, and copolymers of benzene-2,4-diisocyanato-1,3,5-tris(1-methylethyl) homopolymer, 2,4-diisocyanato-1,3,5-tris(1-methylethyl) and 2,6-diisopropyl diisocyanate.

[0191] The weight average molecular weight (Mw) of the above carbodiimide compound may be 500 g / mol to 50,000 g / mol, 600 g / mol to 50,000 g / mol, 700 g / mol to 50,000 g / mol, 800 g / mol to 50,000 g / mol, 900 g / mol to 50,000 g / mol, 1,000 g / mol to 50,000 g / mol, 1,000 g / mol to 40,000 g / mol, or 1,000 g / mol to 30,000 g / mol.

[0192] In the above carbodiimide-based compound, the content of the NCN group may be 1 wt% to 20 wt%, 1 wt% to 19 wt%, 1 wt% to 18 wt%, 1 wt% to 17 wt%, 1 wt% to 16 wt%, 1 wt% to 15 wt%, 2 wt% to 15 wt%, 3 wt% to 15 wt%, 4 wt% to 15 wt%, 5 wt% to 15 wt%, or 6 wt% to 15 wt%. The content of the NCN group in the carbodiimide-based compound can be measured by titration with oxalic acid. When the above range is satisfied, compatibility with a biodegradable resin is not reduced, and the water resistance of the biodegradable resin composition can be improved.

[0193] The content of the hydrolysis inhibitor may be 0.1 wt% to 5.0 wt%, 0.1 wt% to 4.0 wt%, 0.1 wt% to 3.0 wt%, 0.1 wt% to 2.0 wt%, 0.1 wt% to 1.5 wt%, or 0.1 wt% to 1.0 wt% based on the total weight of the biodegradable resin composition. When the above range is satisfied, the hydrolysis resistance and odor reduction effect of the biodegradable resin composition may be improved.

[0194] The biodegradable resin composition may contain a compound containing a urea group in an amount of 0.01 wt% to 10.00 wt%, 0.01 wt% to 9.00 wt%, 0.01 wt% to 8.00 wt%, 0.01 wt% to 7.00 wt%, 0.01 wt% to 6.00 wt%, 0.01 wt% to 5.00 wt%, 0.01 wt% to 4.00 wt%, or 0.01 wt% to 3.00 wt%, based on the total weight of the biodegradable resin composition. When the above range is satisfied, the proportion of the ester group contained in the biodegradable resin that can react with moisture or acid is reduced, so that water resistance can be improved.

[0195]

[0196] The biodegradable resin composition may include a UV stabilizer. The UV stabilizer absorbs ultraviolet rays, thereby inhibiting photooxidation caused by ultraviolet rays. The content of the UV stabilizer may be 0.1 wt% to 5.0 wt%, 0.1 wt% to 4.0 wt%, 0.1 wt% to 3.0 wt%, 0.1 wt% to 2.0 wt%, or 0.1 wt% to 1.0 wt%, based on the total weight of the biodegradable resin composition. The weight average molecular weight (Mw) of the UV stabilizer may be 100 g / mol to 10,000 g / mol, 100 g / mol to 5,000 g / mol, 100 g / mol to 3,000 g / mol, 100 g / mol to 1,000 g / mol, 100 g / mol to 800 g / mol, or 200 g / mol to 800 g / mol. The melting point of the UV stabilizer may be 50°C or higher, 80°C or higher, 100°C or higher, 150°C or higher, or 150°C or higher to 230°C or lower. When the above range is satisfied, the decrease in tensile strength and elongation due to the influence of ultraviolet rays can be minimized without decreasing biodegradability.

[0197] The above UV stabilizer may include at least one selected from the group consisting of benzotriazole derivatives, hydroxybenzophenone, hydroxyphenyltrizine, and esters of substituted or unsubstituted benzoic acid.

[0198] Specifically, the UV stabilizer may include a compound represented by the following chemical formula 5.

[0199] [Chemical Formula 5]

[0200]

[0201] In the above chemical formula 5, R1 and R2 are each independently a substituted or unsubstituted alkyl having 1 to 20 carbon atoms.

[0202]

[0203] <Biodegradable molded products>

[0204] A biodegradable molded article according to the present invention can be manufactured from the biodegradable resin composition. The biodegradable molded article can be manufactured by molding the biodegradable resin composition by a method known in the art, such as extrusion or injection molding, and the molded article can be a non-woven fabric, a vacuum-formed sheet, a blown molded article, or an injection molded article, but is not limited thereto. For example, the biodegradable molded article can be an agricultural mulching film, disposable gloves, food packaging material, a fabric, a knitted fabric, a non-woven fabric, a rope, or a food packaging container. Since the biodegradable molded article can be manufactured from a biodegradable resin composition having excellent UV resistance, mechanical properties, and water resistance, it can exhibit excellent properties when applied to packaging materials and mulching films that require dimensional stability against moisture, etc. in an external environment.

[0205] The above biodegradable molded article comprises a biodegradable resin composition comprising a biodegradable resin, light-shielding particles, and an inorganic filler, and having an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method. The biodegradable resin, light-shielding particles, and inorganic filler may be the same as the biodegradable resin, light-shielding particles, and inorganic filler in the above-described biodegradable resin composition.

[0206] [measurement method]

[0207] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C.

[0208] 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm.

[0209] 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine).

[0210] 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine).

[0211] 6) Calculate the elongation retention rate (ΔE) using Equation 1 below.

[0212] [Formula 1]

[0213] ΔE(%) = (E1 / E0) X 100

[0214] Preferably, the biodegradable resin composition may have an elongation retention rate measured by the above measurement method of 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, 50% or more, 20% or more to 95% or less, or 20% or more to 90% or less. When the above ranges are satisfied, the ultraviolet resistance, mechanical properties, and water resistance of the biodegradable molded product may be improved.

[0215] The biodegradable resin composition included in the biodegradable molded product may include a hydrolysis inhibitor. The hydrolysis inhibitor may include a carbodiimide-based compound. The carbodiimide-based compound may be a monomer or a polymer.

[0216] The above carbodiimide compound may include a compound represented by the following chemical formula 4.

[0217] [Chemical Formula 4]

[0218]

[0219] In the above chemical formula 4, n is an integer from 1 to 20.

[0220] The above biodegradable molded product may have an odor grade of 3 or lower according to MS300-34. Specifically, the biodegradable resin composition may be cut according to the MS300-34 standard, manufactured into a sample, and then smelled to determine the odor grade from 1 to 6, with a lower odor grade indicating better odor characteristics. When the grade or lower is satisfied, water resistance is improved and odor is reduced, enabling productization in a wider range of fields compared to conventional biodegradable molded products, and product reliability may be improved.

[0221]

[0222] The biodegradable molded product may be a biodegradable film. The thickness of the biodegradable film may be 5 ㎛ to 500 ㎛, 5 ㎛ to 400 ㎛, 5 ㎛ to 350 ㎛, 10 ㎛ to 350 ㎛, 10 ㎛ to 300 ㎛, 10 ㎛ to 250 ㎛, 10 ㎛ to 200 ㎛, 10 ㎛ to 150 ㎛, 10 ㎛ to 100 ㎛, or 10 ㎛ to 90 ㎛. The tensile strength of the biodegradable film may be 1.00 kgf / mm. 2 Above, 1.50 kgf / mm 2 Above, 1.70 kgf / mm 2 Above, 1.80 kgf / mm 2 Above, 1.90 kgf / mm 2 or 2.00 kgf / mm 2 This may be ideal. When the above range is satisfied, the film is not easily torn, has excellent mechanical properties, and can be easily decomposed when the biodegradable molded product is disposed of.

[0223] The elongation of the biodegradable film may be 85% or more, 90% or more, 95% or more, 1,000% or less, 950% or less, 900% or less, or 850% or less. This ensures the elasticity of the biodegradable molded product, enabling it to withstand a certain load.

[0224]

[0225] The biodegradable molded product may be a biodegradable sheet. The thickness of the biodegradable sheet may be 5 ㎛ to 1,000 ㎛, 10 ㎛ to 1,000 ㎛, 15 ㎛ to 1,000 ㎛, 20 ㎛ to 1,000 ㎛, 25 ㎛ to 1,000 ㎛, 30 ㎛ to 1,000 ㎛, 35 ㎛ to 1,000 ㎛, or 40 ㎛ to 1,000 ㎛. The tensile strength of the biodegradable sheet may be 1.00 kgf / mm. 2 Above, 1.50 kgf / mm 2 Above, 1.70 kgf / mm 2 Above, 1.80 kgf / mm 2 Above, 1.90 kgf / mm 2 or 2.00 kgf / mm 2 The tear strength of the biodegradable sheet may be 100 N / cm or more, 110 N / cm or more, 120 N / cm or more, 130 N / cm or more, 140 N / cm or more, 150 N / cm or more, 700 N / cm or less, 650 N / cm or less, 600 N / cm or less, 550 N / cm or less, or 500 N / cm or less. When the above range is satisfied, the sheet is not easily torn, and can be easily decomposed when the biodegradable molded product is disposed of.

[0226] The elongation of the above biodegradable sheet may be 10% or more, 15% or more, 20% or more, 50% or less, 70% or more, 700% or less, 650% or less, 550% or less, 500% or less, or 450% or less. When the above range is satisfied, the elasticity of the biodegradable molded product can be secured, so that it can withstand a certain load.

[0227]

[0228] <Method for manufacturing biodegradable molded products>

[0229] The method for manufacturing a biodegradable molded product according to the present invention may include (a) a step of manufacturing a prepolymer by esterifying a diol component and a dicarboxylic acid component, (b) a step of manufacturing a biodegradable resin by polycondensation of the prepolymer, (c) a step of manufacturing a biodegradable resin composition by mixing the biodegradable resin, light-blocking particles, and inorganic filler, (d) a step of manufacturing pellets from the biodegradable resin composition, and (e) a step of drying and melt-extruding the pellets.

[0230]

[0231] The above manufacturing method may include a step of (a) producing a prepolymer by subjecting a diol component and a dicarboxylic acid component to an esterification reaction.

[0232] The above diol component and the above dicarboxylic acid component may be the same as the diol component and the dicarboxylic acid component in the biodegradable resin composition described above. The step (a) may be prepared by producing a composition comprising the diol component, the dicarboxylic acid component, and optionally the nanocellulose through a one-step esterification reaction or a two-step esterification reaction through a first esterification reaction and a second esterification reaction.

[0233] The above two-step esterification reaction may include a step (a-1) of subjecting the diol component and the dicarboxylic acid component to a first esterification reaction, and a step (a-2) of adding the diol component and the dicarboxylic acid component to the reaction product of the step (a-1) and subjecting the diol component and the dicarboxylic acid component to a second esterification reaction.

[0234] When the biodegradable resin comprises nanocellulose, the binding strength of the nanocellulose can be improved by introducing the nanocellulose in the second esterification reaction step. In addition, the binding strength of the nanocellulose can be further improved by introducing water-dispersed nanocellulose in the second esterification reaction step.

[0235] The above nanocellulose can be introduced at a temperature of 100°C to 160°C, 110°C to 140°C, or 110°C to 150°C. When the above range is satisfied, solvent resistance can be improved.

[0236] The above nanocellulose can be introduced at a rate of 2 kg / min to 10 kg / min, 2.5 kg / min to 9.5 kg / min, or 3 kg / min to 8 kg / min. When the above range is satisfied, the efficiency of the manufacturing process can be improved without causing re-agglomeration of the nanocellulose.

[0237] In the above step (a), a titanium catalyst, a germanium catalyst, an antimony catalyst, an additive, and a stabilizer may be added before the esterification reaction. The esterification reaction may be performed at a temperature range of 250°C or less, 240°C or less, 235°C or less, 180°C to 250°C, 185°C to 240°C, or 180°C to 240°C for 0.5 to 5 hours, 0.5 to 4.5 hours, 0.5 to 3.5 hours, or 1 to 3 hours, respectively. The esterification reaction may be performed at atmospheric pressure until the byproducts, water and methanol, theoretically reach 90%.

[0238] The number average molecular weight of the above prepolymer may be 500 g / mol to 10,000 g / mol, 500 g / mol to 8,500 g / mol, 500 g / mol to 7,000 g / mol, 1,000 g / mol to 6,000 g / mol, or 2,500 g / mol to 5,500 g / mol. The number average molecular weight can be measured by gel permeation chromatography (GPC). When the above range is satisfied, the molecular weight of the prepolymer can be efficiently increased in the polycondensation reaction, thereby improving the strength properties.

[0239]

[0240] The above manufacturing method may include a step (b) of manufacturing a biodegradable resin by subjecting the prepolymer to a polycondensation reaction.

[0241] The above polycondensation reaction can be carried out at a temperature range of 180°C to 280°C, 190°C to 270°C, 210°C to 260°C, or 230°C to 255°C, at a pressure range of 1.0 Torr or less, 0.9 Torr or less, 0.7 Torr or less, 0.2 Torr to 1.0 Torr, 0.3 Torr to 0.9 Torr, or 0.5 Torr to 0.9 Torr, for 1 hour to 6 hours, 1.5 hours to 5.5 hours, 2 hours to 5 hours, or 3.5 hours to 4.5 hours.

[0242] The inherent viscosity of the biodegradable resin manufactured in the above step (b) may be 0.05 to 10 dL / gr. The melt viscosity of the biodegradable resin may be 100 s -1When measured with a rheometrics dynamic spectrometer (RDS) under conditions, it can be 1,000 to 30,000 poise. The number average molecular weight (Mn) of the biodegradable resin can be 40,000 g / mol or more, 43,000 g / mol or more, 45,000 g / mol or more, or 40,000 g / mol to 70,000 g / mol. The weight average molecular weight (Mw) of the biodegradable resin can be 60,000 g / mol or more, 65,000 g / mol or more, 75,000 g / mol or more, 80,000 g / mol or more, or 85,000 g / mol to 100,000 g / mol. The polydispersity index (PDI) of the biodegradable resin may be 1.2 to 2.0, 1.5 to 1.9, or 1.6 to 1.8. When the number average molecular weight, weight average molecular weight, or polydispersity index of the biodegradable resin satisfies the above ranges, the strength and processability may be further improved. The acid value of the biodegradable resin may be 1.8 mgKOH / g or less, 1.5 mgKOH / g or less, 1.3 mgKOH / g or less, or 1.25 mgKOH / g or less. When the above ranges are satisfied, the solvent resistance may be improved.

[0243]

[0244] The above manufacturing method may include a step (c) of manufacturing a biodegradable resin composition by mixing the biodegradable resin, light-blocking particles, and inorganic filler.

[0245] The above mixing can be appropriately set according to the molding method. For example, the biodegradable resin, shading particles, and inorganic filler can be mixed and melted before being fed into the molding machine from the hopper, or the biodegradable resin, shading particles, and inorganic filler can be mixed and melted simultaneously with the molding machine. The mixing is preferably performed by uniformly dispersing the shading particles and inorganic filler in the biodegradable resin while applying high shear stress. Specifically, mixing is preferably performed using a kneader reactor, an extrusion molding machine equipped with a single screw, or a twin-screw mixer. If necessary, step (c) may additionally add one or more of the plasticizer or the additive.

[0246] The step (c) may include one or more mixing steps. In the case of a single mixing step, it may be a single mixing step for producing a biodegradable resin composition comprising 60 to 80 wt%, 61 to 80 wt%, 62 to 80 wt%, 63 to 80 wt%, 64 to 80 wt%, 65 to 80 wt%, 60 to 75 wt%, 61 to 75 wt%, 62 to 75 wt%, 63 to 75 wt%, 64 to 75 wt%, 65 to 75 wt%, or 65 to 72 wt% of the inorganic filler based on the total weight of the biodegradable resin composition. In the case of a two-stage mixing step, a first mixing step for producing a biodegradable resin composition comprising 60 to 80 wt%, 61 to 80 wt%, 62 to 80 wt%, 63 to 80 wt%, 64 to 80 wt%, 65 to 80 wt%, 60 to 75 wt%, 61 to 75 wt%, 62 to 75 wt%, 63 to 75 wt%, 64 to 75 wt%, 65 to 75 wt%, or 65 to 72 wt% of the inorganic filler based on the total weight of the biodegradable resin composition, and 30 to 85 wt%, 30 to 80 wt%, 30 to 75 wt%, 30 to 70 wt%, 35 to 85 wt%, 35 to 80 wt%, A second mixing step may be included to prepare a biodegradable resin composition comprising 35 to 75 wt%, 35 to 70 wt%, 40 to 85 wt%, 40 to 80 wt%, 40 to 75 wt%, 40 to 70 wt%, 45 to 85 wt%, 45 to 80 wt%, 45 to 75 wt%, 45 to 70 wt%, 50 to 85 wt%, 50 to 80 wt%, 50 to 75 wt%, or 50 to 70 wt%.

[0247] The above one or more mixing steps may be a tandem continuous process. The temperature of the mixing step may be 150 to 190°C, 150 to 180°C, or 160 to 180°C. When the above ranges are satisfied, the phenomenon of torque increasing in the mixing step and the phenomenon of thermal decomposition of the mixed biodegradable resin composition can be reduced.

[0248] The step (c) above may include adding a hydrolysis inhibitor. The hydrolysis inhibitor may be added in an amount of 0.1 wt% to 5.0 wt%, 0.1 wt% to 4.0 wt%, 0.1 wt% to 3.0 wt%, 0.1 wt% to 2.0 wt%, 0.1 wt% to 1.5 wt%, or 0.1 wt% to 1.0 wt% based on the total weight of the biodegradable resin composition. The hydrolysis inhibitor may include a carbodiimide-based compound. The carbodiimide-based compound reacts with moisture and acid to be converted into a urea structure, thereby reducing the reactivity between moisture and acid and the ester group contained in the biodegradable resin, thereby reducing the phenomenon of the biodegradable resin being hydrolyzed by moisture and acid, and consequently improving the hydrolysis resistance of the biodegradable resin composition.

[0249] The above carbodiimide compounds are N,N'-di-o-tolylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-dioctyldecylcarbodiimide, N,N'-di-2,6-diketylphenylcarbodiimide, N-tolyl-N'cyclohexylcarbodiimide, N,N'-di-2,6-diisopropylphenylcarbodiimide, N,N'-di-2,6-di-tert-butylphenylcarbodiimide, N-tolyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, It may be at least one selected from the group consisting of N,N'-di-p-tolylcarbodiimide, p-phenylene-bis-di-o-tolylcarbodiimide, p-phenylene-bisdicyclohexylcarbodiimide, hexamethylene-bisdicyclohexylcarbodiimide, ethylene-bisdiphenylcarbodiimide, and copolymers of benzene-2,4-diisocyanato-1,3,5-tris(1-methylethyl) homopolymer, 2,4-diisocyanato-1,3,5-tris(1-methylethyl) and 2,6-diisopropyl diisocyanate.

[0250]

[0251] The above manufacturing method may include a step of (d) manufacturing pellets from the biodegradable resin composition.

[0252] The step (d) above may be performed by putting the biodegradable resin composition into an extrusion molding machine equipped with a single screw or an extrusion molding machine equipped with a twin screw, extruding it at a temperature of 150°C to 180°C, cutting it with a hot-cut type pellet cutting machine, and cooling it at 30°C or less, 25°C or less, 5 to 50°C, 10 to 30°C, 15 to 25°C, or 20 to 25°C to manufacture pellets. The cutting step is not particularly limited as long as it is a pellet cutting machine used in the art, and the shape of the manufactured pellets is not particularly limited.

[0253]

[0254] The above manufacturing method may include (e) a step of drying and melt-extruding the pellets.

[0255] The drying may be performed at a temperature range of 60°C to 100°C, 65°C to 95°C, 70°C to 90°C, or 75°C to 85°C, for 2 hours to 12 hours, 3 hours to 12 hours, or 4 hours to 10 hours. When the above conditions are satisfied, the appearance, mechanical properties, and chemical properties of the biodegradable molded product produced may be further improved.

[0256] The above melt extrusion can be performed at 270°C or less, 265°C or less, 260°C or less, 255°C or less, 130°C to 270°C, 130°C to 250°C, 140°C to 230°C, 150°C to 200°C, or 150°C to 180°C. The above melt extrusion can be performed by a blown film process or a press process, but is not particularly limited. The torque during the melt extrusion can be 100 N·m to 300 N·m, or 150 N·m to 250 N·m.

[0257]

[0258] Hereinafter, the present invention will be described in more detail based on examples and comparative examples. However, the following examples and comparative examples are merely illustrative examples for further explaining the present invention, and the present invention is not limited to the following examples and comparative examples.

[0259]

[0260] Example

[0261] - Biodegradable Resin #1: Ecopond

[0262] - Biodegradable Resin #2: Ecovance

[0263] - Biodegradable Resin #3: NatureWorks, 4032D

[0264] - Calcium carbonate: Omya

[0265] - Plasticizer: Glycerol monostearate (GMS)

[0266] - Active ingredient #1: Stearyl stearate

[0267] - Active ingredient #2: Calcium stearate

[0268] Antioxidant #1: Phenolic antioxidant, Adeca Korea AO-60

[0269] Antioxidant #2: Phosphorus Antioxidant, Adeca Korea 2112

[0270] - Carbon black: average diameter of about 20 nm, BET surface area of ​​about 130.5 m 2 / g, 25℃ temperature, 90% relative humidity, and moisture absorption rate of about 1.55% at 120 hours

[0271] - UV stabilizer: SONGSORB ® 3600

[0272]

[0273] Example 1

[0274] Biodegradable resin #1: calcium carbonate: plasticizer: antioxidant #1: antioxidant #2: carbon black were charged in a weight ratio of 52.9:43.9:1.0:0.05:0.15:2.0 into a kneader reactor and kneaded at a temperature of 155°C. Thereafter, the composition was extruded using an extruder equipped with a single screw, and cut and cooled using a hot-cut type pellet cutter to produce a pelletized biodegradable resin composition.

[0275]

[0276] Examples 2 to 5 and Comparative Examples 1 to 3

[0277] A pelletized biodegradable resin composition was prepared by the same process as Example 1, except that the pelletized biodegradable resin composition was prepared with the composition described in Table 1 below.

[0278]

[0279] Classification Biodegradable Resin #1 Biodegradable Resin #2 Biodegradable Resin #3 Calcium Carbonate Plasticizer Activator #1 Activator #2 Antioxidant #1 Antioxidant #2 Carbon Black UV Stabilizer Unit Weight % Example 1 52.90--43.90 1.00--0.05 0.152.00 Example 2 52.90--43.90 1.00--0.05 0.152.00 Example 3 52.90--43.90 1.00--0.05 0.151.00 Example 4 75.00 10.00 15.00-----2.00 Example 5 50.60-47.00-0.70 0.50 0.05 0.151.00 Comparative Example 169.50-10.0020.00----0.50Comparative Example 252.90--43.901.000.050.15--Comparative Example 3-52.90-43.901.000.050.15--

[0280]

[0281] Experimental example

[0282] <Manufacturing of film samples>

[0283] Each pelletized biodegradable resin composition manufactured in Examples 1 to 5 and Comparative Examples 1 to 3 was dried at 80°C for 5 hours, and then melt-extruded at 160°C using a blown film extruder (Blown Film Extrusion Line, manufacturer: Eugene Engineering) to manufacture a film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm. Thereafter, the film was cut to have a width of 15 mm to manufacture a sample of the biodegradable resin film.

[0284] <Manufacturing of sheet samples>

[0285] Each pelletized biodegradable resin composition manufactured in Examples 1 to 5 and Comparative Examples 1 to 3 was placed on a flat stainless steel (SUS) plate measuring 12 cm in width and 12 cm in length, and then a biodegradable resin sheet having an average thickness of 0.9 mm was manufactured under conditions of 180°C and 20 MPa of pressure. Thereafter, the sheet was cut into pieces measuring 10 cm in width and 3 cm in length to manufacture a sample of the biodegradable resin sheet.

[0286]

[0287] Experimental Example 1 - QUV Test

[0288] For the film samples manufactured in Examples 1 to 5 and Comparative Examples 1 to 3, the tensile strength and elongation in the MD (Machine Direction) direction for a 50 mm length of the sample were measured using INSTRON's UTM (Universal Testing Machine, 4206-001). Here, the elongation refers to the rate at which the sample elongates before breaking.

[0289] Afterwards, the above samples were placed in the QUV tester, and the temperature was 60℃ and the pressure was 0.89 W / m 2 After irradiating the sample with UV light under the illumination, a cycle of maintaining the sample at 50°C was performed. Afterwards, the sample was removed and dried at room temperature for 24 hours. The tensile strength and elongation of the sample in the machine direction (MD) were measured using the UTM (Universal Testing Machine). The QUV test conditions and results are shown in Table 2 below.

[0290]

[0291] Classification Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Comparative Example 3 Initial tensile strength (kgf / mm)2 )2.243.172.134.173.112.031.841.63Elongation(%)289199342.5180200241.11311240A 1) Tensile strength (kgf / mm) 2 )2.203.102.043.843.121.851.641.51Elongation (%)25017527617617415010495B 2) Tensile strength (kgf / mm) 2 )2.172.971.983.642.981.751.341.42Elongation (%)210167230170168804535C 3) Tensile strength (kgf / mm) 2 )2.142.841.953.422.811.361.041.33Elongation(%)168.62158.57195.47166.62159.8030.0227.3737.04D 4) Tensile strength (kgf / mm) 2 )2.032.572.253.092.551.751.241.09Elongation(%)151.04141.75139.54141.65142.7529.1524.1526.86E 5) Tensile strength (kgf / mm) 2 )2.042.482.232.862.491.85N.A. 7) Elongation (%) 103.92 118.04 107.29 130.83 117.3 126.19F 6) Tensile strength (kgf / mm) 2)2.012.482.172.842.461.84Elongation (%)78.1487.1980.18118.487.1124.181) A: 2 cycles of maintaining at 50℃ for 4 hours after UV irradiation for 8 hours2) B: 4 cycles of maintaining at 50℃ for 4 hours after UV irradiation for 8 hours3) C: 8 cycles of maintaining at 50℃ for 4 hours after UV irradiation for 8 hours4) D: 16 cycles of maintaining at 50℃ for 4 hours after UV irradiation for 8 hours5) E: 24 cycles of maintaining at 50℃ for 4 hours after UV irradiation for 8 hours6) F: 2 cycles of maintaining at 50℃ for 4 hours after UV irradiation for 8 hours 34 cycles of 4-hour hold time7) NA: Not measured

[0292]

[0293] Experimental Example 2 - Hydrophilicity Test

[0294] The initial number average molecular weights of the sheet samples manufactured in Examples 1 to 5 and Comparative Examples 1 to 3 were measured using gel permeation chromatography (GPC) under the following measurement conditions.

[0295] Afterwards, the sheet samples were immersed in a beaker containing water, sealed, and stored in an oven at 80°C for 7 days. Afterwards, the sheet samples were taken out of the beaker, the surfaces of the sheet samples were wiped twice with gauze, and the number average molecular weight after aging was measured using gel permeation chromatography (GPC) under the following measurement conditions.

[0296] The hydrolysis reduction rate was calculated using Equation 2 below, and the results are shown in Table 3 below. The smaller the difference between the initial number average molecular weight and the number average molecular weight after aging, i.e., the larger the hydrolysis reduction rate, the better the hydrolysis resistance was determined to be.

[0297] [Formula 2]

[0298] Hydrolysis reduction rate (%) = [(initial number average molecular weight) - (number average molecular weight after aging)] / (initial number average molecular weight) × 100

[0299]

[0300] <Measurement conditions>

[0301] - Device: APC system (Waters)

[0302] - Column: Acquity APC XT Column 45A (4.6*150mm)x2

[0303] - Mobile phase: THF

[0304] - Flow rate: 0.5mL / min

[0305] - Sample concentration: 10mg / 10mL

[0306] - Injection volume: 10 ㎕

[0307] - Detector: RID 40℃

[0308] - Total driving time: 10 minutes

[0309]

[0310] Experimental Example 3 - Biodegradability Test

[0311] An inoculum container containing only compost manufactured in a compost factory was prepared, and each test container was prepared by adding 5 wt% of the dry weight of the sheet samples manufactured in Examples 1 to 5 and Comparative Examples 1 to 3 onto the compost. Thereafter, the containers were cultured for 180 days under conditions of a temperature of 60°C, humidity of 90%, and an oxygen concentration of 6% or more, and the carbon dioxide generated in each test container was captured and titrated with an aqueous phenolphthalein solution to measure the amount of carbon dioxide generated. The biodegradability was calculated by the following Equation 3, and the results are shown in Table 3.

[0312] [Formula 3]

[0313] Biodegradability (%) = [(carbon dioxide generation in the test vessel) - (carbon dioxide generation in the inoculation vessel)] / (theoretical carbon dioxide generation in the test vessel) × 100

[0314]

[0315] Experimental Example 4 - Tear Strength

[0316] After a 2 mm notch was made in the center of each film sample manufactured in Examples 1 to 5 and Comparative Examples 1 to 3, the initial tear strength was calculated by Equation 4 below using INSTRON's UTM (Universal Testing Machine, 4206-001). Thereafter, the tear strength after the QUV test according to C in Table 2 was calculated, and the results are shown in Table 3.

[0317] [Formula 4]

[0318] Tear strength (N / cm) = Force applied when tearing (N) / Thickness of sample (cm)

[0319]

[0320] First elongation 1) (E0) Second elongation 2) (E1) Elongation retention rate 3) (ΔE) Hydrolysis reduction rate Biodegradability Initial tear strength Tear strength after QUV test Tear strength retention 4)Unit %N / cm%Example 1289168.6258.3709044038086.4Example 2199158.5779.7729044539588.7Example 3342.5195.4757.1709044038587.5Example 4180166.6292.6738545039086.7Example 5200159.8079.9729044539087.6Comparative Example 1241.1130.0212.5438542018042.9Comparative Example 233127.378.3428541015537.8Comparative Example 324037.0415.4458541017542.71) First elongation (E0): Initial elongation in the above Table 22) Second elongation (E1): Elongation of C in the above Table 23) Elongation retention (ΔE): (E1 / E0) Х 1004) Tear strength retention: (Tear strength after QUV test / Initial tear strength) Х 100

[0321]

[0322] As can be confirmed in Tables 1 to 3 above, Examples 1 to 5, which satisfy an elongation retention rate of 20% or more, have a biodegradability equivalent to or higher than that of Comparative Examples 1 to 3, and have excellent water resistance and resistance to ultraviolet rays, so that it can be confirmed that a user can appropriately maintain a certain level of mechanical strength and chemical properties within a typical period of use.

[0323]

[0324] The embodiment can be applied to a biodegradable resin composition and a biodegradable molded article comprising the same.

Claims

1. Biodegradable resin; Shading particles; and Includes weapon refills, A biodegradable resin composition having an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method: [measurement method] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C. 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm. 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine). 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine). 6) Calculate the elongation retention rate (ΔE) using Equation 1 below. [Formula 1] ΔE(%) = (E1 / E0) X 100 2. In paragraph 1, A biodegradable resin composition having a content of the biodegradable resin of 30 wt% to 90 wt% based on the total weight of the biodegradable resin composition.

3. In paragraph 1, A biodegradable resin composition having a content of the light-blocking particles of 0.1 wt% to 10.0 wt% based on the total weight of the biodegradable resin composition.

4. In paragraph 1, A biodegradable resin composition wherein the average diameter of the above-mentioned light-shielding particles is 10 nm to 500 nm.

5. In paragraph 1, The BET surface area of ​​the above-mentioned light-shielding particles is 100 m 2 / g to 700 m 2 A biodegradable resin composition having a mass of / g.

6. In paragraph 1, A biodegradable resin composition wherein the above-mentioned shading particles have a moisture absorption rate of 0.01% to 2.00% at a temperature of 25°C, a relative humidity of 90%, and after 120 hours.

7. In paragraph 1, A biodegradable resin composition wherein the content of the inorganic filler is 10 wt% to 90 wt% based on the total weight of the biodegradable resin composition.

8. In paragraph 1, A biodegradable resin composition wherein the inorganic filler comprises calcium carbonate surface-treated with an organic acid.

9. In paragraph 1, A biodegradable resin composition, wherein the first elongation of the biodegradable resin composition is 150% to 400%.

10. In paragraph 1, A biodegradable resin composition, wherein the second elongation of the biodegradable resin composition is 100% to 300%.

11. In paragraph 1, A biodegradable resin composition further comprising a plasticizer.

12. A biodegradable molded article comprising a biodegradable resin composition comprising a biodegradable resin, a light-blocking particle, and an inorganic filler, and having an elongation retention rate (ΔE) of 20% or more as measured by the following measurement method: [measurement method] 1) The above biodegradable resin composition is pelletized at a temperature of 155°C. 2) The pelletized biodegradable resin composition is manufactured into a biodegradable film having a blow-up ratio (BUR) of 2.6, an average thickness of 15 μm, and a width of 300 mm. 3) After manufacturing the above biodegradable film into a sample having a width of 15 mm, the first elongation (E0) in the MD (Machine Direction) direction for a 50 mm length of the sample is measured using a UTM (Universal Testing Machine). 4) Put the above sample into the QUV tester, and set the temperature to 60℃ and the pressure to 0.89 W / m 2 After irradiating the sample with UV light for 8 hours under a bright light, a cycle of maintaining the sample at 50°C for 4 hours was repeated 8 times. Afterwards, the sample was taken out and dried at room temperature for 24 hours, and the second elongation (E1) of the sample in the MD (Machine Direction) direction was measured using the UTM (Universal Testing Machine). 6) Calculate the elongation retention rate (ΔE) using Equation 1 below. [Formula 1] ΔE(%) = (E1 / E0) X 100 13. In paragraph 12, The biodegradable molded product is a biodegradable molded product that is a non-woven fabric, a vacuum-formed sheet, a blown molded product, or an injection-molded product.

Citation Information

Patent Citations

  • Preparation of polylactic acid and copolymers of lactic acids

    US4797468A

  • Production of high molecular weight polylactic acid

    US5470944A

  • Method for producing polylactic acid

    US5770682A

  • Process for preparing polylactic acid

    US5821327A

  • Method for producing polylactic acid and apparatus used therefor

    US5880254A