Metal-ceramic substrate, and method for dividing a metal-ceramic substrate
The use of ultrashort pulse laser light and controlled local heating for cutting metal-ceramic substrates addresses the inefficiencies of manual methods, achieving precise and automated cutting with reduced damage and defects.
Patent Information
- Application Number
- PCT/EP2026/062473
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for cutting metal-ceramic substrates often result in damaging effects and require manual or mechanical intervention, leading to potential defects and inefficiencies.
A method involving ultrashort pulse laser light to create discontinuous amorphous phases with controlled depth ratios and local heating without active cooling, allowing for automated and precise cutting of metal-ceramic substrates into individual units.
The method enables precise, reliable, and damage-free cutting of metal-ceramic substrates, reducing the risk of defects and manual errors, while allowing for efficient automation and improved fracture behavior.
Smart Images

Figure EP2026062473_12112026_PF_FP_ABST
Abstract
Description
[0001] Rogers Germany GmbH MSP Ref: 49670 PT-WO PM / SK
[0002] Metal-ceramic substrate and method for dividing a metal-ceramic substrate
[0003] The present invention relates to a method for dividing a metal-ceramic substrate, a system for such a method and metal-ceramic individual substrates produced by such a method.
[0004] Electronic modules are well known from the prior art, for example as power electronics modules. Such electronic modules typically use switchable or controllable electronic components that are interconnected via conductive traces on a common metal-ceramic substrate. Essential components of the metal-ceramic substrate are an insulating layer, which in the case of a metal-ceramic substrate is made of a ceramic material, and a metallization layer, which is preferably structured to form conductive traces and is applied to one side of the metal-ceramic substrate.
[0005] Typically, a metal-ceramic substrate is produced as a large card, which is then separated into smaller metal-ceramic substrates, i.e., individual metal-ceramic substrates, either before or after structuring. These large cards are processed using laser light to create predetermined breaking lines and / or separation points. The individual metal-ceramic substrates can then be separated from the large card, for example, by manual breaking. The use of ultrashort pulse lasers has proven advantageous in this process, as described, for example, in WO 2017 / 108950 A1.
[0006] Starting from this prior art, the present invention aims to improve, and in particular simplify, the cutting of metal-ceramic substrates, and to reduce any damaging effects on the metal-ceramic substrate during cutting.49670 PT-WO PM / SK © This objective is achieved by a metal-ceramic substrate according to claim 1, a method according to claim 9, and a single metal-ceramic substrate produced by such a method according to claim 10. Further embodiments can be found in the dependent claims and the description.
[0007] According to a first aspect, a metal-ceramic substrate is a large card for singulation into metal-ceramic individual substrates, comprising
[0008] - a ceramic element and a component metallization, arranged one above the other along a stacking direction, and
[0009] - at least one predetermined breaking line between metal-ceramic individual substrates to be separated, extending along a predetermined breaking line direction, wherein along the predetermined breaking line
[0010] -- an amorphous phase formed by exposure to ultrashort pulse laser light is interrupted and / or
[0011] -- the depth of the predetermined breaking line assumes a first depth dimensioned parallel to the stacking direction, wherein the ratio between the first depth and the thickness of the ceramic element assumes a value greater than 0.2, preferably greater than 0.3 and particularly preferably greater than 0.4
[0012] In contrast to the prior art, the predetermined breaking line is designed to either have a discontinuous amorphous phase along the direction of the predetermined breaking line or a depth that is comparatively large compared to the thickness of the ceramic element. It has been shown that the use of ultrashort pulse laser light is advantageous in the production of such metal-ceramic substrates as large cards. This is particularly true when the applied pulse laser light energy is sufficiently high to form amorphous phases. It has been found that cutting or breaking can be carried out with particularly precise control and, in particular, with greater process reliability when the amorphous phases are not continuous along the predetermined breaking line, but rather discontinuous along its direction.
[0013] Provided the pulse energy, i.e., the light pulse energy, is below a certain threshold, improved fracture behavior can also be observed if the corresponding depth for the predetermined fracture line is achieved. This can be caused or induced, for example, by multiple passes over or longer processing of the ceramic element with the laser light. Accordingly, improved fracture behavior can be observed if the corresponding phenomena, depending on the light pulse energy used, are visible on the provided metal-ceramic substrate as a large-scale map. These phenomena can also be observed on individual metal-ceramic substrates, particularly on the edge profiles of the respective substrates, as these still exhibit the angled sidewall sections resulting from the predetermined fracture line.on the notch that was inserted into the ceramic element to create the predetermined breaking line. Alternatively or additionally, an amorphous phase can be observed at the upper edge of the former predetermined breaking line, which is interrupted along the line. This is also visible on the manufactured metal-ceramic substrate, unless it was removed in a post-processing step.
[0014] In particular, the depth of the predetermined breaking line is designed to change along the line, especially along its direction. Specifically, the depth of the predetermined breaking line is adapted to particular areas that are especially susceptible to breakage.
[0015] Furthermore, it is preferably provided that the ratio of the first depth to a distance measured perpendicular to the stacking direction between the predetermined breaking line and the component metallization has a value between 0.05 and 1, preferably between 0.1 and 0.7, and particularly preferably between 0.15 and 0.4. It has been found, for example, that in a method which provides for the generation of a predetermined breaking line by means of an ultrashort pulse laser, tool-free or non-manual separation is possible if the metal-ceramic substrate is subjected to local heating of the predetermined breaking line and subsequently to a temperature between 15° and 25°. It has been found that a particularly gentle breaking of the predetermined breaking line is possible in this way.However, this requires a corresponding energy input, which is limited by the component's metallization. This metallization prevents the applied light heat from sufficiently warming the predetermined fracture line to produce a successful fracture. To compensate for this, it is advantageous in such cases for the ultrashort pulse laser to create a predetermined fracture line with a greater initial depth. The deeper the initial depth of the predetermined fracture line, the narrower the illumination with the heating light can be. Therefore, for metal-ceramic substrates where the component's metallization is particularly close to the edge of the ceramic element, it is beneficial to provide an initial depth greater than 0.5 times the thickness of the ceramic element.49670 PT-WO PM / SK © Preferably, the metal-ceramic substrates are provided to have at least one chamfer, wherein the predetermined breaking line in the chamfer area has a second depth, the second depth being greater than the first depth. Corner areas of the metal-ceramic substrates, especially those corner areas with a chamfer, are particularly susceptible to uncontrolled and unwanted breakage. Here, it is advantageous if the predetermined breaking line has a second depth that is greater than a first depth.
[0016] Preferably, the metal-ceramic substrates are surrounded by a frame element, with a predetermined breaking line of a third depth provided between the metal-ceramic substrates, the third depth being greater than the first depth. The frame element, which preferably comprises exclusively ceramic and no component metallization, and which surrounds the metal-ceramic substrates to be separated, is also separated from an arrangement of metal-ceramic substrates to be separated by a predetermined breaking line of a second and / or third depth. Here, too, it proves advantageous to implement a greater second and / or third depth to ensure successful breaking or snapping of this arm.
[0017] Furthermore, it is preferably provided that the first depth of the predetermined breaking line is essentially constant outside of a region of the chamfer and / or the frame element. This not only simplifies the manufacturing of the predetermined breaking line, but also increases the stability of the predetermined breaking line to an extent that ensures safe transport and at the same time allows for easier breaking off of the frame element, especially if only the frame element is to be separated in one process step.
[0018] In particular, the ratio between the first depth and the second depth takes on a value less than 0.95, preferably less than 0.9, and most preferably less than 0.85. This significantly reduces the probability of a failed break in the corner and / or frame area.
[0019] Preferably, a transition is provided along the predetermined fracture line direction from a first area with the first depth to a second area with the second or third depth, wherein the transition is step-shaped, arc-shaped and / or ramp-shaped.49670 PT-WO PM / SK © According to a further aspect, a method for cutting a metal-ceramic substrate, in particular according to one of the preceding claims, wherein the metal-ceramic substrate is preferably cut into individual metal-ceramic substrates, is provided, comprising:
[0020] - Providing a metal-ceramic substrate, wherein the metal-ceramic substrate comprises at least one metal layer and one ceramic element,
[0021] - Formation of a target book line, in particular by removing ceramic material from the ceramic element and
[0022] - local heating of the ceramic element in the area of the predetermined breaking line using laser light, wherein the metal-ceramic substrate is cut by exposing it to a temperature between 5 °C and 45 °C and in particular without active cooling, and wherein the cutting is carried out without mechanical and / or manual intervention on the metal-ceramic substrate.
[0023] In contrast to prior art methods, this process deliberately avoids active cooling, particularly shock cooling after local heating. Specifically, the local heating is designed to fracture or break the metal-ceramic substrates intended as large cards without the need for cooling, especially shock cooling. Furthermore, the breaking occurs without mechanical means or by manual means. This results in particularly gentle breaking of the metal-ceramic substrates. Surprisingly, it has been found that, particularly due to the introduction of sufficient heat during local heating, it is unnecessary to break the created fracture line by targeted, especially active, cooling.This approach proves particularly advantageous because the bond between the metal layer and the ceramic element is subjected to less stress from the strong temperature change. This strong temperature change, which is otherwise caused by the active cooling required in prior art processes, is precisely what is avoided. Therefore, it proves to be particularly reliable and gentle to cut the metal-ceramic substrates without cooling in order to divide them into individual metal-ceramic substrates.
[0024] Preferably, for local heating, heat input from the laser light is introduced into the ceramic element via a longitudinally extended surface, wherein the longitudinally extended surface preferably runs substantially parallel to a predetermined fracture line direction. It is provided that the laser light for heating follows an oscillating motion and / or several laser light sources are used for heating and / or laser light is guided through an optical element for beam shaping. In particular, it is provided that an illuminated area produced by the laser light during local heating is not circular, but, for example, has an elliptical cross-section. This is achieved, for example, by moving the laser light back and forth, i.e., an oscillating motion, along the predetermined fracture line direction, i.e., the direction of travel.It would also be conceivable to use an optical (imaging) element for beam cross-section shaping, such as a cylindrical lens, which shapes the beam in such a way that an elliptical cross-section is formed. In other words, in addition to the relative movement between the substrate and the laser light, an additional, especially oscillating, movement of the laser light is provided in order to illuminate and heat a longitudinally elongated area locally and for a defined period of time.
[0025] It is also conceivable that a correspondingly elongated area for heating could be achieved using several laser spots positioned side by side and overlapping. This elongation ensures that a sufficiently large area is used for heat input, in order to force the desired fracture. In particular, this approach ensures that a sufficiently large area is illuminated without illuminating the component's metallization, which spatially limits the area available for heating the ceramic element. It is also conceivable that a desired elliptical path could be achieved by appropriately tilting the laser light.
[0026] Preferably, an illuminated area intended for heating is designed such that the surface has a first major axis and a minor second axis measured perpendicular to the major axis, wherein the ratio of the first axis to the second axis is greater than 1.5, preferably greater than 2, and particularly preferably greater than 2.5. This results in a particularly preferably longitudinally extended illuminated area on the ceramic element, which is advantageous for the desired and successful local heating of the ceramic element in the region of the predetermined fracture line. 49670 PT-WO PM / SK © Preferably, the laser light for heating is adjusted such that the heat input by means of the laser light is below a melting point of the ceramic element. It is therefore advantageous to introduce sufficient heat on one side so that a successful fracture occurs even if the fracture is to be initiated without further cooling.On the other hand, uncontrolled melting of the ceramic element should be avoided. It is evident to a person skilled in the art that the corresponding energy inputs depend on the ceramic element, in particular on its absorption behavior, especially in relation to the laser light used.
[0027] Preferably, the material removal from the ceramic element is carried out on a first side of the ceramic element, while the heating of the ceramic element is performed on a second side opposite the first. This allows for the treatment of opposite sides without the respective treatment steps interfering with each other. Furthermore, the area located below the predetermined fracture line—that is, the area actually intended to fracture—can be heated precisely. This ensures that as much energy as possible is introduced into the area that is actually relevant to the fracture behavior of the ceramic element.
[0028] The described method, which combines the generation of local thermomechanical stress with the generated predetermined fracture lines, proves particularly advantageous because it enables the automatic separation or splitting of the ceramic element. Consequently, manual breaking or breaking caused by mechanical action on the ceramic element can be avoided. This reduces the probability of a defective fracture, as, for example, the possibility of incorrect force application during fracture is eliminated. Furthermore, potential scratches that can be caused by manual or mechanical breaking are avoided. Finally, it also prevents fingerprints or similar marks that might be left on the metal-ceramic substrate, especially on the at least one metal layer, during manual breaking.This is therefore an essentially non-contact process that can be automated and leads to the desired division of the metal-ceramic substrate into individual metal-ceramic substrates. The person skilled in the art will preferably not consider clamping the metal-ceramic substrate, particularly for holding it in place, as an action with a mechanical tool, especially since such a clamping tool is primarily intended for holding the large card and / or the metal-ceramic substrate. Such a clamping tool can, for example, be equipped with a vacuum element to act on the large card.
[0029] Specifically, it is a metal-ceramic single substrate used as a printed circuit board (PCB) where a metallization, i.e., a component metallization, is formed on the component side, which, due to its structuring, has several electrically isolated metallization sections. These metallization sections form, for example, connection pads or conductor tracks of the PCB.
[0030] Preferably, the ceramic element comprises AI₂O₃, SisN₄, AIN, an HPSX ceramic (i.e., a ceramic with an AI₂O₃ matrix comprising an x percent proportion of ZrÜ₂, for example, AI₂O₃ with 9% ZrÜ₂ = HPS₅ or AI₂O₃ with 25% ZrÜ₂ = HPS₅₅), SiC, BeO, MgO, high-density MgO (> 90% of the theoretical density), or TSZ (tetragonally stabilized zirconia) as the ceramic material. In particular, the ceramic element has a thermal conductivity greater than 100 W / mK, preferably greater than 120 W / mK, or most preferably greater than 130 W / mK. It is also conceivable that the ceramic element is designed as a composite or hybrid ceramic, in which several ceramic layers, each differing in terms of their material composition, are arranged on top of each other and joined together to form an insulating element in order to combine various desired properties.
[0031] Suitable materials for component metallization and / or backside metallization include copper, aluminum, molybdenum, tungsten, and / or their alloys such as CuZr, AlSi, or AlMgSi, as well as laminates such as CuW, CuMo, CuAl, and / or AICu or MMC (metal matrix composite), such as CuW, CuMo, or AlSiC. Preferably, the component metallization is identical to the backside metallization in terms of material or differs from it. Furthermore, it is preferably provided that the component metallization and / or the backside metallization is surface-modified on the manufactured metal-ceramic substrate, particularly as component metallization. Surface modification could include, for example, sealing with a precious metal, especially silver and / or gold, or (electroless) nickel or EN IG (electroless nickel immersion gold), or edge sealing of the metallization to suppress crack formation or propagation.49670 PT-WO PM / SK © For example, the metal used for component metallization also differs from the metal used for backside metallization.
[0032] The bonding of the metal layer, i.e., the component metallization and / or the backside metallization, to the ceramic element can be achieved, for example, via a DCB process, an AM B process, a diffusion bond, in particular ADB, and / or hot isostatic pressing.
[0033] A "DCB process" (Direct Copper Bond Technology) or a "DAB process" (Direct Aluminum Bond Technology) is understood by those skilled in the art to be a process used, for example, to bond metal layers or sheets (e.g., copper sheets or foils or aluminum sheets or foils) to each other and / or to ceramics or ceramic layers, using metal or copper sheets or foils that have a layer or coating (fused-on layer) on their surface. In this process, described, for example, in US 3,744,120 A or DE 2319854 C2, this layer or coating (fused-on layer) forms a eutectic with a melting point below that of the metal (e.g., copper), so that by placing the foil on the ceramic and heating all layers, they can be bonded together by melting the metal or foil.Copper is essentially only present in the area of the molten layer or oxide layer.
[0034] Preferably, the ceramic layer and the metal layer are joined by means of a direct metal bonding process, hot isostatic pressing, a soldering process and / or a diffusion bonding process.
[0035] In particular, the DCB method then includes, for example, the following procedural steps:
[0036] • Oxidizing a copper foil in such a way that a uniform copper oxide layer is formed;
[0037] • Applying the copper foil to the ceramic layer;
[0038] • Heating the composite to a process temperature between approximately 1025 and 1083°C, e.g., to approximately 1071°C; 49670 PT-WO PM / SK ©
[0039] • Cool to room temperature.
[0040] An active soldering process, e.g., for joining metal layers or foils, especially copper layers or foils, to ceramic material, is a process specifically used for producing metal-ceramic substrates. At a temperature between approximately 600 and 1000°C, a bond is created between a metal foil, for example, copper foil, and a ceramic substrate, for example, aluminum nitride ceramic, using a hard solder. In addition to a main component such as copper, silver, and / or gold, this hard solder also contains an active metal. This active metal, which is, for example, at least one element from the group Hf, Ti, Zr, Nb, Ce, forms a bond between the solder and the ceramic through a chemical reaction. The bond between the solder and the metal is a metallic brazing joint. Alternatively, a thick-film bonding process is also conceivable.Preferably, a separate active metal layer is used for bonding, which is introduced, for example, as a solder system between the ceramic element and the metal layer in addition to a solder base material layer.
[0041] Preferably, an ADB (active diffusion bonding) process is used, which includes, for example, the following steps:
[0042] - Providing a ceramic element and a metal layer,
[0043] - Providing a gas-tight container that encloses the ceramic element, wherein the container is preferably formed from or comprises the metal layer,
[0044] - Formation of the metal-ceramic substrate by bonding the metal layer to the ceramic element using hot isostatic pressing,
[0045] In order to form the metal-ceramic substrate, at least in sections an active metal layer or a contact layer comprising an active metal is arranged between the metal layer and the ceramic element to support the bonding of the metal layer to the ceramic element. The container is preferably formed as a metal container consisting of a metal layer and / or another metal layer. Alternatively, it is also conceivable that a glass container is used.
[0046] In hot isostatic pressing, it is specifically designed that bonding occurs through heating under pressure, ensuring that the metal layer of the metal container, particularly the subsequent metal layer of the metal-ceramic substrate and any eutectic layer present there, does not enter the molten phase. Accordingly, hot isostatic pressing requires lower temperatures than a direct metal bonding process, especially a DCB process.
[0047] In contrast to bonding a metal layer to a ceramic layer using a solder material, which typically involves temperatures below the melting point of at least one metal layer, the present method advantageously eliminates the need for a solder base material and requires only an active metal. Furthermore, the use of pressure during hot isostatic pressing proves beneficial because it reduces air inclusions or voids between the metal layer and the ceramic element. This, in turn, reduces or even eliminates the formation of voids in the resulting metal-ceramic substrate. This positively impacts the bond quality between the metal layer of the metal container and the ceramic element.Furthermore, it is advantageously possible to simplify the "second etching" and avoid solder residues and silver migration.
[0048] The active metal layer comprises a comprehensive contact layer of active metal exceeding 15 wt.%.
[0049] Hot isostatic pressing is known, for example, from EP 3080055 B1, the content of which is hereby explicitly referenced with regard to hot isostatic pressing.
[0050] According to a preferred embodiment of the present invention, it is provided that in the manufactured metal-ceramic substrate a bonding layer is formed between the component metallization and the ceramic element, wherein an adhesion promoter layer of the bonding layer has a surface resistance greater than 0.5 ohms / sq, preferably greater than 1 ohm / sq and particularly preferably greater than 2 ohms / sq or even greater than 15 ohms / sq, in particular greater than 20 ohms / sq.
[0051] The surface resistance is directly related to the proportion of active metal in the adhesion promoter layer, which is crucial for bonding the at least one metal layer to the ceramic element. The surface resistance increases with decreasing active metal content in the bonding layer. A correspondingly high surface resistance therefore corresponds to a low active metal content in the adhesion promoter layer.
[0052] The surface resistance does not depend on a single parameter, but can be influenced by the interplay of several parameters. For example, the purity of the active metal, the thickness of the bonding layer, and / or the surface roughness of the ceramic element also contribute to determining the surface resistance. In particular, high surface resistances can only be achieved through the interaction of at least two parameters.
[0053] It has been found that an increasing proportion of active metal promotes the formation of brittle, intermetallic phases, which in turn is detrimental to the pull-off strength of the metal layer at the insulating layer. In other words, the specified surface resistances describe bonded layers whose pull-off strength is improved, i.e., increased, due to the reduced formation of brittle intermetallic phases.
[0054] A structuring is preferably incorporated into the at least one metal layer prior to the formation of the predetermined breaking line by removing material from the bonded at least one metal layer.
[0055] According to a preferred embodiment of the present invention, the ablation of ceramic materials is achieved using light from a first laser source and / or the local heating of the ceramic element in the region of the predetermined fracture line is achieved using light from a second laser source. It is preferably provided that the first and second light sources differ from one another, particularly with regard to wavelength, intensity, and / or operating mode; i.e., they can be pulsed or continuous wave (CW) radiation. Alternatively, it is conceivable that the first and / or the second laser source are lasers of the same type, but operated, for example, at different wavelengths and / or intensities, perhaps by varying the light cross-section. For example, it is conceivable that the first and / or the second laser source is a YAG, fiber, or CO2 laser.49670 PT-WO PM / SK © Preferably, the first laser source is an ultrashort pulse laser source, in particular a source that generates pulse durations of less than 100 ns, preferably less than 100 ps, and most preferably less than 1 ps. It has been found that particularly favorable amorphous phases can be generated at the edge of the predetermined breaking point with such ultrashort pulse lasers, which have a positive effect on the fracture behavior and, in particular, avoid undesired fracture behavior and fracture patterns when the individual metal-ceramic substrates break apart. The second laser source, which is used for heating, is in particular a laser source that generates pulses greater than 1 ns or lasers that operate in continuous wave mode. Thus, the first laser source is different from the second laser source, differing in particular with regard to its pulse duration.The pulse length of the second laser source is at least 10 times, preferably at least 50 times, and particularly preferably 70 times longer than the pulse length of the first laser source. This allows sufficient thermal energy to be introduced into the ceramic element by the second laser source to achieve the desired self-breaking effect, while the first light source creates a predetermined fracture line, which, together with the thermal heating, has proven particularly suitable for controlled and therefore process-reliable cutting.
[0056] In particular, the first light source is designed to cause material removal from the ceramic element, especially from its top or outer surface, while the second light source is configured or designed to cause only heating without material removal. It is also conceivable that the second light source is selected to contribute at least a small amount of material removal. For example, it is also conceivable that the first light source is used to at least partially create the predetermined breaking point and also to heat or preheat the ceramic element. Furthermore, it is conceivable that the predetermined breaking point is created using a chemical or mechanical process.
[0057] Preferably, the first laser source is an ultrashort pulse (USP) laser source that provides light pulses with a pulse duration of 0.01 to 800 ps, preferably 1 to 500 ps, and particularly preferably 10 to 50 ps. It has proven particularly advantageous to produce predetermined fracture lines or fracture points using such pulses, especially at processing speeds between 0.2 and 8 m / s. These fracture lines exhibit a particularly favorable ratio between molten ceramic and crack formation within the fracture lines, thereby ensuring particularly reliable and successful fracturing along the fracture lines without causing damage to the individual metal-ceramic substrate during fracturing.
[0058] Preferably, the area heated by means of the laser light, in particular the second laser source, is smaller than 5 mm. 2 , preferably smaller than 2 mm 2and especially preferably smaller than 0.7 mm 2 Preferably, the area heated by the light is larger than 0.2 mm. 2 , preferably larger than 1 mm 2 and especially preferably larger than 1.5 mm 2 .
[0059] Preferably, the removal of ceramic material is carried out on a first side of the ceramic element, and the heating of the ceramic element is performed on a second side opposite the first, and / or the predetermined breaking line is interrupted or continuous. In the case of opposite processing, particularly when creating the predetermined breaking line on one side and generating the thermomechanical stress on the other, it is advantageously possible to realize the predetermined breaking line and the separation or cutting process in the ceramic element as simultaneously or in parallel as possible. Alternatively or additionally, it is conceivable that the heating takes place on the same side as the creation of the predetermined breaking line. In this case, a common holding element can be used for creating the predetermined breaking line and the subsequent separation by combining heating and cooling of the ceramic element in a locally limited area.
[0060] Furthermore, the predetermined breaking line can be designed, for example, as a notch or V-shaped feature and / or have varying depths along its direction, and may even be interrupted. For instance, the predetermined breaking line could be a perforation or, alternatively, a continuous notch that defines the desired separation path.
[0061] Furthermore, it is preferably provided that the generation of the predetermined breaking line and / or the heating takes place after structuring the metal-ceramic substrate, i.e., after the at least one metal layer has been structured in such a way that conductive traces and / or contact surfaces have been generated on the component side.49670 PT-WO PM / SK © Furthermore, it is preferably provided that a predetermined breaking line with a depth of less than 50 pm, preferably less than 20 pm, and particularly preferably less than 15 pm is realized by removing ceramic material.Furthermore, it is preferably provided that a predetermined breaking line with a depth greater than 1 pm, preferably greater than 4 pm, and particularly preferably greater than 8 pm, is created by removing ceramic material. It has been found that predetermined breaking lines with a shallow depth are necessary or required, meaning that the predetermined breaking lines need not be as deep as those usually created to guarantee a clean break or to improve mechanical stability during subsequent handling. This saves time in the manufacturing process when creating the predetermined breaking line. In addition, it saves the energy required to create the predetermined breaking line.
[0062] Preferably, a maximum temperature change of more than 1,000 °C / s, preferably more than 10,000 °C / s, and particularly preferably more than 50,000 °C / s is achieved during heating. This correspondingly high temperature change allows the desired thermomechanical stresses to be selectively generated in the target area, causing or resulting in automatic fracture.
[0063] Preferably, the metal-ceramic substrate is fixed, at least temporarily, and preferably throughout the entire separation or division process, for example, by means of a vacuum. The skilled person defines the entire division process as the process that begins with the creation of the predetermined breaking line and ends with the removal of the individual metal-ceramic substrates. By appropriate fixing and the application of the vacuum, additional stress can also be generated in the metal-ceramic substrate, which leads to the desired fracture or separation being produced automatically.
[0064] Another object of the present invention is a metal-ceramic single substrate produced from a metal-ceramic substrate according to the present invention. All properties described for the metal-ceramic substrate can be applied analogously to the metal-ceramic single substrate and vice versa. As already stated above, the properties of the metal-ceramic substrate in the form of the large card can be recognized in the isolated metal-ceramic single substrate, provided no post-processing step has been carried out. Under certain circumstances, a corresponding post-processing step can also be identified, for example, by an uneven removal of ceramic material on the top or bottom surface of the ceramic element.
[0065] Further advantages and features will become apparent from the following description of preferred embodiments of the invention with reference to the accompanying figures. Individual features of the individual embodiments can be combined with one another within the scope of the invention.
[0066] It shows:
[0067] Fig. 1: Schematic representation of a method for singulating metal-ceramic substrates according to a first exemplary embodiment of the present invention,
[0068] Fig. 2: Schematic representation of a method for singulating metal-ceramic substrates according to a second exemplary embodiment of the present invention and
[0069] Fig. 3a, 3b. Sectional views through a metal-ceramic substrate (Fig. 3a) and a metal-ceramic single substrate (Fig. 3b)
[0070] Figure 1 schematically illustrates a method for providing a metal-ceramic single substrate 1, which is separated from a metal-ceramic substrate 10 provided as a large card, according to a first preferred embodiment of the present invention. Such a metal-ceramic single substrate 1 preferably serves as a carrier for electronic or electrical components that can be bonded to the metal-ceramic single substrate 1. Essential components of such a metal-ceramic single substrate 1 are a ceramic element 20 extending along a principal extension plane HSE and at least one metal layer 21 bonded to the ceramic element 20. The ceramic element 20 is made of at least one material comprising a ceramic.The at least one metal layer 21 and the ceramic element 20 are arranged one above the other along a stacking direction S perpendicular to the principal extension plane HSE and, in a finished state, are at least partially bonded to one another via a bonding surface. Preferably, the at least one metal layer 21 is then structured to form conductive tracks or connection points for the electrical components. For example, this structuring is etched into the at least one metal layer 21. However, a permanent bond, in particular a material-bonded bond, must first be formed between the at least one metal layer 21 and the ceramic element 20.
[0071] To permanently bond the metal layer 21 to the ceramic element 21, a system for producing the metal-ceramic substrate 10, particularly in a DCB or DAB bonding process, comprises a furnace in which a stacked arrangement of the ceramic element 20 and the at least one metal layer 21 is heated, thereby achieving the bond. For example, the at least one metal layer 21 is made of copper, and the at least one metal layer 21 and the ceramic element 20 are joined together using a DCB (Direct Copper Bonding) process. Alternatively, the at least one metal layer 21 can be bonded to the ceramic element 20 using an active soldering process, an ADB (Active Diffusion Bonding) process, hot isostatic pressing, or a thick-film process.
[0072] After bonding, in particular by means of a DCB process, a soldering process, active diffusion bonding, hot isostatic pressing, and / or a thick-film process, the metal-ceramic substrate 10 is structured and provided as a large sheet. In the subsequent process, such large sheets are to be separated to provide individual metal-ceramic substrates 1. Preferably, for such separation, the large sheet is processed using laser light from a first laser source, in particular using ultrashort pulse laser light (not shown here). It is possible to create a predetermined breaking line 7 along which the large sheet is broken in the subsequent process, forming the individual metal-ceramic substrates 1. An ultrashort pulse laser is understood by those skilled in the art to be, in particular, laser sources that emit laser pulses whose pulse durations are less than one nanosecond.Preferably, the pulse duration is between 0.01 and 100 ps. Furthermore, it is conceivable that the pulse duration is in the femtosecond range, i.e., the pulse length is 0.01 to 100 ps. For example, the metal-ceramic substrate 1 is arranged in a holding element, at least during the production of the predetermined breaking line, and preferably during the entire cutting process.49670 PT-WO PM / SK © It is particularly provided that the metal-ceramic substrate 1 is fixedly arranged in the holding element for the production of the predetermined breaking line 7. In order to create a predetermined breaking line 7 in the metal-ceramic substrate 1, which in particular has a specific course, i.e., along a predetermined breaking line direction, across the metal-ceramic substrate 1, it is provided that the laser light or a laser beam from the first laser source is moved across the metal-ceramic substrate 1. In other words: Instead of the metal-ceramic substrate 1 relative to the laser light orTo change the orientation of the metal-ceramic substrate 1, it is preferably provided that the laser light or laser beam of the first laser source is aligned to form the predetermined fracture line 7 such that the laser light passing over the metal-ceramic substrate 1 creates a predetermined fracture line 7 at the respective points of impact. The laser light from the first laser source passing over the metal-ceramic substrate 1 has a processing speed between 0.1 and 2 m / s, and preferably between 0.8 and 1.5 m / s. Alternatively, it is conceivable that the metal-ceramic substrate 1 is moved to change the position of the laser light 10 striking the metal-ceramic substrate 1. In particular, the first laser source is designed to effect material removal from the ceramic element 20, for example, by appropriately adjusting the wavelength of the light and / or the light intensity.Alternatively, it is also conceivable that the predetermined breaking line 7 is produced using a mechanical or chemical process.
[0073] At the point in time shown in Figure 1 of the process for cutting or processing the metal-ceramic substrate, the predetermined breaking line 7 has already been created. The predetermined breaking line 7 shown in Figure 1 has a V- or notch-shaped form in a sectional view, which runs perpendicular to the principal extension plane HSE and perpendicular to the direction of the predetermined breaking line 7. Furthermore, the predetermined breaking line 7 has a first depth T, which is dimensioned, in particular, along the stacking direction S. It is conceivable that, in particular, the first depth T is modulated or varied along a predetermined breaking line direction along which the predetermined breaking line 7 extends, or is essentially constant, i.e., deviates by no more than 5%, particularly preferably no more than 2.5%, and particularly preferably no more than 1% from a mean value of the first depth T along the predetermined breaking line direction.For example, it is conceivable that a jagged or wavy course along the direction of the predetermined breaking line is provided for a floor of predetermined breaking line 7.
[0074] In particular, the trench bottom of the predetermined breaking line 7, which is set back from the outer surface of the ceramic element 20, assumes a linear shape and is, in particular, height-modulated along the predetermined breaking line direction VR. Height modulation is preferably understood by those skilled in the art to mean a deviation from a first depth T averaged along the direction VR of more than 5% of the averaged depth. If there are no deviations from the first depth T greater than 5% of the averaged depth, the depth T is assumed to be substantially constant. For example, the depth T of the predetermined breaking line 7 can also be constant.
[0075] To enable the automation of the cutting of the metal-ceramic substrate 10 into individual metal-ceramic substrates 1, it is provided that the ceramic element 20 is subjected to a targeted local thermomechanical stress in the area where the predetermined breaking line 7 is formed. It has been shown that it is sufficient to selectively introduce heat locally in the area of the predetermined breaking line 7, in particular by means of light from a second laser source. This induces thermomechanical stresses in the ceramic element 20 such that a fracture occurs in the correspondingly treated area of the predetermined breaking line 7, especially along the predetermined breaking line 7. The ceramic element 20 is thereby selectively heated briefly in a spatially limited area.
[0076] It has been found that it is advantageous to have a predetermined breaking line 7 to prevent uncontrolled breakage, particularly breakage that does not occur along the desired dividing line. In other words, the predetermined breaking line 7 embedded in the ceramic element 20 specifies the direction along which the automated breakage occurs, which in turn is triggered by the process sequence in which the ceramic element 20 is locally heated.
[0077] In the embodiment shown in Figure 1, the ceramic element 20 is heated in the area of the predetermined breaking point 7 by means of laser light 15 from a second laser source. It is particularly intended that the second laser source is designed such that it can generate heat input or a temperature increase in the ceramic element 20 in the irradiated area, but does not cause any material removal. For example, the desired heat input can be achieved without material removal by appropriately selecting the wavelength and / or intensity.
[0078] In the embodiment shown in Figure 1, the laser light 15 of the second laser source is directed towards the side of the ceramic element 20 opposite the predetermined breaking point 7. Alternatively, it is conceivable that the light 15 of the second laser source is directed towards the same side of the ceramic element 20, particularly in the areas of the predetermined breaking point 7, in which the breaking point 7 is also embedded. Furthermore, it is preferred that the heating takes place in a locally restricted partial area of the ceramic element 20 in which the predetermined breaking point 7 is located and / or which is sufficiently far removed from the at least one metal layer 21 of the metal-ceramic substrate 10.
[0079] For example, it is provided that a distance A between the light 15, in particular a laser beam, and the at least one metal layer 21 is at least 200 pm. This advantageously prevents the thermomechanical stress generated in the region of the predetermined breaking line 7 from impairing or even damaging the bond between the at least one metal layer 21 and the ceramic element 20 in the metal-ceramic substrate 10.
[0080] Furthermore, it is provided that the first depth T of the predetermined breaking line 7 is reduced compared to those required to effect purely manual division of the metal-ceramic substrate 10 into the individual metal-ceramic substrates 1. For example, the first depth T, or the mean depth, of the predetermined breaking line 7 is less than 130 pm, preferably less than 100 pm, and particularly preferably less than 70 pm. Preferably, the ratio of a first depth T, or mean depth, to the thickness of the ceramic element 20 is less than 50%, preferably less than 30%, and particularly preferably less than 20% of the thickness of the ceramic element 30.
[0081] The automatic separation of the ceramic element 20 reduces cycle time and the likelihood of uneven breakage due to inconsistent force application during manual breaking. Specifically, the automatically separated metal-ceramic substrates 10 are removed from the holding element, and in particular, automatically removed and packaged. This eliminates the need to manually break and package the individual metal-ceramic substrates 1. It also prevents fingerprints that would otherwise be unintentionally left on the individual metal-ceramic substrates 1.
[0082] Figure 2 shows a metal-ceramic substrate 10 in the form of a large card according to a second exemplary embodiment of the present invention. In particular, the metal-ceramic substrate 10, designed as a large card, comprises several individual metal-ceramic substrates 1, each separated from the others by predetermined breaking lines 7. The individual metal-ceramic substrates 1 are enclosed or surrounded by a frame element 4, which is formed as a closed perimeter around the outermost circumference of the large card or the metal-ceramic substrate 1. The frame element 4 is also separated from the individual metal-ceramic substrates 1 by a predetermined breaking line 7. The top view shown in Figure 2 is directed towards the side of the metal-ceramic substrate 10 on which the predetermined breaking lines 7 have already been created. As shown in Figure 1, a state is depicted in which the predetermined breaking lines 7 have already been created.In particular, the predetermined breaking lines 7 exhibit amorphous phases that do not form continuously along the predetermined breaking line 7, but rather are uninterrupted. Specifically, these phases are statistically distributed across the large map, i.e., not distributed according to a recurring pattern across the large map or the metal-ceramic substrate. Furthermore, the lengths of the continuous amorphous phases also differ from one another. In addition, an elongated surface 30 is included in Figure 2, which is illuminated by light from the second laser source in this snapshot of the figure. Heat is introduced here. The ceramic element 20 is heated locally in the region of the predetermined breaking line 7. During the heating process, the elongated surface 30 migrates along the predetermined breaking line 7, specifically along the direction of the predetermined breaking line.The longitudinally extended surface 30, which in particular has an elliptical cross-section, serves the purpose of introducing thermal energy into the ceramic element 20 in order to generate thermomechanical stresses that cause spontaneous fracture of the ceramic element 20, i.e., without mechanical or manual intervention, without the introduction of an active cooling element. A correspondingly longitudinally extended surface 30, which is illuminated, can be realized, for example, by an oscillating, i.e., back-and-forth movement of the laser spot. An alternative possibility for realizing the longitudinally extended surface 30 is the use of several superimposed laser spots. It has been found that the longitudinally extended surface 30 makes it possible to introduce sufficient thermal energy to achieve targeted heating without the need for active cooling of the Meta II ceramic substrate 1.This longitudinally extended surface can, for example, also be realized by an arrangement of lenses forming an optical element. The optical element is inserted into a light beam path and, due to its imaging properties, changes the shape of the light cross-section. For pulsed applications, components are preferably used that can correct the pulse duration if necessary.49670 PT-WO PM / SK © The longitudinal extension of the surface 30 results in particular from the fact that the lateral extent of the area to be heated is limited by the position of the metal sections 21, from which the laser light is spaced, or rather, that its illumination does not lead to heating of the ceramic element 20. Therefore, a corresponding elliptical shape is advantageous in order to introduce sufficient heat into the ceramic element 20.Preferably, the longitudinally extended surface 30 is extended along a direction that runs essentially parallel to the direction of the predetermined breaking line. In particular, the longitudinally extended surface 30 has a first axis and a second axis perpendicular to the first axis, wherein the ratio of the second axis to the first axis is less than 0.5, preferably less than 0.3, and preferably less than 0.2. This results in a particularly elliptical shape of the longitudinally extended direction. The first axis preferably runs parallel to the longitudinal extent of the predetermined breaking line 7, i.e., the direction of the predetermined breaking line. Furthermore, the representation of this large map includes a so-called chamfer. This refers to corner areas, in particular rhombus- or quadrilateral intermediate areas between several adjacent corners of metal-ceramic single substrates 1.In particular, these necessitate an angled predetermined breaking line direction, especially in the area where the corners of the metal-ceramic individual substrates abut each other. In the embodiment shown here, the corner profile in the form of a chamfer 17 results in a change in the predetermined breaking line direction of 30°–70°, particularly 45°, compared to the predetermined breaking line direction along the longitudinal edges of the metal-ceramic individual substrates 1. It has been found that a corresponding chamfer 17 is advantageous for the fracture behavior and can also be used as a stop for further processing of the metal-ceramic individual substrate 1.
[0083] Preferably, the predetermined breaking line 7, which has a first depth T particularly outside the corner areas of the metal-ceramic individual substrates 1, has a second depth T in the fiber area that is greater than the first depth T, especially because these areas are prone to uncontrolled and random breakage, while the other predetermined breaking lines 7 located outside the corner areas, with their first depth, can provide a certain degree of stability that allows for the safe and stable transport of the metal-ceramic substrates 10 in the form of large cards. Furthermore, the predetermined breaking line 7 between the frame element 4 and the individual metal-ceramic individual substrates 1 has a second and / or third depth that is also greater than the first depth T.This allows the frame element 4 to be advantageously removed first, and only then, with the correspondingly advantageous spatial freedom, the metal-ceramic single substrates 1 to be further broken. It is conceivable that at least at the frame element 4, mechanical breaking is still supported, since imprints of tools and / or fingers are irrelevant for subsequent processes.
[0084] Preferably, at least two predetermined breaking lines 7, in particular opposing predetermined breaking lines 7, extend to the outermost edge of the large card to delineate the frame element 4. This avoids the probability of errors when separating the frame element 4. Preferably, only two predetermined breaking lines 7 are provided, extending continuously across the entire large card.
[0085] Figure 3a shows a cross-sectional view through the metal-ceramic substrate 1 in the form of a large map. It is evident to those skilled in the art that, after fracture, the individual metal-ceramic substrates 1 in Figure 3a exhibit a profile in the cross-sectional view that corresponds to half of the layer view shown here, in particular up to the dividing line indicated below the predetermined fracture line 7. In Figure 3a, a predetermined fracture line 7 is formed with an amorphous phase 2. In particular, an amorphous phase 2 forms as a deposit on the upper surface of the ceramic element 20. As already mentioned in connection with Figure 2, this phase is distributed across the individual predetermined fracture line profiles or along the respective predetermined fracture line directions when ultrashort pulse lasers are used. Such amorphous phases 2 occur particularly when light pulses with high light energy are used.If light pulses with lower energy are used, it is necessary to choose a greater first depth of the predetermined breaking line 7 in order to enable successful and process-reliable breaking without active cooling.
[0086] Figure 3b shows a sectional view in which a second light source 12 was used during heating. The energy of this light source is significantly above the threshold that leads to ablation of the ceramic element 20 or to a physical change in the surface properties of the ceramic element 20. Consequently, a stepped gradient is visible on the top surface of the ceramic element 20 and on the side of the ceramic element 20 that faces the secondary light source 12. This is due to the corresponding ablation of the ceramic element 20 by the light of the secondary light source. Additionally, it is conceivable that the laser light causes a modification to the top surface of the ceramic element 20 that faces the secondary light source during processing. Such a change, particularly an optical change, could be, for example, a color change or a matting.This makes it possible to identify, even after the predetermined fracture, those metal-ceramic individual substrates 1 that were subjected to the corresponding cutting process, since they are clearly attributable to the use of a heating second laser light 12, which has resulted in the form of the recess in the edge area, i.e. a step-like progression of the ceramic element 20 at the edge area and / or a discoloration, or optical modification of the ceramic element 20 in the edge area of the ceramic element 20.
[0087] In particular, Figure 3b shows a side wall region SB that bounds the metal-ceramic single substrate 1 at its outer circumference. This side wall region SB has a first side wall section S1 and a second side wall section S2, which are arranged one above the other when viewed in the stacking direction S. The first side wall section S1 runs essentially parallel to the stacking direction S, while the second side wall section S2 runs obliquely to the stacking direction S. The second side wall section S2 is the result of a predetermined breaking line 7 introduced into the ceramic element 20 and is still recognizable on the manufactured, i.e., divided, metal-ceramic single substrate 1. Furthermore, a region 4 with reduced thickness and, in particular, with optically modified properties extends over a width extending from the outer circumference.This width B is preferably in such a ratio to the thickness D of the ceramic element 20 that this ratio takes on a value that is less than 0.5, preferably 0.3 and particularly preferably less than 0.25.
[0088] 1 metal-ceramic single substrate
[0089] 2 amorphous phase
[0090] 4 frame element
[0091] 6. Reduced thickness area
[0092] 7 Break line
[0093] 10 Metal-ceramic substrate
[0094] 12 second laser source
[0095] 15 lights
[0096] 17th phase
[0097] 20 ceramic elements
[0098] 21 Metal layer
[0099] 30 area
[0100] T first depth HSE main extent plane S stacking direction
[0101] SB side wall area
[0102] S1 first side wall section S2 second side wall section B width
[0103] A distance
[0104] Thickness
Claims
49670 PT-WO PM / SK © Claims 1. Metal-ceramic substrate (10) as a large card for separating into metal-ceramic individual substrates (1), comprising a ceramic element (20) and a component metallization (21) arranged one above the other along a stacking direction (S), and at least one draft line (7) between metal-ceramic substrates (1) to be separated, extending along a draft line direction where along the predetermined breaking line (7) -- an amorphous phase (2) formed by the action of ultrashort pulse laser light is interrupted and / or -- the depth of the predetermined breaking line assumes a first depth dimensioned parallel to the stacking direction (S), wherein a ratio between the first depth to a thickness (D) of the ceramic element (20) assumes a value greater than 0.2, preferably greater than 0.3 and particularly preferably greater than 0.
4.
2. Metal-ceramic substrate (10) according to claim 1, wherein the first depth (T) changes along the direction of the predetermined fracture line.
3. Metal-ceramic substrate (10) according to one of the preceding claims, wherein the ratio of the first depth (T) to a distance (A) measured perpendicular to the stacking direction (S) between the predetermined breaking line and the component metallization (21) has a value between 0.05 and 1, preferably between 0.1 and 0.7 and particularly preferably between 0.15 and 0.
4.
4. Metal-ceramic substrate (10) according to one of the preceding claims, wherein the metal-ceramic single substrates (1) have at least one chamfer (17), wherein the predetermined breaking line (7) in the area of the chamfer (17) has a second depth, wherein the second depth is greater than the first depth (T).
5. Metal-ceramic substrate (10) according to one of the preceding claims, wherein the metal-ceramic individual substrates (10) are surrounded by a frame element (4), wherein a predetermined breaking line (7) with a third depth is provided between the metal-ceramic individual substrates (1), wherein the third depth is greater than the first depth.
6. Metal-ceramic substrate (10) according to one of the preceding claims, wherein the first depth (T1) of the predetermined breaking line (7) is substantially constant outside a region of the chamfer (17) and / or the frame element (4).
7. Metal-ceramic substrate (10) according to one of the preceding claims, wherein the ratio between the first depth (T1) and the second depth is less than 0.95, preferably less than 0.9 and particularly preferably less than 0.
85.
8. Metal-ceramic substrate (10) according to one of the preceding claims, wherein a transition occurs along the predetermined fracture line direction from a first area with the first depth to a second area with the second depth or third depth, wherein the transition is formed in a step-like, arc-like and / or ramp-like manner.
9. Method for dividing a metal-ceramic substrate (10), in particular according to one of the preceding claims, wherein the metal-ceramic substrate (10) is preferably divided into individual metal-ceramic substrates (1), comprising: - Providing a metal-ceramic substrate (10) wherein the metal-ceramic substrate (10) comprises at least a metal layer (21) and a ceramic element (20), - Forming a target book line (7), in particular by removing ceramic material from the ceramic element (20) and - local heating of the ceramic element (20) in the area of the predetermined breaking line (7) using laser light (15), wherein the metal-ceramic substrate (10) is separated by exposing it to a temperature between 5 °C and 45 °C and in particular without active cooling, and wherein the separation is carried out without mechanical and / or manual action on the metal-ceramic substrate (10).
10. Method according to claim 9, wherein for local heating a heat input of the laser light (15) is introduced into the ceramic element (30) via a longitudinally extended surface, wherein the longitudinally extended surface preferably runs substantially parallel to a predetermined fracture line direction.
11. Method according to claim 10, wherein the laser light (15) follows an oscillating motion sequence for heating and / or several laser light sources are used for heating and / or laser light is guided through an optical element for beam shaping.
12. Method according to claim 9 or 10, wherein a removal of ceramic materials is carried out by means of light (15) from a first laser source and / or the local heating of the ceramic element (30) in the area of the predetermined breaking line is carried out by means of light from a second laser source.
13. Method according to claim 12, wherein the first laser source is an ultrashort pulse (USP) laser source providing light pulses with a pulse duration of 0.01 to 800 ps, preferably 1 to 500 ps, particularly preferably 10 to 50 ps.
14. Method according to any one of claims 9 to 13, wherein the removal of ceramic material on a first side of the ceramic element (30) and the heating of the ceramic element (30) on a second side opposite the first side is carried out.
15. A single metal-ceramic substrate produced by dividing a metal-ceramic substrate according to any of the preceding claims.