Silver nano-zinc oxide composite nanostructure for amplifying fluorescence signal of gene probe labeled with fluorescence, method for manufacturing same, and method for detecting fluorescence signal

The 3D silver nano-oxide composite nanostructure enhances fluorescence signal amplification and sensitivity for DNA detection by optimizing the interaction between silver nanoparticles and fluorescent molecules, addressing limitations of 2D MEF substrates in biosensor technology.

WO2025014212A1PCT designated stage expired Publication Date: 2025-01-16KOREA RES INST OF CHEM TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/009637
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-10
Filing Date
2024-07-08
Publication Date
2025-01-16

AI Technical Summary

Technical Problem

Current 2D metal-enhanced fluorescent (MEF) substrates for biosensors face limitations in sensitivity and reproducibility due to limited interaction between biomolecules and metal structures in aqueous environments, particularly in DNA detection, where low quantum efficiency and fluorescence signal amplification are constraints.

Method used

Development of a 3D silver nano-oxide composite nanostructure (AG-ZNO NC) using thermal water synthesis of ZnO nanowires and silver nanoparticles, which enhances fluorescence signal amplification by optimizing the distance between silver nanoparticles and fluorescent molecules, thereby improving interaction and sensitivity.

Benefits of technology

The AG-ZNO NC substrate achieves significant fluorescence signal amplification, with improvements of up to 100 times, and demonstrates 50 times higher sensitivity for DNA detection compared to traditional 2D MEF substrates, facilitating more accurate and efficient DNA detection in aqueous environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024009637_16012025_PF_FP_ABST
    Figure KR2024009637_16012025_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a silver nano-zinc oxide composite nanostructure for amplifying a fluorescence signal of a gene probe labeled with fluorescence, to a method for manufacturing same, and to a method for detecting a fluorescence signal and, more specifically, to a silver nano-zinc oxide nanowire in which a nanowire is grown on a substrate, silver nanoparticles formed on the nanowire and a gene probe labeled with fluorescence are comprised, and a distance, at which a metal fluorescence signal can be amplified, between the silver nanoparticles formed on the nanowire and fluorescent molecules of the gene probe is maintained so that the fluorescence signal is amplified. The silver nano-zinc oxide nanowire of the present invention has improved detection sensitivity, thereby enabling more accurate diagnosis.
Need to check novelty before this filing date? Find Prior Art

Description

Silver nano-zinc oxide composite nanostructure for amplifying the fluorescence signal of a fluorescently labeled genetic probe, a method for manufacturing the same, and a method for detecting the fluorescence signal

[0001] The present invention relates to a silver nano-zinc oxide composite nanostructure that amplifies the fluorescence signal of a fluorescently labeled genetic probe, a method for producing the same, and a method for detecting the fluorescence signal.

[0002] Fluorescence-based detection is a key technology in biosensor applications for detecting disease biomarkers. Using fluorescent molecules as biosensors offers numerous advantages, including simplicity, sensitivity, and multi-analyte detection. However, fluorescence-based detection faces limitations due to low quantum efficiency and photostability, which are crucial criteria for biosensor development.

[0003] Enhancement of fluorescence signals has been extensively investigated in biosensor technology. Metal-enhanced fluorescence (MEF) is a phenomenon resulting from plasmonic coupling between metal nanostructures / nanoparticles (NPs) and fluorophores, which enhances quantum yield and photostability at an optimal distance of 5–90 nm. It has been studied in the development of sensitive biosensors for detecting biomarkers such as genes and proteins. In particular, two-dimensional (2D) MEF substrates, which can be easily controlled at an optimal distance, have been thoroughly explored, but their applications remain limited due to their sensitivity to biological environments. Various fabrication methods for 2D MEF substrates, including layer-by-layer (LbL) deposition of metal thin films, rough NP deposition, aligned NP array nanostructures, nanoimprinted metal pattern arrays, polymer spacers, dielectric spacers, or hybrid composite spacers, have been developed for biosensor applications. However, these 2D MEF substrates suffer from several limitations, such as low enhancement factors and poor reproducibility, due to limited recognition and diffusion of biomolecules between target molecules, biological probes, and the MEF substrate in aqueous environments. Recently, three-dimensional (3D) substrates for MEFs have been studied, and their advantages include significant fluorescence enhancement, sensitive detection, and an enhanced dynamic range for biomarker detection. Therefore, novel 3D MEF substrates are required as biosensors to improve the interactions between biomolecules and metal structures in aqueous environments.

[0004] The present invention developed Ag-ZnO nanocomposite (NC) through two steps: hydrothermal synthesis of ZnO NWs as building blocks of Ag NPs and photochemical deposition of AgNPs onto ZnO NWs. The fluorescence enhancement of Ag-ZnO NCs as a 3D MEF substrate was 14.8-fold, 16.9-fold, 11.4-fold, and 14.2-fold in the presence of 10, 20, 40, and 60 base pair (bp) double-stranded (ds) DNA, respectively. This enhancement is suggested to be related to the improved interaction between the fluorophore and the Ag-ZnO NC substrate. Ag-ZnO NCs exhibited 50-fold higher sensitivity than Ag nanoisland films (AgNIFs) for detecting dsDNA when used as a 2D MEF substrate. These results indicate that the fluorophore can be enhanced through a wide range of interactions with Ag-ZnO NCs in various scenarios, including not only the interaction between the fluorophore and AgNPs when the fluorophore is immobilized, but also the interaction between the fluorophore and adjacent AgNPs within the ZnO NW strand, and other interactions between the fluorophore and adjacent AgNPs fabricated on different ZnO NW strands. Our Ag-ZnO NCs can facilitate the development of MEF-based biosensors for DNA detection in aqueous environments.

[0005] Meanwhile, Korean Patent No. 1878404 relates to a metal-enhanced fluorescent composite nanostructure and a method for manufacturing the same, and a method for detecting a fluorescent material, and discloses a metal-enhanced fluorescent composite nanostructure and a method for manufacturing the same, and a method for detecting a fluorescent material, in which a first plasmonic material and a second plasmonic material are simultaneously deposited on a substrate surface by a thermal evaporation method to form a plurality of plasmonic composite nanoislands; Korean Patent No. 1470819 relates to a method for manufacturing a fluorescent signal amplification substrate and a DNA and protein microarray chip using the method, and discloses a method for manufacturing a fluorescent signal amplification substrate using a stamp substrate on which a nanostructure having a groove-shaped pattern is formed; and Korean Patent No. 1597894 relates to a core-shell nanocomposite for metal-enhanced fluorescent light, and discloses a core-shell nanocomposite including fluorescent materials positioned at a constant interval in a direction perpendicular to a surface, a method for manufacturing the same, and a use as a probe for metal-enhanced fluorescent light.

[0006] However, a silver nano-zinc oxide composite nanostructure that amplifies the fluorescence signal of the fluorescently labeled genetic probe of the present invention, a method for producing the same, and a method for detecting the fluorescence signal have not been disclosed.

[0007] The purpose of the present invention is to solve the above problems, and to enable the introduction of more biomolecules based on the effect of increasing the surface area by applying zinc oxide nanowires, and to complete the present invention by confirming the effect of amplifying the fluorescence signal by up to 100 times by metal-enhanced fluorescence when the distance between the fluorescent molecule and the silver nanoparticle is 5 to 95 nm by using zinc oxide nanowires formed with silver nanoparticles.

[0008] In order to solve the above problem, the present invention provides a silver nano zinc oxide nanowire comprising: a substrate; a nanowire grown on the substrate; and silver nanoparticles formed on the nanowire; a fluorescently labeled genetic probe; and a distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, which allows amplification of a metal fluorescent signal, thereby amplifying the fluorescent signal.

[0009] In one example of the present invention, the distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the gene probe, which allows for amplification of the metal fluorescence signal, is 5 to 95 nm, and the distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the gene probe is formed by a gene probe composed of 10 to 90 nucleotides, and preferably, the gene probe is selected from the group composed of 10 to 60 base pairs of double-stranded nucleotides.

[0010] In another example of the present invention, the substrate is any one selected from the group consisting of glass, paper, silica gel, silicon wafer, alumina, polystyrene, polyethylene, polypropylene, and polymer membrane.

[0011] The nanowire contains 0.01 M zinc acetate dihydrate and 0.03 M sodium hydroxide as a seed solution, and the nanowire contains 25 mM zinc nitrate hexahydrate and 25 mM hexamethylene tetramine as a precursor solution, and the nanowire is formed by hydrothermal synthesis for 1 to 2 hours.

[0012] The silver nanoparticles formed on the nanowire are formed by photochemical deposition, and preferably, the silver nanoparticles formed on the nanowire are formed by photochemical deposition containing a 0.1 to 0.5 mM silver nitrate solution, and preferably, the silver nanoparticles formed on the nanowire are formed by photochemical deposition for 15 to 60 minutes.

[0013] In another example of the present invention, the gene probe has biotin bound to one side and a fluorescently labeled other side, and the gene probe has a covalently bondable functional group introduced to one side or has biotin bound to one side and a fluorescently labeled other side.

[0014] In addition, the present invention provides a method for detecting a fluorescence signal using a silver nano-zinc oxide nanowire, comprising: a substrate; a nanowire grown on the substrate; and silver nanoparticles formed on the nanowire; a fluorescently labeled genetic probe; and a distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, which allows for amplification of a metal fluorescence signal, thereby amplifying the fluorescence signal.

[0015] In one example of the present invention, the fluorescence signal amplification occurs when biotin and biotin of a fluorescently labeled genetic probe bind to streptavidin.

[0016] Additionally, the present invention provides a method for producing silver nano-zinc oxide nanowires, characterized by comprising the steps of (a) preparing a nanowire seed solution; (b) preparing a nanowire precursor solution; (c) growing a nanowire on a substrate; (d) forming silver nanoparticles on the nanowire; (e) introducing streptavidin; and (f) immobilizing a genetic probe.

[0017] In addition, the present invention provides a silver nano zinc oxide nanowire manufactured by the steps of (a) preparing a nanowire seed solution; (b) preparing a nanowire precursor solution; (c) growing a nanowire on a substrate; (d) forming silver nanoparticles on the nanowire; (e) introducing streptavidin; and (f) fixing a genetic probe.

[0018] The present invention relates to a silver nanoparticle zinc oxide composite nanostructure that amplifies the fluorescence signal of a fluorescently labeled genetic probe, a method for manufacturing the same, and a method for detecting the fluorescence signal. The nanostructure includes a zinc oxide nanowire on which silver nanoparticles are formed, and not only allows for the introduction of more biomolecules to be introduced, but also allows for the omission of an amplification step in genetic diagnostic testing based on the fluorescence signal amplification effect, so that it can be usefully used in on-site diagnostic testing.

[0019] Figure 1 is a schematic diagram of metal-enhanced fluorescence induced by Ag-ZnO NCs, showing the interactions between fluorophores and Ag-ZnO NCs in various scenarios. (A) Interaction between a fluorophore and an AgNP immobilized with the fluorophore. (B) Interaction between a fluorophore and an adjacent AgNP within a ZnO NW strand. (C) Interaction between a fluorophore and an adjacent AgNP prepared from another ZnO NW strand.

[0020] Figure 2 illustrates the synthesis of ZnO NWs and Ag-ZnO NCs. (a) Schematic diagram of Ag-ZnO NC synthesis. (b) Top-view SEM images of ZnO NWs and Ag-ZnO NCs. Hydrothermal growth times of ZnO NWs ranged from 0 to 2 h. (c) Cross-sectional SEM images of ZnO NWs and Ag-ZnO NCs after 1 h or 2 h of NW growth. Left, ZnO NWs; right, Ag-ZnO NCs. The numbers in parentheses indicate the growth times of ZnO NWs.

[0021] Figure 3 shows the characteristics of Ag-ZnO NCs. (a) UV-Vis absorption spectra of ZnO NWs (solid line) and Ag-ZnO NCs (dashed line) at different hydrothermal growth times. The numbers in parentheses indicate the growth times of ZnO NWs. (b) XRD patterns of ZnO NWs (black) and Ag-ZnO NCs (red). (c) EDS mapping analysis of Ag-ZnO NCs. The plan-view SEM image (top) and elemental mapping image (bottom) show the distribution of Ag (pink). (d) XPS spectra of ZnO NWs (black) and Ag-ZnO NCs (red). (e) High-resolution XPS spectra of Ag 3d orbitals of ZnO NWs (black) and Ag-ZnO NCs (red).

[0022] Figure 4 shows high-resolution XPS spectra of the N1s orbitals of (a) ZnO NWs and (b) Ag-ZnO NCs before (black) and after (red) streptavidin coating.

[0023] Figure 5 shows the fluorescence signal enhancement of ssDNA hybridization probes on Ag-ZnO NCs. (a) Comparison of UV-visible absorption spectra of Ag-ZnO NCs (solid line) and excitation (blue region) / emission (green region) spectra of FAM-labeled DNA hybridization probes. The numbers in parentheses indicate the growth time of ZnO NWs. (b) Fluorescence emission spectra and (c) fluorescence decay curves of FAM-labeled ssDNA hybridization probes on glass (gray), ZnO NWs (blue), and Ag-ZnO NCs (red).

[0024] Figure 6 shows the fluorescence enhancement of a fluorescently labeled ssDNA hybridization probe under various Ag-ZnO NC synthesis conditions. (a) Effect of ZnO NW growth time on fluorescence intensity. Normalized fluorescence intensities at 528 nm are shown for the ssDNA hybridization probe of ZnO NWs (gray) and Ag-ZnO NCs (green). ZnO NWs were prepared at various growth times (0, 0.5, 1, and 2 h). (b) Effect of AgNO3 concentration and (c) reaction time during photochemical deposition on fluorescence intensity. Fluorescence intensities are shown at 528 nm for the ssDNA hybridization probe of Ag-ZnO NCs. Error bars represent the standard deviation of the fluorescence intensities obtained from three independent samples.

[0025] Figure 7 shows a 15% polyacrylamide gel image of double-stranded DNA generated by hybridization of FAM-labeled DNA hybridization probes with their complementary strands. M, 100 / 25 bp DNA ladder; 1, FAM-labeled DNA hybridization probe; 2, complementary strand; 3, dsDNA (FAM-labeled DNA probe / complementary strand).

[0026] Figure 8 shows the detection of dsDNA. (a) Effect of growth time of ZnO NWs on fluorescence enhancement. Normalized fluorescence intensities are shown at 528 nm for dsDNA of ZnO NWs (gray) and Ag-ZnO NCs (green). ZnO NWs were prepared at various growth times (0, 0.5, 1, and 2 h). Normalized fluorescence intensity at 528 nm = (F 528, 기질 ) / (F 528, 유리). (b) Effect of dsDNA length on fluorescence enhancement. Normalized fluorescence intensities at 528 nm are shown for dsDNA on ZnO NWs (gray) and Ag-ZnO NCs (green). The length of dsDNA varied from 10 to 60 bp. (c) Fluorescence decay curves of dsDNA (20 bp) immobilized on glass (gray), ZnO NWs (blue), and Ag-ZnO NCs (red). (d) Fluorescence images and (e) intensity plots of dsDNA (20 bp) in serial dilutions of glass, ZnO NWs, AgNIF, and Ag-ZnO NCs. Error bars represent the standard deviation of the fluorescence intensities obtained from three independent samples. (f) Linear relationship between fluorescence intensity and dsDNA concentration on Ag-ZnO NCs. The concentration of dsDNA ranged from 0 to 5 nM.

[0027] Figure 9 illustrates the synthesis of AgNIF. (a) UV-vis absorption spectrum of AgNIF. (b) Top-view (left) and cross-sectional (right) SEM images of AgNIF. The synthesized AgNIF is a single-layer 2D substrate.

[0028] Hereinafter, preferred embodiments of the present invention will be described in detail. Furthermore, the following description includes numerous specific details, such as specific components, but these are provided to facilitate a more comprehensive understanding of the present invention. It will be apparent to those skilled in the art that the present invention can be practiced without these specific details. Furthermore, in describing the present invention, detailed descriptions of known functions or configurations will be omitted if they are deemed to unnecessarily obscure the gist of the present invention.

[0029]

[0030] The present invention provides a silver nano-zinc oxide nanowire comprising: a substrate; a nanowire grown on the substrate; and silver nanoparticles formed on the nanowire; a fluorescently labeled genetic probe; and a distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, which allows amplification of a metal fluorescent signal, thereby amplifying the fluorescent signal.

[0031] FIG. 1 and FIG. 2 are schematic diagrams of a silver nano zinc oxide nanowire of the present invention, which may be configured to include a nanowire grown on a substrate, silver nanoparticles formed on the nanowire, streptavidin formed on the silver nanoparticles, and a fluorescently labeled genetic probe.

[0032] In one example of the present invention, the distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the gene probe, which allows for amplification of the metal fluorescence signal, is 5 to 95 nm, and the distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the gene probe is formed by a gene probe composed of 10 to 90 nucleotides, and preferably, the gene probe is selected from the group composed of 10 to 60 base pairs of double-stranded nucleotides.

[0033] In the present invention, the substrate is any one selected from the group consisting of glass, paper, silica gel, silicon wafer, alumina, polystyrene, polyethylene, polypropylene, and polymer membrane, but is not limited thereto.

[0034] In the present invention, zinc oxide has a very stable polar surface, making it easy to form various nanostructures. When nanowires are grown on this substrate, they provide a large surface area for probe immobilization, making them an effective substrate for DNA binding. However, when zero-dimensional nanoparticles are used instead of nanowires, the wide size distribution of the nanoparticles and their uneven distribution on the substrate can make it difficult to achieve accurate signal enhancement or reproducibility.

[0035] The seed solution for forming the zinc oxide seed layer may include zinc acetate dihydrate, and preferably includes, but is not limited to, 0.01 M zinc acetate dihydrate and 0.03 M sodium hydroxide.

[0036] The above nanowire can be synthesized by selecting a synthesis method known in the relevant field and an appropriate time accordingly, and is preferably formed by hydrothermal synthesis for 1 to 2 hours, but is not limited thereto.

[0037] Additionally, the genetic probe may use any means known in the art, but is preferably one in which biotin is bound to one side and a fluorescently labeled molecule is present, and preferably one in which a covalently bondable functional group is introduced to one side or biotin is bound to one side and a fluorescently labeled molecule is present to the other side. Examples of fluorescent markers include FAM, VIC, TAMRA, JOE, ROX, HEX, Cy3, Cy5, Texas Red, etc.

[0038] The zinc precursor solution may include zinc nitrate hexahydrate and hexamethylene tetramine. The hexamethylene tetramine allows the zinc precursor to grow in a specific plane direction (one-dimensional direction) on the substrate when converted to zinc oxide, thereby affecting the morphological characteristics of the nanowire. Specifically, it plays a role in promoting or inhibiting the growth of a specific crystal plane. That is, it plays a role in inhibiting lateral growth so that the zinc precursor is converted to an oxide and grows into a one-dimensional structure of the nanowire. At this time, the hexamethylene tetramine functions as a reducing agent. Preferably, the nanowire precursor solution includes, but is not limited to, 25 mM zinc nitrate hexahydrate and 25 mM hexamethylene tetramine.

[0039] The silver nanoparticles formed on the nanowire can be manufactured by various methods known in the art, and preferably, the silver nanoparticles formed on the nanowire are formed by photochemical deposition, and preferably, the silver nanoparticles formed on the nanowire are formed by photochemical deposition containing a 0.1 to 0.5 mM silver nitrate solution, and preferably, the silver nanoparticles formed on the nanowire are formed by photochemical deposition for 15 to 60 minutes, but are not limited thereto.

[0040] In addition, the present invention provides a method for detecting a fluorescence signal using a silver nano-zinc oxide nanowire, comprising: a substrate; a nanowire grown on the substrate; and silver nanoparticles formed on the nanowire; a fluorescently labeled genetic probe; and a distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, which allows for amplification of a metal fluorescence signal, thereby amplifying the fluorescence signal.

[0041] Depending on the characteristics of the silver nano-zinc oxide nanowire composite structure, particularly the silver nanoparticles, there is a fluorescence wavelength range in which a metal fluorescence signal can be amplified. The fluorescence signal of the present invention is a green wavelength range, and can be measured at an exit of 380 to 540 nm and an emission of 440 to 560 nm, preferably an exit of 485 nm and an emission of 528 nm, but is not limited thereto.

[0042] In one example of the present invention, the fluorescence signal amplification occurs when biotin and biotin of a fluorescently labeled genetic probe bind to streptavidin.

[0043] Additionally, the present invention provides a method for producing silver nano-zinc oxide nanowires, characterized by comprising the steps of (a) preparing a nanowire seed solution; (b) preparing a nanowire precursor solution; (c) growing a nanowire on a substrate; (d) forming silver nanoparticles on the nanowire; (e) introducing streptavidin; and (f) immobilizing a genetic probe.

[0044] In addition, the present invention provides a silver nano zinc oxide nanowire manufactured by the steps of (a) preparing a nanowire seed solution; (b) preparing a nanowire precursor solution; (c) growing a nanowire on a substrate; (d) forming silver nanoparticles on the nanowire; (e) introducing streptavidin; and (f) fixing a genetic probe.

[0045] It is preferable that the diameter of the above nanowire is 20 to 100 nm.

[0046] In the above step (c), the nanowire can be grown using a hydrothermal synthesis method, and the step (c) includes: i) a step of forming a seed layer by applying the zinc seed solution to a substrate; and ii) a step of immersing the substrate in the zinc precursor solution with the seed layer facing downward and reacting at 95°C. At this time, the length of the nanowire can be controlled by controlling the reaction time between the zinc oxide seed layer and the zinc precursor solution, and the nanowire grows in length at about 500 nm / hr.

[0047] The silver nanoparticles of the above step (d) can be formed to have a size of 50 to 300 nm, and the size of the silver nanoparticles can be controlled by controlling the concentration and deposition time of the silver solution (0.4 mM AgNO3 in 25% ethyl alcohol).

[0048] The step (e) above can use a protein labeled with histidine amino acids on a zinc oxide nanowire without surface treatment by utilizing the binding force between zinc oxide and histidine, specifically streptavidin labeled with histidine at the N-terminus or C-terminus.

[0049] The above step (f) is for amplifying the fluorescence signal generated when the biotin of the biotin- and fluorescently labeled gene probe binds to the streptavidin.

[0050]

[0051] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims.

[0052]

[0053] <Example 1> Materials

[0054] Zinc acetate dihydrate (≥98%), sodium hydroxide (≥98%), zinc nitrate hexahydrate (98%), hexamethylenetetramine (≥99%), silver nitrate (≥99.0%), butylamine (≥99.5%), and methanol (≥98%) were purchased from Sigma-Aldrich (St. Louis, MO, USA). Ethyl alcohol (anhydrous, 99.9%) was obtained from Samchun Chemical (Pyeongtaek, South Korea). Streptavidin was purchased from Abcam (Cambridge, UK). DNA hybridization probes were synthesized by SFC Probe (Cheongju, South Korea), and the sequences are listed in Table 1. Phosphate-buffered saline (PBS; 10X) and 10X tris-buffered saline containing 0.5% Tween 20 were purchased from Bio-Rad (Hercules, CA, USA) and Biosolution Co., Ltd. (Seoul, Korea), respectively. All chemicals used in this study were of analytical grade without further purification. Deionized (DI) water obtained from a Cascada III. I water purification system (PALL Co., NY, USA) was used throughout all experiments.

[0055]

[0056] SEQ ID NODNA Probe Length (nt) Sequence (5' -> 3') 1105' FAM - ACA TGG CTT T - biotin 3'2205' FAM - ACA TGG CTT TGA GTT GAC AT - biotin 3'3405' FAM - ACA TGG CTT TGA GTT GAC ATC TAT GAA GTA ACA TGG CTT T - biotin 3'4605' FAM - ACA TGG CTT TGA GTT GAC ATC TAT GAA GTA ACA TGG CTT TGA GTT GAC ATC TAT GAA GTA - biotin 3'5Complement 10AAA GCC ATG T6Complement 20ATG TCA ACT CAA AGC CAT GT7Complement 40AAA GCC ATG TTA CTT CAT AGA TGT CAA CTC AAA GCC ATG T8Complement 60TAC TTC ATA GAT GTC AAC TCA AAG CCA TGT TAC TTC ATA GAT GTC AAC TCA AAG CCA TGT

[0057]

[0058] <Example 2> Hydrothermal growth of ZnO nanowires (nonowires, NW)

[0059] 1. Preparation of seed solution

[0060] ZnO seed solution was synthesized using wet chemistry. Specifically, 0.01 M zinc acetate dihydrate and 0.03 M sodium hydroxide solutions were dissolved in methanol at 60°C with stirring. Then, 65 mL of sodium hydroxide solution was slowly added dropwise to 125 mL of zinc acetate dihydrate while continuously stirring. The mixed solution was stirred at 60°C until the solution volume was reduced to half of its initial volume and incubated at room temperature for 1 h. The obtained ZnO seed solution was stored at 4°C until use.

[0061]

[0062] 2. ZnO NW fabrication

[0063] The seed solution was drop-cast onto a glass slide, washed with ethanol and deionized water, and then dried with N2 gas. After repeating drop-casting of the seed solution three times, the seed-coated glass slide was heated at 150°C for 15 min. The precursor solution for ZnO NW synthesis was prepared by mixing zinc nitrate hexahydrate and hexamethylenetetramine (both 25 mM) and stirring at room temperature for 10 min. For hydrothermal growth, the precursor solution was incubated at 95°C for 0.5–2 h in a convection oven. The grown ZnO nanowire substrate was thoroughly washed with DI water and dried with N2 gas.

[0064]

[0065] <Example 3> Photochemical deposition of silver nanoparticles on ZnO NWs

[0066] Ag-ZnO nanocomposite (NC) was synthesized using a simple photochemical deposition method. Silver nitrate was dissolved in 25% ethyl alcohol at a final concentration of 0.4 mM. The prepared ZnO NWs were immersed in the silver nitrate solution and exposed to UV-A lamp (365 nm) at 4.77 mW / cm 2 Ag on the surface of ZnO NW was irradiated for 15 minutes at an intensity of + After irradiation, the Ag-ZnO NCs were rinsed with deionized water and dried under N2 gas. The Ag-ZnO NCs were immersed again in the silver nitrate solution, and the above procedure was repeated 0 to 3 times (final irradiation time ranged from 15 to 60 min).

[0067]

[0068] <Example 4> Characteristics of ZnO NWs and Ag-ZnO NCs

[0069] UV-visible absorption spectra of ZnO NWs and Ag-ZnO NCs were obtained using a UV-1800 UV-vis spectrophotometer (Shimadzu, Kyoto, Japan). The morphology of the nanostructures was characterized by field-emission scanning electron microscopy (FE-SEM) (S-4800 instrument, Hitachi, Tokyo, Japan) using an accelerating voltage at 10 kV and 20 k magnification. The side-view SEM images were obtained using a SU8230 ultra-high-resolution (UHR) FE-SEM instrument (Hitachi) under a 5 kV electron beam at 50 k magnification. The elemental distribution mapping images were obtained using a SU8230 UHR FE-SEM instrument at an accelerating voltage of 10 kV. X-ray photoelectron spectroscopy (XPS) analysis was performed using a K-Alpha + XPS was performed using a system (Thermo Scientific, Waltham, MA, USA). X-ray diffraction (XRD) analysis was performed at 45 kV and 200 mA using a SmartLab 9 kW (Rigaku Co., Tokyo, Japan) to investigate the crystal phases of ZnO NWs and Ag-ZnO NCs. The Cu Kα radiation (λ = 1.54056 Å) at 2θ ranged from 20° to 80°.

[0070]

[0071] <Example 5> Detection of fluorophore-labeled DNA probe

[0072] 1. Detection of single-stranded DNA (ssDNA)

[0073] To immobilize ssDNA hybridization probes on ZnO and Ag surfaces, the substrates were incubated with a diluted streptavidin solution (2000:1, 1X PBS) at room temperature for 1 h. After washing three times with 1X Tris-buffered saline with 0.05% Tween 20 (TBS-T), the streptavidin-coated substrates were dried under N2 gas and stored at 4°C until use. An aliquot (20 μL) of the ssDNA hybridization probe diluted in 1X PBS was dispersed on the streptavidin-coated surfaces. After incubation for 1 h at room temperature, the substrates were rinsed three times with 1X TBS-T to remove residual DNA hybridization probes. Fluorescence intensity was excited at 485 nm and measured at 528 nm using a Synergy H1 hybrid multimode reader (Agilent, Santa Clara, CA, USA). The fluorescence intensity of the DNA hybridization probe is expressed as a value excluding the background signal of the substrate (F 528 , DNA-F 528 , Blank).

[0074]

[0075] 2. Detection of double-stranded DNA (dsDNA)

[0076] To generate dsDNA of various lengths, DNA hybridization probes were incubated with their corresponding complementary strands at 95°C for 5 min and 37°C for 30 min. Fluorescence images of the dsDNA-immobilized substrate were acquired using an Azure Sapphire biomolecule imager (Azure Biosystems, Dublin, CA, USA), and fluorescence intensities were analyzed using ImageJ software.

[0077]

[0078] <Example 6> Fluorescence lifetime analysis of ssDNA and dsDNA on a substrate

[0079] Time-resolved fluorescence decay of ssDNA and dsDNA prepared on various substrates was measured using a 467 nm pulsed laser diode as an excitation source in a Fluorolog 3 spectrofluorometer (Horiba Scientific, Kyoto, Japan). em = 10,000 fluorescence decay peaks at 520 nm were accumulated to determine the fluorescence lifetime. The fluorescence lifetime was analyzed from the time-resolved fluorescence decay curves by fitting them to triple and quadruple exponential decay models in the presence of ssDNA and dsDNA, respectively.

[0080]

[0081] <Example 7> Synthesis of Ag nanoisland film

[0082] Silver nitrate and butylamine solutions were prepared by dissolving them in anhydrous ethyl alcohol to a final concentration of 2 mM. Glass slides were immersed in a 1:1 mixture of silver nitrate and butylamine solutions and incubated at 55°C. After 40 min, the prepared Ag nanoisland films were washed with deionized water and dried under N2 gas.

[0083]

[0084] <Example 8> Polyacrylamide gel electrophoresis

[0085] Hybridized dsDNA products were verified by 15% polyacrylamide gel electrophoresis performed in 1X TBE buffer. After running at 120 V for 45 min, the polyacrylamide gel was stained with GelRed (Biotium, Hayward, CA, USA) and visualized using an Azure 280 imaging system (Azure Biosystems, Dublin, CA, USA).

[0086]

[0087] <Experimental Example 1> Ag-ZnO NC design

[0088] The 3D MEF substrate was designed and constructed in the present invention through hydrothermal synthesis of ZnO NWs and photochemical deposition of AgNPs to improve the interaction between the fluorophore and the 3D metal nanostructure. The various properties of ZnO NW arrays have been extensively studied in the field of biosensors, providing a suitable 3D template for fabricating AgNPs. The interaction between the fluorophore and the metal surface can occur in various scenarios (Fig. 1). At an optimal distance, the fluorophore can interact with the immobilized AgNPs (Fig. 1a). At a suboptimal distance, too close or too far from the metal surface, the fluorescence signal may be quenched or not enhanced. The MEF effect of 2D MEF substrates, such as AgNPs deposited on glass, primarily arises from this phenomenon. However, in Ag-ZnO NCs, where AgNPs are positioned in a 3D environment, the fluorophore can be positioned at an appropriate distance from adjacent AgNPs within the ZnO NW strand (Fig. 1b). AgNPs fabricated on other NW strands can also interact with the fluorophore (Fig. 1c). Therefore, Ag-ZnO NCs can contribute to enhancing sensitivity through interaction at the optimal distance for DNA detection.

[0089]

[0090] <Experimental Example 2> Fabrication and Characterization of Ag-ZnO NC Structure

[0091] Ag-ZnO NCs were prepared through hydrothermal growth of ZnO NWs and site-specific photochemical deposition of AgNPs. A schematic diagram of the AgNP deposition on ZnO NWs consists of three steps (Fig. 2a). First, a ZnO seed layer was formed on glass by drop casting. Next, ZnO NWs were grown from the ZnO seed layer at 95°C. The length of the ZnO NWs was controlled by adjusting the growth time (0–2 h). In the final step, AgNPs were deposited on the NW surface through photochemical reduction, as ZnO generates electron-hole pairs under UV light exposure.

[0092] The morphologies of ZnO NWs and Ag-ZnO NCs dependent on the ZnO NW growth time were analyzed by FE-SEM (Figs. 2b and c). The numbers in parentheses of ZnO NWs and Ag-ZnO NCs indicate the ZnO NW growth time. The ZnO NWs became longer with increasing growth time, and completely covered the seed layer after growing for 1 h (ZnO NW(1)) (Fig. 2b). As shown in the cross-sectional SEM images, the lengths of the ZnO NWs synthesized for 1 h and 2 h were 149 and 723 nm, respectively (Fig. 2c). After immersing the ZnO NWs in an aqueous AgNO3 solution and irradiating with UV, AgNPs with a diameter of 50–200 nm were decorated on the surface of the ZnO NWs. AgNPs were fabricated on the entire NW surface when the growth duration of ZnO NWs was 1 h (Ag-ZnO NC (1)), whereas they were mostly deposited at the ends of the NWs when ZnO NWs were synthesized for 2 h (Ag-ZnO NC (2)). When the height of the NWs was ≥723 nm, the incident light and Ag + Tip-grafted AgNPs can be formed on ZnO NWs because ions cannot approach the bottom.

[0093] To investigate the characteristics of Ag-ZnO NCs, UV-visible absorption spectra, XPS spectra, and EDS mapping analyses were performed. The UV-visible absorption spectra of Ag-ZnO NCs and ZnO NWs were analyzed (Fig. 3a). Strong absorption of ZnO NWs was observed only at wavelengths below 400 nm. The peak intensity of ZnO NWs enhanced with growth time (0, 0.5, 1, and 2 h). In contrast, Ag-ZnO NCs exhibited a broad absorption spectrum in the visible wavelength range. This result was confirmed by the SEM image in Fig. 2b, which shows that the AgNPs of Ag-ZnO NCs had a size distribution ranging from 50 to 200 nm.

[0094] XRD, EDS mapping, and XPS analyses were performed to analyze the AgNPs synthesized on the surface of ZnO NWs. The XRD patterns of both ZnO NWs and Ag-ZnO NCs exhibited diffraction peaks characteristic of the hexagonal wurtzite structure of ZnO (2θ = 31.77°, 34.41°, 36.26°, 47.55°, 56.62°, 62.87°, and 68.01°, which represent the (100), (002), (101), (102), (110), (103), and (112) crystal planes, respectively) (Fig. 3b). The characteristic diffraction peaks of metallic Ag (111), (200), (220), and (311) crystal planes appear only in Ag-ZnO NCs at 2θ = 38.11°, 44.30°, 64.44°, and 77.40°. The characteristic diffraction peaks of impurities such as Ag2O were not observed in ZnO NWs or Ag-ZnO NCs. The distribution of Ag element in Ag-ZnO NCs was further clarified by performing EDS mapping image analysis (Fig. 3c). The chemical states of ZnO NWs and Ag-ZnO NCs were investigated by examining the XPS spectra (Fig. 3d and e). Peaks representing Zn, O, and C were obtained from the full XPS spectra of both substrates. Two distinct Ag 3d peaks located at 367.7 and 373.7 eV in the Ag-ZnO NC substrate 5 / 2 and Ag 3d 3 / 2 Peaks were measured. The binding energies of these two peaks are much lower than those of pure AgNPs (374.2 and 368.2 eV), suggesting a strong interaction between AgNPs and ZnO NWs. It is well known that the Fermi energy level of ZnO is lower than that of Ag. Therefore, electrons from Ag can be transferred to ZnO. Ag + The binding energy of Ag 0 Ag 3d is much lower than 5 / 2 and Ag 3d 3 / 2The corresponding peak shifts to a lower binding energy level. This result confirmed the fabrication of AgNPs from ZnO NWs according to the process shown in Fig. 2a.

[0095]

[0096] <Experimental Example 3> Enhanced fluorescence of DNA probe labeled with a fluorophore in Ag-ZnO NCs

[0097] After demonstrating the characteristics of Ag-ZnO NCs, the fluorescence enhancement effect of Ag-ZnO NCs was investigated using a fluorophore-labeled ssDNA hybridization probe as a reporter. To immobilize the ssDNA hybridization probe on the substrate, the unlabeled end of the ssDNA was modified with a biotin moiety. Glass, ZnO NWs, and Ag-ZnO NCs were coated with streptavidin, so that the ssDNA hybridization probe could be immobilized on the substrate through streptavidin-biotin interactions. The presence of streptavidin on ZnO NWs and Ag-ZnO NCs after the coating step was confirmed by analyzing high-resolution XPS spectral data for the N1s orbital (Fig. 4).

[0098] Next, before measuring the fluorescence intensity for the above substrate, the UV-visible absorption spectra of Ag-ZnO NCs were compared with the excitation / emission spectra of the fluorescein (FAM) fluorophore. Ag-ZnO NCs have a broad absorption spectrum ranging from 350 to 700 nm, and the intensity increases with growth time (Fig. 5a). No absorption spectra corresponding to AgNPs were observed in Ag-ZnO NCs (0) and Ag-ZnO NCs (0.5). This weak intensity of Ag-ZnO NCs in short ZnO NWs may be due to insufficient formation of AgNPs on the surface of ZnO NWs. An enhanced intensity of the UV spectrum was observed after AgNPs were formed in ZnO NWs grown for 1 and 2 h (Ag-ZnO NCs (1) and Ag-ZnO NCs (2)). The absorption spectra of Ag-ZnO NCs overlapped with the excitation / emission peaks of FAM. These results imply a strong plasmonic coupling effect between Ag-ZnO NCs and FAM, which is one of the mechanisms of the MEF phenomenon when ZnO NWs were synthesized for 1 and 2 h (Fig. 5a). The fluorescence intensities of glass, ZnO NWs, and Ag-ZnO NCs were measured using a FAM-labeled ssDNA hybridization probe (Fig. 5b). The fluorescence intensity of ZnO NWs was not different from that of glass. However, the fluorescence intensity of Ag-ZnO NCs was dramatically enhanced. Fluorescence lifetime analysis of the ssDNA hybridization probe on glass, ZnO NWs, and Ag-ZnO NCs was also performed to demonstrate the fluorescence enhancement in Ag-ZnO NCs through the MEF phenomenon (Fig. 5c and Table 2). When a fluorophore interacts with a metal nanostructure, the fluorescence lifetime of the fluorophore decreases because the metal nanostructure modifies the radiative decay rate of the fluorophore. The average lifetimes of glass, ZnO NWs, and Ag-ZnO NCs were 13.03, 12.65, and 10.79 ns, respectively.

[0099]

[0100] GlassZnO NWAg-ZnO NCτ1 (ns)18.03 ± 0.3817.27 ± 0.3516.35 ± 0.39%52.1852.154.37τ2 (ns)128.68 ± 2.10124.30 ± 1.902.40 ± 0.08%32.332.6213.61τ3 (ns)3.43 ± 0.073.31 ± 0.07122.95 ± 2.45%15.5215.2932.02Average τ a (ns)13.0312.6510.79χ 2 1.191.121.22

[0101] a The fluorescence lifetime of the ssDNA hybridization probe was analyzed from the time-resolved fluorescence decay curve (Fig. 5c) by fitting it to a triple exponential decay model.

[0102] Because the MEF effect is influenced by the properties of metal nanostructures, the synthesis conditions of nanomaterials must be optimized. First, the effect of the hydrothermal growth period of NWs on the fluorescence enhancement was investigated. Since ZnO NWs can serve as building blocks for AgNPs, the length of ZnO NWs can affect the fabrication of AgNPs and the subsequent fluorescence enhancement. To investigate the effect of ZnO NW length on fluorescence enhancement, the fluorescence intensities of ZnO NWs and Ag-ZnO NCs were divided by the fluorescence intensity of glass (normalized fluorescence intensity, Fig. 6a). In the case of ZnO NWs, the fluorescence intensities of ZnO NW(0), ZnO NW(0.5), ZnO NW(1), and ZnO NW(2) increased 6-, 18-, 2-, and 21-fold, respectively. For Ag-ZnO NCs, the fluorescence enhancement was 6-, 15-, 95-, and 70-fold for Ag-ZnO NC(0), Ag-ZnO NC(0.5), Ag-ZnO NC(1), and Ag-ZnO NC(2), respectively. The highest fluorescence enhancement was observed for Ag-ZnO NC(1). The normalized fluorescence intensities of ZnO NWs and Ag-ZnO NCs were very similar at ZnO NW growth times of 0 and 0.5 h. However, after 1 and 2 h of ZnO NW growth, the fluorescence enhancement of Ag-ZnO NCs was much higher than that of ZnO NWs. The weak fluorescence enhancement of Ag-ZnO NCs(0.5) may be due to the insufficient formation of AgNPs on the ZnO NW surface.

[0103] The concentration of the AgNO3 solution and the reaction time of the photochemical deposition step can affect the MEF effect of Ag-ZnO NCs. The fluorescence intensity of Ag-ZnO NCs deposited at various concentrations of AgNO3 was compared (Fig. 6b). The fluorescence intensity increased as the AgNO3 concentration increased from 0.1 to 0.4 mM, but decreased when the concentration exceeded 0.5 mM. The highest fluorescence intensity was observed at 0.4 mM AgNO3. To investigate the effect of deposition time on AgNPs (0, 15, 30, 45, and 60 min), the fluorescence intensity of Ag-ZnO NCs was analyzed. As shown in Fig. 6c, the fluorescence intensity increased with increasing AgNP deposition time and saturated after 30 min. Therefore, photochemical deposition with a 0.4 mM AgNO3 solution for 30 min was optimal for enhancing fluorescence to form AgNPs on the ZnO NW surface.

[0104]

[0105] <Experimental Example 4> Detection of dsDNA through MEF effect on Ag-ZnO NCs

[0106] Previous studies on MEF have emphasized the importance of an optimal distance (5-90 nm) between fluorophores and metal nanostructures. However, MEF substrates have limited applications in biosensors because they struggle to maintain fluorophores at an optimal distance from metal nanostructures in aqueous environments. Double-stranded DNA molecules are a key target for biosensors and can be readily prepared in various lengths through primer design. Therefore, in this study, we investigated the fluorescence enhancement of Ag-ZnO NC substrates using dsDNA of various lengths.

[0107] Although the number of bases in a DNA strand is the same, the persistence lengths of ssDNA and dsDNA are significantly different. The normalized fluorescence intensities of ZnO NWs and Ag-ZnO NCs were analyzed at various ZnO NW growth times. dsDNA molecules were prepared by hybridizing an ssDNA hybridization probe with its complementary strand. The formation of dsDNA was confirmed by polyacrylamide gel electrophoresis images (Fig. 7). Before measuring the fluorescence signal, the Ag-ZnO NC substrate was incubated with FAM-labeled dsDNA in PBS and then washed with TBS-T buffer. The fluorescence intensity of dsDNA in ZnO NWs was not dramatically enhanced at any growth time (1.1-1.6 times, Fig. 8a). In the presence of Ag-ZnO NCs, the fluorescence enhancement of dsDNA in Ag-ZnO NCs was 3.1-fold, 7.0-fold, 16.9-fold, and 15.3-fold at growth times of 0, 0.5, 1, and 2 h, respectively. The highest fluorescence enhancement in Ag-ZnO NCs was observed at a ZnO NW growth time of 1 h. These results, together with those in Fig. 6a, indicate that the formation of AgNPs in ZnO NWs grown for 1 h may be optimal for fluorescence enhancement of both ssDNA and dsDNA.

[0108] The effect of the distance between the fluorophore and Ag-ZnO NCs on fluorescence enhancement was investigated by adjusting the number of bp of dsDNA. The number of bp of dsDNA ranged from 10 to 60, and the calculated distance ranged from ~8.4 to 25.4 nm (Table 3). The normalized fluorescence intensities of dsDNA with different numbers of bp in ZnO NWs and Ag-ZnO NCs are shown in Figure 8b. Ag-ZnO NCs enhanced the fluorescence intensities for dsDNA of all lengths, but a decrease or similar intensity was observed in ZnO NWs compared to glass. The fluorescence enhancement of Ag-ZnO NCs was 14.8-fold, 16.9-fold, 11.4-fold, and 14.2-fold in the presence of 10, 20, 40, and 60 bp dsDNA, respectively. As shown in Figure 8b, there was no correlation between the length of dsDNA and the fluorescence enhancement of Ag-ZnO NCs. These results demonstrate that dsDNA of various lengths can be positioned at an optimal distance from the Ag-ZnO NC for MEF development. We propose that the fluorescence enhancement may be related to improved interaction between the fluorophore and the Ag-ZnO NC substrate.

[0109]

[0110] Distance (nm)Streptavidin-biotin complex4.2

[0111] The fluorescence lifetimes of dsDNA, ZnO NWs, AgNIF, and Ag-ZnO NCs on glass were also analyzed, confirming that this fluorescence enhancement of dsDNA was a result of the MEF effect (Fig. 8c and Table 4). As shown in Table 4, the average lifetimes of fluorophore-labeled dsDNA on glass, ZnO NWs, and Ag-ZnO NCs were 9.76, 9.34, and 7.86 ns, respectively. By comparing the fluorescence intensities of serially diluted dsDNA on glass, ZnO NWs, AgNIF, and Ag-ZnO NCs, we demonstrated that Ag-ZnO NCs could enhance the target detection sensitivity for 2D MEF substrates. To compare the fluorescence enhancement of Ag-ZnO NCs with that of 2D MEF substrates, AgNIF was synthesized on glass and characterized by UV-visible absorption spectra and SEM images (Fig. 9). The typical absorption spectrum of AgNPs is shown in Fig. 9a. The cross-sectional SEM image confirmed that AgNIF was a single layer (Fig. 9b). Fluorescence images of dsDNA were obtained and the fluorescence intensities of dsDNA serially diluted on the above substrates were compared (Fig. 8d and e). Compared with glass, no fluorescence enhancement was observed in ZnO NWs and AgNIF, but only in Ag-ZnO NCs (Fig. 8d and e). The fluorescence intensity of Ag-ZnO NCs gradually enhanced with increasing dsDNA concentration and was saturated above 25 nM. Based on the fluorescence intensity plot in Fig. 8e, R for dsDNA concentrations between 0 and 5 nM 2 A linear regression curve with a value of 0.94 was established (fluorescence intensity = 7.11*concentration DNA + 4.67, Fig. 8f). The limit of detection (LOD) was F blank + 3*SD blankis the concentration exceeding the fluorescence intensity value. The LOD was not obtained for ZnO NWs, but the LOD was estimated to be 25 nM and 0.5 nM for AgNIF and Ag-ZnO NCs, respectively. Ag-ZnO NCs showed 50-fold higher sensitivity for dsDNA detection than AgNIF, a 2D MEF substrate. These results indicate that the fluorophore can be at an optimal distance from the metal nanostructure in various scenarios, as presented in Figure 1.

[0112]

[0113] GlassZnO NWAg-ZnO NCτ1 (ns)10.32 ± 0.4310.20 ± 0.499.79 ± 0.40%43.4642.3343.21τ2 (ns)45.19 ± 1.2939.89 ± 1.3042.33 ± 1.36%29.7729.5429.49τ3 (ns)1.25 ± 0.051.29 ± 0.050.94 ± 0.03%6.657.377.07Average τ a (ns)9.769.347.86χ 2 1.171.181.22

[0114] a The fluorescence lifetime of the dsDNA hybridization probe was analyzed from the time-resolved fluorescence decay curve (Fig. 8c) by fitting it to a quadruple exponential decay model.

[0115]

[0116] <Experimental Example 5> Conclusion

[0117] 3D MEF substrates have several advantages, including large fluorescence enhancement, sensitive detection, and an enhanced dynamic range for biomarker detection. Novel 3D MEF substrates as biosensors can enhance the interaction of biomolecules and metal structures in aqueous environments. In this study, Ag-ZnO NCs were developed and characterized as 3D MEF substrates using hydrothermal synthesis of ZnO NWs, photochemical deposition of AgNPs, SEM imaging, UV-visible absorption spectra, XPS spectra, and EDS mapping. The fluorescence enhancements of the novel Ag-ZnO NC 3D MEF substrates were 14.8-fold, 16.9-fold, 11.4-fold, and 14.2-fold in the presence of 10, 20, 40, and 60 bp dsDNA, respectively. We propose that these enhancements may be related to the improved interaction between the fluorophore and the Ag-ZnO NC substrate. The MEF effects on glass, ZnO NWs, and Ag-ZnO NCs were analyzed based on the fluorescence lifetimes of FAM-labeled dsDNA, and the average lifetimes for each substrate were 9.76, 9.34, and 7.86 ns, respectively. Ag-ZnO NCs showed 50-fold higher sensitivity for dsDNA detection than AgNIF, a 2D MEF substrate.

[0118] In summary, the results of the present invention indicate that Ag-ZnO NCs have potential as 3D MEF substrates. The MEF phenomenon can occur through a wide range of interactions between the metallic nanostructured surface of Ag-ZnO NCs and fluorophores in various scenarios: interactions between fluorophores and AgNPs immobilized with fluorophores, interactions between fluorophores and adjacent AgNPs within ZnO NW strands, and interactions between fluorophores and adjacent AgNPs fabricated on different ZnO NW strands. The Ag-ZnO NCs of the present invention provide a foundation for the development of MEF-based biosensors for DNA detection in aqueous environments.

Claims

1. A substrate; a nanowire grown on the substrate; and silver nanoparticles formed on the nanowire; a fluorescently labeled genetic probe; and a silver nano zinc oxide nanowire in which a distance capable of amplifying a metal fluorescent signal is maintained between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, thereby amplifying the fluorescent signal.

2. In the first paragraph, a silver nano zinc oxide nanowire characterized in that the distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, which enables amplification of the metal fluorescence signal, is 5 to 95 nm.

3. In the first paragraph, the distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe is characterized in that it is formed by the genetic probe consisting of 10 to 90 nucleotides.

4. In the third paragraph, the gene probe is a silver nano zinc oxide nanowire characterized in that it is selected from the group consisting of 10 to 60 base pairs of double-stranded nucleotides.

5. In the first paragraph, the substrate is characterized in that it is one selected from the group consisting of glass, paper, silica gel, silicon wafer, alumina, polystyrene, polyethylene, polypropylene, and polymer membrane.

6. In the first paragraph, the nanowire is characterized in that it contains 0.01 M zinc acetate dihydrate and 0.03 M sodium hydroxide as a seed solution.

7. In the first paragraph, the nanowire is characterized in that it contains 25 mM zinc nitrate hexahydrate and 25 mM hexamethylene tetramine as a precursor solution.

8. In the first paragraph, the nanowire is a silver nano zinc oxide nanowire characterized in that it is formed by hydrothermal synthesis for 1 to 2 hours.

9. In the first paragraph, the silver nanoparticles formed on the nanowire are characterized in that they are formed by photochemical deposition.

10. In the first paragraph, the silver nanoparticles formed on the nanowire are characterized in that they are formed by photochemical deposition containing a 0.1 to 0.5 mM silver nitrate solution.

11. In the first paragraph, the silver nanoparticles formed on the nanowire are characterized in that they are formed by photochemical deposition for 15 to 60 minutes.

12. In the first paragraph, the genetic probe is a silver nano zinc oxide nanowire characterized in that biotin is bound to one side and fluorescently labeled to the other side.

13. In the first paragraph, the genetic probe is a silver nano zinc oxide nanowire characterized in that a functional group capable of covalent bonding is introduced on one side or biotin is bound and a fluorescent label is applied on the other side.

14. A method for detecting a fluorescence signal using a silver nano-zinc oxide nanowire, comprising: a substrate; a nanowire grown on the substrate; and silver nanoparticles formed on the nanowire; a fluorescently labeled genetic probe; and a distance between the silver nanoparticles formed on the nanowire and the fluorescent molecules of the genetic probe, which allows for amplification of a metal fluorescence signal, thereby amplifying the fluorescence signal.

15. In the 14th paragraph, the fluorescence signal amplification is characterized in that the silver nano zinc oxide nanowire occurs when biotin and the biotin of the fluorescently labeled genetic probe bind to streptavidin. 16.(a) Step of preparing a nanowire seed solution; (b) a step of preparing a nanowire precursor solution; (c) a step of growing a nanowire on a substrate; (d) a step of forming silver nanoparticles on the nanowire; (e) a step of introducing streptavidin; and (f) A method for manufacturing a silver nano zinc oxide nanowire, characterized by comprising a step of fixing a genetic probe; 17.(a) Step of preparing a nanowire seed solution; (b) a step of preparing a nanowire precursor solution; (c) a step of growing a nanowire on a substrate; (d) a step of forming silver nanoparticles on the nanowire; (e) a step of introducing streptavidin; and (f) a step of fixing a genetic probe; a silver nano zinc oxide nanowire manufactured by

Citation Information

Patent Citations

  • Fabrication method for fluorescence signal amplification substrate and DNA and protein micro array chip using method

    KR1020140000817A

  • Core-shell nanocomplex for metal-enhanced fluorescence

    KR1020150133873A

  • RNA microchip detection using nanoparticle-assisted signal amplification

    KR1020150139582A

  • Biomolecule detecting sensor, method for manufacturing the same and biomolecule detecting method

    KR1020170105718A

  • System for auto generating 3D modeling of permanent drain method and method thereof and record medium recorded with program thereof

    KR102613082B1