Semiconductor device and method for producing semiconductor device
The method of two heat treatments improves crystallinity and reduces defects in semiconductor films, addressing issues of stress and impurities, resulting in high-performance, reliable, and low-power semiconductor devices.
Patent Information
- Application Number
- PCT/IB2026/054260
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Existing semiconductor devices face challenges in achieving high-performance, reliable, and low-power operation due to issues with crystallinity, stress, and impurities in semiconductor films, which affect electrical properties and reliability.
A method involving two heat treatments is employed to enhance crystallinity and reduce defects in semiconductor films, where a first heat treatment improves crystallinity and changes stress, followed by a second heat treatment to release hydrogen and supply oxygen, using specific insulating layers to manage hydrogen and oxygen interactions.
This approach results in semiconductor devices with improved electrical properties and high reliability by enhancing crystallinity, reducing strain, and minimizing defects, leading to transistors with good performance and low power consumption.
Smart Images

Figure IB2026054260_12112026_PF_FP_ABST
Abstract
Description
Semiconductor device and method for manufacturing a semiconductor device.
[0001] One aspect of the present invention relates to a semiconductor device, a memory device, a display device, and an electronic device.
[0002] It should be noted that one aspect of the present invention is not limited to the above-mentioned technical field. Examples of technical fields of one aspect of the present invention disclosed herein include semiconductor devices, display devices, light-emitting devices, energy storage devices, memory devices, electronic devices, lighting devices, input devices, input / output devices, methods for driving them, or methods for manufacturing them. A semiconductor device refers to any device that can function by utilizing semiconductor properties.
[0003] In recent years, semiconductor device development has progressed, and semiconductor devices are mainly used in LSIs, CPUs (Central Processing Units), and memory. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors and memory) formed on chips by processing semiconductor wafers, and electrodes that serve as connection terminals are formed on them.
[0004] IC chips, which include semiconductor circuits such as LSIs, CPUs, and memory, are mounted on circuit boards, such as printed circuit boards, and used as components in various electronic devices.
[0005] Furthermore, the technology of constructing transistors using semiconductor thin films formed on substrates with insulating surfaces is attracting attention. These transistors are widely applied in electronic devices such as integrated circuits and image display devices (also simply referred to as display devices). While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors are attracting attention as other materials.
[0006] Transistors using oxide semiconductors are known to have extremely low leakage current in the non-conductive state. For example, Patent Document 1 discloses a low-power CPU that utilizes the characteristic of low leakage current of transistors using oxide semiconductors. Patent Document 2 also discloses a memory device that uses oxide semiconductors and can retain memory contents for a long period of time. Non-Patent Document 1 also discloses In 2 O 3Its use in thin-film transistors has been reported.
[0007] Japanese Patent Publication No. 2012-257187 Japanese Patent Publication No. 2011-151383
[0008] Dhananjay and C. W. Chu, “Realization of In2O3 thin film transistors through reactive evaporation process,” Appl. Phys. Lett. 91, 132111 (2007). Takashi Koida, “High-mobility transparent conductive film,” National Institute of Advanced Industrial Science and Technology, AIST Photovoltaic Power Generation Research Results Presentation Meeting 2019, Internet <URL: https: / / unit.aist.go.jp / rpd-envene / PV / ja / results / 2019 / oral / T13.pdf>
[0009] One aspect of the present invention aims to provide a high-performance semiconductor device. Another aspect of the present invention aims to provide a semiconductor device having good electrical characteristics. Another aspect of the present invention aims to provide a highly reliable semiconductor device. Another aspect of the present invention aims to provide a low-power semiconductor device.
[0010] One aspect of the present invention aims to provide a semiconductor device having a novel configuration. Another aspect of the present invention aims to mitigate at least one of the problems of the prior art.
[0011] Furthermore, the description of these problems does not preclude the existence of other problems. Moreover, one aspect of the present invention does not need to solve all of these problems. Other problems can be identified from the description in the specification, drawings, claims, etc.
[0012] One aspect of the present invention is a method for manufacturing a semiconductor device, comprising the steps of: forming a semiconductor film on a first insulating layer; performing a first heat treatment to enhance the crystallinity of the semiconductor film; processing the semiconductor film into island shapes to form a semiconductor layer; forming a gate insulating layer in contact with the semiconductor film; forming a gate electrode in contact with the gate insulating layer; and performing a second heat treatment. The first heat treatment is performed at a higher temperature than the second heat treatment. In the second heat treatment, oxygen is supplied into the semiconductor layer, and hydrogen in the semiconductor layer is released to one or both of the first insulating layer and the gate insulating layer.
[0013] Furthermore, in the above, it is preferable to use a semiconductor film containing indium and oxygen.
[0014] Furthermore, in the above, it is preferable that one or both of the first insulating layer and the gate insulating layer be films containing hafnium and oxygen.
[0015] Furthermore, in the above, it is preferable that the semiconductor film exhibits tensile stress at a temperature of 25°C before the first heat treatment, and compressive stress at a temperature of 25°C after the first heat treatment.
[0016] Furthermore, in the above, it is preferable that the absolute value of the stress of the semiconductor film at a temperature of 25°C after the first heat treatment is smaller than the absolute value of the stress at a temperature of 25°C before the first heat treatment.
[0017] Furthermore, in the above, it is preferable that the semiconductor film has a first film, a second film, and a third film from the first insulating layer side. In this case, it is preferable that the second film is a film containing indium and oxygen, and that the first film and the third film each have a wider band gap than the second film.
[0018] Furthermore, it is preferable that the first and third films each contain a first element and oxygen. It is also preferable that the first element is one or more selected from indium, gallium, and zinc.
[0019] Furthermore, in the above, it is preferable that the semiconductor film has a fourth film between the first film and the second film. Moreover, it is preferable that the fourth film has a wider band gap than the second film. In this case, it is even more preferable that the first film is a film containing indium, gallium, zinc, and oxygen, and the fourth film is a film containing gallium and oxygen.
[0020] Another aspect of the present invention is a semiconductor device having a first insulating layer, a semiconductor layer, a gate insulating layer, and a gate electrode. The semiconductor layer is located on the first insulating layer. The gate insulating layer is in contact with the upper surface of the semiconductor layer. The gate electrode is in contact with the upper surface of the first insulating layer. The semiconductor layer has a first film, a second film, and a third film from the first insulating layer side. The second film contains indium and oxygen and is single crystal or polycrystalline. The first film and the third film each have a wider band gap than the second film.
[0021] Furthermore, in the above, it is preferable that the first film and the third film each contain the first element and oxygen. Moreover, it is preferable that the first element is one or more selected from indium, gallium, and zinc.
[0022] Furthermore, it is preferable that a fourth film is present between the first film and the second film. Preferably, the first film contains indium, gallium, zinc, and oxygen, and the fourth film contains gallium and oxygen.
[0023] According to one aspect of the present invention, a high-performance semiconductor device can be provided. Alternatively, a semiconductor device with good electrical characteristics can be provided. Alternatively, a highly reliable semiconductor device can be provided. Alternatively, a semiconductor device with low power consumption can be provided.
[0024] According to one aspect of the present invention, a semiconductor device having a novel configuration can be provided. According to one aspect of the present invention, at least one of the problems of the prior art can be mitigated.
[0025] Furthermore, the description of these effects does not preclude the existence of other effects. Moreover, one aspect of the present invention does not necessarily have to possess all of these effects. Other effects can be extracted from the description in the specification, drawings, claims, etc.
[0026] Figures 1A, 1B, 1C, 1D, and 1E illustrate the method for manufacturing a semiconductor device. Figures 2A, 2B, 2C, and 2D show examples of semiconductor device configurations. Figures 3A and 3B show examples of semiconductor device configurations. Figures 4A, 4B, 4C, 4D, and 4E show examples of semiconductor device configurations. Figures 5A, 5B, 5C, and 5D show examples of semiconductor device configurations. Figures 6A, 6B, 6C, and 6D show examples of semiconductor device configurations. Figures 7A and 7B show examples of semiconductor device configurations. Figures 8A1, 8B1, 8C1, 8D1, 8A2, 8B2, 8C2, and 8D2 illustrate the method for manufacturing a semiconductor device. Figures 9A1, 9B1, 9C1, 9A2, 9B2, and 9C2 illustrate the method for manufacturing a semiconductor device. Figures 10A and 10B illustrate the carrier concentration dependence of hole mobility. Figure 10C is a cross-sectional view illustrating an indium oxide film. Figure 11 is an example of a memory device configuration. Figures 12A and 12B are examples of memory device configurations. Figures 13A, 13B, 13C, and 13D are examples of memory device configurations. Figure 14 is an example of a memory device configuration. Figures 15A and 15B are examples of display device configurations. Figure 16 is an example of display device configuration. Figures 17A, 17B, 17C, and 17D are examples of electronic device configurations. Figures 18A, 18B, 18C, 18D, 18E, and 18F are examples of electronic device configurations. Figures 19A, 19B, 19C, 19D, 19E, 19F, and 19G are examples of electronic device configurations. Figures 20A and 20B are examples of electronic component configurations. Figures 21A, 21B, and 21C show examples of the configuration of a large computer. Figures 22A, 22B, and 22C show the stress measurement results for Example 1. Figures 23A and 23B show the Id-Vg characteristics for Example 2. Figure 24 shows the Id-Vg characteristics for Example 3.
[0027] The embodiments will be described below with reference to the drawings. However, it will be readily apparent to those skilled in the art that the embodiments can be implemented in many different ways, and their form and details can be modified in various ways without departing from the spirit and scope thereof. Accordingly, the present invention shall not be construed as being limited to the contents of the following embodiments.
[0028] In the invention described below, the same reference numerals are used in common across different drawings for identical parts or parts having similar functions, and repeated explanations are omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used, and reference numerals may not be assigned.
[0029] In the figures described herein, the size of each component, the thickness of the layers, or the area may be exaggerated for clarity. Therefore, the scale is not necessarily limited to those figures.
[0030] Furthermore, ordinal numbers such as "first," "second," etc., used in this specification are added to avoid confusion of components and do not limit the number of components or their order (for example, process order or layering order). In addition, the ordinal numbers used for components in one part of this specification may not be the same as the ordinal numbers used for those components in other parts of this specification or in the claims.
[0031] A transistor is a type of semiconductor device that can perform functions such as amplifying current or voltage, and switching operations that control conduction or non-conductivity. Transistors as used herein include IGFETs (Insulated Gate Field Effect Transistors) and thin-film transistors (TFTs).
[0032] Furthermore, the functions of "source" and "drain" may be reversed when transistors with different polarities are used, or when the direction of current changes during circuit operation. For this reason, in this specification, the terms "source" and "drain" may be used interchangeably.
[0033] Furthermore, in this specification, either the source or the drain of a transistor may be referred to as the "first electrode," and the other of the source or drain may be referred to as the "second electrode." The gate may also be referred to as the "gate" or "gate electrode."
[0034] Furthermore, in this specification, "electrically connected" includes cases where a connection is made via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it enables the exchange of electrical signals between the connected objects. For example, "something that has some kind of electrical function" includes electrodes or wiring, switching elements such as transistors, resistive elements, coils, and other elements with various functions.
[0035] In this specification, cases where two nodes are connected via an insulator, such as the dielectric of a capacitive element, the gate insulating film of a transistor, or an interlayer insulating film, are not included in the definition of "electrical connection."
[0036] In this specification, "approximately matching top surface shapes" means that at least a portion of the contours overlap between stacked layers. For example, this includes cases where the upper and lower layers are processed with the same mask pattern, or partially with the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer; in these cases, it may also be said that the "top surface shapes are approximately matching."
[0037] In this specification, the top surface shape of a component refers to the contour shape of that component in a plan view. A plan view refers to a view from the direction normal to the surface on which the component is formed, or to the surface of the support (e.g., substrate) on which the component is formed.
[0038] In the following, expressions indicating direction, such as "up" and "down," will generally be used in accordance with the orientation shown in the drawings. However, for the purpose of simplifying explanations, the direction referred to as "up" or "down" in the specification may not always coincide with that of the drawings. For example, when explaining the stacking order (or formation order) of a laminate, even if the side on which the laminate is provided (the surface to be formed, the support surface, the adhesive surface, the flat surface, etc.) is located above the laminate in the drawing, the surface to be formed may be described as "down" and the laminate side as "up."
[0039] In this specification, when we use expressions such as "A is above (or below) B" or "A is above (or below) B," we mean that the height of A from the reference plane is higher (or lower) than the height of B from the same reference plane. This includes cases where A and B overlap in a plan view, cases where A and B partially overlap in a plan view, and cases where A and B do not overlap in a plan view.
[0040] Furthermore, in this specification, the terms "film" and "layer" are interchangeable. For example, the term "insulating layer" may be interchangeable with the term "insulating film."
[0041] Furthermore, unless otherwise specified in this specification, off-current refers to the drain current when the transistor is in the off state (also called the non-conducting state or cutoff state). Unless otherwise specified, the off state refers to the state in an n-type transistor where the voltage Vgs between the gate and source is lower than the threshold voltage Vth (in a p-type transistor, it is higher than Vth).
[0042] (Embodiment 1) This embodiment describes a method for manufacturing a semiconductor device according to one aspect of the present invention. Here, a transistor will be used as an example of the semiconductor device.
[0043] A semiconductor device according to one aspect of the present invention is a transistor having at least a semiconductor layer, a gate insulating layer, and a gate electrode. It is preferable to use a metal oxide (also called an oxide semiconductor) exhibiting semiconductor properties for the semiconductor layer. In particular, it is preferable to use a metal oxide containing indium and oxygen (typically indium oxide).
[0044] In a method for manufacturing a semiconductor device according to one aspect of the present invention, at least two heat treatments are performed. The first heat treatment (first heat treatment) is performed after the semiconductor film is formed. The first heat treatment can improve the crystallinity of the semiconductor layer. For example, by performing the first heat treatment after forming a semiconductor film having an amorphous structure, a microcrystalline structure, or a polycrystalline structure with relatively small crystal grains, a semiconductor film having a polycrystalline structure with large crystal grains or a single-crystal structure can be obtained.
[0045] Furthermore, the stress of the semiconductor film can be made different before and after the first heat treatment. More specifically, the stress of the semiconductor film can be relaxed after the first heat treatment, thereby relieving the strain within the semiconductor film. For example, the absolute value of the stress in the semiconductor film after the first heat treatment can be made smaller than the absolute value of the stress before the first heat treatment. Also, for example, if the stress of the semiconductor film before the first heat treatment is tensile stress, performing the first heat treatment can yield a semiconductor film that exhibits a smaller absolute value of compressive stress than before the first heat treatment. In this way, by relieving the strain in the semiconductor film through the first heat treatment, the generation of lattice defects in the semiconductor film can be suppressed, and a semiconductor film exhibiting good electrical properties can be obtained. This makes it possible to obtain a transistor with good electrical properties and high reliability.
[0046] Next, the semiconductor film is processed into island shapes to form a semiconductor layer, after which a gate insulating layer and a gate electrode are formed. After that, a second heat treatment (second heat treatment) is performed. The second heat treatment releases hydrogen contained in the semiconductor layer to the insulating layer in contact with the semiconductor layer (underlying insulating layer or gate insulating layer), thereby reducing the hydrogen concentration in the semiconductor layer. Furthermore, the second heat treatment supplies oxygen to the semiconductor layer, compensating for oxygen deficiencies in the semiconductor layer. At this time, it is preferable to form an insulating layer that releases oxygen upon heating (e.g., an interlayer insulating layer) in advance near the semiconductor layer. This allows oxygen to be efficiently supplied to the semiconductor layer directly from the insulating layer or via the gate insulating layer during the second heat treatment. The second heat treatment may be performed using the heat generated during the formation of the gate insulating layer or the gate electrode, and may be combined with these processes.
[0047] Furthermore, it is preferable to perform the first heat treatment at a higher temperature than the second heat treatment. Since the first heat treatment is performed before forming the conductive layer that will become the electrodes of the transistor, it is possible to perform the treatment at a relatively high temperature. As a result, the crystallinity of the semiconductor layer can be improved.
[0048] It is preferable to use an insulating film having a function to capture or fix hydrogen (hereinafter also referred to as a gettering function) in either the gate insulating layer or the under insulating layer, or both. This allows the hydrogen released from the semiconductor layer by the second heat treatment to be retained in the gate insulating layer or the under insulating layer, thereby preventing hydrogen from being supplied to the semiconductor layer again.
[0049] As described above, by forming a semiconductor film with high crystallinity and good electrical properties through the first heat treatment, and then reducing defects and impurities in the semiconductor layer through the second heat treatment, it is possible to realize a transistor with extremely good electrical properties and high reliability.
[0050] Below, we will explain more specific examples with reference to the diagrams.
[0051] Figures 1A to 1E show schematic cross-sectional diagrams of each step in a method for manufacturing a semiconductor device according to one embodiment of the present invention.
[0052] First, an insulating layer 12 is formed on the substrate 11 (Figure 1A). The insulating layer 12 functions as an underlying insulating layer.
[0053] As the insulating layer 12, it is preferable to use an insulator that has the function of getting hydrogen. Examples of insulators that have the function of getting hydrogen include metal oxides having an amorphous structure. For example, it is preferable to use metal oxides such as magnesium oxide, aluminum oxide, hafnium oxide, and oxides containing aluminum and hafnium (hafnium aluminate). In such metal oxides having an amorphous structure, oxygen atoms have dangling bonds, and these dangling bonds may have the property of getting hydrogen. In other words, metal oxides having an amorphous structure can be said to have a high ability to get hydrogen.
[0054] For example, it is preferable to use hafnium oxide, aluminum oxide, hafnium aluminate, etc., as the insulating layer 12.
[0055] Furthermore, a film that releases oxygen upon heating may be used as the insulating layer 12. For example, an oxide film with high oxygen permeability such as silicon oxide or silicon oxynitride can be used.
[0056] For example, the insulating layer 12 can be made by laminating a film that has the function of getting hydrogen and a film that releases oxygen when heated. In this case, by using a film that has the function of getting hydrogen on the side that is in contact with the semiconductor layer 21 that will be formed later, hydrogen can be efficiently extracted from the semiconductor layer.
[0057] The insulating layer 12 can be formed by methods such as sputtering, chemical vapor deposition (CVD), or atomic layer deposition (ALD).
[0058] The insulating layer 12 is preferably a film having an amorphous structure. If a film having a polycrystalline or single-crystal structure is used as the insulating layer 12, when the semiconductor film 21f is formed later, the semiconductor film 21f may crystallize, reflecting the crystal structure of the insulating layer 12, and a polycrystalline structure with small crystal grains may be formed. Therefore, by using a film having an amorphous structure for the insulating layer 12, it is possible to suppress unintended crystallization of the semiconductor film 21f and obtain a semiconductor film 21f with low crystallinity. Furthermore, by making the insulating layer 12 amorphous, the hydrogen gettering performance can also be improved as described above. Note that if the absolute value of the lattice mismatch between the insulating layer 12 and the semiconductor film 21f is large, unintended crystallization of the semiconductor film 21f can be suppressed, so a film having a polycrystalline or single-crystal structure can be used as the insulating layer 12.
[0059] Next, a semiconductor film 21f is formed on the insulating layer 12 (Figure 1B). The semiconductor film 21f can be a metal oxide film. In particular, it is preferable to use an oxide film mainly composed of indium, tin, or zinc. Among these, transistors using single-crystal indium oxide are particularly preferred because they combine high mobility and high reliability.
[0060] The semiconductor film 21f can be formed by methods such as ALD, sputtering, CVD, pulsed laser deposition (PLD), molecular beam epitaxy (MBE), and wet methods. In particular, it is preferable to form it by the ALD or sputtering method.
[0061] The semiconductor film 21f is preferably deposited by sputtering. In particular, hydrogen gas (H) is used as the deposition gas. 2It is preferable to use a sputtering method using ( ). By using hydrogen gas as the film deposition gas, the generation of crystal nuclei during the deposition of the semiconductor film 21f can be suppressed or the disappearance of crystal nuclei can be promoted. As a result, a semiconductor film 21f with low crystallinity can be deposited. It is preferable to use a mixed gas of a noble gas (typically argon) and hydrogen gas as the sputtering gas. In addition, it is preferable to use a noble gas or oxygen gas (O) as the film deposition gas. 2 It can be used alone, or a mixed gas containing a noble gas and oxygen gas can be used.
[0062] When depositing a semiconductor film 21f by sputtering, if the substrate temperature is high, there is a risk that the semiconductor film 21f may crystallize unintentionally. Therefore, a lower substrate temperature is preferable. For example, it is preferable to set the temperature of the stage on which the substrate is placed to room temperature or higher and 100°C or lower, preferably 25°C or higher and 80°C or lower, and more preferably 25°C or higher and 50°C or lower. Here, room temperature includes both controlling the temperature to be the same as room temperature and not controlling the temperature. If no temperature control is performed, the substrate temperature may rise above room temperature due to the energy supplied to the substrate during film deposition. Furthermore, since a lower substrate temperature is preferable, if the stage temperature can be controlled to a temperature lower than room temperature, it is preferable to deposit the film at a stage temperature below room temperature, as this can yield a semiconductor film 21f with lower crystallinity. For example, it is also possible to deposit the film at a stage temperature of liquid nitrogen temperature (-196°C) or higher and below 25°C. In this case, it is preferable to set the temperature higher than the dew point in the deposition chamber in order to prevent condensation on the stage.
[0063] The semiconductor film 21f can also be formed using the ALD method. By using the ALD method, which deposits atoms individually, rather than the sputtering method, which impacts the surface to be formed with particles, it is sometimes possible to suppress the formation of crystal nuclei in the film. This can suppress unintended polycrystallization of the semiconductor film 21f. On the other hand, the sputtering method allows for film formation at lower temperatures than the ALD method, and various gases can be used during film formation. For example, by applying a gas containing hydrogen as the film formation gas and forming the film at a low temperature (e.g., room temperature), a high-quality amorphous film with fewer crystal nuclei can be formed.
[0064] For the deposition of the semiconductor film 21f, an ALD method using, for example, a precursor and an oxidizing agent can be used. When forming a film containing indium as the semiconductor film 21f, an indium-containing precursor can be used. As for the ALD method, a thermal ALD method or a plasma-enhanced ALD (PEALD) method can be used.
[0065] Indium-containing precursors that can be used include trimethylindium, triethylindium, ethyldimethylindium, tris(1-methylethyl)indium, tris(2,2,6,6-tetramethyl-3,5-heptanedionic acid)indium, cyclopentadienylindium, indium(III) acetylacetonate, [3-(dimethylamino)propyl]dimethylindium, (diethylphosphino)dimethylindium, chlorodimethylindium, bromodimethylindium, and dimethyl(2-propanolat)indium.
[0066] Furthermore, inorganic precursors that do not contain hydrocarbons may be used as indium precursors. Examples of indium-containing inorganic precursors include halogenated indium compounds such as trifluoroindium (indium(III) fluoride), indium trichloride (indium(III) chloride), indium tribromide (indium(III) bromide), and indium triiodide (indium(III) iodide). Indium trichloride has a decomposition temperature of approximately 500°C to 700°C. Therefore, by using indium trichloride, film deposition by the ALD method can be performed while heating the substrate at approximately 400°C to 600°C, for example, at 500°C.
[0067] In the method for forming the semiconductor film 21f, it is preferable to use a material with a low impurity concentration, that is, a high-purity material. For example, the purity of the material to be used is 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 5N (99.999%) or higher, and further preferably 6N (99.9999%) or higher. By using a high-purity material, impurities in the semiconductor film 21f can be reduced.
[0068] The gallium content and the aluminum content in the indium-containing precursor can each be 1000 ppm or less, preferably 500 ppm or less, more preferably 100 ppm or less, further preferably 50 ppm or less, still further preferably 10 ppm or less, and even more preferably 1 ppm or less. By reducing the gallium concentration in the semiconductor film 21f, the reliability of the transistor can be improved. In addition, by reducing the aluminum concentration in the semiconductor film 21f, the crystallinity of the semiconductor film 21f can be improved. Further, by using a high-purity precursor, the composition of the obtained film can be easily controlled when the semiconductor film 21f is formed using two or more precursors.
[0069] Examples of the oxidizing agent include ozone (O 3 ), oxygen (O 2 ), water (H 2 O), nitrogen dioxide (NO 2 ), nitrous oxide (N 2 O), hydrogen peroxide (H 2 O 2 ), and the like, and two or more of these may be used.
[0070] In the case where a single crystal or a polycrystal with a large grain size is formed by a subsequent heat treatment, it is preferable to use an oxidizing agent containing hydrogen in order to suppress the generation of crystal nuclei at the initial stage of film formation. For example, H 2 O, or H 2 O 2 is preferably used. After forming a film with few crystal nuclei, crystal growth is performed by heat treatment, whereby a single crystal film or a polycrystalline film with a large grain size can be formed. On the other hand, when reducing the hydrogen concentration and the nitrogen concentration in the film, O 2 or O3 It is preferable to use O 3 It is preferable to use
[0071] Methods for controlling the composition of the resulting film include adjusting the flow rate ratio of the source gases, the duration of the source gas flow, and the order in which the source gases are flowed. By adjusting these factors, it is also possible to deposit films with continuously changing compositions. Furthermore, it becomes possible to deposit two or more films with different compositions in succession.
[0072] When introducing the precursor into the reaction chamber, the substrate heating temperature is preferably set to a temperature corresponding to the decomposition temperature of the precursor. In the case of a thermal ALD method using triethylindium as the indium-containing precursor, for example, the substrate heating temperature can be 100°C to 350°C, preferably 150°C to 300°C.
[0073] Next, a first heat treatment is performed to improve the crystallinity of the semiconductor film 21f (Figure 1C).
[0074] The heat treatment is carried out in an atmosphere of an inert gas such as nitrogen gas or a noble gas, or in an atmosphere containing 10 ppm (0.001%) or more, 1% or more, or 10% or more of an oxidizing gas. For example, when heat treatment is carried out in a mixed atmosphere of nitrogen gas and oxygen gas, it is preferable to have about 20% oxygen gas. For example, the heat treatment can be carried out under conditions where the flow rate ratio of nitrogen gas to oxygen gas introduced into the treatment chamber is 4:1. The heat treatment may also be carried out under reduced pressure. Alternatively, after heat treatment in an atmosphere of an inert gas such as nitrogen gas or a noble gas, heat treatment can be carried out in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas to replenish the desorbed oxygen.
[0075] Furthermore, it is preferable that the gas used in the above heat treatment is highly purified. For example, the amount of water contained in the gas used in the above heat treatment should be 1 ppb (1 × 10⁻¹⁶). −3A concentration of 0.1 ppb or less is preferred, 0.1 ppb or less is more preferred, and 0.05 ppb or less is even more preferred. By performing heat treatment using a highly purified gas, it is possible to prevent moisture and other substances from being incorporated into the semiconductor film 21f as much as possible.
[0076] There are no special limitations on the heating device used for the heat treatment; it may be a device that heats the object to be treated by heat conduction or thermal radiation from a heat source such as a resistance heating element. For example, an electric furnace or an RTA (Rapid Thermal Anneal) device such as an LRTA (Lamp Rapid Thermal Anneal) device or a GRTA (Gas Rapid Thermal Anneal) device can be used. An LRTA device is a device that heats the object to be treated by radiation of light (electromagnetic waves) emitted from a lamp such as a halogen lamp, metal halide lamp, xenon arc lamp, carbon arc lamp, high-pressure sodium lamp, or high-pressure mercury lamp. A GRTA device is a device that performs heat treatment using high-temperature gas.
[0077] The heat treatment can be performed at a temperature higher than the temperature at which the semiconductor film 21f crystallizes. When an indium oxide film is used for the semiconductor film 21f, crystallization occurs at 150°C or near that temperature, so it is preferable to perform the heat treatment at 150°C or a higher temperature. For example, the heat treatment can be performed at a temperature of 150°C to 1000°C, preferably 200°C to 800°C, and more preferably 250°C to 700°C. Furthermore, if the heating device is an electric furnace or other device with a relatively long processing time, it is preferable to heat at a relatively low temperature (for example, 200°C to 500°C). On the other hand, when using an RTA device, the heat treatment can be performed at a high temperature (for example, 600°C to 1000°C) in a short time. By using an RTA device and performing the heat treatment in a short time, the throughput of the heat treatment process can be improved, and manufacturing costs can be reduced.
[0078] In this process, the first heat treatment causes the semiconductor film 21f to crystallize, which rearranges the atoms within the film, relieving stress and reducing strain. Furthermore, the dramatic change in crystallinity can significantly alter the stress of the semiconductor film 21f itself. For example, if the semiconductor film 21f exhibits tensile stress at room temperature (e.g., 25°C) before the first heat treatment, it may exhibit compressive stress at room temperature after the first heat treatment. Conversely, depending on the material and composition of the semiconductor film 21f, the opposite may also occur.
[0079] Stress can be divided into two types: true stress, which originates from the structure of the thin film, and thermal stress, which originates from the difference in thermal expansion coefficients between the substrate and the thin film. Here, the first heat treatment changes the crystal structure of the thin film, so both true stress and thermal stress change. Therefore, as mentioned above, not only the magnitude of the stress but also its direction (tensile stress or compressive stress) may change before and after the first heat treatment.
[0080] Here, it is preferable that the absolute value of the stress of the semiconductor film 21f at room temperature (e.g., 25°C) after the first heat treatment is smaller than the absolute value of the stress at room temperature before the first heat treatment. For example, the stress can be adjusted by the thickness of the semiconductor film 21f, the film deposition conditions, etc. Furthermore, by making the semiconductor film 21f a stacked structure of two or more layers, and each layer having a different composition or film deposition conditions, the absolute value of the stress of the semiconductor film 21f at room temperature after the first heat treatment can be adjusted to be smaller.
[0081] For example, an indium oxide film and a gallium-doped indium oxide film can be stacked as the semiconductor film 21f. By adding gallium to indium oxide, the crystallinity decreases, so a film with a different stress magnitude than the indium oxide film can be obtained. Therefore, by stacking an indium oxide film and a gallium-doped indium oxide film, the stress of the semiconductor film 21f at room temperature can be made 0 Pa or close to 0 Pa. As a result, a semiconductor film 21f with extremely low strain can be obtained, and by applying such a semiconductor film 21f, a transistor with good electrical characteristics and high reliability can be realized.
[0082] Furthermore, the semiconductor film 21f can be configured by stacking multiple oxide films. For example, a three-layer structure can be formed with a first film, a second film, and a third film from the insulating layer 12 side. In this case, it is preferable to use indium oxide for the second film. Moreover, it is preferable to use films for the first and third films that contain materials with a wider band gap than the second film. For example, the first and third films can each contain a first element and oxygen. In this case, it is preferable that the first element is one or more selected from indium, gallium, and zinc.
[0083] Furthermore, it is preferable to provide a fourth film between the first film and the second film. In this case, it is preferable to use a fourth film with a wider band gap than the second film. For example, it is preferable to use a film containing indium, gallium, zinc, and oxygen for the first film, and a film containing gallium and oxygen for the fourth film.
[0084] Next, the semiconductor film 21f is processed into island shapes to form a semiconductor layer 21 (Figure 1D). For example, a resist mask can be formed on the semiconductor film 21f, and the parts of the semiconductor film 21f not covered by the resist mask can be removed by etching, and then the resist mask can be removed to form the semiconductor layer 21.
[0085] Next, an insulating layer 22 is formed in contact with the semiconductor layer 21 to serve as a gate insulating layer (Figure 1D).
[0086] It is preferable to use a film having the hydrogen gettering function described above as the insulating layer 22. This allows hydrogen in the semiconductor layer 21 to be captured not only on the insulating layer 12 side but also on the insulating layer 22 side by the subsequent second heat treatment.
[0087] Furthermore, it is preferable to use the above-mentioned oxide film with high oxygen permeability as the insulating layer 22. This allows oxygen contained in the insulating layer 31, which will be formed later, to be effectively supplied to the channel formation region of the semiconductor layer 21 via the insulating layer 22.
[0088] The insulating layer 22 is preferably made by laminating a film that has the function of getting hydrogen and a film with high oxygen diffusivity.
[0089] Next, a conductive layer 23, which functions as a gate electrode, is formed on the insulating layer 22 (Figure 1D). For example, after depositing a conductive film that will become the conductive layer 23 on the insulating layer 22, the conductive layer 23 can be formed by removing unnecessary parts by etching, similar to the semiconductor layer 21. At this time, the conductive film and the insulating layer 22 may be etched continuously to expose a part of the semiconductor layer 21.
[0090] Next, an insulating layer 31 is formed by covering the semiconductor layer 21, the insulating layer 22, and the conductive layer 23 (Figure 1E). The insulating layer 31 functions as an interlayer insulating layer.
[0091] As the insulating layer 31, it is preferable to use an oxide film that releases oxygen upon heating as described above. Alternatively, as the insulating layer 31, a film with low oxygen permeability (high oxygen barrier properties) may be laminated on the oxygen-releasing film. For example, insulating films containing silicon nitride, aluminum oxide, hafnium oxide, yttrium oxide, zirconium oxide, etc., can be used. This prevents oxygen from being released to the outside from the top surface during the subsequent second heat treatment, making it possible to efficiently supply oxygen to the semiconductor layer 21.
[0092] Furthermore, after the formation of the insulating layer 31, a process to supply oxygen to the insulating layer 31 may be performed. Examples of oxygen supply processes include heating in an oxygen-containing atmosphere and plasma treatment (including microwave treatment) in an oxygen-containing atmosphere. Alternatively, oxygen may be supplied to the insulating layer by forming an oxide film (preferably a metal oxide film) in an oxygen-containing atmosphere using a sputtering method. The formed oxide film may be removed immediately or left as is. The oxygen-containing atmosphere may be oxygen gas (O 2 ) as well as ozone (O 3 ), nitrous oxide (N 2 The atmosphere includes an atmosphere containing oxygen-containing compound gases such as O).
[0093] Furthermore, when the insulating layer 31 consists of a film that releases oxygen and a film with low oxygen permeability laminated on top of it, it is preferable to perform the oxygen supply treatment on the first layer. Alternatively, a metal oxide film such as an aluminum oxide film may be used as the oxide film for supplying oxygen and used as is as the second layer.
[0094] Next, a second heat treatment is performed (Figure 1E). For the method of the heat treatment, refer to the description of the first heat treatment above.
[0095] The second heat treatment releases hydrogen (hydrogen H in the figure) contained in the semiconductor layer 21 to the insulating layer 12 or insulating layer 22, where it is gettered. This reduces the hydrogen concentration in the semiconductor layer 21. Furthermore, the second heat treatment supplies oxygen (oxygen O in the figure) from the insulating layer 31 to the semiconductor layer 21 either directly or via the insulating layer 22. This compensates for oxygen deficiencies in the semiconductor layer 21. In this way, the second heat treatment reduces impurities and defects in the semiconductor layer 21.
[0096] Here, the region of the semiconductor layer 21 that overlaps with the conductive layer 23 functions as a channel formation region. This example shows that the insulating layer 22 is provided in a position that overlaps with the channel formation region. By the insulating layer 22 being in contact with the channel formation region of the semiconductor layer 21, hydrogen in the channel formation region of the semiconductor layer 21 can be effectively reduced, and a large amount of oxygen can be selectively supplied to the channel formation region of the semiconductor layer 21 via the insulating layer 22.
[0097] In this example, the second heat treatment is performed after the formation of the insulating layer 31. However, depending on the transistor structure, the gate insulating layer and gate electrode may be formed after forming an insulating layer that releases oxygen, such as the insulating layer 31. In this case, the heat generated during the formation of the gate insulating layer, or the heat generated during the formation of the conductive film that forms the gate electrode, may be combined with the second heat treatment. Even in this case, it is preferable to perform the second heat treatment after the formation of the gate electrode.
[0098] The above is a description of the method for manufacturing semiconductor devices. According to the manufacturing method described here, by first forming a semiconductor film with high crystallinity and good electrical properties through a first heat treatment, and then reducing defects and impurities in the semiconductor layer through a second heat treatment, it is possible to realize a transistor with extremely good electrical properties and high reliability. At this time, it is preferable to perform the first heat treatment at a higher temperature than the second heat treatment. Since the first heat treatment is performed before forming the conductive layer that will become the electrodes of the transistor, it is possible to perform the treatment at a relatively high temperature. Therefore, the crystallinity of the semiconductor layer can be further improved. In addition, by performing the second heat treatment at a lower temperature, for example, at a lower temperature than the first heat treatment, oxidation of conductive layers such as gate electrodes can be suppressed.
[0099] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0100] (Embodiment 2) This embodiment describes an example of the configuration of a semiconductor device according to one aspect of the present invention, and an example of a method for manufacturing the same. Here, a transistor will be described as an example of a semiconductor device.
[0101] [Example of semiconductor device configuration] Figures 2A to 2D are top view and cross-sectional view of transistor 200. Figure 2A is a top view of transistor 200, and Figures 2B to 2D are schematic cross-sectional views corresponding to the cutting lines A1-A2, A3-A4, and A5-A6 in Figure 2A, respectively. Figure 2B corresponds to the cross-section of transistor 200 in the channel length direction, and Figures 2C and 2D correspond to the cross-section in the channel width direction, respectively. Figure 3A is an enlarged view of Figure 2B. Note that some of the components shown in Figure 3A are omitted in Figures 2B and 2D.
[0102] The transistor 200 includes a substrate 210, an insulating layer 201 provided on the substrate 210, a semiconductor layer 230 provided on the insulating layer 201, conductive layers 242a and 242b on the semiconductor layer 230, an insulating layer 250 on the semiconductor layer 230, and a conductive layer 260 on the insulating layer 250. An insulating layer 275 is provided covering the semiconductor layer 230, the conductive layer 242a, and the conductive layer 242b, and an insulating layer 280 is provided on the insulating layer 275. The insulating layer 280 and the insulating layer 275 are provided with grooves that reach the semiconductor layer 230, and the conductive layer 242a and the conductive layer 242b are separated by these grooves. The insulating layer 250 is provided inside the grooves along the surfaces of the insulating layer 280, the insulating layer 275, the conductive layer 242a, the conductive layer 242b, and the semiconductor layer 230. The conductive layer 260 is provided on the insulating layer 250 so as to fill the groove. In addition, insulating layers 282, 283, and 285 are provided in order to cover the insulating layer 280, insulating layer 250, and conductive layer 260. Furthermore, an insulating layer 271a is provided on the conductive layer 242a, and an insulating layer 271b is provided on the conductive layer 242b.
[0103] The semiconductor layer 230 functions as the channel formation region of the transistor 200. The conductive layer 260 functions as the gate electrode of the transistor 200. The insulating layer 250 functions as the gate insulating layer of the transistor 200. The conductive layer 242a functions as either the source electrode or the drain electrode of the transistor 200, and the conductive layer 242b functions as the other.
[0104] The semiconductor layer 21 exemplified in Embodiment 1 can be applied to the semiconductor layer 230. The insulating layer 22 can be applied to the insulating layer 250, and the conductive layer 23 can be applied to the conductive layer 260. The insulating layer 12 can be applied to the insulating layer 201.
[0105] It is preferable that the conductive layers 242a and 242b have a laminated structure. It is preferable to use a conductor that is resistant to oxidation, such as a metal nitride, on the side in contact with the semiconductor layer 230. This prevents the conductive layers 242a and 242b from being excessively oxidized by the oxygen contained in the semiconductor layer 230. It is also preferable to use a metal or alloy with higher conductivity than the layer in contact with the semiconductor layer 230 on the side that does not contact the semiconductor layer 230. This allows the conductive layers 242a and 242b to function as highly conductive wiring or electrodes.
[0106] In the conductive layers 242a and 242b, it is preferable to use a metal nitride on the side in contact with the semiconductor layer 230. For example, it is preferable to use a tantalum nitride, a titanium nitride, a molybdenum nitride, a tungsten nitride, a tantalum and aluminum nitride, or a titanium and aluminum nitride. Alternatively, for example, ruthenium, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel may be used. These materials are preferred because they are conductive materials that are resistant to oxidation or maintain conductivity even when absorbing oxygen.
[0107] The insulating layer 201 is a film in contact with the semiconductor layer 230, and it is preferable to use an oxide insulating film. For example, it is preferable to use silicon oxide or silicon oxide nitride as the insulating layer 201. Alternatively, silicon nitride, silicon nitride, aluminum oxide, hafnium oxide, gallium oxide, yttrium oxide, or zirconium oxide can be used as the insulating layer 201.
[0108] Furthermore, an insulating layer that functions as a barrier layer may be provided between the insulating layer 201 and the semiconductor layer 230, or between the insulating layer 201 and the substrate 210. Preferably, the insulating layer has barrier properties against hydrogen. Examples of hydrogen barrier layers include oxides such as aluminum oxide, hafnium oxide, and tantalum oxide, and nitrides such as silicon nitride. This makes it possible to keep the hydrogen concentration in the semiconductor layer 230 low, thereby improving the reliability of the transistor 200.
[0109] It is preferable to use a metal oxide (also called an oxide semiconductor) that functions as a semiconductor for the semiconductor layer 230.
[0110] The band gap of the metal oxide functioning as a semiconductor is preferably 2 eV or more, and more preferably 2.5 eV or more. By using a metal oxide with a large band gap, the off-current of the transistor can be reduced. A transistor having a metal oxide in the channel formation region in this way is called an OS (Oxide Semiconductor) transistor. Because OS transistors have a small off-current, the power consumption of semiconductor devices can be significantly reduced. In addition, because OS transistors have high frequency characteristics, semiconductor devices can be operated at high speeds.
[0111] It is preferable to use indium oxide as the semiconductor layer 230. In particular, it is preferable to use a single-crystal indium oxide film. It is preferable to use a crystalline film for the semiconductor layer 230, and it is particularly preferable to use indium oxide with a single-crystal structure, but it is also possible to use indium oxide with a polycrystalline or microcrystalline structure. By using indium oxide with a single-crystal structure, carrier scattering at the grain boundaries can be suppressed, and a transistor with high field-effect mobility can be realized. Furthermore, a highly reliable transistor can be realized.
[0112] When using indium oxide having a polycrystalline structure, it is preferable that no grain boundaries are observed, at least in the channel-forming region (the region superimposed on the conductive layer 260). This allows indium oxide having a polycrystalline structure to achieve the same effects as when it has a single-crystal structure.
[0113] The thickness of the semiconductor layer 230 is more preferably 2 nm to 50 nm, more preferably 2.5 nm to 30 nm, more preferably 2.5 nm to 20 nm, more preferably 5 nm to 20 nm, and even more preferably 5 nm to 10 nm. By setting the thickness of the semiconductor layer 230 within the above range, the crystallinity of the semiconductor layer 230 can be improved.
[0114] Among highly crystalline oxide semiconductors, indium oxide is a film in which hydrogen and / or oxygen can move more easily compared to, for example, an IGZO film. Therefore, indium oxide can be said to be a film in which hydrogen and / or oxygen can be easily supplied and expelled compared to, for example, an IGZO film. As a result, excess oxygen or excess hydrogen that can become carriers or fixed charges is less likely to accumulate in the semiconductor layer 230, making it possible to create a transistor with good electrical characteristics and reliability.
[0115] It is preferable that the semiconductor layer 230 has a reduced concentration of elements that decrease crystallinity. For example, the concentration of elements such as boron and aluminum is preferably 1 atomic percent or less, more preferably 0.1 atomic percent or less, and even more preferably 0.01 atomic percent (100 ppm) or less.
[0116] Furthermore, because gallium has a tendency to bond with excess oxygen atoms, if a large amount of gallium is present, the fluctuation in the threshold voltage in the PBTS (Positive Bias Temperature Stress) test may become large. For this reason, the gallium concentration in the semiconductor layer 230 is preferably 1 atomic percent or less, more preferably 0.1 atomic percent or less, and even more preferably 0.01 atomic percent (100 ppm) or less.
[0117] In addition, metal oxides that can be used in the semiconductor layer 230 include tin oxide, zinc oxide, indium tin oxide, indium titanium oxide, indium gallium oxide, indium tungsten oxide, indium zinc oxide, indium gallium aluminum oxide, indium gallium tin oxide, gallium zinc oxide, aluminum zinc oxide, indium aluminum zinc oxide, indium tin zinc oxide, indium titanium zinc oxide, indium gallium zinc oxide, indium gallium tin zinc oxide, and indium gallium aluminum zinc oxide. Alternatively, silicon-containing indium tin oxide, gallium tin oxide, aluminum tin oxide, etc., can also be used. When using these, it is preferable that the film has at least crystalline properties, and more preferably that it has a single-crystal structure.
[0118] The insulating layer 250, which functions as a gate insulating layer, preferably has the function of getting hydrogen. This reduces the hydrogen concentration in the channel formation region of the semiconductor layer 230. This makes it possible to make the channel formation region i-type or substantially i-type.
[0119] In this case, the insulating layer 250 is preferably a laminated structure comprising a first layer in contact with the semiconductor layer 230, a second layer on the first layer, and a third layer on the second layer. In this case, it is preferable that the first layer has a hydrogen gettering function.
[0120] Examples of insulators that have the function of getting hydrogen include metal oxides having an amorphous structure. It is preferable to use a metal oxide as the first layer, such as magnesium oxide, or an oxide containing one or both of aluminum and hafnium. In such amorphous metal oxides, oxygen atoms have dangling bonds, and these dangling bonds may have the property of getting hydrogen. In other words, amorphous metal oxides have a high ability to get hydrogen.
[0121] Furthermore, it is preferable to use a high-dielectric constant (high-k) material for the first layer. An example of a high-k material is an oxide containing either or both aluminum and hafnium. By using a high-k material as the first layer, it becomes possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulating layer. Additionally, it becomes possible to thin the equivalent oxide thickness (EOT) of the insulator that functions as the gate insulating layer.
[0122] It is preferable to use an oxide containing one or both of aluminum and hafnium as the first layer, and it is more preferable to use an oxide having an amorphous structure that contains one or both of aluminum and hafnium, and it is even more preferable to use aluminum oxide having an amorphous structure.
[0123] Next, it is preferable to use an insulator with a thermally stable structure, such as silicon oxide or silicon oxide-nitride, for the second layer.
[0124] Alternatively, a structure may be provided in which a fourth layer is placed on top of the second layer. In this case, the fourth layer can be an insulator that can be used for the first layer. For example, hafnium oxide can be used as the fourth layer. By providing the fourth layer between the third layer and the second layer, hydrogen contained in the second layer and the like can be more effectively gettered.
[0125] The third layer preferably has oxygen barrier properties. The third layer is provided between the channel-forming region of the semiconductor layer 230 and the conductive layer 260, and between the insulating layer 280 and the conductive layer 260. This configuration suppresses the diffusion of oxygen contained in the channel-forming region of the semiconductor layer 230 into the conductive layer 260, thereby preventing the formation of oxygen vacancies in the channel-forming region of the semiconductor layer 230. Furthermore, it suppresses the diffusion of oxygen contained in the semiconductor layer 230 and the oxygen contained in the insulating layer 280 into the conductive layer 260, thereby preventing the oxidation of the conductive layer 260. The third layer preferably has lower oxygen permeability than at least the insulating layer 280. For example, it is preferable to use a silicon nitride film as the third layer. In this case, the third layer is an insulator containing at least nitrogen and silicon.
[0126] Furthermore, it is preferable that the third layer has hydrogen barrier properties. This prevents impurities such as hydrogen contained in the conductive layer 260 from diffusing into the semiconductor layer 230.
[0127] The insulating layer 275 preferably has barrier properties against oxygen. The insulating layer 275 is provided between the insulating layer 280 and the conductive layer 242a, and between the insulating layer 280 and the conductive layer 242b. This configuration suppresses the diffusion of oxygen contained in the insulating layer 280 into the conductive layers 242a and 242b. Therefore, it is possible to suppress the oxidation of the conductive layers 242a and 242b by oxygen contained in the insulating layer 280, which increases their resistivity and reduces the on-current. The insulating layer 275 preferably has lower oxygen permeability than at least the insulating layer 280. For example, silicon nitride is preferably used as the insulating layer 275. In this case, the insulating layer 275 is an insulator having at least nitrogen and silicon.
[0128] Furthermore, in this embodiment, it is preferable to configure the semiconductor device to suppress the ingress of hydrogen into the transistor 200, etc., in addition to the above configuration. For example, it is preferable to provide an insulator having the function of suppressing hydrogen diffusion so as to cover the transistor 200. In the semiconductor device described in this embodiment, the insulator is, for example, an insulating layer 282 and an insulating layer 283. Alternatively, a similar film may be provided under the transistor 200.
[0129] Preferably, one or more of the insulating layers 282 and 283 have barrier properties against water, hydrogen, etc. Alternatively, they preferably have barrier properties against oxygen.
[0130] The insulating layer 282 and insulating layer 283 can be made of, for example, aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, silicon nitride, or silicon nitride oxide, respectively. For example, it is preferable to use silicon nitride, which has higher hydrogen barrier properties, as the insulating layer 283. Also, for example, it is preferable that the insulating layer 282 has aluminum oxide, hafnium oxide, or magnesium oxide, which have high hydrogen gettering properties. This suppresses the diffusion of impurities such as water and hydrogen from the interlayer insulating film located outside the insulating layer 283 to the transistor 200, etc. It also suppresses the diffusion of oxygen contained in the insulating layer 280, etc., upward from the transistor 200, etc., via the insulating layer 282, etc. Furthermore, by providing a film similar to one or both of the insulating layers 282 and 283 below the transistor 200, it is possible to suppress the diffusion of impurities such as water and hydrogen from the substrate side to the transistor 200, etc.
[0131] The insulating layers 271a and 271b are inorganic insulators that function as etching stoppers during processing of the conductive layers 242a and 242b, protecting them. Furthermore, since the insulating layers 271a and 271b are in contact with the conductive layers 242a and 242b, it is preferable that they are inorganic insulators that do not easily oxidize the conductive layers 242a and 242b. For example, the insulating layers 271a and 271b can be arranged in a laminated structure, with silicon nitride used on the side in contact with the conductive layers 242a and 242b, and silicon oxide used on the other sides.
[0132] Insulating layers 285, 283, 282, 280, 275, and 271a have openings that reach the conductive layer 242a, and the conductive layer 240a and insulating layer 241a are provided within these openings. An insulating layer 241a is provided adjacent to the side wall of the opening, and the conductive layer 240a is provided inside the insulating layer 241a. In addition, insulating layers 285, 283, 282, 280, 275, and 271b have openings that reach the conductive layer 242b, and the conductive layer 240b and insulating layer 241b are provided within these openings. An insulating layer 241b is provided adjacent to the side wall of the opening, and the conductive layer 240b is provided inside the insulating layer 241b. The conductive layers 240a and 240b function as vias (also called plugs) that connect wiring and the like provided on the transistor 200 to the source or drain of the transistor 200.
[0133] The conductive layers 240a and 240b are preferably made of conductive materials mainly composed of tungsten, copper, or aluminum. The conductive layers 240a and 240b may also be arranged in a laminated structure.
[0134] For example, as shown in Figure 3A, the conductive layer 240a and conductive layer 240b may be arranged in a two-layer laminated structure. The conductive layer 240a has a conductive layer 240a1 formed along the opening and a conductive layer 240a2 formed inside the conductive layer 240a1. The conductive layer 240b has a conductive layer 240b1 formed along the opening and a conductive layer 240b2 formed inside the conductive layer 240b1.
[0135] It is preferable to use conductive materials such as tantalum, tantalum nitride, titanium, titanium nitride, ruthenium, or ruthenium oxide for conductive layers 240a1 and 240b1, which are resistant to the diffusion of impurities such as water and hydrogen. These conductive materials may be used as single layers or in laminates. By providing conductive layers 240a1 and 240b1, it is possible to suppress the incorporation of impurities such as water and hydrogen into the semiconductor layer 230 through conductive layers 240a2 and 240b2. The conductive layers 240a2 and 240b2 may be made of conductive materials that can be used for conductive layers 240a and 240b described above.
[0136] Furthermore, as shown in Figure 2B, the upper surfaces of the conductive layers 240a and 240b can be formed to coincide with or substantially coincide with the upper surface of the insulating layer 285. Also, as shown in Figure 3A, the lower part of the conductive layer 240a may be formed to be embedded in the conductive layer 242a. Similarly, the lower part of the conductive layer 240b may be formed to be embedded in the conductive layer 242b.
[0137] As insulating layers 241a and 241b, any barrier insulator that can be used for insulating layer 275, etc., may be used. For example, silicon nitride may be used as insulating layer 241a and insulating layer 241b. Insulating layers 241a and 241b are provided in contact with insulating layers 285, 283, 282, 275, 271a, and 271b. This makes it possible to suppress the mixing of impurities such as water and hydrogen contained in insulating layer 280, etc., into semiconductor layer 230 through conductive layer 240a and conductive layer 240b. Silicon nitride is particularly suitable because it has high barrier properties against hydrogen. In addition, it is possible to prevent oxygen contained in insulating layer 280 from being absorbed by conductive layer 240a and conductive layer 240b.
[0138] The conductive layer 260 functions as the gate electrode of the transistor 200. Here, it is preferable that the conductive layer 260 extends in the channel width direction, as shown in Figures 2A and 2C. With this configuration, when multiple transistors are provided, the conductive layer 260 functions as wiring.
[0139] The conductive layer 260 may have a laminated structure. Figure 3A shows an example in which the conductive layer 260 has a conductive layer 260a located on the side in contact with the insulating layer 250 and a conductive layer 260b above it. In this case, it is preferable to use a conductive material that is resistant to oxidation, such as titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, or ruthenium oxide, or a conductive material that has the function of suppressing oxygen diffusion, for the conductive layer 260a. It is also preferable to use a conductive material with low resistance, such as tungsten, copper, or aluminum, for the conductive layer 260 (or conductive layer 260a). In addition, it is preferable to use a conductive material with a large work function, such as cobalt, nickel, gold, copper, or platinum, as the conductive layer 260 (or conductive layer 260a), because it shifts the threshold voltage of the transistor positively and makes it easier to realize a transistor with normally-off characteristics.
[0140] The insulating layer 280 preferably has a low dielectric constant. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance between wirings can be reduced. For example, the insulating layer 280 preferably has one or more of the following: silicon oxide, silicon oxynitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, and silicon oxide with vacancies. Silicon oxide and silicon oxynitride are preferred because they are thermally stable. In particular, materials such as silicon oxide, silicon oxynitride, and silicon oxide with vacancies are preferred because they can easily form regions containing oxygen that is desorbed by heating.
[0141] Next, we will explain the configuration of the semiconductor layer 230.
[0142] Figure 4A shows an enlarged view of the channel formation region and its vicinity in Figure 3A. Figure 4A shows an example where the semiconductor layer 230 has a single-layer structure.
[0143] Figure 4B shows an example where the semiconductor layer 230 has a two-layer structure consisting of an oxide layer 230a and an oxide layer 230b. Here, an example is shown where the current mainly flows through the oxide layer 230b, and the oxide layer 230a is shown with a different hatching pattern than the oxide layer 230b.
[0144] For the oxide layer 230a, a material with a wider band gap than the oxide layer 230b, or a material with lower conductivity than the oxide layer 230b, can be used. For example, if an indium oxide film is used for the oxide layer 230b, the oxide layer 230a can be selected from among the metal oxides that can be used for the semiconductor layer 230 described above, excluding indium oxide. For example, it is preferable to use a metal oxide film containing metal elements such as gallium, zinc, aluminum, titanium, and tungsten for the oxide layer 230a. More specific examples include gallium oxide, indium gallium oxide, indium gallium zinc oxide, indium titanium oxide, indium tungsten oxide, indium zinc oxide, indium gallium aluminum oxide, indium gallium tin oxide, gallium zinc oxide, aluminum zinc oxide, indium aluminum zinc oxide, and indium titanium zinc oxide.
[0145] Furthermore, it is preferable to use a metal oxide film for the oxide layer 230a that can take on a crystalline structure that serves as a seed crystal for the oxide layer 230b, which functions as a channel. This makes it possible to make the oxide layer 230b a film having a single-crystal structure or a polycrystalline structure with a large grain size, thereby realizing a transistor that combines reliability and good electrical characteristics.
[0146] Here, the crystal structure of indium oxide is cubic (Bixbite type). Therefore, it is preferable to use a metal oxide film that can adopt the same cubic crystal structure (more preferably Bixbite type) as indium oxide for the oxide layer 230a. This allows the indium oxide film to be epitaxially grown on the oxide layer 230a.
[0147] Alternatively, the crystal structure of the oxide layer 230a does not have to be the same as that of the indium oxide in terms of crystal system or crystal orientation. For example, a film having a hexagonal or trigonal crystal structure can be used. For example, by setting the crystal orientation of the surface of the oxide layer 230a to
[001] and the crystal orientation of the lower surface of the indium oxide film to
[111] , the requirements related to crystal orientation necessary for epitaxial growth can be met. Examples of hexagonal or trigonal crystals include wurtzite-type structure, YbFe 2 O 4 Type structure, Yb 2 Fe 3 O 7 These include type structures and their modified type structures. YbFe 2 O 4 Type structure or Yb 2 Fe 3 O 7 An example of a crystal having a crystalline structure is In-Ga-Zn oxide (IGZO).
[0148] Figure 4C shows an example in which the semiconductor layer 230 has a two-layer structure in which an oxide layer 230b that functions as a channel and an oxide layer 230c stacked on top of it are shown.
[0149] As the oxide layer 230c, a material with a wider band gap than oxide layer 230b, similar to the oxide layer 230a, or a material with lower conductivity than oxide layer 230b, can be used.
[0150] When the oxide layer 230b and the insulating layer 250, which functions as a gate insulating layer, are in contact, carriers may be trapped at their interface, potentially leading to fluctuations in the threshold voltage and a decrease in reliability. Therefore, by providing an oxide layer 230c between the oxide layer 230b and the insulating layer 250, the current path can be moved away from the interface between the insulating layer 250 and the semiconductor layer 230, thereby suppressing the effects of the aforementioned carrier trap and improving reliability.
[0151] Figure 4D shows an example in which the semiconductor layer 230 has a three-layer structure consisting of an oxide layer 230a, an oxide layer 230b, and an oxide layer 230c.
[0152] For example, the oxide layer 230a can be made of a gallium oxide film or an In-Ga-Zn oxide film, the oxide layer 230b can be made of an indium oxide film, and the oxide layer 230c can be made of a gallium oxide film or an In-Ga-Zn oxide film.
[0153] Furthermore, as shown in Figure 4E, the oxide layer 230a may have a two-layer structure. Figure 4E shows an example in which the oxide layer 230a has a two-layer structure consisting of oxide layer 230a1 and oxide layer 230a2.
[0154] In this case, oxide layers 230a1 and 230a2 can be made of materials that can be used for oxide layer 230a, which have a wider band gap than oxide layer 230b, or materials that have lower conductivity than oxide layer 230b.
[0155] For example, the oxide layer 230a1 can be made of either a gallium oxide film or an In-Ga-Zn oxide film, the oxide layer 230a2 can be made of the other of the gallium oxide film or an In-Ga-Zn oxide film, the oxide layer 230b can be made of an indium oxide film, and the oxide layer 230c can be made of either a gallium oxide film or an In-Ga-Zn oxide film.
[0156] The above is a description of the configuration of the semiconductor layer 230.
[0157] [Variations] The following describes an example with some configuration differences from the above example. Note that the following explanation omits parts that overlap with the above.
[0158] Figure 3B shows an example having a conductive layer 205 that functions as a back gate. The configuration shown in Figure 3B has a conductive layer 205 and an insulating layer 202.
[0159] The conductive layer 205 is provided so as to be embedded in the insulating layer 202. The insulating layer 201 is provided so as to cover the insulating layer 202 and the conductive layer 205.
[0160] The conductive layer 205 functions as the second gate (back gate) of the transistor 200. The conductive layer 205 is provided in a region that overlaps with the conductive layer 260 via the semiconductor layer 230.
[0161] The conductive layer 205 can be made of a material that can be used for the conductive layer 260. Furthermore, the conductive layer 205 may have a laminated structure.
[0162] In this case, the insulating layer 201 functions as a second gate insulating layer. In this case, it is preferable to have a laminated structure for the insulating layer 201 and to use a high dielectric constant material such as hafnium oxide, aluminum oxide, or hafnium aluminate in part thereof.
[0163] The insulating layer 202 can be made of a silicon oxide film. It is preferable to provide an insulating film, such as silicon nitride or aluminum oxide, which has barrier properties against oxygen, between the insulating layer 202 and the conductive layer 205, as this can suppress oxidation of the conductive layer 205. Alternatively, the conductive layer 205 may be made of a laminated structure of a film containing a nitride such as titanium nitride or tantalum nitride and a film containing a low-resistance metal such as tungsten or copper, thereby suppressing oxidation of the conductive layer 205.
[0164] The conductive layer 260, which functions as the first gate (front gate), and the conductive layer 205, which functions as the second gate, may be supplied with the same signal (or potential), or they may be supplied with different signals (or potentials). Furthermore, the conductive layer 205 may be connected to the conductive layer 242a or the conductive layer 242b.
[0165] [Modification 2] Figures 5A to 5D show examples of transistor 200 configurations that differ in some aspects from the above. Figure 5A is a top view, and Figures 5B to 5D are cross-sectional views. The configurations shown in Figures 5A to 5D differ from the above configuration mainly in that they have an insulating layer 255. In addition, the insulating layer 250 is in contact with the side surface of the insulating layer 255.
[0166] Here, conductive layers 242a and 242b are shown as having a two-layer structure. Conductive layer 242a has a laminated structure consisting of conductive layer 242a1 and conductive layer 242a2 on conductive layer 242a1. Conductive layer 242b has a laminated structure consisting of conductive layer 242b1 and conductive layer 242b2 on conductive layer 242b1.
[0167] The insulating layer 255 is positioned inside an opening formed in the insulating layer 280, etc., and is in contact with the side surface of the insulating layer 280, the side surface of the conductive layer 242a2, the side surface of the conductive layer 242b2, the upper surface of the conductive layer 242a1, the upper surface of the conductive layer 242b1, and the upper surface of the insulating layer 201 within the opening. In other words, the insulating layer 255 can be said to be formed in a sidewall shape in contact with the side wall of the opening formed in the insulating layer 280, etc. Here, the side wall of the opening corresponds, for example, to the side surface of the insulating layer 280, etc. within the opening.
[0168] The insulating layer 255 preferably has barrier properties against oxygen. The insulating layer 255 having barrier properties against oxygen suppresses oxidation of the sides of the conductive layers 242a and 242b, preventing the formation of an oxide film on those sides. This suppresses a decrease in the on-current of the transistor 200 or a decrease in the field-effect mobility. As the insulating layer 255, a barrier insulator that can be used for the insulating layer 275, etc., can be used. For example, silicon nitride can be used as the insulating layer 255.
[0169] The opening in the insulating layer 280 overlaps with the region between the conductive layer 242a2 and the conductive layer 242b2. In a top view, the side surface of the insulating layer 280 at the opening coincides with or substantially coincides with the side surface of the conductive layer 242a2 and the side surface of the conductive layer 242b2. Furthermore, parts of the conductive layer 242a1 and the conductive layer 242b1 are formed to protrude inward into the opening. In other words, in the conductive layer 242a1, the portion on which the insulating layer 255 is formed on the upper surface (hereinafter sometimes referred to as the protruding portion of the conductive layer 242a1) protrudes toward the conductive layer 260 from the conductive layer 242a2. Similarly, in the conductive layer 242b1, the portion on which the insulating layer 255 is formed on the upper surface (hereinafter sometimes referred to as the protruding portion of the conductive layer 242b1) protrudes toward the conductive layer 260 from the conductive layer 242b2.
[0170] Here, a portion of the upper surface of conductive layer 242a1 is in contact with conductive layer 242a2, and a portion of the upper surface of conductive layer 242b1 is in contact with conductive layer 242b2. Therefore, the insulating layer 255 is in contact with the other portion of the upper surface of conductive layer 242a1, the other portion of the upper surface of conductive layer 242b1, the side surface of conductive layer 242a2, and the side surface of conductive layer 242b2 inside the opening. In addition, the insulating layer 250 is in contact with the upper surface of semiconductor layer 230, the side surface of conductive layer 242a1, the side surface of conductive layer 242b1, and the side surface of insulating layer 255.
[0171] The insulating layer 255 is formed in a sidewall shape in contact with the side walls of the openings provided in the insulating layer 280 using anisotropic etching. The insulating layer 255 is formed in contact with the side surfaces of the conductive layer 242a2 and the conductive layer 242b2, and has the function of protecting the conductive layer 242a2 and the conductive layer 242b2.
[0172] [Modification 3] Figures 6A to 6D show examples of the configuration of the transistor 200 illustrated below. The configuration shown in Figures 6A to 6D differs from Modification 2 above mainly in that it does not have an insulating layer 255.
[0173] In the configuration without the insulating layer 255, a portion of the insulating layer 250 is positioned overlapping the protrusions of the conductive layer 242a1 and the conductive layer 242b1. In some cases, a portion of the conductive layer 260 is positioned overlapping the protrusions of the conductive layer 242a1 and the conductive layer 242b1. Here, the protrusions of the conductive layer 242a1 and the conductive layer 242b1 are in contact with the insulating layer 250. Also, the side surface of the insulating layer 250 is in contact with the side surface of the insulating layer 280, the side surface of the insulating layer 275, the side surface of the insulating layer 271a, the side surface of the insulating layer 271b, the side surface of the conductive layer 242a2, and the side surface of the conductive layer 242b2.
[0174] The portion of the insulating layer 250 that is positioned in the opening provided in the insulating layer 280 is formed to reflect the shape of the opening. Therefore, the insulating layer 250 is formed to reflect the shape of the conductive layer 242a1 and conductive layer 242b1 that protrude into the opening.
[0175] As shown in Figure 6B, in a cross-sectional view of the transistor 200 in the channel length direction, the distance between conductive layer 242a1 and conductive layer 242b1 is smaller than the distance between conductive layer 242a2 and conductive layer 242b2. This configuration allows for a shorter distance between the source and drain, and consequently, a shorter channel length. Therefore, the frequency characteristics of transistor 200 can be improved. In this way, by miniaturizing the semiconductor device, a semiconductor device with improved operating speed can be provided.
[0176] [Modification 4] The above describes a configuration in which the gate electrode is embedded, but the following describes a transistor with a different configuration.
[0177] Figure 7A shows a cross-sectional view of transistor 200a in the channel length direction. Transistor 200a has a semiconductor layer 230, an insulating layer 250, a conductive layer 260, a conductive layer 242a, and a conductive layer 242b.
[0178] An insulating layer 250 is provided covering the semiconductor layer 230, and a conductive layer 260 is provided on the insulating layer 250 at a position overlapping with the semiconductor layer 230. Furthermore, insulating layers 281 and 280 are laminated and provided covering the insulating layer 250 and the conductive layer 260. A pair of openings reaching the semiconductor layer 230 is provided in the insulating layer 281, insulating layer 280, and insulating layer 250, respectively. Conductive layers 242a and 242b are provided on the insulating layer 280 and are in contact with the semiconductor layer 230 at their respective openings.
[0179] As the insulating layer 281, an insulator having barrier properties against hydrogen and oxygen, similar to that of the insulating layer 275, can be used. This makes it possible to suppress the diffusion of impurities contained in the insulating layer 280 into the semiconductor layer 230, and the diffusion of oxygen contained in the semiconductor layer 230 towards the insulating layer 280.
[0180] The region of the semiconductor layer 230 that overlaps with the conductive layer 260 functions as a channel-forming region. Furthermore, a pair of regions 230n flanking the channel-forming region function as a source region or a drain region. It is preferable that regions 230n have lower resistance than the channel-forming region.
[0181] For example, region 230n preferably contains an element that imparts conductivity to the semiconductor layer 230. Examples of such elements include titanium, aluminum, tantalum, tungsten, tin, silicon, germanium, zirconium, hafnium, antimony, hydrogen, boron, and phosphorus. These elements can be introduced into a portion of the semiconductor layer 230 by methods such as doping, ion implantation, or thermal diffusion. For example, using the conductive layer 260 as a mask, the above elements can be introduced into a region of the semiconductor layer 230 that does not overlap with the conductive layer 260 via the insulating layer 250 by doping or ion implantation.
[0182] Figure 7B shows an example where the insulating layer 250 is located only in the region overlapping with the conductive layer 260 and is not provided on the region 230n of the semiconductor layer 230. In this case, by using a film containing the above-mentioned elements for the insulating layer 281 in contact with region 230n, the elements can be introduced into region 230n during the formation of the insulating layer 281 or by subsequent heat treatment. For example, it is preferable to use silicon nitride containing hydrogen for the insulating layer 281. Alternatively, oxides of the above-mentioned metal elements may be used.
[0183] The above is an explanation of the variations.
[0184] [Example of Manufacturing Method] Below, an example of a method for manufacturing a transistor according to one aspect of the present invention will be described. Here, the transistor 200 illustrated in Figures 2A to 2D above will be used as an example.
[0185] Figures 8A1, 8B1, 8C1, 8D1, 9A1, 9B1, and 9C1 are schematic cross-sectional views of each stage of the example manufacturing method described below, while Figures 8A2, 8B2, 8C2, 8D2, 9A2, 9B2, and 9C2 are perspective views. Note that the perspective views are partially cut off. Furthermore, in the perspective views, only the outlines of some components (such as the insulating layer) are shown with dashed lines.
[0186] First, an insulating layer 201 is formed on the substrate 210, followed by the formation of a semiconductor film 230f. The substrate 210, insulating layer 201, and semiconductor film 230f can be fabricated by referring to the methods for manufacturing the substrate 11, insulating layer 12, and semiconductor film 21f in Embodiment 1, respectively. Next, a first heat treatment is performed. The first heat treatment can improve the crystallinity of the semiconductor film 230f. Furthermore, by relieving the strain in the semiconductor film 230f through the first heat treatment, the generation of lattice defects in the semiconductor film can be suppressed, and a semiconductor film exhibiting good electrical properties can be obtained. For details on the first heat treatment, refer to the description in Embodiment 1.
[0187] Next, a conductive film 242f is deposited on the semiconductor film 230f (Figures 8A1 and 8A2). By depositing the conductive film 242f in contact with the semiconductor film 230f without an etching process after the semiconductor film 230f has been deposited, the upper surface of the semiconductor film 230f can be protected by the conductive film 242f. This suppresses the diffusion of impurities into the semiconductor layer 230 that constitutes the transistor, thereby improving the electrical characteristics and reliability of the semiconductor device.
[0188] The conductive film 242f can be deposited using sputtering, CVD, MBE, PLD, or ALD methods.
[0189] In this embodiment, tantalum nitride is deposited as the conductive film 242f using a sputtering method. A heat treatment may be performed before depositing the conductive film 242f. This heat treatment may be carried out under reduced pressure, and the conductive film 242f may be deposited continuously without exposure to the atmosphere. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the semiconductor film 230f can be removed, and the moisture and hydrogen concentrations in the semiconductor film 230f can be further reduced. The heat treatment temperature is preferably between 100°C and 400°C.
[0190] Next, the semiconductor film 230f and the conductive film 242f are processed into island-like structures using lithography to form the semiconductor layer 230 and the conductive layer 242 (Figures 8B1 and 8B2).
[0191] The above processing can be performed using either a dry etching method or a wet etching method. Dry etching is suitable for microfabrication. Furthermore, the semiconductor film 230f and the conductive film 242f may be processed under different conditions.
[0192] Alternatively, a layer that functions as a hard mask may be formed on the conductive film 242f. Using a hard mask is preferable because it improves processability and makes it easier to process into the desired shape.
[0193] In this case, it is preferable to process the semiconductor layer 230 and the conductive layer 242 together in an island shape. In this case, it is preferable that the side edge of the conductive layer 242 coincides with or substantially coincides with the side edge of the semiconductor layer 230. By adopting such a configuration, the number of processes for the semiconductor device according to one aspect of the present invention can be reduced. Therefore, a method for manufacturing a semiconductor device with good productivity can be provided.
[0194] As shown in Figure 8B1, the sides of the semiconductor layer 230 and the conductive layer 242 may be tapered. The taper angle of the sides of the semiconductor layer 230 and the conductive layer 242 can be, for example, 60° or more and less than 90°. By making the sides tapered in this way, the coverage of the insulating layer 275 and other components can be improved in subsequent processes, and defects such as porosity can be reduced.
[0195] In lithography, the resist is first exposed through a mask. Next, the exposed area is removed or left intact using a developer to form a resist mask. Then, by etching through this resist mask, conductors, semiconductors, or insulators can be processed into the desired shape. For example, a resist mask can be formed by exposing the resist using KrF excimer laser light, ArF excimer laser light, or EUV (Extreme Ultraviolet) light. Alternatively, immersion technology may be used, where a liquid (e.g., water) is filled between the substrate and the projection lens for exposure. In addition, an electron beam or ion beam may be used instead of the aforementioned light. When using an electron beam or ion beam, a mask may not be necessary in some cases.
[0196] Furthermore, the resist mask that is no longer needed after processing can be removed by dry etching, such as ashing using oxygen plasma (hereinafter sometimes referred to as oxygen plasma treatment), wet etching, wet etching after dry etching, or dry etching after wet etching.
[0197] Furthermore, a hard mask made of an insulator or conductor may be used beneath the resist mask. When a hard mask is used, an insulating film or conductive film that will serve as the hard mask material is formed on the conductive film 242f, a resist mask is formed on top of it, and a hard mask of the desired shape can be formed by etching the hard mask material. For example, tungsten may be used as the hard mask material. Etching of the conductive film 242f may be performed after removing the resist mask, or it may be performed while the resist mask is still in place. In the latter case, the resist mask may disappear during etching. The hard mask may also be removed by etching after etching of the semiconductor film 230f. On the other hand, if the hard mask material does not affect subsequent processes or can be used in subsequent processes, it is not always necessary to remove the hard mask.
[0198] Alternatively, a configuration may be used in which an SOC (Spin On Carbon) film and an SOG (Spin On Glass) film are deposited between the workpiece and the resist mask. By using the SOC film and SOG film as masks, the adhesion to the resist mask can be improved, and the durability of the mask pattern can be enhanced. For example, lithography can be performed by depositing the SOC film, SOG film, and resist mask in that order on the workpiece.
[0199] Next, an insulating layer 275 is formed to cover the semiconductor layer 230 and the conductive layer 242, and then an insulating layer 280 is formed on top of the insulating layer 275 (Figures 8C1 and 8C2).
[0200] Preferably, the insulating layer 280 is formed by creating an insulating film that will serve as the insulating layer 280, and then performing CMP treatment on the insulating film to form an insulator with a flat upper surface. Alternatively, silicon nitride may be deposited on the insulating layer 280, for example, by sputtering, and then CMP treatment may be performed on the silicon nitride until it reaches the insulating layer 280.
[0201] The insulating layer 275 and the insulating layer 280 can be formed using, for example, sputtering, CVD, MBE, PLD, or ALD.
[0202] It is preferable to use an insulator that has the function of suppressing oxygen permeation for the insulating layer 275. For example, it is preferable to deposit silicon nitride as the insulating layer 275 using the PEALD method. Alternatively, the insulating layer 275 may be configured by depositing aluminum oxide using the sputtering method and then depositing silicon nitride on top of it using the PEALD method. By making the insulating layer 275 such a structure, it is possible to improve the function of suppressing the diffusion of impurities such as water and hydrogen, and oxygen.
[0203] Furthermore, it is preferable to deposit silicon oxide as the insulating layer 280 using a sputtering method. By depositing the insulating film that will become the insulating layer 280 using a sputtering method in an oxygen-containing atmosphere, an insulating layer 280 containing excess oxygen can be formed. In addition, by using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 280 can be reduced. Before depositing the insulating film, a heat treatment may be performed. The heat treatment may be performed under reduced pressure, and the insulating film may be deposited continuously without exposure to the atmosphere. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the insulating layer 275 can be removed. The heat treatment conditions described above can be used for this heat treatment.
[0204] Next, the conductive layer 242, the insulating layer 275, and the insulating layer 280 are processed using lithography to form openings (also called grooves) that reach the semiconductor layer 230 and the insulating layer 201 (Figures 8D1 and 8D2). Here, the conductive layer 242 is divided to form conductive layers 242a and 242b. The openings formed in the insulating layers 280 and 275 overlap with the semiconductor layer 230.
[0205] Next, an insulating layer 250 is formed to cover the openings formed in the insulating layer 280 and the like. Here, the insulating layer 250 is formed along the openings in the insulating layer 280. The insulating layer 250 is in contact with the insulating layer 280, the conductive layer 242a, the conductive layer 242b, the insulating layer 201, and the semiconductor layer 230.
[0206] The insulating layer 250 can be formed using sputtering, CVD, MBE, PLD, or ALD. Since it is preferable to form the insulating layer 250 with a thin film thickness, it is preferable to form it using the ALD method, which has excellent coverage and allows for easy film thickness control.
[0207] Furthermore, when forming the insulating layer 250 using the ALD method, ozone (O) is used as the oxidizing agent. 3 ), oxygen (O 2 ), water (H 2 O) and other substances can be used. By using hydrogen-free substances such as ozone or oxygen as oxidizing agents, the amount of hydrogen diffusing into the semiconductor layer 230 can be reduced.
[0208] Furthermore, it is preferable to perform microwave treatment before, after, or during the formation of the insulating layer 250.
[0209] More specifically, microwave processing is preferably performed in an oxygen-containing atmosphere. Here, microwave processing refers to processing using, for example, a device having a power supply that generates high-density plasma using microwaves. Furthermore, in this specification, microwaves refer to electromagnetic waves having a frequency of 300 MHz or more and 300 GHz or less.
[0210] In microwave processing, it is preferable to use a microwave processing apparatus that has a power supply for generating high-density plasma using microwaves. The frequency of the microwave processing apparatus can typically be set to 2.45 GHz. By using high-density plasma, high-density oxygen radicals can be generated. Furthermore, the power of the power supply for applying microwaves to the microwave processing apparatus is preferably 1000 W to 10000 W, and preferably 2000 W to 5000 W. The microwave processing apparatus may also have a power supply for applying RF to the substrate side. Furthermore, by applying RF to the substrate side, oxygen ions generated by the high-density plasma can be efficiently guided into the semiconductor layer 230.
[0211] Furthermore, the microwave treatment described above is preferably carried out under reduced pressure, with a pressure of 10 Pa to 1000 Pa, and more preferably 300 Pa to 700 Pa. The treatment temperature is preferably 750°C or lower, more preferably 500°C or lower, and can be, for example, around 250°C. In addition, after the oxygen plasma treatment, a continuous heat treatment may be performed without exposure to the outside air. The heat treatment temperature is preferably, for example, 100°C to 750°C, and more preferably 300°C to 500°C.
[0212] Next, a conductive film to form the conductive layer 260 is deposited. This conductive film can be deposited using sputtering, CVD, MBE, PLD, plating, or ALD. For example, a titanium nitride film and a tungsten film can be deposited by laminating them using the CVD method.
[0213] Next, the conductive film, which will become the insulating layer 250 and the conductive layer 260, is polished by CMP treatment until the insulating layer 280 is exposed. In other words, the portion of the insulating layer 250 and the conductive film exposed through the opening is removed. This forms the insulating layer 250 and the conductive layer 260 within the opening that reaches the semiconductor layer 230 (Figures 9A1 and 9A2).
[0214] As a result, the insulating layer 250 is provided within the opening in contact with the conductive layer 242a, the conductive layer 242b, the semiconductor layer 230, and the insulating layer 201. The conductive layer 260 is also arranged to fill the opening via the insulating layer 250. In this way, the transistor 200 is formed.
[0215] Next, an insulating layer 282 is formed on the insulating layer 250, the conductive layer 260, and the insulating layer 280. The insulating layer 282 can be formed using, for example, sputtering, CVD, MBE, PLD, or ALD. It is preferable to form the insulating layer 282 using the sputtering method. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 282 can be reduced.
[0216] Here, by using the sputtering method to deposit the insulating layer 282 in an oxygen-containing atmosphere, oxygen can be added to the insulating layer 280 during film formation. This allows the insulating layer 280 to contain excess oxygen.
[0217] Next, an insulating layer 285 is formed on the insulating layer 282 (Figures 9B1 and 9B2). The insulating layer 285 can be deposited using sputtering, CVD, MBE, PLD, or ALD. It is preferable to deposit the insulating layer 285 using sputtering. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 285 can be reduced.
[0218] Next, openings reaching the conductive layers 242a and 242b are formed in the insulating layer 275, insulating layer 280, insulating layer 282, and insulating layer 285, respectively. These openings can be formed using lithography. It is preferable to process the workpiece using a dry etching method when forming these openings. The shape of the openings in a top view can be a circle, an ellipse or other approximate circle, a quadrilateral or other polygon, or a quadrilateral or other polygon with rounded corners.
[0219] Next, after the opening is formed, a heat treatment can be performed. The temperature of the heat treatment should be 100°C to 600°C, preferably 250°C to 550°C, and more preferably 350°C to 450°C. It is preferable to perform the heat treatment in an atmosphere of an inert gas such as nitrogen gas or a noble gas. Furthermore, since the heat treatment is performed with the conductive layer 242a and conductive layer 242b exposed, it is preferable to perform it in an atmosphere that does not contain oxidizing gases or oxygen gas. For example, it is preferable to perform the heat treatment in a nitrogen gas atmosphere at a temperature of 400°C for 1 hour. The heat treatment may also be performed under reduced pressure. Through the heat treatment, oxygen contained in the insulating layer 280 can be supplied to the semiconductor layer 230 via the insulating layer 250. In addition, by performing the heat treatment at the stage when the opening is provided in the insulating layer 280, some of the oxygen contained in the insulating layer 280 can be released, and the amount of oxygen contained in the insulating layer 280 can be adjusted. This prevents the reliability from being compromised due to excessive oxygen.
[0220] Next, insulating films, which will become insulating layers 241a and 241b, are deposited along the shape of the opening. These insulating films can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. Since the insulating films that will become insulating layers 241a and 241b are deposited in an opening with a large aspect ratio, it is preferable to deposit them using the ALD method. Furthermore, it is preferable to use insulating films that have the function of suppressing oxygen permeability as insulating films that will become insulating layers 241a and 241b. For example, it is preferable to deposit silicon nitride using the PEALD method. Silicon nitride is preferred because it has high barrier properties against hydrogen.
[0221] Next, the insulating film is anisotropically etched to form insulating layers 241a and 241b. Here, insulating layer 241a is formed to cover the sidewall of the opening on the conductive layer 242a, and insulating layer 241b is formed to cover the sidewall of the opening on the conductive layer 242b. For the anisotropic etching of the insulating film that will become insulating layers 241a and 241b, a dry etching method or the like may be used. For example, reactive ion etching is preferred. By providing insulating layers 241a and 241b on the sidewalls of the openings, the permeation of oxygen from the outside is suppressed, and oxidation of the conductive layers 240a and 240b to be formed next can be prevented. In addition, impurities such as water and hydrogen contained in the insulating layer 280 can be prevented from diffusing into the conductive layers 240a and 240b. Note that, as a result of this anisotropic etching, recesses may be formed on a part of the upper surface of conductive layers 242a and 242b.
[0222] Next, conductive films that will become conductive layers 240a and 240b are formed. It is desirable that the conductive films have a laminated structure that includes a conductor that has the function of suppressing the permeation of impurities such as water and hydrogen. For example, it can be a laminate of tantalum nitride, titanium nitride, etc., and tungsten, molybdenum, copper, etc. The conductive films that will become conductive layers 240a and 240b can be formed using sputtering, CVD, MBE, PLD, or ALD methods.
[0223] Next, by performing a CMP treatment, a portion of the conductive film that will become the conductive layer 240a and conductive layer 240b is removed, exposing the upper surface of the insulating layer 285 (Figures 9C1 and 9C2). As a result, the conductive film remains only in the openings, making it possible to form conductive layers 240a and conductive layers 240b with flat upper surfaces. Note that in some cases, a portion of the upper surface of the insulating layer 285 may be removed by this CMP treatment.
[0224] Based on the above, the transistor 200 shown in Figures 2A to 2D can be manufactured.
[0225] After this, multiple wirings can be formed on the insulating layer 285 that are in contact with the upper surface of the conductive layer 240a and the conductive layer 240b, respectively. Alternatively, before forming the wiring, openings reaching the conductive layer 260 may be formed in the insulating layer 285 and the insulating layer 282, and an insulating layer similar to the insulating layer 241a and a conductive layer similar to the conductive layer 240a may be formed to fill these openings.
[0226] After the formation of the transistor 200, a second heat treatment is performed. The second heat treatment allows hydrogen in the semiconductor layer 230 to be gettered by either or both of the insulating layer 250 and the insulating layer 201, thereby reducing the hydrogen concentration in the semiconductor layer 230. Furthermore, oxygen contained in the insulating layer 280, insulating layer 250, insulating layer 201, etc., can be supplied to the semiconductor layer 230, thereby reducing oxygen deficiencies in the semiconductor layer 230. For details on the second heat treatment, refer to the description in Embodiment 1.
[0227] Furthermore, the second heat treatment may be performed at any time after the formation of the insulating layer 250. Alternatively, the heat generated during the formation of the insulating layer 250 may be combined with the second heat treatment. For example, the second heat treatment may be performed after the formation of the conductive layer 260, after the formation of the insulating layer 282, after the formation of the insulating layer 285, after the formation of the insulating layers 241a and 241b, after the formation of the conductive layers 240a and 240b, etc. Also, the heat generated during the formation of the conductive layer 260, the formation of the insulating layer 282, the formation of the insulating layer 285, the formation of the conductive layers 240a and 240b, etc. may be combined with the second heat treatment.
[0228] The above is a description of the method for manufacturing semiconductor devices.
[0229] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0230] (Embodiment 3) This embodiment describes an indium oxide film that can be used in the semiconductor layer of a transistor in a semiconductor device according to one aspect of the present invention.
[0231] In this specification, indium oxide having at least a crystalline portion or crystalline region in the film is referred to as crystalline indium oxide (crystal IO) or crystalline indium oxide (crystalline IO). Examples of crystal IO or crystalline IO include single-crystal indium oxide, polycrystalline indium oxide, and microcrystalline indium oxide.
[0232] Indium oxide is a semiconductor material with completely different physical properties from oxide semiconductors such as In-Ga-Zn oxide (hereinafter also referred to as IGZO) and zinc oxide.
[0233] The carrier concentration dependence of the hole (Hall) mobility of indium oxide, silicon, and IGZO is described. Figure 10A shows silicon (Si) and indium oxide (InO X Figure 10B is a schematic diagram of the carrier concentration dependence of hole mobility with respect to IGZO.
[0234] First, as indicated by the arrows in Figure 10B, IGZO tends to show higher hole mobility as the carrier concentration increases. On the other hand, as indicated by the arrows in Figure 10A, indium oxide tends to show higher hole mobility as the carrier concentration decreases (see Non-Patent Literature 2). This trend is similar to that of silicon, where the lower the concentration of dopants (impurities) in the material, the less impurity scattering occurs and the higher the hole mobility. In other words, the higher the purity and intrinsic nature of indium oxide, the higher its hole mobility. From these results, it can be said that indium oxide, unlike IGZO, is a material with physical properties similar to silicon. Note that the properties of indium oxide shown in Figure 10A are assumed to be for a single crystal. Therefore, when indium oxide is not a single crystal (for example, polycrystalline), the properties may differ from those shown in Figure 10A.
[0235] In Figure 10A, the range R1 with low carrier concentration exhibits extremely high hole mobility, making it a suitable carrier concentration range for, for example, the channel formation region of a transistor. For example, in the case of indium oxide, the range R1 has a carrier concentration of 1 × 10⁻⁶. 15 cm −3 This range includes, for example, 1 × 1014 cm −3 The above is 1 x 10 18 cm −3 The range is as follows: By sufficiently reducing the carrier concentration, the hole mobility value can be increased to 270 cm⁻¹. 2 It can be expected to be raised to the level of / (V・s).
[0236] Furthermore, in indium oxide, the region where the carrier concentration is in the range R1 may contain elements that lower the carrier concentration. Examples of elements that lower the carrier concentration include magnesium, calcium, zinc, cadmium, and copper. By substituting these elements for indium, the carrier concentration can be lowered. Other elements that lower the carrier concentration include nitrogen, phosphorus, arsenic, and antimony. For example, by substituting nitrogen, phosphorus, arsenic, or antimony for oxygen, the carrier concentration can be lowered.
[0237] Elements that reduce carrier concentration can also be called elements that confer p-type properties. Adding elements that reduce carrier concentration to an indium oxide film can make the indium oxide film i-type or substantially i-type. In this case, the concentration of the above-mentioned carrier-reducing element in the indium oxide film is 1 × 10⁻⁶. 16 atoms / cm 3 The above 8 x 10 20 atoms / cm 3 The following is preferable: 1 × 10 16 atoms / cm 3 The above 4 x 10 20 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 8 x 10 19 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 5 x 10 19 atoms / cm 3 The following is even more preferable. By using such concentrations, the carrier concentration can be reduced while maintaining the crystal structure of indium oxide.
[0238] On the other hand, the range R2 with high carrier concentration has low electrical resistance and can be said to be a suitable range of carrier concentration for applications such as the source and drain regions of a transistor, or for resistors or transparent conductive films. The range R2 is when the carrier concentration value is 1 × 10⁻⁶. 20 cm −3 This range includes, for example, 1 × 10 19 cm −3 The above is 1 x 10 22 cm −3 The range is as follows: By making the carrier concentration sufficiently high, the resistivity can be increased to 1 × 10⁻⁶. −4 It is expected that the level can be reduced to below Ω·cm.
[0239] In the case of indium oxide, the region where the carrier concentration is in the range R2 may contain elements that increase the carrier concentration. For example, it is preferable to include elements common to the source and drain electrodes of the transistor. Examples of elements that increase the carrier concentration include titanium, zirconium, hafnium, tantalum, tungsten, molybdenum, tin, silicon, and boron. In particular, it is more preferable to use elements whose oxides are conductive or semiconducting. As for the supply method of elements that increase the carrier concentration, a method of forming a film containing the element and diffusing it, ion implantation, ion doping, plasma immersion ion implantation, or plasma treatment can be used. In this specification, unless otherwise specified, the presence or absence of mass separation is not limited. For example, in this specification, a method of supplying ions by mass separation is called ion implantation, and a method of supplying ions without mass separation is called ion doping.
[0240] Elements that increase carrier concentration can also be called elements that confer n-type properties. The concentration of the above-mentioned carrier-increasing elements in an indium oxide film is 1 × 10⁻⁶ 16 atoms / cm 3 The above 8 x 10 20 atoms / cm 3 The following is preferable: 1 × 10 16 atoms / cm 3 The above 4 x 10 20 atoms / cm 3 The following is more preferable: 1 × 1016 atoms / cm 3 The above 8 x 10 19 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 5 x 10 19 atoms / cm 3 The following is even more preferable. By using such concentrations, the carrier concentration can be increased while maintaining the crystal structure of indium oxide. Antimony can also function as an element that increases the carrier concentration.
[0241] As indium oxide is an oxide whose valence electrons can be controlled, the threshold voltage of a transistor using a semiconductor layer containing indium oxide can be controlled. Furthermore, in indium oxide, regions with low carrier concentrations can be used as the channel formation region of the transistor, while regions with high carrier concentrations can be used as the source and drain regions. In contrast, with IGZO, strain can form in the source and drain regions due to stress on the electrodes in contact with the IGZO, sometimes resulting in the formation of an n-type region. On the other hand, unlike IGZO, indium oxide allows for valence electron control, so it does not require the formation of strain in the film as in IGZO. Less strain in the film is expected to improve reliability. For example, by creating regions with carrier concentrations in the range R1 and range R2 shown in Figure 10A within the indium oxide film, a so-called n-i-n junction (a junction of an n-type region, an i-type region, and an n-type region) can be created. Valence electron control in transistors using silicon is generally known. On the other hand, valence electron control in transistors using indium oxide is a novel technological concept that would not normally be conceived.
[0242] By using the above technical concept, the indium oxide transistor described herein has two or more, preferably three or more, more preferably four or more, and most preferably five of the following features (1) to (5): (1) High on-current (in other words, high mobility). (2) Low off-current. (3) Achieves normally-off characteristics. (4) Has high reliability. (5) Has a high cutoff frequency (fT). For example, the indium oxide transistor described herein has high mobility, low off-current, and can achieve normally-off characteristics. This transistor is different from a transistor that has high mobility and normally-on characteristics.
[0243] In addition, the i-type nature of a semiconductor means that the Fermi level (Ef) and the intrinsic Fermi level (Ei) are the same (Ef = Ei). As shown in Figure 10B, in IGZO, the lower the carrier concentration, the lower the hole mobility. Therefore, when Ef = Ei is reached, there are no carriers left (in other words, the material has properties similar to an insulator), and it may cease to function as a transistor. On the other hand, in indium oxide, as shown in Figure 10A, the lower the carrier concentration, the higher the hole mobility, and when Ef = Ei is reached, the hole mobility is maximized. That is, transistors containing indium oxide can achieve high field-effect mobility by setting Ef = Ei. Furthermore, because transistors containing indium oxide have a low carrier concentration, they tend to exhibit normally-off characteristics. Therefore, transistors containing indium oxide can achieve both normally-off characteristics and high field-effect mobility.
[0244] The normally-off characteristic refers to the state in which no current flows through a transistor when no potential is applied to the gate or when the gate-source voltage is 0V. The normally-off characteristic can be evaluated using the transistor's threshold voltage (Vth) or shift value (Vsh). Unless otherwise specified, Vth will be calculated using the constant current method. More specifically, Vth is the value of drain current (Id) × channel length (L) ÷ channel width (W) in the transistor's Id-Vg characteristic, where Vth is 1nA (1 × 10⁻¹⁰). −9 Let Vg be the gate voltage (Vg) when A) is true. Also, Vsh is the tangent to the maximum slope when the drain current (Id) in the Id-Vg characteristic of the transistor is expressed logarithmically, and Id = 1pA (1 × 10⁻¹⁰). −12 Vg is the gate voltage (Vg) at the intersection with line A), or the Vg at the intersection of the line extrapolated from the two points where the slope of Id is maximized when Id is expressed logarithmically in the transistor's Id-Vg characteristic, and the line where Id = 1 pA. For example, if either or both of Vth and Vsh are zero or positive values, the transistor can be considered to have a normally-off characteristic.
[0245] Furthermore, in transistors containing indium oxide, the film configuration in contact with the indium oxide film is crucial for making the semiconductor i-type, that is, for achieving Ef = Ei. For example, in transistors containing indium oxide, a film configuration can be obtained in which a silicon oxide film, a hafnium oxide film, and a silicon nitride film are stacked in contact with the indium oxide film. By using this film configuration, it is possible to create a semiconductor device that satisfies Ef = Ei and is highly reliable.
[0246] Furthermore, in the above film configuration, oxygen-containing films such as silicon oxide-nitride films, silicon oxide nitride films, aluminum oxide films, and gallium oxide films can be used instead of the silicon oxide film. Also, in the above film configuration, silicon oxide nitride films, silicon oxide nitride films, etc. can be used instead of the silicon nitride film. In addition, the hafnium oxide film located on the indium oxide side of the silicon nitride film functions as a hydrogen gettering site.
[0247] Furthermore, the above film configuration can also be viewed as a layered structure consisting of a film that can supply oxygen to the indium oxide film (e.g., a silicon oxide film), a film that can getter hydrogen (e.g., a hafnium oxide film), and a film that suppresses the intrusion of oxygen and hydrogen (e.g., a silicon nitride film). With this configuration, oxygen deficiencies in the indium oxide film are compensated for by oxygen in the silicon oxide film. Also, hydrogen in the indium oxide film is captured by the hafnium oxide film through heat treatment or other means. In addition, the silicon nitride film provides a film configuration that minimizes the intrusion of oxygen and hydrogen from the outside. In other words, by using the above film configuration, the indium oxide film can be made closer to type i. Therefore, transistors having the above-described indium oxide film have high field-effect mobility and high reliability.
[0248] Next, we will describe indium oxide films applied to transistors. Indium oxide films are preferably crystalline (i.e., they have crystal grains). Examples of films with crystal grains include single-crystal films, polycrystalline films, or amorphous films containing crystal grains (also called microcrystalline films). In particular, polycrystalline films are preferred for indium oxide films, and single-crystal films are more preferred. Single-crystal films do not have crystal grain boundaries. Impurities that inhibit carrier flow (typically insulating impurities, insulating oxides, etc.) tend to segregate at crystal grain boundaries. By using single-crystal films, carrier scattering at crystal grain boundaries can be suppressed, enabling the realization of transistors exhibiting high field-effect mobility. Furthermore, it has the excellent effect of suppressing variations in transistor characteristics caused by these crystal grain boundaries.
[0249] Furthermore, polycrystalline films are preferable because they can reduce carrier scattering and exhibit high field-effect mobility compared to microcrystalline or amorphous films. When using polycrystalline films, it is preferable to use films with the largest possible grain size and few grain boundaries. In a transistor to which a polycrystalline indium oxide film is applied, if there are no grain boundaries in the channel formation region, or if no grain boundaries are observed, the channel formation region is located within the single-crystal region contained in the polycrystalline film, and therefore it can be considered a transistor to which single-crystal indium oxide is applied.
[0250] The crystallinity of indium oxide can be analyzed, for example, by X-ray diffraction (XRD), transmission electron microscopy (TEM), or electron diffraction (ED). Alternatively, a combination of these methods may be used for analysis.
[0251] Furthermore, in this specification, a semiconductor layer in which no grain boundaries are observed in the channel-forming region, a semiconductor layer in which the channel-forming region is contained within a single crystal grain, or a semiconductor layer in which the direction of the crystal axes is the same in at least two regions within the channel-forming region can be called a single crystal film. In addition, a semiconductor layer in which, within a single crystal grain in the channel-forming region, the direction of other crystal axes changes continuously with respect to a certain crystal axis or crystal orientation as the axis of rotation can be called a single crystal film.
[0252] The channel formation region refers to the area within the semiconductor layer that overlaps with (or faces) the gate electrode via the gate insulating layer, and is located between the region in contact with the source electrode and the region in contact with the drain electrode. The current path in the channel formation region is the shortest distance between the source electrode and the drain electrode. Therefore, the crystal grains, grain boundaries, crystal axes, and crystal orientation in the channel formation region can be confirmed by cross-sectional observation including the semiconductor layer, source electrode, and drain electrode.
[0253] The indium oxide film in the channel formation region preferably has a lower impurity concentration. Impurities in the indium oxide film in the channel formation region can act as carrier scattering sources, which may cause a reduction in field-effect mobility. In addition, these impurities can also be a factor that inhibits crystal growth of the indium oxide film. Examples of impurities for the indium oxide film include boron and silicon. The indium oxide film preferably has a concentration of each of these impurities of 0.1% or less, more preferably 0.01% (100 ppm) or less. Note that carbon, hydrogen, and the like are elements that can be contained in a deposition gas or a precursor during film formation, and may remain in the indium oxide film in a larger amount than the above impurities.
[0254] Note that the indium oxide film may contain an element that can be a trivalent cation, similarly to indium, within a range where its crystal maintains a cubic structure (bixbyite type). Examples include Group 13 elements of the periodic table such as gallium and aluminum, and Group 3 elements of the periodic table. Since these elements have a stronger bonding force with oxygen than indium, adding these elements to the indium oxide film reduces oxygen vacancies (V in the indium oxide film O ) can be suppressed. In addition, since these elements mainly exist as trivalent cations in oxides, the carrier concentration of the indium oxide film can be kept low. Therefore, the threshold voltage of the transistor can be shifted to the positive side. In addition, normally-off characteristics can be obtained. Accordingly, a transistor with favorable electrical characteristics can be provided.
[0255] The concentration of the above elements in the indium oxide film is 1×10 16 atoms / cm 3 or more and 8×10 20 atoms / cm 3 or less, preferably 1×10 16 atoms / cm 3 or more and 4×10 20 atoms / cm 3 or less, more preferably 1×10 16 atoms / cm 3 or more and 8×10 19 atoms / cm 3The following is more preferable, 1×10 16 atoms / cm 3 or more and 5×10 19 atoms / cm 3 or less is even more preferable.
[0256] Note that the above-described element imparting n-type, element imparting p-type, and element capable of becoming a trivalent cation can each be added to the indium oxide film by a method such as an ion doping method, an ion implantation method, or a thermal diffusion method. Alternatively, the above-described element imparting n-type, element imparting p-type, and element capable of becoming a trivalent cation can each be added to a sputtering target, a deposition gas, an ALD deposition precursor, or the like when forming the indium oxide film. Alternatively, the above-described element imparting n-type, element imparting p-type, and element capable of becoming a trivalent cation can each be auto-doped from a chamber when forming the indium oxide film. Note that auto-doping refers to the phenomenon that elements contained in members of the deposition chamber or the like are automatically added into the film during the deposition of the indium oxide film.
[0257] Further, the indium oxide film in this specification and the like has a high film density. Note that the theoretical value of the film density of the indium oxide film is 7.18 g / cm 3 . The range of the film density of the indium oxide film in this specification and the like is 6.70 g / cm 3 or more and 7.18 g / cm 3 or less, preferably 6.90 g / cm 3 or more and 7.18 g / cm 3 or less, further preferably 7.00 g / cm 3 or more and 7.18 g / cm 3 or less.
[0258] Note that for the evaluation of film density, for example, Rutherford backscattering spectrometry (RBS) or X-ray reflectometry (XRR) can be used. Differences in film density can sometimes be evaluated by a cross-sectional transmission electron microscope (TEM) image. In TEM observation, when the film density is high, the transmission electron (TE: Transmission Electron) image is dark, and when the film density is low, the transmission electron (TE) image is light (bright).
[0259] By using such an indium oxide film in a transistor, the field-effect mobility of the transistor can be increased to 50 cm². 2 / (V·s) or more, preferably 100 cm 2 / (V·s) or more, more preferably 150 cm 2 / (V·s) or more, more preferably 200 cm 2 / (V·s) or more, more preferably 250 cm 2 It can be set to (V・s) or more.
[0260] One of the characteristics of indium oxide films is that they have higher oxygen permeability (diffusivity) compared to IGZO films. As shown in Figure 10C, indium oxide films (InO X Oxygen (O) diffusing into the indium oxide film passes through the indium oxide film and oxygen molecules (O) 2 It is released as water molecules (H) by reacting with hydrogen contained in the membrane. 2 It may also be released as O. Furthermore, oxygen deficiencies (V) can form in the membrane. O If oxygen atoms are present, diffusing oxygen atoms will fill the oxygen deficiency. Indium oxide films allow oxygen to diffuse easily, so they can be said to fill oxygen deficiencies more easily than IGZO films.
[0261] Thus, because indium oxide films are more likely to reduce oxygen vacancies in the film compared to IGZO films, applying such indium oxide films to transistors makes it possible to realize transistors with extremely high reliability.
[0262] Furthermore, as shown in Figure 10C, the indium oxide film diffuses hydrogen. Hydrogen diffusing into the indium oxide film from the outside permeates the film and forms hydrogen molecules (H 2 It is released as ) or by reacting with oxygen contained in the film, and released as water molecules. The above-mentioned oxygen and hydrogen diffuse through the indium oxide film by heat treatment. The temperature of the heat treatment is 200°C to 700°C, preferably 350°C to 650°C, and more preferably 400°C to 500°C.
[0263] Transistors using indium oxide films are storage-type transistors that use electrons as majority carriers. Assuming that the carrier relaxation time is constant, the smaller the effective mass of electrons (carriers), the higher the electron mobility. In other words, by using indium oxide, which has a small effective mass of electrons, in a transistor, the on-current or field-effect mobility of the transistor can be increased.
[0264] Table 1 shows single crystal indium oxide (here, In 2 O 3 The effective masses of indium oxide and single-crystal silicon (Si) are shown below. As shown in Table 1, indium oxide is characterized by a small effective electron mass and a large effective hole mass. Furthermore, the effective electron mass of indium oxide is almost independent of the crystal orientation. Therefore, by using crystalline indium oxide in transistors, transistors with high field-effect mobility and high frequency characteristics (also called f-characteristics) can be realized. In addition, because the effective hole mass is large, transistors with extremely low off-currents can be realized. For example, by applying an indium oxide film to a vertical transistor, the off-current per 1 μm of channel width is 1 fA (1 × 10⁻¹⁶) in an environment of 125°C. −15 A) Less than or equal to, or 1aA (1 × 10 −18 A) Less than or equal to 1aA (1 × 10) in a room temperature (25°C) environment. −18 A) Less than or equal to, or 1zA (1 × 10⁻¹⁰ −21 A) The following is possible. Also, as shown in Table 1, indium oxide has a smaller effective electron mass and a larger effective hole mass than silicon, so it may be possible to realize a transistor with higher field-effect mobility and lower off-current than a Si transistor.
[0265]
[0266] It is preferable to provide a seed layer so as to be in contact with at least a portion of the crystalline indium oxide film. It is preferable to use a material containing crystals with a small difference in lattice constant (also called lattice mismatch) with the indium oxide for the seed layer. This improves the crystallinity of the indium oxide film. A substrate (e.g., a single-crystal substrate) may be used as one of the layers in contact with at least a portion of the crystalline indium oxide film.
[0267] One method for evaluating the degree of lattice mismatch is to use the following lattice mismatch value. The lattice mismatch Δa [%] of the crystals in the formed film (in this case, the indium oxide film) relative to the crystals in the seed layer is given by Δa = ((L 1 -L 2 ) / L 2 It is calculated as ) × 100. Here L 1 L is the length of the unit cell vector of the crystals in the formed film, or the lattice constant. 2 This is the length of the unit cell vector of the crystal in the seed layer, or the lattice constant.
[0268] The lattice mismatch Δa between the seed layer and the indium oxide film is preferably small in absolute value, and most preferably zero. For example, Δa can be -5% or more and 5% or less, preferably -4% or more and 4% or less, more preferably -3% or more and 3% or less, and even more preferably -2% or more and 2% or less.
[0269] Here, the indium oxide crystal has a cubic structure (bixbite type). For example, yttria-stabilized zirconia (YSZ) crystals can have a cubic structure (fluorite type). The lattice mismatch of the indium oxide crystal with respect to the cubic YSZ crystal is in the range of -2% to 2%, and a single crystal film of indium oxide can be epitaxially grown on a YSZ substrate.
[0270] Furthermore, the crystal structure of the seed layer and the crystal structure of the indium oxide film do not necessarily have to be the same in terms of crystal system or crystal orientation. For example, a film with a hexagonal or trigonal crystal structure can be used beneath an indium oxide film with a cubic crystal structure. For example, by setting the crystal orientation of the surface of the seed layer to
[001] and the crystal orientation of the underside of the indium oxide film to
[111] , the requirements related to crystal orientation necessary for epitaxial growth can be met. Examples of hexagonal or trigonal crystals include wurtzite-type structures and YbFe. 2 O 4 Type structure, Yb 2 Fe 3 O 7 These include type structures and their modified type structures. YbFe 2 O 4 Type structure or Yb 2 Fe 3 O 7 An example of a crystal with a crystalline structure is IGZO. Indium oxide single crystal films can be formed not only on YSZ substrates but also on insulating films. On the other hand, it is difficult to form silicon single crystal films on insulating films. Silicon crystals have a diamond structure. Thus, in terms of single crystals, indium oxide and silicon have similar properties. However, when comparing indium oxide and silicon from the perspective of whether single crystals can be formed on insulating films, they have different properties.
[0271] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0272] (Embodiment 4) In this embodiment, a memory device according to one aspect of the present invention will be described with reference to Figures 11 to 14. In this embodiment, an example of the configuration of a memory device in which a layer having memory cells is stacked on a layer on which a drive circuit including a sense amplifier is provided will be described.
[0273] The transistors in the memory cells exemplified below can be the same type of transistor (referred to as an OS transistor) exemplified in Embodiment 2, in which a channel is formed in an oxide semiconductor having a single-crystal region.
[0274] <Example of Storage Device Configuration> Figure 11 shows a block diagram illustrating an example of the configuration of a storage device 480 according to one aspect of the present invention. The storage device 480 shown in Figure 11 has a layer 420 and a stacked layer 470.
[0275] Layer 420 is a layer having Si transistors. Layer 470 is formed by stacking element layers 430[1] to 430[m] (where m is an integer of 2 or more). Each element layer 430 is a layer having OS transistors. Layer 470 can be formed by stacking on top of layer 420.
[0276] In this specification, when describing matters common to components distinguished by letters or numbers attached to their reference numerals (such as the element layer 430[1] and memory cell 432[m,n]), the letters or numbers may be omitted without further explanation.
[0277] The element layer 430 has memory cells 432 composed of OS transistors and capacitive elements. Figure 11 shows an example in which the element layers 430[1] to 430[m] have a plurality of memory cells 432 arranged in a matrix of m rows and n columns (where n is an integer of 2 or more).
[0278] Memory cell 432[1,1] is the memory cell in the 1st row and 1st column, and memory cell 432[m,n] is the memory cell in the mth row and nth column. Additionally, when referring to an arbitrary row, it may be written as row i, column j, etc. i is an integer between 1 and m (inclusive), and j is an integer between 1 and n (inclusive).
[0279] Figure 11 also shows m wirings WL and m wirings PL extending in the row direction, and n wirings BL extending in the column direction. Multiple memory cells 432 located in row i are connected to the wiring WL[i] and the wiring PL[i] of row i.
[0280] Wiring BL functions as a bit line for writing and reading data. Wiring WL functions as a word line for controlling the on or off state (conductive or non-conductive) of the access transistor, which functions as a switch. Wiring PL functions as a constant potential line connected to the capacitor. A separate wire can be provided to transmit the back gate potential.
[0281] The memory cell 432 is connected to the sense amplifier 446 via a wiring BL. The wiring BL can consist of wiring arranged horizontally on the substrate surface as well as wiring arranged vertically. This shortens the length of the wiring between the element layer 430 and the sense amplifier 446. As a result, the resistance and parasitic capacitance of the wiring BL are significantly reduced, and the power consumption and signal delay of the memory device 480 can be reduced. Furthermore, it becomes possible to operate the memory cell 432 even with a smaller capacitor capacity, enabling miniaturization of the memory device 480.
[0282] Layer 420 includes a PSW 471 (power switch), a PSW 472, and peripheral circuits 422. Peripheral circuits 422 include a drive circuit 440, a control circuit 473, and a voltage generation circuit 474. Each circuit in layer 420 is a circuit containing a Si transistor.
[0283] In the storage device 480, each circuit, each signal, and each voltage can be appropriately selected or omitted as needed. Alternatively, other circuits or other signals may be added. Signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are external input signals, and signal RDA is an external output signal. Signal CLK is a clock signal.
[0284] Furthermore, signals BW, CE, and GW are control signals. Signal CE is the chip enable signal, signal GW is the global write enable signal, and signal BW is the byte write enable signal. Signal ADDR is the address signal. Signal WDA is the write data signal, and signal RDA is the read data signal. Signals PON1 and PON2 are power gating control signals. Signals PON1 and PON2 may be generated by the control circuit 473.
[0285] The control circuit 473 is a logic circuit that has the function of controlling the overall operation of the storage device 480. For example, the control circuit performs logical operations on signals CE, GW, and BW to determine the operating mode of the storage device 480 (e.g., write operation, read operation). Alternatively, the control circuit 473 generates a control signal for the drive circuit 440 so that this operating mode is executed.
[0286] The voltage generation circuit 474 has the function of generating a negative voltage. The signal WAKE has the function of controlling the input of the signal CLK to the voltage generation circuit 474. For example, when a high-level signal is applied to the signal WAKE, the signal CLK is input to the voltage generation circuit 474, and the voltage generation circuit 474 generates a negative voltage.
[0287] The drive circuit 440 is a circuit for writing and reading data to and from the memory cell 432. The drive circuit 440 includes a row decoder 442, a column decoder 444, a row driver 443, a column driver 445, an input circuit 447, an output circuit 448, and the aforementioned sense amplifier 446.
[0288] The row decoder 442 and column decoder 444 have the function of decoding the ADDR signal. The row decoder 442 is a circuit for specifying the row to access, and the column decoder 444 is a circuit for specifying the column to access. The row driver 443 has the function of selecting the wiring WL specified by the row decoder 442. The column driver 445 has the function of writing data to the memory cell 432, reading data from the memory cell 432, and holding the read data.
[0289] The input circuit 447 has the function of holding the signal WDA. The data held by the input circuit 447 is output to the column driver 445. The output data of the input circuit 447 is the data (Din) to be written to the memory cell 432. The data (Dout) read by the column driver 445 from the memory cell 432 is output to the output circuit 448. The output circuit 448 has the function of holding Dout. The output circuit 448 also has the function of outputting Dout to the outside of the storage device 480. The data output from the output circuit 448 is the signal RDA.
[0290] PSW 471 has the function of controlling the supply of VDD to the peripheral circuit 422. PSW 472 has the function of controlling the supply of VHM to the row driver 443. Here, the high power supply potential of the storage device 480 is VDD, and the low power supply potential is GND (ground potential). VHM is a high power supply potential used to raise the word line to a high level, and is higher than VDD. The on / off state of PSW 471 is controlled by signal PON1, and the on / off state of PSW 472 is controlled by signal PON2. In Figure 11, the number of power supply domains to which VDD is supplied in the peripheral circuit 422 is set to 1, but it can be multiple. In this case, a power switch can be provided for each power supply domain.
[0291] The element layers 430[1] to 430[m] can be layered on top of layer 420. Figure 12A shows a perspective view of a memory device 480 in which five (m=5) element layers 430[1] to 430[5] are layered on top of layer 420.
[0292] Figure 12A shows wiring WL and wiring PL extending in the X direction, and wiring BL and wiring BLB extending in the Y and Z directions (directions perpendicular to the substrate surface on which the drive circuit is installed). Wiring BLB is an inverting bit line. For the sake of clarity, some of the wiring WL and wiring PL of each element layer 430 have been omitted from the diagram.
[0293] Figure 12B shows a schematic diagram of a sense amplifier 446 and multiple memory cells 432 connected via wiring BL and wiring BLB. Note that a configuration in which multiple memory cells are connected to a single bit line is also called a "memory string".
[0294] Figure 12B shows an example of the circuit configuration of a memory cell 432 connected to the wiring BLB. The memory cell 432 has a transistor 437 and a capacitive element 438.
[0295] Transistor 437 has one source and drain connected to wiring BLB, the other connected to one electrode of capacitive element 438, and its gate connected to wiring WL. Capacitive element 438 has its other electrode connected to wiring PL.
[0296] The wiring PL is a wire that provides a constant potential to the capacitive element 438. By connecting multiple wiring PLs together and using them as a single wire, the number of wires can be reduced.
[0297] In one aspect of the present invention, memory cells having OS transistors are stacked, and bit lines are arranged to extend perpendicularly to the substrate surface. This allows for a reduction in the length of wiring between element layers and an increase in the density of elements per unit area. As a result, a memory device with excellent memory capacity and reduced power consumption can be obtained.
[0298] [Example Configuration of Memory Cell 432 and Sense Amplifier 446] Figures 13A and 13B show the circuit diagram corresponding to the memory cell 432 described above, and the circuit block diagram corresponding to the said circuit diagram. The same applies when wiring BL is replaced with wiring BLB.
[0299] Figures 13C and 13D show the circuit diagram corresponding to the sense amplifier 446 described above, and the circuit block diagram corresponding to the said circuit diagram. The sense amplifier 446 has a switch circuit 482, a precharge circuit 483, a precharge circuit 484, and an amplification circuit 485. Also shown are the signal output wirings SA_OUT and SA_OUTB.
[0300] The switch circuit 482 has n-type transistors 482_1 and 482_2. Transistors 482_1 and 482_2 switch the conduction state of the wiring pair SA_OUT and SA_OUTB and the wiring pair BL and BLB according to the signal CSEL.
[0301] The pre-charge circuit 483 has n-type transistors 483_1 to 483_3. The pre-charge circuit 483 is a circuit for pre-charging wiring BL and wiring BLB to an intermediate potential VPRE corresponding to the potential VDD / 2, in accordance with the signal EQ.
[0302] The precharge circuit 484 has p-type transistors 484_1 to 484_3. The precharge circuit 484 is a circuit for precharging wiring BL and wiring BLB to an intermediate potential VPRE corresponding to the potential VDD / 2, in accordance with the signal EQB.
[0303] The amplification circuit 485 has p-type transistors 485_1 and 485_2 connected to wiring SAP, and n-type transistors 485_3 and 485_4 connected to wiring SAN. Wiring SAP or wiring SAN is wiring that has the function of providing VDD or VSS. Transistors 485_1 to 485_4 are transistors that constitute an inverter loop.
[0304] Figure 13D also shows a circuit block diagram corresponding to the sense amplifier 446.
[0305] Figure 14 is a circuit block diagram of the storage device 480 shown in Figure 11. As shown in Figure 14, layer 470 has a plurality of memory cells 432. The memory cells 432 are connected to wiring BL or wiring BLB. The memory cells 432 connected to wiring BL are memory cells on which data is written or read.
[0306] Wiring BL and wiring BLB are connected to the sense amplifier 446. The sense amplifier 446 can read data according to the various signals described in Figure 13C.
[0307] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0308] (Embodiment 5) This embodiment describes an example of the configuration of a display device to which a transistor according to one aspect of the present invention can be applied.
[0309] Since the transistor according to one aspect of the present invention can be made extremely small, a display device to which the transistor according to one aspect of the present invention is applied can be an extremely high-resolution display device. For example, the display device according to one aspect of the present invention can be used in the display section of information terminals (wearable devices) such as wristwatches and bracelets, and in the display section of head-mounted devices such as VR (Virtual Reality) devices such as head-mounted displays and AR (Augmented Reality) devices such as glasses.
[0310] In one embodiment of the present invention, a display device can be provided with a drive circuit and a pixel circuit stacked on top of each other. In this case, the transistors constituting the pixels can be transistors in which channels are formed in an oxide semiconductor having a single-crystal region, as exemplified in Embodiment 2.
[0311] [Display Module] Figure 15A shows a perspective view of the display module 580. The display module 580 includes a display device 500A and an FPC 590. The display module 580 includes a substrate 591 and a substrate 592. The display module 580 includes a display unit 581. The display unit 581 is an area for displaying an image.
[0312] Figure 15B shows a schematic perspective view illustrating the configuration of the substrate 591. On the substrate 591, a circuit section 582, a pixel circuit section 583 on the circuit section 582, and a pixel section 584 on the pixel circuit section 583 are stacked. In addition, a terminal section 585 for connecting to the FPC 590 is provided in the portion of the substrate 591 that does not overlap with the pixel section 584. The terminal section 585 and the circuit section 582 are connected by a wiring section 586, which is composed of multiple wires.
[0313] The pixel section 584 has a plurality of pixels 584a arranged periodically. An enlarged view of one pixel 584a is shown on the right side of Figure 15B. The pixel 584a has a light-emitting element 110R that emits red light, a light-emitting element 110G that emits green light, and a light-emitting element 110B that emits blue light.
[0314] The pixel circuit section 583 has a plurality of periodically arranged pixel circuits 583a. Each pixel circuit 583a is a circuit that controls the light emission of three light-emitting devices that one pixel 584a has. A single pixel circuit 583a may be configured to have three circuits that control the light emission of one light-emitting device. For example, each pixel circuit 583a may have at least one selection transistor, one current control transistor (drive transistor), and a capacitive element. In this case, a gate signal is input to the gate of the selection transistor, and a source signal is input to the source. This realizes an active matrix type display panel.
[0315] The circuit section 582 has circuits for driving each pixel circuit 583a of the pixel circuit section 583. For example, it is preferable to have one or both of a gate line drive circuit and a source line drive circuit. In addition, it may have at least one of the following: an arithmetic circuit, a memory circuit, and a power supply circuit. Furthermore, transistors provided in the circuit section 582 may constitute a part of the pixel circuit 583a. That is, the pixel circuit 583a may be composed of transistors in the pixel circuit section 583 and transistors in the circuit section 582.
[0316] The FPC 590 functions as wiring for supplying video signals and power potential, etc., to the circuit section 582 from an external source. An IC may also be mounted on the FPC 590.
[0317] The display module 580 can be configured such that one or both of the pixel circuit section 583 and the circuit section 582 are superimposed on the lower side of the pixel section 584, thereby making the aperture ratio (effective display area ratio) of the display section 581 extremely high. For example, the aperture ratio of the display section 581 can be 40% or more and less than 100%, preferably 50% or more and 95%, and more preferably 60% or more and 95%. Furthermore, it is possible to arrange the pixels 584a at an extremely high density, making the resolution of the display section 581 extremely high. For example, it is preferable that the pixels 584a in the display section 581 be arranged with a resolution of 2000 ppi or more and 30000 ppi or less, preferably 3000 ppi or more and 20000 ppi or less, more preferably 5000 ppi or more and 15000 ppi or less, and even more preferably 6000 ppi or more and 10000 ppi or less.
[0318] Because such a display module 580 is extremely high-resolution, it can be suitably used in VR devices such as head-mounted displays, or in glasses-type AR devices. For example, even in a configuration where the display part of the display module 580 is viewed through lenses, the display module 580 has an extremely high-resolution display part 581, so even when the display part is magnified with lenses, pixels are not visible, allowing for a highly immersive display. Furthermore, the display module 580 is not limited to this, and can be suitably used in electronic devices with relatively small display parts. For example, it can be suitably used in the display part of wearable electronic devices such as wristwatches.
[0319] [Display device 500A] The display device 500A shown in Figure 16 has a substrate 301, a light-emitting element 110R, a light-emitting element 110G, a light-emitting element 110B, a capacitor 540, a transistor 310, and a transistor 320.
[0320] Transistor 310 is a transistor in which a channel is formed on a single-crystal substrate. Transistor 320 can be a transistor in which a channel is formed on a single-crystal oxide semiconductor, as exemplified in Embodiment 2.
[0321] The transistor 310 is a transistor having a channel-forming region in the substrate 301. The substrate 301 can be a semiconductor substrate such as a single-crystal silicon substrate. The transistor 310 comprises a portion of the substrate 301, a conductive layer 311, a low-resistance region 312, an insulating layer 313, and an insulating layer 314. The conductive layer 311 functions as a gate electrode. The insulating layer 313 is located between the substrate 301 and the conductive layer 311 and functions as a gate insulating layer. The low-resistance region 312 is a region of the substrate 301 doped with impurities and functions as either a source or a drain. The insulating layer 314 is provided covering the side surface of the conductive layer 311.
[0322] Furthermore, an element isolation layer 315 is provided between two adjacent transistors 310 so as to be embedded in the substrate 301.
[0323] The transistor 320 has a semiconductor layer 351, an insulating layer 353, a conductive layer 354, a pair of conductive layers 355, an insulating layer 356, and a conductive layer 357.
[0324] An insulating layer 352 is provided on the layer on which the transistor 310 is located, via a wiring layer 316 and an interlayer insulating layer. The insulating layer 352 functions as a barrier layer to prevent impurities from diffusing from the substrate 301 side to the transistor 320, and to prevent oxygen from detaching from the semiconductor layer 351 to the insulating layer 352 side. As the insulating layer 352, for example, a film that is less permeable to hydrogen or oxygen than a silicon oxide film, such as an aluminum oxide film, a hafnium oxide film, or a silicon nitride film, can be used.
[0325] A conductive layer 357 is provided on an insulating layer 352, and an insulating layer 356 is provided covering the conductive layer 357. The conductive layer 357 functions as the second gate electrode of the transistor 320, and a portion of the insulating layer 356 functions as the second gate insulating layer. It is preferable to use an oxide insulating film, such as a silicon oxide film, for at least the portion of the insulating layer 356 that is in contact with the semiconductor layer 351. It is preferable that the upper surface of the insulating layer 356 is flattened.
[0326] The semiconductor layer 351 is provided on the insulating layer 356. Preferably, the semiconductor layer 351 has a metal oxide (also called an oxide semiconductor) film that exhibits semiconductor properties. A pair of conductive layers 355 are provided in contact with the semiconductor layer 351 and function as a source electrode and a drain electrode.
[0327] An insulating layer 358 and an insulating layer 350 are provided to cover the top and side surfaces of the pair of conductive layers 355, as well as the side surfaces of the semiconductor layer 351. The insulating layer 358 functions as a barrier layer to prevent impurities such as water or hydrogen from diffusing into the semiconductor layer 351 and to prevent oxygen from detaching from the semiconductor layer 351. An insulating film similar to that used for the insulating layer 352 can be used for the insulating layer 358.
[0328] The insulating layer 358 and the insulating layer 350 are provided with openings that reach the semiconductor layer 351. An insulating layer 353 in contact with the upper surface of the semiconductor layer 351 and a conductive layer 354 are embedded inside these openings. The conductive layer 354 functions as a first gate electrode, and the insulating layer 353 functions as a first gate insulating layer.
[0329] The upper surfaces of the conductive layer 354, the insulating layer 353, and the insulating layer 350 are flattened so that their heights are the same or approximately the same, and an insulating layer 359 is provided covering them. The insulating layer 359 functions as a barrier layer to prevent impurities such as water or hydrogen from diffusing into the transistor 320. An insulating film similar to that used for the insulating layer 352 can be used for the insulating layer 359.
[0330] The transistor 320 employs a configuration in which a semiconductor layer on which a channel is formed is sandwiched between two gates. The transistor may be driven by connecting the two gates and supplying them with the same signal. Alternatively, the threshold voltage of the transistor may be controlled by applying a potential to control the threshold voltage to one of the two gates and a potential to drive the other gate.
[0331] An insulating layer 564 is provided on the insulating layer 359. The insulating layer 564 functions as an interlayer insulating layer.
[0332] The plug 574, which connects to one side of the conductive layer 355, is provided so as to be embedded in the insulating layer 564, insulating layer 359, insulating layer 350, and insulating layer 358. Here, it is preferable that the plug 574 has a conductive layer 574a that covers the side surface of the opening in the insulating layer 564, etc., and a part of the upper surface of the conductive layer 355, and a conductive layer 574b that is in contact with the upper surface of the conductive layer 574a. In this case, it is preferable to use a conductive material that does not easily allow oxygen to diffuse as the conductive layer 574a.
[0333] Furthermore, a capacitor 540 is provided on the insulating layer 564. The capacitor 540 has a conductive layer 541, a conductive layer 545, and an insulating layer 543 located between them. The conductive layer 541 functions as one electrode of the capacitor 540, the conductive layer 545 functions as the other electrode of the capacitor 540, and the insulating layer 543 functions as the dielectric of the capacitor 540.
[0334] The conductive layer 541 is embedded in an insulating layer 554 provided on an insulating layer 564. The conductive layer 541 is electrically connected to the conductive layer 355 of the transistor 320 by a plug 574. The insulating layer 543 is provided covering the conductive layer 541. The conductive layer 545 is provided in the region that overlaps with the conductive layer 541 via the insulating layer 543.
[0335] An insulating layer 555a is provided covering the capacitance 540, an insulating layer 555b is provided on top of the insulating layer 555a, and an insulating layer 555c is provided on top of the insulating layer 555b.
[0336] Insulating layers 555a, 555b, and 555c can each preferably be made of inorganic insulating films. For example, it is preferable to use silicon oxide films for insulating layers 555a and 555c, and silicon nitride films for insulating layer 555b. This allows insulating layer 555b to function as an etching protective film. In this embodiment, an example is shown in which a part of insulating layer 555c is etched and a recess is formed, but the insulating layer 555c does not necessarily have to have a recess.
[0337] A light-emitting element 110R, a light-emitting element 110G, and a light-emitting element 110B are provided on the insulating layer 555c.
[0338] The light-emitting element 110R has a pixel electrode 111R, an organic layer 112R, a common layer 114, and a common electrode 113. The light-emitting element 110G has a pixel electrode 111G, an organic layer 112G, a common layer 114, and a common electrode 113. The light-emitting element 110B has a pixel electrode 111B, an organic layer 112B, a common layer 114, and a common electrode 113. The common layer 114 and the common electrode 113 are provided in common to the light-emitting elements 110R, 110G, and 110B.
[0339] The organic layer 112R of the light-emitting element 110R contains at least a luminescent organic compound that emits red light. The organic layer 112G of the light-emitting element 110G contains at least a luminescent organic compound that emits green light. The organic layer 112B of the light-emitting element 110B contains at least a luminescent organic compound that emits blue light. The organic layers 112R, 112G, and 112B can each also be called EL layers and each contains at least a luminescent substance (luminescent layer).
[0340] The display device 500A has different light-emitting devices for each light-emitting color, resulting in minimal change in chromaticity between low-brightness and high-brightness illumination. Furthermore, because the organic layers 112R, 112G, and 112B are separated, crosstalk between adjacent sub-pixels can be suppressed even in high-resolution display panels. Therefore, a display panel with high resolution and high display quality can be realized.
[0341] An insulating layer 125, a resin layer 126, and a layer 128 are provided in the region between adjacent light-emitting elements.
[0342] The pixel electrodes 111R, 111G, and 111B of the light-emitting element are electrically connected to the conductive layer 355 of the transistor 320 by plugs 556 embedded in insulating layers 555a, 555b, and 555c, a conductive layer 541 embedded in insulating layer 554, and plugs 574. The height of the upper surface of insulating layer 555c and the height of the upper surface of plug 556 are equal or approximately equal. Various conductive materials can be used for the plugs.
[0343] Furthermore, a protective layer 121 is provided on the light-emitting elements 110R, 110G, and 110B. The substrate 170 is bonded to the protective layer 121 by an adhesive layer 171.
[0344] There is no insulating layer covering the upper edge of the pixel electrode 111 between two adjacent pixel electrodes 111. Therefore, the spacing between adjacent light-emitting elements can be made extremely narrow. Consequently, a high-definition or high-resolution display device can be made.
[0345] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0346] (Embodiment 6) In this embodiment, an electronic device according to one aspect of the present invention will be described with reference to Figures 17 to 19.
[0347] The electronic device of this embodiment has a display panel (display device) to which a transistor according to one aspect of the present invention is applied in the display unit. The display device according to one aspect of the present invention can be easily made high-definition and high-resolution, and can achieve high display quality. Therefore, it can be used in the display unit of various electronic devices.
[0348] Examples of electronic devices include television sets, desktop or notebook personal computers, computer monitors, digital signage, and large game machines such as pachinko machines, as well as other electronic devices with relatively large screens, digital cameras, digital video cameras, digital photo frames, mobile phones, portable game consoles, personal digital assistants, and audio playback devices.
[0349] In particular, a display panel according to one embodiment of the present invention can be used suitably in electronic devices having a relatively small display area because it can increase the resolution. Examples of such electronic devices include wristwatch-type and bracelet-type information terminals (wearable devices), as well as wearable devices that can be worn on the head, such as VR devices such as head-mounted displays, AR devices such as glasses, and MR (Mixed Reality) devices.
[0350] A display panel according to one embodiment of the present invention preferably has an extremely high resolution such as HD (1280 x 720 pixels), FHD (1920 x 1080 pixels), WQHD (2560 x 1440 pixels), WQXGA (2560 x 1600 pixels), 4K (3840 x 2160 pixels), or 8K (7680 x 4320 pixels). In particular, a resolution of 4K, 8K, or higher is preferred. Furthermore, the pixel density (resolution) of the display panel according to one embodiment of the present invention is preferably 100 ppi or more, preferably 300 ppi or more, more preferably 500 ppi or more, more preferably 1000 ppi or more, more preferably 2000 ppi or more, more preferably 3000 ppi or more, more preferably 5000 ppi or more, and even more preferably 7000 ppi or more. By using a display panel having either high resolution or high detail, or both, it becomes possible to further enhance the sense of presence and depth. Furthermore, there are no particular limitations on the aspect ratio of the display panel in one embodiment of the present invention. For example, the display panel can support various aspect ratios such as 1:1 (square), 4:3, 16:9, and 16:10.
[0351] The electronic device of this embodiment may have sensors (including those with the function of detecting, detecting, or measuring force, displacement, position, velocity, acceleration, angular velocity, rotational speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared radiation).
[0352] The electronic device of this embodiment can have a variety of functions. For example, it can have a function to display various information (still images, videos, text images, etc.) on the display unit, a touch panel function, a function to display a calendar, date or time, a function to execute various software (programs), a wireless communication function, a function to read programs or data recorded on a recording medium, and so on.
[0353] Figures 17A to 17D illustrate an example of a wearable device that can be worn on the head. These wearable devices have one or both functions: the ability to display AR content and / or VR content. In addition to AR and VR, these wearable devices may also have the ability to display SR (Substantial Reality) or MR content. By having an electronic device that has the ability to display at least one of the following content types, such as AR, VR, SR, and MR, it is possible to enhance the user's sense of immersion.
[0354] The electronic device 700A shown in Figure 17A and the electronic device 700B shown in Figure 17B each include a pair of display panels 751, a pair of housings 721, a communication unit (not shown), a pair of mounting units 723, a control unit (not shown), an imaging unit (not shown), a pair of optical members 753, a frame 757, and a pair of nose pads 758.
[0355] A display panel according to one embodiment of the present invention can be applied to the display panel 751. Therefore, an electronic device capable of displaying extremely high resolution can be created.
[0356] Electronic devices 700A and 700B can project an image displayed on the display panel 751 onto the display area 756 of the optical element 753. Because the optical element 753 is translucent, the user can see the image displayed on the display area superimposed on the transmitted image visible through the optical element 753. Therefore, electronic devices 700A and 700B are electronic devices capable of AR display.
[0357] Electronic devices 700A and 700B may be equipped with cameras capable of capturing images of the area in front of them as imaging units. Furthermore, electronic devices 700A and 700B may each be equipped with acceleration sensors such as gyro sensors to detect the orientation of the user's head and display an image corresponding to that orientation in the display area 756.
[0358] The communications unit has a wireless communication device, which can supply video signals and the like. Alternatively, instead of the wireless communication device, or in addition to the wireless communication device, it may be equipped with a connector to which a cable supplying video signals and power potential can be connected.
[0359] Furthermore, electronic devices 700A and 700B are equipped with batteries that can be charged wirelessly, wired, or both.
[0360] The housing 721 may be equipped with a touch sensor module. The touch sensor module has the function of detecting when the outer surface of the housing 721 is touched. The touch sensor module can detect the user's tap or slide operations and perform various processes. For example, a tap operation can be used to pause or resume the video, and a slide operation can be used to fast forward or rewind. Furthermore, by providing a touch sensor module in each of the two housings 721, the range of operations can be expanded.
[0361] Various types of touch sensors can be applied to the touch sensor module. For example, various methods such as capacitive, resistive, infrared, electromagnetic induction, surface acoustic wave, and optical sensors can be used. In particular, it is preferable to apply a capacitive or optical sensor to the touch sensor module.
[0362] When using an optical touch sensor, a photoelectric conversion device (also called a photoelectric element) can be used as the light-receiving device (also called a photoelectric element). The active layer of the photoelectric conversion device can be made of either an inorganic semiconductor or an organic semiconductor, or both.
[0363] The electronic device 800A shown in Figure 17C and the electronic device 800B shown in Figure 17D each include a pair of display units 820, a housing 821, a communication unit 822, a pair of mounting units 823, a control unit 824, a pair of imaging units 825, and a pair of lenses 832.
[0364] A display panel according to one embodiment of the present invention can be applied to the display unit 820. Therefore, an electronic device capable of displaying extremely high resolution can be created. This allows the user to experience a high level of immersion.
[0365] The display unit 820 is located inside the housing 821 in a position visible through the lens 832. Furthermore, by displaying different images on a pair of display units 820, a three-dimensional display using parallax can be achieved.
[0366] Electronic devices 800A and 800B can each be described as electronic devices for VR. A user wearing electronic device 800A or electronic device 800B can view the image displayed on the display unit 820 through the lens 832.
[0367] It is preferable that electronic devices 800A and 800B each have a mechanism that allows adjustment of the left and right positions of the lens 832 and the display unit 820 so that they are in the optimal position according to the user's eye position. It is also preferable that they have a mechanism that adjusts the focus by changing the distance between the lens 832 and the display unit 820.
[0368] The attachment portion 823 allows the user to attach the electronic device 800A or 800B to their head. While Figure 17C and other figures illustrate the attachment portion as resembling the temples (or arms) of eyeglasses, it is not limited to this shape. The attachment portion 823 only needs to be wearable by the user; for example, it may be helmet-shaped or band-shaped.
[0369] The imaging unit 825 has the function of acquiring external information. The data acquired by the imaging unit 825 can be output to the display unit 820. An image sensor can be used in the imaging unit 825. In addition, multiple cameras may be provided to accommodate multiple angles of view, such as telephoto and wide-angle.
[0370] Although an example with an imaging unit 825 is shown here, any distance measuring sensor (hereinafter also referred to as a detection unit) capable of measuring the distance to an object can be provided. In other words, the imaging unit 825 is one form of the detection unit. As the detection unit, for example, an image sensor or a distance image sensor such as LiDAR (Light Detection and Ranging) can be used. By using the image obtained by the camera and the image obtained by the distance image sensor, more information can be acquired, enabling more accurate gesture control.
[0371] The electronic device 800A may have a vibration mechanism that functions as a bone conduction earphone. For example, a configuration having such a vibration mechanism can be applied to one or more of the display unit 820, housing 821, and mounting unit 823. This allows users to enjoy video and audio simply by wearing the electronic device 800A, without needing separate audio equipment such as headphones, earphones, or speakers.
[0372] Electronic devices 800A and 800B may each have input terminals. Cables can be connected to the input terminals to supply video signals from video output devices, etc., and power for charging batteries provided in the electronic devices.
[0373] An electronic device according to one aspect of the present invention may have a function for wireless communication with an earphone 750. The earphone 750 has a communication unit (not shown) and has a wireless communication function. The earphone 750 can receive information (e.g., voice data) from the electronic device through its wireless communication function. For example, the electronic device 700A shown in Figure 17A has a function for transmitting information to the earphone 750 through its wireless communication function. Also, for example, the electronic device 800A shown in Figure 17C has a function for transmitting information to the earphone 750 through its wireless communication function.
[0374] Furthermore, the electronic device may have an earphone section. The electronic device 700B shown in Figure 17B has an earphone section 727. For example, the earphone section 727 and the control unit can be connected to each other by wire. Part of the wiring connecting the earphone section 727 and the control unit may be located inside the housing 721 or the mounting section 723.
[0375] Similarly, the electronic device 800B shown in Figure 17D has an earphone unit 827. For example, the earphone unit 827 and the control unit 824 can be connected to each other by a wire. Part of the wiring connecting the earphone unit 827 and the control unit 824 may be located inside the housing 821 or the mounting unit 823. Also, the earphone unit 827 and the mounting unit 823 may have magnets. This allows the earphone unit 827 to be fixed to the mounting unit 823 by magnetic force, which is preferable as it facilitates storage.
[0376] Furthermore, the electronic device may have an audio output terminal to which earphones or headphones can be connected. The electronic device may also have an audio input terminal and / or an audio input mechanism. For example, a sound-collecting device such as a microphone can be used as the audio input mechanism. By having an audio input mechanism, the electronic device may be given the function of a so-called headset.
[0377] Thus, as one embodiment of the present invention, both eyeglass-type (electronic devices 700A and 700B, etc.) and goggle-type (electronic devices 800A and 800B, etc.) are preferred as electronic devices.
[0378] The electronic device 6500 illustrated in FIG. 18A is a portable information terminal that can be used as a smartphone.
[0379] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, buttons 6504, a speaker 6505, a microphone 6506, a camera 6507, a light source 6508, a control device 6509, and the like. The display portion 6502 has a touch panel function. Note that the control device 6509 includes, for example, one or more selected from a CPU, a GPU (Graphics Processing Unit), and a storage device. The semiconductor device of one embodiment of the present invention can be applied to the display portion 6502, the control device 6509, and the like. Using the semiconductor device of one embodiment of the present invention for the control device 6509 is preferable because power consumption can be reduced.
[0380] The display panel of one embodiment of the present invention can be applied to the display portion 6502.
[0381] FIG. 18B is a schematic cross-sectional view including an end portion of the housing 6501 on the microphone 6506 side.
[0382] A light-transmitting protective member 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, an optical member 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, and the like are arranged in a space surrounded by the housing 6501 and the protective member 6510.
[0383] The display panel 6511, the optical member 6512, and the touch sensor panel 6513 are fixed to the protective member 6510 with an adhesive layer (not illustrated).
[0384] Part of the display panel 6511 is folded back in a region outside the display portion 6502, and an FPC 6515 is connected to the folded portion. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on the printed circuit board 6517.
[0385] A display device according to one embodiment of the present invention can be applied to the display panel 6511. As a result, an extremely lightweight electronic device can be realized. Furthermore, because the display panel 6511 is extremely thin, a large-capacity battery 6518 can be installed while keeping the thickness of the electronic device low. In addition, by folding back a part of the display panel 6511 and placing the connection part with the FPC 6515 on the back of the pixel section, an electronic device with a narrow bezel can be realized.
[0386] Figure 18C shows an example of a television system. The television system 7100 has a display unit 7000 incorporated into a housing 7101. Here, the housing 7101 is shown to be supported by a stand 7103.
[0387] The television device 7100 shown in Figure 18C can be operated using the operation switches on the housing 7101 and a separate remote control unit 7111. Alternatively, the display unit 7000 may be equipped with a touch sensor, and the television device 7100 can be operated by touching the display unit 7000 with a finger or the like. The remote control unit 7111 may have a display unit that displays information output from the remote control unit 7111. Channels and volume can be controlled and the image displayed on the display unit 7000 can be controlled using the operation keys or touch panel on the remote control unit 7111.
[0388] The television system 7100 is configured to include a receiver and a modem. The receiver can receive general television broadcasts. Furthermore, by connecting to a wired or wireless communication network via the modem, it is possible to perform one-way (from sender to receiver) or two-way (between sender and receiver, or between receivers, etc.) information communication.
[0389] Figure 18D shows an example of a notebook personal computer. The notebook personal computer 7200 includes a casing 7211, a keyboard 7212, a pointing device 7213, an external connection port 7214, a control device 7216, etc. A display unit 7000 is incorporated into the casing 7211. The control device 7216 includes, for example, one or more selected from a CPU, a GPU, and a storage device. A semiconductor device according to one aspect of the present invention can be applied to the display unit 7000, the control device 7216, etc. Using a semiconductor device according to one aspect of the present invention as the control device 7216 is preferable because it can reduce power consumption.
[0390] Figures 18E and 18F show examples of digital signage.
[0391] The digital signage 7300 shown in Figure 18E includes a housing 7301, a display unit 7000, and a speaker 7303, etc. Furthermore, it may include LED lamps, operation keys (including a power switch or operation switch), connection terminals, various sensors, a microphone, etc.
[0392] Figure 18F shows a digital signage 7400 mounted on a cylindrical column 7401. The digital signage 7400 has a display unit 7000 that is provided along the curved surface of the column 7401.
[0393] The larger the display area 7000, the more information can be provided at once. Furthermore, a larger display area 7000 is more eye-catching, which can, for example, enhance the effectiveness of advertising.
[0394] Applying a touch panel to the display unit 7000 is preferable because it not only allows images or videos to be displayed on the display unit 7000, but also enables intuitive operation by the user. Furthermore, when used for purposes such as providing route information or traffic information, intuitive operation can enhance usability.
[0395] Furthermore, as shown in Figures 18E and 18F, it is preferable that the digital signage 7300 or digital signage 7400 can be linked wirelessly with an information terminal 7311 or information terminal 7411 such as a smartphone owned by the user. For example, the advertising information displayed on the display unit 7000 can be displayed on the screen of the information terminal 7311 or information terminal 7411. Also, the display on the display unit 7000 can be switched by operating the information terminal 7311 or information terminal 7411.
[0396] Furthermore, the digital signage 7300 or digital signage 7400 can be used to run games using the screen of the information terminal 7311 or information terminal 7411 as the control device (controller). This allows an unspecified number of users to participate in and enjoy the game simultaneously.
[0397] In Figures 18C to 18F, a display panel according to one embodiment of the present invention can be applied to the display unit 7000.
[0398] The electronic device shown in Figures 19A to 19G includes a housing 9000, a display unit 9001, a speaker 9003, operation keys 9005 (including a power switch or operation switch), connection terminals 9006, a sensor 9007 (including a function to detect, identify, or measure force, displacement, position, velocity, acceleration, angular velocity, rotational speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared radiation), a microphone 9008, etc.
[0399] The electronic devices shown in Figures 19A to 19G have various functions. For example, they may have functions to display various information (still images, videos, text images, etc.) on a display unit, a touch panel function, a function to display a calendar, date or time, a function to control processing by various software (programs), a wireless communication function, a function to read and process programs or data recorded on a recording medium, etc. However, the functions of electronic devices are not limited to these and can have various functions. Electronic devices may have multiple display units. Furthermore, electronic devices may be equipped with a camera, etc., and have functions to capture still images or videos and save them on a recording medium (external or built into the camera), a function to display the captured images on a display unit, etc.
[0400] Details of the electronic equipment shown in Figures 19A to 19G will be explained below.
[0401] Figure 19A is a perspective view showing a personal digital information terminal (PDI) 9101. The PDI 9101 can be used, for example, as a smartphone. The PDI 9101 may also be equipped with a speaker 9003, connection terminals 9006, sensors 9007, etc. Furthermore, the PDI 9101 can display text and image information on multiple surfaces. Figure 19A shows an example where three icons 9050 are displayed. Information 9051, indicated by a dashed rectangle, can also be displayed on other surfaces of the display unit 9001. Examples of information 9051 include notifications of incoming emails, SNS messages, and phone calls, the subject of an email or SNS message, the sender's name, date and time, battery level, and signal strength. Alternatively, icons 9050 or the like may be displayed in the location where the information 9051 is displayed.
[0402] Figure 19B is a perspective view showing a personal digital assistant (PDA) 9102. The PDA 9102 has the function of displaying information on three or more sides of the display unit 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different sides. For example, a user can check information 9053, which is displayed in a position that can be observed from above the PDA 9102, while the PDA 9102 is stored in the breast pocket of their clothing. The user can check the display without taking the PDA 9102 out of their pocket and decide, for example, whether or not to answer a call.
[0403] Figure 19C is a perspective view showing the tablet terminal 9103. The tablet terminal 9103 can run various applications, such as mobile phone calls, email, document viewing and creation, music playback, internet communication, and computer games. The tablet terminal 9103 has a display unit 9001, a camera 9002, a microphone 9008, and a speaker 9003 on the front of the housing 9000. The left side of the housing 9000 has operation keys 9005 as buttons for operation, and the bottom has connection terminals 9006.
[0404] Figure 19D is a perspective view showing a wristwatch-type personal information terminal 9200. The personal information terminal 9200 can be used, for example, as a smartwatch (registered trademark). The display unit 9001 has a curved display surface, allowing it to display information along the curved surface. The personal information terminal 9200 can also make hands-free calls by communicating with, for example, a wireless communication headset. Furthermore, the personal information terminal 9200 can transmit data to other information terminals and be charged via a connection terminal 9006. The charging operation may be performed by wireless power supply.
[0405] Figures 19E to 19G are perspective views showing a foldable portable information terminal 9201. Figure 19E shows the portable information terminal 9201 in an unfolded state, Figure 19G shows it in a folded state, and Figure 19F shows a perspective view of the state in between, transitioning from one of Figures 19E or 19G to the other. The portable information terminal 9201 offers excellent portability in its folded state and excellent readability of the display due to its seamless, wide display area in its unfolded state. The display unit 9001 of the portable information terminal 9201 is supported by three housings 9000 connected by hinges 9055. For example, the display unit 9001 can be bent with a radius of curvature of 0.1 mm to 150 mm.
[0406] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0407] (Embodiment 7) This embodiment describes an application example of a semiconductor device according to one aspect of the present invention. A semiconductor device according to one aspect of the present invention can be used, for example, in electronic components, electronic devices, large computers, space equipment, and data centers (also referred to as Data Centers: DCs). Electronic components, electronic devices, large computers, space equipment, and data centers using a semiconductor device according to one aspect of the present invention are effective in achieving high performance, such as low power consumption.
[0408] Electronic components and the like to which a semiconductor device according to one embodiment of the present invention is applied can be applied to the electronic device exemplified in Embodiment 6.
[0409] [Electronic Components] Figure 20A shows a perspective view of a substrate (mounted substrate 704) on which electronic components 700 are mounted. The electronic component 700 shown in Figure 20A has a semiconductor device 710 inside a mold 711. Some details are omitted in Figure 20A to show the inside of the electronic component 700. The electronic component 700 has a land 712 on the outside of the mold 711. The land 712 is electrically connected to an electrode pad 713, and the electrode pad 713 is electrically connected to the semiconductor device 710 via a wire 714. The electronic component 700 is mounted on a printed circuit board 702, for example. Multiple such electronic components are combined and electrically connected on the printed circuit board 702 to complete the mounted substrate 704.
[0410] Furthermore, the semiconductor device 710 includes a drive circuit layer 715 and a storage layer 716. The storage layer 716 has a configuration in which multiple memory cell arrays are stacked. The configuration in which the drive circuit layer 715 and the storage layer 716 are stacked can be a monolithic stack configuration. In a monolithic stack configuration, the layers can be connected without using through-electrode technologies such as TSV (Through Silicon Via) and bonding technologies such as Cu-Cu direct bonding. By configuring the drive circuit layer 715 and the storage layer 716 in a monolithic stack configuration, for example, a so-called on-chip memory configuration can be achieved in which memory is directly formed on the processor. By using an on-chip memory configuration, it is possible to speed up the operation of the interface portion between the processor and the memory.
[0411] Furthermore, by using an on-chip memory configuration, the size of connection wiring can be reduced compared to technologies using through-hole electrodes such as TSVs, making it possible to increase the number of connection pins. Increasing the number of connection pins enables parallel operation, which in turn improves the memory bandwidth (also called memory bandwidth).
[0412] Further, it is preferable that the plurality of memory cell arrays included in the memory layer 716 are formed using OS transistors, and the plurality of memory cell arrays are monolithically stacked. By employing a monolithic stacking configuration for the plurality of memory cell arrays, one or both of the memory bandwidth and the memory access latency can be improved. Note that the bandwidth refers to the amount of data transferred per unit time, and the access latency refers to the time from when access is initiated until data exchange starts. Note that in the case of a configuration using Si transistors for the memory layer 716, it is more difficult to adopt a monolithic stacking configuration compared to using OS transistors. Therefore, in a monolithic stacking configuration, OS transistors can be said to have a superior structure to Si transistors.
[0413] Further, the semiconductor device 710 may also be referred to as a die. Note that in this specification and the like, a die refers to a chip piece obtained by forming a circuit pattern on, for example, a disk-shaped substrate (also referred to as a wafer) in a semiconductor chip manufacturing process, and cutting the substrate into a grid. Examples of semiconductor materials that can be used for the die include silicon (Si), silicon carbide (SiC), gallium nitride (GaN), and the like. For example, a die obtained from a silicon substrate (also referred to as a silicon wafer) may be referred to as a silicon die in some cases.
[0414] Next, a perspective view of the electronic component 730 is shown in FIG. 20B. The electronic component 730 is an example of a SiP (System in Package) or an MCM (Multi Chip Module). In the electronic component 730, an interposer 731 is provided over a package substrate 732 (printed wiring board), and a semiconductor device 735 and a plurality of semiconductor devices 710 are provided over the interposer 731.
[0415] The electronic component 730 illustrates an example in which the semiconductor device 710 is used as a high-bandwidth memory (HBM: High Bandwidth Memory). Further, the semiconductor device 735 can be used for an integrated circuit such as a CPU, a GPU, or an FPGA (Field Programmable Gate Array).
[0416] The package substrate 732 can be, for example, a ceramic substrate, a plastic substrate, or a glass epoxy substrate. The interposer 731 can be, for example, a silicon interposer or a resin interposer.
[0417] The interposer 731 has multiple wirings and functions to electrically connect multiple integrated circuits with different terminal pitches. The multiple wirings are provided in a single layer or multiple layers. The interposer 731 also functions to electrically connect integrated circuits provided on the interposer 731 to electrodes provided on the package substrate 732. For these reasons, the interposer is sometimes called a "redistribution board" or "intermediate board". In addition, through electrodes may be provided on the interposer 731, and these through electrodes may be used to electrically connect the integrated circuits and the package substrate 732. Furthermore, in silicon interposers, TSVs can also be used as through electrodes.
[0418] In HBMs, many connections are necessary to achieve a wide memory bandwidth. Therefore, the interposer on which the HBM is mounted requires fine and high-density wiring. For this reason, it is preferable to use a silicon interposer for mounting the HBM.
[0419] Furthermore, in SiP and MCM using silicon interposers, reliability degradation due to differences in expansion coefficients between the integrated circuit and the interposer is less likely to occur. In addition, because silicon interposers have high surface flatness, connection failures between the integrated circuit and the silicon interposer are less likely to occur. In particular, in 2.5D packages (2.5-dimensional packaging) where multiple integrated circuits are arranged side by side on the interposer, it is preferable to use a silicon interposer.
[0420] On the other hand, when electrically connecting multiple integrated circuits with different terminal pitches using silicon interposers and TSVs, space is required, such as the width of the terminal pitch. Therefore, when attempting to reduce the size of the electronic component 730, the width of the terminal pitch becomes a problem, and it may become difficult to provide the many wires necessary to achieve a wide memory bandwidth. For this reason, as mentioned above, a monolithic stacked configuration using OS transistors is preferable. A composite structure combining a memory cell array stacked using TSVs and a monolithic stacked memory cell array may also be used.
[0421] Alternatively, a heat sink (heat dissipation plate) may be provided on top of the electronic component 730. If a heat sink is provided, it is preferable to align the heights of the integrated circuits provided on the interposer 731. For example, in the electronic component 730 shown in this embodiment, it is preferable to align the heights of the semiconductor device 710 and the semiconductor device 735.
[0422] To mount the electronic component 730 onto another substrate, electrodes 733 may be provided at the bottom of the package substrate 732. Figure 20B shows an example in which the electrodes 733 are formed with solder balls. By providing solder balls in a matrix at the bottom of the package substrate 732, BGA (Ball Grid Array) mounting can be achieved. Alternatively, the electrodes 733 may be formed with conductive pins. By providing conductive pins in a matrix at the bottom of the package substrate 732, PGA (Pin Grid Array) mounting can be achieved.
[0423] The electronic component 730 can be mounted on other boards using various mounting methods, not limited to BGA and PGA. Examples of mounting methods include SPGA (Staggered Pin Grid Array), LGA (Land Grid Array), QFP (Quad Flat Package), QFJ (Quad Flat J-leaded package), and QFN (Quad Flat Non-leaded package).
[0424] [Large-scale computer] Figure 21A shows a perspective view of the large-scale computer 5600. The large-scale computer 5600 houses multiple rack-mount type computers 5620 in rack 5610. The large-scale computer 5600 may also be referred to as a supercomputer.
[0425] Figure 21B shows a perspective view of an example of a computer 5620. The computer 5620 has a motherboard 5630. The motherboard 5630 is provided with multiple slots 5631 and multiple connection terminals. A PC card 5621 is inserted into a slot 5631. In addition, the PC card 5621 has connection terminals 5623, 5624, and 5625, which are connected to the motherboard 5630.
[0426] Figure 21C shows an example of a PC card 5621. The PC card 5621 is a processing board equipped with, for example, a CPU, GPU, and memory device. The PC card 5621 has a board 5622 and connection terminals 5623, 5624, 5625, electronic component 5626, electronic component 5627, electronic component 5628, and connection terminal 5629 mounted on the board 5622. Note that Figure 21C shows components other than electronic component 5626, electronic component 5627, and electronic component 5628.
[0427] The connector 5629 has a shape that allows it to be inserted into the slot 5631 of the motherboard 5630, and functions as an interface for connecting the PC card 5621 and the motherboard 5630. Examples of standards for the connector 5629 include PCIe.
[0428] Terminals 5623, 5624, and 5625 can serve as interfaces for, for example, power supply and signal input to the PC card 5621. They can also serve as interfaces for, for example, outputting signals calculated by the PC card 5621. Examples of standards for terminals 5623, 5624, and 5625 include USB (Universal Serial Bus), SATA (Serial ATA), and SCSI (Small Computer System Interface). When outputting video signals from terminals 5623, 5624, and 5625, examples of standards include HDMI (registered trademark).
[0429] The electronic component 5626 has terminals (not shown) for inputting and outputting signals, and by inserting these terminals into a socket (not shown) on the board 5622, the electronic component 5626 and the board 5622 can be electrically connected.
[0430] Electronic components 5627 and 5628 have multiple terminals, and these terminals can be mounted to the wiring provided on board 5622 by, for example, reflow soldering. Examples of electronic component 5627 include FPGAs, GPUs, and CPUs. For example, electronic component 730 can be used as electronic component 5627. Examples of electronic component 5628 include memory devices. For example, electronic component 700 can be used as electronic component 5628.
[0431] The 5600 mainframe computer can also function as a parallel computer. By using the 5600 mainframe computer as a parallel computer, it is possible to perform large-scale calculations necessary for, for example, artificial intelligence training and inference.
[0432] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.
[0433] In this example, the temperature dependence of stress on the metal oxide film was measured.
[0434] [Sample Preparation] In this example, three types of samples (Sample A1 to Sample A3) were prepared. For all samples, a metal oxide film with a thickness of approximately 200 nm was formed on a silicon wafer by sputtering.
[0435] Sample A1 had an indium oxide film formed as a metal oxide film. The metal oxide film was deposited using an indium oxide target as the sputtering target, argon gas as the deposition gas, and at room temperature on the substrate.
[0436] Samples A2 and A3 formed indium oxide films with gallium added as the metal oxide film. Sample A2 used an indium oxide target containing 0.5 atomic% Ga. Sample A3 used an indium oxide target containing 5.0 atomic% Ga. All other conditions were the same as for sample A1.
[0437] Based on the above, samples A1 to A3 were prepared.
[0438] [Stress Measurement] Stress was measured on the prepared samples A1 to A3 while varying the temperature. A thin-film stress measuring device FLX2320S (manufactured by Toho Technology Co., Ltd.) was used for stress measurement. The heating rate was 5°C per minute, and cooling was allowed by natural cooling. Stress measurements were taken each time the temperature changed by 5°C. The error in stress measurement was ±5%.
[0439] Figures 22A to 22C show the temperature dependence of stress for Sample A1, Sample A2, and Sample A3, respectively. In the figures, the dashed line corresponds to 25°C (equivalent to room temperature).
[0440] As shown in Figure 22A, the indium oxide film exhibited negative stress before heating. This indicates that the indium oxide film exhibits compressive stress. As the temperature increased, the absolute value of the stress tended to increase between approximately 25°C and 150°C, and the slope changed between 150°C and 200°C, with the absolute value of the stress decreasing (approaching 0). This suggests that the temperature dependence of the stress changed due to the crystallization of the indium oxide film. Above 300°C, the stress changed from compressive to tensile, and at 400°C, it showed positive stress. Subsequently, as the temperature decreased from 400°C, the stress tended to increase gradually, and around 25°C, it showed tensile stress, with the absolute value of the stress being similar to or smaller than that of the pre-heating state. From the above, it was suggested that heating at a temperature of 150°C or higher, preferably 200°C or higher, causes the indium oxide film to crystallize, that is, the crystallinity of the indium oxide film can be improved. Therefore, it was suggested that heat treatment can form semiconductor films with high crystallinity and good electrical properties.
[0441] As shown in Figure 22B, in sample A2, the temperature at which the gradient of crystallization changed was between 200°C and 250°C, which is a higher temperature compared to sample A1. This suggests that the addition of Ga makes crystallization more difficult. Furthermore, compressive stress was observed even when the temperature reached 400°C. During cooling, the stress increased gradually, changing from compressive stress to tensile stress around 150°C, and showing tensile stress around 25°C. The absolute value of the stress was smaller than that of the state before heating.
[0442] As shown in Figure 22C, in sample A3, the slope changed and the stress increased between 150°C and 200°C as the temperature rose, but it always showed negative stress. Furthermore, the slope changed again near 250°C, and there was a tendency for the magnitude of the compressive stress to increase. Also, as the temperature decreased, the stress gradually relaxed and approached zero, but near 25°C, the compressive stress was the same as before heating. Since sample A3 exhibits a different trend during heating compared to samples A1 and A2, it is suggested that it has a different crystal structure, or that different crystal structures are mixed together.
[0443] From the above results, it was confirmed that in all samples, stress was relieved as crystallization occurred due to heating. Furthermore, it was found that even when the film deposition temperature and thickness were the same, the magnitude and sign of the absolute value of the film stress before and after heat treatment differed depending on the composition of the film. It was confirmed that by stacking two or more such films, the film stress after heat treatment can be reduced to zero or approached to zero. For example, a laminated film of a relatively easily crystallized indium oxide film and a gallium-doped indium oxide film, in which the absolute value of the film stress after heat treatment is smaller than that before heat treatment, is suitable for semiconductor films.
[0444] In this example, a transistor according to one aspect of the present invention was fabricated and its electrical characteristics were measured.
[0445] In this embodiment, two types of samples (sample B1 and sample B2) were prepared. The configuration of the prepared transistors can be found in the transistor shown in Figure 3B, which was illustrated in Embodiment 2 above.
[0446] [Sample Preparation] For both Sample B1 and Sample B2, first, an aluminum oxide film and a silicon oxide film were formed on the silicon wafer substrate as an underlayer insulating layer by sputtering. Then, a portion of the silicon oxide film was removed to form a groove for embedding the back gate electrode. Subsequently, a titanium nitride film and a tungsten film were formed as the back gate electrode by CVD, and then planarized by CMP until the silicon oxide film was exposed. Next, a silicon nitride film and a hafnium oxide film were formed as the back gate insulating layer by ALD, and then a silicon oxide film was further formed by sputtering.
[0447] Next, a semiconductor film was formed. Here, a four-layer laminated film was used as the semiconductor film. First, an In-Ga-Zn oxide film with a thickness of approximately 10 nm and a gallium oxide film with a thickness of approximately 2 nm were formed by sputtering. Subsequently, an indium oxide film with a thickness of approximately 6 nm and an In-Ga oxide film with a thickness of approximately 4 nm were formed by ALD (Advanced Laser Deposition). The In-Ga-Zn oxide film was formed using a metal oxide target with a metal element composition of In:Ga:Zn = 1:3:2. For the In-Ga oxide film, the ALD deposition cycle was adjusted so that In:Ga = 4:1.
[0448] Next, the first heat treatment was performed. The first heat treatment was carried out using an RTA apparatus at 650°C for 6 minutes in an atmosphere containing nitrogen gas and oxygen gas.
[0449] Next, an In-Sn oxide film and a tungsten film were formed as conductive films to serve as the source and drain electrodes by sputtering. These conductive films and the semiconductor film were then etched to create island-like structures. This resulted in a semiconductor layer and the source and drain electrodes located on it. Subsequently, a silicon nitride film was deposited as a protective layer. Next, a silicon oxide film and a silicon nitride film were formed as interlayer insulating films by sputtering, and then planarized by CMP until the silicon oxide film was exposed. Finally, the interlayer insulating layer and parts of the source and drain electrodes were etched to expose parts of the semiconductor layer.
[0450] Next, hafnium oxide film, silicon oxide film, hafnium oxide film, and silicon nitride film were deposited as gate insulating layers by ALD method. Subsequently, titanium nitride film and tungsten film were deposited as gate electrodes, and then planarized by CMP method until the interlayer insulating film was exposed. Next, aluminum oxide film, silicon nitride film, and silicon oxide film were deposited as protective layers by sputtering method. Next, openings reaching the source electrode and drain electrode were formed in the interlayer insulating layer. After that, silicon nitride film was formed as a protective layer in contact with the side surface of the opening by ALD method. Next, titanium nitride film and tungsten film were formed as plugs to fill the opening by CVD method, and then planarized by CMP method until the interlayer insulating layer was exposed. Subsequently, titanium film, titanium nitride film, aluminum film, titanium film, and titanium nitride film were formed by sputtering method, and these were processed to obtain wiring.
[0451] Next, only sample B2 underwent a second heat treatment. The second heat treatment was carried out in an electric furnace at 400°C for 4 hours in an atmosphere containing nitrogen gas.
[0452] Based on the above, samples B1 and B2 were obtained.
[0453] [Evaluation of Transistor Electrical Characteristics] The Id-Vg characteristics of the transistors contained in sample B1 and sample B2 were measured. The channel length L and channel width W of the measured transistors were 0.388 μm and 0.323 μm, respectively. The measurement was performed by setting the drain voltage to 0.1 V or 1.2 V and measuring the source-drain current when the gate voltage was swept from -4 V to 4 V. Figures 23A and 23B show the Id-Vg characteristics of sample B1 and sample B2, respectively. The field-effect mobility (μFE) derived from the Id-Vg characteristics is also shown in each figure. The number of measurements, excluding outliers, was 23 for both sample B1 and sample B2.
[0454] As shown in Figures 23A and 23B, both sample B1 and sample B2 were confirmed to exhibit good electrical characteristics. Focusing on the median threshold voltage (Vth), sample B1 had a threshold voltage of -0.27V, while sample B2 had a threshold voltage of -0.01V. In other words, it was confirmed that the threshold voltage shifted positively after the second heat treatment. This can be attributed to the reduction of defects in the channel formation region due to the second heat treatment.
[0455] In this example, a transistor according to one embodiment of the present invention was fabricated and its electrical characteristics were evaluated.
[0456] In this embodiment, sample C was prepared, which included a transistor with a different semiconductor layer configuration than that of Example 2.
[0457] [Sample Preparation] For sample C, steps other than the semiconductor layer fabrication step can be followed in the example of Example 2 described above.
[0458] Here, a three-layer laminated film was used as the semiconductor film. First, a gallium oxide film with a thickness of approximately 2 nm was formed by sputtering, and then an indium oxide film with a thickness of approximately 6 nm and an In-Ga oxide film with a thickness of approximately 4 nm were formed by ALD (Advanced Laser Deposition). In other words, the semiconductor film of sample C corresponds to the semiconductor films of samples B1 and B2 described above, with the In-Ga-Zn oxide film omitted.
[0459] Furthermore, in sample C, similar to sample B2 in Example 2, a first heat treatment was performed after the semiconductor film was formed, and a second heat treatment was performed after the wiring was formed.
[0460] [Evaluation of Transistor Electrical Characteristics] The Id-Vg characteristics of the transistor contained in sample C were measured. The channel length L and channel width W of the measured transistor were 5.021 μm and 0.322 μm, respectively. The measurement was performed in the same manner as in Example 2. The number of measurements, excluding outliers, was 24.
[0461] Figure 24 shows the Id-Vg characteristics of sample C. It was confirmed that the transistors in sample C exhibited good electrical characteristics with little variation. Focusing on the maximum value of the field-effect mobility (μFE), the median value under the condition Vd = 0.1V was 103.2 cm⁻¹.2 The value of / Vs was extremely high.
[0462] From these results, it was confirmed that by performing both the first and second heat treatments, a transistor with extremely good electrical characteristics can be obtained.
[0463] 11: Substrate, 12: Insulating layer, 21: Semiconductor layer, 21f: Semiconductor film, 22: Insulating layer, 23: Conductive layer, 31: Insulating layer, 110B: Light-emitting element, 110G: Light-emitting element, 110R: Light-emitting element, 111: Pixel electrode, 111B: Pixel electrode, 111G: Pixel electrode, 111R: Pixel electrode, 112B: Organic layer, 112G: Organic layer, 112R: Organic layer, 113: Common electrode, 114: Common layer, 121: Protective layer, 125: Insulating layer, 126: Resin layer, 128: Layer, 170: Substrate, 171: Adhesive layer, 200: Transistor, 200a: Transistor, 201: Insulating layer, 202: Insulating layer, 2 05: conductive layer, 210: substrate, 230: semiconductor layer, 230a: oxide layer, 230b: oxide layer, 230c: oxide layer, 230f: semiconductor film, 230n: region, 240a: conductive layer, 240b: conductive layer, 241a: insulating layer, 241b: insulating layer, 242: conductive layer, 242a: conductive layer, 242b: conductive layer, 242f: conductive film, 250: insulating layer, 255: insulating layer, 260: conductive layer, 260a: conductive layer, 260b: conductive layer, 271a: insulating layer, 271b: insulating layer, 275: insulating layer, 280: insulating layer, 281: insulating layer, 282: insulating layer, 283: insulating layer, 285: insulating layer, 301: substrate, 310: transistor, 311: conductive layer, 312: low-resistance region, 313: insulating layer, 314: insulating layer, 315: element isolation layer, 316: wiring layer, 320: transistor, 350: insulating layer, 351: semiconductor layer, 352: insulating layer, 353: insulating layer, 354: conductive layer, 355: conductive layer, 356: insulating layer, 357: conductive layer, 358: insulating layer, 359: insulating layer, 420: layer, 422: peripheral circuit, 430[1]: element layer, 430[5]: element layer, 430[m]: element layer, 430: element layer, 432[1,1]: memory cell, 432[m,n]: memory cell, 43 2: Memory cell, 437: Transistor, 438: Capacitive element, 440: Drive circuit, 442: Row decoder, 443: Row driver, 444: Column decoder, 445: Column driver, 446: Sense amplifier, 447: Input circuit, 448: Output circuit, 470: Layer, 471: PSW, 472: PSW, 473: Control circuit, 474: Voltage generation circuit, 480: Memory device, 482: Switch circuit, 482_1: Transistor, 482_2: Transistor, 483: Precharge circuit, 483_1: Transistor, 483_3: Transistor, 484: Precharge circuit,484_1: Transistor, 484_3: Transistor, 485: Amplifier circuit, 485_1: Transistor, 485_2: Transistor, 485_3: Transistor, 485_4: Transistor, 500A: Display device, 540: Capacitor, 541: Conductive layer, 543: Insulating layer, 545: Conductive layer, 554: Insulating layer, 555a: Insulating layer, 555b: Insulating layer, 555c: Insulating layer, 556: Plug, 564: Insulating layer, 574: Plug, 574a: Conductive layer, 574b: Conductive layer, 580: Display module, 581: Display unit, 582: Circuit unit, 583: Pixel circuit unit, 583a: Pixel circuit, 584: Pixel section, 584a: Pixel, 585: Terminal section, 586: Wiring section, 590: FPC, 591: Substrate, 592: Substrate, 700: Electronic component, 700A: Electronic device, 700B: Electronic device, 702: Printed circuit board, 704: Mounted substrate, 710: Semiconductor device, 711: Mold, 712: Land, 713: Electrode pad, 714: Wire, 715: Drive circuit layer, 716: Memory layer, 721: Housing, 723: Mounting section, 727: Earphone section, 730: Electronic component, 731: Interposer, 732: Package substrate, 733: Electrode, 735: Semiconductor device, 750 : Earphone, 751: Display panel, 753: Optical component, 756: Display area, 757: Frame, 758: Nose pad, 800A: Electronic equipment, 800B: Electronic equipment, 820: Display unit, 821: Housing, 822: Communication unit, 823: Mounting unit, 824: Control unit, 825: Imaging unit, 827: Earphone unit, 832: Lens, 5600: Large computer, 5610: Rack, 5620: Computer, 5621: PC card, 5622: Board, 5623: Connection terminal, 5624: Connection terminal, 5625: Connection terminal, 5626: Electronic component, 5627: Electronic component, 5628: Electronic component, 56 29: Connection terminal, 5630: Motherboard, 5631: Slot, 6500: Electronic equipment, 6501: Enclosure, 6502: Display unit, 6503: Power button, 6504: Button, 6505: Speaker, 6506: Microphone, 6507: Camera, 6508: Light source, 6509: Control device, 6510: Protective component, 6511: Display panel, 6512: Optical component, 6513: Touch sensor panel, 6515: FPC, 6516: IC, 6517: Printed circuit board, 6518: Battery, 7000: Display unit, 7100: Television equipment, 7101: Enclosure, 7103: Stand,7111: Remote control unit, 7200: Notebook personal computer, 7211: Enclosure, 7212: Keyboard, 7213: Pointing device, 7214: External connection port, 7216: Control unit, 7300: Digital signage, 7301: Enclosure, 7303: Speaker, 7311: Information terminal, 7400: Digital signage, 7401: Pillar, 7411: Information terminal, 9000: Enclosure, 90 01: Display unit, 9002: Camera, 9003: Speaker, 9005: Operation keys, 9006: Connection terminal, 9007: Sensor, 9008: Microphone, 9050: Icon, 9051: Information, 9052: Information, 9053: Information, 9054: Information, 9055: Hinge, 9101: Personal digital assistant, 9102: Personal digital assistant, 9103: Tablet terminal, 9200: Personal digital assistant, 9201: Personal digital assistant,
Claims
A step of forming a semiconductor film on a first insulating layer, A step of performing a first heat treatment to improve the crystallinity of the semiconductor film, The process of forming a semiconductor layer by processing the aforementioned semiconductor film into an island shape, A step of forming a gate insulating layer in contact with the semiconductor film, A step of forming a gate electrode in contact with the gate insulating layer, The process includes a second step of performing a heat treatment, The first heat treatment is performed at a higher temperature than the second heat treatment. In the second heat treatment described above, oxygen is supplied into the semiconductor layer, and hydrogen in the semiconductor layer is released to one or both of the first insulating layer and the gate insulating layer. Method for manufacturing semiconductor devices. In claim 1, the semiconductor film is a film containing indium and oxygen. Method for manufacturing semiconductor devices. In claim 1, The first insulating layer and the gate insulating layer, or both, use a film containing hafnium and oxygen. Method for manufacturing semiconductor devices. In claim 1, Prior to the first heat treatment, the semiconductor film exhibits tensile stress at a temperature of 25°C. After the first heat treatment, the semiconductor film exhibits compressive stress at a temperature of 25°C. Method for manufacturing semiconductor devices. In claim 1, The semiconductor film has a stress value at 25°C after the first heat treatment that is smaller than the stress value at 25°C before the first heat treatment. Method for manufacturing semiconductor devices. In claim 1, The semiconductor film has a first film, a second film, and a third film from the first insulating layer side, The second film uses a film containing indium and oxygen, The first and third films each use films with a wider band gap than the second film. Method for manufacturing semiconductor devices. In claim 6, The first and third films each use films containing a first element and oxygen, The first element is one or more selected from indium, gallium, and zinc. Method for manufacturing semiconductor devices. In claim 6, The semiconductor film has a fourth film between the first film and the second film. The fourth film uses a film with a wider band gap than the second film. Method for manufacturing semiconductor devices. In claim 8, The first film is a film containing indium, gallium, zinc, and oxygen. The fourth membrane uses a membrane containing gallium and oxygen. Method for manufacturing semiconductor devices. It has a first insulating layer, a semiconductor layer, a gate insulating layer, and a gate electrode. The semiconductor layer is located on the first insulating layer, The gate insulating layer is in contact with the upper surface of the semiconductor layer, The gate electrode is in contact with the upper surface of the first insulating layer, The semiconductor layer has a first film, a second film, and a third film from the side of the first insulating layer. The second film contains indium and oxygen, and is single-crystal or polycrystalline. The first and third films each have a wider band gap than the second film. Semiconductor equipment. In claim 10, The first film and the third film each contain a first element and oxygen, The first element is one or more selected from indium, gallium, and zinc. Semiconductor equipment. In claim 10, The semiconductor layer has a fourth film between the first film and the second film. The first film comprises indium, gallium, zinc, and oxygen. The fourth film contains gallium and oxygen, Method for manufacturing semiconductor devices.