Efficient flotation separation method for talc secondary copper-molybdenum bulk concentrate
Through low-concentration stirring and rapid scrubbing, multi-stage selection steps combining talc inhibitors and secondary copper inhibitors, the problem of difficulty in separating copper-molybdenum in talc secondary copper-molybdenum mixed concentrate is solved, and efficient copper-molybdenum is achieved Separation and high-grade concentrate acquisition.
Patent Information
- Application Number
- PCT/CN2023/115907
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-08
- Filing Date
- 2023-08-30
- Publication Date
- 2024-12-12
AI Technical Summary
In the talc secondary copper-molybdenum mixed concentrate, the floating ability of talc is good and the floating ability of molybdenum is small, which makes it difficult to separate copper-molybdenum. Conventional methods also inhibit molybdenum sulfide minerals when inhibiting talc, resulting in molybdenum. massive loss.
The talc inhibitor HD-3, composed of hypochlorite, sodium sulfide and sodium thiosulfate, is composed of low-concentration stirring and concentrated primary de-drug, rapid scrubbing and secondary de-drug. The secondary copper inhibitor NS can achieve efficient separation of copper and molybdenum through multi-stage selection steps.
It has achieved efficient flotation separation of talc secondary copper-molybdenum mixed concentrate, with short and stable process flow, low cost of drug consumption, good copper-molybdenum separation effect, and high grade of concentrate obtained, strong adaptability and high stability.
Smart Images

Figure CN2023115907_12122024_PF_FP_ABST
Abstract
Description
A high-efficiency flotation separation method for talc-type secondary copper-molybdenum mixed concentrate Technical Field
[0001] The invention belongs to the technical field of metallurgy and chemical industry, and in particular relates to a method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate. Background Art
[0002] Based on the strategic position of copper, molybdenum and other metals in the development of the national economy and their consumption demand, developing and utilizing copper, molybdenum and other metal resources and increasing their efficient separation and recovery are effective means to increase resource quantities. Technical issues
[0003] In talc-type secondary copper-molybdenum mixed concentrates, talc has good natural floatability, with little difference in floatability from molybdenite. Conventional methods for separating copper and molybdenum without the influence of talc include either removing the talc before separation or using CMC to suppress the flotation of sulfide minerals from the talc. However, actual production data shows that CMC not only suppresses the talc but also the molybdenum sulfide minerals, resulting in a large loss of molybdenum. Therefore, the development of a product that can address these technical issues is highly desirable. Technical Solutions
[0004] The object of the present invention is to provide a method for the efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate.
[0005] The object of the present invention is achieved in that the efficient flotation separation method of talc-type secondary copper-molybdenum mixed concentrate includes the steps of primary decontamination, secondary decontamination, rough separation, primary concentration, secondary concentration, tertiary concentration and quaternary concentration, specifically comprising:
[0006] A. Primary de-doping: Add water to the talc-type secondary copper-molybdenum mixed concentrate to be treated to prepare a slurry with a concentration of 5-15%, stir for 5-10 minutes to perform primary de-doping, and then concentrate it through a thickener to obtain thickener underflow a and return water b;
[0007] B. Secondary decontamination: The thickener underflow a enters the mill for scrubbing for 10-15 seconds to perform secondary decontamination to obtain a mixed concentrate c with a fineness of 70-95%-0.045mm;
[0008] C. Separation and roughing: The mixed concentrate c enters the flotation tank for separation and roughing to obtain molybdenum rough concentrate d and copper concentrate e;
[0009] D. Primary concentration: The molybdenum coarse concentrate d is slurried to obtain a slurry with a slurry concentration of 20-30%, and then 30-80 g / t of talc inhibitor is added and stirred for 2-4 minutes. Then, 70-150 g / t of secondary copper inhibitor is added and stirred for 4-6 minutes. The material f and the middlings g are obtained by flotation, and the middlings g are returned to the separation and roughing step;
[0010] E. Secondary concentration: Material f is slurried to obtain a slurry with a slurry concentration of 20-25%, and then 10-20 g / t of talc inhibitor is added and stirred for 4-6 minutes. Then, 15-50 g / t of secondary copper inhibitor is added and stirred for 4-6 minutes. Material h and middlings i are obtained by flotation, and middlings i are returned to the primary concentration step;
[0011] F. Tertiary concentration: Material h is slurried to obtain a slurry with a concentration of 20-25%, and flotation is performed without adding any reagents to obtain material j and middlings k. Middlings k are returned to the secondary concentration step;
[0012] G. Quaternary concentration: Material j is slurried to obtain a slurry with a slurry concentration of 20-25%, and flotation is performed without adding any reagents to obtain molybdenum concentrate and middlings l. The middlings l are returned to the tertiary concentration step.
[0013] The present invention utilizes a low-concentration stirring and concentration process for primary drug removal, rapid scrubbing for secondary drug removal, and a highly efficient flotation separation process. This process is short and stable, with low reagent costs, good return water utilization, and excellent copper-molybdenum separation. The resulting copper-molybdenum concentrate is high-grade, thus achieving efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate. The talc inhibitor HD-3 used is a combination of citric acid and polydextrose, and NS is a combination of hypochlorite, sodium sulfide, and sodium thiosulfate. HD-3 is easily soluble and selectively adheres to the talc surface, forming a hydrophilic film. NS favorably adsorbs copper minerals, reducing the surface contact angle and enhancing their hydrophilicity, thereby inhibiting their decomposition.
[0014] The specific operations are as follows:
[0015] (1) Primary de-doping: Add water to the prepared talc-type secondary copper-molybdenum mixed concentrate and stir it at a concentration of 5% to 15% for 5 to 10 minutes to promote the desorption of the agent on the mineral surface. After stirring, the concentrate is concentrated and de-doped by a thickener.
[0016] (2) Secondary dedoping: The thickener bottom flow in step (1) enters the mill and is quickly scrubbed for 10 to 15 seconds for secondary dedoping, while allowing the copper and molybdenum minerals to dissociate onto more fresh surfaces. After scrubbing, the fineness of the mixed concentrate is 70% to 95% -0.045mm.
[0017] (3) Separation and roughing: Add the mixed concentrate after scrubbing in step (2) into the flotation tank, adjust the pulp concentration to 35%~45%, add 50~100g / t talc inhibitor HD-3, stir for 3 minutes, then add 150~300g / t secondary copper inhibitor NS, stir for 5 minutes, and float out the molybdenum rough concentrate and copper concentrate.
[0018] (4) Selection 1: Add the molybdenum concentrate to the flotation tank, adjust the pulp concentration to 20%~30%, add 30~80g / t talc inhibitor HD-3, stir for 3 minutes, then add 70~150g / t secondary copper inhibitor NS and stir for 5 minutes, float out A and middling 1, and return middling 1 to step (3).
[0019] (5) Selection 2: Add the A obtained in step (4) into the flotation tank, adjust the pulp concentration to 20%~30%, add 10~20g / t talc inhibitor HD-3, stir for 3 minutes, then add 15~50g / t secondary copper inhibitor NS, stir for 5 minutes, float out B and middling 2, and return middling 2 to step (4).
[0020] (6) Selection 3: Add B from step (5) into the flotation tank, adjust the pulp concentration to 20%~25%, and perform blank selection without adding any reagents. Float out C and middling 3, and return middling 3 to step (5).
[0021] (7) Selection 4: Add C from step (6) into the flotation tank, adjust the pulp concentration to 20%~25%, and perform blank selection without adding any reagents. Float out the molybdenum concentrate and middlings 4, and return the middlings 4 to step (6). Beneficial effects
[0022] The present invention concentrates a 5%-15% talc-based secondary copper-molybdenum mixed concentrate to a concentration of 35%-45%, dehydrates it, and then scrubs it to remove the drug. The scrubbed concentrate is then transferred to a flotation cell, where a talc depressant and a secondary copper mineral depressant are added sequentially for rough separation of copper and molybdenum, yielding a rough molybdenum concentrate and a copper concentrate. The rough molybdenum concentrate is then subjected to five rounds of beneficiation to yield a molybdenum concentrate. The present invention utilizes a low-concentration talc-based secondary copper-molybdenum mixed concentrate for drug removal, followed by secondary drug removal by grinding and scrubbing, and then combines talc depressants with secondary copper mineral depressants for efficient flotation separation. This process shortens the process flow, provides good adaptability to talc-based secondary copper-molybdenum mixed concentrates with varying copper and molybdenum contents, enhances flotation stability, and achieves excellent copper-molybdenum separation. The resulting copper-molybdenum concentrate is of high grade, thus enabling efficient recycling of the talc-based secondary copper-molybdenum mixed concentrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] FIG1 is a schematic diagram of the process flow of the present invention. Modes for Carrying Out the Invention
[0024] The present invention is further described below with reference to the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention fall within the scope of protection of the present invention.
[0025] The high-efficiency flotation separation method of talc-type secondary copper-molybdenum mixed concentrate of the present invention comprises the steps of primary drug removal, secondary drug removal, rough separation, primary concentration, secondary concentration, tertiary concentration and quaternary concentration, specifically comprising:
[0026] A. Primary de-doping: Add water to the talc-type secondary copper-molybdenum mixed concentrate to be treated to prepare a slurry with a concentration of 5-15%, stir for 5-10 minutes to perform primary de-doping, and then concentrate it through a thickener to obtain thickener underflow a and return water b;
[0027] B. Secondary decontamination: The thickener underflow a enters the mill for scrubbing for 10-15 seconds to perform secondary decontamination to obtain a mixed concentrate c with a fineness of 70-95%-0.045mm;
[0028] C. Separation and roughing: The mixed concentrate c enters the flotation tank for separation and roughing to obtain molybdenum rough concentrate d and copper concentrate e;
[0029] D. Primary concentration: The molybdenum coarse concentrate d is slurried to obtain a slurry with a slurry concentration of 20-30%, and then 30-80 g / t of talc inhibitor is added and stirred for 2-4 minutes. Then, 70-150 g / t of secondary copper inhibitor is added and stirred for 4-6 minutes. The material f and the middlings g are obtained by flotation, and the middlings g are returned to the separation and roughing step;
[0030] E. Secondary concentration: Material f is slurried to obtain a slurry with a slurry concentration of 20-25%, and then 10-20 g / t of talc inhibitor is added and stirred for 4-6 minutes. Then, 15-50 g / t of secondary copper inhibitor is added and stirred for 4-6 minutes. Material h and middlings i are obtained by flotation, and middlings i are returned to the primary concentration step;
[0031] F. Tertiary concentration: Material h is slurried to obtain a slurry with a concentration of 20-25%, and flotation is performed without adding any reagents to obtain material j and middlings k. Middlings k are returned to the secondary concentration step;
[0032] G. Quaternary concentration: Material j is slurried to obtain a slurry with a slurry concentration of 20-25%, and flotation is performed without adding any reagents to obtain molybdenum concentrate and middlings l. The middlings l are returned to the tertiary concentration step.
[0033] The primary separation in step C is to slurry the mixed concentrate c to a pulp concentration of 35-45%, add 50-100 g / t of talc inhibitor, stir for 2-4 minutes, then add 150-300 g / t of secondary copper inhibitor, stir for 4-6 minutes, and flotate to obtain molybdenum crude concentrate d and copper concentrate e.
[0034] The talc inhibitor is HD-3, which is composed of citric acid and polydextrose.
[0035] The mass ratio of citric acid to polydextrose is (2-6): (4-8).
[0036] The secondary copper inhibitor is NS, which is composed of hypochlorite, sodium sulfide and sodium thiosulfate.
[0037] The mass ratio of the hypochlorite, sodium sulfide and sodium thiosulfate is (1-3): (4-8): (1-5).
[0038] The present invention will be further described below with reference to specific implementation cases:
[0039] Example 1
[0040] 1. Take talc-type secondary copper-molybdenum mixed concentrate containing 26.49% copper and 1.54% molybdenum. Add the mixed concentrate to a stirring tank with a slurry concentration of 8% and stir for 10 minutes. After stirring, the concentrate is concentrated in a thickener.
[0041] 2. The underflow of the thickener enters the grinding mill for scrubbing for 10 seconds. The fineness of the mixed concentrate is 80%-0.045mm, and then enters the flotation tank for separation and roughing.
[0042] 3. Separation and Roughing: Adjust the pulp concentration to 40%, first add 80g / t HD-3, stir for 3 minutes, then add 250g / t NS, and stir for 5 minutes. Roughing produces molybdenum concentrate and copper concentrate. The copper concentrate contains 27.33% copper, most of the talc is contained in the copper concentrate, and the copper concentrate contains 1.22% magnesium oxide.
[0043] 4. Adjust the slurry concentration of the molybdenum coarse concentrate to 30%, add 50g / t HD-3, stir for 3 minutes, then add 100g / t NS, stir for 5 minutes, float out A and middling ore 1, and return middling ore 1 to step 3.
[0044] 5. Adjust the concentration of slurry A to 25%, add 20g / t HD-3, stir for 3 minutes, then add 40g / t NS, stir for 5 minutes, float out B and middling ore 2, and return middling ore 2 to step 4.
[0045] 6. Adjust the concentration of B slurry to 25%, perform blank selection without adding any reagents, float out C and middling ore 3, and return middling ore 3 to step 5.
[0046] 7. Adjust the concentration of C slurry to 25%, and perform blank concentration without adding any reagents to float out molybdenum concentrate and middlings 4. Middlings 4 are returned to step 6. The molybdenum concentrate contains 47.82% molybdenum and the copper content in the molybdenum concentrate is 0.61%.
[0047] Example 2
[0048] 1. Take talc-type secondary copper-molybdenum mixed concentrate containing 28.62% copper and 1.86% molybdenum. Add the mixed concentrate to a stirring tank with a slurry concentration of 5%. Stir for 10 minutes and then concentrate it in a thickener.
[0049] 2. The underflow of the thickener enters the grinding mill for scrubbing for 15 seconds. The fineness of the mixed concentrate is 95%-0.045mm, and then enters the flotation tank for separation and roughing.
[0050] 3. Separation and Roughing: Adjust the pulp concentration to 35%, add 30g / t HD-3, stir for 4 minutes, then add 200g / t NS, and stir for 4 minutes. Roughing produces molybdenum concentrate and copper concentrate. The copper concentrate contains 29.63% copper, most of the talc is contained in the copper concentrate, and the copper concentrate contains 1.02% magnesium oxide.
[0051] 4. Adjust the slurry concentration of the molybdenum coarse concentrate to 20%, add 50g / t HD-3, stir for 3 minutes, then add 70g / t NS, stir for 5 minutes, float out A and middling ore 1, and return middling ore 1 to step 3.
[0052] 5. Adjust the concentration of A slurry to 20%, add 10g / t HD-3, stir for 2 minutes, then add 30g / t NS, stir for 4 minutes, float out B and middling ore 2, and return middling ore 2 to step 4.
[0053] 6. Adjust the concentration of B slurry to 20%, perform blank selection without adding any reagents, float out C and middling ore 3, and return middling ore 3 to step 5.
[0054] 7. Adjust the concentration of C slurry to 20%, and perform blank concentration without adding any reagents to float out molybdenum concentrate and middlings 4. Middlings 4 are returned to step 6. The molybdenum concentrate contains 49.53% molybdenum and the copper content in the molybdenum concentrate is 0.53%.
[0055] Example 3
[0056] 1. Take talc-type secondary copper-molybdenum mixed concentrate containing 31.17% copper and 1.34% molybdenum. Add the mixed concentrate to a stirring tank with a slurry concentration of 15%. Stir for 5 minutes and then concentrate it in a thickener.
[0057] 2. The underflow of the thickener enters the grinding mill for scrubbing for 13 seconds. The fineness of the mixed concentrate is 70%-0.045mm, and then enters the flotation tank for separation and roughing.
[0058] 3. Separation and Roughing: Adjust the pulp concentration to 38%. First, add 100g / t HD-3 and stir for 4 minutes. Then add 300g / t NS and stir for 6 minutes. Roughing produces molybdenum concentrate and copper concentrate. The copper concentrate contains 32.46% copper. Most of the talc is contained in the copper concentrate. The copper concentrate contains 0.98% magnesium oxide.
[0059] 4. Adjust the slurry concentration of the molybdenum coarse concentrate to 25%, add 80g / t HD-3, stir for 4 minutes, then add 150g / t NS, stir for 6 minutes, float out A and middling ore 1, and return middling ore 1 to step 3.
[0060] 5. Adjust the concentration of ore A to 23%, add 15g / t HD-3, stir for 4 minutes, then add 50g / t NS, stir for 6 minutes, float out ore B and middling ore 2, and return middling ore 2 to step 4.
[0061] 6. Adjust the concentration of B slurry to 23%, perform blank selection without adding any reagents, float out C and middling ore 3, and return middling ore 3 to step 5.
[0062] 7. Adjust the concentration of C slurry to 23%, and perform blank concentration without adding any reagents to float out molybdenum concentrate and middlings 4. Middlings 4 are returned to step 6. The molybdenum concentrate contains 48.88% molybdenum and the molybdenum concentrate contains 0.24% copper.
[0063] Example 4
[0064] 1. Take talc-type secondary copper-molybdenum mixed concentrate containing 29.12% copper and 1.47% molybdenum. Add the mixed concentrate to a stirring tank with a slurry concentration of 7% and stir for 8 minutes. After stirring, the concentrate is concentrated in a thickener.
[0065] 2. The underflow of the thickener enters the grinding mill for scrubbing for 12 seconds. The fineness of the mixed concentrate is 85%-0.045mm, and then enters the flotation tank for separation and roughing.
[0066] 3. Separation and Roughing: Adjust the pulp concentration to 36%. First, add 60g / t HD-3 and stir for 2 minutes. Then add 150g / t NS and stir for 5 minutes. Roughing produces molybdenum concentrate and copper concentrate. The copper concentrate contains 30.58% copper. Most of the talc is contained in the copper concentrate. The copper concentrate contains 1.21% magnesium oxide.
[0067] 4. Adjust the slurry concentration of the molybdenum coarse concentrate to 28%, add 60g / t HD-3, stir for 2 minutes, then add 120g / t NS, stir for 4 minutes, float out A and middling ore 1, and return middling ore 1 to step 3.
[0068] 5. Adjust the concentration of ore A to 22%, add 16g / t HD-3, stir for 3 minutes, then add 15g / t NS, stir for 5 minutes, float out ore B and middling ore 2, and return middling ore 2 to step 4.
[0069] 6. Adjust the concentration of B slurry to 22%, perform blank selection without adding any reagents, float out C and middling 3, and return middling 3 to step 5.
[0070] 7. Adjust the concentration of C slurry to 22%, and perform blank concentration without adding any reagents to float out molybdenum concentrate and middlings 4. Middlings 4 are returned to step 6. The molybdenum concentrate contains 48.98% molybdenum and the molybdenum concentrate contains 0.57% copper.
Claims
1. A method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate, characterized in that: The highly efficient flotation separation method of talc-type secondary copper-molybdenum mixed concentrate comprises the steps of primary decontamination, secondary decontamination, separation roughing, primary concentration, secondary concentration, tertiary concentration and quaternary concentration, specifically comprising: A. Primary dedoping: add water to the talc-type secondary copper-molybdenum mixed concentrate to be treated to prepare a slurry with a concentration of 5-15%, stir for 5-10 minutes to perform primary dedoping, and then concentrate it through a thickener to obtain a thickener underflow a and return water b; B. Secondary decontamination: The thickener underflow a enters the mill for scrubbing for 10-15 seconds to obtain a mixed concentrate c with a fineness of 70-95%-0.045mm; C. Separation and roughing: The mixed concentrate c is sent into the flotation tank for separation and roughing to obtain molybdenum rough concentrate d and copper concentrate e; D. Primary concentration: the molybdenum rough concentrate d is slurried to obtain a slurry with a slurry concentration of 20-30%, and then 30-80 g / t of talc inhibitor is added, stirred for 2-4 min, and then 70-150 g / t of secondary copper inhibitor is added, stirred for 4-6 min, and flotation is performed to obtain material f and middlings g, and the middlings g are returned to the separation and roughing step; E. Secondary concentration: Material f is slurried to obtain a slurry with a slurry concentration of 20-25%, and then 10-20 g / t of talc inhibitor is added, stirred for 4-6 min, and then 15-50 g / t of secondary copper inhibitor is added, stirred for 4-6 min, and flotation is performed to obtain material h and middlings i, and the middlings i are returned to the primary concentration step; F. Tertiary concentration: Material h is slurried to obtain a slurry with a slurry concentration of 20-25%, and flotation is performed without adding any reagents to obtain material j and middling k, and middling k is returned to the secondary concentration step; G. Fourth-stage concentration: Material j is slurried to obtain a slurry with a slurry concentration of 20-25%, and molybdenum concentrate and middlings l are obtained by flotation without adding any reagents. The middlings l are returned to the third-stage concentration step.
2. The method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate according to claim 1, characterized in that: The preliminary separation in step C is to slurry the mixed concentrate c to a slurry concentration of 35-45%, add 50-100 g / t of talc inhibitor, stir for 2-4 min, then add 150-300 g / t of secondary copper inhibitor, stir for 4-6 min, and flotate to obtain molybdenum rough concentrate d and copper concentrate e.
3. The method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate according to claim 1 or 2, characterized in that: The talc inhibitor is HD-3, which is composed of citric acid and polydextrose.
4. The method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate according to claim 3, characterized in that: The mass ratio of citric acid to polydextrose is (2-6):(4-8).
5. The method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate according to claim 1 or 2, characterized in that: The secondary copper inhibitor is NS, which is composed of hypochlorite, sodium sulfide and sodium thiosulfate.
6. The method for efficient flotation separation of talc-type secondary copper-molybdenum mixed concentrate according to claim 5, characterized in that: The mass ratio of the hypochlorite, sodium sulfide and sodium thiosulfate is (1-3): (4-8): (1-5).
Citation Information
Patent Citations
Copper-molybdenum separation depressant and application and use method thereof
CN110813542A
Method for utilizing copper-molybdenum bulk concentrate beneficiation backwater
CN113275129A
Beneficiation method for realizing efficient separation of copper and molybdenum by strengthening reagent removal of copper-molybdenum concentrate
CN113941434A
Flotation separation method for copper-molybdenum bulk concentrate
CN115025875A
Efficient flotation separation method for talc type secondary copper-molybdenum bulk concentrate
CN116493139A
Cited By
Flotation method for porphyry type copper-molybdenum ore
CN122273688A