Graft copolymer, preparation method therefor, and resin composition comprising same

The method for producing graft copolymers with controlled grafting factors addresses the trade-off between impact and tensile strength in thermoplastic resin compositions, achieving improved impact resistance and scratch resistance without increasing rubber content, thereby enhancing the performance of thermoplastic resin compositions.

WO2024248443A1PCT designated stage expired Publication Date: 2024-12-05LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007141
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conjugated diene-based graft copolymers used in thermoplastic resin compositions face a trade-off between impact strength and tensile strength, where increasing the content of these copolymers reduces scratch resistance and internal resistance.

Method used

A method for producing graft copolymers with improved impact resistance by controlling the grafting factor, involving a process where conjugated diene-based polymers, aromatic vinyl monomers, and vinyl cyanide monomers are polymerized in the absence of a molecular weight regulator, with specific ratios and amounts of molecular weight regulators added during polymerization to maintain grafting rate and molecular weight, resulting in a graft copolymer with a graft density of 0.1 or less.

Benefits of technology

The method achieves a balance between excellent impact strength and scratch resistance without increasing rubber content, enhancing the overall performance of thermoplastic resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007141_05122024_PF_FP_ABST
    Figure KR2024007141_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a graft factor-controlled conjugated diene-based graft copolymer and a preparation method therefor. In addition, the present invention relates to a thermoplastic resin composition that, due to the inclusion of the graft factor-controlled conjugated diene-based graft copolymer, ensures excellent impact strength and scratch resistance simultaneously without increasing the rubber content.
Need to check novelty before this filing date? Find Prior Art

Description

Graft copolymer, method for producing the same, and resin composition comprising the same

[0001] [Cross-reference with related applications]

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0069530, filed May 30, 2023, the entire disclosure of which is incorporated herein by reference.

[0003]

[0004] [Technical Field]

[0005] The present invention relates to a method for producing a graft copolymer and a thermoplastic resin composition comprising the same.

[0006] Conjugated diene graft copolymers, which are prepared by graft polymerizing monomers such as vinyl aromatic monomers and vinyl cyan monomers onto conjugated diene polymers, are widely used as impact modifiers in thermoplastic resin compositions due to the excellent rubber properties of conjugated diene polymers. In addition, thermoplastic resin compositions containing conjugated diene graft copolymers have excellent impact resistance, chemical resistance, and processability, and are therefore widely used in office equipment, electrical and electronic components, and automotive interior materials.

[0007] In general, a thermoplastic resin composition includes a conjugated diene graft copolymer as an impact modifier as described above, and a styrene-acrylonitrile copolymer as a matrix resin. However, when the content of the conjugated diene graft copolymer is increased to improve the impact strength of the thermoplastic resin composition, there is a problem that the tensile strength and hardness decrease compared to the improvement in impact strength, resulting in a decrease in the scratch resistance of the thermoplastic resin composition itself. Therefore, there is a need for the development of a conjugated diene graft copolymer with improved impact resistance.

[0008]

[0009] [Prior Art Literature]

[0010] [Patent Document]

[0011] (Patent Document 1) JP 4741202 B2

[0012] The present invention has been devised to solve the problems of the above-mentioned prior art, and provides a graft copolymer with improved impact resistance by controlling the graft factor of the graft copolymer and a method for producing the same.

[0013] In addition, the present invention provides a thermoplastic resin composition that simultaneously secures excellent impact strength and scratch resistance without increasing the rubber content.

[0014] (1) The present invention provides a method for producing a graft copolymer, comprising: a step (S1) of simultaneously introducing a conjugated diene polymer, an aromatic vinyl monomer, and a vinyl cyan monomer into a reactor, and initiating polymerization in the absence of a molecular weight regulator; and a step (S2) of simultaneously and continuously introducing an aromatic vinyl monomer, a vinyl cyan monomer, a first molecular weight regulator, and a second molecular weight regulator different from the first molecular weight regulator into the reactor after the start of step (S1), and performing polymerization, wherein the weight of the first molecular weight regulator introduced is greater than or equal to the weight of the second molecular weight regulator introduced.

[0015] (2) The present invention provides a method for producing a graft copolymer in (1) above, wherein the weight of the second molecular weight regulator and the weight of the first molecular weight regulator are added in a ratio of 1:1 to 8.

[0016] (3) The present invention provides a method for producing a graft copolymer, wherein the first molecular weight regulator is at least one selected from the group consisting of α-methyl styrene dimer, p-methyl styrene dimer, and 2,4-dimethyl styrene dimer, in any one of the above (1) or (2).

[0017] (4) The present invention provides a method for producing a graft copolymer, wherein the second molecular weight modifier is at least one selected from the group consisting of t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, carbon tetrachloride, methylene chloride, methylene bromide, tetraethyl thiuram disulfide, dipentamethylene thiuram disulfide, and diisopropylxanthogen disulfide, in any one of the above (1) to (3).

[0018] (5) The present invention provides a method for producing a graft copolymer, wherein the S1 step is performed at a temperature of 40°C or higher and 55°C or lower in any one of the above (1) to (4).

[0019] (6) The present invention provides a method for producing a graft copolymer, wherein the S2 step is performed at a temperature of 60°C or higher and 75°C or lower in any one of the above (1) to (5).

[0020] (7) The present invention provides a method for producing a graft copolymer, wherein, in any one of the above (1) to (6), the first molecular weight regulator is added in an amount of 0.10 parts by weight or more and 0.55 parts by weight or less, based on 100 parts by weight of the total of the conjugated diene polymer, aromatic vinyl monomer, and vinyl cyan monomer added in the step S1 and the aromatic vinyl monomer and vinyl cyan monomer added in the step S2.

[0021] (8) The present invention provides a method for producing a graft copolymer, wherein, in any one of (1) to (7), the second molecular weight regulator is added in an amount of 0.05 parts by weight or more and 0.4 parts by weight or less, based on 100 parts by weight of the total of the conjugated diene polymer, aromatic vinyl monomer, and vinyl cyan monomer added in the step S1 and the aromatic vinyl monomer and vinyl cyan monomer added in the step S2.

[0022] (9) The present invention is a graft copolymer comprising a conjugated diene polymer; and a plurality of polymer chains grafted onto the conjugated diene polymer, wherein the polymer chains include aromatic vinyl monomer units and vinyl cyan monomer units, and the surface area of ​​the conjugated diene polymer is 1 nm. 2 A graft copolymer is provided wherein the number of polymer chains is 0.11 or less.

[0023] (10) The present invention provides a graft copolymer having a graft ratio of 0.2 or more and 0.45 or less in the above (9).

[0024] (11) The present invention provides a graft copolymer having a weight average molecular weight of 80,000 g / mol or more and 140,000 g / mol or less in any one of the above (9) or (10).

[0025] (12) The present invention provides a graft copolymer comprising a conjugated diene polymer according to any one of the above (9) to (11), and a plurality of polymer chains grafted onto the conjugated diene polymer, wherein the polymer chains include aromatic vinyl monomer units and vinyl cyan monomer units, and the graft density defined by the following mathematical formula 1 is 0.11 or less.

[0026] [Mathematical Formula 1]

[0027] Graft density (nm) -2 ) = g d Dρ p N A / 6M g

[0028] In mathematical equation 1,

[0029] g d is the grafting rate (%) calculated by the following mathematical formula 2,

[0030] D is the average particle diameter of the above conjugated diene polymer,

[0031] ρ pis the particle density of the graft copolymer,

[0032] N A is Avogadro's number,

[0033] M g is the weight average molecular weight of the grafted multiple polymer chains measured by GPC after dissolving the dried product of the graft copolymer sol separated from the supernatant of the sol-gel separation method in a TFT solution.

[0034] [Equation 2]

[0035] Grafting ratio = weight (g) of the grafted plurality of polymer chains / weight (g) of the conjugated diene polymer

[0036] (13) The present invention provides a thermoplastic resin composition comprising a graft copolymer according to any one of (8) to (12) above; and a non-graft copolymer comprising an aromatic vinyl monomer unit and a vinyl cyan monomer unit.

[0037] According to the present invention, a graft copolymer with improved impact resistance and a method for producing the same can be provided.

[0038] In addition, according to the present invention, a thermoplastic resin composition can be provided that simultaneously secures excellent impact strength and scratch resistance without increasing the rubber content.

[0039] Figure 1 is a TEM image of a graft copolymer according to Comparative Example 3 of the present invention.

[0040] Figure 2 is a TEM image of a graft copolymer according to Example 1 of the present invention.

[0041] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0042] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0043] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0044] In the present invention, the term 'monomer unit' may refer to a component, structure, or substance itself derived from a monomer, and as a specific example, may refer to a repeating unit formed within a polymer by a monomer introduced during polymerization of the polymer and participating in the polymerization reaction.

[0045] In the present invention, the "weight average molecular weight" is measured by gel permeation chromatography (GPC). For example, the sample to be measured can be dissolved in a THF (tetrahydrofuran) solution, and then measured as a relative value to a standard sample (PS, standard polystyrene) through gel permeation chromatography (GPC).

[0046] The term 'composition' as used in the present invention includes a mixture of materials comprising the composition as well as reaction products and decomposition products formed from the materials of the composition.

[0047] In the present invention, the 'average particle diameter' may refer to the arithmetic mean particle diameter in the particle size distribution measured by dynamic light scattering, specifically, the scattering intensity average particle diameter. The average particle diameter of the conjugated diene polymer can be measured using the Nicomp 380 equipment (product name, manufacturer: PSS Nicomp).

[0048]

[0049] <Method for producing graft copolymer>

[0050] A method for producing a graft copolymer according to one embodiment of the present invention comprises the steps of (S1) introducing a conjugated diene polymer, an aromatic vinyl monomer, and a vinyl cyan monomer into a reactor at once, and initiating polymerization in the absence of a molecular weight regulator; and (S2) simultaneously and continuously introducing an aromatic vinyl monomer, a vinyl cyan monomer, a first molecular weight regulator, and a second molecular weight regulator different from the first molecular weight regulator into the reactor after the initiation of step (S1), and performing polymerization, wherein the amount of the first molecular weight regulator introduced is greater than or equal to the amount of the second molecular weight regulator introduced.

[0051] The present inventors have discovered that by initiating polymerization in the absence of a molecular weight regulator and adjusting the weight ratio of the first molecular weight regulator and the second molecular weight regulator to a specific ratio in the polymerization step, a graft ratio is effectively lowered, the molecular weight is maintained, and the graft density (the number of polymers per particle surface area) is 0.1 or less, thereby producing a graft copolymer with significantly improved impact strength, thereby completing the present invention.

[0052]

[0053] Hereinafter, a method for producing a graft copolymer according to one embodiment of the present invention will be described.

[0054]

[0055] 1. First polymerization stage (S1 stage)

[0056] First, according to one embodiment of the present invention, the method for producing the graft copolymer comprises a first polymerization step. The first polymerization step is to collectively introduce a conjugated diene polymer, an aromatic vinyl monomer, and a vinyl cyan monomer into a reactor and initiate polymerization in the absence of a molecular weight modifier (CTA, Chain Transfer Agent).

[0057]

[0058] According to one embodiment of the present invention, the conjugated diene polymer may be manufactured by polymerizing a conjugated diene monomer and may include a conjugated diene monomer unit. As a more specific example, the conjugated diene polymer may be manufactured by emulsion polymerizing a conjugated diene monomer. In this case, the average particle diameter of the conjugated diene polymer can be easily controlled, so that a conjugated diene polymer suitable for the desired mechanical properties can be used. The conjugated diene polymer may refer to a synthetic rubber manufactured by crosslinking polymerizing a diene monomer or a diene monomer and a vinyl aromatic monomer.

[0059] According to one embodiment of the present invention, the conjugated diene monomer for forming the conjugated diene monomer unit of the conjugated diene polymer may be at least one selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, piperylene, 3-butyl-1,3-octadiene, isoprene, and 2-phenyl-1,3-butadiene, and a more specific example may be 1,3-butadiene.

[0060] The average particle diameter of the above conjugated diene polymer may be 50 to 500 nm, preferably 70 to 400 nm.

[0061]

[0062] According to one embodiment of the present invention, the aromatic vinyl monomer may be at least one selected from the group consisting of styrene, α-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 1-vinylnaphthalene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, and 1-vinyl-5-hexylnaphthalene, and a specific example thereof may be styrene.

[0063]

[0064] According to one embodiment of the present invention, the vinyl cyan monomer may be at least one selected from the group consisting of acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, and α-chloroacrylonitrile, and a specific example may be acrylonitrile.

[0065]

[0066] According to one embodiment of the present invention, the first polymerization step is performed in the absence of a molecular weight regulator introduced in the subsequent polymerization step. If polymerization is initiated in the presence of a molecular weight regulator, the weight average molecular weight and graft ratio of the polymer change, making it difficult to control the graft density.

[0067]

[0068] According to one embodiment of the present invention, the first polymerization step may be performed at a temperature of 40°C or higher and 55°C or lower. When the above-described range is satisfied, a graft copolymer having excellent polymerization stability and conversion rate can be obtained.

[0069]

[0070] According to one embodiment of the present invention, the first polymerization step may be performed in the presence of at least one selected from the group consisting of an initiator, an activator, an emulsifier, and an aqueous solvent.

[0071]

[0072] According to one embodiment of the present invention, the initiator may be at least one selected from the group consisting of sodium persulfate, potassium persulfate, ammonium persulfate, hydroperoxide, t-butyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, p-menthane hydroperoxide, di-t-butyl peroxide, t-butyl cumyl peroxide, acetyl peroxide, isobutyl peroxide, octanoyl peroxide, dibenzoyl peroxide, 3,5,5-trimethylhexanol peroxide, t-butyl peroxy isobutyrate, azobisisobutyronitrile, azobis-2,4-dimethylvaleronitrile, azobiscyclohexanecarbonitrile and azobisisobutyric acid (butyric acid) methyl, as a specific example. It could be hydroperoxide.

[0073] According to one embodiment of the present invention, the initiator introduced in the first polymerization step may be present in an amount of 0.001 to 1.000 parts by weight, preferably 0.010 to 0.800 parts by weight, based on 100 parts by weight of the total of the conjugated diene polymer, vinyl cyan monomer, and aromatic vinyl monomer introduced during the production of the graft copolymer (i.e., introduced in the first polymerization step and the second polymerization step below). When the above-described range is satisfied, the polymerization stability of the graft polymerization can be improved while minimizing the residual amount of the initiator in the graft copolymer powder.

[0074]

[0075] According to one embodiment of the present invention, an activator may be further added to promote the reaction of the first polymerization step together with the initiator. The activator may be at least one selected from the group consisting of sodium formaldehyde sulfoxylate, sodium ethylenediamine tetraacetate, ferrous sulfate, dextrose, sodium pyrrolate, tetrasodium pyrophosphate, sodium pyrophosphate anhydrous, and sodium sulfate.

[0076] According to one embodiment of the present invention, the activator introduced in the first polymerization step may be introduced in an amount of 0.001 to 0.500 parts by weight, preferably 0.010 to 0.300 parts by weight, based on 100 parts by weight of the total of the conjugated diene polymer, vinyl cyan monomer, and aromatic vinyl monomer introduced during the production of the graft copolymer (i.e., introduced in the first polymerization step and the second polymerization step below). When the above-described range is satisfied, the polymerization stability of the graft polymerization can be improved, while the residual amount of the activator in the graft copolymer powder can be minimized.

[0077]

[0078] According to one embodiment of the present invention, the emulsifier may be at least one selected from the group consisting of sodium dicyclohexyl sulfosuccinate, sodium dodecyl sulfate, sodium dodecyl benzene sulfonate, sodium octadecyl sulfate, sodium oleic sulfate, potassium dodecyl sulfate and potassium octadecyl sulfate, fatty acid potassium salts and fatty acid sodium salts.

[0079] According to one embodiment of the present invention, the emulsifier introduced in the first polymerization step may be introduced in an amount of 0.05 to 1.00 parts by weight, preferably 0.10 to 0.300 parts by weight, based on 100 parts by weight of the total of the conjugated diene polymer, vinyl cyan monomer, and aromatic vinyl monomer introduced during the production of the graft copolymer (i.e., introduced in the first polymerization step and the second polymerization step below). When the above-described range is satisfied, a graft copolymer powder having a desired average particle size can be produced while improving the polymerization stability of the graft polymerization.

[0080]

[0081] According to one embodiment of the present invention, the aqueous solvent may be ion-exchanged water or pure water.

[0082]

[0083] 2. Second polymerization stage (S2 stage)

[0084] According to one embodiment of the present invention, the method for producing the graft copolymer comprises a second polymerization step. The second polymerization step is performed subsequent to the first polymerization step, and polymerization is performed by continuously introducing a first molecular weight modifier, a second molecular weight modifier, an aromatic vinyl monomer, and a vinyl cyan monomer into the reactor.

[0085]

[0086] According to one embodiment of the present invention, the first molecular weight modifier is an alkyl styrene dimer, and may be at least one selected from the group consisting of α-methyl styrene dimer, p-methyl styrene dimer, and 2,4-dimethyl styrene dimer, and a specific example thereof may be α-methyl styrene dimer.

[0087] According to one embodiment of the present invention, the first molecular weight regulator may be added in an amount of 0.10 parts by weight or more and 0.55 parts by weight or less, based on 100 parts by weight of the total of the conjugated diene polymer, the vinyl cyan monomer, and the aromatic vinyl monomer added during the production of the graft copolymer (i.e., added during the first polymerization step and the second polymerization step below). Specifically, the first molecular weight regulator may be added in an amount of 0.11 parts by weight or more, 0.12 parts by weight or more, 0.13 parts by weight or more, 0.14 parts by weight or more, or 0.15 parts by weight or more, based on 100 parts by weight of the total of the conjugated diene polymer, the vinyl cyan monomer, and the aromatic vinyl monomer added during the production of the graft copolymer, and may be added in an amount of 0.54 parts by weight or less, 0.53 parts by weight or less, 0.52 parts by weight or less, 0.51 parts by weight or less, or 0.50 parts by weight or less. When the above-described range is satisfied, the graft ratio of the graft copolymer produced is lowered, the weight average molecular weight is maintained, and the graft density becomes 0.1 or less, so that the impact strength can be improved.

[0088]

[0089] According to one embodiment of the present invention, the second molecular weight modifier may be a mercaptan compound, and may be at least one selected from the group consisting of t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, carbon tetrachloride, methylene chloride, methylene bromide, tetraethyl thiuram disulfide, dipentamethylene thiuram disulfide, and diisopropylxanthogen disulfide, and a specific example may be t-dodecyl mercaptan.

[0090] According to one embodiment of the present invention, the second molecular weight regulator may be added in an amount of 0.05 parts by weight or more and 0.4 parts by weight or less, based on 100 parts by weight of the total of the conjugated diene polymer, the vinyl cyan monomer, and the aromatic vinyl monomer added during the production of the graft copolymer (i.e., added during the first polymerization step and the second polymerization step below). Specifically, the second molecular weight regulator may be added in an amount of 0.06 parts by weight or more, 0.07 parts by weight or more, 0.08 parts by weight or more, 0.09 parts by weight or more, or 0.10 parts by weight or more, based on 100 parts by weight of the total of the conjugated diene polymer, the vinyl cyan monomer, and the aromatic vinyl monomer added during the production of the graft copolymer, and further may be added in an amount of 0.38 parts by weight or less, 0.36 parts by weight or less, 0.34 parts by weight or less, 0.32 parts by weight or less, or 0.30 parts by weight or less. When the above-described range is satisfied, the graft ratio of the graft copolymer produced is lowered, the weight average molecular weight is maintained, and the graft density becomes 0.1 or less, so that the impact strength can be improved.

[0091]

[0092] According to one embodiment of the present invention, the first molecular weight regulator and the second molecular weight regulator may be added in an amount of 0.15 parts by weight or more and 0.95 parts by weight or less, based on 100 parts by weight of the total of the conjugated diene polymer, vinyl cyan monomer, and aromatic vinyl monomer added during the production of the graft copolymer (i.e., added in the first polymerization step and the second polymerization step). Specifically, the first molecular weight modifier may be added in an amount of 0.2 parts by weight or more, 0.25 parts by weight or more, 0.3 parts by weight or more, 0.35 parts by weight or more, 0.4 parts by weight or more, 0.45 parts by weight or more, or 0.5 parts by weight or more, and may be added in an amount of 0.9 parts by weight or less, 0.85 parts by weight or less, 0.8 parts by weight or less, 0.75 parts by weight or less, 0.7 parts by weight or less, 0.65 parts by weight or less, or 0.6 parts by weight or less, based on 100 parts by weight of the total of the conjugated diene polymer, the vinyl cyan monomer, and the aromatic vinyl monomer added during the production of the graft copolymer. When the above-described range is satisfied, the graft ratio of the produced graft copolymer is lowered, and the weight average molecular weight is maintained so that the graft density becomes 0.1 or less, thereby improving the impact strength.

[0093]

[0094] According to one embodiment of the present invention, since an alkyl styrene-based dimer is more advantageous in controlling the grafting rate of a graft copolymer than a mercaptan-based compound, the weight of the first molecular weight modifier added may be greater than or equal to the weight of the second molecular weight modifier added.

[0095] The weight ratio of the second molecular weight regulator to the weight ratio of the first molecular weight regulator (second molecular weight regulator input amount: first molecular weight regulator input amount) may be 1:1 to 8. As a specific example, the weight ratio of the second molecular weight regulator to the weight ratio of the first molecular weight regulator may be 1:1 to 7, 1:1 to 6, 1:1 to 5, 1:1 to 4, or 1:1 to 3. When the above-described range is satisfied, the graft ratio of the produced graft copolymer is lowered, and the weight average molecular weight is maintained so that the graft density becomes 0.1 or less, thereby improving the impact strength.

[0096]

[0097] According to one embodiment of the present invention, the first molecular weight regulator and the second molecular weight regulator can be simultaneously and continuously introduced in the second polymerization step. When the first molecular weight regulator and the second molecular weight regulator are continuously introduced, it is easier to adjust the graft ratio and the weight average molecular weight compared to when they are introduced all at once, and thus a graft copolymer having a desired graft ratio and weight average molecular weight can be produced.

[0098]

[0099] According to one embodiment of the present invention, the point in time at which the continuous addition of the first molecular weight regulator and the second molecular weight regulator is initiated may be a point in time at which the polymerization conversion rate is 10% or less, preferably a point in time at which the polymerization conversion rate is 0% to 5%. If the above-described conditions are satisfied, the first molecular weight regulator and the second molecular weight regulator are added from the polymerization propagation stage, so that the effects of the first molecular weight regulator and the second molecular weight regulator can be maximized.

[0100] According to one embodiment of the present invention, the point in time at which the continuous addition of the first molecular weight regulator and the second molecular weight regulator ends may be a point in time at which the polymerization conversion rate is 80 to 97%, preferably 90 to 95%. When the above-described conditions are satisfied, polymerization stability can be improved and the polymerization conversion rate can be increased.

[0101]

[0102] According to one embodiment of the present invention, the weight ratio of the aromatic vinyl monomer introduced in the first polymerization step and the aromatic vinyl monomer introduced in the second polymerization step may be 1:1.857 to 9, preferably 1:2.333 to 5.667. When the above-described conditions are satisfied, a graft copolymer having a uniform composition throughout the polymerization process can be produced while improving polymerization stability.

[0103]

[0104] According to one embodiment of the present invention, the weight ratio of the vinyl cyan monomer introduced in the first polymerization step and the vinyl cyan monomer introduced in the second polymerization step may be 1:1.857 to 9, preferably 1:2.3333 to 5.667. When the above-described conditions are satisfied, a graft copolymer having a uniform composition throughout the polymerization can be produced while improving polymerization stability.

[0105]

[0106] According to one embodiment of the present invention, the second polymerization step may be performed at a temperature of 60°C or more and 75°C or less. When the above-described range is satisfied, the polymerization stability of the graft copolymer is improved during polymerization, and a graft copolymer having an excellent polymerization conversion rate can be produced.

[0107]

[0108] According to one embodiment of the present invention, the second polymerization step may be performed in the presence of at least one selected from the group consisting of an emulsifier, an initiator, an activator, and an aqueous solvent. The description of the emulsifier, initiator, activator, and aqueous solvent is as described above.

[0109]

[0110] 3. Drying stage

[0111] According to one embodiment of the present invention, the method for producing a graft copolymer may further include a process of producing a graft copolymer powder (DP, Dry powder) having a moisture content of less than 1% by dehydrating and hot-air drying the graft copolymer latex produced through the first polymerization step and the second polymerization step.

[0112]

[0113] <Graft copolymer>

[0114] A graft copolymer according to one embodiment of the present invention is produced by the graft copolymer production method of the present invention, and may be a copolymer in which an aromatic vinyl monomer unit and a vinyl cyan monomer unit are graft-polymerized onto a conjugated diene polymer. Accordingly, the graft copolymer may include the conjugated diene polymer and an aromatic vinyl monomer unit and a vinyl cyan monomer unit grafted onto the conjugated diene polymer. In the present specification, the aromatic vinyl monomer unit and the vinyl cyan monomer unit grafted onto the conjugated diene polymer may be expressed as a polymer chain.

[0115] According to one embodiment of the present invention, a graft copolymer comprises a conjugated diene polymer; and a plurality of polymer chains grafted onto the conjugated diene polymer, wherein the polymer chains include aromatic vinyl monomer units and vinylcyan monomer units, and the surface area of ​​the conjugated diene polymer is 1 nm. 2 The number of the above polymer chains may be 0.06 or more and 0.11 or less. Specifically, the surface area of ​​the conjugated diene polymer is 1 nm. 2The number of the polymer chains may be 0.065 or more, 0.07 or more, 0.075 or more, or 0.08 or more, and may also be 0.108 or less, 0.106 or less, 0.104 or less, 0.102 or less, or 0.1 or less. When the above-described range is satisfied, the dispersibility of the graft copolymer particles in the non-graft resin is improved, and thus the impact strength of the graft copolymer itself can be improved.

[0116] According to one embodiment of the present invention, the surface area of ​​the conjugated diene polymer is 1 nm 2 The number of the polymer chains can be expressed as a graft density, and the graft density can be defined by the following mathematical expression 1.

[0117] [Mathematical Formula 1]

[0118] Graft density (nm) -2 ) = g d Dρ p N A / 6M g

[0119] In mathematical expression 1,

[0120] g d is the grafting rate (%) calculated by the following mathematical formula 2,

[0121] D is the average particle diameter (nm) of the conjugated diene polymer included in the graft copolymer,

[0122] ρ p is the particle density of the graft copolymer,

[0123] N A is Avogadro's number,

[0124] M g is the weight average molecular weight of the grafted monomer, i.e., the grafted multiple polymer chains, measured by GPC after dissolving the dried product of the graft copolymer sol separated from the supernatant of the sol-gel separation method in a TFT solution.

[0125]

[0126] [Equation 2]

[0127] Grafting ratio = weight (g) of grafted monomer, i.e., the grafted plurality of polymer chains / weight (g) of the conjugated diene polymer

[0128]

[0129] According to one embodiment of the present invention, the particle density (ρ) of the graft copolymer p ) can be measured by the ASTM D792 method, and the particles of the graft copolymer may mean a powder-state graft copolymer.

[0130] According to one embodiment of the present invention, the particle density (ρ) of the graft copolymer p ) is 0.95 g / cm 3 Above 0.99 g / cm 3 It could be as follows:

[0131] According to one embodiment of the present invention, the surface area of ​​the conjugated diene polymer is 1 nm 2 The number of the polymer chains, i.e., the graft density, may be 0.06 or more and 0.11 or less. Specifically, the graft density of the conjugated diene polymer may be 0.065 or more, 0.07 or more, 0.075 or more, or 0.08 or more, and may also be 0.108 or less, 0.106 or less, 0.104 or less, 0.102 or less, or 0.1 or less. When the above-described range is satisfied, the dispersibility of the graft copolymer particles within the non-graft resin is improved, and thus the impact strength of the graft copolymer itself can be improved.

[0132]

[0133] <Thermoplastic resin composition>

[0134] A thermoplastic resin composition according to one embodiment of the present invention may include the graft copolymer of the present invention.

[0135]

[0136] According to one embodiment of the present invention, the thermoplastic resin composition may further include a non-graft copolymer including an aromatic vinyl monomer unit and a vinyl cyan monomer unit to improve processability.

[0137]

[0138] The thermoplastic resin composition may contain the graft copolymer in an amount of 10 parts by weight or more and 21 parts by weight or less, based on 100 parts by weight of the total of the graft copolymer and the non-graft copolymer. Specifically, the thermoplastic resin composition may contain the graft copolymer in an amount of 11 parts by weight or more, 12 parts by weight or more, 13 parts by weight or more, 14 parts by weight or more, or 15 parts by weight or more, based on 100 parts by weight of the total of the graft copolymer and the non-graft copolymer, and may also contain the graft copolymer in an amount of 20.8 parts by weight or less, 20.6 parts by weight or less, 20.4 parts by weight or less, 20.2 parts by weight or less, or 20 parts by weight or less. When the above-described ranges are satisfied, excellent impact strength, tensile strength, and scratch resistance can be secured simultaneously.

[0139]

[0140] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0141]

[0142] Example 1

[0143] <Graft copolymer manufacturing>

[0144] (First polymerization step) For a total of 100 parts by weight of conjugated diene polymers, styrene and acrylonitrile used throughout the manufacturing process, a mixed solution containing 100 parts by weight of ion-exchanged water, 58 parts by weight of conjugated diene polymer (average particle size 320 nm), 7.5 parts by weight of styrene as monomers, 2.5 parts by weight of acrylonitrile, 0.1 parts by weight of potassium salt of fatty acid as emulsifier, 0.05 parts by weight of hydroperoxide as initiator, 0.08 parts by weight of dextrose as activator, 0.05 parts by weight of sodium pyrophosphate and 0.001 parts by weight of ferrous sulfate was simultaneously introduced into a nitrogen-filled polymerization reactor, and the reaction was initiated at 50°C.

[0145] (Second polymerization step) At the start of the first polymerization step, 24 parts by weight of styrene as a monomer, 8 parts by weight of acrylonitrile, 0.2 parts by weight of a fatty acid potassium salt as an emulsifier, 0.6 parts by weight or less of a total of t-dodecyl mercaptan (second molecular weight regulator) and alpha methyl styrene dimer (first molecular weight regulator) as molecular weight regulators (t-dodecyl mercaptan input amount: alpha methyl styrene dimer input amount is 1:3), and 0.1 parts by weight of hydroperoxide as an initiator were continuously input in an emulsified state (emulsified monomer) at 70°C for about two hours.

[0146] Afterwards, at the end of the second polymerization step, 0.04 parts by weight of dextrose, 0.03 parts by weight of sodium pyrrolate, and 0.0005 parts by weight of ferrous sulfate were added in batches, and the temperature was raised to 80°C over 1 hour to complete the reaction.

[0147] (Drying step) 0.4 parts by weight of antioxidant (A / O) is added to the latex in which the reaction is completed, and after coagulation with 2 parts by weight of sulfuric acid and dehydration process, it is dried in a hot air fluidized bed dryer and the moisture content is less than 1% and the density measured by the ASTM D792 method is 0.99 g / cm. 3 In-graft copolymer powder (DP, Dry powder) was obtained.

[0148]

[0149] <Manufacturing of thermoplastic resin composition>

[0150] A thermoplastic resin composition was obtained by mixing 20 parts by weight of the obtained graft copolymer powder and 80 parts by weight of styrene-acrylonitrile (SAN) pellets in a mixer, pelletizing them using an extruder, and then injection molding them using an injection molding machine.

[0151]

[0152] Example 2

[0153] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that in the second polymerization step of Example 1, the amount of t-dodecyl mercaptan added: the amount of alpha methyl styrene dimer added was 1:1.5.

[0154]

[0155] Example 3

[0156] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that in the second polymerization step of Example 1, the amount of t-dodecyl mercaptan added was 1:5:alpha methyl styrene dimer added.

[0157]

[0158] Example 4

[0159] A thermoplastic resin composition was obtained by performing the same method as Example 1 except that in the second polymerization step of Example 1, the amount of t-dodecyl mercaptan added: the amount of alpha methyl styrene dimer added was 2:3.

[0160]

[0161] Example 5

[0162] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that in the second polymerization step of Example 1, the amount of t-dodecyl mercaptan added: the amount of alpha methyl styrene dimer added was 1:1.

[0163]

[0164] Comparative Example 1

[0165] In the second polymerization step of Example 1, a thermoplastic resin composition was obtained by performing the same method as Example 1 except that alphamethylstyrene dimer was not added.

[0166]

[0167] Comparative Example 2

[0168] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that in the second polymerization step of Example 1, the amount of t-dodecyl mercaptan was doubled and alpha methyl styrene dimer was not added.

[0169]

[0170] Comparative Example 3

[0171] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that in the second polymerization step of Example 1, the amount of t-dodecyl mercaptan was increased by four times and alpha methyl styrene dimer was not added.

[0172]

[0173] Comparative Example 4

[0174] In the second polymerization step of Example 1, a graft copolymer powder was obtained by performing the same procedure as Example 1, except that the amount of t-dodecyl mercaptan was increased by 5 times and alpha methyl styrene dimer was not added.

[0175]

[0176] Comparative Example 5

[0177] In the second polymerization step of Example 1, a graft copolymer powder was obtained by performing the same procedure as Example 1, except that the amount of t-dodecyl mercaptan was increased by four times and alpha methyl styrene dimer was not added.

[0178] A thermoplastic resin composition was obtained by mixing 22 parts by weight of the obtained graft copolymer powder and 78 parts by weight of styrene-acrylonitrile (SAN) pellets in a mixer, pelletizing them using an extruder, and then injection molding them using an injection molding machine.

[0179]

[0180] Comparative Example 6

[0181] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that 0.1 part by weight of alpha methyl styrene dimer was additionally added as a molecular weight regulator in the first polymerization step of Example 1.

[0182]

[0183] Comparative Example 7

[0184] A thermoplastic resin composition was obtained by performing the same method as Example 1 except that the amount of t-dodecyl mercaptan was increased by four times in the second polymerization step of Example 1.

[0185]

[0186] Comparative Example 8

[0187] A thermoplastic resin composition was obtained by performing the same method as Example 1, except that the amount of t-dodecyl mercaptan was increased by 5 times in the second polymerization step of Example 1.

[0188]

[0189] Experimental Example 1

[0190] The physical properties of the graft copolymer latex or powder obtained in Examples 1 to 5 and Comparative Examples 1 to 8 were measured by the methods described below, and the results are shown in Tables 1 to 3 below.

[0191]

[0192] * Graft density: Calculated according to the following mathematical formula 1.

[0193] [Mathematical Formula 1]

[0194] Graft density = gd Dρ p N A / 6M g

[0195] In mathematical expression 1,

[0196] g d is the grafting rate (%) calculated by the following mathematical formula 2,

[0197] D is the average particle diameter of the conjugated diene polymer included in the graft copolymer,

[0198] ρ p is the particle density of the graft copolymer (i.e., the density of the graft copolymer powder),

[0199] N A is Avogadro's number,

[0200] M g is the weight average molecular weight of the grafted monomer (i.e., multiple grafted polymer chains) measured by GPC after dissolving the dried sol of the graft copolymer separated from the supernatant of the sol-gel separation method in a TFT solution.

[0201]

[0202] * Grafting ratio: 1 g of graft copolymer powder was added to 50 ml of acetone and stirred for 24 hours, and then the solution was separated into sol-gel using a centrifuge, and the separated acetone solution was dropped into methanol to obtain a non-grafted monomer portion, which was dried at 60 to 120°C and weighed. Then, the sum of the weight of the introduced rubber polymer and the weight of the non-grafted monomer was subtracted from the total weight of the rubber polymer, styrene, and acrylonitrile introduced in the production of the graft copolymer to calculate the weight of the grafted monomer, and then the weight was calculated based on the following mathematical formula 2.

[0203] [Equation 2]

[0204] Grafting ratio = Weight of grafted monomer (i.e., multiple grafted polymer chains) (g) / Weight of conjugated diene polymer (g)

[0205]

[0206] * Polymerization conversion rate: 1g of polymer latex was dried in a hot air dryer at 150℃ for 15 minutes, and the weight was measured to obtain the total solid content (TSC), which was then calculated based on the following mathematical formula 3.

[0207] [Equation 3]

[0208] Polymerization conversion rate (%) = Total solids content (TSC) × (weight parts of monomers and auxiliary materials added) / 100 - (weight parts of auxiliary materials added other than monomers)

[0209]

[0210] * Weight average molecular weight (g / mol): The supernatant described in the graft ratio measurement method was dried, the dried product was dissolved in tetrahydrofuran (THF) solution, filtered through a 1 ㎛ filter, and measured as a relative value to a standard PS (standard polystyrene) sample through gel permeation chromatography.

[0211]

[0212] Experimental Example 2

[0213] The thermoplastic resin compositions obtained in Examples 1 to 5 and Comparative Examples 1 to 8 were extruded and injected to manufacture specimens, and the physical properties of the specimens were measured by the methods described below, and the results are shown in Tables 1 to 3 below.

[0214]

[0215] * Izod impact strength (kg·cm / cm, 1 / 4''): Measured according to ASTM D265.

[0216]

[0217] * Flow index (MI, g / 10 min): Measured at 220℃, 10kg according to ASTM D1238.

[0218]

[0219] * Tensile strength (TS, kg / cm) 2): According to ASTM D638, a UTM (manufacturer; Instron, model number 4466) was used to pull a specimen with a thickness of 3.2 mm at a cross head speed of 5 mm / min, and the point where the specimen was cut was measured.

[0220]

[0221] * Pencil hardness: Using a pencil hardness measuring device from Jungdo Testing Instrument, the pencil lead was placed at a 45° angle to the surface of the film, pressed with a load of 750 g, and pressed horizontally at a speed of 0.5 to 1 mm / s for a distance of at least 7 mm to observe whether a scar was formed on the pencil lead. The hardness of the hardest pencil that did not form a scar was determined as the pencil hardness. (9H > 8H > 7H > 6H > 5H > 4H > 3H > 2H > F > HB > B > 2B > 3B > 4B > 5B > 6B > 7B > 8B > 9B)

[0222]

[0223] Example 12345 (S1) Step AMSD input amount (weight part)-----(S2) Step TDDM input amount: AMSD input amount 1:31:1.51:52:31:1 Graft copolymer conversion rate (%) 98.1 98.2 93.5 97.7 97.1 Graft ratio 0.37 0.4 10.30.3 10.26 Molecular weight (g / mol) 120,000 130,000 110,000 100,000 87,000 Graft density (nm) -2 )0.0970.1000.0870.0990.095Thermoplastic resin compositionGraft copolymer(parts by weight)2020202020Non-graft copolymer(parts by weight)808080808080IMP (1 / 4)1918191817MI (g / 10min)4341444546TS480483485477479Pencil hardnessBBBBB

[0224] Comparative Example 12345 (S1) Step AMSD input (weight part)-----(S2) Step TDDM input: AMSD input 1:02:04:05:04:0 Graft copolymer conversion rate (%) 98.3 98.0 97.5 96.4 97.5 Graft ratio 0.57 0.50 0.35 0.26 0.35 Molecular weight (g / mol) 140,000 115,000 80,000 65,000 80,000 Graft density (nm) -2 )0.1290.1380.1390.1270.139Thermoplastic resin compositionGraft copolymer(parts by weight)2020202022Non-graft copolymer(parts by weight)8080808078IMP (1 / 4)1616151318MI (g / 10min)3840454840TS488485480472450Pencil hardnessBBBB2B

[0225] Comparative Example 678 (S1) AMSD input amount (weight part) 0.10--(S2) Step TDDM input amount: AMSD input amount 1:34:35:3 Graft copolymer conversion rate (%) 96.5 96.6 96.1 Graft ratio 0.36 0.23 0.19 Molecular weight (g / mol) 100,000 62,000 49,000 Graft density (nm) -2 )0.1140.1180.123Thermoplastic resin compositionGraft copolymer(parts by weight)202020Non-graft copolymer(parts by weight)808080IMP (1 / 4)161412MI (g / 10min)424749TS477481483Pencil hardnessBBB

[0226] Referring to Tables 1 and 2 above, the graft copolymers of Examples 1 to 5, in which polymerization was initiated in the absence of a molecular weight regulator and the weight of the first molecular weight regulator added was greater than or equal to the weight of the second molecular weight regulator added, were measured to have a graft density of 0.1 or less. The thermoplastic resin compositions of Examples 1 to 5 prepared with the graft copolymers having such characteristics had an appropriate flow index, thus exhibiting excellent processability, excellent impact strength, and excellent tensile strength, and a pencil hardness of B, confirming that excellent scratch resistance was secured.

[0227]

[0228] In particular, it was confirmed that the graft copolymers of Examples 1 to 4, in which the weight of the first molecular weight regulator was greater than the weight of the second molecular weight regulator, had improved impact strength compared to the graft copolymer of Example 5, in which the weights of the first and second molecular weight regulators were the same.

[0229]

[0230] In Comparative Examples 1 to 4, where no first molecular weight modifier was added, it was confirmed that the impact strength was significantly reduced compared to Examples 1 to 5. Meanwhile, referring to FIGS. 1 and 2, it was confirmed that the graft copolymer of Comparative Example 3 having a graft density exceeding 0.1 (FIG. 1) and the graft copolymer of Example 1 having a graft density not exceeding 0.1 (FIG. 2) were distinguishable in the TEM images.

[0231]

[0232] In the case of Comparative Example 5, in which the first molecular weight regulator was not added but the content of the graft copolymer was increased, it was confirmed that the impact strength was secured compared to Examples 1 to 5, but the tensile strength and pencil hardness were significantly reduced.

[0233]

[0234] In the case of Comparative Example 6, where a molecular weight regulator was added at the polymerization initiation stage, it was confirmed that the pencil hardness was similar to Examples 1 to 5, but the impact strength and fluidity index were reduced.

[0235]

[0236] In Comparative Examples 7 and 8, where the weight of the first molecular weight regulator was less than the weight of the second molecular weight regulator, it was confirmed that the impact strength was significantly reduced compared to Examples 1 to 5.

Claims

1. A step (S1) of initiating polymerization by batch-feeding a conjugated diene polymer, an aromatic vinyl monomer, and a vinyl cyan monomer into a reactor in the absence of a molecular weight regulator; and After the above step (S1) is initiated, a step (S2) is included in which an aromatic vinyl monomer, a vinyl cyan monomer, a first molecular weight regulator, and a second molecular weight regulator different from the first molecular weight regulator are simultaneously and continuously introduced into the reactor to perform polymerization. A method for producing a graft copolymer, wherein the weight of the first molecular weight regulator added is greater than or equal to the weight of the second molecular weight regulator added.

2. In paragraph 1, A method for producing a graft copolymer, wherein the weight of the second molecular weight regulator and the weight of the first molecular weight regulator are added in a ratio of 1:1 to 8.

3. In paragraph 1, A method for producing a graft copolymer, wherein the first molecular weight modifier is at least one selected from the group consisting of α-methyl styrene dimer, p-methyl styrene dimer, and 2,4-dimethyl styrene dimer.

4. In paragraph 1, A method for producing a graft copolymer, wherein the second molecular weight modifier is at least one selected from the group consisting of t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, carbon tetrachloride, methylene chloride, methylene bromide, tetraethyl thiuram disulfide, dipentamethylene thiuram disulfide, and diisopropylxanthogen disulfide.

5. In paragraph 1, A method for producing a graft copolymer, wherein the above step S1 is performed at a temperature of 40°C or higher and 55°C or lower.

6. In paragraph 1, A method for producing a graft copolymer, wherein the above step S2 is performed at a temperature of 60°C or higher and 75°C or lower.

7. In paragraph 1, For 100 parts by weight of the conjugated diene polymer, aromatic vinyl monomer, and vinyl cyan monomer introduced in the above step S1 and the aromatic vinyl monomer and vinyl cyan monomer introduced in the above step S2, A method for producing a graft copolymer, wherein the first molecular weight regulator and the second molecular weight regulator are added in an amount of 0.15 parts by weight or more and 0.95 parts by weight or less.

8. In paragraph 7, For 100 parts by weight of the conjugated diene polymer, aromatic vinyl monomer, and vinyl cyan monomer introduced in the above step S1 and the aromatic vinyl monomer and vinyl cyan monomer introduced in the above step S2, A method for producing a graft copolymer, wherein the first molecular weight regulator and the second molecular weight regulator are added in an amount of 0.3 parts by weight or more and 0.8 parts by weight or less.

9. Conjugated diene polymer; and A graft copolymer comprising a plurality of polymer chains grafted onto the above conjugated diene polymer, The above polymer chain includes an aromatic vinyl monomer unit and a vinyl cyan monomer unit, Surface area of ​​the above conjugated diene polymer is 1 nm 2 A graft copolymer having the number of polymer chains of which is 0.11 or less.

10. In paragraph 9, A graft copolymer having a graft ratio of 0.2 or more and 0.45 or less.

11. In paragraph 9, A graft copolymer having a weight average molecular weight of 80,000 g / mol or more and 140,000 g / mol or less.

12. Conjugated diene polymer; and A graft copolymer comprising a plurality of polymer chains grafted onto the above conjugated diene polymer, The above polymer chain includes an aromatic vinyl monomer unit and a vinyl cyan monomer unit, A graft copolymer having a graft density of 0.11 or less, as defined by the following mathematical formula 1: [Mathematical Formula 1] Graft density (nm) -2 ) = g d Dρ p N A / 6M g In mathematical equation 1, g d is the grafting rate (%) calculated by the following mathematical formula 2, D is the average particle diameter of the above conjugated diene polymer, ρ p is the particle density of the graft copolymer, N A is Avogadro's number, M g is the weight average molecular weight of the grafted multiple polymer chains measured by GPC after dissolving the dried product of the graft copolymer sol separated from the supernatant of the sol-gel separation method in a TFT solution. [Equation 2] Grafting ratio = weight (g) of the grafted plurality of polymer chains / weight (g) of the conjugated diene polymer 13. Graft copolymer according to claims 8 to 12; and A thermoplastic resin composition comprising a non-grafic copolymer comprising an aromatic vinyl monomer unit and a vinyl cyan monomer unit.

Citation Information

Patent Citations

  • Process for the preparation of thermoplastic resin composition

    KR100215389B1

  • Matted acrylonitile butadiene styrene resin and process thereof

    KR1019920008091A

  • Thermoplastic resin composition having superiorcoloring properties and impact strength and method forpreparing the same

    KR1020020035712A

  • Semiconductor package and a method of manufacturing the same

    KR102365004B1

  • KR20220154910A