- 2026-11-12
AI Technical Summary
Existing coating compositions provide insufficient scuff resistance against common scuff media like coins and shoe heels, limiting their application versatility and durability.
A coating composition comprising polymer particles, polymeric organic crosslinked spheres, silica particles, and polysiloxane particles, which synergistically enhance scuff resistance and maintain low gloss, with specific particle size and concentration ranges.
The composition achieves excellent scuff resistance against both coins and shoe heels with ≤ 0.8 and ≤ 0.5 color change, respectively, while maintaining a gloss value ≤ 10, as determined by standard test methods.
Smart Images

Figure PCTCN2025092827-FTAPPB-I100001 
Figure PCTCN2025092827-FTAPPB-I100002 
Figure PCTCN2025092827-FTAPPB-I100003
Abstract
Description
COATING COMPOSITIONFIELD
[0001] The present invention relates to a coating composition that provides coatings obtained therefrom with excellent scuff resistance properties and low gloss.
[0002] INTRODUCTION
[0003] There is a growing market demand for interior broad wall paints with enhanced scuff resistance, particularly in the architectural paint segment. This is particularly important for scuff media commonly encountered by customers, such as coins and shoe heels.
[0004] Silicone additives such as polyorganosiloxane particles are known to improve burnish resistance or mar resistance of waterborne paints. For example, US11981830B2 relates to a paint composition affording coatings with excellent burnish resistance, however, the obtained coating surfaces tend to be easily damaged by various scuffmedia in daily usage. Burnish resistance and mar resistance focus on coatings’ gloss changes after rubbing with cheesecloth, while scuff resistance refers to a coating’s ability to resist color changes after rubbing with scuff media like shoe heels and metal coins. Scuff resistance is crucial for coatings as it ensures their durability and is more relevant to end-user application scenarios. Different materials typically have different scuff mechanisms, and incumbent coating compositions in the market can only work for a specific scuff material. This limitation restricts their applications since users typically need coatings to provide scuff resistance for common scuff media such as coins and shoe heels simultaneously. Therefore, there is a need to develop a versatile solution that can provide scuff resistance against different scuff materials, especially coins and shoe heels.SUMMARY
[0005] The present invention solves the problem of discovering a coating composition comprising a novel combination of polymer particles, specified silica particles, polymeric organic crosslinked spheres, and polysiloxane particles. The coating composition has shown synergistic effects in achieving excellent scuff resistance against both coins and shoe heels, as demonstrated by a heel scuff color change ≤ 0.8 and a coin scuff color change ≤ 0.5, while maintaining a low gloss with a 60° gloss value ≤ 10. These properties can be determined according to the test methods described in the Examples section below.
[0006] In a first aspect, the present invention is a coating composition comprising, by dry weight based on the weight of coating composition, an aqueous dispersion of:
[0007] (A) from 9.6%to 24%of polymer particles having a Z-average particle size in a range of from 80 nanometers (nm) to 500 nm;
[0008] (B) from 1%to 6.5%of polymeric organic crosslinked microspheres having a median weight average particle size in a range of from 1 micrometer (μm) to 40 μm;
[0009] (C) from 2%to less than 10%of silica particles having a D50 particle size in a range of from 5 μm to 30 μm and having a BET surface area less than 50 m2 / g; and
[0010] (D) from 0.24%to 4.4%ofpolysiloxane particles having a D50 particle size in a range of from 1 μm to 20 μm.
[0011] In a second aspect, the present invention is method of providing a coating. The method comprises the steps of:
[0012] a) applying the coating composition of the first aspect to a substrate; and
[0013] b) drying, or allowing to dry, the applied coating composition.DETAILED DESCRIPTION
[0014] Test methods refer to the most recent test method as of the priority date of this document when a date is not indicated with the test method number. References to test methods contain both a reference to the testing society and the test method number. The following test method abbreviations and identifiers apply herein: ASTM refers to ASTM International methods and ISO refers to International Organization for Standardization.
[0015] Products identified by their tradename refer to the compositions available under those tradenames on the priority date of this document.
[0016] “And / or” means “and, or as an alternative” . All ranges include endpoints unless otherwise indicated. Unless otherwise stated, all percent (%) values are weight precent values relative to composition weight.
[0017] “Aqueous” dispersion herein means that polymer particles dispersed in an aqueous medium. By “aqueous medium” herein is meant water and 0 to 30%, by weight based on the weight of the medium, of water-miscible compound (s) such as, for example, alcohols, glycols, glycol ethers, glycol esters, or mixtures thereof.
[0018] “Structural units” , also known as “polymerized units” , of the named monomer, refers to the remnant of the monomer after polymerization, that is, polymerized monomer or the monomer in polymerized form. For example, a structural unit of methyl methacrylate is as illustrated: where the dotted lines represent the points of attachment of the structural unit to the polymer backbone.
[0019] “Nonionic monomer” herein refers to a monomer that does not bear an ionic charge between pH=1-14.
[0020] The term “D50” particle size (interchangeably used with “average particle size” ) represents the average volume particle size of particles. D50 is the particle size measured in volume corresponding to 50%of the cumulative particle population. For example, if D50 = 10 μm, 50%of the particle have an average volume particle size below 10 μm and 50%of the particle have a volume average particle size above 10 μm. Unless indicated otherwise, all average particle sizes are calculated using D50.
[0021] Throughout this document, the word fragment “ (meth) acryl” refers to both “methacryl” and “acryl” . For example, (meth) acrylic acid refers to both methacrylic acid and acrylic acid, and methyl (meth) acrylate refers to both methyl methacrylate and methyl acrylate.
[0022] “Solids content” of an aqueous dispersion refers to weight percentages of solids weight of the aqueous dispersion after drying at 150 ℃ for 20 minutes, relative to the aqueous dispersion weight.
[0023] The coating composition comprises an aqueous dispersion of components (A) to (D) , and optionally, pigments and / or extenders.
[0024] The coating composition comprises component (A) polymer particles. The polymer particles (A) can be acrylic polymer particles. “Acrylic polymer” herein includes i) a polymer comprising structural units of one or more acrylic monomers without other comonomers, and / or ii) a polymer comprising structural units of one or more acrylic monomers with other comonomers (including, for example, styrene, substituted styrene, other compatible olefmic monomer, or mixtures thereof) , e.g., styrene acrylic copolymers, vinyl acetate-acrylic copolymers, or mixtures thereof. “Acrylic monomer” may include, for example, (meth) acrylic acid, alkyl (meth) acrylate, (meth) acrylamide, (meth) acrylonitrile and their modified forms such as hydroxyalkyl (meth) acrylate.
[0025] The polymer particles (A) may comprise structural units of an alkyl (meth) acrylate. “Alkyl (meth) alkylate” refers to an alkyl ester of (meth) acrylic acid containing a linear, branched, or cyclic alkyl group. The alkyl (meth) acrylate can be a C1-C24-alkyl (meth) acrylate (i.e., an alkyl (meth) acrylate having an alkyl with from 1 to 24 carbon atoms) , desirably, a C1-C8-alkyl (meth) acrylate such as a C1-C2-alkyl (meth) arylate, a C4-C8-alkyl (meth) arylate, or mixtures thereof. Examples of suitable alkyl (meth) acrylates include methyl acrylate, methyl methacrylate (MMA) , butyl acrylate (n-butyl acrylate, BA) , ethyl methacrylate, ethyl acrylate (EA) , 2-ethylhexyl acrylate (2-EHA) ; butyl methacrylate (n-butyl methacrylate, BMA) , t-butyl methacrylate, 2-ethylhexyl methacrylate; cycloalkyl (meth) acrylates such as cyclohexyl (meth) acrylate, methcyclohexyl (meth) acrylate, dihydrodicyclopentadienyl (meth) acrylate, trimethylcyclohexyl (meth) acrylate, and t-butyl cyclohexyl (meth) acrylate; or mixtures thereof, desirably, MMA, BA, EA, 2-EHA, or mixtures thereof. The concentration of structural units of the alkyl (meth) acrylate may be at least 30%, and can be in a range of 30%to 99.5%, 70%to 98%, or 80%to 95%, by weight based on the weight of the polymer particles (A) . Unless otherwise stated, the weight of the polymer particles refers to the dry weight of the polymer particles.
[0026] The polymer particles (A) may comprise, or be free of, structural units of an ethylenically unsaturated acid monomer. Examples of suitable ethylenically unsaturated acid monomers include α, β-ethylenically unsaturated carboxylic acids such as methacrylic acid (MAA) , acrylic acid (AA) , itaconic acid, maleic acid, or fumaric acid; or a monomer bearing an acid-forming group which yields or is subsequently convertible to, such an acid group such as anhydride, (meth) acrylic anhydride, or maleic anhydride; ethylenically unsaturated sulfuric acid-or sulfonic acid-containing monomers and / or salts thereof including, for example, sodium styrene sulfonate (SSS) , sodium vinyl sulfonate (SVS) , 2-acrylamido-2-methylpropanesulfonic acid (AMPS) , sodium salt of 2-acrylamido-2-methyl-1-propanesulfonic acid, ammonium salt of 2-acrylamido-2-methyl-1-propane sulfonic acid; sodium salt of allyl ether sulfonate; sodium 1-allyloxy-2-hydroxypropane sulfonate; or mixtures thereof; ethylenically unsaturated phosphorous acid-containing monomers and / or salts thereof including, for example, phosphoalkyl (meth) acrylates such as phosphoethyl (meth) acrylate, phosphopropyl (meth) acrylate, phosphobutyl (meth) acrylate, salts thereof, and mixtures thereof; CH2=C (Rp1) -C (O) -O- (Rp2O) p-P (O) (OH) 2, wherein Rp1=H or CH3, Rp2=alkyl and p=1-10, such as SIPOMER PAM-100, SIPOMER PAM-200, SIMPOMER COPS-3, SIPOMER PAM-6835, SIPOMER PAM-5000, and SIPOMER PAM-300 all available from Syensqo; phosphoalkoxy (meth) acrylates such as phospho ethylene glycol (meth) acrylate, phospho di-ethylene glycol (meth) acrylate, phospho tri-ethylene glycol (meth) acrylate, phospho propylene glycol (meth) acrylate, phospho di-propylene glycol (meth) acrylate, phospho tri-propylene glycol (meth) acrylate, allyl ether phosphate, and vinyl phosphonic acid; salts thereof; or mixtures thereof. Desirably, the ethylenically unsaturated acid monomer is selected from phosphoethyl methacrylate (PEM) and / or salts thereof, AA, MAA, or mixtures thereof. The concentration of structural units of the ethylenically unsaturated acid monomer may be in a range of 0.1%to 5%, and can be 0.5%or more, 0.8%or more, 1%or more, even 1.1%or more while at the same time is generally 5%or less, and can be 4.5%or less, 4%or less, 3%or less, 2.5%or less, 2%or less, or even 1.5%or less, desirably from 1%to 2.5%, based on the weight of the polymer particles (A) .
[0027] The polymer particles (A) may comprise, or can be free of, structural units of a monoethylenically unsaturated functional monomer carrying at least one functional group selected an acetoacetyl such as acetoacetoxy or acetoacetamide functional group, alkoxysilane, amide, ureido, or hydroxyl group; or combinations thereof (hereinafter referred to as “functional monomer” ) . Examples of suitable functional monomers include acetoacetoxyalkyl (meth) acrylates such as acetoacetoxyethyl methacrylate (AAEM) , acetoacetoxyethyl acrylate, acetoacetoxypropyl methacrylate, acetoacetoxybutyl methacrylate, and 2, 3-di (acetoacetoxy) propyl methacrylate; allyl acetoacetate; vinyl acetoacetate; acetoacetamidoalkyl (meth) acrylates such as acetoacetamidoethyl methacrylate, acetoacetamidoethyl acrylate, or mixtures thereof; acrylamide (AM) , methacrylamide, monosubstituted (meth) acrylamide, N-methylacrylamide, N-ethylacrylamide, N-isopropylacrylamide, N-butylacrylamide, N-tertiary butylacrylamide, N-2-ethylhexylacrylamide, N, N-dimethylacrylamide, N, N-diethylacrylamide; hydroxy-functional (meth) acrylic acid alkyl ester such as hydroxyethyl methacrylate (HEMA) and hydroxypropyl methacrylate; alkoxysilane monomers such as methacryloxypropyl trimethoxysilane (MTMS) or vinyltrimethoxysilane (VTMS) ; ureido monomers such as methacrylo ethylethylene urea and SIMPOMER WAM II from Solvay, or mixtures thereof. Desirably, the functional monomer is selected from AM, HEMA, AAEM, MTMS, VTMS, or mixtures thereof. The concentration of structural units of the functional monomer in the polymer particles (A) may be in a range of zero to 15%, and can be 0.1%or more, 0.3%or more, 0.5%or more, 0.8%or more, 0.9%or more, 1.0%or more, 1.1%or more, 1.2%or more, 1.5%or more, even 1.8%or more while at the same time is generally 15%or less, and can be 8%or less, 6%or less, 5%or less, 4%or less, 3%or less, 3.2%or less, or even 2.8%or less, by weight based on the weight of the polymer particles (A) .
[0028] The polymer particles (A) may comprise, or be free of, structural units of an additional monoethylenically unsaturated monomer that is other than the alkyl (meth) alkylate and the functional monomer described above, such as an itaconate ester, a vinyl aromatic monomer, a vinyl ester monomer such as vinyl acetate (VA) , acrylonitrile, methacrylonitrile, or mixtures thereof. Examples of suitable itaconate esters include dibutyl itaconate, dihexyl itaconate, dioctyl itaconate, didecanyl itaconate, or mixtures thereof. Examples of suitable vinyl aromatic monomers include styrene (ST) and substituted styrene such as . alpha. -methyl styrene, α-ethylstyrene, p-methyl styrene, t-butyl styrene, trans-beta-methylstyrene, 2, 4-dimethylstyrene, ethylstyrene, o-, m-, and p-methoxystyrene; p-trifluoromethylstyrene, vinyl xylene, or mixtures thereof, desirably styrene. Desirably, the additional monoethylenically unsaturated monomer is selected from ST, VA, or mixtures thereof. The concentration of structural units of the additional monoethylenically unsaturated monomer in the polymer particles (A) may be in a range of zero to 70%, and can be 10%to 60%, 20%to 50%, 30%to 40%, by weight based on the weight of the polymer particles (A) .
[0029] The polymer particles (A) may comprise, or be free of, structural units of a multiethylenically unsaturated nonionic monomer. Suitable multiethylenically unsaturated nonionic monomers may include, for example, butadiene, allyl (meth) acrylate, divinyl benzene, ethylene glycol dimethacrylate, butylene glycol dimethacrylate, or mixtures thereof. The concentration of structural units of the multiethylenically unsaturated nonionic monomers in the polymer particles (A) may be in a range of from zero to 3.0%, from 0.05%to 0.8%, or from 0.1%to 0.5%, desirably less than 1%, more desirably less than 0.2%, by weight based on the weight of the polymer particles (A) .
[0030] Desirably, the polymer particles (A) comprise, by weight based on the weight of the polymer particles (A) , from 45%to 99%of structural units of the alkyl (meth) acrylate such as MMA, EA, or mixtures thereof; from 1%to 5%of structural units of the ethylenically unsaturated acid monomer such as PEM, AA, MAA, or mixtures thereof; from 0 to 10%of structural units of the functional monomer such as AAEM; and from 0 to 40%of structural units of the additional monoethylenically unsaturated monomer such as ST, VA, or mixtures thereof.
[0031] Types and levels of the monomers described above for preparing the polymer particles (A) may be chosen to provide a polymer glass transition temperature (Tg) in a range of from -10 to 50 degrees Celsius (℃) , and can be -5 ℃ or higher, 0 ℃ or higher, 5 ℃ or higher, even 10 ℃ or higher while at the same time is generally 50 ℃ or less, and can be 45 ℃ or less, 40 ℃ or less, 35 ℃ or less, 30 ℃ or less, 25 ℃ or less, 20 ℃ or less, or even 15 ℃ or less, desirably from 10 to 35 ℃. Tgs of the polymer particles (A) can be measured by differential scanning calorimetry (DSC) . Desirably, the polymer particles (A) are acrylic polymer particles having a Tg in a range of 10 to 35 ℃, as measured by DSC.
[0032] The polymer particles (A) have a Z-average particle size in a range of 80 nanometers (nm) to 500 nm, and can be 90 nm or more, 100 nm or more, greater than 100 nm, even 105 nm or more while at the same time is generally 500 nm or less, and can be 450 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, 180 nm or less, or even 150 nm or less, desirably from 100 nm to 200 nm. The Z-average particle size can be measured using a Zetasizer Nano S90 available from Malvern or Brookhaven BI-90 Plus Particle Size Analyzer.
[0033] The polymer particles (A) , typically present in an aqueous dispersion, can be prepared by emulsion polymerization of the monomers described above. Emulsion polymerization is known to one skilled in the art, typically in the presence of one or more surfactants. Multistage emulsion polymerization can also be used in preparing the binder, which at least two stages are formed sequentially, and usually results in the formation of the multistage polymer comprising at least two polymer compositions.
[0034] The concentration of the polymer particles (A) in the coating composition may be in a range of from 9.6%to 24%, and can be 10%or more, 10.5%or more, 11%or more, 11.5%or more, 12%or more, 12.5%or more, 13%or more, 13.5%or more, 14%or more, even 14.5%or more while at the same time is generally 24%or less, and can be 22%or less, 20%or less, 19.2%or less, 18%or less, 17.5%or less, 16.8%or less, or even 16%or less, desirably from 12%to 16.8%, more desirably from 14.5%to 16.0%, by dry weight based on the weight of the coating composition. Unless otherwise stated, “weight of the coating composition” refers to the wet weight of the coating composition.
[0035] The coating composition also comprises component (B) polymeric organic crosslinked microspheres. The polymeric organic crosslinked microspheres (B) may comprise a low Tg first stage polymer that is crosslinked (hereinafter also referred to as “first stage crosslinked polymer” ) to provide resiliency and no diffusion to the substrate; and a high Tg second stage polymer to provide microspheres that are not film-forming at room temperature. The first stage polymer may have a Tg ≤ 20 ℃, desirably <10 ℃, more desirably < 0 ℃; and the second stage polymer may have a Tg ≥ 30 ℃, desirably greater than 50 ℃. Desirably, at least 50%, more desirably at least 70%, and most desirably at least 90%of the first stage crosslinked polymer of the polymeric organic crosslinked microspheres (B) comprises structural units of I) methyl acrylate, butyl acrylate, or ethyl acrylate, or combinations thereof; and II) a multiethylenically unsaturated nonionic monomer, described herein below, at a weight to weight ratio of I) to II) in a range of 99.5: 0.5 to 90: 10; desirably, methyl methacrylate comprises at least 60%, more desirably at least 80%, most desirably at least 90%of the second stage polymer. Tgs values herein are those calculated by using the Fox equation (T.G. Fox, Bull. Am. Physics Soc., Volume 1, Issue No. 3, page 123 (1956) ) described below. For example, for calculating the Tg of a copolymer of monomers M1 and M2,
[0036] where Tg (calc. ) is the glass transition temperature calculated for the copolymer, w (M1) is the weight fraction of monomer M1 in the copolymer, w (M2) is the weight fraction of monomer M2 in the copolymer, Tg (M1) is the glass transition temperature of the homopolymer of monomer M1, and Tg (M2) is the glass transition temperature of the homopolymer of monomer M2, all temperatures being in K. The glass transition temperatures of the homopolymers may be found, for example, in “Polymer Handbook” , edited by J. Brandmp and E. H. Immergut, Interscience Publishers.
[0037] The polymeric organic crosslinked microspheres (B) may have a median weight average particle size in a range of 1 micrometer (μm) to 40 μm, and can be 2 μm or more, 3 μm or more, 4 μm or more, 4.5 μm or more, 4.6 μm or more, 4.7 μm or more, 4.8 μm or more, 4.9 μm or more, 5 μm or more, 5.5 μm or more, 6 μm or more, even 6.5 μm or more while at the same time is generally 40 μm or less, and can be 35 μm or less, 30 μm or less, 25 μm or less, 22.5 μm or less, 20 μm or less, 17.5 μm or less, 15 μm or less, 12.5 μm or less, 10 μm or less, or even 9 μm or less, desirably from 4 to 12 μm, as measured by Disc Centrifuge Photosedimentometer (DCP) . Further details may refer to the DCP Particle Sizing Method described in the Examples section below. Desirably, the polymeric organic crosslinked microspheres (B) comprise the first stage crosslinked polymer having a Tg ≤ 20 ℃ and the second stage polymer having a Tg ≥ 30 ℃, as calculated by the Fox equation; and the median weight average particle size is in a range of from 2 μm to 15 μm.
[0038] Aqueous dispersions of polymeric organic crosslinked microspheres can be prepared in a variety of ways, including those described in US Pat. Pub. 2013 / 0052454; US4,403,003; US7,768,602; US7,829,626, US11,981,830, and US10,676,580B2. For example, the aqueous dispersion of polymeric organic crosslinked microspheres may be prepared by a process comprising the step of contacting, under polymerization conditions, an aqueous dispersion of first microspheres comprising a first monoethylenically unsaturated nonionic monomer with first stage monomers, to grow out the first microspheres to form the aqueous dispersion of second microspheres. Desirably, the aqueous dispersion of the first microspheres is contacted under polymerization conditions, optionally in the presence of an emulsifying surfactant such as a phosphate or an alkyl benzene sulfonate or sulfate, with the first stage monomers comprising, by weight based on the weight of the first stage monomers, a) from 0 to 5%of a polymerizable organic phosphate or a salt thereof, and can be 0.05%or more, 0.1%or more, even 0.2%or more while at the same time is generally 5%or less, and can be 3%or less, or even 2%or less; and b) from 70%to 99.95%of a second monoethylenically unsaturated nonionic monomer, and can be 80%or more, or even 90%or more while at the same time is generally 99.95%or less, or 99.8%or less. Suitable polymerizable organic phosphate and / or the salt thereof may include those described in US1,1981,830B. Desirably, the first stage monomers further comprise a multiethylenically unsaturated nonionic monomer, typically at a concentration in a range of 0.1%to 15%, and can be 0.5%or more, 1%or more, even 2%or more while at the same time is generally 15%or less, and can be 12%or less, 10%or less, or even 8%or less, by weight based on the weight of the first stage monomers. The multiethylenically unsaturated nonionic monomers may include those described above in the polymer particles (A) section above. Particularly suitable multiethylenically unsaturated nonionic monomers may include allyl methacrylate, allyl acrylate, divinyl benzene, trimethyolopropane trimethacrylate, trimethylolpropane triacrylate, butylene glycol (1, 3) dimethacrylate, butylene glycol (1, 3) diacrylate, ethylene glycol dimethacrylate.
[0039] Desirably, the first microspheres comprise from 90%to 99.9%of structural units of the first monoethylenically unsaturated nonionic monomer. Examples of suitable monoethylenically unsaturated nonionic monomers include acrylates such as ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate; methacrylates such as methyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, acetoacetoxyethyl methacrylate and uredio methacrylate; acrylonitrile; acrylamides such as acrylamide and diacetone acrylamide; styrene; and vinyl esters such as vinyl acetate. Although it is possible for the first microspheres to include structural units of carboxylic acid monomers such as methacrylic acid or acrylic acid, it is preferred that the first microspheres comprise less than 5%, less than 3%, or even less than 1%of structural units of a carboxylic acid monomer, by weight based on the weight of the first microspheres. More desirably, the first microspheres comprise structural units of acrylate or methacrylates or combinations of acrylates and methacrylates.
[0040] The first microspheres are advantageously prepared from an aqueous dispersion of an oligomeric seed having a weight average molecular weight (Mw) in a range of 800 grams per mole (g / mol) to 20,000 g / mol, and can be 1,000 g / mol or more, even 1, 500 g / mol or more while at the same time is generally 20,000 g / mol or less, and can be 10,000 g / mol or less, or even 5,000 g / mol or less, as determined by size exclusion chromatography using polystyrene standards. The oligomeric seed may have an average diameter in a range of 200 nm to 8,000 nm, and can be 400 nm or more, even 600 nm or more while at the same time is generally 8,000 nm or less, and can be 5,000 nm or less, 1,500 nm or less, or even 1,000 nm or less, as measured by DCP. Further details may refer to the DCP Particle Sizing Method described in the Examples section below. as described in the Examples section below. The oligomeric seed contains structural units of a chain transfer agent. Particularly, suitable chain transfer agents include an alkyl mercaptan, examples of which include n-dodecyl mercaptan, 1-hexanethiol, 1-octane thiol, and 2-butyl mercaptan. The oligomeric seed is advantageously contacted with the first monoethylenically unsaturated nonionic monomer described above in the presence of a hydrophobic initiator, in any order, to transport the initiator into the seed, or seed swollen with monomer. As used herein, a hydrophobic initiator refers to an initiator having a water solubility in the range of 5 ppm or more, or 10 ppm or more, and at the same time, 10,000 ppm or less, 1,000 ppm or less, or even 100 ppm or less. Examples of suitable hydrophobic initiators include t-amyl peroxy-2-ethyl hexanoate (water solubility=17.6 mg / L at 20℃) , t-butyl peroxy-2-ethylhexanoate (water solubility=46 mg / L at 20℃) , or mixtures thereof. The extent of swelling (seed growth) can be controlled by the ratio of the monomer to the seed.
[0041] Forming microspheres from oligomeric seed provides an effective way of controlling the particle size distribution of the microspheres. Desirably, the coefficient of variation of the first microspheres and the second microspheres, as determined by DCP, is less than 25%, less than 20%, less than 15%, or even less than 10%. Desirably, the particle size of the first microspheres is in a range of 2.5 μm to 20 μm, and can be 3.5 μm or more, 4.0 μm or more, 4.5 μm or more, 5.0 μm or more, even 5.5 μm or more while at the same time is generally 20 μm or less, and can be 18 μm or less, 15 μm or less, 12 μm or less, or even 10 μm or less, as measured by DCP. Further details may refer to the DCP Particle Sizing Method described in the Examples section below.
[0042] Desirably, the first microspheres as well as the second microspheres comprise a substantial absence of structural units of a carboxylic acid monomer. As used herein, a substantial absence of structural units of a carboxylic acid monomer means less than 5%, less than 3%, less than 1%, or even less than 0.2%of structural units of a carboxylic acid monomer such as methacrylic acid or acrylic acid, by weight based on the weight of the microspheres.
[0043] Desirably, the second microspheres comprise, by weight based on the weight of the second microspheres, from 90%to 98%structural units of a second monoethylenically unsaturated nonionic monomers including those described above for the first microspheres, which may be the same as or different from the first monoethylenically unsaturated nonionic monomer.
[0044] The concentration of the polymeric organic crosslinked microspheres (B) in the coating composition is in a range of from 1%to 6.5%, and can be 1.2%or more, 1.3%or more, 1.4%or more, 1.5%or more, 1.6%or more, 1.7%or more, 1.8%or more, 2.0%or more, 2.1%or more, even 2.2%or more while at the same time is generally 6.5%or less, and can be 6.1%or less, 6.0%or less, 5.5%or less, 5.2%or less, 5.0%or less, 4.8%or less, 4.6%or less, 4.4%or less, 4.2%or less, 4.1%or less, 3.9%or less, 3.8%or less, or even 3.7%or less, desirably from 1.2%to 4.5%, more desirably from 1.3%to 4.4%, by dry weight based on the weight of the coating composition.
[0045] The coating composition also comprises component (C) silica (interchangeably used with “silicon dioxide” and “SiO2” ) particles. The silica particles (C) may have a D50 particle size in a range of from 5 μm to 30 μm, and can be 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, 10 μm or more, greater than 10 μm, 12 μm or more, even 15 μm or more while at the same time is generally 30 μm or less, and can be 25 μm or less, 20 μm or less, 18 μm or less, 16 μm or less, or even 15 μm or less, desirably greater than 10 μm to 20 μm, more desirably from 12 μm to 18 μm, as measured according to ISO 13320: 2020 Particle Size Analysis -Laser Diffraction Methods.
[0046] The silica particles (C) may have a BET surface area less than 50 square meters per gram (m2 / g) , and can be less than 45 m2 / g, less than 40 m2 / g, less than 35 m2 / g, less than 30 m2 / g, less than 25 m2 / g, less than 20 m2 / g, less than 18 m2 / g, less than 15 m2 / g, less than 14 m2 / g, even less than 12 m2 / g while at the same time is generally 1 m2 / g or more, and can be 2 m2 / g or more, 3 m2 / g or more, or even 4 m2 / g or more, desirably less than 12 m2 / g. Brunauer-Emmett-Teller (BET) surface area analysis is the multi-point measurement of an analyte′s specific surface area (m2 / g) through gas adsorption analysis, where an inert gas such as nitrogen is continuously flowed over a solid sample, or the solid sample is suspended in a defined gaseous volume. Further details may refer to the BET Surface Area Analysis described in the Examples section below.
[0047] The silica particles (C) may have an average aspect ratio in a range of from 1.0 to less than 2.0. The “aspect ratio” refers to the ratio of major axis length to the minor axis length of the ellipse that has the same normalized second central moments as the silica particle in a SEM image, where the ellipse is obtained by fitting a multivariate normal distribution to the silica particle. Further details may refer to Figure 5, M. Fritz et. al., Microplasfics, 2024, 3 (1) , pages 124-146. The average aspect ratio is calculated as the arithmetic mean of all analyzed silica particles. Desirably, the average aspect ratio of the silica particles is in a range of 1.0 to 1.8, more desirably in a range of 1.0 to 1.5, and most desirably in a range of 1.0 to 1.4.
[0048] Desirably, the pH value of the silica particles (C) is more than 6, desirably more than 6.5, most desirably more than 7.0. The pH value is measured using a pH meter with 5%silica particles dispersed in di-ionized water. The silica particles can be precipitated silica particles, which are typically prepared by a precipitated process such as those described in US8,945,517.
[0049] The concentration of the silica particles (C) in the coating composition is in a range of 2%to less than 10%, and can be 2.2%or more, 2.4%or more, 2.5%or more, 2.6%or more, 2.8%or more, 2.9%or more, 3%or more, greater than 3%, 3.2%or more, 3.5%or more, 3.8%or more, 4.0%or more, 4.2%or more, 4.5%or more, 4.8%or more, even 5%or more while at the same time is generally less than 10%, and can be 9.8%or less, 9.5%or less, 9.2%or less, 9%or less, 8.8%or less, 8.5%or less, 8.2%or less, 8%or less, 7.5%or less, 7%or less, 6.5%or less, or even 6%or less, desirably from 2.5%to 7%, more desirably from 2.9%to 6%, by dry weight based on the weight of the coating composition.
[0050] The coating composition also comprises component (D) polysiloxane particles. The polysiloxane can be a linear and / or branched polymer comprising repeat units of Si-O-Si groups and Si-alkyl groups; the polysiloxane optionally comprises, for example, Si-O-alkyl, Si-O-aryl, Si-OH, Si-H, and / or Si-O-trialkylsilyl groups. Desirably, the polysiloxane is a linear polymer represented by the following structure (I) :
[0051] wherein each R1 is independently C1-C30 alkyl, O-C1-C6-alkyl, or H, provided that at least one R1 is C1-C30-alkyl; each R2 is independently C1-C30-alkyl, H, or Si (R3) 3, wherein each R3 is independently C1-C6-alkyl; and n is in a range of from 1,000 to 11,000, desirably from 1,500 to 11,000.
[0052] Desirably, each R1 is independently C1-C6-alkyl, more desirably ethyl or methyl, and most desirably methyl; desirably, each R2 is H; and desirably, R3 is methyl.
[0053] The polysiloxane particles (D) have a D50 particle size in a range of from 1 μm to 20 μm, and can be 2 μm or more, 2.5 μm or more, 3 μm or more, 3.5 μm or more, even 4 μm or more while at the same time is generally 20 μm or less, and can be 15 μm or lower, 10 μm or lower, or even 9 μm or lower, desirably from 3 to 10 μm, as measured by a Malvern Mastersizer 3000 Particle Size Analyzer, e.g., from Malvern Instruments.
[0054] The concentration of the polysiloxane particles (D) in the coating composition is in a range of from 0.24%to 4.4%, and can be 0.3%or more, 0.4%or more, 0.5%or more, 0.6%or more, 0.7%or more, even 0.8%or more while at the same time is generally 4.4%or less, and can be 4.2%or less, 4.0%or less, 3.8%or less, 3.6%or less, 3.4%or less, 3.2%or less, 3.0%or less, 2.8%or less, 2.6%or less, 2.4%or less, 2.2%or less, 2.1%or less, 2%or less, 1.9%or less, 1.8%or less, 1.6%or less, 1.4%or less, 1.3%or less, 1.2%or less, 1.1%or less, 1.0%or less, or even 0.8%or less, desirably from 0.4%to 2.4%, by dry weight based on the weight of coating composition.
[0055] Desirably, the coating composition comprises, by dry weight based on the weight of the coating composition, from 9.6%to 24%of the polymer particles (A) , from 1.3%to 4.4%of the polymeric organic crosslinked microspheres (B) , from 2.9%to 6%of the silica particles (C) , and from 0.4%to 2.4%of the polysiloxane particles (D) .
[0056] The coating composition may comprise, or can be free of, (E) one or more pigments. “Pigments” herein refers to particulate inorganic materials which are capable of materially contributing to the opacity or hiding capability of a coating. Such materials typically have a refractive index greater than 1.9. The pigments may include, for example, zinc oxide, titanium dioxide (TiO2) , iron oxide, barium sulfate, barium carbonate, or mixtures thereof. Desirably, the pigment is TiO2. TiO2 typically exists in two crystal forms, anastase and rutile. TiO2 may be also available in concentrated dispersion form. The coating composition may comprise or be free of one or more extenders. The pigment volume concentration of TiO2 (hereinafter referred to as “PVC (TiO2) ” ) may be in a range of from 5%to 30%, from 8%to 25%, or from 15%to 22%. PVC (TiO2) is defined by the following equation:
[0057] PVC (TiO2) = (Volume solids of TiO2) / Total volume solids of coating composition) x 100%,
[0058] where “total volume solids” includes the contribution from components (A) to (D) described above, TiO2 (if present) , extender (if present) , and other solids (if present) that constitute the volume of the final dried coating.
[0059] The coating composition may comprise, or can be free of, one or more extenders. “Extender” herein refers to a particulate material having a refractive index of less than or equal to 1.9 and greater than 1.0 that is other than the silica particles (C) described above. Examples of suitable extenders include calcium carbonate, clay, calcium sulfate, aluminosilicates, silicates, zeolites, mica, diatomaceous earth, solid or hollow glass, ceramic beads, nepheline syenite, feldspar, calcined diatomaceous earth, talc (hydrated magnesium silicate) , alumina, kaolin, pyrophyllite, perlite, baryte, wollastonite, opaque polymers such as ROPAQUETM Ultra E polymer available from The Dow Chemical Company (ROPAQUE is a trademark of The Dow Chemical Company) , or mixtures thereof. The pigment volume concentration of extender (hereinafter referred to as PVC (extender) ) may be less than 5%, less than 1%, less than 0.1%, or even zero. PVC (extender) is defined by the following equation:
[0060] PVC (extender) = (Volume solids of extender) / Total volume solids of coating composition) x 100%, where “total volume solids” is as described above.
[0061] The coating composition may comprise, or can be free of, one or more surfactants. The surfactant may be selected from an anionic surfactant, a nonionic surfactant, or mixtures thereof. Examples of suitable surfactants include alkali metal or ammonium salts of alkyl, aryl, or alkylaryl sulfates such as sodium lauryl sulfate, sulfonates, or phosphates; alkyl sulfonic acids; sulfosuccinate salts; fatty acids; polymerizable surfactants; and ethoxylated alcohols or phenols. Commercially available surfactants may include, for example, anionic surfactants such as Rhodafac RS-610 alkyl ethoxylated phosphate available from Solvay S.A., ABS-15 sodium dodecyl benzene sulfonate from Shanghai Honesty Fine Chemical Co., Ltd., and Disponil FES 32 fatty alcohol ether sulfate available from BASF; nonionic surfactants such as TERGITOLTM 15-S-40 Surfactant (a secondary alcohol ethoxylate) available from Dow Chemical Company (TERGITOL is a trademark of The Dow Chemical Company) ; or mixtures thereof. The surfactant may be present at a concentration of zero to 10%, and can be 0.1%to 9.5%, 0.3%to 9%, 0.4%to 8.5%, 0.5%to 8%, or 0.5%to 2.5%, by weight based on the dry weight of the coating composition.
[0062] The coating composition may comprise, or can be free of, one or more dispersants. The dispersant may be a nonionic dispersant described above, an anionic dispersant, or mixtures thereof. Suitable dispersants may include, for example, nonionic dispersants such as 2-amino-2-methyl-1-propanol (AMP) , dimethyl amino ethanol (DMAE) , or mixtures thereof; anionic dispersants such as polyacids with suitable molecular weight, 2-amino-2-methyl-1-propanol (AMP) , dimethyl amino ethanol (DMAE) , potassium tripolyphosphate (KTPP) , trisodium polyphosphate (TSPP) , citric acid and other carboxylic acids; or mixtures thereof. The polyacids used may include homopolymers and copolymers based on polycarboxylic acids (e.g., weight average molecular weight ranging from 1,000 to less than 50,000 g / mol as measured by gel permeation chromatography (GPC) ) , including those that have been hydrophobically- or hydrophilically-modified, e.g., polyacrylic acid or polymethacrylic acid or maleic anhydride with various monomers such as styrene, acrylate or methacrylate esters, diisobutylene, and other hydrophilic or hydrophobic comonomers; salts of thereof; or mixtures thereof. The dispersant may be present at a concentration of from zero to 5%, from 0.2%to 3.0%, or from 0.5%to 2.5%, by dry weight based on the dry weight of the coating composition.
[0063] The coating composition may comprise, or can be free of, one or more rheology modifiers. The rheology modifiers may include polyvinyl alcohol (PVA) , clay materials, acid derivatives, acid copolymers, urethane associate thickeners (UAT) , polyether urea polyurethanes (PEUPU) , polyether polyurethanes (PEPU) , or mixtures thereof. Examples of suitable thickeners include alkali swellable emulsions (ASE) such as sodium or ammonium neutralized acrylic acid polymers; hydrophobically modified alkali swellable emulsions (HASE) such as hydrophobically modified acrylic acid copolymers; associative thickeners such as hydrophobically modified ethoxylated urethanes (HEUR) ; and cellulosic thickeners such as methyl cellulose ethers, hydroxymethyl cellulose (HMC) , hydroxyethyl cellulose (HEC) , hydrophobically-modified hydroxy ethyl cellulose (HMHEC) , sodium carboxymethyl cellulose (SCMC) , sodium carboxymethyl 2-hydroxyethyl cellulose, 2-hydroxypropyl methyl cellulose, 2-hydroxyethyl methyl cellulose, 2-hydroxybutyl methyl cellulose, 2-hydroxyethyl ethyl cellulose, and 2-hydoxypropyl cellulose. Desirably, the thickener is selected from HEC, HEUR, or mixtures thereof. The rheology modifiers may be present at a concentration of from zero to 5.0%, 0.2%to 4.0%, or 0.3%to 3%, by dry weight based on the dry weight of the coating composition.
[0064] The coating composition may also comprise water. Water may be present, by weight based on the weight of the coating composition, from 10%to 90%, from 15%to 85%, or from 20%to 80%.
[0065] In addition to the components described above, the coating composition may further comprise any one or combination of the following additives: coalescents, defoamers, buffers, anti-freezing agents, humectants, mildewcides, biocides, anti-skinning agents, colorants, flowing agents, antioxidants, plasticizers, leveling agents, neutralizing agents, thixotropic agents, adhesion promoters, and grind vehicles. These additives may be present in a combined amount of from zero to 20%, from 0.5%to 15%, or from 1.0%to 10%, by weight based on the dry weight of coating composition.
[0066] The present invention also relates to a process for preparing the coating composition. The process comprises admixing the polymer particles (A) , the polymeric organic crosslinked microspheres (B) , the silica particles (C) , the polysiloxane particles (D) , and optionally, any one or combination of other components described above such as the pigment. Components in the coating composition may be mixed in any order to provide the coating composition of the present invention. Any of the above-mentioned optional components may also be added to the composition during or prior to the mixing to form the coating composition.
[0067] The present invention also provides a method of providing a coating or a coated substrate. The method comprises the steps of: a) applying the coating composition to a substrate, and b) drying, or allowing to dry, the applied coating composition, thereby forming the antimicrobial coating (hereinafter also referred to as “coating” ) or the coating substrate. The coating composition can be applied to a substrate by incumbent means including brushing, dipping, rolling, and spraying. Desirably, the coating composition is applied by spraying. The standard spray techniques and equipment for spraying such as air-atomized spray, air spray, airless spray, high volume low pressure spray, and electrostatic spray such as electrostatic bell application, and either manual or automatic methods can be used. After The coating composition has been applied to a substrate, the coating composition can dry, or allow to dry, to form a film (this is, coating or paint) at room temperature (20-25 degrees Celsius (℃) ) , or at an elevated temperature, for example, from 35 to 60 ℃. The coating (that is, a film) obtained therefrom or the coated substrate has demonstrated both excellent heel scuff resistance as indicated by a heel scuffcolor change ≤ 0.8 and excellent coin scuffresistance as indicated by a coin scuff color change ≤ 0.5 while at the same time demonstrated a low gloss, showing a 60° gloss value ≤ 10. Further details for determining the properties may refer to the Heel Scuff Resistance Test, Coin Scuff Resistance Test, and 60 ° Gloss Test described in the Examples section below.
[0068] The coating composition can be applied to, and adhered to, various substrates. Examples of suitable substrates include concrete, cementious substrates, wood, metals, stones, elastomeric substrates, glass, and fabrics. The coating composition can be used as is suitable for various applications where antiviral properties are desired, including, for example, wood coatings, metal protective coatings, architecture coatings, traffic paints, marine and protective coatings, automotive coatings, wood coatings, joinery coatings, floor coatings, coil coatings, traffic paints, and civil engineering coatings. The coating composition can be used alone, or in combination with other coatings to form multi-layer coatings.
[0069] EXAMPLES
[0070] Some embodiments of the invention will now be described in the following Examples, wherein all parts and percentages are weight percentages relative to composition, unless otherwise specified. The materials used in the examples and their abbreviations are given in Table 1 below. TERGITOL, OROTAN, ACRYSOL, DOWSIL, and PRIMAL are trademarks of The Dow Chemical Company or its affiliates.
[0071] Table 1
[0072] 1particle size analysis of silica particles: The D50 particle size of silica particles was measured by laser diffraction method according to ISO 13320: 2020.
[0073] 2BET surface area analysis: Brunauer-Emmett-Teller (BET) surface area analysis is the multi-point measurement of an analyte′s specific surface area (m2 / g) through gas adsorption analysis, where an inert gas such as nitrogen is continuously flowed over a solid sample, or the solid sample is suspended in a defined gaseous volume. The samples were pretreated in degasser (Flovac Degasser) ; after vacuum stabilized to about 0.4 mmHg, ramp to 75 ℃ and keep stable for more than 12 hours before testing, but a transparent substance appeared in the upper quarter of the bottom of the glass tube, suspected to be vaporized at 75℃ and recondensed on the glass tube wall at lower temperatures. The data is analyzed through Quantachrome Quadrasorb SI automated surface area and pore size analyzer.
[0074] 3Average aspect ratio of silica particles: SEM images of DP-0115 were used for analysis. The aspect ratio of each silica particle was determined by the ratio of major axis length to the minor axis length of the ellipse that has the same normalized second central moments as the silica particle in a SEM image of DP-0115, where the ellipse was obtained by fitting a multivariate normal distribution to the silica particle (further details may refer to Figure 5, M. Fritz et. al., Microplastics, 2024, 3 (1) , pages 124-146) . Totally, the aspect ratio of 81 particles were calculated, and the average aspect ratio was obtained by sum of aspect ratios of 81 particles / 81.
[0075] 4DCP Particle Sizing Method: Particle sizes and distribution of polymeric organic crosslinked microspheres were measured using Disc Centrifuge Photosedimentometer (DCP, CPS Instruments, Inc., Prairieville, La. ) that separates modes by centrifugation and sedimentation through a sucrose gradient. The samples were prepared by adding 1 to 2 drops of the microsphere dispersion into 10 mL of deionized (DI) water containing 0.1%sodium lauryl sulfate, followed by injection of 0.1 mL of the sample into a spinning disc filled with 15 g / mL of sucrose gradient. For the microspheres, a 2-8%sucrose gradient disc spinning at 3,000 rpm was used, and 9-μm polystyrene calibration standard was injected prior to injection of the sample. Median weight average particle size and coefficient of variation (CV) were calculated using instrument’s algorithm.
[0076] 5Particle size analysis of polysiloxane particles: The D50 particle size of the polysiloxane particles was measured using a Malvern Mastersizer 3000 Particle Size Analyzer.
[0077] 6particle size analysis of binder particles: The Z-average particle size was measured using a Brookhaven BI-90 Plus Particle Size Analyzer.
[0078] 7Tg of polymer particles: Tgs of polymer particles were tested by DSC with DSC-Q2000 instrument over a range of-50 ℃ to 160 ℃ at a ramp rate of 10 ℃ / min for 2 cycles, where the Tg in cycle 2 was recorded.
[0079] IEs 1-7 and CEs 1-7 Samples
[0080] Components for preparing coating composition samples are given in Table 2, with the amount of each component reported in grams (g) . Firstly, all components in the grind stage were added sequentially and mixed using a high-speed Cowles disperser at 1,000 rpm for 30 minutes to get a well dispersed slurry. Then components in the letdown stage were added sequentially into the slurry and mixed by a conventional agitator at a speed of 500 rpm for 15 minutes, thereby forming coating composition samples ( “paint samples” ) . The obtained coating composition samples each had weight solids of 53%.
[0081] The obtained coating composition samples were characterized for heel scuff resistance, coin scuff resistance, and gloss properties according to the test methods described below:
[0082] Heel Scuff Resistance Test
[0083] Paint drawdown was performed on a black vinyl chart by using a 175 μm film caster. Paint drawdown was then air-dried horizontally for 7 days in a Constant Temperature Room (CTR) (25 ℃, 50%relative humidity (RH) ) . A heel (HG / T 3082-2022 Rubber Soles) was used to rub the obtained paint surface by hand one time. The color change, denoted as “ΔE (heel scuff resistance) ” , were measured by BYK Gardner Color-guide sphere spectrophotometer on paint surface before and after rubbing. The smaller color change represented better heel scuff resistance. The objective of the present invention is to achieve a ΔE (heel scuff resistance) of 0.8 or less for good heel scuff resistance.
[0084] Coin Scuff Resistance Test
[0085] Paint drawdown was performed on a black vinyl chart by using a 175 μm film caster. Paint drawdown was then air-dried horizontally for 7 days in a CTR (25 ℃, 50%RH) . A nickel-plate coin was used to rub the obtained paint surface by hand one time. The color change, denoted as “ΔE (coin scuff resistance) ” , were measured by BYK Gardner Color-guide sphere spectrophotometer on paint surface before and after rubbing. The smaller color change represented better coin scuff resistance. The objective of the present invention is to achieve a ΔE (coin scuff resistance) of 0.5 or less for good coin scuff resistance.
[0086] 60° Gloss Test
[0087] Paint drawdown was performed on a black vinyl chart by using a 100 μm film caster. Paint drawdown was then air-dried horizontally for one day in a CTR (25 ℃, 50%RH) . The 60° gloss of the obtained paint film was measured using MICRO-TRI Gloss meter. The objective of the present invention is to achieve a 60° Gloss of 10 or less.
[0088] The characterization results of the coating properties are given in Table 3. As shown in Table 3, all IEs 1-7 samples of the present invention meet the requirements of excellent heel scruff resistance as indicated by ΔE (heel scuff resistance) ≤ 0.8, excellent coin scruff resistance as indicated by ΔE (coin scuff resistance) ≤ 0.5, and 60° gloss ≤ 10 simultaneously.
[0089] In contrast, CEs 1-7 samples failed at least one or more than one of the requirements of heel scuff resistance, coin scuff resistance, and 60° gloss. CE-1 sample that does not contain the specified silica particles (C) and polysiloxane particles (D) failed to meet both requirements for heel and coin scuff resistance. CE-2 sample that does not contain the specified polymeric organic crosslinked microspheres (B) and polysiloxane particles (D) failed to provide acceptable heel scuff resistance. CE-3 sample that does not contain the specified polymeric organic crosslinked microspheres (B) and silica particles (C) , even with a high amount of the specified polysiloxane particles (D) (5.6%) , still failed to meet the requirements for ΔE (coin scuff resistance) and gloss. CE-4 sample that does not contain the specified silica particles (C) failed to achieve ΔE targets for both heel scuff resistance and coin scuff resistance. CE-5 sample that does not contain the specified polysiloxane particles (D) provided ΔE (heel scuff resistance) too high to meet the requirement. CE-6 sample that comprises TS-100 silica with a large BET surface area replacing the specified silica particles (C) provided too high ΔE (coin scuff resistance) , indicating poor coin scuff resistance. CE-7 sample that contains excessive DP-0115 (10%) showed undesirably high ΔE (heel scuff resistance) , thus demonstrating poor heel scuff resistance.
[0090] Table 3 *Percent values are by dry weight based on the wet weight of the coating composition
Claims
1.A coating composition comprising, by dry weight based on the weight of coating composition, an aqueous dispersion of:(A) from 9.6%to 24%of polymer particles having a Z-average particle size in a range of from 80 nm to 500 nm;(B) from 1%to 6.5%of polymeric organic crosslinked microspheres having a median weight average particle size in a range of from 1 μm to 40 μm;(C) from 2%to less than 10%of silica particles having a D50 particle size in a range of from 5 μm to 30 μm and having a BET surface area less than 50 m2 / g; and(D) from 0.24%to 4.4%ofpolysiloxane particles having a D50 particle size in a range of from 1 μm to 20 μm.2.The coating composition of claim 1, wherein the silica particles have an average aspect ratio in a range of from 1.0 to less than 2.3.The coating composition of claim 1 or 2, wherein the silica particles have a D50 particle size in a range of greater than 10 μm to 20 μm.4.The coating composition of any one of claims 1-3, wherein the polysiloxane is a linear polymer represented by the following structure: wherein each R1 is independently C1-C30 alkyl, O-C1-C6-alkyl, or H, provided that at least one R1 is C1-C30-alkyl; each R2 is independently C1-C30-alkyl, H, or Si (R3) 3, wherein each R3 is independently C1-C6-alkyl; and n is in a range of from 1000 to 11000.5.The coating composition of any one of claims 1-4, comprising, by dry weight based on the weight of the coating composition, from 9.6%to 24%of the polymer particles (A) ; from 1.3%to 4.4%of the polymeric organic crosslinked microspheres (B) , from 2.9%to 6%of the silica particles (C) , and from 0.4%to 2.4%of the polysiloxane particles (D) .6.The coating composition of any one of claims 1-5, wherein the polymer particles (A) are acrylic polymer particles having a glass transition temperature in a range of 10 to 35 ℃, as measured by differential scanning calorimetry.7.The coating composition of any one of claims 1-6, wherein the polymeric organic crosslinked microspheres (B) comprise a first stage crosslinked polymer having a glass transition temperature ≤ 20 ℃ and a second stage polymer having a glass transition temperature ≥ 30 ℃, as calculated by the Fox equation; and the median weight average particle size is in a range of from 2 μm to 15 μm.8.The coating composition of any one of claims 1-7, wherein the coating formed by the coating composition demonstrates heel scuff resistance as indicated by a heel scuff color change of 0.8 or less and good coin scuff resistance as indicated by a coin scuff color change of 0.5 or less, and has a 60° gloss of 10 or less.9.A method of providing a coating, comprising the steps of:a) applying the coating composition of any one of claims 1-8 to a substrate; andb) drying, or allowing to dry, the applied coating composition.