Low-alkali accelerator and preparation method therefor
By using strong alkali weak acid salts and silica gel modified fluoride salts in the preparation of low alkali quick-coagulant, the silica gel is used to encapsulate fluoride ions, which solves the problem of poor storage stability of low alkali quick-coagulant. It achieves better storage stability and the effect of fast-setting in cement.
Patent Information
- Application Number
- PCT/CN2024/089389
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-09
- Filing Date
- 2024-04-23
- Publication Date
- 2024-12-12
AI Technical Summary
The poor storage stability of existing low-alkali accelerator affects its promotion and use.
Through the preparation method, sodium metaaluminate solution and aluminum sulfate are added first, and the pH value is adjusted to neutral, and the modified fluoride salt is added. The fluoride salt is modified using strong alkali and weak acid salt and silica gel. , promote the hydrolysis of fluoride salt, generate silica gel wrapped with fluoride ions and aluminum ions, weaken their binding chances, avoid the formation of aluminum fluoride crystals, and improve storage stability.
It effectively avoids the low-alkali accelerator to generate crystals during storage, improves storage stability, and plays a quick-coagulation role in cement slurry or mortar, which is better than the low-alkali accelerator with unmodified fluoride salts.
Smart Images

Figure CN2024089389_12122024_PF_FP_ABST
Abstract
Description
A low-alkali quick-setting agent and its preparation method
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on June 9, 2023, with application number 202310682303.5 and application name, entitled A low-alkali quick-setting agent and a preparation method thereof, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The present application relates to the technical field of concrete processing, and in particular to a low-alkali quick-setting agent and a preparation method thereof. Background Art
[0003] Accelerators are essential ingredients in concrete preparation, increasing the early strength of concrete while also increasing the shrinkage of mortar and cement. Commonly used accelerators for cement concrete are categorized by their alkali content: alkaline accelerators and low-alkali accelerators. Alkaline accelerators, due to their high alkali content, are highly corrosive, corroding construction equipment and potentially endangering human health during production and construction. Consequently, they are being replaced by low-alkali accelerators.
[0004] However, in actual use, it was found that the storage stability of low-alkali accelerator was poor, which affected the promotion and use of low-alkali accelerator.
[0005] Application Contents
[0006] (1) Technical problems solved
[0007] In view of the shortcomings of the existing technology, the present application provides a low-alkali accelerator and a preparation method thereof, which solves the technical problem of poor storage stability of the existing low-alkali accelerator.
[0008] (2) Technical solution
[0009] To achieve the above objectives, this application is implemented through the following technical solutions:
[0010] A method for preparing a low-alkali quick-setting agent comprises the following steps:
[0011] S1, prepare sodium aluminate solution;
[0012] S2. Add water to the sodium aluminate solution, stir evenly, then add aluminum sulfate, and react at 50-80° C. under stirring for 0.5-1 h;
[0013] S3. Within 10 to 30 minutes after the aluminum sulfate reaction is complete, add a regulator dropwise to adjust the pH value to neutral;
[0014] S4, after uniformly mixing the strong base weak acid salt and the silica gel, add the fluoride salt, mix them uniformly to obtain a modified fluoride salt; add the modified fluoride salt to the neutral solution of S3, and keep the temperature at 50-80°C for 1-1.5 hours;
[0015] S5. Add organic alcohol amine and stir for 0.5 to 1 hour to obtain low-alkali quick-setting agent.
[0016] Preferably, the silica gel is hydrophilic.
[0017] Preferably, the specific surface area of the silica gel is 600 to 800 m2 / g.
[0018] Preferably, the sodium metaaluminate solution comprises sodium hydroxide and aluminum hydroxide, and the mass ratio of the sodium hydroxide to the aluminum hydroxide is 1:2.5 to 3.5.
[0019] On the other hand, a low-alkali accelerator prepared by the preparation method, wherein the weight percentage of the low-alkali accelerator is:
[0020] The modifier comprises: a strong base weak acid salt and silicon dioxide gel, and the mass ratio of the strong base weak acid salt to the silicon dioxide gel is 2 to 4:1.
[0021] Preferably, the strong base and weak acid salt includes at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, sodium sulfite, sodium acetate, sodium sulfide, and sodium phosphate.
[0022] Preferably, the fluoride salt includes at least one of sodium fluoride, sodium fluorosilicate, and magnesium fluorosilicate.
[0023] Preferably, the fluoride salt includes sodium fluoride, sodium fluorosilicate, and magnesium fluorosilicate.
[0024] Preferably, the mass ratio of sodium fluoride, sodium fluorosilicate and magnesium fluorosilicate is (1-2):(5-7):(2-3).
[0025] Preferably, the mass ratio of sodium fluoride, sodium fluorosilicate and magnesium fluorosilicate is 1.5:6:2.5.
[0026] (3) Beneficial effects
[0027] This application provides a low-alkali accelerator and its preparation method. Compared with the existing technology, it has the following advantages:
[0028] The preparation method of the low-alkali accelerator provided in the present application is to first add sodium metaaluminate solution and aluminum sulfate, adjust the pH value to neutral, and then add modified fluoride salt. The modifier includes a strong base weak acid salt. Under neutral conditions, the strong base weak acid salt hydrolyzes, and the hydrolysis of the strong base weak acid salt further promotes the hydrolysis of the fluoride salt. The hydrolysis of the fluoride salt generates fluoride ions and silica gel. In the prepared low-alkali accelerator system, the generated silica gel encapsulates the fluoride ions and aluminum ions in the system, reducing the probability of the fluoride ions and aluminum ions combining, thereby avoiding the formation of aluminum fluoride crystals during storage and slowly agglomerating into large particles. Therefore, the prepared low-alkali accelerator does not produce crystals during storage and has good storage stability. The modifier also includes silica gel, which further encapsulates fluoride ions and chloride ions, thereby improving the storage stability of the low-alkali accelerator during storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0030] FIG1 is a state diagram of the low-alkali quick-setting agent prepared in Example 1 after storage for 90 days;
[0031] FIG2 is a state diagram of the low-alkali quick-setting agent prepared in Comparative Example 1 after storage for 3 days;
[0032] FIG3 is a state diagram of the low-alkali quick-setting agent prepared in Comparative Example 2 after storage for 5 days;
[0033] FIG4 is a state diagram of the low-alkali quick-setting agent prepared in Comparative Example 3 after storage for 5 days. DETAILED DESCRIPTION
[0034] To make the objectives, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application are clearly and completely described. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0035] The embodiments of the present application solve the technical problem of poor storage stability of existing low-alkali accelerators by providing a low-alkali accelerator and a preparation method thereof.
[0036] The technical solution in the embodiments of the present application is to solve the above technical problems, and the overall idea is as follows:
[0037] During the preparation of low-alkali accelerators, fluoride salts are first modified using a strong base weak acid salt and silica gel, and then the modified fluoride salt is used to prepare the low-alkali accelerator system. The modified fluoride salt promotes the hydrolysis of sodium fluorosilicate to form silica gel. The newly generated silica gel and the silica gel in the modifier can respectively encapsulate the fluoride and chloride ions in the low-alkali accelerator system, reducing the binding probability of fluoride and aluminum ions. This prevents the formation of small aluminum fluoride particles that slowly agglomerate into larger particles during storage, thereby improving the storage stability of the low-alkali accelerator.
[0038] The modifier also includes silica gel, which further encapsulates fluoride and chloride ions, improving the storage stability of the low-alkali accelerator. Especially during the initial hydrolysis of the fluoride salt, when less silica gel is produced, the silica gel can better encapsulate the fluoride ions produced by hydrolysis, preventing them from contacting the chloride ions and ensuring that small aluminum fluoride particles are not generated during the preparation process.
[0039] In the early stage of fluoride salt hydrolysis, the silica gel in the modifier can also inhibit the hydrolysis of fluoride salt and reduce its hydrolysis rate to avoid the hydrolysis rate being too fast and producing a large amount of fluoride ions that combine with aluminum ions to form small aluminum fluoride particles, which will cause the low-alkali accelerator to produce particulate matter during the preparation process.
[0040] In order to better understand the above technical solution, the above technical solution will be described in detail below with reference to the accompanying drawings and specific implementation methods.
[0041] Example 1:
[0042] This embodiment provides a method for preparing a low-alkali accelerator, comprising the following steps:
[0043] S1. Take appropriate amount of water and prepare sodium metaaluminate solution by mixing sodium hydroxide and aluminum hydroxide in a mass ratio of 1:2.5;
[0044] S2. Add appropriate amount of water to the sodium aluminate solution, stir evenly, then add aluminum sulfate to the above system at once, start stirring and heating, set the reaction temperature to 60°C and keep the reaction for 0.5h;
[0045] S3. After the aluminum sulfate reaction is complete, a regulator is added dropwise to the above system within 10 minutes to adjust the pH value to neutral;
[0046] S4. Using a stirring device, sodium carbonate and hydrophilic silica gel in a mass ratio of 2:1 are mixed to obtain a modifier, which is then added to sodium fluorosilicate and mixed to obtain modified sodium fluorosilicate;
[0047] The specific surface area of silica gel is 600㎡ / g;
[0048] Add modified sodium fluorosilicate to the neutral solution of S3 and keep the temperature at 60℃ for 1 hour;
[0049] S5. Turn off the heating, add organic alcohol amine, and stir for 0.5 hours to obtain the low-alkali quick-setting agent.
[0050] Low-alkali accelerator does not produce particulate matter during the preparation process.
[0051] The weight percentage of the prepared low-alkali quick-setting agent is:
[0052] Example 2
[0053] This embodiment provides a method for preparing a low-alkali accelerator, comprising the following steps:
[0054] S1, sodium hydroxide and aluminum hydroxide are prepared into a sodium metaaluminate solution in a mass ratio of 1:3;
[0055] S2. Add water to the sodium aluminate solution and stir evenly. Then add aluminum sulfate to the above system at once. Start stirring and heating. Set the reaction temperature to 70°C and keep the reaction warm for 0.8h.
[0056] S3. After the aluminum sulfate reaction is complete, a regulator is added dropwise to the above system within 20 minutes to adjust the pH value to neutral;
[0057] S4. Using a stirring device, sodium bicarbonate and silica gel in a mass ratio of 3:1 are mixed to obtain a modifier, which is then added to magnesium fluorosilicate and mixed to obtain modified magnesium fluorosilicate;
[0058] Silica gel is hydrophilic and has a specific surface area of 700 m2 / g;
[0059] Add the modified magnesium fluorosilicate to the neutral solution of S3 and keep the temperature at 70℃ for 1.2h;
[0060] S5. Turn off the heating, add organic alcohol amine, and stir for 0.8h to obtain the low-alkali quick-setting agent.
[0061] Low-alkali accelerator does not produce particulate matter during the preparation process.
[0062] The weight percentage of the prepared low-alkali quick-setting agent is:
[0063] Example 3
[0064] This embodiment provides a method for preparing a low-alkali accelerator, comprising the following steps:
[0065] S1, sodium hydroxide and aluminum hydroxide are prepared into a sodium metaaluminate solution in a mass ratio of 1:3.5;
[0066] S2. Add water to the sodium aluminate solution and stir evenly. Then add aluminum sulfate to the above system at once. Start stirring and heating. Set the reaction temperature to 80°C and keep the reaction for 1 hour.
[0067] S3. After the aluminum sulfate reaction is complete, a regulator is added dropwise to the above system within 30 minutes to adjust the pH value to neutral;
[0068] S4. Use a stirring device to mix potassium carbonate and silica gel in a mass ratio of 4:1, and then add them to the fluoride salt, and mix them evenly to obtain modified fluoride salt; the fluoride salt includes sodium fluoride, sodium fluorosilicate, and magnesium fluorosilicate, and the mass ratio of sodium fluoride, sodium fluorosilicate, and magnesium fluorosilicate is 1.5:6:2.5.
[0069] Silica gel is hydrophilic and has a specific surface area of 800 m2 / g;
[0070] Add the modified fluoride salt to the neutral solution of S3 and keep the temperature at 80℃ for 1.5h;
[0071] S5. Turn off the heating, add organic alcohol amine, and stir for 1 hour to obtain the low-alkali quick-setting agent.
[0072] Low-alkali accelerator does not produce particulate matter during the preparation process.
[0073] The weight percentage of the prepared low-alkali quick-setting agent is:
[0074] Comparative Example 1:
[0075] The difference between this comparative example and Example 1 is that sodium fluorosilicate is not modified, that is, sodium fluorosilicate is added to the neutral solution of S3. Other aspects are the same as Example 1.
[0076] Particulate matter was generated during the formulation process.
[0077] Comparative Example 2:
[0078] The difference between this comparative example and Example 1 is that only sodium carbonate is used to modify sodium fluorosilicate, and the other conditions are the same as Example 1.
[0079] The prepared low-alkali quick-setting agent contains no particles.
[0080] Comparative Example 3
[0081] The difference between this comparative example and Example 1 is that only silica gel is used to modify sodium fluorosilicate, and the rest is the same as Example 1.
[0082] The prepared low-alkali quick-setting agent contains no particles.
[0083] The storage stability of the low-alkali quick-setting agents prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was tested. The test results are shown in Table 1.
[0084] Storage stability test method: Store the prepared low-alkali accelerator at room temperature and pressure. After standing for a certain period of time, observe whether obvious crystals appear in the low-alkali accelerator system and record the time. The maximum standing time is 90 days. Figure 1 shows the state of the low-alkali accelerator prepared in Example 1 after 90 days of storage. No obvious crystals appear. Figure 2 shows the state of the low-alkali accelerator prepared in Comparative Example 1 after 3 days of storage. Clear crystals appear. Figure 3 shows the state of the low-alkali accelerator prepared in Comparative Example 2 after 5 days of storage. Clear crystals appear. Figure 4 shows the state of the low-alkali accelerator prepared in Comparative Example 3 after 5 days of storage. Clear crystals appear.
[0085] Table 1 Storage stability test results of low-alkali accelerator prepared
[0086] The results in Table 1 show that the low-alkali accelerator prepared by modifying the fluoride salt with a strong base, weak acid salt and silica gel before adding it to the system exhibited excellent stability, with no obvious crystallization within 90 days. When the fluoride salt was added directly to the system without modification, the low-alkali accelerator exhibited obvious crystallization after 3 days. Therefore, modifying the fluoride salt with a strong base, weak acid salt and silica gel can improve the stability of the low-alkali accelerator. However, when the fluoride salt was modified with either a strong base, weak acid salt or silica gel alone, the low-alkali accelerator also exhibited obvious crystallization after 5 days, respectively. This may be because the synergistic effect of the strong base, weak acid salt and silica gel effectively improves the storage stability of the low-alkali accelerator.
[0087] In accordance with the standard of GB / T 35159-2017 "Accelerators for Shotcrete", the low-alkali accelerators prepared in Examples 1 to 3 and Comparative Examples 1 to 3 after storage for 5 days were added to the cement paste at an amount of 4% and 6% of the weight of the cement, respectively. The setting time of the cement paste and the compressive strength of the cement mortar were tested, as shown in Table 2.
[0088] The test ratio of cement paste setting time is: base cement: water = 400:140.
[0089] The test ratio of cement mortar compressive strength is: base cement: standard sand: water = 900:1350:450.
[0090] Table 2 Setting time and compressive strength test results
[0091] As can be seen from Table 2, the low-alkali accelerators prepared in Examples 1-3 have better setting time and compressive strength when used in cement paste or cement mortar than the low-alkali accelerators prepared in Comparative Examples 1-3. This is because the low-alkali accelerators prepared by modifying the fluoride salt with a strong base and weak acid salt and silica gel before adding it to the system have good stability. When the low-alkali accelerator is added to the cement paste or cement mortar, the amount of effective ingredients that can exert the accelerating effect is large.
[0092] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply the existence of any such actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article, or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or device. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of other identical elements in the process, method, article, or device comprising the element.
[0093] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing a low-alkali accelerating setting agent, characterized in that: The steps include: S1, preparing sodium aluminate solution; S2, adding water to the sodium aluminate solution, stirring evenly, then adding aluminum sulfate, and reacting at 50-80° C. for 0.5-1 h under stirring conditions; S3, after the aluminum sulfate is completely dissolved, adjusting the pH value to neutral to obtain a neutral solution; S4, after uniformly mixing the strong base weak acid salt and the silica gel, adding the fluoride salt, and mixing them uniformly to obtain the modified fluoride salt; Adding the modified fluoride salt to the neutral solution, and keeping the temperature at 50-80° C. for 1-1.5 hours; S5. Add organic alcohol amine and stir for 0.5 to 1 hour to obtain the low-alkali quick-setting agent.
2. The preparation method according to claim 1, characterized in that The silica gel is hydrophilic.
3. The preparation method according to claim 1, characterized in that: The specific surface area of the silica gel is 600-800 m2 / g.
4. The preparation method according to claim 1, characterized in that: The sodium aluminate solution comprises sodium hydroxide and aluminum hydroxide, and the mass ratio of the sodium hydroxide to the aluminum hydroxide is 1:2.5-3.
5.
5. A low-alkali quick-setting agent prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The weight percentage of the low-alkali accelerating setting agent is: The modifier comprises: a strong base and a weak acid salt and silicon dioxide gel, wherein the strong base and the weak acid salt, The mass ratio of silica gel is 2 to 4:
1.
6. The low-alkali quick-setting agent according to claim 5, characterized in that: The strong base and weak acid salt include at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, sodium sulfite, sodium acetate, sodium sulfide, and sodium phosphate.
7. The low-alkali quick-setting agent according to claim 5, characterized in that: The fluoride salt includes at least one of sodium fluoride, sodium fluorosilicate and magnesium fluorosilicate.
8. The low-alkali quick-setting agent according to claim 5, characterized in that: The fluoride salts include sodium fluoride, sodium fluorosilicate, and magnesium fluorosilicate.
9. The low-alkali quick-setting agent according to claim 8, characterized in that: The mass ratio of the sodium fluoride, sodium fluorosilicate and magnesium fluorosilicate is (1-2):(5-7):(2-3).
10. The low-alkali quick-setting agent according to claim 8, characterized in that: The mass ratio of the sodium fluoride, sodium fluorosilicate and magnesium fluorosilicate is 1.5:6:2.5.
Citation Information
Patent Citations
Low-alkaline accelerator and preparation method thereof
CN103979818A
Preparation method of alkalescent liquid accelerator
CN107311499A
Alkali-free liquid accelerator and preparation method thereof
CN109896771A
Low-temperature-resistant liquid alkali-free accelerator and preparation method thereof
CN110615638A
High-performance alkali-free liquid accelerator and preparation method thereof
CN111960713A
Cited By
Waterproof dense setting accelerator as well as preparation method and application thereof
CN120554022A