Method for producing a coke cake
The method addresses the scarcity of high-quality bituminous coal by using non-bituminous coal and coking aids to form stable coke cakes through comminution and mixing, enhancing coking capacity and reducing costs.
Patent Information
- Application Number
- PCT/EP2026/062185
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-12
AI Technical Summary
The increasing scarcity and high cost of high-quality bituminous coal, coupled with the inefficiency of mixing non-bituminous coal in coke production, result in unstable coke products and elevated operating costs, necessitating new processes to utilize a broader range of coal types for stable coke production.
A method involving the comminution of non-bituminous coal and bituminous coal to specific particle sizes, mixing with petroleum-independent coking aids, and using a stamping process to produce a feedstock for coking, which forms adhesive fusion bridges during pyrolysis, enhancing the coking capacity of non-bituminous coals.
Enables the production of stable coke cakes using a higher proportion of non-bituminous coal, improving the efficiency and reducing production costs by utilizing a broader range of coal types, including biochars and biomass, with coking aids forming adhesive bridges during coking.
Smart Images

Figure EP2026062185_12112026_PF_FP_ABST
Abstract
Description
[0001] Method for producing a coke cake
[0002] The present invention relates to a method for producing a coke cake according to claim 1.
[0003] Coke is an indispensable raw material for every economy, requiring a high level of supply security and a stable price. Lump coke is particularly important in this regard. In its coarsest form, it is used primarily in the metallurgical industry, but even in finer grains, it can find applications, for example, as an adsorbent in gas and water purification or as a soil amendment. Fine-grained coke or coke dust is also increasingly used, for instance, as an energy carrier or as a reducing agent.
[0004] Coke cakes are produced in coke ovens from coking coal mixtures with high baking capacity. These coke ovens, combined into coke oven batteries, consist longitudinally of up to 90 interconnected oven chambers, each framed on both sides by a brick wall. Transversely, these walls are composed of up to 42 individual, interconnected hollow channels in which the heat required to heat the chambers is generated by combustion processes. In the oven chambers, which are filled from the top by free fall (pounding operation) or from the side (tamping operation), a coal mixture is heated from ambient temperature to a target temperature of up to 1150°C and thus transformed into coke.
[0005] A coke cake represents the complete batch of coke in an oven chamber after pyrolysis. A coke cake is approximately 10 to 20 meters long, 0.4 to 0.6 meters wide, and 4 to 7 meters high.
[0006] Lump coke is the product after coking and quenching on the ramp outside the oven. The coke cake inside the oven forms from the coal cake through pyrolysis and is also called a coke charge. As it falls out of the oven chamber, the coke cake breaks down into thousands of individual coke lumps. The feed mixture (pressed or rammed) that is filled into the oven from the raw materials (coal or biomass) and the additives / binders is called a coal cake or coal charge.
[0007] Due to their high baking properties, so-called "bituminous coals" are preferably used as raw material for coking in coke ovens. The following are characteristics that a bituminous coal must fully possess in order to be classified as such:
[0008] Volatile components, measured in the water- and ash-free substance: 19 - 28% by mass
[0009] Carbon content, measured in the water- and ash-free substance: 86 - 89% by mass
[0010] Hydrogen content, measured in the water- and ash-free substance: 5.0 - 5.5 wt%
[0011] Oxygen content, measured in the water- and ash-free substance: 3.5 - 4.5% by mass
[0012] Water content in the raw material: 2 - 4% by mass
[0013] Bloating number (according to DIN 5174): 4.5 - 9.0
[0014] Baking ability number (according to ROGA, ISO 15585:2019): >45
[0015] Average vitrinite reflectance under oil (according to DIN 22020 / 5): 1.2 - 1.6%
[0016] Maximum fluidity measured in the GIESELER plastometer test device (according to ASTM D 2639-74): 50 - 1000 ddpm
[0017] Energy content: 35,000 - 36,000 kJ / kg
[0018] All types of coal that do not exhibit at least one of these characteristics, i.e., that lie outside one of the above-mentioned limit ranges, are considered "non-bituminous coals".
[0019] These coal types ensure a stable coke cake after pyrolysis, as required, for example, as a feedstock in the downstream blast furnace during iron production. For metallurgical applications, the coke cake should exhibit not only high mechanical strength but also low reactivity and high thermal stability.
[0020] Coal types with differing levels of the listed characteristics are distinguished by reduced or completely absent baking properties and thus coking potential. During coking of these types, these components often disintegrate in the furnace and do not form a mechanically stable coke structure, rendering the coke unusable for industrial purposes.
[0021] Due to the increasing global demand for bituminous coal, particularly from emerging economies like China and India, the availability of high-quality bituminous coal, which constitutes the main feedstock in a coke oven battery, has become increasingly scarce over the last two decades, leading to a sharp rise in prices. This shortage of high-quality bituminous coal is currently resulting in higher costs for the feedstock mix used in coking plants, and consequently, higher operating costs. Furthermore, the uneven distribution of global coking coal resources leads to significantly higher transportation costs.
[0022] At the same time, there is an increasing availability worldwide of inexpensive "non-bituminous coals". However, these non-bituminous coals are characterized by weaker or non-existent baking properties.
[0023] To ensure economical and competitive coke production, many countries and coke producers are increasingly seeking alternative processes for producing high-quality coke from the remaining available low- and non-abrasive coking feedstocks. In actual plant operation, these inexpensive grades, i.e., the non-bituminous coals, are often mixed with the high-quality bituminous coals without further processing to reduce operating costs. However, this method reaches its limits in terms of process engineering, as even small proportions of non-abrasive components reduce the coking capacity of the mixture, resulting in an unstable coke product after pyrolysis.
[0024] To further increase the proportion of weak or non-baking coals in the production of lump coke, lump coke for metallurgical purposes is also produced in the established stamping process, which is based on compacting the raw material components before pyrolysis.
[0025] After compaction, the crushed coal is inserted laterally into the hot oven chambers and pyrolyzed to produce coke. Using this method, significantly larger proportions of low-grade, non-coking coals, i.e., non-bituminous coals, can be used than in bulk operation.
[0026] The addition of binders in the ambient state is also known and can lead to a significant improvement in coke quality. Small quantities of oil residues from the petroleum industry or shredded used tires are often used for this purpose. However, these methods also have their limitations, as each raw material requires individual, application- and raw material-specific pretreatment to be mechanically and thermally stable as coke after pyrolysis. For example, the addition of binders is linked to precise ratios of quantity, moisture content, and viscosity, as well as local availability. Generally applicable application limits for non-clogging raw material mixtures are not known for the stamping process and must therefore be developed individually.
[0027] In order to produce mechanically and thermally stable coke cakes or lump cokes from non-coking raw materials such as non-coking hard coal, lignite or biomass, new processes and plants are needed to produce a usable feedstock for coking.
[0028] The object of the present invention is now to propose a method for producing a coke cake in which a maximum proportion of actually unsuitable coal, i.e. non-bituminous coal, and a minimum proportion of bituminous coal can be used as starting material to produce a sufficiently stable coke cake.
[0029] According to the invention, this problem is solved by a method with the features of claim 1. The following method steps are provided for this purpose:
[0030] a) Comminution of non-bituminous coal, in particular to a particle size of 0 to 4 mm, preferably of 0 to 1 mm, e.g. by impact and collision;
[0031] b) Crushing of bituminous coal, in particular to a particle size of 0 to 4 mm, preferably of 0 to 1 mm, e.g. by impact and collision;
[0032] c) Mixing the crushed non-bituminous coal and bituminous coal to form a first intermediate product, wherein the proportion of bituminous coal in the first intermediate product is between 40 and 90%, preferably 60%, of the mass of the first intermediate product;
[0033] d) Mixing and heating the first intermediate product with a petroleum-independent coking aid in a mixer with heating, preferably in an intensive mixer, to form a second intermediate product at a temperature between 15 °C and 95 °C, preferably between 50 °C and 80 °C, wherein the proportion of the petroleum-independent coking aid in the second intermediate product is between 2% and 30% of the mass of the second intermediate product;
[0034] e) Feeding the mixed and heated second intermediate product into a stamping machine to produce a feedstock for coking;
[0035] f) Feeding the feedstock for coking into the coke oven to produce a coke cake by coking. The coal is preferably crushed by impact, particularly in a mill with a suitable screen. This screen ensures that the particles are no larger than the specified particle size. However, the resulting particle size range is then, for example, 4 to 0 mm. If a finer screen is selected, the maximum particle size is reduced, for example, to 1 mm. However, the total particle size coming from the mill also contains significantly finer particles. Therefore, the resulting particle size range is then 1 to 0 mm.
[0036] To broaden the range of coal types usable in coking plants, it is particularly proposed to produce coking feedstock (coking cake) from mixtures of low-coking, non-coking, and coking coals. Specifically, biochars and biomass of primarily biogenic origin, but with petroleum-independent coking aids, should be added. These aids do not primarily act as binders in the uncoked state of the raw material or during the production of, for example, a compacted mixture, but rather exert their effect only during coking at temperatures above 150 °C, by forming, in particular, adhesive fusion bridges between the feedstocks and especially the mixture components.
[0037] This process makes it possible to convert increased proportions of weakly and non-coking raw materials, such as lean / EB / gas / flame / gas-flame coal and mixtures of coal, biochar, and / or biomass, into solid, lumpy coke or coke cake. For this purpose, the input materials are first crushed to a high degree of fineness, preferably particle sizes below 4 mm and above 1 mm, e.g., by impact grinding, and then mixed together. Subsequently, the coking aid can be added to the first intermediate product in proportions of 2% to 30% by mass, either individually or as a mixture.
[0038] Further advantageous embodiments of the proposed invention arise in particular from the features of the dependent claims. The subject matter or features of the various claims can, in principle, be combined with one another in any way.
[0039] In an advantageous embodiment of the invention, the bituminous charcoal may be characterized by the following features:
[0040] Volatile components, measured in the water- and ash-free substance: 19–28% by mass. Carbon content, measured in the water- and ash-free substance: 86–89% by mass.
[0041] Hydrogen content, measured in the water- and ash-free substance: 5.0 - 5.5 wt%
[0042] Oxygen content, measured in the water- and ash-free substance: 3.5 - 4.5% by mass
[0043] Water content in the raw material: 2 - 4% by mass
[0044] Bloating number (according to DIN 5174): 4.5 - 9.0
[0045] Baking ability number (according to ROGA, ISO 15585:2019): >45
[0046] Average vitrinite reflectance under oil (according to DIN 22020 / 5): 1.2 - 1.6%
[0047] Maximum fluidity measured in the GIESELER plastometer test device (according to ASTM D 2639-74): 50 - 1000 ddpm
[0048] Energy content: 35,000 - 36,000 kJ / kg.
[0049] Conversely, it is stipulated that non-bituminous coal is characterized by the fact that at least one of the above-mentioned characteristics is not fulfilled.
[0050] In a further advantageous embodiment of the invention, it can be provided that the non-fatty coal consists of weakly and non-abrasive raw materials such as lean / EB / gas / flame-ZGasflamm coals and mixtures of coals, biochar and / or biomass.
[0051] In a further advantageous embodiment of the invention, it can be provided that
[0052] Lye from the pulp industry, such as sulfite and sulfate lye
[0053] processed lignins in solid (powder, granules) or liquid form of varying viscosity and dilution,
[0054] Molasses as a by-product of sugar production from sugar beets and sugar cane in varying viscosities and dilutions,
[0055] bamboo or birch fibers,
[0056] Rapeseed or soybean extraction meal,
[0057] Porridges made from palm oil or lentil shells,
[0058] Spent grain from brewing is primarily a residue from the leached malt, and / or
[0059] Pomace from seeds (e.g., grapes) is used as a press residue in oil, wine, and juice production, either alone or in mixtures, as a coking aid. Such raw materials are sometimes inexpensive and available in sufficient quantities.
[0060] In a further advantageous embodiment of the invention, it can be provided that the petroleum-independent coking aids are arranged not to act as binders in the uncoked state of the feedstock, but to exert their effect only during coking in the temperature range above 150 °C, in particular by forming adhesive melt bridges in the feedstock.
[0061] In a further advantageous embodiment of the invention, it can be provided that a binder is added to the first intermediate product before, during or after the addition of the coking aid.
[0062] In a further advantageous embodiment of the invention, the coking aids can be added in uncoked or already coked form, in granular or fibrous form. Depending on the mechanism of action of the coking aid, it can be added uncoked or coked. For example, if fiber reinforcement is intended to contribute to an additional increase in strength, (partially) coked fibrous materials could also be used as coking aids.
[0063] In a further advantageous embodiment of the invention, it can be provided that coal anthracites are additionally added to the first intermediate product, in particular the coal mixture, in proportions of up to 5% by mass.
[0064] The addition of anthracite coal is considered a novelty because it is also a non-coking component, but its high carbon content allows it to be used as a carburizing agent. This means that when non-coking components, which are typically less carbonized than bituminous coals (e.g., gas flame coals), are used, they usually also have higher levels of volatile components, which in turn results in higher reactivity. The addition of anthracite coal is intended to counteract this. Furthermore, the ash content and, if applicable, the nitrogen and sulfur emissions during coking can also be reduced. In principle, no additional adjustment of the mixture is necessary. However, it is important to ensure that the proportion of the coking aid is not reduced when adding anthracite.As an example, consider the production of a mixture of non-coking coal (e.g., gas flame coal) and 10 wt.% coking aid. If 5 wt.% anthracite is now to be added, the mass of coking aid remains unchanged, and 5 wt.% of the gas flame coal is replaced by anthracite.
[0065] In a further advantageous embodiment of the invention, the mixing of the first intermediate product with a petroleum-independent coking aid to form a second intermediate product can be carried out in a heated intensive mixer with high energy input. The high energy input is achieved through the high relative speed of the mixing tool compared to the mixing vessel and the high peripheral speed of the mixing tool itself. This ensures high mixing quality with optimal homogeneity of the mixture. Providing performance data is not useful, as this depends on the size of the mixer.
[0066] In a further advantageous embodiment of the invention, the mixing of the first intermediate product with a petroleum-independent coking aid to form a second intermediate product can be carried out at mixing temperatures of 60 °C to 100 °C, preferably at 80 °C, when using lignin-containing coking aids. Lignin softening depends on the moisture content of the material and the pressure. Softening typically only occurs at temperatures above 100 °C. By applying pressure, this lignin softening can partially occur at a lower temperature. This initially forms liquid bridges between solid particles. Upon cooling, these harden into solid bridges.
[0067] In a further advantageous embodiment of the invention, the mixing of the first intermediate product with a petroleum-independent coking aid to form a second intermediate product can be carried out at mixing temperatures of 40 °C to 60 °C, particularly at 50 °C, when using protein-containing coking aids. Through denaturation of the proteins in the specified temperature range, they bind together and solidify the carbon substance; during coking, they form molten coke. This is also an example of a simultaneous action as a binding and coking aid.
[0068] In a further advantageous embodiment of the invention, the mixing of the first intermediate product with a petroleum-independent coking aid can take place over a period of between 2 and 10 minutes. A longer mixing time usually results in more homogeneous mixing. However, at this point, it seems more appropriate to aim for a certain mixing quality, since the mixing time can also depend on the quantity. Mixing quality refers to the homogeneity of a mixture. That is, in a defined "control volume element" of the mixture, the actual distribution of the mixture components should correspond as closely as possible to the target composition. For example, a deviation of 5% might be acceptable, meaning the mixing quality should be 95%.
[0069] In a further advantageous embodiment of the invention, the mixer, in particular the intensive mixer, can be equipped with a heating unit, especially an infrared hot air or induction heater. The advantage of heating the mixer by one of the aforementioned methods is twofold: firstly, it leads to the plasticization of the material, and secondly, it can promote the effects of lignin softening or protein denaturation. With liquid coking aids, the viscosity is advantageously reduced and the wetting behavior is positively influenced. Otherwise, separate preheating of the mixture is advisable.
[0070] In a further advantageous embodiment of the invention, the mixer, in particular the intensive mixer, can be equipped with a moisture sensor, dosing devices, storage containers, and / or an electromagnetic scale. The aforementioned devices allow integration into an automated manufacturing process. Furthermore, the preferred parameters can be easily measured and adjusted accordingly.
[0071] In a further advantageous embodiment of the invention, the coking agent can be supplied as a grinding slurry, the grinding slurry being processed in perforated disc mills, (twin-screw) extruders, or in a vibratory mill with grinding media, preferably with the addition of water in solid-liquid ratios of 1:1, 1:2, and 1:3. The production of grinding slurries from coking agents can prove advantageous because it allows for a mechano-chemical breakdown that leads to a more intensively effective form of the binding and coking agent. For example, protein-containing substances such as soybean meal can be mixed with water in the specified mass ratios. In this way, the protein is denatured during processing in a vibratory mill or the other specified machines.Furthermore, cell disruption can partially lead to the release and activation of the binding and coking aids, resulting in a better, more homogeneous distribution in the mixture. When the resulting milled slurries are mixed with the coal, they already act as binding agents, and their effect as coking aids is also intensified because they can come into better contact with the coal. In a further advantageous embodiment of the invention, it can be provided that the previous mixing temperature is maintained when the second intermediate product is tamped in the tamping machine.
[0072] In a further advantageous embodiment of the invention, it can be provided that the tamping pressure of the second intermediate product in the tamping machine is between 5 and 50 MPa, preferably between 20 and 30 MPa. Coals with caking properties form a fused coke when the temperature is increased under anaerobic conditions during coking in bulk operation. If, instead, weakly or non-caking coals are used, this does not occur during coking or only to a limited (insufficient) extent. By tamping the coal or a coal-coking agent mixture, the coal particles are brought closer together, and partial fusion bridges can still form between the particles when using weakly caking coals. The introduced coking agent can thus also exert its effect as a fused coke former at the grain boundaries. In addition, a shrinkage of the coke occurs as a result of the volume loss.Depending on the type of coal or coal mixture, a specific tamping pressure is optimal or sufficient. Generally, a higher tamping pressure leads to greater compaction, which ideally results in a denser coke.
[0073] In a further advantageous embodiment of the invention, it can be provided that when stamping the second intermediate product in the stamping machine, the stamping time does not exceed 5 min and is preferably 30 s to 3 min.
[0074] In a further advantageous embodiment of the invention, it can be provided that when stamping the second intermediate product in the stamping machine, the density of the feedstock for coking (stamp cake density) exceeds 1000 kg / m³. 3 achieved in a dry state. By ensuring a rammed cake density of > 1000 kg / m³. 3 This also ensures a sufficient bulk density of coke.
[0075] In a further advantageous embodiment of the invention, the feedstock for coking in the coke oven can be heated non-linearly, with at least two coupled coking rates with different temperature increases. The purpose of combining different heating rates is to achieve the most advantageous formation of lump coke. If, for example, low-carbon coals or biomass with a higher content of volatile components are used for coke production, higher quantities of gas are to be expected, which must be expelled from the ram cake. Excessively rapid heating leads to damage to the ram cake or the coke formed from it due to the resulting gas pressure. For this purpose, steady-state ramps can also be integrated into the heating regime. This ensures uniform "cooking through," i.e., that the coke (or the resulting lump coke) is heated evenly.the forming coke) has also reached a certain temperature inside and sufficient time has been given for the structural change (bulk density).
[0076] In a further advantageous embodiment of the invention, it can be provided that, between the at least two coupled coking rates, temperature-related steady-state ramps specific to the raw material and application can also be inserted. Further features and advantages of the present invention will become clear with reference to the following description of preferred embodiments and the accompanying figures. The elements or features of the various embodiments can, in principle, be combined with one another as desired. These show:
[0077] Fig. 1 Example of a multi-stage heating regime.
[0078] The following reference symbols are used in the illustration:
[0079] 1-3 time intervals in the heating regime
[0080] Features and details described in connection with a method naturally also apply to the device according to the invention, and vice versa, so that the disclosure regarding the individual aspects of the invention always makes or can make reciprocal reference. Furthermore, any described method according to the invention can be carried out with the device according to the invention.
[0081] The terminology used herein serves only to describe certain embodiments and is not intended to limit the disclosure. As used herein, the singular forms "a" and "the" are intended to include the plural forms unless the context otherwise makes clear. It will also be clear that the expressions "indicates" and / or "indicating," when used in this description, specify the presence of the aforementioned features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. As used herein, the expression "and / or" includes any and all combinations of one or more of the associated, listed elements.
[0082] Of particular importance for the following description of the process according to the invention is the definition of "bituminous coal," which is especially well suited for the production of a coke cake. As already explained, the bituminous coal generally required for this purpose is becoming increasingly scarce and / or increasingly expensive. Bituminous coal is characterized by the following parameters, which a bituminous coal must fully possess in order to be designated as such:
[0083] - Volatile components, measured in the water- and ash-free substance: 19 - 28% by mass
[0084] - Carbon content, measured in the water- and ash-free substance: 86 - 89 wt% - Hydrogen content, measured in the water- and ash-free substance: 5.0 - 5.5 wt%
[0085] - Oxygen content, measured in the water- and ash-free substance: 3.5 - 4.5% by mass
[0086] - Water content in the raw substance: 2 - 4% by mass
[0087] - Bloating number (according to DIN 5174): 4.5 - 9.0
[0088] - Baking ability number (according to ROGA, ISO 15585:2019): >45
[0089] - Average vitrinite reflectance under oil (according to DIN 22020 / 5): 1.2 - 1.6%
[0090] - Maximum fluidity measured in the GIESELER plastometer test device (according to ASTM D 2639-74): 50 - 1000 ddpm
[0091] - Energy content: 35,000 - 36,000 kJ / kg
[0092] All types of coal that do not exhibit at least one of these characteristics, i.e., that lie outside one of the above-mentioned limit ranges, are considered "non-bituminous coals".
[0093] Such non-fatty coal has little or no baking ability.
[0094] The proposed method is intended to remedy this by enabling the use of "non-bituminous coal" for the production of a coke cake, or at least by adding a not insignificant proportion of non-bituminous coal, so that a comparable or at least approximately comparable coke cake is produced from bituminous coal and non-bituminous coal, as would have been produced from bituminous coal.
[0095] The method according to the invention will be explained in more detail below. It is understood that only a few selected process steps are presented here, as they are helpful for understanding the method according to the invention. The method may include further steps or intermediate steps known to those skilled in the art.
[0096] According to the invention, the following method is proposed: a) Comminution of non-fatty coal, in particular to a particle size of 0 to 4 mm, preferably of 0 to 1 mm, e.g. by impact and collision;
[0097] b) Crushing of bituminous coal, in particular to a particle size of 0 to 4 mm, preferably of 0 to 1 mm, e.g. by impact and collision;
[0098] c) Mixing the crushed non-bituminous coal and bituminous coal to form a first intermediate product, wherein the proportion of bituminous coal in the first intermediate product is between 40 and 90%, preferably 60%, of the mass of the first intermediate product;
[0099] d) Mixing and heating the first intermediate product with a petroleum-independent coking aid in a mixer with heating, preferably in an intensive mixer, to form a second intermediate product at a temperature between 15°C and 95°C, preferably between 50°C and 80°C, wherein the proportion of the petroleum-independent coking aid in the second intermediate product is between 2% and 30% of the mass of the second intermediate product;
[0100] e) Feeding the mixed and heated second intermediate product into a stamping machine to produce a feedstock for coking;
[0101] f) Introducing the feedstock for coking into the coke oven to produce a coke cake by coking.
[0102] In other words, to broaden the range of coal usable in coking plants, it is proposed to produce feedstock for coking (coking cake) from low-coking coals, as well as mixtures of low-coking, non-coking, and high-coking coals, biochars and biomass with coking aids of primarily biogenic or biogenic origin, but independent of petroleum, which are designed not to act as binders in the uncoked state of the feedstock, but to exert their effect only during coking in the temperature range above 100 °C, in particular by forming adhesive fusion bridges in the feedstock.
[0103] Coking aids are substances or mixtures of substances that significantly or even fundamentally improve the coke-forming capacity of non- and weakly abrasive raw materials. These agents often act as molten coke formers, but can also undergo chemical reactions with the non-abrasive base material before and during coking. The specific mode of action cannot be fully elucidated for all substances. In contrast, a binder, in the form of a matrix-type or film-type binder, acts during agglomeration and is intended to increase the strength of the agglomerate by improving the binding capacity of the system (here, the "feedstock for coking"). This refers to the binding effect in the "low-temperature range." Thus, a coking aid can also act as a binder, or a binder can also act as a coking aid in the subsequent pyrolysis process.
[0104] This process makes it possible to convert increased proportions of weakly and non-coking raw materials, such as lean / EB / gas / flame / gas-flame coal and mixtures of coal, biochar, and / or biomass, into solid, lumpy coke. For this purpose, the feedstocks are first crushed to a high degree of fineness, preferably particle size of 0 to 1 mm, e.g., by impact grinding, and then mixed together. Subsequently, the coking aid can be added to the first intermediate product in proportions of 2% to 30% by mass, either individually or as a mixture.
[0105] The production of high-quality lump coke is even more advantageous under the conditions that
[0106] 1. the raw materials are refined through optimal processing and agglomeration into mash cakes with excellent lump coke formation capacity and
[0107] 2. then gently coked using a raw material- and application-specific heating regime.
[0108] The following additives, either alone or as a mixture, may be considered as examples of coking aids for non- or weakly acrid coal mixtures.
[0109] - Lye from the pulp industry, such as sulfite and sulfate liquor
[0110] - processed lignins in solid (powder, granules) or liquid form of varying viscosity and dilution,
[0111] - Molasses as a by-product of sugar production from sugar beets and sugar cane of varying viscosity,
[0112] - Bamboo or birch fibers,
[0113] - Rapeseed or soybean extraction meal,
[0114] - Porridges made from palm oil or lentil shells,
[0115] - Spent grain primarily as a residue of the leached malt or
[0116] - Pomace from seeds (e.g., grapes) as a press residue during oil, wine, and juice production. In one embodiment of the invention, the coking aid is mixed with a binder and added to the raw material components, and then compacted. However, for certain raw material mixtures, it is advantageous to add the binder before or after the coking aid to the mixture.
[0117] This sequential addition of these agents to the original raw materials can also take place in different particle size distributions or temperature ranges.
[0118] The optimal temperature range in which the binders and / or coking aids can be added to the raw material mixture is between 15 and 95°C, preferably between 50 and 80°C.
[0119] The coking aid, in particular the biomass, can be added, for example, in uncoked or already coked form, in granular or fibrous form.
[0120] For carburization, coal anthracites can be added to the first intermediate product, especially the coal mixture, in proportions of up to 5% by mass. It should be noted that these anthracites themselves possess neither binding nor lump coke-forming properties and can only be converted into lump coke through a suitable process within this raw material mixture.
[0121] The mixing of coal and coking aids preferably takes place in a heated intensive mixer with high energy input within a temperature range of 15°C to 95°C. Higher mixing temperatures of 80°C are preferably chosen for lignin-containing coking aids than for protein-containing coking aids, where a mixing temperature of 50°C is preferable.
[0122] The mixing time is usually between 2 min and 10 min, ensuring that the desired target temperature is reached in the homogeneous mixture.
[0123] Preferably, the raw materials are mixed according to the following procedure:
[0124] 1. Intensive mixing of half of the coal (mixture) with all other solid components. 2. Addition of the liquid mixture components, preferably to the running intensive mixer. The moisture content of the second intermediate product, in particular the coal mixture, should be between 5 and 20 wt%, but preferably 9 to 11 wt%. The second intermediate product may also contain liquid mixture components.
[0125] The intensive mixer is equipped with a heating unit, such as an infrared, hot air, or induction heater, for precisely setting an application-specific temperature regime during the mixing process. It can also be equipped with a moisture sensor, dosing devices, storage containers, or an electromagnetic scale.
[0126] It is preferably provided that the coking aid is supplied as a grinding slurry, wherein the grinding slurry is processed in perforated disc mills, (twin screw) extruders or in a vibrating mill with grinding media, each preferably with the addition of water in solid-liquid ratios of 1:1, 1:2 and 1:3.
[0127] This process denatures and swells the proteins from the extraction meal, spent grain, and pomace. The conversion of polysaccharides is also promoted. Consequently, the coarse particles dispersed in the water are transformed into a pasty mass. The proteins and polysaccharides denatured in this way can be converted into molten coke during the process in the furnace chamber, which leads to increased strength in the developing coke mass.
[0128] After the first intermediate product, in particular the carbon carrier, has been mixed with the coking aids, it is introduced into the stamping machine and the feedstock for coking (stamp cake) is transferred into the furnace chamber.
[0129] During tamping, the mixing temperature should be maintained as much as possible. Tamping pressures should be between 5 and 50 MPa, preferably between 20 and 30 MPa. The tamping time should not exceed 5 minutes and preferably be between 30 seconds and 3 minutes. The resulting tamping cake density is over 1000 kg / m³. 3 (dry).
[0130] The heating regimes for coking should not be linear and should be based on at least two coupled coking rates with different temperature increases. Temperature steady-state ramps, specific to the raw material and application, can also be incorporated between these stages. Figure 1 shows an example of a multi-stage heating regime. Three coupled coking rates with different temperature increases are depicted here, with section 3 representing a steady-state ramp.
[0131] In principle, the invention is not limited to the embodiments outlined above. Rather, variations are conceivable without deviating from the inventive idea.
Claims
Claims 1. A method for producing a coke cake, comprising the following process steps: a) Crushing non-bituminous coal, in particular to a particle size of 0 to 4 mm, preferably of 0 to 1 mm, e.g. by impact and collision; b) Crushing of bituminous coal, in particular to a particle size of 0 to 4 mm, preferably of 0 to 1 mm, e.g. by impact and collision; c) Mixing the crushed non-bituminous coal and bituminous coal to form a first intermediate product, wherein the proportion of bituminous coal in the first intermediate product is between 40 and 90%, preferably 60%, of the mass of the first intermediate product; d) Mixing and heating the first intermediate product with a petroleum-independent coking aid in a mixer with heating, preferably in an intensive mixer, to form a second intermediate product at a temperature between 15°C and 95°C, preferably between 50°C and 80°C, wherein the proportion of the petroleum-independent coking aid in the second intermediate product is between 2% and 30% of the mass of the second intermediate product; e) Feeding the mixed and heated second intermediate product into a stamping machine to produce a feedstock for coking; f) Feeding the feedstock for coking into the coke oven to produce a coke cake by coking.
2. The method according to claim 1, characterized in that the bituminous charcoal is characterized by the following features: - Volatile components, measured in the water- and ash-free substance: 19 - 28% by mass, - Carbon content, measured in the water- and ash-free substance: 86 - 89 mass %, - Hydrogen content, measured in the water- and ash-free substance: 5.0 - 5.5 mass %, - Oxygen content, measured in the water- and ash-free substance: 3.5 - 4.5 wt% • Water content in the raw substance: 2 - 4 wt% • Bloating number (according to DIN 5174): 4.5 - 9.0 - Baking ability number (according to ROGA, ISO 15585:2019): >45, - Average vitrinite reflectance under oil (according to DIN 22020 / 5): 1.2 - 1.6%, - Maximum fluidity measured in the GIESELER plastometer test device (according to ASTM D 2639-74): 50 - 1000 ddpm, - Energy content: 35,000 - 36,000 kJ / kg, where non-bituminous coal lacks at least one of these characteristics.
3. Method according to at least one of the preceding claims, characterized in that the non-fatty coal is a weak and non-abrasive raw material such as, in particular, lean / EB / gas / flame / gas flame coals and mixtures of coals, biochar and / or biomass.
4. Method according to at least one of the preceding claims, characterized in that one or more of the substances listed below are used: - Lye from the pulp industry, such as sulfite and sulfate lye, - processed lignins in solid (powder, granules) or liquid form of varying viscosity and dilution, - Molasses as a by-product of sugar production from sugar beets and sugar cane, of varying viscosity and dilution, - Bamboo or birch fibers, - Rapeseed or soybean extraction meal, - Porridges made from palm oil or lentil shells, - Spent grain primarily as a residue of leached malt and / or - Pomace from seeds (e.g. grapes) as a press residue in oil, wine and juice production, It can be used alone or as a mixture as a coking aid.
5. Method according to at least one of the preceding claims, characterized in that the petroleum-independent coking aids are designed not to act as binders in the uncoked state of the feedstock, but to exert their effect only during coking in the temperature range above 100 °C, in particular by forming adhesive melt bridges in the feedstock.
6. Method according to at least one of the preceding claims, characterized in that a binder is added to the first intermediate product before, during or after the addition of the coking aid.
7. Method according to at least one of the preceding claims, characterized in that the coking aids are added in uncoked or already coked form in granular or fibrous form.
8. Method according to at least one of the preceding claims, characterized in that coal anthracites are additionally added to the first intermediate product, in particular the coal mixture, in proportions of up to 5% by mass.
9. Method according to at least one of the preceding claims, characterized in that the mixing of the first intermediate product with a petroleum-independent coking aid to form a second intermediate product takes place in a heatable intensive mixer with high energy input.
10. Method according to at least one of the preceding claims, characterized in that the mixing of the first intermediate product with a petroleum-independent coking aid to form a second intermediate product with lignin-containing coking aids takes place at mixing temperatures of 60 °C to 100 °C, preferably at 80 °C.
11. Method according to at least one of the preceding claims, characterized in that the mixing of the first intermediate product with a petroleum-independent coking aid to a second intermediate product with protein-containing coking aids takes place at mixing temperatures of 40 °C to 60 °C, in particular at 50 °C.
12. Method according to at least one of the preceding claims, characterized in that the mixing of the first intermediate product with a petroleum-independent coking aid takes place over a period of time between 2 min and 10 min.
13. Method according to at least one of the preceding claims, characterized in that the mixer, in particular the intensive mixer, is equipped with a heating unit, in particular an infrared, hot air or induction heater.
14. Method according to at least one of the preceding claims, characterized in that the mixer, in particular the intensive mixer, is equipped with a moisture measuring probe, dosing devices, storage containers and / or an electromagnetic scale.
15. Method according to at least one of the preceding claims, characterized in that the coking aid is supplied as a grinding slurry, wherein the grinding slurry is processed in perforated disc mills, (twin screw) extruders or in a vibrating mill with grinding media, each preferably with the addition of water in solid-liquid ratios of 1:1, 1:2 and 1:
3.
16. Method according to at least one of the preceding claims, characterized in that the previous mixing temperature is maintained when stamping the second intermediate product in the stamping machine.
17. A method according to at least one of the preceding claims, characterized in that, when stamping the second intermediate product in the stamping machine, the stamping pressure is between 5 and 50 MPa, preferably between 20 and 30 MPa.
18. A method according to at least one of the preceding claims, characterized in that, when stamping the second intermediate product in the stamping machine, the stamping duration does not exceed 5 minutes and is preferably 30 seconds to 3 minutes.
19. Method according to at least one of the preceding claims, characterized in that, during the stamping of the second intermediate product in the stamping machine, the density of the feedstock for coking (stamp cake density) exceeds 1000 kg / m³. 3is achieved in a dry state.
20. Method according to at least one of the preceding claims, characterized in that a non-linear heating of the feedstock for coking takes place in the coke oven, wherein at least two coking rates coupled to each other with different temperature increases are provided.
21. Method according to at least one of the preceding claims, characterized in that, between the at least two coupled coking rates, temperature-related steady-state ramps are also inserted, specific to the raw material and application.