Method for producing a dry-processed electrode
The cryogenic mixing process addresses the challenge of achieving homogeneous distribution and fibrillation in electrode production by using a liquid gas to mix conductive additives and active materials with PTFE binders, resulting in improved electrode performance.
Patent Information
- Application Number
- PCT/EP2026/061533
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-22
- Publication Date
- 2026-11-12
AI Technical Summary
Existing dry mixing processes for electrode production, particularly using polytetrafluoroethylene (PTFE) binders, face challenges in achieving homogeneous distribution of conductive additives and active materials without inducing binder fibrillation, leading to inadequate electrical and mechanical contact.
A cryogenic mixing process using a liquid gas with a boiling point below 273 K ensures homogeneous mixing of conductive additives and active materials with a fibrillable binder, followed by controlled fibrillation to form a stable electrode composite.
This method achieves a homogeneous distribution of conductive additives and active materials within the binder, ensuring good electrical conductivity and cohesion with minimal additives, while preserving the fibrillation properties of the binder.
Smart Images

Figure EP2026061533_12112026_PF_FP_ABST
Abstract
Description
[0001] 24-2520
[0002] 1
[0003] Method for producing a dry-processed electrode
[0004] The present disclosure relates to a process for manufacturing a dry-processed electrode.
[0005] Lithium-ion batteries are used in a wide variety of mobile electronic applications. The demand for affordable and long-lasting energy storage devices is high. Electromobility, in particular, is significantly driven by battery technology, which depends on the ongoing development of battery cell chemistry. Solvent-free electrode manufacturing, also known as "dry coating," promises cost and energy reductions compared to the conventional "wet coating" process. For solvent-free dry coatings, a polytetrafluoroethylene (PTFE) binder is primarily used. One possible method is described, for example, in WO2023179969A1 or US2013157141A1.
[0006] US2013157141A1 describes a solvent-free manufacturing process for an electrode, in particular the electrode is manufactured from recycled particles, such as carbon and binders, without using solvents or other additives.
[0007] To achieve good electrical conductivity of the electrodes with a minimal amount of conductive additive and to ensure sufficient coating cohesion and adhesion, a binder-conductive additive matrix that is as homogeneous as possible is crucial. Since the PTFE used is already fibrillated by the shear and temperature introduced during conventional dry mixing processes, premixing the conductive additive with the binder without fibrillating the binder is not possible. An active material cannot be introduced into a fibrillated binder-conductive additive matrix without at least partially destroying the binder fibrils. Insufficient mixing of the active material into the binder-conductive additive matrix would result in inadequate electrical and mechanical contact of the electrode.
[0008] Furthermore, dry cold milling, where the mixing vessel is only cooled externally, can lead to damage, fragmentation, or premature fibrillation of the binder, which can negatively affect the fibrillation properties. Such fragmentation and damage of PTFE was described by Lee et al. in Energy & Environmental Science, Issue 5, 2023, “High-areal-capacity and long-cycle-life all-solid-state battery enabled by freeze drying technology”.
[0009] In light of this prior art, one objective of the present disclosure is to specify a method which is suitable in each case to advance the prior art.24-2520
[0010] 2
[0011] to enrich and at least improve the aforementioned aspects of the prior art. In particular, the purpose of the disclosure is to provide a process for producing a dry-processed electrode with a homogeneous mixture of the conductive additive and the active material in the binder.
[0012] The problem is solved by the features of the independent claims. The dependent claims contain further developments of the disclosure.
[0013] The problem is then solved, according to one aspect of the disclosure, by a method for producing a dry-processed electrode. The method comprises:
[0014] - Mixing a conductive additive and a fibrillable binder in a liquid gas to produce a cryogenic mixture;
[0015] - Mixing an active material into the cryogenic mixture;
[0016] - Fibrillation of the binder to produce an electrode composite;
[0017] - Coating a substrate with the electrode composite to produce an electrode.
[0018] Surprisingly, it has been shown that a cryogenic mixing step in a liquid gas, such as liquid nitrogen, ensures homogeneous mixing of the fibrillable binder and the conductive additive without inducing fibrillation of the binder. A cryogenic mixing step describes a mixing step in a liquid gas that is inert and has a boiling point and / or a supercritical point below 273 K. Furthermore, mixing in a liquid gas does not cause damage, reactions, or comminution of the binder, and its fibrillating properties are preserved.
[0019] A non-fibrillated binder-conducting additive matrix is prepared in which the conducting additive is homogeneously distributed within the binder. This homogeneous mixture is then added to the active material. Fibrillation of the binder is only induced when the conducting additive, homogeneously distributed within the binder, is mixed into the active material. Fibrillation of the binder can be induced by mixing the active material with the conducting additive-binder matrix. Alternatively, a homogeneous mixture of the active material with the conducting additive-binder matrix can be achieved first, particularly in a liquid gas and at low temperatures. Subsequent fibrillation can then be induced by increasing the temperature and removing the liquid gas from the mixture.
[0020] The liquid gas can be removed before or after the active material is added. Likewise, some of the liquid gas can be removed before 24-2520.
[0021] 3
[0022] Mixing with the active material and complete removal of the liquid gas takes place after homogeneous distribution of the active material in the conductive additive-binder matrix.
[0023] The disclosed method offers the possibility of optimizing the steps for the homogeneous distribution of the conductive additive, used in small quantities, within the binder, while simultaneously ensuring the homogeneous distribution of the active material within the binder structure. An electrode with a homogeneous distribution of components such as the active material or the conductive additive within the binder is particularly efficient.
[0024] Mixing the active material with the binder-conductive additive matrix and fibrillating the binder produces an electrode composite that can be further processed using known methods. In particular, a carrier film is coated with the electrode composite to produce an electrode. Good electrical conductivity of the electrode with a minimal conductive additive content can be achieved, and sufficient coating cohesion and adhesion can be ensured by the disclosed method.
[0025] According to one embodiment, the method further comprises:
[0026] - Removal of the liquid gas from the cryogenic mixture to produce a binder-conducting additive matrix.
[0027] After removing the liquid gas from the cryogenic mixture, a powdered binder-conducting additive matrix remains, in which the binder exists as particles and has not yet been fibrillated. This powdered, non-fibrillated binder-conducting additive matrix is stable and can be easily processed further for electrode manufacturing. This has the advantage that the production of the binder-conducting additive matrix can be carried out separately from electrode manufacturing. The binder-conducting additive matrix can then be added to the active material. Fibrillation of the binder is only induced once the conducting additive is homogeneously distributed and mixed into the active material.
[0028] According to one embodiment, the method further comprises:
[0029] - Adding a leading additive and a binder to a chilled mixing vessel;
[0030] - Condensation of a liquid gas into the conductive additive and the binder.
[0031] The solid components of the cryogenic mixtures can be placed in a stirred vessel that can be cooled. In particular, an overpressure can be created in the stirred vessel. The liquid gas can be introduced into the stirred vessel and condenses into its liquid form within it. Specifically, by applying a pressure above the critical point of the liquid gas, the liquid gas can be brought into a supercritical state.24-2520
[0032] 4
[0033] According to one embodiment, the liquid gas is in a supercritical state.
[0034] A supercritical state of the gas is reached when the gas is heated and compressed beyond its critical temperature and pressure. In this state, the gas exhibits properties of both liquids and gases. It has a high density like a liquid, a low dynamic viscosity, and a high diffusion coefficient like gases. These properties make supercritical gases effective solvents, as they are capable of dissolving a wide variety of substances. Using the liquid gas in its supercritical state in the disclosed process offers the advantage that the gas removal takes place under reduced pressure to atmospheric pressure.
[0035] According to one embodiment, the liquid gas is liquid nitrogen or liquid carbon dioxide.
[0036] Carbon dioxide and nitrogen, in their liquid form, are cost-effective solvents used in the disclosed process. Liquid nitrogen, in particular, is climate-neutral.
[0037] According to one embodiment, the binder is PTFE. The disclosed method is particularly advantageous when using PTFE. PTFE is resistant to many chemicals, making it advantageous for electrode applications. Under the influence of shear forces and heat, which are already introduced in conventional dry mixing processes, it forms fibrils that are beneficial for electrode stability. The disclosed method enables a dry mixing process without inducing fibrillation of the PTFE binder. This allows mixing processes for the production of electrode composites to be optimized in order to obtain a homogeneous distribution of the components in an electrode, which improves the electrode's performance.
[0038] According to one embodiment, the conductive additive is carbon nanotubes. Carbon nanotubes (CNTs) are very difficult to process in powder form during mixing. Extremely strict occupational safety measures are required because carbon nanotubes, as nanofibers, can become lodged in the lungs and never degrade in the body. The disclosed method binds these carbon nanotubes with the binder, particularly in a conductive additive-binder matrix, ensuring safe handling during dosing and mixing without the release of carbon nanotube dust. The carbon nanotube-binder matrix can be advantageously further processed for electrode manufacturing and homogenized in an active material.24-2520
[0039] 5
[0040] According to one embodiment, the conductive additive and the fibrillable binder and / or the active material are mixed at a temperature of less than 10°C. The mixing temperature can be kept so low by using liquid gas that the binder does not fibrillate. In particular, the temperature can also be kept low at points where energy is introduced, such as at the agitators. This is not possible when the mixing vessel is heated solely from the outside.
[0041] According to one embodiment, the conductive additive and the fibrillable binder and / or the active material are mixed at a temperature between -10°C and 5°C. The active material can become brittle at very low temperatures. In particular, when mixing the active material into the conductive additive-binder matrix, a temperature must be selected that does not impair the quality of the active material.
[0042] According to one embodiment, the liquid gas is removed by raising the temperature above the boiling point of the liquid gas and / or lowering the pressure below the critical point of the liquid gas.
[0043] The liquid gas can be easily removed by increasing the temperature. The conductive additive-binder matrix and / or the mixture of active material and conductive additive-binder matrix remain fluffy and easily processable.
[0044] The liquid gas can also be removed by lowering the pressure. This allows for the removal of the liquid gas when increasing the temperature is not suitable, especially if the binder is already prone to fibrillation at moderate temperatures.
[0045] Similarly, the temperature can be increased and the pressure decreased simultaneously to remove the liquid gas from the mixture.
[0046] The liquid gas can be removed from the cryogenic mixture after mixing the conductive additive and binder to create a conductive additive-binder matrix. The liquid gas can also be removed after or during mixing the active material with the cryogenic mixture. Alternatively, the liquid gas can be removed during fibrillation.
[0047] One embodiment of each is described below with reference to the figures.
[0048] Fig. 1 schematically shows a flowchart of a process according to one aspect of the disclosure;
[0049] Fig. 2 schematically shows a flowchart of a method according to one embodiment; and24-2520
[0050] 6
[0051] Fig. 3 shows a schematic representation of a method according to a further embodiment.
[0052] In the figures, identical or corresponding elements are marked with the same reference symbols.
[0053] Figure 1 schematically shows a flowchart of a process 100 according to one aspect of the disclosure. The process 100 according to Figure 2 is a process 100 for producing a dry-processed electrode. In step 105, a conductive additive and a fibrillable binder are mixed in a liquid gas, and a cryogenic mixture is produced. In the cryogenic mixture, the conductive additive is homogeneously distributed in the binder. An active material is added to the cryogenic mixture and mixed (see step 110) so that the conductive additive, binder, and active material are homogeneously mixed together. In step 115, the binder is fibrillated. During fibrillation 115, the polymer fibers of the binder are broken down into very fine, fibrous structures. This occurs, for example, through mechanical treatment by the stirrer while increasing the temperature, which also causes the liquid gas to escape from the mixture.An electrode composite is created, which is coated onto a substrate, for example a current collector, to produce an electrode (see step 120).
[0054] Figure 2 schematically shows a flowchart of a process 100a according to one embodiment. In step 105, a conductive additive and a fibrillable binder are mixed in a liquid gas to produce a cryogenic mixture. In step 125, the liquid gas is removed from the cryogenic mixture by increasing the temperature and / or decreasing the pressure. This yields a powdered binder-conductive additive matrix in which the binder is present as particles and has not yet been fibrillated. The binder-conductive additive matrix is stable and can be added to an active material for further processing.
[0055] Figure 3 shows a schematic representation of a method 100b according to a further embodiment. In step 130, a conducting additive and a binder are placed in a cooled stirred vessel. A liquid gas is condensed into the stirred vessel containing the conducting additive and the binder (see step 135). In particular, the stirred vessel is cooled. Alternatively or additionally, pressure can be built up in the stirred vessel to bring the liquid gas to a supercritical state. In step 105, a conducting additive and a fibrillable binder are mixed in a liquid gas, and a cryogenic mixture is produced. In the cryogenic mixture, the conducting additive is homogeneously distributed in the binder. An active material is added to the cryogenic mixture and mixed (see step 110) so that the conducting additive and binder are 24-2520.
[0056] 7
[0057] and active material are homogeneously mixed together. In step 115, the binder is fibrillated. During fibrillation 115, the polymer fibers of the binder are broken down into very fine, fibrous structures. This occurs, for example, through mechanical treatment by the stirrer at an increased temperature. An electrode composite is created, which is then coated onto a substrate, such as a current collector, to produce an electrode (see step 120).
[0058] The person skilled in the art recognizes that the process 100 and process 100b according to Figure 1 and Figure 3 can also be carried out in a different order than the one shown.
[0059] In particular, it is possible that steps of procedure 100 or 100b can be swapped, postponed, repeated and / or performed simultaneously.24-2520
[0060] 8
[0061] Reference symbol (part of the description)
[0062] 100, 100a, 100b procedures
[0063] 105 Mixing a conductive additive and a fibrillable binder 110 Mixing an active material
[0064] 115 Fibrillation
[0065] 120 coatings
[0066] 125 Removing the liquid gas
[0067] 130 Present
[0068] 135 Condensation
Claims
24-2520 9 Claims 1. Method (100) for producing a dry-processed electrode, wherein the method (100) comprises: - Mixing (105) a leading additive and a fibrillable binder in a liquid gas to produce a cryogenic mixture; - Mixing (110) an active material into the cryogenic mixture; - Fibrillation (115) of the binder to produce an electrode composite; - Coating (120) a carrier with the electrode composite to produce an electrode.
2. Method (100) according to claim 1, wherein the method (100) further comprises: - Removal (125) of the liquid gas from the cryogenic mixture to produce a binder-conducting additive matrix.
3. Method (100) according to claims 1 and 2, wherein the method (100) further comprises: - Place (130) a leading additive and a binder into a cooled stirring vessel; - Condensing (135) a liquid gas into the conducting additive and the binder.
4. Method (100) according to any of the preceding claims, wherein the liquid gas is in a supercritical state.
5. Method (100) according to any one of the preceding claims, wherein the liquid gas is liquid nitrogen or liquid carbon dioxide.
6. Method (100) according to any one of the preceding claims, wherein the binder is PTFE.
7. Method (100) according to any one of the preceding claims, wherein the leading additive is carbon nanotubes.
8. Method (100) according to any one of the preceding claims, wherein the conductive additive and the fibrillable binder and / or the active material are mixed at a temperature of less than 10°C. 24-2520 10 9. Method (100) according to claim 8, wherein the conductive additive and the fibrillable binder and / or the active material are mixed at a temperature between -10°C and 5°C.
10. Method (100) according to any of the preceding claims, wherein the liquid gas is removed by raising the temperature above the boiling point of the liquid gas and / or lowering the pressure below the critical point of the liquid gas.