Semiconductor device and method for manufacturing semiconductor device
The fin-shaped semiconductor layer design with indium oxide and precise layer configurations addresses the challenges of semiconductor devices, enhancing performance in speed, integration, and reliability with reduced power consumption.
Patent Information
- Application Number
- PCT/IB2026/054264
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Existing semiconductor devices face challenges in achieving high operating speed, miniaturization, high integration, large on-current, small footprint, high field-effect mobility, low power consumption, and reliable electrical characteristics with minimal variation in transistor electrical characteristics.
A semiconductor device design featuring a fin-shaped semiconductor layer with a tapered shape and specific conductive and insulating layers configuration, utilizing indium oxide with crystalline structure, and a manufacturing method that includes multiple processing steps to form island-shaped semiconductor layers and conductive layers with precise alignments.
The design enables high-speed operation, miniaturization, high integration, large on-current, and reduced footprint with improved field-effect mobility and reliability, while maintaining low power consumption and consistent electrical characteristics.
Smart Images

Figure IB2026054264_12112026_PF_FP_ABST
Abstract
Description
Semiconductor device and method for manufacturing a semiconductor device.
[0001] One aspect of the present invention relates to a semiconductor device and an electronic device. Another aspect of the present invention relates to a method for manufacturing the above-mentioned semiconductor device.
[0002] It should be noted that one aspect of the present invention is not limited to the above-mentioned technical field. Examples of technical fields of one aspect of the present invention include semiconductor devices, display devices, light-emitting devices, energy storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), methods for driving them, or methods for manufacturing them.
[0003] In this specification, the term "semiconductor device" refers to any device that can function by utilizing semiconductor properties. Semiconductor elements such as transistors, as well as semiconductor circuits, computing devices, and memory devices, are all forms of semiconductor devices. Display devices (liquid crystal displays, light-emitting displays, etc.), projection devices, lighting devices, electro-optical devices, energy storage devices, memory devices, semiconductor circuits, imaging devices, and electronic devices may also be considered to have semiconductor devices.
[0004] In recent years, the development of semiconductor devices has progressed, and LSIs (Large Scale Integration), CPUs (Central Processing Units), and memory are mainly used in semiconductor devices. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors and memory) formed into chips by processing semiconductor wafers, and electrodes which are connection terminals are formed on them.
[0005] Semiconductor circuits (IC chips) such as LSIs, CPUs, and memory are mounted on circuit boards, such as printed circuit boards, and used as components in various electronic devices.
[0006] Furthermore, the technology of constructing transistors using semiconductor thin films formed on substrates with insulating surfaces is attracting attention. These transistors are widely applied in electronic devices such as integrated circuits (ICs) and image display devices (also simply referred to as display devices). While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors are attracting attention as other materials.
[0007] Furthermore, transistors using oxide semiconductors are known to have extremely low leakage current in the non-conductive state. For example, Patent Document 1 discloses a low-power CPU that takes advantage of the low leakage current characteristic of transistors using oxide semiconductors. Also, for example, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by taking advantage of the low leakage current characteristic of transistors using oxide semiconductors.
[0008] Furthermore, Patent Document 3 discloses a transistor with a microstructure in which a source electrode and a drain electrode are provided in contact with the upper surface of an oxide semiconductor.
[0009] Also, In 2 O 3 Its use in thin-film transistors has been reported (Non-Patent Document 1).
[0010] Japanese Patent Publication No. 2012-257187, Japanese Patent Publication No. 2011-151383, International Publication No. 2016-125052
[0011] Dhananjay and C. W. Chu, “Realization of In2O3 thin film transistors through reactive evaporation process,” Appl. Phys. Lett. 91, 132111 (2007). Takashi Koida, “High-mobility transparent conductive film,” National Institute of Advanced Industrial Science and Technology, AIST Photovoltaic Power Generation Research Results Presentation Meeting 2019, Internet <URL: https: / / unit.aist.go.jp / rpd-envene / PV / ja / results / 2019 / oral / T13.pdf>
[0012] One aspect of the present invention aims to provide a semiconductor device with a high operating speed. Alternatively, one aspect of the present invention aims to provide a semiconductor device that can be miniaturized or highly integrated. Alternatively, one aspect of the present invention aims to provide a semiconductor device having a transistor with a large on-current. Alternatively, one aspect of the present invention aims to provide a semiconductor device having a transistor with a small footprint per unit. Alternatively, one aspect of the present invention aims to provide a semiconductor device having a transistor with high field-effect mobility. Alternatively, one aspect of the present invention aims to provide a semiconductor device with high reliability. Alternatively, one aspect of the present invention aims to provide a semiconductor device with good electrical characteristics. Alternatively, one aspect of the present invention aims to provide a semiconductor device with little variation in the electrical characteristics of the transistors. Alternatively, one aspect of the present invention aims to provide a semiconductor device with low power consumption. Alternatively, one aspect of the present invention aims to provide a novel semiconductor device. Alternatively, one aspect of the present invention aims to provide a method for manufacturing the above-mentioned semiconductor device. Alternatively, one aspect of the present invention aims to provide a method for manufacturing a semiconductor device with high productivity.
[0013] Furthermore, the description of these problems does not preclude the existence of other problems. One aspect of the present invention does not necessarily have to solve all of these problems. It is possible to extract other problems from the description in the specification, drawings, and claims.
[0014] One aspect of the present invention is a semiconductor device comprising a semiconductor layer, a first insulating layer, a second insulating layer, a first conductive layer, a second conductive layer, and a third conductive layer, wherein the first conductive layer and the second conductive layer each have a region in contact with the side surface of the semiconductor layer, the first insulating layer is provided on the first conductive layer and the second conductive layer, the first insulating layer has a first opening that at least a portion overlaps with the region between the first conductive layer and the second conductive layer, the second insulating layer covers the side surface of the semiconductor layer inside the first opening, the third conductive layer has a region inside the first opening that faces the side surface of the semiconductor layer with the second insulating layer in between, the semiconductor layer has a tapered shape with a taper angle of less than 90°, and in a cross-sectional view in the channel width direction, the height of the semiconductor layer is greater than the width of the bottom surface of the semiconductor layer.
[0015] Alternatively, in the above embodiment, the semiconductor device may have a fourth conductive layer and a fifth conductive layer, the first insulating layer having a second opening having a region overlapping with the first conductive layer and a third opening having a region overlapping with the second conductive layer, the fourth conductive layer having a region inside the second opening that contacts a surface of the first conductive layer along the side surface of the semiconductor layer, and the fifth conductive layer having a region inside the third opening that contacts a surface of the second conductive layer along the side surface of the semiconductor layer.
[0016] Alternatively, in the above embodiment, the semiconductor device has a fourth conductive layer and a fifth conductive layer, where the fourth conductive layer and the fifth conductive layer each have a region in contact with the upper surface of the semiconductor layer, the first conductive layer has a region in contact with the upper surface of the fourth conductive layer, the second conductive layer has a region in contact with the upper surface of the fifth conductive layer, and the sum of the area of the lower surface of the fourth conductive layer and the area of the lower surface of the fifth conductive layer may be smaller than the area of the lower surface of the semiconductor layer.
[0017] Alternatively, in the above embodiment, the side edge of the fourth conductive layer on the first opening side may coincide with or substantially coincide with the side edge of the first conductive layer on the first opening side in a plan view, and the side edge of the fifth conductive layer on the first opening side may coincide with or substantially coincide with the side edge of the second conductive layer on the first opening side in a plan view.
[0018] Alternatively, in the above embodiment, the semiconductor layer may have indium and oxygen, and the semiconductor layer may have a cubic crystal structure.
[0019] Alternatively, in the above embodiment, the semiconductor layer may have a metal oxide layer, the metal oxide layer may have crystals, and the semiconductor layer may have a region in contact with the upper surface of the metal oxide layer.
[0020] Alternatively, in the above embodiment, the semiconductor layer has a first region, a second region, and a third region, the first region being a region in contact with the upper surface of the metal oxide layer, the second region being a region located closer to the third conductive layer than the first region, and the third region including a region overlapping with the third conductive layer, and the length in the channel width direction of the third region of the semiconductor layer may be shorter than the length in the channel width direction of the second region of the semiconductor layer.
[0021] Alternatively, in the above embodiment, the third region may have a cross-section in which no grain boundaries are observed in the channel length direction by analysis using a transmission electron microscope.
[0022] Alternatively, in the above embodiment, the semiconductor layer may have crystal grains that overlap with a pair of side edges of the third conductive layer that face each other in the channel length direction.
[0023] Alternatively, one aspect of the present invention comprises first to eleven steps: in the first step, a metal oxide layer having crystals is formed; in the second step, a first semiconductor film having indium and oxygen is formed so as to cover the metal oxide layer; in the third step, the first semiconductor film is processed to form island-shaped first semiconductor layers; in the fourth step, the first semiconductor layer is subjected to a crystallization process; and in the fifth step, a first semiconductor film having indium and oxygen and having a thickness greater than the first semiconductor film is formed. In the sixth step, a semiconductor film is formed to cover the first semiconductor layer; in the seventh step, the second semiconductor film is crystallized; in the eighth step, a first conductive layer is formed to cover the first and second semiconductor layers; in the ninth step, a first insulating layer is formed on the first conductive layer; and in the tenth step, the first insulating layer and the first conductive layer are processed to form the first semiconductor layer and In the first step, a first opening having a region overlapping with the second semiconductor layer is formed in the first insulating layer, and a second conductive layer and a third conductive layer are formed, exposing a part of the side surface of the first semiconductor layer. In the eleventh step, a second insulating layer covering the exposed side surface of the first semiconductor layer and a fourth conductive layer on the second insulating layer are formed inside the first opening. In the third step, the first semiconductor layer is formed to have a first region, a second region, and a third region, and the first region The first region is a region in contact with the upper surface of the metal oxide layer, the second region is a region located closer to the fourth conductive layer than the first region, the third region includes a region overlapping with the fourth conductive layer, the length in the channel width direction of the third region of the first semiconductor layer is shorter than the length in the channel width direction of the second region of the first semiconductor layer, and in a cross-sectional view in the channel width direction, the height of the second semiconductor layer is greater than the width of the lower surface of the first semiconductor layer, in this method for manufacturing a semiconductor device.
[0024] Alternatively, in the above embodiment, in the seventh step, the first film may be formed on the second semiconductor film, the first film may be processed to form a first layer, and then the second semiconductor film may be processed using the first layer as a mask.
[0025] Alternatively, in the above embodiment, the first film may be formed using a conductive material, and in the 10th step, by removing the region overlapping with the first opening of the first layer, a second layer having a region in contact with the upper surface of the second semiconductor layer and a region in contact with the second conductive layer, and a third layer having a region in contact with the upper surface of the second semiconductor layer and a region in contact with the third conductive layer may be formed.
[0026] Alternatively, in the above embodiment, the method may include a twelfth step and a thirteenth step, wherein in the twelfth step, a second opening having a region overlapping with the second conductive layer and a third opening having a region overlapping with the third conductive layer are formed to expose at least a portion of the surface of the second conductive layer that is aligned with the side surface of the second semiconductor layer and at least a portion of the surface of the third conductive layer that is aligned with the side surface of the second semiconductor layer, and in the thirteenth step, a fifth conductive layer is formed inside the second opening and a sixth conductive layer is formed inside the third opening.
[0027] Alternatively, in the above embodiment, in the seventh step, the second semiconductor film may be processed so that the second semiconductor layer has a tapered shape with a taper angle of less than 90°.
[0028] According to one aspect of the present invention, a semiconductor device with a high operating speed can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device having a transistor with a large on-current can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device having a transistor with a small footprint per unit can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device having a transistor with high field-effect mobility can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device with high reliability can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device having good electrical characteristics can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device with less variation in the electrical characteristics of transistors can be provided. Alternatively, according to one aspect of the present invention, a semiconductor device with low power consumption can be provided. Alternatively, according to one aspect of the present invention, a novel semiconductor device can be provided. Alternatively, according to one aspect of the present invention, a method for manufacturing the above-mentioned semiconductor device can be provided. Alternatively, according to one aspect of the present invention, a method for manufacturing a highly productive semiconductor device can be provided.
[0029] Furthermore, the description of these effects does not preclude the existence of other effects. One aspect of the present invention does not necessarily have to possess all of these effects. Other effects can be extracted from the description, drawings, and claims.
[0030] Figures 1A and 1B are perspective views showing examples of semiconductor device configurations. Figures 2A and 2B are perspective views showing examples of semiconductor device configurations. Figure 3A is a plan view showing an example of semiconductor device configuration. Figure 3B is a cross-sectional view showing an example of semiconductor device configuration. Figures 4A and 4B are cross-sectional views showing examples of semiconductor device configurations. Figure 5A is a plan view showing an example of semiconductor device configuration. Figure 5B is a cross-sectional view showing an example of semiconductor device configuration. Figures 6A and 6B are cross-sectional views showing examples of semiconductor device configurations. Figure 7A is a plan view showing an example of semiconductor device configuration. Figure 7B is a cross-sectional view showing an example of semiconductor device configuration. Figures 8A and 8B are cross-sectional views showing examples of semiconductor device configurations. Figures 9A and 9B are plan views showing examples of semiconductor device configurations. Figures 10A and 10B are cross-sectional views showing examples of semiconductor device configurations. Figure 11A is a plan view showing an example of semiconductor device configuration. Figure 11B is a cross-sectional view showing an example of semiconductor device configuration. Figure 12 is a cross-sectional view showing an example of semiconductor device configuration. Figure 13A is a plan view showing an example of a semiconductor device manufacturing method. Figures 13B, 13C, and 13D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 14A is a plan view showing an example of a semiconductor device manufacturing method. Figures 14B, 14C, and 14D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 15A is a plan view showing an example of a semiconductor device manufacturing method. Figures 15B, 15C, and 15D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 16A is a plan view showing an example of a semiconductor device manufacturing method. Figures 16B, 16C, and 16D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 17A is a plan view showing an example of a semiconductor device manufacturing method. Figures 17B, 17C, and 17D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 18A is a plan view showing an example of a semiconductor device manufacturing method. Figures 18B, 18C, and 18D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 19A is a plan view showing an example of a semiconductor device manufacturing method. Figures 19B, 19C, and 19D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 20A is a plan view showing an example of a semiconductor device manufacturing method. Figures 20B, 20C, and 20D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 21A is a plan view showing an example of a semiconductor device manufacturing method.Figures 21B, 21C, and 21D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 22A is a plan view showing an example of a semiconductor device manufacturing method. Figures 22B, 22C, and 22D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 23A is a plan view showing an example of a semiconductor device manufacturing method. Figures 23B, 23C, and 23D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 24A is a plan view showing an example of a semiconductor device manufacturing method. Figures 24B, 24C, and 24D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 25A is a plan view showing an example of a semiconductor device manufacturing method. Figures 25B, 25C, and 25D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 26A is a plan view showing an example of a semiconductor device manufacturing method. Figures 26B, 26C, and 26D are cross-sectional views showing examples of semiconductor device manufacturing methods. Figure 27A is a plan view showing an example of a semiconductor device manufacturing method. Figures 27B, 27C, and 27D are cross-sectional views showing examples of semiconductor device fabrication methods. Figure 28A is a plan view showing an example of a semiconductor device fabrication method. Figures 28B, 28C, and 28D are cross-sectional views showing examples of semiconductor device fabrication methods. Figure 29A is a plan view showing an example of a semiconductor device fabrication method. Figures 29B, 29C, and 29D are cross-sectional views showing examples of semiconductor device fabrication methods. Figure 30A is a plan view showing an example of a semiconductor device fabrication method. Figures 30B, 30C, and 30D are cross-sectional views showing examples of semiconductor device fabrication methods. Figure 31A is a plan view showing an example of a semiconductor device fabrication method. Figures 31B, 31C, and 31D are cross-sectional views showing examples of semiconductor device fabrication methods. Figures 32A and 32B illustrate the carrier concentration dependence of Hall mobility. Figure 32C is a cross-sectional view illustrating an indium oxide film. Figure 33A is a plan view showing an example of a memory device configuration. Figure 33B is a cross-sectional view showing an example of a memory device configuration. Figure 34 is a cross-sectional view showing an example of a memory device configuration. Figure 35 is a block diagram showing an example of a semiconductor device configuration. Figures 36A, 36B, 36C, 36D, 36E, 36F, 36G, and 36H are circuit diagrams showing an example of a memory cell configuration. Figures 37A, 37B, and 37C are perspective views of a semiconductor device. Figures 38A and 38B are examples of semiconductor device configurations. Figure 39 is an example of a semiconductor device configuration.Figures 40A and 40B show examples of electronic components. Figures 41A, 41B, and 41C show examples of large-scale computers. Figure 41D shows an example of space equipment. Figure 41E shows an example of a storage system applicable to data centers.
[0031] Embodiments will be described in detail with reference to the drawings. However, it will be readily apparent to those skilled in the art that the present invention is not limited to the following description, and that its form and details can be modified in various ways without departing from the spirit and scope of the present invention. Accordingly, the present invention shall not be construed as being limited to the descriptions of the embodiments shown below.
[0032] In the invention described below, the same reference numerals are used in common across different drawings for identical parts or parts having similar functions, and repeated explanations are omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used, and reference numerals may not be assigned.
[0033] Furthermore, the position, size, and scope of each component shown in the drawings may not represent the actual position, size, and scope for the sake of ease of understanding. Therefore, the disclosed invention is not necessarily limited to the position, size, and scope disclosed in the drawings.
[0034] Furthermore, in particular, in plan views (also called "top views") or perspective views, the description of some components may be omitted to facilitate understanding of the invention. In addition, the description of some hidden lines may be omitted.
[0035] In this specification, ordinal numbers such as "first," "second," etc., are added to avoid confusion of components and do not limit the number of components or the order of components (e.g., process order or stacking order). Furthermore, even if a term does not have an ordinal number in this specification, an ordinal number may be added in the claims to avoid confusion of components. Even if a term has an ordinal number in this specification, a different ordinal number may be added in the claims. Even if a term has an ordinal number in this specification, an ordinal number may be omitted in the claims.
[0036] It should be noted that the terms "film" and "layer" can be interchanged depending on the context or situation. For example, the term "conductive layer" can be changed to "conductive film." Or, for example, the term "insulating film" can be changed to "insulating layer."
[0037] Furthermore, in this specification, "parallel" means a state in which two lines are arranged at an angle of -10° or more and 10° or less. Therefore, the case of -5° or more and 5° or less is also included. Furthermore, "approximately parallel" means a state in which two lines are arranged at an angle of -20° or more and 20° or less. Furthermore, "perpendicular" means a state in which two lines are arranged at an angle of 80° or more and 100° or less. Therefore, the case of 85° or more and 95° or less is also included. Furthermore, "approximately perpendicular" means a state in which two lines are arranged at an angle of 70° or more and 110° or less.
[0038] In this specification, "connection" includes, for example, "electrical connection." The term "electrical connection" is sometimes used to define the connection relationship of circuit elements as a physical object. Furthermore, "electrical connection" includes both "direct connection" and "indirect connection." "A and B are directly connected" means that A and B are connected without the use of circuit elements (e.g., transistors, switches, etc.; wiring is not considered a circuit element). On the other hand, "A and B are indirectly connected" means that A and B are connected through one or more circuit elements. A, B, and C (described later) refer to objects such as elements, circuits, wiring, electrodes, terminals, semiconductor layers, and conductive layers.
[0039] For example, assuming a circuit including A and B is in operation, if there is a timing during the circuit's operation when electrical signals are exchanged or potential interactions occur between A and B, then it can be defined that "A and B are indirectly connected" as physical objects. Furthermore, even if there is a timing during the circuit's operation when no electrical signals are exchanged or potential interactions occur between A and B, if there is a timing during the circuit's operation when electrical signals are exchanged or potential interactions occur between A and B, then it can be defined that "A and B are indirectly connected."
[0040] An example of a case where "A and B are indirectly connected" is when A and B are connected via the source and drain of one or more transistors. On the other hand, an example of a case where "A and B are not indirectly connected" is when an insulator is interposed in the path from A to B. Specifically, this includes cases where a capacitive element is connected between A and B, or where the gate insulating layer of a transistor is interposed between A and B. Therefore, it cannot be said that "the gate (A) of a transistor and the source or drain (B) of a transistor are indirectly connected."
[0041] Another example of a situation where it cannot be said that "A and B are indirectly connected" is when multiple transistors are connected via source and drain in the path from A to B, and a constant potential V is supplied from a power supply, GND, etc., to the nodes between the transistors.
[0042] An opening can include, for example, grooves, slits, etc. Furthermore, the area in which an opening is formed may also be referred to as an opening.
[0043] In this specification, a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined with respect to the substrate surface or the surface to be formed. For example, it is preferable to have a region in which the angle between the inclined side surface and the substrate surface or the surface to be formed (hereinafter sometimes referred to as the taper angle) is less than 90°. The side surface of the structure and the substrate surface do not necessarily have to be perfectly flat, and may be a generally planar shape with a small curvature, or a generally planar shape with fine irregularities.
[0044] In this specification, "heights match or roughly match" refers to a configuration in which the heights from a reference surface (e.g., a flat surface such as the substrate surface) are equal in a cross-sectional view. For example, in the manufacturing process of semiconductor devices, the surfaces of multiple layers may be exposed by planarization (typically by chemical mechanical polishing (CMP)). In this case, the surfaces to be processed by CMP have a configuration in which the heights from the reference surface are equal. However, the heights of the multiple layers may differ depending on the processing apparatus, processing method, or material of the surface to be processed during CMP. In this specification, this case is also treated as "heights match or roughly match." For example, if there are two layers with heights (here referred to as a first layer and a second layer) with respect to a reference surface, if the difference between the height of the top surface of the first layer and the height of the top surface of the second layer is 20 nm or less, it is also said that the heights match or roughly match.
[0045] In this specification, a layer is considered flat if its average surface roughness (Ra) is less than 3 nm. The average surface roughness (Ra) is defined as that specified in JIS B 0601:2001 (ISO 4287:1997). The average surface roughness (Ra) can be evaluated using an atomic force microscope (AFM). For example, the average surface roughness (Ra) can be calculated over a 2 μm square area. If the layer is island-like and does not have a 2 μm square area in plan view, the calculation may be performed over the entire area of the layer in plan view.
[0046] Furthermore, the flatness of the upper surface of a layer can also be evaluated by performing image analysis of a transmission electron microscope (TEM) image. For example, it is assumed that the shape of the interface between the first layer and the second layer observed in the TEM image is the roughness curve of the first layer. Then, the arithmetic mean roughness can be calculated from the assumed roughness curve. The reference length may be the length of the upper surface of the first layer observed in the TEM image, or the length of the region where the first layer and the second layer overlap. The reference length may be, for example, 100 nm. In this case, it is preferable that the observation range of the TEM image is 100 nm or more in either the vertical or horizontal direction. If the arithmetic mean roughness of the upper surface of the first layer calculated using this method is less than 3 nm, the upper surface of the first layer can also be said to be flat.
[0047] In this specification, "side edges coincide or roughly coincide" or "sides coincide or roughly coincide" means that, in a plan view, at least a portion of the contours of the stacked layers overlap. For example, this includes cases where the upper and lower layers are processed with the same mask pattern, or partially with the same mask pattern. However, strictly speaking, the contours may not overlap, and the contour of the upper layer may be located inside the contour of the lower layer, or the contour of the upper layer may be located outside the contour of the lower layer; in this case, it is also referred to as "side edges coincide or roughly coincide" or "sides coincide or roughly coincide."
[0048] In this specification, "shapes in plan view are identical or roughly identical" means that at least a portion of the contours overlaps between stacked layers. For example, this includes cases where the upper and lower layers are processed with the same mask pattern, or partially with the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer; in this case, it may also be said that the shapes in plan view are identical or roughly identical. Furthermore, when the shapes in plan view are identical or roughly identical, it may also be said that the edges are aligned or roughly aligned, or the side edges are identical or roughly identical.
[0049] In this specification, "island-like" refers to a state in which two or more layers made of the same material and formed in the same process are physically separated. For example, an island-like layer refers to a state in which that layer and an adjacent layer are physically separated.
[0050] In this specification, space groups are expressed using international notation (or Hermann-Mauguin notation) in short notation. Crystal planes and crystal orientations are expressed using Miller indices. In crystallography, space groups, crystal planes, and crystal orientations are expressed by superscripting numbers, but in this specification, due to formatting constraints, a minus sign (-) may be placed before the number instead of a superscript. Individual orientations within a crystal are represented by [ ], collective orientations representing all equivalent orientations are represented by < >, individual crystal planes are represented by ( ), and collective planes with equivalent symmetry are represented by {}.
[0051] In this specification and elsewhere, the cubic crystal structure is sometimes referred to as cubic crystal, cubic structure, etc. The same applies to other crystal systems (hexagonal, trigonal, tetragonal, orthorhombic, monoclinic, and triclinic).
[0052] (Embodiment 1) In this embodiment, a semiconductor device having a transistor and a method for manufacturing the semiconductor device will be described with reference to the drawings.
[0053] One aspect of the present invention relates to a transistor having a fin-shaped semiconductor layer. In a cross-sectional view of the transistor in the channel width direction, the aspect ratio (height divided by width) of the semiconductor layer is large, specifically greater than 1. The source electrode, drain electrode, and gate insulating layer of the transistor are provided so as to cover the sides of the semiconductor layer. Specifically, the source electrode, drain electrode, and gate insulating layer are provided so as to have a region in contact with the top surface of the semiconductor layer as well as a region in contact with the side surface. A gate electrode is provided on the gate insulating layer.
[0054] As described above, in a cross-sectional view of the transistor in the channel width direction, the gate electrode faces the top and side surfaces of the semiconductor layer with the gate insulating layer in between. Therefore, because the semiconductor layer has a fin-like shape, compared to the case where the semiconductor layer has a flat plate shape, the area occupied by the semiconductor layer can be reduced while increasing the area in which the semiconductor layer and the gate electrode face each other with the gate insulating layer in between. Thus, the channel width of the transistor can be increased while reducing the area occupied by the transistor.
[0055] In this specification, a semiconductor layer having a fin-like shape refers to a semiconductor layer having an aspect ratio greater than 1 in a cross-sectional view in the channel width direction of a transistor having the semiconductor layer. A semiconductor layer having a flat plate-like shape refers to a semiconductor layer having an aspect ratio of 1 or less in a cross-sectional view in the channel width direction of a transistor having the semiconductor layer. A transistor equipped with a fin-like semiconductor layer is called a fin-type transistor. Furthermore, a transistor equipped with a flat plate-like semiconductor layer is called a flat plate-type transistor.
[0056] In this specification, the aspect ratio of the semiconductor layer of a transistor in a cross-sectional view in the channel width direction is sometimes simply referred to as the aspect ratio of the semiconductor layer.
[0057] Furthermore, because the semiconductor layer has a fin-like shape, compared to the case where the semiconductor layer has a flat plate shape, the area occupied by the semiconductor layer can be reduced while increasing the contact area between the semiconductor layer and the source electrode, and the contact area between the semiconductor layer and the drain electrode. Therefore, the area occupied by the transistor can be reduced while reducing the contact resistance between the semiconductor layer and the source electrode, and the contact resistance between the semiconductor layer and the drain electrode.
[0058] As a result, a semiconductor device can be provided that has transistors with a small footprint per unit and a large on-current. Therefore, a semiconductor device that is miniaturized or highly integrated and operates at a high speed can be provided. In particular, the larger the aspect ratio of the semiconductor layer in a cross-sectional view in the channel width direction of the transistor, the larger the channel width of the transistor can be made without increasing the footprint of the transistor. In addition, the contact resistance between the semiconductor layer and the source electrode, and the contact resistance between the semiconductor layer and the drain electrode can be made smaller. Therefore, it is preferable that the aspect ratio of the semiconductor layer in a cross-sectional view in the channel width direction of the transistor is as large as possible, while keeping the semiconductor layer from collapsing during the transistor manufacturing process.
[0059] It is preferable to use indium oxide (also known as IO) for the semiconductor layer. In this case, the semiconductor layer contains indium and oxygen. It is preferable that the semiconductor layer is crystalline, for example, it is preferable that it has crystal grains. The crystalline nature of the semiconductor layer reduces carrier scattering in the semiconductor layer, enabling the realization of a transistor with high field-effect mobility. Furthermore, it enables the realization of a transistor with high reliability.
[0060] Here, the effective mass of electrons in indium oxide has the characteristic that it is almost independent of the crystal orientation. Therefore, in a semiconductor device according to one aspect of the present invention, if indium oxide is used as the semiconductor layer, even if the crystal orientation of the side surface of the semiconductor layer differs from that of the top surface of the semiconductor layer, the effective mass of electrons remains almost unchanged between the side surface and the top surface of the semiconductor layer. Therefore, even if the transistor is of the fin type, the decrease in field-effect mobility caused by the difference in the effective mass of electron carriers between the side surface and the top surface of the semiconductor layer can be suppressed. For this reason, it is particularly preferable to use indium oxide, specifically crystalline indium oxide, for the semiconductor layer of a semiconductor device according to one aspect of the present invention. Note that indium oxide may contain elements other than indium and oxygen. Examples of such elements include silicon, gallium, and zinc. In this case, the concentration of the element should be lower than the concentration of indium. For example, if gallium is contained in indium oxide, it is preferable that the concentration of gallium be, for example, 5 atomic% or less.
[0061] In this specification, the concentration of element A in a semiconductor layer using indium oxide containing element A represents the ratio of the number of atoms of element A to the total number of atoms of all elements other than oxygen that constitute the semiconductor layer.
[0062] <Example of semiconductor device configuration 1> Figures 1A to 4B show examples of semiconductor device configurations having a transistor 200 on a substrate (not shown).
[0063] Figures 1A, 1B, 2A, and 2B are perspective views showing examples of the configuration of the semiconductor device described above. In Figure 1B, some of the elements shown in Figure 1A are shown transparently. In Figure 2A, the elements shown transparently in Figure 1B are omitted, and some of the elements shown in Figure 1B are shown transparently. In Figure 2B, the elements shown transparently in Figure 2A are omitted, and some of the elements shown in Figure 2A are shown transparently.
[0064] Figure 3A is a plan view showing an example of the configuration of the semiconductor device described above. Figure 3B is a cross-sectional view between the dashed lines A1 and A2 shown in Figure 3A, and is also a cross-sectional view of the transistor 200 in the channel length direction. Figure 4A is a cross-sectional view between the dashed lines B1 and B2 shown in Figure 3A, and is also a cross-sectional view of the transistor 200 in the channel width direction. Figure 4B is a cross-sectional view between the dashed lines B3 and B4 shown in Figure 3A, and is also a cross-sectional view of the transistor 200 in the channel width direction. Here, the dashed lines A1 and A2 are perpendicular to the dashed lines B1 and B2, and the dashed lines B3 and B4, respectively. Also, the dashed lines B1 and B2 and the dashed lines B3 and B4 are parallel to each other. Note that in the plan view of Figure 3A, some elements have been omitted for clarity. In the subsequent plan views, some elements have also been omitted for clarity.
[0065] In this specification, the term "cross-section in the channel width direction" does not necessarily include the channel formation region of the transistor. In some cases, the term "cross-section in the channel width direction" may include a cross-section parallel to the cross-section in the channel width direction that includes the channel formation region. For example, the cross-sectional view of the area indicated by the dashed line B3-B4 in Figure 4B is referred to as a cross-sectional view in the channel width direction.
[0066] A semiconductor device according to one aspect of the present invention includes an insulating layer 215 on a substrate (not shown), an insulating layer 216 on the insulating layer 215, an insulating layer 221 on the insulating layer 216, an insulating layer 222 on the insulating layer 221, an insulating layer 224 on the insulating layer 222, a semiconductor layer 230 on the insulating layer 224, conductive layers 242a and 242b on the semiconductor layer 230 and on the insulating layer 222, an insulating layer 250 on the semiconductor layer 230 and on the insulating layer 222, and a conductive layer 260 on the insulating layer 250.
[0067] As shown in Figures 2B, 3A, 3B, and 4B, the conductive layer 242a covers a portion of the upper surface and a portion of the side surface of the semiconductor layer 230. Similarly, the conductive layer 242b also covers a portion of the upper surface and a portion of the side surface of the semiconductor layer 230. In Figure 3B, the first side surface of the semiconductor layer 230 is shown as side surface 211a, and the second side surface is shown as side surface 211b. The conductive layer 242a can cover the entire side surface 211a. The conductive layer 242b can cover the entire side surface 211b. Side surfaces 211a and side surfaces 211b are opposite surfaces. Note that in Figure 2B, the insulating layer 215, insulating layer 216, insulating layer 221, insulating layer 222, insulating layer 224, and semiconductor layer 230 are shown, and the conductive layers 242a and 242b are shown transparently.
[0068] The conductive layer 242a may have a region in contact with the upper surface of the semiconductor layer 230, a region in contact with the side surface of the semiconductor layer 230, a region in contact with the side surface of the insulating layer 224, and a region in contact with the upper surface of the insulating layer 222. Similarly, the conductive layer 242b may also have a region in contact with the upper surface of the semiconductor layer 230, a region in contact with the side surface of the semiconductor layer 230, a region in contact with the side surface of the insulating layer 224, and a region in contact with the upper surface of the insulating layer 222. The region of the semiconductor layer 230 in contact with the conductive layer 242a functions as one of the source region and drain region of the transistor 200. The region of the semiconductor layer 230 in contact with the conductive layer 242b functions as the other of the source region and drain region of the transistor 200.
[0069] An insulating layer 275 is provided on the conductive layer 242a and the conductive layer 242b, and an insulating layer 280 is provided on the insulating layer 275. The insulating layer 275 and the insulating layer 280 have an opening 201. At least a portion of the opening 201 overlaps with the region between the conductive layer 242a and the conductive layer 242b. The sides of the insulating layer 275 and the sides of the insulating layer 280 each function as side walls of the opening 201.
[0070] Figure 3B shows an example where the upper surface of the semiconductor layer 230 in the region overlapping with the opening 201 is lower than the upper surface of the semiconductor layer 230 in the region overlapping with the conductive layer 242a and the upper surface of the semiconductor layer 230 in the region overlapping with the conductive layer 242b. In other words, it shows an example where a recess is provided in the region of the semiconductor layer 230 that overlaps with the opening 201. A recess may be formed in the semiconductor layer 230 due to the formation process of the conductive layers 242a and 242b.
[0071] The insulating layer 250 and the conductive layer 260 are provided inside the opening 201. The opening 201 reaches the semiconductor layer 230 and the insulating layer 222. As shown in Figure 4A, the insulating layer 250 covers the top and side surfaces of the semiconductor layer 230 inside the opening 201. The insulating layer 250 may have a region in contact with the top surface of the semiconductor layer 230, a region in contact with the side surface of the semiconductor layer 230, a region in contact with the side surface of the conductive layer 242a on the opening 201 side, a region in contact with the side surface of the conductive layer 242b on the opening 201 side, a region of the insulating layer 275 on the opening 201, a region of the insulating layer 280 on the side surface of the opening 201, a region in contact with the side surface of the insulating layer 224, and a region in contact with the top surface of the insulating layer 222.
[0072] The conductive layer 260 has a region that overlaps with the semiconductor layer 230 via the insulating layer 250. As shown in Figure 4A, the conductive layer 260 has a region within the opening 201 that faces the side surface of the semiconductor layer 230 with the insulating layer 250 in between. The region of the semiconductor layer 230 that faces the conductive layer 260 with the insulating layer 250 in between functions as the channel formation region of the transistor 200. Furthermore, the height of the upper surface of the conductive layer 260 can be made to match or approximately match the height of the uppermost part of the insulating layer 250 and the height of the upper surface of the insulating layer 280.
[0073] An insulating layer 282 is provided on the insulating layer 280, on the insulating layer 250, and on the conductive layer 260, an insulating layer 283 is provided on the insulating layer 282, and an insulating layer 285 is provided on the insulating layer 283. The insulating layers 275, 280, 282, 283, and 285 have openings 203a and 203b. Opening 203a has a region that overlaps with the conductive layer 242a. Opening 203b has a region that overlaps with the conductive layer 242b. An insulating layer 241a and a conductive layer 240a are provided inside opening 203a. An insulating layer 241b and a conductive layer 240b are provided inside opening 203b. In the following, matters common to openings 203a and 203b may be described as opening 203. Furthermore, matters common to insulating layer 241a and insulating layer 241b may be described as insulating layer 241. In addition, matters common to conductive layer 240a and conductive layer 240b may be described as conductive layer 240.
[0074] In Figure 1B, the conductive layers 240a and 240b shown in Figure 1A are shown through. In Figure 2A, the conductive layers 240a and 240b shown in Figure 1B are omitted, and the insulating layer 250 and conductive layer 260 are shown through. In Figure 2B, the insulating layer 250 and conductive layer 260 shown in Figure 2A are omitted, and the conductive layers 242a and 242b are shown through.
[0075] The insulating layer 241a is provided along the side wall of the opening 203a. The insulating layer 241b is provided along the side wall of the opening 203b. The insulating layer 241a may have a region of insulating layer 275 in contact with the side surface of the opening 203a, a region of insulating layer 280 in contact with the side surface of the opening 203a, a region of insulating layer 282 in contact with the side surface of the opening 203a, a region of insulating layer 283 in contact with the side surface of the opening 203a, and a region of insulating layer 285 in contact with the side surface of the opening 203a. The insulating layer 241b may have a region in contact with the side surface of the opening 203b of the insulating layer 275, a region in contact with the side surface of the opening 203b of the insulating layer 280, a region in contact with the side surface of the opening 203b of the insulating layer 282, a region in contact with the side surface of the opening 203b of the insulating layer 283, and a region in contact with the side surface of the opening 203b of the insulating layer 285.
[0076] In this specification, the side wall of an opening refers to the side surface within the opening of the layer in which the opening is formed.
[0077] The conductive layer 240a has a region in contact with the upper surface of the conductive layer 242a, a region of the conductive layer 242a in contact with the surface along the side of the semiconductor layer 230, and a region in contact with the insulating layer 241a, all within the opening 203a. The conductive layer 240b has a region in contact with the upper surface of the conductive layer 242b, a region of the conductive layer 242b in contact with the surface along the side of the semiconductor layer 230, and a region in contact with the insulating layer 241b, all within the opening 203b. For example, the conductive layer 240a can be in contact with the entire surface of the conductive layer 242a along the side 211a of the semiconductor layer 230. Also, the conductive layer 240b can be in contact with the entire surface of the conductive layer 242b along the side 211b of the semiconductor layer 230.
[0078] Although not shown in Figures 1A to 4B, conductive layers that function as wiring can be provided on conductive layer 240a and conductive layer 240b. In this case, conductive layer 240a functions as a plug for connecting conductive layer 242a and the wiring on conductive layer 240a. Similarly, conductive layer 240b functions as a plug for connecting conductive layer 242b and the wiring on conductive layer 240b.
[0079] The conductive layer 260 has a region that functions as the gate electrode of the transistor 200. The insulating layer 250 has a region that functions as the gate insulating layer of the transistor 200. Figures 1A to 2A, 3A, and 4A show an example in which the conductive layer 260 extends in the channel width direction of the transistor 200. With this configuration, when multiple transistors 200 are provided in the semiconductor device, the conductive layer 260 functions as wiring, specifically gate wiring.
[0080] Conductive layer 242a has a region that functions as one of the source and drain electrodes of transistor 200. Conductive layer 240a functions as a plug connected to conductive layer 242a. Conductive layer 242b has a region that functions as the other of the source and drain electrodes of transistor 200. Conductive layer 240b functions as a plug connected to conductive layer 242b.
[0081] The semiconductor layer 230 may have a metal oxide (also called an oxide semiconductor) that functions as a semiconductor. In the following, a transistor in which the channel is formed in an oxide semiconductor may be referred to as an OS transistor. When the semiconductor layer 230 has an oxide semiconductor, the transistor 200 is an OS transistor. When the semiconductor layer 230 has an oxide semiconductor, the semiconductor layer 230 can be referred to as an oxide semiconductor layer or a metal oxide layer. In this specification, a transistor having silicon in the channel formation region may be referred to as a Si transistor.
[0082] Figures 1A to 2A, 3B, and 4B show an example in which the conductive layer 242a has a laminated structure consisting of conductive layer 242a1 and conductive layer 242a2 on conductive layer 242a1. Also, Figures 2A and 3B show an example in which the conductive layer 242b has a laminated structure consisting of conductive layer 242b1 and conductive layer 242b2 on conductive layer 242b1. It is preferable that the conductive layers 242a1 and 242b1 that are in contact with the semiconductor layer 230 are conductive layers that are not easily oxidized excessively. This suppresses the increase in resistance of conductive layers 242a and 242b due to oxygen contained in the semiconductor layer 230. Thus, the contact resistance between conductive layer 242a1 and the semiconductor layer 230, and the contact resistance between conductive layer 242b1 and the semiconductor layer 230 can be reduced. Furthermore, it is preferable that the conductive layers 242a2 and 242b2 are conductive layers such as metal layers that have higher conductivity than conductive layers 242a1 and 242b1. This makes it possible to increase the conductivity of conductive layers 242a and 242b.
[0083] Figures 1A, 1B, 3B, and 4A show an example in which the conductive layer 260 has a laminated structure consisting of conductive layer 260_1 and conductive layer 260_2 on conductive layer 260_1. In this case, conductive layer 260_1 can be provided so as to enclose the bottom and sides of conductive layer 260_2. In this case, it is preferable to use a conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion for conductive layer 260_1. This makes it possible to suppress an increase in the electrical resistance of the conductive layer 260 due to oxygen contained in the semiconductor layer 230. Furthermore, it is preferable to use a material with higher conductivity for conductive layer 260_2 than the conductive material used for conductive layer 260_1. This makes it possible to improve the conductivity of conductive layer 260.
[0084] Figures 3B and 4B show an example in which the conductive layer 240a has a laminated structure consisting of conductive layer 240a1 and conductive layer 240a2 on conductive layer 240a1. Also, Figure 3B shows an example in which the conductive layer 240b has a laminated structure consisting of conductive layer 240b1 and conductive layer 240b2 on conductive layer 240b1. It is preferable to use conductive materials for conductive layer 240a1 and conductive layer 240b1 that have the function of suppressing the permeation of impurities such as water and hydrogen. Furthermore, it is preferable to use materials for conductive layer 240a2 and conductive layer 240b2 that have higher conductivity than the conductive materials used for conductive layer 240a1 and conductive layer 240b1. This makes it possible to increase the conductivity of conductive layer 240a and conductive layer 240b.
[0085] In Figure 4A, the height of the semiconductor layer 230, specifically the length perpendicular to the surface of the semiconductor layer 230 (for example, the upper surface of the insulating layer 224) in the region overlapping with the opening 201, is shown as height H. Height H corresponds to the thickness of the semiconductor layer 230 in the channel formation region of the transistor 200. The width of the lower surface of the semiconductor layer 230, specifically the length of the lower surface of the semiconductor layer 230 in a cross-sectional view in the channel width direction of the transistor 200, is shown as width W. Note that if the semiconductor layer 230 has a recess that overlaps with the opening 201, the width of the lower surface of the semiconductor layer 230 in the region overlapping with the opening 201 may be smaller than the width of the lower surface of the semiconductor layer 230 in the region not overlapping with the opening 201. In this case, the width of the lower surface of the semiconductor layer 230 in the cross-section including the region overlapping with the opening 201, for example, the channel formation region of the transistor 200, can be defined as width W. As shown in Figure 4A, in a cross-sectional view of the transistor 200 in the channel width direction, specifically in the cross-section including the channel formation region of the transistor 200, the height H is greater than the width W. That is, the aspect ratio of the semiconductor layer 230 (height H divided by width W) is greater than 1. Therefore, the semiconductor layer 230 has a fin-like shape.
[0086] As described above, in a cross-sectional view of the transistor 200 in the channel width direction, the conductive layer 260 faces the upper and side surfaces of the semiconductor layer 230 with the insulating layer 250 in between. Therefore, because the semiconductor layer 230 has a fin-like shape, compared to the case where the semiconductor layer 230 has a flat plate shape, the area occupied by the semiconductor layer 230 can be reduced while increasing the area of the region where the semiconductor layer 230 and the conductive layer 260 face each other with the insulating layer 250 in between. Consequently, the channel width of the transistor 200 can be increased. By increasing the channel width of the transistor 200, the on-current of the transistor 200 can be increased. In addition, the transconductance of the transistor 200 can be increased. Furthermore, the frequency characteristics of the transistor 200 can be improved.
[0087] Furthermore, as described above, the conductive layer 242a and the conductive layer 242b are provided such that they have a region in contact with the upper surface of the semiconductor layer 230 as well as a region in contact with the side surface of the semiconductor layer 230. Furthermore, as described above, the conductive layer 240a has a region in contact with the upper surface of the conductive layer 242a as well as a region of the conductive layer 242a that is in contact with the surface along the side surface of the semiconductor layer 230. Furthermore, as described above, the conductive layer 240b has a region in contact with the upper surface of the conductive layer 242b as well as a region of the conductive layer 242b that is in contact with the surface along the side surface of the semiconductor layer 230. As described above, by having a fin-like shape for the semiconductor layer 230, compared to the case where the semiconductor layer 230 has a flat plate shape, the occupied area of the semiconductor layer 230 can be reduced while increasing the contact area between the semiconductor layer 230 and the conductive layer 242a, the contact area between the semiconductor layer 230 and the conductive layer 242b, the contact area between the conductive layer 240a and the conductive layer 242a, and the contact area between the conductive layer 240b and the conductive layer 242b. Therefore, the contact resistance between the semiconductor layer 230 and the conductive layer 242a, the contact resistance between the semiconductor layer 230 and the conductive layer 242b, the contact resistance between the conductive layer 240a and the conductive layer 242a, and the contact resistance between the conductive layer 240b and the conductive layer 242b can be reduced. Consequently, the on-current of the transistor 200 can be increased. In addition, the transconductance of the transistor 200 can be increased. Furthermore, the frequency characteristics of the transistor 200 can be improved.
[0088] As a result, a semiconductor device that is miniaturized or highly integrated and operates at a high speed can be provided.
[0089] In particular, the larger the aspect ratio of the semiconductor layer 230 in a cross-sectional view in the channel width direction of the transistor 200, the larger the channel width of the transistor 200 can be without increasing the area occupied by the transistor 200. In addition, the contact resistance between the semiconductor layer 230 and the conductive layer 242a, the contact resistance between the semiconductor layer 230 and the conductive layer 242b, the contact resistance between the conductive layer 240a and the conductive layer 242a, and the contact resistance between the conductive layer 240b and the conductive layer 242b can be reduced. Therefore, it is preferable that the aspect ratio of the semiconductor layer 230 in a cross-sectional view in the channel width direction of the transistor 200 is as large as possible, while not causing the semiconductor layer 230 to collapse during the manufacturing process of the transistor 200.
[0090] The height H is preferably greater than 1 times the width W and 500 times or less, more preferably 5 times or more and 200 times or less, and still more preferably 10 times or more and 100 times or less. The height H is preferably 30 nm or more and 2000 nm or less, more preferably 50 nm or more and 1000 nm or less, more preferably 70 nm or more and 500 nm or less, and still more preferably 80 nm or more and 300 nm or less. The width W is preferably 2 nm or more and 50 nm or less, more preferably 3 nm or more and 30 nm or less, and still more preferably 5 nm or more and 20 nm or less. By setting the height H and width W within the above ranges, the channel width of the transistor 200 can be increased while preventing the semiconductor layer 230 from collapsing during the manufacturing process of the transistor 200. Furthermore, the contact resistance between the semiconductor layer 230 and the conductive layer 242a, the contact resistance between the semiconductor layer 230 and the conductive layer 242b, the contact resistance between the conductive layer 240a and the conductive layer 242a, and the contact resistance between the conductive layer 240b and the conductive layer 242b can be reduced.
[0091] The semiconductor layer 230 preferably has a tapered shape with a taper angle of less than 90°. In Figure 4A, the taper angle is shown as the angle θ between the side surface of the semiconductor layer 230 and the upper surface of the insulating layer 224. A small angle θ makes it easier to prevent the semiconductor layer 230 from tipping over during the manufacturing process of the transistor 200. On the other hand, if the angle θ is too small, the occupied area of the semiconductor layer 230 becomes large. Based on the above, it is preferable to set the angle θ. The angle θ can be, for example, 65° or more and less than 90°, preferably 65° or more and 85° or less, and more preferably 70° or more and 80° or less. Here, when the angle θ is less than 90°, the area of the lower surface of the semiconductor layer 230 is larger than the area of the upper surface of the semiconductor layer 230.
[0092] It is preferable to use indium oxide for the semiconductor layer 230. In this case, the semiconductor layer 230 contains indium and oxygen. For example, it is preferable that the semiconductor layer 230 has an indium oxide film. The higher the ratio of the number of indium atoms to the sum of the number of atoms of all metal elements contained in the metal oxide, the higher the field-effect mobility of the transistor can be. Therefore, by using indium oxide for the semiconductor layer 230, the transistor 200 can obtain a large on-current and high frequency characteristics. The indium oxide that can be used for the semiconductor layer 230 will be described in detail in Embodiment 2. Note that indium zinc oxide (also known as In-Zn oxide, IZO®), indium gallium oxide (In-Ga oxide), or indium gallium zinc oxide (also known as In-Ga-Zn oxide, IGZO) may be used as the semiconductor layer 230.
[0093] The semiconductor layer 230 preferably has good crystallinity. This reduces carrier scattering in the semiconductor layer 230, enabling the realization of a transistor with high field-effect mobility. Furthermore, it enables the realization of a highly reliable transistor. Here, if the semiconductor layer 230 contains indium oxide, the semiconductor layer 230 has a cubic crystal structure (bixbite type).
[0094] A transistor using an indium oxide film is a storage-type transistor with electrons as the majority carrier. Assuming that the carrier relaxation time is constant, the smaller the effective mass of electrons (carriers), the higher the electron mobility. In other words, by using indium oxide, which has a small effective mass of electrons, in the semiconductor layer 230, the on-current or field-effect mobility of the transistor 200 can be increased.
[0095] As mentioned above, the effective mass of electrons in indium oxide has the characteristic that it is almost independent of the crystal orientation. Therefore, when indium oxide is used as the semiconductor layer 230, even if the crystal orientation of the side surface of the semiconductor layer 230 differs from the crystal orientation of the top surface of the semiconductor layer 230, the effective mass of electrons remains almost unchanged between the side surface and the top surface of the semiconductor layer 230. Therefore, even if the transistor 200 is fin-shaped, the decrease in field-effect mobility caused by the difference in the effective mass of electron carriers between the side surface and the top surface of the semiconductor layer 230 can be suppressed. For these reasons, it is particularly preferable to use indium oxide, specifically crystalline indium oxide, for the semiconductor layer 230. Note that indium oxide may contain oxygen other than indium and oxygen. Examples of such elements include silicon, gallium, and zinc. In this case, the concentration of the element should be lower than the concentration of indium. For example, if gallium is contained in the indium oxide, the concentration of gallium should preferably be, for example, 5 atomic% or less, as mentioned above.
[0096] The following describes a detailed configuration example of transistor 200.
[0097] In transistors using oxide semiconductors as semiconductor layers, impurities such as hydrogen and oxygen vacancies (V) are present in the region where channels are formed in the oxide semiconductor layer. O If a hydrogen vacancy exists, the electrical properties are prone to fluctuations, and reliability may be reduced. Also, hydrogen near the oxygen vacancy can fill the oxygen vacancy, creating a defect (hereinafter referred to as V). OThis can form a channel (sometimes called H) and generate electrons that act as carriers. Therefore, if oxygen vacancies and hydrogen are present in the channel formation region of the oxide semiconductor layer, the transistor is likely to exhibit normally-on characteristics (a characteristic in which a channel exists and current flows through the transistor even without applying voltage to the gate electrode). Consequently, in the channel formation region of the oxide semiconductor layer, impurities, oxygen vacancies, and V are present. O It is preferable that H is reduced as much as possible. In other words, it is preferable that the channel-forming region in the oxide semiconductor layer has a reduced carrier concentration and is intrinsically i-type or substantially i-type.
[0098] In contrast, by providing an insulating layer containing excess oxygen near the oxide semiconductor layer and performing a heat treatment, oxygen is supplied from the insulating layer to the oxide semiconductor layer, eliminating oxygen deficiencies and V O H can be reduced. Furthermore, an insulating layer having a barrier property against hydrogen is formed near the transistor 200, and V in the channel formation region of the semiconductor layer 230 and its vicinity is reduced. O It is preferable to reduce H.
[0099] Based on the above, it is preferable that at least one of the insulating layers 215, 221, 222, 275, 282, and 283 functions as a barrier insulating layer against hydrogen. Furthermore, it is preferable that at least one of the insulating layers 215, 221, 222, 275, 282, and 283 functions as a barrier insulating layer against impurities. Furthermore, it is preferable that at least one of the insulating layers 215, 221, 222, 275, 282, and 283 functions as a barrier insulating layer against oxygen. Note that it is not necessarily required to provide all of the insulating layers 215, 221, 222, 275, 282, and 283. If sufficient barrier properties are provided against hydrogen, impurities, oxygen, etc., the insulating layer can be appropriately selected from insulating layer 215, insulating layer 221, insulating layer 222, insulating layer 275, insulating layer 282, and insulating layer 283 to form the layer.
[0100] Note that in this specification and the like, a barrier insulating layer refers to an insulating layer having barrier properties. In addition, in this specification and the like, having barrier properties refers to having a property that a corresponding substance is less likely to diffuse (also referred to as a property that a corresponding substance is less likely to permeate, a property that the permeability of a corresponding substance is low, or a function of suppressing diffusion of a corresponding substance). Alternatively, it refers to having a function of trapping or fixing the corresponding substance inside the insulating layer (also referred to as gettering). Note that hydrogen when described as the corresponding substance includes, for example, at least one of a hydrogen atom, a hydrogen molecule, a water molecule, and OH − and the like, which are substances bonded to hydrogen. In addition, impurities when described as the corresponding substance refer to impurities in a channel formation region or a semiconductor layer unless otherwise specified, and include, for example, at least one of a hydrogen atom, a hydrogen molecule, a water molecule, a nitrogen atom, a nitrogen molecule, and a nitrogen oxide molecule (N 2 O, NO, NO 2 and the like), a copper atom, or the like. In addition, oxygen when described as the corresponding substance refers to at least one of, for example, an oxygen atom, an oxygen molecule, and the like.
[0101] As the insulating layer having a function of suppressing diffusion of hydrogen, for example, silicon nitride or silicon nitride oxide is preferably used. Further, for example, aluminum oxide, magnesium oxide, hafnium oxide, zirconium oxide, an oxide containing aluminum and hafnium (hafnium aluminate), an oxide containing hafnium and zirconium (hafnium zirconium oxide), gallium oxide, indium gallium zinc oxide, or the like can sometimes be used.
[0102] Note that in this specification and the like, an oxynitride refers to a material having a higher oxygen content than nitrogen in its composition, and a nitride oxide refers to a material having a higher nitrogen content than oxygen in its composition. For example, when silicon oxynitride is described, it refers to a material having a higher oxygen content than nitrogen in its composition, and when silicon nitride oxide is described, it refers to a material having a higher nitrogen content than oxygen in its composition.
[0103] It is preferable to use insulating layers that have the function of suppressing hydrogen diffusion for insulating layer 221, insulating layer 275, and insulating layer 283. For example, it is preferable to use silicon nitride with higher hydrogen barrier properties for insulating layer 221, insulating layer 275, and insulating layer 283.
[0104] As an insulating layer having the function of capturing or fixing hydrogen, it is preferable to use metal oxides such as hafnium oxide, aluminum oxide, aluminum and hafnium oxide (hafnium aluminate), or magnesium oxide. The insulating layer having the function of capturing or fixing hydrogen preferably has an amorphous structure. In metal oxides having such an amorphous structure, oxygen atoms have dangling bonds, and these dangling bonds may have the property of capturing or fixing hydrogen. In other words, metal oxides having an amorphous structure can be said to have a high ability to capture or fix hydrogen. By adding silicon to the above metal oxide, polycrystallization can be suppressed and it can be made more amorphous. Therefore, it is preferable to use metal oxides to which silicon has been added (for example, hafnium silicate, aluminum silicate, etc.).
[0105] It is preferable to use insulating layers that have the function of capturing or fixing hydrogen in insulating layer 222 and insulating layer 282. For example, it is preferable to use aluminum oxide in insulating layer 282. Also, for example, it is preferable to use hafnium oxide in insulating layer 222.
[0106] Furthermore, the inorganic insulating layers listed as having the function of suppressing hydrogen diffusion and the function of capturing or fixing hydrogen also possess barrier properties against oxygen.
[0107] Furthermore, as shown in Figure 3B, it is preferable to provide an insulating layer 221 having the function of suppressing hydrogen diffusion and an insulating layer 222 having the function of capturing or fixing hydrogen below the transistor 200. By providing the insulating layer 221 below the transistor 200, the diffusion of hydrogen from the layer below the transistor 200 can be suppressed. Also, by providing the insulating layer 222 on top of the insulating layer 221, hydrogen contained in the insulating layer 224, etc., can be captured or fixed to the insulating layer 222. This makes it possible to reduce the hydrogen concentration in and near the semiconductor layer 230.
[0108] Furthermore, as shown in Figure 3B, it is preferable to provide an insulating layer 275 that covers the conductive layer 242a, conductive layer 242b, etc. By providing the insulating layer 275 in this way, it is possible to suppress the diffusion of hydrogen from the insulating layer 280 to the semiconductor layer 230, conductive layer 242a, conductive layer 242b, etc.
[0109] Furthermore, as shown in Figure 3B, it is preferable to provide an insulating layer 282 having the function of capturing or fixing hydrogen, and an insulating layer 283 having the function of suppressing hydrogen diffusion, on top of the transistor 200. By providing the insulating layer 283 on top of the transistor 200, the diffusion of hydrogen from the upper layer of the transistor 200 can be suppressed. Also, by providing the insulating layer 282 below the insulating layer 283, hydrogen contained in the insulating layer 280, etc., can be captured or fixed to the insulating layer 282. This makes it possible to reduce the hydrogen concentration in and near the semiconductor layer 230.
[0110] The insulating layer 215 provided beneath the transistor 200 may have the same configuration as either one or both of the insulating layers 282 and 283. In this case, the insulating layer 215 may have a laminated structure of insulating layers 282 and 283, and may be configured with insulating layer 282 at the bottom and insulating layer 283 at the top, or with insulating layer 282 at the top and insulating layer 283 at the bottom.
[0111] In this way, by surrounding the top and bottom of the transistor 200 with a barrier insulating layer against hydrogen, the diffusion of hydrogen into the semiconductor layer 230 is reduced, and the V in the channel formation region is reduced. OThis allows for a reduction in H. This, in turn, improves the electrical characteristics and reliability of transistor 200.
[0112] Furthermore, it is preferable to include oxygen that is desorbed by heating in the insulating layer 280. By supplying this oxygen to the semiconductor layer 230 via the insulating layer 250 through the heat treatment, oxygen deficiencies in the channel formation region can be reduced. Similarly, it is preferable to include oxygen that is desorbed by heating in the insulating layer 224. This allows oxygen to be supplied from the insulating layer 224 to the semiconductor layer 230, further reducing oxygen deficiencies in the channel formation region.
[0113] In this embodiment, oxygen can be added to the insulating layer 280 by forming the insulating layer 282 using a sputtering method in an atmosphere containing oxygen gas.
[0114] As described above, by heat treatment on the insulating layer 280, which contains oxygen that is desorbed by heating, oxygen can be supplied to the semiconductor layer 230 via the insulating layer 250. In this heat treatment, insulating layers 282 and 283, which have barrier properties against oxygen, are formed on the insulating layer 280, so it is possible to prevent excessive diffusion of oxygen contained in the insulating layer 280 from the insulating layer 280.
[0115] If an excessive amount of oxygen is supplied to the source or drain region, it may cause a decrease in the on-current or field-effect mobility of the transistor 200. Furthermore, variations in the amount of oxygen supplied to the source or drain region within the substrate surface can lead to variations in the characteristics of the semiconductor device containing the transistor. In addition, if the amount of oxygen supplied from the insulating layer to the oxide semiconductor layer becomes excessively large, it may adversely affect the electrical characteristics and reliability of the transistor. Moreover, oxygen may diffuse into conductive layers such as the gate electrode, source electrode, and drain electrode, causing oxidation of these conductive layers and impairing their conductivity.
[0116] In contrast, since an insulating layer 275 having an oxygen barrier property is formed between the insulating layer 280 and the conductive layers 242a and 242b, it is possible to prevent oxygen contained in the insulating layer 280 from excessively diffusing into the semiconductor layer 230, the conductive layer 242a, and the conductive layer 242b.
[0117] The insulating layer 224 has its lower surface in contact with the insulating layer 222 and its upper surface in contact with the semiconductor layer 230. The shape of the insulating layer 224 in plan view is the same as that of the semiconductor layer 230, and in plan view, the insulating layer 224 overlaps with the semiconductor layer 230. In other words, the side edges of the insulating layer 224 coincide with or roughly coincide with the side edges of the semiconductor layer 230 in plan view. Here, if the semiconductor layer 230 has a tapered shape with a taper angle of less than 90°, the insulating layer 224 may also have a tapered shape with a taper angle of less than 90°. In this case, the upper end of the insulating layer 224 coincides with or roughly coincides with the lower end of the semiconductor layer 230.
[0118] As shown in Figure 4A, it is preferable that the thickness of the insulating layer 224 inside the opening 201 is greater than the thickness of the insulating layer 250. With this configuration, the lower surface of the conductive layer 260 located inside the opening 201 can be positioned below the lower surface of the semiconductor layer 230 by the difference between the thickness of the insulating layer 224 inside the opening 201 and the thickness of the insulating layer 250.
[0119] By positioning the lower surface of the conductive layer 260 below the lower surface of the semiconductor layer 230, a sufficient gate electric field can be applied from the upper surface to the lower surface of the semiconductor layer 230. In other words, within an opening in the insulating layer 280, the entire semiconductor layer 230 can be electrically surrounded by the electric field of the conductive layer 260, allowing it to function as a channel formation region. This configuration prevents the lower surface of the semiconductor layer 230 and its vicinity from functioning as a parasitic channel, thereby reducing the leakage current between the conductive layer 242a and the conductive layer 242b. Furthermore, it is possible to suppress characteristic defects such as normally-on behavior of the transistor 200 caused by the parasitic channel. In short, the electrical characteristics of the transistor 200 can be improved.
[0120] Furthermore, as described above, by making the entire semiconductor layer 230 function as a channel formation region from top to bottom, the channel width can be increased. This allows for increased on-current and transconductance of the transistor 200. In addition, the frequency characteristics of the transistor 200 can be improved.
[0121] In this specification, the transistor structure in which the channel formation region is electrically surrounded by the electric field of the gate electrode, as described above, is called a surrounded channel (S-channel) structure. In an S-channel structure, the gate electrode is arranged to surround at least two sides of the channel (specifically, two, three, or four sides, etc.). By adopting an S-channel structure, it is possible to increase resistance to short-channel effects, or in other words, to create a transistor in which short-channel effects are less likely to occur.
[0122] Furthermore, since the S-channel structure electrically surrounds the channel formation region, it can be said that it is essentially equivalent to the GAA (Gate All Around) structure or the LGAA (Lateral Gate All Around) structure. By making the transistor 200 an S-channel structure, a GAA structure, or an LGAA structure, the channel formation region formed at or near the interface between the semiconductor layer 230 and the gate insulating layer can be made the entire bulk. Therefore, it becomes possible to improve the current density flowing through the transistor, and thus an improvement in the transistor's on-current or an increase in the transistor's field-effect mobility can be expected.
[0123] The conductive layers 242a and 242b can be made from conductive materials described in the section on "conductive layers". It is preferable to use conductive materials that are not easily oxidized excessively for each of the conductive layers 242a and 242b. Examples of such conductive materials include conductive oxides and conductive nitrides. By using these, it is possible to suppress excessive oxidation of the conductive layers 242a and 242b, which would reduce the conductivity of the conductive layers 242a and 242b.
[0124] It is preferable to use a conductive material that is less susceptible to excessive oxidation for the layers of conductive layer 242a and conductive layer 242b that are in contact with the semiconductor layer 230 (conductive layer 242a1 and conductive layer 242b1). This suppresses excessive oxidation of conductive layer 242a and conductive layer 242b, which reduces their conductivity. It also suppresses the extraction of oxygen from the semiconductor layer 230, which can lead to the formation of excessive oxygen deficiencies.
[0125] As conductive layers 242a1 and 242b1, materials such as ITO, ITSO, IZO (registered trademarks), indium titanium oxide (In-Ti oxide), ruthenium, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, and oxides containing lanthanum and nickel can be used. These materials are preferred because they are conductive materials that are resistant to oxidation or maintain conductivity even when absorbing oxygen. Furthermore, because these materials are conductive metal oxides, the contact resistance between conductive layer 242a and semiconductor layer 230, and the contact resistance between conductive layer 242b and semiconductor layer 230 can be reduced. With such a structure, the on-current of the transistor 200 can be increased.
[0126] Furthermore, it is preferable to use metal nitrides as conductive layers 242a1 and 242b1, for example, nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing titanium and aluminum, etc. For example, tantalum nitride can be used as conductive layer 242a1 and conductive layer 242b1.
[0127] Furthermore, it is preferable that the conductive layers 242a2 and 242b2 have higher conductivity than the conductive layers 242a1 and 242b1. For example, it is preferable that the film thickness of the conductive layers 242a2 and 242b2 be thicker than the film thickness of the conductive layers 242a1 and 242b1. For example, tungsten, copper, or aluminum can be used as the conductive layers 242a2 and 242b2. By adopting the above structure, the resistance of the conductive layers 242a2 and 242b2 can be reduced. This makes it possible to increase the on-current of the transistor 200 and improve the operating speed of the semiconductor device according to this embodiment.
[0128] For example, ITO can be used as conductive layer 242a1 and conductive layer 242b1, and tungsten can be used as conductive layer 242a2 and conductive layer 242b2.
[0129] In the above example, the conductive layer 242a and conductive layer 242b are shown as a two-layer laminated structure, but the present invention is not limited to this, and the conductive layer 242a and conductive layer 242b can also be a single layer or a laminated structure of three or more layers. In this case, conductive materials that can be used for conductive layer 242a1 and conductive layer 242b1 can be used for conductive layer 242a and conductive layer 242b.
[0130] The conductive layer 260 can use the conductive material described in the section on "Conductive Layers," similar to conductive layers 242a and 242b. It is preferable to use a conductive material that is not easily oxidized excessively, or a conductive material that has a function to suppress oxygen diffusion, as the conductive layer 260. Examples of such conductive materials include conductive materials containing nitrogen and conductive materials containing oxygen. This helps to suppress a decrease in the conductivity of the conductive layer 260.
[0131] Figures 3B and 4A show an example in which the conductive layer 260 has a conductive layer 260_1 and a conductive layer 260_2 on the conductive layer 260_1. In this case, it is preferable to use a conductive material that is resistant to oxidation, as described above, or a conductive material that has the function of suppressing oxygen diffusion, as the conductive layer 260_1.
[0132] The conductive layer 260_1 preferably uses a conductive material that has the function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, and copper atoms. Alternatively, it is preferable to use a conductive material that has the function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms and oxygen molecules).
[0133] Furthermore, because the conductive layer 260_1 has the function of suppressing oxygen diffusion, it is possible to suppress oxidation of the conductive layer 260_2 and a decrease in conductivity due to oxygen contained in the insulating layer 280, etc. As a conductive material that has the function of suppressing oxygen diffusion, it is preferable to use, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, ruthenium oxide, etc.
[0134] Furthermore, it is preferable to use a material with high conductivity for the conductive layer 260_2. For example, the conductive layer 260_2 can be tungsten, copper, or aluminum. The conductive layer 260_2 may also be a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above-mentioned conductive material.
[0135] Furthermore, in transistor 200, the conductive layer 260 is formed self-aligned to fill the opening 201 formed in the insulating layer 280, etc. Here, the side surface of the insulating layer 280 at the opening 201 coincides with or approximately coincides with the side surface of the conductive layer 242a and the side surface of the conductive layer 242b. Therefore, the conductive layer 260 can be provided superimposed on the region between the conductive layer 242a and the conductive layer 242b without the need for alignment.
[0136] It is preferable that insulating layers 216, 280, and 285 each have a lower dielectric constant than insulating layer 222. By using materials with low dielectric constants as interlayer insulating layers, parasitic capacitance between wiring can be reduced.
[0137] For example, it is preferable that the insulating layer 216, insulating layer 280, and insulating layer 285 each contain one or more of the following: silicon oxide, silicon oxynitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, and silicon oxide with voids.
[0138] In particular, silicon oxide and silicon oxide-nitride are preferred because they are thermally stable. Materials such as silicon oxide, silicon oxide-nitride, and silicon oxide with vacancies are especially preferred because they can easily form regions containing oxygen that is released by heating.
[0139] Furthermore, the upper surfaces of insulating layer 216, insulating layer 280, and insulating layer 285 may each be flattened.
[0140] It is preferable that the concentration of impurities such as water and hydrogen in the insulating layer 280 is reduced. For example, it is preferable that the insulating layer 280 has an oxide containing silicon, such as silicon oxide or silicon oxynitride.
[0141] The conductive layer 240 is preferably made of tungsten, copper, or aluminum. Alternatively, the conductive layer 240 may have a laminated structure in which the first conductive layer is provided in contact with the side surface of the insulating layer 241, and a second conductive layer is provided further inside. In this case, the above-mentioned conductive material can be used as the second conductive layer. Here, the first conductive layer corresponds to conductive layer 240a1 and conductive layer 240b1 shown in Figures 3B, 4B, etc. The second conductive layer corresponds to conductive layer 240a2 and conductive layer 240b2 shown in Figures 3B, 4B, etc.
[0142] Furthermore, when the conductive layer 240 has a laminated structure, it is preferable to use conductive materials that have the function of suppressing the permeation of impurities such as water and hydrogen for the conductive layers 240a1 and 240b1 provided near the insulating layers 285, 283, 282, 280, and 275, respectively. For example, it is preferable to use tantalum, tantalum nitride, titanium, titanium nitride, ruthenium, ruthenium oxide, etc. Also, the conductive material that has the function of suppressing the permeation of impurities such as water and hydrogen may be used in a single layer or in a laminated structure. With such a configuration, it is possible to suppress the mixing of impurities such as water and hydrogen contained in the layers above the insulating layer 285 into the semiconductor layer 230 through the conductive layers 240a and 240b.
[0143] As the insulating layer 241, any material that can be used for the insulating layer 275, etc., can be used. For example, silicon nitride, aluminum oxide, silicon oxide nitride, etc., can be used as the insulating layer 241. By providing the insulating layer 241, it is possible to suppress the mixing of impurities such as water and hydrogen contained in the insulating layer 280, etc., into the semiconductor layer 230 through the conductive layer 240a and conductive layer 240b. Silicon nitride is particularly suitable because it has high barrier properties against hydrogen. In addition, it is possible to prevent oxygen contained in the insulating layer 280 from being absorbed by the conductive layer 240a and conductive layer 240b.
[0144] In the above description, as shown in Figure 3A, the shapes of openings 203a and 203b are rectangular in plan view, but are not limited to this. For example, openings 203a and 203b may be circular, elliptical or other approximate circular shapes, quadrilateral or other polygonal shapes, or quadrilateral or other polygonal shapes with rounded corners, respectively, in plan view.
[0145] <Example of Semiconductor Device Configuration 2> Below, we will describe a semiconductor device having a transistor with some configuration differences from transistor 200. Note that we will mainly describe the configuration differences from transistor 200, and similar configurations will be omitted as appropriate.
[0146] [Configuration Example 2-1] Figures 5A to 6B show an example configuration of a semiconductor device having a transistor 200A on a substrate (not shown). Figure 5A is a plan view showing the above example configuration of the semiconductor device. Figure 5B is a cross-sectional view between the dashed lines A1 and A2 shown in Figure 5A, and is also a cross-sectional view of the transistor 200A in the channel length direction. Figure 6A is a cross-sectional view between the dashed lines B1 and B2 shown in Figure 5A, and is also a cross-sectional view of the transistor 200A in the channel width direction. Figure 6B is a cross-sectional view between the dashed lines B3 and B4 shown in Figure 5A, and is also a cross-sectional view of the transistor 200A in the channel width direction.
[0147] Transistor 200A differs from transistor 200 in that it has conductive layers 233a and 233b. Conductive layers 233a and 233b each have a region in contact with the upper surface of semiconductor layer 230. In transistor 200A, conductive layer 242a may have a region in contact with the upper surface of conductive layer 233a, a region in contact with the side surface of conductive layer 233a, a region in contact with the side surface of semiconductor layer 230, a region in contact with the side surface of insulating layer 224, and a region in contact with the upper surface of insulating layer 222. Conductive layer 242b may have a region in contact with the upper surface of conductive layer 233b, a region in contact with the side surface of conductive layer 233b, a region in contact with the side surface of semiconductor layer 230, a region in contact with the side surface of insulating layer 224, and a region in contact with the upper surface of insulating layer 222. In transistor 200A, the opening 201 has a region that overlaps with the region between conductive layer 233a and conductive layer 233b. The insulating layer 250 may also have a region that is in contact with the side surface of conductive layer 233a and a region that is in contact with the side surface of conductive layer 233b.
[0148] The sum of the areas of the undersides of conductive layer 233a and conductive layer 233b is smaller than the area of the underside of semiconductor layer 230. The sum of the areas of the undersides of conductive layer 233a and conductive layer 233b can be equal to, or approximately equal to, the area of the region of semiconductor layer 230 that does not overlap with the opening 201. In this case, as shown in Figure 5A, the side edge of conductive layer 233a on the opening 201 side can coincide with or approximately coincide with the side edge of conductive layer 242a on the opening 201 side in a plan view. Also, the side edge of conductive layer 233b on the opening 201 side can coincide with or approximately coincide with the side edge of conductive layer 242b on the opening 201 side in a plan view. Furthermore, as shown in Figures 5B and 6B, the lower ends of conductive layer 233a and conductive layer 233b opposite to the opening 201 can coincide with or approximately coincide with the upper end of semiconductor layer 230, respectively.
[0149] For conductive layers 233a and 233b, materials that can be used for conductive layers 242a and 242b can be used, for example. In this case, conductive layer 233a functions as one of the source and drain electrodes of transistor 200A, similar to conductive layer 242a. Conductive layer 233b functions as the other of the source and drain electrodes of transistor 200A, similar to conductive layer 242b.
[0150] The conductive layers 233a and 233b can each be arranged in a laminated structure, similar to the conductive layers 242a and 242b. In this case, the conductive layers 233a and 233b can each be arranged in a laminated structure consisting of a first conductive layer that is less susceptible to excessive oxidation and a second conductive layer that has higher conductivity than the first conductive layer.
[0151] By providing conductive layers 233a and 233b, the thickness of the source electrode and the drain electrode of the transistor in the region overlapping with the upper surface of the semiconductor layer 230 can be increased. Therefore, the electrical resistance of the source electrode and the drain electrode can be reduced.
[0152] [Configuration Example 2-2] Figures 7A to 8B show an example configuration of a semiconductor device having a transistor 200B on a substrate (not shown). Figure 7A is a plan view showing the above example configuration of the semiconductor device. Figure 7B is a cross-sectional view between the dashed lines A1 and A2 shown in Figure 7A, and is also a cross-sectional view of the transistor 200B in the channel length direction. Figure 8A is a cross-sectional view between the dashed lines B1 and B2 shown in Figure 7A, and is also a cross-sectional view of the transistor 200B in the channel width direction. Figure 8B is a cross-sectional view between the dashed lines B3 and B4 shown in Figure 7A, and is also a cross-sectional view of the transistor 200B in the channel width direction.
[0153] Transistor 200B differs from transistor 200 in that it has a metal oxide layer 235. The metal oxide layer 235 is provided on the insulating layer 224. In transistor 200B, the semiconductor layer 230 has a region in contact with the metal oxide layer 235, for example, a region in contact with the upper surface of the metal oxide layer 235. Figure 7B shows an example in which the semiconductor layer 230 covers the metal oxide layer 235 in a cross-sectional view of transistor 200B in the channel length direction. Figure 8B shows an example in which the upper end of the metal oxide layer 235 coincides with or roughly coincides with the lower end of the semiconductor layer 230 in a cross-sectional view of transistor 200B in the channel width direction.
[0154] The metal oxide layer 235 has crystals and functions as a seed or nucleus to enhance the crystallinity of the semiconductor layer 230. Therefore, the metal oxide layer 235 can be called a seed layer, seed crystal, crystal nucleus, etc.
[0155] For example, indium oxide or IGZO can be used as the metal oxide layer 235. When In-Ga-Zn oxide is used as the metal oxide layer 235, it is preferable to have a composition such as In:Ga:Zn = 1:1:1 [atomic ratio] or close to that, In:Ga:Zn = 1:1:1.2 [atomic ratio] or close to that, or In:Ga:Zn = 1:3:2 [atomic ratio] or close to that. In addition, zinc oxide, indium gallium oxide (In-Ga oxide), gallium zinc oxide (Ga-Zn oxide, also written as GZO), aluminum zinc oxide (Al-Zn oxide, also written as AZO), indium aluminum zinc oxide (In-Al-Zn oxide, also written as IAZO), or indium tin zinc oxide (In-Sn-Zn oxide, also written as ITZO®) can be used as the metal oxide layer 235. In addition, yttrium oxide, erbium oxide, etc., can be used. Furthermore, indium tin oxide (In-Sn oxide, also called ITO), silicon-containing indium tin oxide (In-Sn-Si oxide, also called ITSO), etc., can be used. Note that the boundary between the metal oxide layer 235 and the semiconductor layer 230 may not be clearly visible.
[0156] In-Ga-Zn oxides and In-Sn-Zn oxides, etc., tend to have a CAAC (c-axis aligned crystal) structure. When an oxide having a CAAC structure is used in the metal oxide layer 235, the c-axis direction of the metal oxide layer 235 is parallel or approximately parallel to the thickness direction of the insulating layer 224. Therefore, by using an oxide that tends to have a CAAC structure in the metal oxide layer 235, the controllability of the crystal planes of the crystal grains in the metal oxide layer 235 can be improved.
[0157] The shape of the metal oxide layer 235 in plan view can be island-like or striped. The sides of the metal oxide layer 235 may also have a tapered shape. The number of metal oxide layers 235 provided on the insulating layer 224 may be one or multiple.
[0158] A thin metal oxide layer 235 is preferable. The metal oxide layer 235 is preferably greater than 0 nm and 5 nm or less, more preferably greater than 0 nm and 3 nm or less, and even more preferably greater than 0 nm and 2 nm or less. It is preferable that the metal oxide layer 235 has a region with the above-mentioned thickness in at least a part of it. By making the metal oxide layer 235 thinner, the step difference between the metal oxide layer 235 and the insulating layer 224 is reduced. Therefore, the coverage of the semiconductor layer 230 is improved, and defects such as porosity can be reduced. In addition, the crystallinity of the semiconductor layer 230 can be improved.
[0159] [Configuration Example 2-3] Figure 9A is a plan view showing an example configuration of a semiconductor device having a transistor 200C on a substrate (not shown). Figure 9B is an enlarged plan view showing an excerpt of the semiconductor layer 230 and conductive layer 260 of the transistor 200C shown in Figure 9A. Figure 10A is a cross-sectional view between the dashed lines A1 and A2 shown in Figure 9A, and is also a cross-sectional view of the transistor 200C in the channel length direction. Figure 10B is a cross-sectional view between the dashed lines B1 and B2 shown in Figure 9A, and is also a cross-sectional view of the transistor 200C in the channel width direction. Note that the cross-sectional view between the dashed lines B3 and B4 shown in Figure 9A can be found in Figure 8B.
[0160] The shape of the semiconductor layer 230 in a plan view of transistor 200C differs from that of transistor 200B shown in Figure 7A. However, transistor 200C, like transistor 200B, has a metal oxide layer 235.
[0161] The semiconductor layer 230 of the transistor 200C has a first region 231_1, a second region 231_2, and a third region 231_3. The first region 231_1 is in contact with the upper surface of the metal oxide layer 235. The second region 231_2 and the third region 231_3 are in contact with the insulating layer 224. The second region 231_2 is adjacent to the first region 231_1 and is located between the first region 231_1 and the third region 231_3.
[0162] In the third region 231_3, the channel widthwise length of transistor 200C is shorter than the channel widthwise length of transistor 200C in the first region 231_1 and the second region 231_2, respectively. In Figure 9B, the channel widthwise length of transistor 200C in the third region 231_3 is shown as width j1. Also, the channel widthwise length of transistor 200C in the second region 231_2 is shown as width j2.
[0163] The third region 231_3 has a first portion that overlaps with the conductive layer 260. The first portion functions as a channel formation region for the transistor 200C. The third region 231_3 also has a second portion that is in contact with the conductive layer 242a and a third portion that is in contact with the conductive layer 242b. The first portion is located between the second and third portions. Here, the second region 231_2 is adjacent to either the second or third portion of the third region 231_3. The second region 231_2 is located closer to the conductive layer 260 than the first region 231_1.
[0164] In Figure 9B, the grain boundaries of the semiconductor layer 230 are shown by solid lines. The first region 231_1 and the second region 231_2 can each have multiple crystal grains. At least one crystal grain in the second region 231_2 extends into the third region 231_3. The grain size of the crystal grain in the second region 231_2 is larger than the grain size of the crystal grain in the first region 231_1. Furthermore, the third region 231_3 has fewer grain boundaries than either or both of the first region 231_1 or the second region 231_2.
[0165] The crystallinity of the metal oxide layer 235 and the semiconductor layer 230 can be analyzed, for example, by methods using X-ray diffraction (XRD), TEM, electron diffraction (ED), or electron diffraction mapping. Alternatively, a combination of these methods may be used for analysis.
[0166] Furthermore, crystal grains can be identified, for example, in high-resolution TEM images. Also, crystal grain boundaries can sometimes be identified, for example, in high-resolution TEM images. In other words, crystal grains and crystal grain boundaries of a crystalline film can sometimes be observed in high-resolution TEM images. When acquiring crystal grains and crystal grain boundaries of a crystalline film using TEM images, the overall magnification is preferably 2 million times or more, and more preferably 4 million times or more.
[0167] Furthermore, the grain size of the crystal grains can also be confirmed, for example, using an optical microscope, a scanning electron microscope (SEM), or an AFM. Additionally, by creating surface irregularities on the metal oxide layer 235 and the semiconductor layer 230 using etchants with different etching rates depending on the crystal plane or crystallinity, the crystal grains can be more easily observed using an optical microscope, SEM, or AFM. When using indium oxide films as the metal oxide layer 235 and the semiconductor layer 230, the crystal grains of indium oxide can be more easily observed by using an etchant containing an acid. For example, one or more of phosphoric acid, oxalic acid, hydrofluoric acid, nitric acid, and hydrochloric acid can be used as the acid. However, if the etching amount is too large, parts of the metal oxide layer 235 and the semiconductor layer 230 may disappear, making it difficult to observe the crystal grains. Therefore, it is preferable to adjust the etching amount by the type, concentration, temperature, and processing time of the etchant so that the metal oxide layer 235 and the semiconductor layer 230 do not disappear but their thickness is reduced (also called half-etching). By performing half-etching, it becomes possible to easily observe the crystal grains.
[0168] Furthermore, the crystallinity of the semiconductor layer 230 can be evaluated by the grain size of the crystal grains. The grain size of the crystal grains can be calculated, for example, by calculating the area of the crystal grains and then determining the diameter of a circle that corresponds to that area. This diameter is sometimes called the area circle equivalent diameter.
[0169] Furthermore, the crystallinity of the semiconductor layer 230 can also be evaluated by the length of the grain boundaries. The length of the grain boundaries can be calculated, for example, by extracting a field of view of a specific area from a TEM image of the film acquired at a total magnification that allows observation of the grain boundaries, and summing the lengths of the grain boundaries observed in that field of view. A longer length of the grain boundaries indicates a greater amount of grain boundary components. A shorter length of the grain boundaries indicates larger grain sizes, while a longer length of the grain boundaries indicates smaller grain sizes.
[0170] Electron diffraction mapping is a technique that uses electron diffraction from a TEM to analyze the orientation distribution of crystalline samples. Crystal information is obtained by measuring the electron diffraction pattern at each point while scanning the electron probe. For example, grain boundaries can be observed by utilizing the difference in orientation between adjacent measurement points. For instance, grain boundaries can be observed by analyzing orientation differences of 5° or more as grain boundaries.
[0171] The semiconductor layer 230 shown in Figure 9B can be formed by a first step of forming an island-shaped metal oxide layer 235 having crystals on an insulating layer 224; a second step of forming a semiconductor layer 230 by covering the upper surface and the side surface on the second region 231_2 side of the metal oxide layer 235; a third step of processing the semiconductor layer 230 to have a first region 231_1, a second region 231_2, and a third region 231_3; and a fourth step of performing a crystallization treatment on the semiconductor layer 230.
[0172] In the method described above, the semiconductor layer 230 can be crystallized by processing it to have a first region 231_1, a second region 231_2, and a third region 231_3, and then performing a treatment to enhance its crystallinity. During crystallization, the first region 231_1, which is in contact with the metal oxide layer 235, crystallizes. Here, multiple crystal grains may be generated in the first region 231_1. Therefore, if the first region 231_1 and the third region 231_3 are adjacent, the third region 231_3 is likely to be composed of multiple crystal grains, and there is a risk of many grain boundaries being generated. For this reason, a distance is required between the first region 231_1 and the third region 231_3 for the crystal to grow.
[0173] Therefore, in one embodiment of the present invention, the semiconductor layer 230 has a second region 231_2 between the first region 231_1 and the third region 231_3. As a result, crystal grains are generated from the first region 231_1 and grow in the second region 231_2. In the second region 231_2, crystal grains with a fast crystal growth rate grow larger, and the number of crystal grains decreases and the size of each crystal grain increases as it moves away from the first region 231_1. This can be called geometric selection in crystal growth. Due to this geometric selection in crystal growth, the crystal grows in the second region 231_2 in such a way that the crystal grains spread out widely. In the semiconductor layer 230, the shape of the third region, where the width j1 is narrower than the width j2 of the second region, allows for the selection of crystal grains. This enables the guidance of only the crystal grains that have grown toward the third region 231_3 from among those grown in the second region 231_2, allowing them to grow in the third region 231_3. Thus, in addition to geometric selection in the second region 231_2, the shape of the semiconductor layer 230 also allows for the selection of crystal grains that grow in the third region 231_3. By preferentially growing crystal grains that have reached the third region 231_3, the formation of crystal grain boundaries in the third region 231_3 can be suppressed. Alternatively, the third region 231_3 can be made into a region where no crystal grain boundaries are observed. Alternatively, the third region 231_3 can be defined as a region having a cross-section in the channel length direction of transistor 200C where no grain boundaries are observed, as determined by analysis using a transmission electron microscope. Alternatively, the third region 231_3 can be defined as a region that does not contain grain boundaries when analyzed by electron diffraction mapping, where adjacent measurement points with an orientation difference of 5° or more are defined as grain boundaries. Alternatively, the third region 231_3 can be defined as a single-grain crystal.
[0174] Furthermore, in a method for forming a metal oxide according to one aspect of the present invention, only the crystal grains that have grown toward the third region 231_3 from among the crystal grains grown in the second region 231_2 can be guided toward the third region 231_3 and allowed to grow crystals there. Therefore, it is preferable to process the semiconductor layer 230 to have a first region 231_1, a second region 231_2, and a third region 231_3, and then perform a process to enhance the crystallinity of the semiconductor layer 230. For this reason, the processing temperature of the third step in which the semiconductor layer 230 is processed to have a first region 231_1, a second region 231_2, and a third region 231_3 is preferably lower than the temperature of the process to enhance the crystallinity of the semiconductor layer 230.
[0175] Of the semiconductor layer 230, part or all of the third region 231_3 can be used as the channel formation region of the transistor 200C. In the transistor 200C, the channel formation region of the third region 231_3 can be a region in which no grain boundaries are observed. Alternatively, the channel formation region of the third region 231_3 can be a single-grain crystal. Alternatively, the channel formation region of the third region 231_3 can be a region having a cross-section in the channel length direction of the transistor 200C in which no grain boundaries are observed, by analysis using a transmission electron microscope. Alternatively, the channel formation region of the third region 231_3 can be a crystal that does not contain grain boundaries when analyzed by electron diffraction mapping, where adjacent measurement points with an orientation difference of 5° or more are considered as grain boundaries. Furthermore, the semiconductor layer 230 can have crystal grains that overlap with a pair of side edges of the conductive layer 260 facing each other in the channel length direction.
[0176] As a result, a semiconductor device with good electrical characteristics can be provided. Furthermore, a semiconductor device with high operating speed can be provided. Furthermore, a semiconductor device with high reliability can be provided. Furthermore, a semiconductor device with minimal variation in characteristics between transistors can be provided. Note that the third region 231_3 can be provided with channel formation regions for one or more transistors 200C.
[0177] The configurations of transistors 200A, 200B, and 200C can be combined as appropriate. For example, the configuration of transistor 200A can be combined with transistors 200B and 200C. That is, transistor 200B may have conductive layers 233a and 233b, and transistor 200C may have conductive layers 233a and 233b.
[0178] [Configuration Example 2-4] Figures 11A to 12 show examples of the configuration of a semiconductor device having a transistor 200 on a substrate (not shown). Figure 11A is a plan view showing the above-mentioned configuration example of the semiconductor device. Figure 11B is a cross-sectional view between the dashed lines A1 and A2 shown in Figure 11A, and is also a cross-sectional view of the transistor 200 in the channel length direction. Figure 12 is a cross-sectional view between the dashed lines B1 and B2 shown in Figure 11A, and is also a cross-sectional view of the transistor 200 in the channel width direction. Note that the cross-sectional view between the dashed lines B3 and B4 shown in Figure 11A can be found in Figure 4B.
[0179] The semiconductor device shown in Figures 11A to 12 differs from the semiconductor device shown in Figures 3A to 4A in that it has an insulating layer 255. The insulating layer 255 is provided inside the opening 201. The insulating layer 255 has a region in contact with the upper surface of the conductive layer 242a1, a region in contact with the upper surface of the conductive layer 242b1, a region in contact with the side surface of the conductive layer 242a2 on the opening 201 side, a region in contact with the side surface of the conductive layer 242b2 on the opening 201 side, a region in contact with the side surface of the insulating layer 275 in the opening 201, and a region in contact with the side surface of the insulating layer 280 in the opening 201. Here, the insulating layer 255 is formed in a sidewall shape in contact with the side wall of the opening 201. The insulating layer 255 is provided along the side wall of the opening 201. Therefore, the insulating layer 255 can also be considered as part of the side wall of the opening 201.
[0180] In Figure 11B, distance D1 is shown as the distance between conductive layer 242a1 and conductive layer 242b1 in a cross-sectional view of transistor 200 in the channel length direction. Distance D2 is shown as the distance between conductive layer 242a2 and conductive layer 242b2 in a cross-sectional view of transistor 200 in the channel length direction. Specifically, distance D1 represents the shortest distance between the opposing sides of conductive layer 242a1 and conductive layer 242b1. Specifically, distance D2 represents the shortest distance between the opposing sides of conductive layer 242a2 and conductive layer 242b2.
[0181] Distance D1 is shorter than distance D2. The difference between distance D1 and distance D2 is, for example, equal to or approximately equal to twice the thickness of the insulating layer 255. Here, the thickness of the insulating layer 255 refers to the thickness of the insulating layer 255 in the channel length direction of the transistor 200 in at least a portion of the insulating layer 255. With this configuration, the distance between the source electrode and the drain electrode of the transistor 200 can be shortened compared to when distance D1 is equal to distance D2. Therefore, the channel length of the transistor 200 can be shortened. Consequently, the on-current of the transistor 200 can be increased. On the other hand, in a configuration where the insulating layer 255 is not provided inside the opening 201, as shown in Figure 3B, for example, and distance D1 is equal to or approximately equal to distance D2, the number of manufacturing steps for the semiconductor device can be reduced, and the productivity of the semiconductor device can be increased.
[0182] Since the distance D1 is reflected in the channel length of the transistor 200, it is preferable that it be short. For example, the distance D1 is preferably 1 nm to 60 nm, more preferably 1 nm to 50 nm, more preferably 1 nm to 40 nm, more preferably 2 nm to 30 nm, more preferably 2 nm to 20 nm, and still more preferably 5 nm to 10 nm.
[0183] The thickness of the insulating layer 255 is preferably 1 nm to 20 nm, more preferably 1 nm to 15 nm, and more preferably 3 nm to 10 nm. For example, the thickness can be about 5 nm. By making the insulating layer 255 the thickness described above, the parasitic capacitance between the conductive layer 260 and the conductive layer 242a, and between the conductive layer 260 and the conductive layer 242b can be reduced, while the area occupied by the opening 201 can be reduced. It is preferable that the insulating layer 255 has a region with the above-described thickness in at least a portion of it.
[0184] The insulating layer 255 functions as a mask when dividing the conductive layers, which will become conductive layers 242a1 and 242b1, into conductive layer 242a1 and conductive layer 242b1. Therefore, in a cross-sectional view of the transistor 200, the inner side surface of the insulating layer 255 (on the insulating layer 250 side) can be made to coincide with or approximately coincide with the side edge of conductive layer 242a1 and the side edge of conductive layer 242b1.
[0185] The insulating layer 255 is preferably an insulating layer that has barrier properties against oxygen, and it is preferable to use a nitride such as silicon nitride. The insulating layer 255 is provided in contact with the side surfaces of the conductive layer 242a2 and the conductive layer 242b2, and has the function of protecting the conductive layer 242a2 and the conductive layer 242b2 from oxidation, for example. In this case, because the insulating layer 255 is formed in contact with the side surfaces of the conductive layer 242a2 and the conductive layer 242b2, it is possible to prevent the conductive layer 242a2 and the conductive layer 242b2 from being excessively oxidized. For example, even if materials that are more easily oxidized than conductive layer 242a1 and conductive layer 242b2 are used for conductive layer 242a2 and conductive layer 242b2, respectively, it is possible to prevent the side surfaces of conductive layer 242a2 and the conductive layer 242b2 from being excessively oxidized. For example, when supplying oxygen to the semiconductor layer 230, specifically when performing a heat treatment in an oxygen-containing atmosphere after the formation of the conductive layer 242a1 and the conductive layer 242b1, and before the deposition of the insulating layer 250, it is possible to prevent excessive oxidation of the sides of the conductive layer 242a2 and the conductive layer 242b2.
[0186] The insulating layer 255 is preferably formed using, for example, an atomic layer deposition (ALD) method, as this allows for good coverage of the opening 201.
[0187] In the semiconductor device shown in Figures 11A to 12, the insulating layer 250 may have a region in contact with the upper surface of the semiconductor layer 230, a region in contact with the side surface of the semiconductor layer 230, a region in contact with the side surface of the insulating layer 255, a region in contact with the side surface of the insulating layer 224, and a region in contact with the upper surface of the insulating layer 222. Furthermore, the height of the upper surface of the conductive layer 260 may be the same as or approximately the same as the height of the uppermost part of the insulating layer 255, the uppermost part of the insulating layer 250, and the height of the upper surface of the insulating layer 280.
[0188] Figures 11A to 12 show an example in which an insulating layer 255 is provided on a semiconductor device having a transistor 200, but the present invention is not limited to this. The insulating layer 255 may be provided on a semiconductor device having a transistor 200A, on a semiconductor device having a transistor 200B, or on a semiconductor device having a transistor 200C.
[0189] <Materials for semiconductor devices> The following describes materials that can be used in semiconductor devices. Note that each layer constituting a semiconductor device may be a single-layer structure or a multilayer structure.
[0190] <Substrate> The substrate for the semiconductor device shown in this embodiment can be any of the following substrates as appropriate.
[0191] As substrates for forming transistors, for example, insulating substrates, semiconductor substrates, or conductive substrates can be used. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (such as yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, gallium oxide, and gallium nitride. Furthermore, there are semiconductor substrates having insulating regions within the aforementioned semiconductor substrates, such as SOI (Silicon On Insulator) substrates. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Alternatively, substrates having metal nitrides or metal oxides can also be used. Furthermore, there are substrates in which a conductive layer or semiconductor layer is provided on an insulating substrate, substrates in which a conductive layer or insulating layer is provided on a semiconductor substrate, and substrates in which a semiconductor layer or insulating layer is provided on a conductive substrate. Alternatively, substrates with elements mounted on them may be used. Elements mounted on the substrate include capacitive elements, resistive elements, switching elements (including transistors), light-emitting elements, memory elements, and the like.
[0192] <Conductive Layers> The conductive layers 240a, 240b, 242a, 242b, and 260 of the semiconductor device shown in this embodiment may be appropriately made from the conductive materials listed below. It is preferable to use a highly conductive material for the conductive layers of the semiconductor device. For these conductive layers, it is preferable to use a metal element selected from, for example, aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, cobalt, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing such a metal element. Alternatively, nitrides of the above metal elements or alloys containing such metal elements, or oxides of the above metal elements or alloys containing such metal elements may be used. For example, it is preferable to use tantalum nitride, titanium nitride, nitrides containing titanium and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, oxides containing lanthanum and nickel, etc. These are preferred because they are conductive materials that are resistant to oxidation or that maintain conductivity even after oxidation. In addition, semiconductor materials with high electrical conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, and silicides such as nickel silicide may be used. Furthermore, tantalum, tantalum nitride, etc. are preferred as conductive materials because they have barrier properties against hydrogen.
[0193] Furthermore, conductive oxides can be used in the conductive layer of semiconductor devices. Examples of conductive oxides include indium oxide, indium tin oxide (In-Sn oxide, also called ITO), silicon-containing indium tin oxide (In-Sn-Si oxide, also called ITSO), In-Zn oxide, In-W oxide, In-W-Zn oxide, In-Ti oxide, In-Ti-Sn oxide, and the like. Conductive oxides containing indium are particularly preferred due to their high conductivity. Alternatively, oxide semiconductors applicable to semiconductor layers can also be used as conductive materials that can increase carrier concentration.
[0194] Furthermore, the conductive layer of the semiconductor device may be a single layer or a laminated structure of two or more layers using the aforementioned conductive material. For example, a single layer structure of conductive oxide, a single layer structure of tantalum nitride, a single layer structure of tungsten, etc., can be used. Also, a two-layer structure in which a conductive oxide is laminated on tungsten, a two-layer structure in which tungsten is laminated on tantalum nitride, a two-layer structure in which tungsten is laminated on a conductive oxide, a two-layer structure in which tungsten is laminated on titanium nitride, etc. can be used. In addition, a three-layer structure in which titanium nitride is laminated on tantalum nitride and tungsten is laminated on the titanium nitride, a three-layer structure in which aluminum is laminated on titanium and titanium is laminated on the aluminum, a three-layer structure in which tungsten is laminated on a titanium nitride film and a conductive oxide is laminated on the tungsten, a three-layer structure in which tungsten is laminated on a conductive oxide and a conductive oxide is laminated on the tungsten film, etc., can be used. Furthermore, a four-layer structure can be used in which tantalum nitride is laminated on tantalum, titanium nitride is laminated on the tantalum nitride, and tungsten is laminated on the titanium nitride; a four-layer structure can be used in which tantalum is laminated on tantalum nitride, titanium nitride is laminated on the tantalum, and tungsten is laminated on the titanium nitride; a four-layer structure can be used in which titanium nitride is laminated on tantalum nitride, tungsten is laminated on the titanium nitride, and a conductive oxide is laminated on the tungsten; and so on. In addition, a five-layer structure can be used in which titanium nitride is laminated on titanium, aluminum is laminated on the titanium nitride, titanium is laminated on the aluminum, and titanium nitride is laminated on the titanium; and so on.
[0195] <Insulating Layers> For the insulating layers 215, 216, 221, 222, 224, 250, 255, 275, 280, 282, 283, and 285 of the semiconductor device shown in this embodiment, the insulating materials shown below can be used as appropriate. Examples of insulating materials include insulating oxides, insulating nitrides, insulating oxidized nitrides, insulating nitride oxides, insulating metal oxides, insulating metal oxidized nitrides, and insulating metal nitride oxides.
[0196] As transistors become smaller and more integrated, thinning of the gate insulating layer can lead to problems such as leakage current. Using an insulating material with a high dielectric constant (high-k) for the gate insulating layer allows for lower voltage operation while maintaining the physical film thickness. On the other hand, using an insulating material with a low dielectric constant for the interlayer insulating layer reduces parasitic capacitance between wiring. Therefore, it is preferable to select materials according to the function of the insulating layer.
[0197] Examples of insulating materials with a high dielectric constant (high-k) include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium-zirconium oxide, oxides containing aluminum and hafnium, oxidized nitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxidized nitrides containing silicon and hafnium, and nitrides containing silicon and hafnium. In addition, an insulating film (also called ZAZ) laminated in the order of zirconium oxide, aluminum oxide, and zirconium oxide can be used. Alternatively, for example, an insulating film (also called ZAZA) laminated in the order of zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide can be used.
[0198] Examples of insulating materials with a lower dielectric constant compared to high-k materials include silicon oxide, silicon oxide nitride, silicon oxide nitride, silicon nitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, porous silicon oxide, and resins.
[0199] Examples of insulating materials with high dielectric strength include silicon oxide, silicon oxide nitride, silicon oxide nitride, and silicon nitride.
[0200] Examples of insulating materials that suppress leakage current include silicon oxide and silicon oxide nitride.
[0201] Furthermore, transistors using metal oxides can have their electrical properties stabilized by surrounding them with an insulating layer that has the function of suppressing the permeation of impurities such as hydrogen and oxygen. Examples of insulating layers that have the function of suppressing the permeation of impurities such as hydrogen and oxygen include insulating layers containing one or more of the following: boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum, which can be used as a single layer or in a multilayer structure. Specifically, examples include oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and nitrides such as aluminum nitride, silicon nitride, and silicon nitride.
[0202] Furthermore, insulating layers that are in contact with the oxide semiconductor layer, such as gate insulating layers, or insulating layers provided near the oxide semiconductor layer, are preferably insulating layers that have regions containing oxygen that is released by heating (hereinafter sometimes referred to as excess oxygen). For example, an insulating layer having regions containing excess oxygen can reduce oxygen vacancies in the oxide semiconductor layer by releasing oxygen and being in contact with or near the oxide semiconductor layer. Examples of insulating layer materials that easily form regions containing excess oxygen include silicon oxide, silicon oxynitride, or silicon oxide with vacancies.
[0203] It is preferable to use an insulating layer that has the function of capturing or fixing hydrogen, or an insulating layer that has barrier properties against hydrogen, as an insulating layer in contact with or near a metal oxide exhibiting semiconductor properties used in transistor channels, etc. This can suppress the diffusion of hydrogen into the metal oxide.
[0204] Examples of insulating materials that have the function of capturing or fixing hydrogen include hafnium oxide, hafnium silicate, and aluminum oxide.
[0205] Examples of insulating materials that have barrier properties against hydrogen include silicon nitride, hafnium oxide, aluminum oxide, magnesium oxide, gallium oxide, or silicon nitride oxide.
[0206] Examples of insulating materials that have barrier properties against oxygen include oxides containing one or both aluminum and hafnium, magnesium oxide, gallium oxide, zinc gallium oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).
[0207] Furthermore, a ferroelectric material may be used for the insulating layer of the semiconductor device. Examples of ferroelectric materials include metal oxides such as hafnium oxide, zirconium oxide, and hafnium-zirconium oxide.
[0208] Furthermore, a ferroelectric material can be used in at least a portion of the gate insulating layer of the transistor. A transistor having such a gate insulating layer can function as an FeFET (Ferroelectric Field Effect Transistor).
[0209] <Gate Insulating Layer> The insulating layer 250 of the semiconductor device shown in this embodiment can be made from the insulating materials described below as appropriate. The insulating layer 250 functions as a gate insulating layer of the transistor. The gate insulating layer, such as the insulating layer 250, can be made from the insulating materials described above in <Insulating Layer> as appropriate. The gate insulating layer, such as the insulating layer 250, can be made from a single layer or a laminated structure of two or more layers. When the gate insulating layer is made from a laminated structure of two or more layers, it is preferable to form it from two or more types of films. By making the gate insulating layer, such as the insulating layer 250, from two or more types of films, multiple functions can be provided.
[0210] Furthermore, the insulating layer 250 can be used by laminating one or more insulating layers, including an insulating layer with a high dielectric constant, an insulating layer with high dielectric strength, and an insulating layer that suppresses leakage current. In addition, a ferroelectric material can be used for the insulating layer 250 or other insulating layers.
[0211] The insulating layer 250 can have a two-layer structure, comprising a first insulating layer in contact with the semiconductor layer 230 and a second insulating layer on the conductive layer 260 side, which functions as the gate electrode. The first insulating layer can be made of an insulating material having the function of capturing or fixing hydrogen, and the second insulating layer can be made of an insulating material having hydrogen barrier properties, an insulating material having the function of suppressing the permeation of impurities such as hydrogen and oxygen, or an insulating material having oxygen barrier properties. With such a configuration, the hydrogen concentration in the semiconductor layer 230 can be reduced, and the diffusion of hydrogen into the semiconductor layer 230 can be suppressed. In addition, the diffusion of oxygen to the conductive layer 260 side can be prevented, and oxidation of the conductive layer 260 can be suppressed. This makes it possible to realize a highly reliable transistor. When the insulating layer 250 has a two-layer structure, for example, a hafnium oxide film or a hafnium silicate film can be used as the first insulating layer, and a silicon nitride film can be used as the second insulating layer.
[0212] Alternatively, an insulating material with high dielectric strength or an insulating material that suppresses leakage current can be used as the first insulating layer, and an insulating material having the function of capturing or fixing hydrogen, an insulating material having barrier properties against hydrogen, an insulating material having the function of suppressing the permeation of impurities such as hydrogen and oxygen, or an insulating material having barrier properties against oxygen can be used as the second insulating layer. With such a configuration, the gate leakage current can be reduced and the diffusion of hydrogen into the semiconductor layer 230 can be suppressed. In addition, the diffusion of oxygen to the conductive layer 260 can be prevented and oxidation of the conductive layer 260 can be suppressed. Therefore, a highly reliable transistor can be realized. When the insulating layer 250 has a two-layer structure, for example, a silicon oxide film can be used as the first insulating layer and a hafnium oxide film can be used as the second insulating layer.
[0213] Alternatively, the insulating layer 250 can have a three-layer structure comprising a first insulating layer, a second insulating layer, and a third insulating layer. In this case, the first insulating layer is in contact with the semiconductor layer 230, and the first insulating layer, the second insulating layer, and the third insulating layer are positioned in that order from the semiconductor layer 230 side toward the conductive layer 260 which functions as the gate electrode side. The first insulating layer can be made of an insulating material with high dielectric strength or an insulating material that suppresses leakage current, the second insulating layer can be made of an insulating material that has the function of capturing or fixing hydrogen, and the third insulating layer can be made of an insulating material that has barrier properties against hydrogen, an insulating material that has the function of suppressing the permeation of impurities such as hydrogen and oxygen, or an insulating material that has barrier properties against oxygen. With such a configuration, gate leakage current can be reduced and the diffusion of hydrogen into the semiconductor layer 230 can be suppressed. In addition, the diffusion of oxygen toward the conductive layer 260 side can be prevented and oxidation of the conductive layer 260 can be suppressed. Therefore, a highly reliable transistor can be realized. If the insulating layer 250 has a three-layer structure, for example, a silicon oxide film can be used as the first insulating layer, a hafnium oxide film or a hafnium silicate film can be used as the second insulating layer, and a silicon nitride film can be used as the third insulating layer.
[0214] Alternatively, the insulating layer 250 can have a four-layer structure comprising a first insulating layer, a second insulating layer, a third insulating layer, and a fourth insulating layer. In this case, the first insulating layer is in contact with the semiconductor layer 230, and the first insulating layer, the second insulating layer, the third insulating layer, and the fourth insulating layer are arranged in the order of first insulating layer, second insulating layer, third insulating layer, and fourth insulating layer, from the semiconductor layer 230 side toward the conductive layer 260 which functions as the gate electrode side. The first insulating layer can be made of an insulating material having barrier properties against oxygen, or an insulating material having the function of suppressing the permeation of impurities such as hydrogen and oxygen; the second insulating layer can be made of an insulating material with high dielectric strength or an insulating material that suppresses leakage current; the third insulating layer can be made of an insulating material having the function of capturing or fixing hydrogen; and the fourth insulating layer can be made of an insulating material having barrier properties against hydrogen, or an insulating material having the function of suppressing the permeation of impurities such as hydrogen and oxygen. With such a configuration, the detachment of oxygen from the semiconductor layer 230 can be suppressed. Furthermore, gate leakage current can be reduced and hydrogen diffusion into the semiconductor layer 230 can be suppressed. In addition, oxygen diffusion to the conductive layer 260 can be prevented and oxidation of the conductive layer 260 can be suppressed. Therefore, a highly reliable transistor can be realized. When the insulating layer 250 has a four-layer structure, for example, an aluminum oxide film can be used as the first insulating layer, a silicon oxide film as the second insulating layer, a hafnium oxide film or hafnium silicate film as the third insulating layer, and a silicon nitride film as the fourth insulating layer.
[0215] The gate insulating layer, such as the insulating layer 250, is preferably a thin film. For example, by setting the thickness of the insulating layer 250 to 1 nm to 50 nm, 1 nm to 20 nm, and preferably 3 nm to 10 nm, the subthreshold swing value (also called the S value), which is one of the transistor characteristics, can be reduced. The S value refers to the amount of change in gate voltage when the drain current is changed by one order of magnitude while the drain voltage is constant in the subthreshold region. It is preferable that the insulating layer 250 has at least a portion of the above-mentioned thickness.
[0216] Furthermore, the film thickness of each layer constituting the insulating layer, such as the insulating layer 250, is preferably 0.1 nm to 40 nm, more preferably 0.1 nm to 10 nm, more preferably 0.1 nm to 5 nm, more preferably 0.5 nm to 5 nm, more preferably 1 nm to less than 5 nm, and even more preferably 1 nm to 3 nm. It is preferable that each layer constituting the insulating layer 250 has at least a portion of the above-mentioned film thickness region.
[0217] As a specific example of the insulating layer 250, it is preferable to use a four-layer structure in which an aluminum oxide film, a silicon oxide film, a hafnium oxide film, and a silicon nitride film are stacked in that order from the semiconductor layer 230 side, with the thicknesses of these layers being 1 nm, 2 nm, 2 nm, and 1 nm from the semiconductor layer 230 side. Alternatively, it is preferable to have the thicknesses of these layers being 1 nm, 30 nm, 1.5 nm, and 1 nm from the semiconductor layer 230 side. Alternatively, it is preferable to have the thicknesses of these layers being 1 nm, 30 nm, 1.5 nm, and 5 nm from the semiconductor layer 230 side.
[0218] Another specific example is a four-layer structure in which a hafnium oxide film, a silicon oxide film, a hafnium oxide film, and a silicon nitride film are stacked in that order from the semiconductor layer 230 side, and it is preferable that the thicknesses of these layers be 1 nm, 2 nm, 2 nm, and 1 nm from the semiconductor layer 230 side.
[0219] Another specific example is a two-layer structure in which a silicon oxide film and a hafnium oxide film are stacked in that order from the semiconductor layer 230 side, and it is preferable that the thicknesses of these layers be 1 nm and 1.5 nm from the semiconductor layer 230 side.
[0220] Furthermore, as a specific example, it is preferable to use a three-layer structure in which a silicon oxide film, a hafnium oxide film, and a silicon nitride film are stacked in that order from the semiconductor layer 230 side, with the thicknesses of these layers being 30 nm, 1.5 nm, and 5 nm from the semiconductor layer 230 side.
[0221] <Example of Semiconductor Device Manufacturing Method> Below, an example of a method for manufacturing a semiconductor device according to one embodiment of the present invention will be described. In the drawings illustrating this example of a semiconductor device manufacturing method, A in each figure shows a plan view. B in each figure is a cross-sectional view between the dashed lines A1 and A2 shown in A of each figure. C in each figure is a cross-sectional view between the dashed lines B1 and B2 shown in A of each figure. Furthermore, D in each figure is a cross-sectional view between the dashed lines B3 and B4 shown in A of each figure.
[0222] In the following, insulating materials for forming an insulating layer, conductive materials for forming a conductive layer, or semiconductor materials for forming a semiconductor layer can be deposited using sputtering, chemical vapor deposition (CVD), molecular beam epitaxy (MBE), pulsed laser deposition (PLD), ALD, etc., as appropriate.
[0223] Sputtering methods include RF sputtering, which uses a high-frequency power supply for sputtering; DC (Direct Current) sputtering, which uses a DC power supply; and pulsed DC sputtering, which changes the voltage applied to the electrodes in pulses. For film deposition using insulating targets, RF (Radio Frequency) sputtering is preferable. DC sputtering is mainly used when depositing films using conductive targets. In addition to forming conductive films, DC sputtering can also form insulating films using reactive sputtering with pulsed DC sputtering. Specifically, pulsed DC sputtering can be used when depositing compounds such as oxides, nitrides, and carbides using reactive sputtering.
[0224] Furthermore, CVD methods can be classified into plasma-enhanced CVD (PECVD), which utilizes plasma; thermal CVD (TCD), which utilizes heat; and photo-CVD (Photo CVD), which utilizes light. They can also be further divided into metal CVD (MCCVD) and metal-organic vapor deposition (MOCVD) depending on the source gas used.
[0225] Plasma CVD allows for the production of high-quality films at relatively low temperatures. Thermal CVD, on the other hand, does not use plasma, thus minimizing plasma damage to the workpiece. For example, wiring, electrodes, and elements (transistors, capacitive elements, etc.) in semiconductor devices can be charged up by receiving charge from the plasma. This accumulated charge can damage the wiring, electrodes, and elements in the semiconductor device. In contrast, thermal CVD, which does not use plasma, avoids this plasma damage, resulting in a higher yield for semiconductor devices. Furthermore, thermal CVD produces films with fewer defects because it avoids plasma damage during deposition.
[0226] Furthermore, as ALD methods, thermal ALD, which carries out the reaction of the precursor and reactant using only thermal energy, and plasma ALD (PEALD: Plasma Enhanced ALD), which uses a plasma-excited reactant, can be used.
[0227] CVD and ALD methods differ from sputtering, where particles emitted from a target or other source are deposited. Therefore, they are less affected by the shape of the workpiece and are film deposition methods that provide good step-level coverage. In particular, the ALD method has excellent step-level coverage and excellent thickness uniformity, making it suitable for coating the surface of openings with high aspect ratios. However, since the ALD method has a relatively slow deposition rate, it is sometimes preferable to use it in combination with other film deposition methods such as the CVD method, which has a faster deposition rate.
[0228] Furthermore, the CVD method allows for the deposition of films with any desired composition by changing the flow rate ratio of the source gases. For example, in the CVD method, by changing the flow rate ratio of the source gases while deposition is occurring, films with continuously changing compositions can be deposited. When deposition is performed while changing the flow rate ratio of the source gases, the time required for deposition can be shortened compared to deposition using multiple deposition chambers, because time spent on transport or pressure adjustment is eliminated. Therefore, it may be possible to increase the productivity of semiconductor devices.
[0229] [Example of Manufacturing Method 1] Below, we will describe an example of a manufacturing method for the semiconductor device shown in Figures 3A to 4B, that is, an example of a manufacturing method for a semiconductor device having a transistor 200.
[0230] First, a substrate (not shown) is prepared, and an insulating layer 215 is deposited on the substrate (see Figures 13A to 13D). For example, sputtering, CVD, MBE, PLD, or ALD can be used to deposit the insulating layer 215. Using a sputtering method, which does not require the use of hydrogen-containing molecules in the deposition gas, is preferable because it allows for a reduction in the hydrogen concentration in the insulating layer 215.
[0231] Next, an insulating layer 216 is formed on the insulating layer 215. The insulating layer 216 is preferably formed using a sputtering method. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 216 can be reduced. However, the deposition of the insulating layer 216 is not limited to the sputtering method; CVD, MBE, PLD, ALD, etc., may be used as appropriate. In this embodiment, silicon oxide is deposited as the insulating layer 216 using the sputtering method.
[0232] It is preferable to continuously deposit the insulating layer 215 and the insulating layer 216 without exposure to the atmosphere. For example, it is preferable to use a multi-chamber type deposition apparatus. This allows for the deposition of the insulating layer 215 and the insulating layer 216 with reduced hydrogen content in the film, and further reduces the incorporation of hydrogen into the film between each deposition process.
[0233] Next, an insulating layer 221 is formed on the insulating layer 216 (see Figures 13A to 13D).
[0234] It is preferable to form an insulating layer 221 that has barrier properties against oxygen, hydrogen, and water as described above. The insulating layer 221 can be formed using, for example, sputtering, CVD, MBE, PLD, or ALD. In this embodiment, silicon nitride is formed as the insulating layer 221 using the PEALD method.
[0235] Next, an insulating layer 222 is formed on the insulating layer 221 (see Figures 13A to 13D).
[0236] As the insulating layer 222, an insulating film containing an oxide of one or both aluminum and hafnium is preferably formed. It is preferable to use, for example, aluminum oxide, hafnium oxide, or an oxide containing aluminum and hafnium (hafnium aluminate) as the insulating film containing an oxide of one or both aluminum and hafnium. Alternatively, it is preferable to use hafnium zirconium oxide. The insulating film containing an oxide of one or both aluminum and hafnium has barrier properties against oxygen, hydrogen, and water. Because the insulating layer 222 has barrier properties against hydrogen and water, the diffusion of hydrogen and water contained in the structure provided around the transistor through the insulating layer 222 to the inside of the transistor is suppressed, thereby suppressing the generation of oxygen vacancies in the semiconductor layer 230.
[0237] The insulating layer 222 can be formed using, for example, sputtering, CVD, MBE, PLD, or ALD. In this embodiment, hafnium oxide is formed as the insulating layer 222 using the thermal ALD method.
[0238] In this embodiment, silicon nitride is deposited as the insulating layer 221 using the PEALD method, and hafnium oxide is deposited as the insulating layer 222 using the thermal ALD method. By using silicon nitride, which has the function of suppressing hydrogen diffusion, for the insulating layer 221, it is possible to suppress the diffusion of hydrogen from the lower layer of the transistor 200. Furthermore, by using hafnium oxide, which has the function of capturing or fixing hydrogen, for the insulating layer 222, hydrogen contained in the semiconductor layer 230 can be captured or fixed to the insulating layer 222. This makes it possible to reduce the hydrogen concentration in and near the semiconductor layer 230.
[0239] Next, an insulating film 224f is deposited on the insulating layer 222 (see Figures 13A to 13D). The insulating film 224f is the insulating film that will become the insulating layer 224 in a later step. Therefore, the insulating film is formed using an insulating material that can be used for the insulating layer 224 described above. The insulating film 224f can be deposited using, for example, sputtering, CVD, MBE, PLD, or ALD. For example, silicon oxide can be deposited as the insulating film 224f using the sputtering method.
[0240] Furthermore, it is preferable to perform a heat treatment after the deposition of the insulating film 224f. By performing a heat treatment, impurities such as water and hydrogen contained in the insulating film 224f can be reduced before the deposition of the semiconductor film 230f which will be deposited later.
[0241] The heat treatment is preferably carried out at a temperature of 250°C to 650°C, preferably 300°C to 500°C, and more preferably 320°C to 450°C. The heat treatment is preferably carried out in a reduced-pressure atmosphere or an inert gas (nitrogen gas or noble gas) atmosphere. Alternatively, an oxygen gas atmosphere or a mixed atmosphere of nitrogen gas and oxygen gas may be used. When performing the treatment in a mixed atmosphere of nitrogen gas and oxygen gas, it is preferable to have an oxygen gas content of about 20%. There are no special limitations on the apparatus used for the heat treatment, and it may be an apparatus that heats the workpiece by heat conduction or thermal radiation from a heating element such as a resistance heating element. For example, an electric furnace or an RTA apparatus such as an LRTA (Lamp Rapid Thermal Anneal) apparatus or a GRTA (Gas Rapid Thermal Anneal) apparatus can be used.
[0242] Furthermore, in order to reduce impurities such as water and hydrogen contained in the insulating film 224f, it is preferable to use silicon oxide deposited by a sputtering method that does not use hydrogen as the deposition gas.
[0243] Next, a semiconductor film 230f is deposited on the insulating film 224f (see Figures 13A to 13D). The semiconductor film 230f is a semiconductor film that will become the semiconductor layer 230 in a later step. Therefore, the semiconductor film 230f can be formed using a material that can be used for the semiconductor layer 230 described above, for example, indium oxide. The semiconductor film 230f can be deposited using sputtering, CVD, MBE, PLD, or ALD. In particular, depositing the semiconductor film 230f using sputtering is preferable because it makes it easier to increase the thickness of the semiconductor layer 230 while maintaining the productivity of the semiconductor device.
[0244] Next, it is preferable to perform a treatment to enhance the crystallinity of the semiconductor film 230f. For example, indium oxide, which has a cubic crystal system, is presumed to grow crystals while maximizing the surface area of the {111} plane at the interface between the crystal and amorphous regions, because the interfacial energy of the {111} plane is smaller than that of other planes. In other words, when indium oxide is used for the semiconductor film 230f, it is presumed that it will preferentially orient towards the {111} plane. Therefore, by performing a treatment to enhance crystallinity, it is possible to form crystal grains (also called <111> oriented crystal grains) on the semiconductor film 230f in which the crystal orientation <111> is oriented parallel to the thickness direction of the insulating film 224f (the direction perpendicular to the surface on which the semiconductor film 230f is formed). Furthermore, when In-Ga-Zn oxide, which has a hexagonal crystal system, and metal oxides having a similar crystal structure are used for the semiconductor film 230f, crystals with a preferential orientation of the {001} plane can be obtained.
[0245] Treatments to enhance crystallinity include, for example, microwave-excited plasma treatment (also simply called microwave plasma treatment), heat treatment, plasma treatment, microwave treatment, and light irradiation treatment. Microwave treatment refers to a treatment using a device equipped with a power supply that generates high-density plasma using microwaves. It is also possible to perform multiple of these treatments simultaneously or sequentially.
[0246] As a treatment to improve the crystallinity of the semiconductor film 230f, it is preferable to use microwave-excited plasma treatment. In particular, it is especially preferable to perform the microwave-excited plasma treatment in an oxygen-containing atmosphere.
[0247] Microwave-excited plasma processing refers to a process that uses equipment equipped with a power supply that generates high-density plasma using microwaves. It can also be called microwave-excited high-density plasma processing.
[0248] In microwave-excited plasma processing, it is preferable to use a plasma processing apparatus that has a power supply for generating high-density plasma using microwaves. Here, the microwave frequency is preferably 300 MHz to 300 GHz, more preferably 2.4 GHz to 2.5 GHz, and can be, for example, 2.45 GHz. By using high-density plasma, high-density oxygen radicals can be generated. Furthermore, the power of the power supply that applies microwaves to the microwave-excited plasma processing apparatus is preferably 1000 W to 10000 W, and preferably 2000 W to 5000 W. The microwave-excited plasma processing apparatus may also have a power supply for applying RF to the substrate side. Furthermore, by applying RF to the substrate side, oxygen ions generated by the high-density plasma can be efficiently guided into the film.
[0249] When performing microwave-excited plasma processing, it is preferable to set the substrate temperature to room temperature (e.g., 25°C) or higher and 1000°C or lower, 100°C or higher and 800°C or lower, 200°C or higher and 650°C or lower, 300°C or higher and 500°C or lower, 400°C or higher and 500°C or lower, or 400°C or higher and 450°C or lower.
[0250] Microwave-excited plasma treatment is preferably carried out under reduced pressure, with a pressure of 10 Pa to 1000 Pa being preferred, more preferably 50 Pa to 700 Pa, and even more preferably 100 Pa to 400 Pa.
[0251] Microwave-excited plasma treatment can be performed, for example, using oxygen gas and argon gas. Here, the oxygen flow rate ratio (O 2 / ( O 2 The value of +Ar) should be greater than 0% and 100% or less. Preferably, it should be greater than 0% and 50% or less. More preferably, it should be between 10% and 40%. Even more preferably, it should be between 10% and 30%. Typically, it should be 25%. When performing processing using oxygen (O) radicals, it is preferable to increase the oxygen flow rate ratio. On the other hand, a high oxygen flow rate ratio may increase the risk of particle generation, or the risk of damage to the processing chamber, or both. For this reason, the oxygen flow rate needs to be set within an appropriate range.
[0252] Furthermore, microwave-excited plasma treatment can be carried out using, for example, hydrogen gas, oxygen gas, and argon gas. Here, the ratio of the hydrogen gas flow rate to the total gas flow rate is defined as the hydrogen flow rate ratio. For example, when using hydrogen gas, oxygen gas, and argon gas, the hydrogen flow rate ratio represents the ratio of the hydrogen gas flow rate to the sum of the hydrogen gas flow rates, oxygen gas flow rates, and argon gas flow rates. For example, the hydrogen flow rate ratio is preferably greater than 0% and 15% or less, more preferably greater than 0% and 10% or less, and even more preferably greater than 0% and 7.5% or less. By setting the hydrogen flow rate ratio within the above range, the number of active species such as OH radicals or OH ions during microwave-excited plasma treatment increases, which may accelerate the reaction. On the other hand, by increasing the amount of hydrogen above the above range, H 2 The proportion of active species decreases due to an increase in inactive species such as O, H 2 Due to the reduction of the semiconductor layer 230, etc., there is a risk that hydrogen in the semiconductor layer 230 may not be sufficiently removed.
[0253] The shorter the processing time for microwave-excited plasma treatment, the higher the productivity. For example, the processing time for microwave-excited plasma treatment is preferably 1 minute or more and 60 minutes or less, more preferably 1 minute or more and 30 minutes or less, and even more preferably 1 minute or more and 10 minutes or less.
[0254] Furthermore, as a treatment to enhance the crystallinity of the semiconductor film 230f, heat treatment is preferred. The heat treatment is preferably carried out in a reduced-pressure atmosphere or an inert gas (nitrogen gas or noble gas) atmosphere. Alternatively, an oxygen gas atmosphere or a mixed atmosphere of nitrogen gas and oxygen gas may be used. When performing the treatment in a mixed atmosphere of nitrogen gas and oxygen gas, it is preferable to have an oxygen gas content of about 20%. There are no special limitations on the apparatus used for the heat treatment, and it may be an apparatus that heats the workpiece by heat conduction or thermal radiation from a heat source such as a resistance heating element. For example, an electric furnace or an RTA apparatus such as an LRTA apparatus or GRTA apparatus can be used.
[0255] Next, a film 233f is deposited on the semiconductor film 230f (see Figures 13A to 13D). Film 233f is the film that will become layer 233 in a later step. Therefore, film 233f can be deposited using a material that can be used for layer 233 as described above, for example, a metallic material such as tungsten. In this case, film 233f can be a conductive film. Film 233f may also be deposited using an insulating material or a semiconductor material. Film 233f can be deposited using sputtering, CVD, MBE, PLD, or ALD.
[0256] Next, the film 233f is processed using lithography to form layer 233. Dry etching or wet etching can be used for this processing. Dry etching is suitable for microfabrication. Layer 233 is used as a hard mask in a later step when the semiconductor film 230f is processed to form the semiconductor layer 230.
[0257] In lithography, the resist is first exposed through a mask. Next, the exposed area is removed or left intact using a developer to form a resist mask. Then, by etching through the resist mask, conductive films, semiconductor films, insulating films, etc., can be processed into the desired shape. For example, a resist mask can be formed by exposing the resist using KrF excimer laser light, ArF excimer laser light, EUV (Extreme Ultraviolet) light, etc. Alternatively, immersion technology may be used, in which a liquid (e.g., water) is filled between the substrate and the projection lens for exposure. In addition, an electron beam or ion beam may be used instead of the aforementioned light. Note that when using an electron beam or ion beam, a mask may not be necessary.
[0258] Furthermore, the resist mask that is no longer needed after processing can be removed by dry etching, such as ashing using oxygen plasma (hereinafter sometimes referred to as oxygen plasma treatment), wet etching, wet etching after dry etching, or dry etching after wet etching.
[0259] Alternatively, a configuration may be used in which an SOC (Spin On Carbon) film and an SOG (Spin On Glass) film are deposited between the workpiece and the resist mask. By using the SOC film and SOG film as masks, the durability of the mask pattern can be improved. For example, lithography can be performed by depositing the SOC film, SOG film, and resist mask in that order on the workpiece.
[0260] For dry etching, an etching gas containing halogens can be used. Specifically, an etching gas containing one or more of fluorine, chlorine, and bromine can be used. For example, as an etching gas, C 4 F 6 Gas, C 5 F 6 Gas, C 4 F 8 Gas, CF 4 Gas, SF 6 Gas, CHF 3 Gas, CH 2 F 2 Gas, Cl 2 Gas, BCl 3 Gas, SiCl 4 Gas, or BBr 3 Gases can be used individually or in mixtures of two or more gases. Furthermore, oxygen, carbon dioxide, nitrogen, helium, argon, hydrogen, or hydrocarbon gases can be appropriately added to the etching gas. Depending on the material being treated in the dry etching process, a gas containing hydrocarbons or hydrogen, but without halogen gases, can be used as the etching gas. Examples of hydrocarbons used in etching gases include methane (CH4). 4 ), ethane (C 2 H 6 ), propane (C 3 H 8 ), butane (C 4 H 10 ), ethylene (C 2 H 4 ), propylene (C 3 H 6 ), acetylene (C 2 H2 ), and propine (C 3 H 4 One or more of the following can be used. The etching conditions can be set as appropriate according to the object to be etched.
[0261] As a dry etching apparatus, a capacitively coupled plasma (CCP) etching apparatus having parallel plate electrodes can be used. The capacitively coupled plasma etching apparatus having parallel plate electrodes may be configured to apply a high-frequency voltage to one electrode of the parallel plate electrodes, or to apply a high-frequency voltage of the same frequency to each of the parallel plate electrodes, or to apply multiple different high-frequency voltages to the parallel plate electrodes. Such a CCP etching apparatus is called a dual-frequency excited capacitively coupled plasma (DF-CCP) etching apparatus. In a DF-CCP etching apparatus, it is possible to configure it to apply high-frequency voltages of different frequencies to each of the parallel plate electrodes, or to apply multiple different high-frequency voltages to one of the parallel plate electrodes. Alternatively, a dry etching apparatus having a high-density plasma source can be used. For example, an inductively coupled plasma (ICP) etching apparatus can be used as a dry etching apparatus having a high-density plasma source. The etching apparatus can be appropriately configured according to the object to be etched. In addition, reactive ion etching can be performed by applying a high-frequency voltage to the electrode on the substrate side of the dry etching apparatus to generate a self-bias potential. In reactive ion etching, etching is performed by accelerating ion species in the plasma and causing them to collide with the workpiece, thus enabling highly anisotropic etching.
[0262] Next, using layer 233 as a mask, the semiconductor film 230f and insulating film 224f are processed into island-like structures to form the semiconductor layer 230 and the insulating layer 224 (see Figures 14A to 14D). Dry etching or wet etching can be used for this processing. Dry etching is suitable for microfabrication.
[0263] Figure 14C shows the taper angle of the semiconductor layer 230, specifically the angle between the side surface of the semiconductor layer 230 and the upper surface of the insulating layer 224, as angle θ. It is preferable to process the semiconductor film 230f so that angle θ is 65° or more and less than 90°, preferably 65° or more and 85° or less, and more preferably 70° or more and 80° or less.
[0264] As described above, by processing the insulating film 224f into an island shape, the lower surface of the conductive layer 260 to be formed later in the transistor 200 can be positioned below the lower surface of the semiconductor layer 230. This allows a sufficient electric field to be applied from the conductive layer 260 to the entire semiconductor layer 230. Therefore, the electrical characteristics of the transistor 200 can be improved.
[0265] Next, layer 233 is removed (see Figures 15A to 15D). There are no particular limitations on the method for removing layer 233, but a wet etching method can be suitably used. By using a wet etching method, etching of the semiconductor layer 230 and the insulating layer 222 can be suppressed when removing layer 233. This prevents the thickness of the semiconductor layer 230 and the insulating layer 222 from becoming thinner. Therefore, the thickness of the semiconductor layer 230 and the insulating layer 222 can be made uniform.
[0266] Next, a conductive layer 242 is formed to cover the semiconductor layer 230 and the insulating layer 224 (see Figures 16A to 16D). The conductive layer 242 is a conductive layer that will become conductive layer 242a and conductive layer 242b in a later step. Figures 16B, 16C, and 16D show an example in which the conductive layer 242 has a laminated structure of conductive layer 242_1 and conductive layer 242_2 on conductive layer 242_1. In this case, conductive layer 242_1 is a conductive layer that will become conductive layer 242a1 and conductive layer 242b1 in a later step. Also, conductive layer 242_2 is a conductive layer that will become conductive layer 242a2 and conductive layer 242b2 in a later step.
[0267] The conductive layer 242 can be formed by depositing a conductive film that will become the conductive layer 242 and then processing the conductive film by lithography. In the examples shown in Figures 16B to 16D, the conductive layer 242_1 is deposited, then the conductive layer 242_2 is deposited, and then these conductive films are processed by lithography. Dry etching or wet etching can be used for this processing. Dry etching is suitable for microfabrication.
[0268] The conductive film that will become conductive layer 242_1 and the conductive film that will become conductive layer 242_2 can be deposited using, for example, sputtering, CVD, MBE, PLD, or ALD. For example, ITO can be deposited as the conductive film that will become conductive layer 242_1 using sputtering. Also, for example, tungsten can be deposited as the conductive film that will become conductive layer 242_2 using sputtering.
[0269] Next, an insulating layer 275 is formed covering the insulating layer 224, the semiconductor layer 230, and the conductive layer 242, and then an insulating layer 280 is formed on top of the insulating layer 275 (see Figures 17A to 17D).
[0270] It is preferable to perform CMP treatment on the insulating layer 280 after it has been formed. This makes it possible to flatten the upper surface of the insulating layer 280. Alternatively, silicon nitride may be formed on the insulating layer 280 by, for example, sputtering, and then CMP treatment may be performed on the silicon nitride until it reaches the insulating layer 280.
[0271] The insulating layer 275 and the insulating layer 280 can be formed using, for example, sputtering, CVD, MBE, PLD, or ALD.
[0272] It is preferable to use an insulating material that has the function of suppressing oxygen permeation for the insulating layer 275. For example, it is preferable to deposit silicon nitride as the insulating layer 275 using the PEALD method. Alternatively, it is preferable to deposit aluminum oxide as the insulating layer 275 using the sputtering method, and then deposit silicon nitride on top of it using the PEALD method. By making the insulating layer 275 as described above, it is possible to improve the function of suppressing the diffusion of impurities such as water and hydrogen, and oxygen.
[0273] In this way, the conductive layer 242 can be covered with an insulating layer 275 that has the function of suppressing the diffusion of oxygen. This makes it possible to suppress the direct diffusion of oxygen from the insulating layer 280, etc., to the semiconductor layer 230 and the conductive layer 242 in subsequent processes.
[0274] Furthermore, it is preferable to deposit silicon oxide as the insulating layer 280 using a sputtering method. By depositing the insulating film that will become the insulating layer 280 using a sputtering method in an oxygen-containing atmosphere, an insulating layer 280 containing excess oxygen can be formed. In addition, by using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 280 can be reduced. Before depositing the insulating film, a heat treatment may be performed. The heat treatment may be performed under reduced pressure, and the insulating film may be deposited continuously without exposure to the atmosphere. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the insulating layer 275 can be removed, and the moisture concentration and hydrogen concentration in the semiconductor layer 230 can be further reduced. The heat treatment conditions described above can be used for this heat treatment.
[0275] Next, the insulating layer 280, insulating layer 275, conductive layer 242_2, and conductive layer 242_1 are processed using lithography. This creates an opening 201 in the insulating layer 280 and insulating layer 275 that overlaps with the semiconductor layer 230. The conductive layer 242_2 is divided to form conductive layers 242a2 and 242b2, and the conductive layer 242_1 is divided to form conductive layers 242a1 and 242b1. This creates conductive layers 242a and 242b (see Figures 18A to 18D). The formation of the opening 201, conductive layers 242a and 242b exposes a portion of the upper surface of the semiconductor layer 230, a portion of the side surface of the semiconductor layer 230, a portion of the side surface of the insulating layer 224, and a portion of the upper surface of the insulating layer 222.
[0276] The above processing is preferably carried out using a dry etching method. Dry etching allows for anisotropic etching. Therefore, it is suitable for forming an opening 201 with a high aspect ratio.
[0277] Furthermore, an ashing treatment using oxygen plasma may be performed after processing the conductive layer 242. By performing such oxygen plasma treatment, impurities generated during the etching process and diffused into the semiconductor layer 230 can be removed. These impurities may be caused by components contained in the workpiece subjected to the etching process, or by components contained in the gas used for etching. Examples include chlorine, fluorine, tantalum, silicon, and hafnium. By removing these impurities attached to the semiconductor layer 230, the electrical characteristics and reliability of the transistor can be improved.
[0278] Furthermore, a cleaning process may be performed to remove impurities and other contaminants adhering to the surface of the semiconductor layer 230 during the etching process described above. Cleaning methods include wet cleaning using a cleaning solution (which can also be called wet etching), plasma treatment using plasma, and cleaning by heat treatment, and these cleaning methods may be combined as appropriate. Note that the grooves may become deeper as a result of this cleaning process.
[0279] For wet cleaning, an aqueous solution may be used in which one or more of oxalic acid, phosphoric acid, and hydrofluoric acid are diluted with carbonated water or distilled water. Alternatively, wet cleaning may be used in which ammonia water is diluted with carbonated water or distilled water. Alternatively, wet cleaning may be used with distilled water or carbonated water, etc. Alternatively, ultrasonic cleaning may be performed using these aqueous solutions, distilled water, or carbonated water. Alternatively, these cleaning methods may be combined as appropriate. Furthermore, the above cleaning process may be performed multiple times, and the cleaning solution may be changed each time the cleaning process is performed.
[0280] It is preferable to perform a heat treatment after etching or cleaning as described above. The temperature of the heat treatment should be between 100°C and 650°C, preferably between 250°C and 600°C, more preferably between 300°C and 550°C, and even more preferably between 350°C and 400°C. The heat treatment should be performed in an atmosphere of an inert gas (nitrogen gas or noble gas) or an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. It is preferable to perform the heat treatment in an atmosphere containing oxygen; for example, it is preferable to perform the treatment at a temperature of 350°C for 1 hour with a flow rate ratio of nitrogen gas to oxygen gas of 4:1. This allows oxygen to be supplied to the semiconductor layer 230, thereby reducing oxygen deficiency. Furthermore, by performing such a heat treatment, the crystallinity of the semiconductor layer 230 can be improved. In addition, the supplied oxygen reacts with the hydrogen remaining in the semiconductor layer 230, thereby converting the hydrogen into H 2 It can be removed as O (dehydrated). As a result, the hydrogen remaining in the semiconductor layer 230 recombines with the oxygen vacancy and V O The formation of H can be suppressed. Therefore, the electrical characteristics of the transistor provided with the semiconductor layer 230 can be improved, and its reliability can be enhanced. In addition, variations in the electrical characteristics of multiple transistors formed on the same substrate can be suppressed. The above heat treatment may be performed under reduced pressure. Alternatively, the heat treatment may be performed in an oxygen atmosphere, and then continuously in a nitrogen atmosphere without exposure to the atmosphere. Furthermore, the above heat treatment can also serve as the heat treatment for the semiconductor film 230f. Therefore, the crystalline region of the semiconductor layer 230 may grow as a result of the above heat treatment.
[0281] Furthermore, when heat treatment is performed with the semiconductor layer 230 in contact with the conductive layer 242a and the conductive layer 242b, the sheet resistance may decrease in the regions of the semiconductor layer 230 that overlap with the conductive layer 242a and the regions that overlap with the conductive layer 242b, respectively. Also, the carrier concentration may increase. Therefore, the resistance of the regions of the semiconductor layer 230 that overlap with the conductive layer 242a and the regions that overlap with the conductive layer 242b can be reduced.
[0282] Furthermore, processing of the conductive layer 242_1 as described above, or subsequent cleaning treatment, may cause a portion of the upper surface of the semiconductor layer 230 to be removed in the region overlapping with the opening 201. As a result, as shown in Figure 18B, the upper surface of the semiconductor layer 230 in the region overlapping with the opening 201 may be lower than the upper surface of the semiconductor layer 230 in the region overlapping with the conductive layer 242a and the upper surface of the semiconductor layer 230 in the region overlapping with the conductive layer 242b. In other words, a recess may be formed in the region of the semiconductor layer 230 that overlaps with the opening 201. Also, if such a recess is formed in the semiconductor layer 230, a portion of the side surface of the semiconductor layer 230 may be removed in the region overlapping with the opening 201. As a result, the width of the lower surface of the semiconductor layer 230 in the region overlapping with the opening 201 may be smaller than the width of the lower surface of the semiconductor layer 230 in the region that does not overlap with the opening 201. For example, the length of the lower surface of the semiconductor layer 230 in the cross-section shown in Figure 18C may be shorter than the length of the lower surface of the semiconductor layer 230 in the cross-section shown in Figure 18D.
[0283] When indium oxide is used as the semiconductor layer 230, an element that can form a trivalent cation may be added after the formation of the opening 201, the conductive layer 242a, and the conductive layer 242b. This element can be added to the surface of the semiconductor layer 230 and its vicinity in the region overlapping with the opening 201. This makes it possible to suppress the formation of oxygen vacancies in the semiconductor layer 230 while maintaining the carrier concentration of the semiconductor layer 230. Gallium is an example of an element that can form a trivalent cation.
[0284] Furthermore, by adding elements that can form divalent or less cations to the semiconductor layer 230, the added atoms substitute for indium atoms, resulting in a deficiency of one or more electrons. This creates a negative charge in the semiconductor layer 230. Alternatively, the carrier concentration in the semiconductor layer 230 can be reduced. Therefore, the threshold voltage of the transistor 200 can be shifted to the positive side. Also, normally-off operation becomes possible. Examples of elements that can form divalent or less cations include zinc and copper. Silicon can also exist as a divalent cation. Hereafter, divalent silicon will be referred to as Si(II).
[0285] As described above, by adding elements that can form trivalent or less cations to the semiconductor layer 230, specifically to the channel formation region of the transistor 200, a transistor with good electrical properties can be provided.
[0286] The presence or absence of divalent silicon oxide (also written as Si=O) or Si(II) in a metal oxide layer can be evaluated by the valence of the silicon atoms or the number of oxygen atoms bonded to the silicon atoms (also called the coordination number of oxygen atoms in silicon atoms). The coordination number of silicon atoms can be evaluated by the chemical bonding state between atoms. The valence of atoms or the chemical bonding state between atoms can be evaluated, for example, using X-ray photoelectron spectroscopy (XPS).
[0287] For example, in the semiconductor layer 230, if the ratio of divalent silicon to silicon is 0.001 or more and 1 or less, then the semiconductor layer 230 can be said to contain Si(II).
[0288] Furthermore, silicon atoms in silicon oxide are bonded to four oxygen atoms. In other words, the coordination number of oxygen atoms in silicon atoms is 4. On the other hand, since Si=O also constitutes part or all of InOx, if semiconductor layer 230 has Si=O, the coordination number of oxygen atoms in silicon atoms in semiconductor layer 230 is not limited to 4, but can be 5 or 6. Therefore, if silicon atoms with an oxygen coordination number of 5 or 6 are detected in semiconductor layer 230, it can be said that semiconductor layer 230 has Si=O.
[0289] The addition of Si(II) to the surface and vicinity of the semiconductor layer 230 can be carried out, for example, using the ALD method or the MBE method. For example, a thin layer (e.g., one atomic layer) in which Si(II) is localized is introduced into the semiconductor layer 230 using the ALD method or the MBE method. By using the ALD method or the MBE method, the diffusion of Si(II) into the interior of the semiconductor layer 230 can be suppressed. Here, by adding Si(II) to the semiconductor layer 230, Si=O can be formed in the semiconductor layer 230. Specifically, Si=O can be formed on the surface and vicinity of the semiconductor layer 230. Note that Si(II) may also be present on the surface and vicinity of the semiconductor layer 230.
[0290] Next, an insulating layer 250 and a conductive layer 260 on the insulating layer 250 are formed inside the opening 201 (see Figures 19A to 19D). The insulating layer 250 is formed to cover the top and side surfaces of the exposed semiconductor layer 230 and the side surfaces of the insulating layer 224. For example, an insulating film to become the insulating layer 250 and a conductive film to become the conductive layer 260 are formed, and the conductive film and the insulating film are polished by CMP treatment until the insulating layer 280 is exposed, thereby forming the insulating layer 250 and the conductive layer 260.
[0291] The insulating film that will become the insulating layer 250 can be deposited using sputtering, CVD, MBE, PLD, or ALD. For example, it is preferable to deposit the insulating film that will become the insulating layer 250 using the ALD method. Similar to the insulating layer 250 described above, it is preferable to form the insulating film that will become the insulating layer 250 with a thin film thickness, and it is necessary to minimize variations in film thickness. In contrast, the ALD method is a film deposition method that alternately introduces a precursor and a reactant (e.g., an oxidizing agent), and the film thickness can be adjusted by the number of times this cycle is repeated, thus enabling precise film thickness adjustment. Furthermore, the insulating film that will become the insulating layer 250 needs to be deposited with good coverage on the bottom and sides of the opening. By using the ALD method, layers of atoms can be deposited one by one on the bottom and sides of the opening, so that the insulating film that will become the insulating layer 250 can be formed with good coverage on the opening.
[0292] Furthermore, when forming the insulating film that will become the insulating layer 250 using the ALD method, ozone (O) is used as the oxidizing agent. 3 ), oxygen (O 2 ), water (H 2 O) etc. can be used. Hydrogen-free ozone (O) 3 ), oxygen (O 2 By using oxidizing agents such as ), the amount of hydrogen diffusing into the semiconductor layer 230 can be reduced.
[0293] The conductive film that will become the conductive layer 260 is formed to fill the openings 201 formed in the insulating layer 280 or the like. The conductive film that will become the conductive layer 260 can be formed using, for example, sputtering, CVD, MBE, PLD, plating, or ALD. For example, as shown in Figures 19B and 19C, when the conductive layer 260 has a laminated structure of conductive layer 260_1 and conductive layer 260_2, titanium nitride can be formed as the conductive film that will become conductive layer 260_1 using the ALD method. Furthermore, tungsten can be formed as the conductive film that will become conductive layer 260_2 using the CVD method.
[0294] The conductive film that will become the conductive layer 260_1 can be deposited by thermal ALD using an inorganic precursor, without using a hydrogen-containing gas. For example, TiCl 4 In this case, NH can be used as the nitride agent. 3 A gas can be used. By forming the film using the method described above, the conductive layer 260_1 can be made into a conductive film with a low hydrogen concentration as described above. Therefore, these conductive films can act as a hydrogen source, preventing hydrogen from diffusing into the semiconductor layer 230.
[0295] Here, the conductive layer 260_1 overlaps with the semiconductor layer 230 via a thin insulating layer 250, and is close to the channel formation region of the semiconductor layer 230. Therefore, if a hydrogen-containing treatment is performed during the film formation process of the conductive layer 260_1, hydrogen will easily diffuse into the channel formation region of the semiconductor layer 230. For this reason, as described above, it is preferable to make the conductive layer 260_1 a conductive film with a low hydrogen concentration.
[0296] As described above, the insulating layer 250 is formed inside the opening 201 so as to have a region in contact with the upper surface of the semiconductor layer 230, a region in contact with the side surface of the semiconductor layer 230, a region in contact with the side surface of the insulating layer 224, and a region in contact with the upper surface of the insulating layer 222. The conductive layer 260 is formed on the insulating layer 250 so as to fill the opening 201. As described above, the transistor 200 is formed.
[0297] Next, an insulating layer 282 is formed on the insulating layer 250, the conductive layer 260, and the insulating layer 280 (see Figures 20A to 20B). The insulating layer 282 can be formed using, for example, sputtering, CVD, MBE, PLD, or ALD. It is preferable to form the insulating layer 282 using sputtering. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 282 can be reduced.
[0298] Here, by using the sputtering method to deposit the insulating layer 282 in an oxygen-containing atmosphere, oxygen can be added to the insulating layer 280 while the film is being deposited. This allows the insulating layer 280 to contain excess oxygen. At this time, it is preferable to deposit the insulating layer 282 while heating the substrate.
[0299] Furthermore, the insulating layer 282 can also be made into a laminated structure. In this case, it is preferable to make the lower layer a thin aluminum oxide film deposited by the ALD method and the upper layer a thick aluminum oxide film deposited by the sputtering method. By depositing an aluminum oxide film on top of the thin aluminum oxide film using the sputtering method in this way, the amount of oxygen injected into the insulating layer 280 can be controlled. This makes it possible to supply a sufficient amount of oxygen to the semiconductor layer 230 and prevent an excessive amount of oxygen from being supplied to the semiconductor layer 230.
[0300] Next, an insulating layer 283 is formed on the insulating layer 282. The insulating layer 283 can be formed using sputtering, CVD, MBE, PLD, or ALD. It is preferable to form the insulating layer 283 using sputtering. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 283 can be reduced. In this embodiment, silicon nitride is formed as the insulating layer 283 using sputtering.
[0301] In this embodiment, silicon nitride is deposited as the insulating layer 283, and aluminum oxide is deposited as the insulating layer 282. By using silicon nitride, which has the function of suppressing hydrogen diffusion, for the insulating layer 283, the diffusion of hydrogen from the upper layer of the transistor 200 to the semiconductor layer 230 can be suppressed. Furthermore, by using aluminum oxide, which has the function of capturing or fixing hydrogen, for the insulating layer 282, hydrogen contained in the insulating layer 280 and the like can be captured or fixed to the insulating layer 282. As a result, the hydrogen concentration in and near the semiconductor layer 230 can be reduced.
[0302] Next, an insulating layer 285 is formed on the insulating layer 283 (see Figures 20A to 20D). The insulating layer 285 can be formed using sputtering, CVD, MBE, PLD, or ALD. It is preferable to form the insulating layer 285 using sputtering. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 285 can be reduced. In this embodiment, silicon oxide is formed as the insulating layer 285 using sputtering.
[0303] Here, it is preferable to deposit insulating layers 282, 283, and 285 continuously by sputtering without exposing them to the atmospheric environment. By depositing the films without exposing them to the atmosphere, it is possible to prevent impurities or moisture from the atmospheric environment from adhering to insulating layers 282, 283, and 285, and to keep the interface or vicinity of the interface between insulating layer 282 and insulating layer 283, and the interface or vicinity of the interface between insulating layer 283 and insulating layer 285 clean.
[0304] Next, insulating layers 285, 283, 282, 280, and 275 are processed using lithography to form openings 203a and 203b, respectively (see Figures 20A to 20D). Opening 203a is formed to have a region that overlaps with conductive layer 242a. Opening 203b is formed to have a region that overlaps with conductive layer 242b. The formation of opening 203a exposes at least a portion of the upper surface of conductive layer 242a and at least a portion of the surface along the side of semiconductor layer 230. The formation of opening 203b exposes at least a portion of the upper surface of conductive layer 242b and at least a portion of the surface along the side of semiconductor layer 230.
[0305] The above processing is preferably carried out using a dry etching method. Dry etching allows for anisotropic etching. Therefore, it is suitable for forming openings 203a and 203b with high aspect ratios.
[0306] After the formation of the above-mentioned openings, a heat treatment may be performed. The temperature of the heat treatment can be 100°C to 600°C, preferably 250°C to 550°C, and more preferably 350°C to 450°C. It is preferable to perform the heat treatment in an inert gas atmosphere (nitrogen gas or noble gas). Furthermore, since the heat treatment is performed with the conductive layers 242a and 242b exposed, it is preferable to perform it in an atmosphere that does not contain oxidizing gases or oxygen gas. For example, it is preferable to perform the heat treatment in a nitrogen gas atmosphere at a temperature of 400°C for 1 hour. The above heat treatment may also be performed under reduced pressure. Through the above heat treatment, oxygen contained in the insulating layer 280 can be supplied to the semiconductor layer 230 via the insulating layer 250. This reduces oxygen vacancies in the channel formation region of the semiconductor layer 230.
[0307] Here, since the side surface of the insulating layer 280 is exposed at the opening, the amount of oxygen contained in the insulating layer 280 can be controlled by the heat treatment by diffusing the oxygen contained in the insulating layer 280 outward. On the other hand, since insulating layers 282 and 283, which have barrier properties against oxygen, are provided on the insulating layer 280, oxygen does not diffuse outward from the upper surface of the insulating layer 280. This prevents excessive oxygen from diffusing outward from the insulating layer 280 and prevents the formation of oxygen vacancies in the insulating layer 280. In addition, the conductive layer 242a and conductive layer 242b are covered by the insulating layer 275. This prevents an excessive amount of oxygen from directly diffusing from the insulating layer 280 to the semiconductor layer 230, conductive layer 242a, and conductive layer 242b during the heat treatment.
[0308] In this way, the amount of oxygen in the insulating layer 280 can be more favorably adjusted, and a suitable amount of oxygen can be supplied to the semiconductor layer 230. This reduces oxygen deficiency in the semiconductor layer 230 and prevents an excessive amount of oxygen from being supplied to the semiconductor layer 230. Therefore, the electrical characteristics and reliability of the transistor 200 can be improved. In addition, since the step of exposing the side surface of the insulating layer 280 can be combined with the step of forming the openings 203a and 203b, the manufacturing process of the semiconductor device can be simplified.
[0309] Next, insulating films that will form insulating layers 241a and 241b are deposited, and these insulating films are anisotropically etched. This forms insulating layer 241a inside opening 203a and insulating layer 241b inside opening 203b (see Figures 21A to 21D). The insulating films that will form insulating layers 241a and 241b can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. It is preferable to use insulating films that have the function of suppressing oxygen permeability as insulating films that will form insulating layers 241a and 241b. For example, it is preferable to deposit silicon nitride using the PEALD method. Silicon nitride is preferred because it has high barrier properties against hydrogen.
[0310] Furthermore, it is preferable to use a dry etching method, for example, for the anisotropic etching of the insulating film that will form the insulating layer 241a and the insulating layer 241b. By forming the insulating layer 241a along the side wall of the opening 203a, the permeation of oxygen from the outside can be suppressed, and the oxidation of the conductive layer 240a to be formed next can be suppressed. In addition, the diffusion of impurities such as water and hydrogen contained in the insulating layer 280, etc., into the conductive layer 240a can be suppressed. Similarly, by forming the insulating layer 241b along the side wall of the opening 203b, the oxidation of the conductive layer 240b to be formed next can be suppressed, and the diffusion of impurities contained in the insulating layer 280, etc., into the conductive layer 240b can be suppressed. Note that, as a result of this anisotropic etching, recesses may be formed on a part of the upper surface of the conductive layer 242a and a part of the upper surface of the conductive layer 242b.
[0311] Next, conductive films that will become conductive layers 240a and 240b are formed. It is desirable that the conductive films that will become conductive layers 240a and 240b have a laminated structure that includes a conductive material that has the function of suppressing the permeation of impurities such as water and hydrogen. For example, as shown in Figures 21B and 21D, when conductive layer 240a has a laminated structure of conductive layer 240a1 and conductive layer 240a2, and conductive layer 240b has a laminated structure of conductive layer 240b1 and conductive layer 240b2, tantalum nitride, titanium nitride, etc. can be formed as conductive films that will become conductive layers 240a1 and 240b1. Also, tungsten, molybdenum, copper, etc. can be formed as conductive films that will become conductive layers 240a2 and 240b2.
[0312] The conductive films that will become conductive layers 240a and 240b can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. For example, it is preferable to deposit the conductive films that will become conductive layers 240a1 and 240b1 using the ALD method. It is also preferable to deposit the conductive films that will become conductive layers 240a2 and 240b2 using sputtering or CVD methods.
[0313] Next, by performing CMP processing, a portion of the conductive film that will become the conductive layer 240a and conductive layer 240b is removed, exposing the upper surface of the insulating layer 285. As a result, the conductive layer 240a can be formed inside the opening 203a, and the conductive layer 240b can be formed inside the opening 203b (see Figures 21A to 21B). Note that in some cases, a portion of the upper surface of the insulating layer 285 may be removed by this CMP processing.
[0314] Based on the above, a semiconductor device having the transistor 200 shown in Figures 3A to 4B can be fabricated.
[0315] When manufacturing the semiconductor device shown in Figures 11A to 12, the conductive layer 242_1 is not processed in the steps shown in Figures 18A to 18D. That is, in the steps shown in Figures 18A to 18D, the opening 201, conductive layer 242a2, and conductive layer 242b2 are formed. Next, an insulating film that will become the insulating layer 255 is deposited so as to cover the opening 201, and a part of the insulating film is removed by anisotropic etching. This forms the insulating layer 255. After that, the conductive layer 242_1 is divided by processing the conductive layer 242_1 using the insulating layer 255 as a mask, thereby forming the conductive layer 242a1 and conductive layer 242b1. After that, the steps shown in Figures 19A to 21D are performed. By doing so, the semiconductor device shown in Figures 11A to 12 can be manufactured.
[0316] [Example of Manufacturing Method 2] Below, we will describe an example of a manufacturing method for the semiconductor device shown in Figures 5A to 6B, that is, an example of a manufacturing method for a semiconductor device having transistor 200A. Note that we will mainly describe the steps that differ from those in [Example of Manufacturing Method 1] above, and will omit explanations of the same steps as appropriate.
[0317] First, the process shown in Figures 13A to 14B is carried out. Here, a film 233f is formed using a conductive material. Preferably, the film 233f is formed using the same material as the material used for the conductive layer 242 which will be formed later. For example, if the conductive layer 242 has a laminated structure of conductive layer 242_1 and conductive layer 242_2 on conductive layer 242_1, then it is preferable that the film 233f also has a laminated structure of a first film and a second film on the first film. For example, if ITO is used as conductive layer 242_1, it is preferable to use ITO as the first film, and if ITSO is used as conductive layer 242_1, it is preferable to use ITSO as the first film. Also, if tungsten is used as conductive layer 242_2, it is preferable to use tungsten as the second film.
[0318] Next, a conductive layer 242 is formed to cover layer 233, semiconductor layer 230, and insulating layer 224 (see Figures 22A to 22D). For details on the formation of the conductive layer 242, please refer to the explanation in Figures 16A to 16D.
[0319] Next, the steps shown in Figures 17A to 17D and Figures 18A to 18D are performed. In the steps shown in Figures 18A to 18D, in addition to the insulating layer 280, insulating layer 275, and conductive layer 242, layer 233 is processed. Specifically, the region of layer 233 that overlaps with the opening 201 is removed. This divides layer 233, forming conductive layer 233a and conductive layer 233b (see Figures 23A to 23D). Conductive layer 233a is formed to have a region in contact with the upper surface of semiconductor layer 230 and a region in contact with conductive layer 242a. Conductive layer 233b is formed to have a region in contact with the upper surface of semiconductor layer 230 and a region in contact with conductive layer 242b. Dry etching or wet etching can be used to process layer 233. Dry etching is suitable for microfabrication.
[0320] Next, the steps shown in Figures 19A to 21D are performed. Through these steps, a semiconductor device having transistor 200A can be fabricated.
[0321] By forming conductive layers 233a and 233b, the conductivity of the source electrode and the drain electrode of the transistor can be increased while reducing the thickness of conductive layer 242a and conductive layer 242b, respectively, compared to the case where conductive layers 233a and 233b are not formed. As mentioned above, the conductive layer 242 is formed to cover the top and side surfaces of the semiconductor layer 230. Therefore, when processing the conductive layer 242 to form conductive layers 242a and 242b, it is necessary to remove a portion of the region of the conductive layer 242 that is along the side surface of the semiconductor layer 230. Here, if the thickness of the conductive layer 242 is thick, it becomes difficult to remove this region. On the other hand, if the thickness of the conductive layer 242 is thin, the conductivity of the source electrode and the drain electrode of the transistor will be low. Therefore, by using layer 233 as a conductive layer and performing the subsequent processes after the formation of the conductive layer 242 without removing layer 233, which was used as a hard mask for processing the semiconductor film 230f, the thickness of the conductive layer 242 can be reduced while maintaining the conductivity of the source electrode and the drain electrode of the transistor. As a result, a semiconductor device having transistor 200A can be made into a semiconductor device with a high manufacturing yield. Furthermore, the smaller the taper angle of semiconductor layer 230, the easier it is to remove the region of the conductive layer 242 that is along the side surface of semiconductor layer 230.
[0322] [Manufacturing Method Example 3] Below, we will describe an example of a manufacturing method for the semiconductor device shown in Figures 7A to 8B, that is, an example of a manufacturing method for a semiconductor device having transistor 200B. Note that we will mainly describe the steps that differ from those in [Manufacturing Method Example 1] above, and will omit explanations of the same steps as appropriate.
[0323] First, a substrate (not shown) is prepared, and insulating layers 215, 216, 221, 222, and insulating film 224f are deposited on the substrate (see Figures 24A to 24D). For details on depositing insulating layers 215, 216, 221, 222, and insulating film 224f, please refer to the explanation in Figures 13A to 13D.
[0324] Next, a metal oxide layer 235 is formed on the insulating film 224f (see Figures 24A to 24D). The metal oxide layer 235 can be formed by depositing a metal oxide film that will become the metal oxide layer 235 and processing the metal oxide film by lithography. The metal oxide film can be deposited using sputtering, CVD, MBE, PLD, or ALD. Dry etching or wet etching can be used for this processing. Dry etching is suitable for microfabrication.
[0325] It is preferable to perform a treatment to enhance the crystallinity of the metal oxide film after its formation. For details on the treatment to enhance crystallinity, please refer to the explanation of the treatment to enhance the crystallinity of the semiconductor film 230f in [Example of Manufacturing Method 1].
[0326] It is preferable to perform the above-mentioned crystallinity-enhancing treatment after the formation of the metal oxide film and before the formation of the metal oxide layer 235, i.e., before processing the metal oxide film. However, the crystallinity-enhancing treatment of the metal oxide layer 235 may also be performed after its formation. This further enhances the crystallinity of the metal oxide layer 235. In addition, the surface or film quality of the region of the insulating layer 224 that does not overlap with the metal oxide layer 235 can be modified. It is also possible to omit the crystallinity-enhancing treatment performed before processing the metal oxide film.
[0327] After forming the metal oxide layer 235, microwave-excited plasma treatment may be performed in a hydrogen-containing atmosphere. This enhances the crystallinity of the metal oxide layer 235 and adds hydrogen to the surface of the region of the insulating layer 224 that does not overlap with the metal oxide layer 235, thereby suppressing nucleation in the semiconductor layer 230 near the metal oxide layer 235.
[0328] Furthermore, by performing microwave-excited plasma treatment after forming the metal oxide layer 235, impurities such as carbon on the surface of the metal oxide layer 235 can be removed. Also, impurities such as carbon within the metal oxide layer 235 film can be removed. By keeping the interface between the metal oxide layer 235 and the semiconductor layer 230 cleaner, impurities in the semiconductor layer 230 can be reduced, and the crystallinity of the semiconductor layer 230 can be further improved.
[0329] Next, a semiconductor film 230f is formed to cover the metal oxide layer 235 (see Figures 24A to 24D). For details on the formation of the semiconductor film 230f, please refer to the explanation in Figures 13A to 13D. For example, it is preferable to form an indium oxide film using the sputtering method.
[0330] In the process shown in Figures 24A to 24D, when depositing an indium oxide film using the sputtering method, hydrogen (H) is used as the sputtering gas. 2 It is preferable to use a gas containing ). By introducing hydrogen when forming the semiconductor film 230f using the sputtering method, it is possible to form a semiconductor film 230f with low crystallinity, for example, an amorphous semiconductor film 230f. In addition, nucleation can be suppressed or crystal nuclei other than the metal oxide layer 235 can be promoted during the formation of the semiconductor film 230f. As the sputtering gas, hydrogen, noble gas (typically argon), and oxygen (O) are preferred. 2 A mixed gas of the following can be used.
[0331] Furthermore, a sputtering gas that does not contain hydrogen may be used. As the sputtering gas, for example, a noble gas or oxygen as a single gas, or a mixture of a noble gas and oxygen, etc., can also be used.
[0332] Furthermore, when forming a semiconductor film 230f using the sputtering method, the substrate temperature during film formation of the semiconductor film 230f is preferably between room temperature (25°C) and 250°C, more preferably between room temperature and 200°C, and even more preferably between room temperature and 140°C. For example, setting the substrate temperature to between room temperature and 140°C is preferable because it increases productivity. It is also preferable because it suppresses nucleation. In addition, the metal oxide layer can be formed at room temperature or without heating the substrate.
[0333] For the deposition of the semiconductor film 230f, it is preferable to use a sputtering target with a low impurity concentration, i.e., a high purity sputtering target. For example, the purity of the sputtering target should be 3N or higher, preferably 4N or higher, more preferably 5N or higher, more preferably 6N or higher, and even more preferably 7N or higher, 8N or higher, 9N or higher, or 10N or higher. This makes it possible to deposit a semiconductor film 230f with a low impurity concentration.
[0334] Next, the semiconductor film 230f is processed into island shapes to form the semiconductor layer 230 (see Figures 25A to 25D). The formation of the semiconductor layer 230 can be seen in Figures 13A to 15D. Note that it is not necessary to remove the layer 233 shown in Figures 14A to 14D. That is, it is not necessary to perform the steps shown in Figures 15A to 15D. In addition, the metal oxide layer 235 may be processed as a result of the processing of the semiconductor film 230f. Specifically, regions of the metal oxide layer 235 that do not overlap with the semiconductor layer 230 may be removed.
[0335] Subsequently, it is preferable to perform a treatment on the semiconductor layer 230 to increase its crystallinity. As mentioned above, it is preferable that the semiconductor film 230f be amorphous. Therefore, the treatment to increase crystallinity here can also be called a treatment to crystallize the semiconductor layer 230.
[0336] Examples of treatments to enhance crystallinity include microwave-excited plasma treatment, heating treatment, plasma treatment, microwave treatment, and light irradiation treatment. Multiple of these treatments can be performed simultaneously or sequentially. By performing these crystallinity-enhancing treatments, the semiconductor layer 230 can be crystallized.
[0337] As a treatment to improve the crystallinity of the semiconductor layer 230, for example, heat treatment is preferred. This heat treatment can be carried out at a temperature higher than 150°C and 650°C or lower, preferably between 155°C and 200°C. The heat treatment is preferably carried out in a reduced-pressure atmosphere or an inert gas (nitrogen gas or noble gas) atmosphere. Alternatively, a mixed atmosphere of nitrogen gas and oxygen gas may be used. When performing the treatment in a mixed atmosphere of nitrogen gas and oxygen gas, it is preferable to have an oxygen gas content of about 20%. There are no special limitations on the apparatus used for the heat treatment, and it may be an apparatus that heats the workpiece by heat conduction or thermal radiation from a heat source such as a resistance heating element. For example, an electric furnace or an RTA (Resistance Processing Actuator) apparatus such as an LRTA apparatus or GRTA apparatus can be used. Furthermore, by performing the heat treatment, impurities such as water and hydrogen in the metal oxide that forms the semiconductor layer can be reduced.
[0338] By performing this heat treatment, crystal growth of the semiconductor layer 230 from the metal oxide layer 235 can be promoted, thereby increasing the crystallinity of the semiconductor layer 230. Alternatively, the semiconductor layer 230 can be crystallized. If the metal oxide layer 235 has crystal grains whose crystal orientation <111> is oriented in the film thickness direction of the metal oxide layer 235 (the direction perpendicular to the surface on which the metal oxide layer 235 is formed), then the semiconductor layer 230 also has crystal grains whose crystal orientation <111> is oriented in the film thickness direction of the metal oxide layer 235 (the direction perpendicular to the surface on which the metal oxide layer 235 is formed). Epitaxial growth can occur at least partially in the semiconductor layer 230 located on the metal oxide layer 235, and crystallization can occur. It is estimated that the semiconductor layer 230 (typically indium oxide), which has a cubic crystal structure, will grow crystallized while maximizing the surface area of the {111} plane, which has low interfacial energy. In other words, it is estimated that the {111} plane will preferentially orient in the film thickness direction. Therefore, by performing a treatment to enhance crystallinity, crystal grains (also called <111> oriented crystal grains) whose crystal orientation <111> is oriented parallel to the thickness direction of the insulating layer 224 (the direction perpendicular to the surface on which the semiconductor layer 230 is formed) can be formed in the semiconductor layer 230. Furthermore, on a metal oxide layer 235 which is preferentially oriented to the {111} plane in the film thickness direction, a semiconductor layer 230 which is preferentially oriented to the {111} plane in the film thickness direction can be obtained by at least partial epitaxial growth. When the crystal grains of the semiconductor layer 230 at the edge of the metal oxide layer 235 have an orientation of the (111) plane in the film thickness direction, crystal growth is promoted on planes that are perpendicular to it, such as the (1-10) plane, (-110) plane, (0-11) plane, (01-1) plane, (10-1) plane, (-101) plane, etc. In this case, since there is a degree of rotational freedom in the horizontal direction with respect to the crystal orientation
[111] in the film thickness direction, while the plane orientation in the film thickness direction of the semiconductor layer 230 preferentially grows on the plane with the smallest interfacial energy, a distribution may occur in the crystal plane orientation in the horizontal direction.
[0339] Furthermore, when the metal oxide layer 235 uses hexagonal In-Ga-Zn oxide or a metal oxide with a similar crystal structure, crystals with the {001} plane preferentially oriented can be obtained as described above. Since the atomic arrangements of the hexagonal (001) plane and the cubic (111) plane are close, the cubic (111) plane tends to grow more easily on the hexagonal (001) plane. Therefore, even when the metal oxide layer 235 uses a metal oxide such as In-Ga-Zn oxide, indium oxide with the {111} plane preferentially oriented can be formed in the same way as described above.
[0340] Next, the steps shown in Figures 16A to 21D are performed. Through these steps, a semiconductor device having transistor 200B can be fabricated.
[0341] By fabricating a semiconductor device using the method described above, it becomes easier to improve the crystallinity of the semiconductor layer 230 compared to fabricating a semiconductor device using the method shown in [Fabrication Method Example 1]. On the other hand, when fabricating a semiconductor device using the method shown in [Fabrication Method Example 1], the number of fabrication steps for the semiconductor device can be reduced compared to fabricating a semiconductor device using the method shown in [Fabrication Method Example 3], thereby increasing the productivity of the semiconductor device.
[0342] [Manufacturing Method Example 4] Below, we will describe an example of a manufacturing method for the semiconductor device shown in Figures 9A to 10B, that is, an example of a manufacturing method for a semiconductor device having transistor 200C. Note that we will mainly describe the steps that differ from those in [Manufacturing Method Example 3] above, and will omit explanations of the same steps as appropriate.
[0343] First, insulating layers 215, 216, 221, 222, 224f, and metal oxide layer 235 are formed by the process shown in Figures 24A to 24D. Next, a semiconductor film 230f1, which will become the semiconductor layer 230_1 in a later step, is formed to cover the metal oxide layer 235 (see Figures 26A to 26D). For example, an indium oxide film is formed as the semiconductor film 230f1.
[0344] The thickness of the semiconductor film 230f1 is preferably thin. The thickness of the semiconductor film 230f1 is preferably, for example, 1 nm to 30 nm, more preferably 1.5 nm to 20 nm, and even more preferably 2 nm to 15 nm. This makes it easier to cause crystal growth using the metal oxide layer 235 as a seed or nucleus to occur throughout the semiconductor layer 230_1 in a later crystallization process.
[0345] The semiconductor film 230f1 can be deposited using a method that can be used to deposit the semiconductor film 230f described above. In particular, sputtering, for example, hydrogen (H 2 When a semiconductor film 230f1 is deposited by a sputtering method using a gas containing ), a semiconductor film 230f1 with low crystallinity, specifically an amorphous semiconductor film 230f, can be formed. Therefore, by a subsequent treatment to increase the crystallinity of the semiconductor layer 230f1, the formation of grain boundaries in the channel formation region of the transistor 200C can be suppressed, for example.
[0346] Next, the semiconductor film 230f1 and the insulating film 224f are processed into island shapes to form the semiconductor layer 230_1 and the insulating layer 224 (see Figures 27A to 27D). For the formation of the semiconductor layer 230_1 and the insulating layer 224, the methods shown in Figures 13A to 15D, specifically the methods for forming the semiconductor layer 230 and the insulating layer 224, can be used. Alternatively, the semiconductor film 230f1 and the insulating film 224f may be processed using lithography without forming layer 233. Furthermore, the metal oxide layer 235 may be processed as a result of the processing of the semiconductor film 230f1. Specifically, regions of the metal oxide layer 235 that do not overlap with the semiconductor layer 230_1 may be removed. Figures 27A and 27B show an example in which the side surface of the metal oxide layer 235 opposite to the second region 231_2 is exposed.
[0347] As shown in Figure 27A, the semiconductor layer 230_1, like the semiconductor layer 230 shown in Figure 9B, has a first region 231_1, a second region 231_2, and a third region 231_3. The third region 231_3 has a portion that functions as a channel formation region for the transistor 200C, as described above. The width j1 of the third region is shorter than the width j2 of the second region.
[0348] Next, it is preferable to perform a treatment to increase the crystallinity of the semiconductor layer 230_1 (see Figures 28A to 28D). The semiconductor film 230f1 is preferably amorphous, similar to the semiconductor film 230f shown in Figures 24A to 24D. Therefore, the treatment to increase crystallinity here can also be called a treatment to crystallize the semiconductor layer 230_1.
[0349] As a treatment to improve the crystallinity of the semiconductor layer 230_1, it is preferable to use a method similar to the treatment for improving the crystallinity of the semiconductor film 230f shown in Figures 24A to 24D. For example, as mentioned above, examples include microwave-excited plasma treatment, heating treatment, plasma treatment, microwave treatment, and light irradiation treatment. Note that multiple types of these treatments can be performed simultaneously or sequentially. The dotted arrows shown in Figures 28A and 28D indicate heat, plasma, microwave, radical, light, etc.
[0350] The first region 231_1 is a region on the metal oxide layer 235 that forms polycrystals preferentially oriented to the {111} plane with respect to the film thickness direction. The second region 231_2 undergoes crystal growth from the first region 231_1. This crystal growth can be called lateral growth. During this process, geometric selection occurs, and the selection of crystal grains occurs due to competition for crystal growth. Subsequently, the semiconductor layer 230_1 selects crystal grains by making the width j1 of the third region narrower than the width j2 of the second region, thereby guiding only the crystal grains that have preferentially grown toward the third region 231_3 to the third region 231_3 and allowing them to grow further.
[0351] As a result, the formation of grain boundaries in the third region 231_3 can be suppressed. Alternatively, the third region 231_3 can be made into a region where no grain boundaries are observed. Alternatively, the third region 231_3 can be made into a region having a cross-section in the channel length direction of transistor 200C where no grain boundaries are observed, by analysis using a transmission electron microscope. Alternatively, the third region 231_3 can be made into a crystal that does not contain grain boundaries when analyzed by electron diffraction mapping, where adjacent measurement points with an orientation difference of 5° or more are considered as grain boundaries. Alternatively, the third region 231_3 can be made into a single-grain crystal.
[0352] As mentioned above, crystal growth in the semiconductor layer 230_1 is mainly lateral growth. Therefore, reducing the thickness of the semiconductor layer 230_1 is preferable because it makes it easier for crystal growth to occur on the upper surface of the semiconductor layer 230_1 and its vicinity.
[0353] Next, a semiconductor film 230f2, which will become semiconductor film 230_2 in a later step, is formed to cover semiconductor film 230_1 and insulating film 224 (see Figures 29A to 29D). Semiconductor film 230f2 is formed using the same material as semiconductor film 230f1. For example, if an indium oxide film is formed as semiconductor film 230f1, then an indium oxide film is formed as semiconductor film 230f2.
[0354] The thickness of the semiconductor film 230f2 is made thicker than the thickness of the semiconductor film 230f1. The semiconductor film 230f2 can be deposited using a method that can be used to deposit the semiconductor film 230f described above. In particular, depositing the semiconductor film 230f2 using the sputtering method is preferable because it makes it easier to deposit a thicker semiconductor film 230f2 while maintaining the productivity of semiconductor devices.
[0355] Next, it is preferable to perform a treatment to increase the crystallinity of the semiconductor film 230f2 (see Figures 30A to 30D). The semiconductor film 230f2 is preferably amorphous, similar to the semiconductor film 230f shown in Figures 24A to 24D. Therefore, the treatment to increase crystallinity here can also be called a treatment to crystallize the semiconductor film 230f2.
[0356] As a treatment to improve the crystallinity of the semiconductor film 230f2, it is preferable to use a method similar to the treatment for improving the crystallinity of the semiconductor film 230f shown in Figures 24A to 24D. The dotted arrows shown in Figures 30A and 30D indicate heat, plasma, microwaves, radicals, light, etc., similar to the dotted arrows shown in Figures 28A and 28D.
[0357] As a result, epitaxial growth occurs in the semiconductor film 230f2 located on the semiconductor layer 230_1. This causes the semiconductor film 230f2 to crystallize. Here, the direction of crystal growth of the semiconductor film 230f2 is perpendicular to the upper surface of the insulating layer 224. Therefore, even if the thickness of the semiconductor film 230f2 is high, crystal growth can be caused up to the upper surface of the semiconductor film 230f2 and its vicinity.
[0358] Next, the semiconductor film 230f2 is processed into island shapes to form semiconductor layers 230_2 (see Figures 31A to 31D). For the formation of semiconductor layers 230_2, the methods shown in Figures 13A to 15D, specifically the methods for forming semiconductor layers 230, can be used. Note that it is not necessary to remove layer 233 shown in Figures 14A to 14D. That is, the steps shown in Figures 15A to 15D may not be performed. In addition, processing of the semiconductor film 230f2 may result in processing of semiconductor layers 230_1, metal oxide layers 235, and insulating layers 224. Specifically, regions of semiconductor layer 230_1 and insulating layer 224 that do not overlap with semiconductor layer 230_2 may be removed.
[0359] As a result, the semiconductor layer 230 is formed as a stacked structure of semiconductor layer 230_1 and semiconductor layer 230_2 on semiconductor layer 230_1. Here, the boundary between semiconductor layer 230_1 and semiconductor layer 230_2 may not be clearly visible. After the formation of semiconductor layer 230_2, the above-mentioned crystallinity-enhancing treatment may be performed. In this case, the above-mentioned crystallinity-enhancing treatment may not be performed before processing the semiconductor film 230f2.
[0360] Here, in a cross-sectional view of the transistor 200C in the channel width direction, semiconductor layer 230_1 and semiconductor layer 230_2 are formed such that the height (film thickness) of semiconductor layer 230_2 is greater than the width of the lower surface of semiconductor layer 230_1 (corresponding to the width W shown in Figure 4A). This allows the semiconductor layer 230 to be formed to have a fin-like shape.
[0361] Furthermore, it is preferable that the semiconductor layer 230_2 be formed to have a tapered shape with a taper angle of less than 90°. In Figure 31C, the taper angle is shown as the angle θ2 between the side surface of the semiconductor layer 230_2 and the top surface of the semiconductor layer 230_1. If the angle θ2 is small, it becomes easier to prevent the semiconductor layer 230_2 from tipping over during the manufacturing process of the transistor 200C. On the other hand, if the angle θ2 is too small, it becomes difficult to make the semiconductor layer 230_2 tall. Based on the above, it is preferable to set the angle θ2. The angle θ2 can be within the range of the angle θ mentioned above. For example, the angle θ2 can be equal to or approximately equal to the angle θ. Alternatively, the angle θ2 can be smaller than the angle θ. Note that if the angle θ is less than 90°, the area of the bottom surface of the semiconductor layer 230_2 will be larger than the area of the top surface of the semiconductor layer 230_2.
[0362] By forming the semiconductor layer 230 using the method described above, the thickness of the semiconductor layer 230 can be increased while simultaneously improving the overall crystallinity of the semiconductor layer 230. As mentioned above, the thicker the semiconductor layer 230, the smaller the area occupied by the semiconductor layer 230, the larger the channel width of the transistor, and the lower the contact resistance between the source electrode and the semiconductor layer 230, as well as the contact resistance between the drain electrode and the semiconductor layer 230. Furthermore, high crystallinity of the semiconductor layer 230 effectively reduces carrier scattering within the semiconductor layer 230. Therefore, the field-effect mobility can be increased, and the reliability of the transistor can be improved. Thus, by forming the semiconductor layer 230 using the method described above, it is possible to manufacture a semiconductor device that is miniaturized or highly integrated, operates at a high speed, and is highly reliable. Note that in the manufacture of a semiconductor device having transistor 200C, it is not necessary to deposit the semiconductor film 230f1 and form the semiconductor layer 230_1. In this case, the number of manufacturing steps for the semiconductor device can be reduced, and the productivity of the semiconductor device can be increased.
[0363] Next, the steps shown in Figures 16A to 21D are performed. As a result, a semiconductor device having transistor 200C can be fabricated. Note that, for example, when fabricating a semiconductor device having transistor 200B, the steps shown in Figures 26A to 31D may also be used to fabricate the semiconductor device.
[0364] This embodiment can be combined with other embodiments as appropriate. Furthermore, if multiple configuration examples are shown within a single embodiment in this specification, these configuration examples can be combined as appropriate.
[0365] (Embodiment 2) This embodiment describes an indium oxide film that can be used in the semiconductor layer of a transistor in a semiconductor device according to one aspect of the present invention.
[0366] Note that in this specification and the like, indium oxide having at least a crystal part or a crystal region in a film is referred to as crystalline indium oxide (crystal IO). For example, single-crystal indium oxide, polycrystalline indium oxide, microcrystalline indium oxide, or the like can be given as crystal IO or crystalline IO.
[0367] Indium oxide is a semiconductor material having physical properties completely different from those of oxide semiconductors such as In-Ga-Zn oxide (hereinafter also referred to as IGZO) and zinc oxide.
[0368] The carrier concentration dependence of Hall mobility of indium oxide, silicon, and IGZO is described. FIG. 32A shows silicon (Si) and indium oxide (InO X ), and FIG. 32B is a schematic diagram of the carrier concentration dependence of Hall mobility for IGZO.
[0369] First, as indicated by an arrow in FIG. 32B, IGZO tends to have higher Hall mobility as the carrier concentration is higher. On the other hand, as indicated by an arrow in FIG. 32A, indium oxide tends to have higher Hall mobility as the carrier concentration is lower (see Non-Patent Document 2). This tendency is similar to that of silicon; the lower the concentration of a dopant (impurity) in the material, the lower the impurity scattering and the higher the Hall mobility. That is, the higher the purity and the more intrinsic indium oxide is, the higher the Hall mobility becomes. From these results, it can be said that indium oxide is a substance having physical properties close to silicon, unlike IGZO. Note that the characteristics of indium oxide shown in FIG. 32A are on the assumption of a single crystal. Therefore, when indium oxide is non-single-crystal (e.g., polycrystalline), the characteristics might differ from those shown in FIG. 32A.
[0370] In FIG. 32A, a range R1 with a low carrier concentration has extremely high Hall mobility, and thus can be said to be a carrier concentration range suitable for, for example, a channel formation region of a transistor. For example, in the case of indium oxide, the range R1 is a range including a carrier concentration value of 1×10 15 cm −3 , and is, for example, 1×10 14 cm−3 The above is 1 x 10 18 cm −3 The range is as follows: By sufficiently reducing the carrier concentration, the hole mobility value can be increased to 270 cm⁻¹. 2 It can be expected to be raised to the level of / (V・s).
[0371] Furthermore, in indium oxide, the region where the carrier concentration is within the range R1 may contain elements that lower the carrier concentration. Examples of elements that lower the carrier concentration include magnesium, calcium, zinc, cadmium, and copper. By substituting these elements for indium, the carrier concentration can be lowered. Other elements that lower the carrier concentration include nitrogen, phosphorus, arsenic, and antimony. For example, by substituting nitrogen, phosphorus, arsenic, or antimony for oxygen, the carrier concentration can be lowered.
[0372] Elements that reduce carrier concentration can also be called elements that confer p-type properties. Adding elements that reduce carrier concentration to an indium oxide film can make the indium oxide film i-type or substantially i-type. In this case, the concentration of the above-mentioned carrier-reducing element in the indium oxide film is 1 × 10⁻⁶. 16 atoms / cm 3 The above 8 x 10 20 atoms / cm 3 The following is preferable: 1 × 10 16 atoms / cm 3 The above 4 x 10 20 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 8 x 10 19 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 5 x 10 19 atoms / cm 3 The following is even more preferable. By using such concentrations, the carrier concentration can be reduced while maintaining the crystal structure of indium oxide.
[0373] On the other hand, the range R2 with a high carrier concentration has low electric resistance, and can be said to be a carrier concentration range suitable for, for example, a source region and a drain region of a transistor, a resistor, or a transparent conductive film. The value of the carrier concentration in the range R2 is 1×10 20 cm −3 and is a range including, for example, 1×10 19 cm −3 or more and 1×10 22 cm −3 or less. By sufficiently increasing the carrier concentration, it is expected that the resistivity can be reduced to 1×10 −4 Ω·cm or less.
[0374] Note that in indium oxide, the region where the carrier concentration is in the range R2 can contain an element that increases the carrier concentration. For example, it is preferable to contain an element common to the source electrode and the drain electrode of the transistor. Examples of the element that increases the carrier concentration include titanium, zirconium, hafnium, tantalum, tungsten, molybdenum, tin, silicon, boron, and the like. In particular, it is more preferable to use an element whose oxide has conductivity or semiconductivity. Note that as a method for supplying the element that increases the carrier concentration, a method of forming and diffusing a film containing the element, an ion implantation method, an ion doping method, a plasma immersion ion implantation method, or plasma treatment can be used. Note that in this specification and the like, unless otherwise specified, the presence or absence of mass separation is not limited. For example, in this specification and the like, a method of supplying ions after mass separation is referred to as an ion implantation method, and a method of supplying ions without mass separation is referred to as an ion doping method.
[0375] The element that increases the carrier concentration can also be referred to as an element that imparts n-type conductivity. The concentration of the element that increases the carrier concentration in the indium oxide film is 1×10 16 atoms / cm 3 or more and 8×10 20 atoms / cm 3 or less is preferable, 1×10 16 atoms / cm 3 or more and 4×10 20 atoms / cm 3 or less is more preferable, and 1×10 16atoms / cm 3 The above 8 x 10 19 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 5 x 10 19 atoms / cm 3 The following is even more preferable. By using such concentrations, the carrier concentration can be increased while maintaining the crystal structure of indium oxide. Antimony can also function as an element that increases the carrier concentration.
[0376] As indium oxide is an oxide whose valence electrons can be controlled, the threshold voltage of a transistor using a semiconductor layer containing indium oxide can be controlled. Furthermore, in indium oxide, regions with low carrier concentrations can be used as the channel formation region of the transistor, while regions with high carrier concentrations can be used as the source and drain regions. In contrast, with IGZO, strain can form in the source and drain regions due to stress on the electrodes in contact with the IGZO, sometimes resulting in the formation of an n-type region. On the other hand, unlike IGZO, indium oxide allows for valence electron control, so it does not require the formation of strain in the film as in IGZO. Less strain in the film is expected to improve reliability. For example, by creating regions with carrier concentrations in the range R1 and range R2 shown in Figure 32A within the indium oxide film, a so-called n-i-n junction (a junction of an n-type region, an i-type region, and an n-type region) can be created. Valence electron control in silicon transistors is generally known. On the other hand, valence electron control in transistors using indium oxide is a novel technological concept that would not normally be conceived.
[0377] By applying the above technical concept, the indium oxide transistor described herein has two or more, preferably three or more, more preferably four or more, and most preferably five of the following features (1) to (5): (1) High on-current (in other words, high mobility). (2) Low off-current. (3) Normally off is possible. (4) High reliability. (5) High cutoff frequency (fT). For example, the indium oxide transistor described herein has high mobility, low off-current, and is normally off. This transistor is different from a transistor that is high mobility and normally on.
[0378] In addition, the i-type nature of a semiconductor means that the Fermi level (Ef) and the intrinsic Fermi level (Ei) are the same (Ef = Ei). As shown in Figure 32B, in IGZO, the lower the carrier concentration, the lower the hole mobility. Therefore, when Ef = Ei is reached, there are no carriers left (in other words, the material has properties similar to an insulator), and it may cease to function as a transistor. On the other hand, in indium oxide, as shown in Figure 32A, the lower the carrier concentration, the higher the hole mobility, and when Ef = Ei is reached, the hole mobility is maximized. That is, transistors containing indium oxide can achieve high field-effect mobility by setting Ef = Ei. Furthermore, because transistors containing indium oxide have a low carrier concentration, they tend to be normally off. Therefore, transistors containing indium oxide can be normally off and achieve high field-effect mobility.
[0379] Normally off refers to the state in which no current flows through a transistor when no potential is applied to the gate or when the gate-source voltage is 0V. Normally off can be evaluated using the transistor's threshold voltage (Vth) or shift value (Vsh). Unless otherwise specified, Vth will be calculated using the constant current method. More specifically, Vth is the value of drain current (Id) × channel length (L) ÷ channel width (W) in the transistor's Id-Vg characteristic where the current is 1nA (1 × 10⁻¹⁰).−9 Let Vg be the gate voltage (Vg) when A) is true. Also, Vsh is defined as the tangent to the maximum slope when the drain current (Id) in the Id-Vg characteristic of the transistor is expressed logarithmically, and Id = 1pA (1 × 10⁻¹⁰). −12 Vg is the gate voltage (Vg) at the intersection with line A), or the Vg at the intersection of the line extrapolated from the two points where the slope of Id is maximized when Id is expressed logarithmically in the transistor's Id-Vg characteristic, and the line where Id = 1 pA. For example, if either or both of Vth and Vsh are zero or positive values, it can be considered a normally-off transistor.
[0380] Furthermore, in transistors containing indium oxide, the film configuration in contact with the indium oxide film is crucial for making the semiconductor i-type, that is, for achieving Ef = Ei. For example, in transistors containing indium oxide, a film configuration can be obtained in which a silicon oxide film, a hafnium oxide film, and a silicon nitride film are stacked in contact with the indium oxide film. By using this film configuration, it is possible to create a semiconductor device that satisfies Ef = Ei and is highly reliable.
[0381] Furthermore, in the above film configuration, oxygen-containing films such as silicon oxide-nitride films, silicon oxide nitride films, aluminum oxide films, and gallium oxide films can be used instead of the silicon oxide film. Also, in the above film configuration, silicon oxide nitride films, silicon oxide nitride films, etc. can be used instead of the silicon nitride film. In addition, the hafnium oxide film located on the indium oxide side of the silicon nitride film functions as a hydrogen gettering site.
[0382] Furthermore, the above film configuration can also be viewed as a layered structure consisting of a film that can supply oxygen to the indium oxide film (e.g., a silicon oxide film), a film that can getter hydrogen (e.g., a hafnium oxide film), and a film that suppresses the intrusion of oxygen and hydrogen (e.g., a silicon nitride film). With this configuration, oxygen deficiencies in the indium oxide film are compensated for by oxygen in the silicon oxide film. Also, hydrogen in the indium oxide film is captured by the hafnium oxide film through heat treatment, etc. In addition, the silicon nitride film is provided to create a film configuration in which oxygen and hydrogen do not easily enter from the outside. In other words, by using the above film configuration, the indium oxide film can be made closer to type i. Therefore, transistors having the above indium oxide film have high field-effect mobility and high reliability.
[0383] Next, we will describe indium oxide films applied to transistors. Indium oxide films are preferably crystalline (i.e., they have crystal grains). Examples of films with crystal grains include single-crystal films, polycrystalline films, or amorphous films containing crystal grains (also called microcrystalline films). In particular, polycrystalline films are preferred for indium oxide films, and single-crystal films are more preferred. Single-crystal films do not have crystal grain boundaries. Impurities that inhibit carrier flow (typically insulating impurities, insulating oxides, etc.) tend to segregate at crystal grain boundaries. By using a single-crystal film, carrier scattering at crystal grain boundaries can be suppressed, enabling the realization of transistors with high field-effect mobility. Furthermore, it offers excellent effects such as suppressing variations in transistor characteristics caused by these crystal grain boundaries.
[0384] Furthermore, polycrystalline films are preferable because they can reduce carrier scattering and exhibit high field-effect mobility compared to microcrystalline or amorphous films. When using polycrystalline films, it is preferable to use films with the largest possible grain size and few grain boundaries. In a transistor to which a polycrystalline indium oxide film is applied, if there are no grain boundaries in the channel formation region, or if no grain boundaries are observed, the channel formation region is located within the single-crystal region contained in the polycrystalline film, and therefore it can be considered a transistor to which single-crystal indium oxide is applied.
[0385] The crystallinity of indium oxide can be analyzed, for example, by XRD, TEM, or ED. Alternatively, a combination of these methods may be used for analysis.
[0386] Furthermore, in this specification, a semiconductor layer in which no grain boundaries are observed in the channel-forming region, a semiconductor layer in which the channel-forming region is contained within a single crystal grain, or a semiconductor layer in which the direction of the crystal axes is the same in at least two regions within the channel-forming region can be called a single crystal film. In addition, a semiconductor layer in which, within a single crystal grain in the channel-forming region, the direction of other crystal axes changes continuously with respect to a certain crystal axis or crystal orientation as the axis of rotation can be called a single crystal film.
[0387] The channel formation region refers to the region within the semiconductor layer that overlaps with (or faces) the gate electrode via the gate insulating layer, and is located between the region in contact with the source electrode and the region in contact with the drain electrode. The current path in the channel formation region is the shortest distance between the source electrode and the drain electrode. Therefore, the crystal grains, grain boundaries, crystal axes, and crystal orientation in the channel formation region can be confirmed by cross-sectional observation including the semiconductor layer, source electrode, and drain electrode.
[0388] The indium oxide film in the channel-forming region is preferable to have a low impurity concentration. Impurities in the indium oxide film in the channel-forming region can act as a scattering source for carriers, and thus can cause a decrease in field-effect mobility. Furthermore, these impurities can also inhibit the crystal growth of the indium oxide film. Examples of impurities in the indium oxide film include boron and silicon. The concentration of these impurities in the indium oxide film is preferably 0.1% or less, and more preferably 0.01% (100 ppm) or less. Note that carbon, hydrogen, and other elements may be present in the film-forming gas or precursor during film formation, and may remain in the indium oxide film in higher concentrations than the above-mentioned impurities.
[0389] Furthermore, the indium oxide film may contain elements that can become trivalent cations like indium, as long as their crystals maintain a cubic crystal structure (Bixbite type). Examples include Group 13 elements of the periodic table such as gallium and aluminum, and Group 3 elements of the periodic table. Since the bonding force of these elements is stronger than that of indium and oxygen, adding these elements to the indium oxide film can reduce oxygen vacancies (V) in the indium oxide film. O This can suppress the formation of ions. Furthermore, since these elements mainly exist as trivalent cations in oxides, the carrier concentration of the indium oxide film can be kept low. Therefore, it becomes possible to shift the threshold voltage of the transistor to the positive side. Also, normally-off becomes possible. Thus, a transistor with good electrical characteristics can be provided.
[0390] The concentration of the above elements in the indium oxide film is 1 × 10⁻⁶ 16 atoms / cm 3 The above 8 x 10 20 atoms / cm 3 The following is preferable: 1 × 10 16 atoms / cm 3 The above 4 x 10 20 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 8 x 10 19 atoms / cm 3The following is more preferable: 1 × 10 16 atoms / cm 3 The above 5 x 10 19 atoms / cm 3 The following are even more preferable.
[0391] Furthermore, the elements that impart n-type, p-type, and trivalent cations mentioned above can be added to the indium oxide film by methods such as ion doping, ion implantation, and thermal diffusion. Alternatively, the elements that impart n-type, p-type, and trivalent cations mentioned above can be added to the sputtering target, deposition gas, ALD deposition precursor, etc., used when depositing the indium oxide film. Alternatively, the elements that impart n-type, p-type, and trivalent cations mentioned above can be auto-doped from the chamber used when depositing the indium oxide film. Auto-doping refers to the automatic addition of elements contained in the chamber components, etc., into the indium oxide film during deposition.
[0392] Furthermore, the indium oxide film described herein has a high film density. The theoretical value of the film density of the indium oxide film is 7.18 g / cm³. 3 In this specification, the range of film density for indium oxide films is 6.70 g / cm³. 3 7.18g / cm or more 3 The following, preferably 6.90 g / cm³ 3 7.18g / cm or more 3 The following, and more preferably 7.00 g / cm³ 3 7.18g / cm or more 3 The following applies:
[0393] Furthermore, film density can be evaluated using methods such as Rutherford backscattering (RBS) or X-ray reflectivity (XRR). Differences in film density can sometimes be evaluated using transmission electron microscopy (TEM) images of the cross-section. In TEM observation, a high film density results in a darker (more intense) transmission electron (TE) image, while a low film density results in a fainter (brighter) transmission electron (TE) image.
[0394] By using such an indium oxide film in a transistor, the field-effect mobility of the transistor can be increased to 50 cm². 2 / (V·s) or more, preferably 100 cm 2 / (V·s) or more, more preferably 150 cm 2 / (V·s) or more, more preferably 200 cm 2 / (V·s) or more, more preferably 250 cm 2 It can be set to (V・s) or more.
[0395] One of the characteristics of indium oxide films is that they have higher oxygen permeability (diffusivity) compared to IGZO films. As shown in Figure 32C, indium oxide films (InO X Oxygen (O) diffusing into the indium oxide film passes through the indium oxide film and oxygen molecules (O) 2 It is released as water molecules (H) by reacting with hydrogen contained in the membrane. 2 It may also be released as O. Furthermore, oxygen deficiencies (V) can form in the membrane. O If oxygen atoms are present, diffusing oxygen atoms will fill the oxygen deficiency. Indium oxide films allow oxygen to diffuse easily, so they can be said to fill oxygen deficiencies more easily than IGZO films.
[0396] Thus, because indium oxide films are more likely to reduce oxygen vacancies in the film compared to IGZO films, applying such indium oxide films to transistors makes it possible to realize transistors with extremely high reliability.
[0397] Furthermore, as shown in Figure 32C, the indium oxide film diffuses hydrogen. Hydrogen diffusing into the indium oxide film from the outside permeates the film and forms hydrogen molecules (H 2 It is released as ) or, by reacting with oxygen contained in the film, it is released as water molecules. The above-mentioned oxygen and hydrogen diffuse through the indium oxide film by heat treatment. The temperature of the heat treatment is 200°C to 700°C, preferably 350°C to 650°C, and more preferably 400°C to 500°C.
[0398] A transistor using an indium oxide film is an accumulation-mode transistor with electrons as majority carriers. Assuming that the carrier relaxation time is a constant value, the smaller the effective mass of electrons (carriers), the higher the electron mobility. In other words, by using indium oxide, which has a small electron effective mass, in a transistor, the on-state current or field-effect mobility of the transistor can be increased.
[0399] Table 1 shows the effective masses of single-crystal indium oxide (here, In 2 O 3 ) and single-crystal silicon (Si), respectively. As shown in Table 1, indium oxide is characterized by a small electron effective mass and a large hole effective mass. Indium oxide also has the feature that its electron effective mass hardly depends on the crystal orientation. Therefore, by using crystalline indium oxide in a transistor, a transistor with high field-effect mobility and a transistor with high frequency characteristics (also referred to as f-characteristics) can be realized. Furthermore, since the hole effective mass is large, a transistor with extremely low off-state current can be realized. For example, by applying an indium oxide film to a vertical transistor, the off-state current per 1 μm of channel width can be 1 fA (1×10 −15 A) or less, or 1 aA (1×10 −18 A) or less in an environment of 125°C, and can be 1 aA (1×10 −18 A) or less, or 1 zA (1×10 −21 A) or less at room temperature (25°C). In addition, as shown in Table 1, indium oxide has a smaller electron effective mass and a larger hole effective mass than silicon, so there is a possibility that a transistor with higher field-effect mobility and lower off-state current than a Si transistor can be realized.
[0400]
[0401] It is preferable to provide a seed layer so as to be in contact with at least a portion of the crystalline indium oxide film. It is preferable to use a material containing crystals with a small difference in lattice constant (also called lattice mismatch) with the indium oxide for the seed layer. This improves the crystallinity of the indium oxide film. A substrate (e.g., a single-crystal substrate) may be used as one of the layers in contact with at least a portion of the crystalline indium oxide film.
[0402] One method for evaluating the degree of lattice mismatch is to use the following lattice mismatch value. The lattice mismatch Δa [%] of the crystals in the formed film (in this case, the indium oxide film) relative to the crystals in the seed layer is given by Δa = ((L 1 -L 2 ) / L 2 It is calculated as ) × 100. Here L 1 L is the length of the unit cell vector of the crystals in the formed film, or the lattice constant. 2 This is the length of the unit cell vector of the crystal in the seed layer, or the lattice constant.
[0403] The lattice mismatch Δa between the seed layer and the indium oxide film is preferably small in absolute value, and most preferably zero. For example, Δa can be -5% or more and 5% or less, preferably -4% or more and 4% or less, more preferably -3% or more and 3% or less, and even more preferably -2% or more and 2% or less.
[0404] Here, the indium oxide crystal has a cubic structure (bixbite type). For example, yttria-stabilized zirconia (YSZ) crystals can have a cubic structure (fluorite type). The lattice mismatch of the indium oxide crystal with respect to the cubic YSZ crystal is in the range of -2% to 2%, and a single crystal film of indium oxide can be epitaxially grown on a YSZ substrate.
[0405] Furthermore, the crystal structure of the seed layer and the crystal structure of the indium oxide film do not necessarily have to be the same in terms of crystal system or crystal orientation. For example, a film with a hexagonal or trigonal crystal structure can be used beneath an indium oxide film with a cubic crystal structure. For example, by setting the crystal orientation of the surface of the seed layer to
[001] and the crystal orientation of the underside of the indium oxide film to
[111] , the requirements related to crystal orientation necessary for epitaxial growth can be met. Examples of hexagonal or trigonal crystals include wurtzite-type structures and YbFe. 2 O 4 Type structure, Yb 2 Fe 3 O 7 There are molded structures and their modified molded structures, etc. YbFe 2 O 4 Type structure or Yb 2 Fe 3 O 7 An example of a crystal with a crystalline structure is IGZO. Indium oxide single crystal films can be formed not only on YSZ substrates but also on insulating films. On the other hand, it is difficult to form silicon single crystal films on insulating films. Silicon crystals have a diamond structure. Thus, in terms of single crystals, indium oxide and silicon have similar properties. However, when comparing indium oxide and silicon from the perspective of whether single crystals can be formed on insulating films, they have different properties.
[0406] This embodiment can be combined with other embodiments as appropriate. Furthermore, if multiple configuration examples are shown within a single embodiment in this specification, these configuration examples can be combined as appropriate.
[0407] (Embodiment 3) In this embodiment, a storage device according to one aspect of the present invention will be described with reference to Figures 33A to 34. The storage device according to one aspect of the present invention has a memory cell. The memory cell has a transistor and a capacitive element. The transistor and memory cell can be a transistor and a semiconductor device including the transistor described in Embodiment 1. Detailed descriptions of the transistor and the semiconductor device including the transistor may be omitted as they can be described by referring to the description of Embodiment 1.
[0408] The configuration of a memory device having a transistor and a capacitive element will be explained using Figures 33A and 33B. Figure 33A is a plan view of a memory device having a memory cell 10. Figure 33B is a cross-sectional view between the dashed lines C1 and C2 shown in Figure 33A. The memory cell 10 has a capacitive element 100 and a transistor 200. Figures 33A and 33B show an example using a semiconductor device including the transistor 200 shown in Embodiment 1, but the semiconductor device is not limited to including the transistor 200, and one or more types of semiconductor devices including each of the transistors exemplified in Embodiment 1 can be used.
[0409] As shown in Figures 33A and 33B, a conductive layer 167a is provided on the conductive layer 240a and on the insulating layer 285. A conductive layer 167b is provided on the conductive layer 240b and on the insulating layer 285. Conductive layer 242a and conductive layer 167a are connected via conductive layer 240a. Conductive layer 242b and conductive layer 167b are connected via conductive layer 240b. Conductive layers 167a and 167b can be formed as single layers or laminates using the materials and configurations described in the <Conductive Layer> section of Embodiment 1. For example, conductive layers 167a and 167b can be made of tungsten. Because highly conductive materials such as tungsten can be used, the wiring resistance of conductive layers 167a and 167b can be reduced.
[0410] In the memory cell 10, the conductive layer 260 functions as a word line and extends in a first direction. The conductive layer 167a functions as a bit line and extends in a second direction. The second direction can be perpendicular to the first direction in a plan view.
[0411] The memory device shown in Figure 33B has a transistor 200 on a substrate (not shown), and a capacitive element 100 on the transistor 200.
[0412] The capacitive element 100 has at least a conductive layer 167b, an insulating layer 191, and a conductive layer 192. The insulating layer 191 is provided between the conductive layer 167b and the conductive layer 192. At least a portion of the conductive layer 167b functions as one electrode of the capacitive element 100. At least a portion of the conductive layer 192 functions as the other electrode of the capacitive element 100. At least a portion of the insulating layer 191 functions as a dielectric layer of the capacitive element 100.
[0413] Furthermore, in the capacitive element 100, the insulating layer 191 covers the conductive layer 167b, and in a plan view, the outer edge of the conductive layer 192 can be formed to be further outward than the outer edge of the conductive layer 167b. By doing so, the capacitance of the capacitive element 100 can be increased.
[0414] As shown in Figures 33A and 33B, the capacitive element 100 is provided on the transistor 200, overlapping with the transistor 200. With this configuration, in a plan view, the capacitive element 100 and the transistor 200 can be provided without significantly increasing the occupied area compared to the case where only one of the capacitive element 100 or the transistor 200 is provided on the semiconductor device. As a result, the occupied area of the memory cell 10 can be reduced, allowing for a high-density arrangement of the memory cell 10 and increasing the storage capacity of the storage device. In other words, the storage device can be highly integrated.
[0415] The insulating layer 193 is provided on the capacitive element 100 so as to cover the capacitive element 100. The insulating layer 194 is provided on the insulating layer 193.
[0416] For insulating layers such as insulating layer 193 and insulating layer 194, one or more insulating materials described in <Insulating Layer> of Embodiment 1 can be used. In particular, for insulating layer 193, it is preferable to use one or more insulating materials that have the function of suppressing the permeation of impurities such as hydrogen and oxygen, insulating materials that have the function of capturing or fixing hydrogen, insulating materials that have barrier properties against hydrogen, or insulating materials that have barrier properties against oxygen. For insulating layer 193, it is preferable to use, for example, silicon nitride or aluminum oxide, or a two-layer structure in which silicon nitride is laminated on aluminum oxide. By using these insulating materials, the diffusion of hydrogen from structures above insulating layer 193 to the semiconductor layer 230 of the transistor 200 can be suppressed. Furthermore, the transistor 200 can be made highly reliable. For insulating layer 194, it is preferable to use one or more insulating materials that have a lower dielectric constant than high-k materials, insulating materials with high dielectric strength, or insulating materials that suppress leakage current. For insulating layer 194, it is preferable to use, for example, silicon oxide. Since the insulating layer 194 functions as an interlayer insulating layer, parasitic capacitance between wirings can be reduced by using an insulating material with a low dielectric constant. Furthermore, the insulating layer 194 may be planarized using a method such as CMP so that its upper surface is flat.
[0417] The conductive layer, such as the conductive layer 192, can be formed as a single layer or in a laminated form using the materials and configuration described in the <Conductive Layer> of Embodiment 1. For example, the conductive layer 192 can be made of tungsten. Because a highly conductive material such as tungsten can be used, the wiring resistance of the conductive layer 192 can be reduced.
[0418] The insulating layer 191 can be formed as a single layer or in a laminate using one or more insulating materials described in the <insulating layer> of Embodiment 1. It is preferable to use one or more insulating materials with a high dielectric constant (high-k), insulating materials with high dielectric strength, or insulating materials that suppress leakage current for the insulating layer 191. For example, an insulating film (also called ZAZ) laminated in the order of zirconium oxide, aluminum oxide, and zirconium oxide can be used. Alternatively, for example, an insulating film (also called ZAZA) laminated in the order of zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide can be used.
[0419] Furthermore, a ferroelectric material may be used for the insulating layer, such as the insulating layer 191. For example, hafnium zirconium oxide can be used. When a ferroelectric material is used for the insulating layer 191, it is preferable to use titanium nitride for at least the portion of one or both of the conductive layer 167b and the conductive layer 192 that is in contact with the insulating layer 191. By using a ferroelectric material for the dielectric layer of the capacitive element 100, the memory device shown in this embodiment can function as a ferroelectric memory.
[0420] Figure 34 shows an example of a cross-sectional configuration of a memory device in which layers having memory cells 10, as shown in Figures 33A and 33B, are stacked on a layer on which a drive circuit including a sense amplifier is provided.
[0421] In the example shown in Figure 34, a memory cell 10 is provided above the Si transistor 900. The Si transistor 900 is one of the transistors in the drive circuit, which includes a sense amplifier.
[0422] Let's describe the Si transistor 900. The Si transistor 900 is a Fin-type transistor. Figure 34 shows a schematic cross-sectional view in the channel length direction.
[0423] The Si transistor 900 is provided on a substrate 901 and has a conductive layer 908a that functions as a gate electrode, an insulating layer 907 that functions as a gate insulating layer, a semiconductor region 903 that functions as a channel forming region, and a low-resistance region 904 that functions as a source region or drain region.
[0424] For example, a silicon substrate, an SOI substrate, or the like can be used as the substrate 901.
[0425] An element isolation layer 902, an insulating layer 905, a dummy gate electrode 908b, and a dummy gate electrode 908c are provided on the substrate 901. The insulating layer 905 functions as a sidewall. In addition, insulating layers 906, 909, 910, 911, 913, 914, 916, 918, and 919 are provided, and these insulating layers function as interlayer insulating films. In addition, insulating layers 909, 911, 914, and 918 function as barrier films. Conductive layers 912, 915, and 917 function as plugs, electrodes, and wiring, respectively.
[0426] One of the sources and drains of the Si transistor 900 (in this case, the low-resistance region 904) is connected to the memory cell 10 via a conductive layer.
[0427] The insulating layers 803 and 804 are provided on the memory cell 10. One or more insulating materials described in the <Insulating Layer> section of Embodiment 1 can be used for the insulating layers such as insulating layer 803 and insulating layer 804. In particular, it is preferable to use an insulating material that has the function of suppressing the permeation of impurities such as hydrogen and oxygen, an insulating material that has the function of capturing or fixing hydrogen, an insulating material that has barrier properties against hydrogen, or an insulating material that has barrier properties against oxygen for insulating layers such as insulating layer 803. It is also preferable to use an insulating material with a lower dielectric constant than high-k material for insulating layers such as insulating layer 804. By using these insulating films, the diffusion of hydrogen into the semiconductor layer 230 of the transistor 200 can be suppressed. Furthermore, the transistor 200 can be made highly reliable.
[0428] The conductive layers 802a, 802b, and 802c are provided so as to be embedded in the insulating layers 191, 193, and 194. The conductive layers such as conductive layers 802a, 802b, and 802c can be formed as single layers or laminates using the materials and configuration described in the <Conductive Layer> of Embodiment 1. For example, conductive layers 802a, 802b, and 802c can be a two-layer structure using tungsten on titanium nitride.
[0429] The conductive layers 805a, 805b, and 805c are provided so as to be embedded in the insulating layer 804. The conductive layers such as conductive layers 805a, 805b, and 805c can be formed as single layers or laminates using the materials and configuration described in the <Conductive Layer> section of Embodiment 1. The conductive layers 805a, 805b, and 805c can be, for example, a two-layer structure using tungsten on titanium nitride. Because highly conductive materials such as tungsten can be used, the wiring resistance of the conductive layers 805a, 805b, and 805c can be reduced. In addition, the conductive layers 805a, 805b, and 805c can also be a three-layer structure of tantalum nitride, titanium nitride, and tungsten from the bottom layer. Alternatively, conductive layers 805a, 805b, and 805c can also be constructed using a four-layer structure consisting of tantalum nitride, tantalum, titanium nitride, and tungsten from the bottom layer.
[0430] The conductive layer 805a is connected to the low-resistance region 904 via conductive layer 802a, conductive layer 167c, conductive layer 240c, conductive layer 917, conductive layer 915, and conductive layer 912. Conductive layer 167c has the same material as conductive layer 167a and conductive layer 167b and can be formed in the same process. Conductive layer 240c has the same material as conductive layer 240a and conductive layer 240b and can be formed in the same process.
[0431] The conductive layer 805b is connected to the conductive layer 242a via the conductive layer 802b, the conductive layer 167a, and the conductive layer 240a. The conductive layer 805c is connected to the conductive layer 192 via the conductive layer 802c.
[0432] The conductive layers 802a, 802b, 802c, 805a, 805b, and 805c each function as a plug or wiring. The conductive layers 805a, 805b, and 805c may also be connected to each other.
[0433] This embodiment can be combined with other embodiments as appropriate. Furthermore, if multiple configuration examples are shown within a single embodiment in this specification, these configuration examples can be combined as appropriate.
[0434] (Embodiment 4) In this embodiment, a semiconductor device 8000 according to one aspect of the present invention will be described. The semiconductor device 8000 can function as a storage device.
[0435] Figure 35 shows a block diagram illustrating an example configuration of the semiconductor device 8000. The semiconductor device 8000 shown in Figure 35 includes a drive circuit 8110 and a memory array 8120. The memory array 8120 has one or more memory cells 8130. Figure 35 shows an example in which the memory array 8120 has multiple memory cells 8130 arranged in a matrix.
[0436] The memory cell 8130 can be a memory device as described in Embodiment 3.
[0437] The drive circuit 8110 includes a PSW 8001 (power switch), a PSW 8002, and a peripheral circuit 8003. The peripheral circuit 8003 includes a peripheral circuit 8004, a control circuit 8005, and a voltage generation circuit 8006.
[0438] In a semiconductor device, each circuit, signal, and voltage can be appropriately selected or omitted as needed. Alternatively, other circuits or signals may be added. Signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are external input signals, and signal RDA is an external output signal. Signal CLK is a clock signal.
[0439] Furthermore, signals BW, CE, and GW are control signals. Signal CE is the chip enable signal, signal GW is the global write enable signal, and signal BW is the byte write enable signal. Signal ADDR is the address signal. Signal WDA is the write data signal, and signal RDA is the read data signal. Signals PON1 and PON2 are power gating control signals. Signals PON1 and PON2 may be generated by the control circuit 8005.
[0440] The control circuit 8005 is a logic circuit that has the function of controlling the overall operation of the semiconductor device 8000. For example, the control circuit 8005 performs a logic operation on signals CE, GW, and BW to determine the operating mode of the semiconductor device 8000 (e.g., write operation, read operation). Alternatively, the control circuit 8005 generates control signals for the peripheral circuit 8004 so that this operating mode is executed.
[0441] The voltage generation circuit 8006 has the function of generating a negative voltage. The signal WAKE has the function of controlling the input of the signal CLK to the voltage generation circuit 8006. For example, when a high-level signal is given as the signal WAKE, the signal CLK is input to the voltage generation circuit 8006, and the voltage generation circuit 8006 generates a negative voltage.
[0442] The peripheral circuit 8004 is a circuit for writing and reading data to and from the memory cell 8130. The peripheral circuit 8004 includes a row decoder 8007, a column decoder 8008, a row driver 8009, a column driver 8010, a sense amplifier 8011, an input circuit 8012, and an output circuit 8013.
[0443] The row decoder 8007 and column decoder 8008 have the function of decoding the ADDR signal. The row decoder 8007 is a circuit for specifying the row to access, and the column decoder 8008 is a circuit for specifying the column to access. The row driver 8009 has the function of selecting the row specified by the row decoder 8007. The column driver 8010 has the function of writing data to the memory cell 8130, reading data from the memory cell 8130, and holding the read data.
[0444] The input circuit 8012 has the function of holding the signal WDA. The data held by the input circuit 8012 is output to the column driver 8010. The output data of the input circuit 8012 is the data (Din) to be written to the memory cell 8130. The data (Dout) read by the column driver 8010 from the memory cell 8130 is output to the output circuit 8013. The output circuit 8013 has the function of holding Dout. The output circuit 8013 also has the function of outputting Dout to the outside of the semiconductor device 8000. The data output from the output circuit 8013 is the signal RDA.
[0445] PSW8001 provides V to peripheral circuit 8003 DD It has the function of controlling the supply. PSW8002 connects to the line driver 8009. HM It has a function to control the supply. Here, the high power supply potential of semiconductor device 8000 is V DD Therefore, the low power supply potential is GND (ground potential). Also, V HM This is a high power supply potential used to raise the word line to a high level, V DD It is higher than that. The on / off state of PSW8001 is controlled by signal PON1, and the on / off state of PSW8002 is controlled by signal PON2. In Figure 35, in peripheral circuit 8003, V DD The number of power domains supplied is set to one, but it can be multiple. In this case, a power switch can be provided for each power domain.
[0446] Using Figures 36A to 36H, other examples of memory cell configurations applicable to the memory cell 8130 will be described.
[0447] [DOSRAM] Figure 36A shows an example of the circuit configuration of a memory cell of a DRAM (Dynamic Random Access Memory). In this specification, a DRAM using an OS transistor is called a DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). The memory cell 8131 has a transistor M1 and a capacitive element CA.
[0448] Transistor M1 may have a front gate (sometimes simply called a gate) and a back gate. In this case, the back gate may be connected to a wire to which a constant potential or signal is supplied, or the front gate and back gate may be connected.
[0449] The first terminal of transistor M1 is connected to the first terminal of capacitive element CA, the second terminal of transistor M1 is connected to wiring BIL, and the gate of transistor M1 is connected to wiring WOL. The second terminal of capacitive element CA is connected to wiring CAL.
[0450] Wiring BIL functions as a bit line, and wiring WOL functions as a word line. Wiring CAL functions as wiring for applying a predetermined potential to the second terminal of the capacitive element CA. When writing and reading data, it is preferable to apply a low-level potential (sometimes called a reference potential) to wiring CAL.
[0451] Data writing and reading are performed by applying a high-level potential to the wiring WOL, turning on transistor M1, and creating a conductive state (a state in which current can flow) between the wiring BIL and the first terminal of the capacitive element CA.
[0452] Furthermore, the memory cell that can be used in memory cell 8130 is not limited to memory cell 8131, and the circuit configuration can be changed. For example, the memory cell 8132 can be configured as shown in Figure 36B. Memory cell 8132 is an example in which there is no capacitive element CA and wiring CAL. The first terminal of transistor M1 is electrically floating.
[0453] In the memory cell 8132, the potential written via transistor M1 is held in the capacitance (also called parasitic capacitance) between the first terminal and the gate, indicated by the dashed line. This configuration significantly simplifies the structure of the memory cell.
[0454] Furthermore, it is preferable to use an OS transistor as transistor M1. OS transistors have the characteristic of having an extremely low off-current. By using an OS transistor as transistor M1, the leakage current of transistor M1 can be made very low. In other words, the written data can be held by transistor M1 for a long time, so the frequency of refreshing the memory cell can be reduced. Alternatively, the refresh operation of the memory cell can be made unnecessary. In addition, because the leakage current is very low, multi-level data or analog data can be held in memory cells 8131 and 8132.
[0455] [NOSRAM] Figure 36C shows an example of a circuit configuration of a gain cell type memory cell with two transistors and one capacitance element. The memory cell 8133 has a transistor M2, a transistor M3, and a capacitance element CB. In this specification, a memory device having a gain cell type memory cell using an OS transistor for transistor M2 is called NOSRAM (Nonvolatil Oxide Semiconductor RAM).
[0456] The first terminal of transistor M2 is connected to the first terminal of capacitive element CB, the second terminal of transistor M2 is connected to wiring WBL, and the gate of transistor M2 is connected to wiring WOL. The second terminal of capacitive element CB is connected to wiring CAL. The first terminal of transistor M3 is connected to wiring RBL, the second terminal of transistor M3 is connected to wiring SL, and the gate of transistor M3 is connected to the first terminal of capacitive element CB.
[0457] Wiring WBL functions as a write bit line, wiring RBL functions as a read bit line, and wiring WOL functions as a word line. Wiring CAL functions as wiring for applying a predetermined potential to the second terminal of the capacitive element CB. When writing data, during data retention, and when reading data, it is preferable to apply a low-level potential (sometimes called a reference potential) to wiring CAL.
[0458] Data writing is performed by applying a high-level potential to the wiring WOL, turning on transistor M2, and creating a conductive state between the wiring WBL and the first terminal of the capacitive element CB. Specifically, when transistor M2 is ON, a potential corresponding to the information to be recorded in the wiring WBL is applied, and this potential is written to the first terminal of the capacitive element CB and the gate of transistor M3. Subsequently, a low-level potential is applied to the wiring WOL, turning off transistor M2, thereby maintaining the potential of the first terminal of the capacitive element CB and the potential of the gate of transistor M3.
[0459] Data is read by applying a predetermined potential to the wiring SL. The current flowing between the source and drain of transistor M3, and the potential of the first terminal of transistor M3, are determined by the potential of the gate and the potential of the second terminal of transistor M3. Therefore, by reading the potential of the wiring RBL connected to the first terminal of transistor M3, the potential held at the first terminal of the capacitive element CB (or the gate of transistor M3) can be read. In other words, the information written to this memory cell can be read from the potential held at the first terminal of the capacitive element CB (or the gate of transistor M3).
[0460] Alternatively, for example, the wiring WBL and wiring RBL may be combined into a single wiring BIL. An example of the circuit configuration of such a memory cell is shown in Figure 36D. Memory cell 8134 is configured such that the wiring WBL and wiring RBL of memory cell 8133 are combined into a single wiring BIL, and the second terminal of transistor M2 and the first terminal of transistor M3 are connected to the wiring BIL. In other words, memory cell 8134 is configured to operate with the write bit line and the read bit line as a single wiring BIL.
[0461] The memory cell 8135 shown in Figure 36E is an example where the capacitive element CB and wiring CAL in memory cell 8133 are omitted. Similarly, the memory cell 8136 shown in Figure 36F is an example where the capacitive element CB and wiring CAL in memory cell 8134 are omitted. By using such a configuration, the integration density of memory cells can be increased.
[0462] Furthermore, it is preferable to use an OS transistor for at least transistor M2. In particular, it is preferable to use OS transistors for transistors M2 and M3.
[0463] Because the OS transistor has the characteristic of having an extremely low off-current, the written data can be held by transistor M2 for a long time, thus reducing the frequency of memory cell refreshes. Alternatively, it may be possible to eliminate the need for memory cell refresh operations altogether. Furthermore, because the leakage current is very low, multi-level data or analog data can be held in memory cells 8133, 8134, 8135, and 8136.
[0464] Memory cells 8133, 8134, 8135, and 8136, which use an OS transistor as transistor M2, represent one embodiment of NOSRAM.
[0465] Furthermore, a Si transistor may be used as transistor M3. Si transistors can increase field-effect mobility and can also be made into p-channel transistors, thus increasing the flexibility of circuit design.
[0466] Furthermore, if an OS transistor is used as transistor M3, the memory cell can be constructed using only n-type transistors.
[0467] Figure 36G also shows a gain cell type memory cell 8137 with three transistors and one capacitance element. The memory cell 8137 has transistors M4 to M6 and a capacitance element CC.
[0468] The first terminal of transistor M4 is connected to the first terminal of capacitive element CC, the second terminal of transistor M4 is connected to wiring BIL, and the gate of transistor M4 is connected to wiring WOL. The second terminal of capacitive element CC is connected to the first terminal of transistor M5 and to wiring GNDL. The second terminal of transistor M5 is connected to the first terminal of transistor M6, and the gate of transistor M5 is connected to the first terminal of capacitive element CC. The second terminal of transistor M6 is connected to wiring BIL, and the gate of transistor M6 is connected to wiring RWL.
[0469] Wiring BIL functions as a bit line, wiring WOL functions as a write word line, and wiring RWL functions as a read word line. Wiring GNDL is a wire that provides a low level potential.
[0470] Data writing is performed by applying a high-level potential to the wiring WOL, turning on transistor M4, and creating a conductive state between the wiring BIL and the first terminal of the capacitive element CC. Specifically, when transistor M4 is ON, a potential corresponding to the information to be recorded in wiring BIL is applied, and this potential is written to the first terminal of the capacitive element CC and the gate of transistor M5. Subsequently, a low-level potential is applied to the wiring WOL, turning off transistor M4, thereby maintaining the potential of the first terminal of the capacitive element CC and the potential of the gate of transistor M5.
[0471] Data is read by precharging the wiring BIL to a predetermined potential, then electrically freezing the wiring BIL, and applying a high-level potential to the wiring RWL. As the wiring RWL reaches a high-level potential, transistor M6 turns ON, and the wiring BIL and the second terminal of transistor M5 become conductive. At this time, the potential of the wiring BIL is applied to the second terminal of transistor M5, but the potential of the second terminal of transistor M5 and the potential of the wiring BIL change depending on the potential held at the first terminal of the capacitive element CC (or the gate of transistor M5). By reading the potential of the wiring BIL, the potential held at the first terminal of the capacitive element CC (or the gate of transistor M5) can be read. In other words, the information written to this memory cell can be read from the potential held at the first terminal of the capacitive element CC (or the gate of transistor M5).
[0472] Furthermore, it is preferable to use an OS transistor for at least transistor M4.
[0473] Note that Si transistors may be used as transistors M5 and M6. As mentioned above, depending on the crystal state of the silicon used in the semiconductor layer, Si transistors may have a higher field-effect mobility than OS transistors.
[0474] Furthermore, if OS transistors are used as transistors M5 and M6, the memory cell can be constructed using only n-type transistors.
[0475] [OS-SRAM] Figure 36H shows an example of SRAM (Static Random Access Memory) using an OS transistor. In this specification, SRAM using an OS transistor is called OS-SRAM (Oxide Semiconductor-SRAM). The memory cell 8138 shown in Figure 36H is a memory cell of a backup-capable SRAM.
[0476] The memory cell 8138 includes transistors M7 to M10, transistors MS1 to MS4, and capacitive elements CD1 and CD2. Transistors MS1 and MS2 are p-channel transistors, while transistors MS3 and MS4 are n-channel transistors.
[0477] The first terminal of transistor M7 is connected to wiring BIL, and the second terminal of transistor M7 is connected to the first terminal of transistor MS1, the first terminal of transistor MS3, the gate of transistor MS2, the gate of transistor MS4, and the first terminal of transistor M10. The gate of transistor M7 is connected to wiring WOL. The first terminal of transistor M8 is connected to wiring BILB, and the second terminal of transistor M8 is connected to the first terminal of transistor MS2, the first terminal of transistor MS4, the gate of transistor MS1, the gate of transistor MS3, and the first terminal of transistor M9. The gate of transistor M8 is connected to wiring WOL.
[0478] The second terminal of transistor MS1 is connected to wiring VDL. The second terminal of transistor MS2 is connected to wiring VDL. The second terminal of transistor MS3 is connected to wiring GNDL. The second terminal of transistor MS4 is connected to wiring GNDL.
[0479] The second terminal of transistor M9 is connected to the first terminal of capacitive element CD1, and the gate of transistor M9 is connected to wiring BRL. The second terminal of transistor M10 is connected to the first terminal of capacitive element CD2, and the gate of transistor M10 is connected to wiring BRL.
[0480] The second terminal of capacitive element CD1 is connected to wiring GNDL, and the second terminal of capacitive element CD2 is connected to wiring GNDL.
[0481] Wires BIL and BILB function as bit lines, wire WOL functions as a word line, and wire BRL controls the on and off states of transistors M9 and M10.
[0482] Wiring VDL is a wiring that provides a high-level potential, and wiring GNDL is a wiring that provides a low-level potential.
[0483] Data is written by applying a high-level potential to the wiring WOL and also to the wiring BRL. Specifically, when transistor M10 is ON, a potential corresponding to the information to be recorded in wiring BIL is applied, and this potential is written to the second terminal side of transistor M10.
[0484] Incidentally, since the memory cell 8138 is configured in an inverter loop by transistors MS1 to MS2, an inverted signal of the data signal corresponding to the potential is input to the second terminal side of transistor M8. Because transistor M8 is ON, the potential applied to wiring BIL, i.e., the inverted signal of the signal input to wiring BIL, is output to wiring BILB. Also, because transistors M9 and M10 are ON, the potential of the second terminal of transistor M7 and the potential of the second terminal of transistor M8 are held at the first terminal of capacitive element CD2 and the first terminal of capacitive element CD1, respectively. Subsequently, by applying a low-level potential to wiring WOL and wiring BRL, and turning off transistors M7 to M10, the potentials of the first terminal of capacitive element CD1 and the first terminal of capacitive element CD2 are maintained.
[0485] The data reading process is described below. First, wiring BIL and wiring BILB are precharged to a predetermined potential. Next, a high-level potential is applied to wiring WOL and wiring BRL. At this time, the potential of the first terminal of capacitive element CD1 is refreshed by the inverter loop of memory cell 8138 and output to wiring BILB. Also, the potential of the first terminal of capacitive element CD2 is refreshed by the inverter loop of memory cell 8138 and output to wiring BIL. In wiring BIL and wiring BILB, the potential changes from the precharged potential to the potential of the first terminal of capacitive element CD2 and the potential of the first terminal of capacitive element CD1, respectively. Therefore, the potential held in the memory cell can be read from the potential of wiring BIL or wiring BILB.
[0486] Furthermore, it is preferable to use OS transistors as transistors M7 to M10. This allows the written data to be retained for a long time by transistors M7 to M10, thereby reducing the frequency of memory cell refreshes, or even eliminating the need for memory cell refresh operations altogether.
[0487] Furthermore, Si transistors may be used as transistors MS1 to MS4.
[0488] Figures 37A and 37C show perspective views of the semiconductor device 8200A. The semiconductor device 8200A has a layer 8220 on which memory arrays are provided on the arithmetic unit 8210. Memory arrays 8120L1, 8120L2, and 8120L3 are provided on layer 8220. The arithmetic unit 8210 and each memory array have overlapping regions. To make the configuration of the semiconductor device 8200A easier to understand, Figure 37B shows the arithmetic unit 8210 and layer 8220 separately. The arithmetic unit 8210 can be, for example, a CPU, GPU, etc.
[0489] By stacking the layer 8220 containing the memory array and the arithmetic unit 8210, the connection distance between them can be shortened. Therefore, the communication speed between them can be increased. In addition, power consumption can be reduced due to the short connection distance.
[0490] As a method for stacking the layer 8220 having a memory array and the arithmetic unit 8210, one may use a method in which the layer 8220 having a memory array is directly stacked on the arithmetic unit 8210 (also called monolithic stacking), or one may use a method in which the arithmetic unit 8210 and the layer 8220 are formed on different substrates, the two substrates are bonded together, and they are connected using through-via or conductive film bonding technology (such as Cu-Cu bonding). The former does not require consideration of positional misalignment during bonding, so not only can the chip size be reduced, but manufacturing costs can also be reduced.
[0491] Here, the arithmetic unit 8210 does not have a cache, and the memory arrays 8120L1, 8120L2, and 8120L3 provided in layer 8220 can each be used as caches. In this case, for example, memory array 8120L1 can be used as an L1 cache (also called a level 1 cache), memory array 8120L2 can be used as an L2 cache (also called a level 2 cache), and memory array 8120L3 can be used as an L3 cache (also called a level 3 cache). Of the three memory arrays, memory array 8120L3 has the largest capacity and the lowest access frequency. Also, memory array 8120L1 has the smallest capacity and the highest access frequency.
[0492] Furthermore, when the cache provided in the arithmetic unit 8210 is used as the L1 cache, each memory array provided in layer 8220 can be used as a lower-level cache or main memory, respectively. Main memory has a larger capacity than cache and is accessed less frequently.
[0493] Furthermore, as shown in Figure 37B, drive circuits 8110L1, 8110L2, and 8110L3 are provided. Drive circuit 8110L1 is connected to memory array 8120L1 via connecting electrode 8230L1. Similarly, drive circuit 8110L2 is connected to memory array 8120L2 via connecting electrode 8230L2, and drive circuit 8110L3 is connected to memory array 8120L3 via connecting electrode 8230L3.
[0494] Note that while this example shows three memory arrays functioning as a cache, it may also use one, two, or four or more arrays.
[0495] When the memory array 8120L1 is used as a cache, the drive circuit 8110L1 may function as part of the cache interface, or the drive circuit 8110L1 may be configured to be connected to the cache interface. Similarly, the drive circuits 8110L2 and 8110L3 may also function as part of the cache interface, or be configured to be connected to it.
[0496] In Figures 37A and 37B, an example is shown in which one layer 8220 on which a memory array is provided is placed on the arithmetic unit 8210. However, as shown in Figure 37C, two or more layers 8220 on which memory arrays are provided may be placed.
[0497] This embodiment can be combined with other embodiments as appropriate. Furthermore, if multiple configuration examples are shown within a single embodiment in this specification, these configuration examples can be combined as appropriate.
[0498] (Embodiment 5) A semiconductor device according to one aspect of the present invention will be described. Figure 38A is a schematic perspective view of a semiconductor device 710 according to one aspect of the present invention. Figure 38B is a schematic perspective view of a part of the semiconductor device 710. Figure 39 is a schematic perspective view illustrating the configuration of the semiconductor device 710.
[0499] In Figures 38A, 38B, and 39, the semiconductor device 710 has an element layer 730 below an element layer 720 which includes a substrate 722 which is a semiconductor substrate, and a support substrate 740 above the element layer 720 via an insulating layer 741. The element layer 720 has a plurality of transistors 721 which constitute a functional circuit 711. The element layer 730 has a plurality of transistors 731 which constitute a switch circuit 715. The transistors 731 function as switches to control the conduction and non-conductivity between an external power supply line and a conductive layer 732 which functions as a power line.
[0500] The transistor exemplified in Embodiment 1 can be used for transistor 731.
[0501] The transistor 721 in element layer 720 is formed on the front side (also called the "first side") of the substrate 722. The element layer 730 is formed on the back side (the side opposite to the front side, also called the "second side") of the substrate 722. Therefore, the transistor 731 in element layer 730 is formed on the second side of the substrate 722.
[0502] In Figure 39, the functional circuit 711 is exemplified as a CPU 712, a GPU 713, and a memory 714.
[0503] Furthermore, the functional circuit 711 is not limited to the CPU 712, GPU 713, and memory 714, and one or more of these can be used. It is also possible to include circuits with functions other than those listed above.
[0504] To improve the operating speed, mounting density, and power consumption of the semiconductor device 710, the functional circuit 711 requires miniaturization and thinning of transistors, wiring, etc., and reduction of the power supply voltage. The switch circuit 715 can control the supply of externally supplied voltage to each circuit of the functional circuit 711, and to stop the supply. This makes it possible to stop the supply of power voltage to circuits in standby mode, thereby reducing power consumption.
[0505] Furthermore, the transistors constituting the switch circuit 715 require high dielectric strength. One effective way to increase the dielectric strength of the transistors is to thicken the gate insulating layer. Thus, transistors 721 and 731 require different performance characteristics. Therefore, different measures are required to improve the characteristics of transistors 721 and 731.
[0506] Furthermore, miniaturization and thinn...
Claims
1. A semiconductor device comprising a semiconductor layer, a first insulating layer, a second insulating layer, a first conductive layer, a second conductive layer, and a third conductive layer, wherein the first conductive layer and the second conductive layer each have a region in contact with the side surface of the semiconductor layer, the first insulating layer is provided on the first conductive layer and the second conductive layer, the first insulating layer has a first opening that at least a portion of which overlaps with the region between the first conductive layer and the second conductive layer, the second insulating layer covers the side surface of the semiconductor layer inside the first opening, the third conductive layer has a region inside the first opening that faces the side surface of the semiconductor layer with the second insulating layer in between, the semiconductor layer has a tapered shape with a taper angle of less than 90°, and in a cross-sectional view in the channel width direction, the height of the semiconductor layer is greater than the width of the bottom surface of the semiconductor layer.
2. The semiconductor device according to claim 1, comprising a fourth conductive layer and a fifth conductive layer, wherein the first insulating layer has a second opening having a region overlapping with the first conductive layer and a third opening having a region overlapping with the second conductive layer, the fourth conductive layer has a region within the second opening that contacts a surface of the first conductive layer along the side surface of the semiconductor layer, and the fifth conductive layer has a region within the third opening that contacts a surface of the second conductive layer along the side surface of the semiconductor layer.
3. The semiconductor device according to claim 1, comprising a fourth conductive layer and a fifth conductive layer, wherein the fourth conductive layer and the fifth conductive layer each have a region in contact with the upper surface of the semiconductor layer, the first conductive layer has a region in contact with the upper surface of the fourth conductive layer, the second conductive layer has a region in contact with the upper surface of the fifth conductive layer, and the sum of the area of the lower surface of the fourth conductive layer and the area of the lower surface of the fifth conductive layer is smaller than the area of the lower surface of the semiconductor layer.
4. The semiconductor device according to claim 3, wherein the side edge of the fourth conductive layer on the first opening side coincides with or substantially coincides with the side edge of the first conductive layer on the first opening side in a plan view, and the side edge of the fifth conductive layer on the first opening side coincides with or substantially coincides with the side edge of the second conductive layer on the first opening side in a plan view.
5. A semiconductor device according to any one of claims 1 to 4, wherein the semiconductor layer comprises indium and oxygen, and the semiconductor layer has a cubic crystal structure.
6. The semiconductor device according to claim 5, wherein the metal oxide layer has a crystal structure, and the semiconductor layer has a region in contact with the upper surface of the metal oxide layer.
7. The semiconductor device according to claim 6, wherein the semiconductor layer comprises a first region, a second region, and a third region, the first region being a region in contact with the upper surface of the metal oxide layer, the second region being a region located closer to the third conductive layer than the first region, the third region including a region overlapping with the third conductive layer, and the length in the channel width direction of the third region of the semiconductor layer being shorter than the length in the channel width direction of the second region of the semiconductor layer.
8. The semiconductor device according to claim 7, wherein the third region has a cross-section in which no grain boundaries are observed in the channel length direction by analysis using a transmission electron microscope.
9. The semiconductor device according to claim 7, wherein the semiconductor layer has crystal grains that overlap with a pair of side edges of the third conductive layer that face each other in the channel length direction.
10. The process comprises first to eleventh steps, wherein in the first step, a metal oxide layer having crystals is formed; in the second step, a first semiconductor film having indium and oxygen is formed so as to cover the metal oxide layer; in the third step, the first semiconductor film is processed to form island-shaped first semiconductor layers; in the fourth step, the first semiconductor layer is subjected to a crystallization process; in the fifth step, a second semiconductor film having indium and oxygen and having a thickness greater than the first semiconductor film is formed so as to cover the first semiconductor layer; in the sixth step, the second semiconductor film is subjected to a crystallization process; in the seventh step, the second semiconductor film is processed to form a second semiconductor layer; in the eighth step, a first conductive layer is formed so as to cover the first semiconductor layer and the second semiconductor layer; and in the ninth step, a first insulating layer is formed on the first conductive layer. In the 10th step, the first insulating layer and the first conductive layer are processed to form a first opening in the first insulating layer having an area overlapping with the first semiconductor layer and the second semiconductor layer, and to form a second conductive layer and a third conductive layer, thereby exposing a part of the side surface of the first semiconductor layer. In the 11th step, a second insulating layer covering the exposed side surface of the first semiconductor layer and a fourth conductive layer on the second insulating layer are formed inside the first opening. In the 3rd step, the first semiconductor layer is formed to have a first region, a second region and a third region, the first region being an area in contact with the upper surface of the metal oxide layer, the second region being an area located closer to the fourth conductive layer than the first region, and the third region including an area overlapping with the fourth conductive layer. A method for manufacturing a semiconductor device, wherein the length in the channel width direction of the third region of the first semiconductor layer is shorter than the length in the channel width direction of the second region of the first semiconductor layer, and in a cross-sectional view in the channel width direction, the height of the second semiconductor layer is greater than the width of the lower surface of the first semiconductor layer.
11. A method for manufacturing a semiconductor device according to claim 10, wherein in the seventh step, a first film is formed on the second semiconductor film, the first film is processed to form a first layer, and then the second semiconductor film is processed using the first layer as a mask.
12. A method for manufacturing a semiconductor device according to claim 11, wherein the first film is formed using a conductive material, and in the 10th step, a region overlapping the first opening of the first layer is removed to form a second layer having a region in contact with the upper surface of the second semiconductor layer and a region in contact with the second conductive layer, and a third layer having a region in contact with the upper surface of the second semiconductor layer and a region in contact with the third conductive layer.
13. A method for manufacturing a semiconductor device according to claim 10, comprising a twelfth step and a thirteenth step, wherein in the twelfth step, a second opening having a region overlapping with the second conductive layer and a third opening having a region overlapping with the third conductive layer are formed to expose at least a portion of the surface of the second conductive layer that is along the side surface of the second semiconductor layer and at least a portion of the surface of the third conductive layer that is along the side surface of the second semiconductor layer, and in the thirteenth step, a fifth conductive layer is formed inside the second opening and a sixth conductive layer is formed inside the third opening.
14. A method for manufacturing a semiconductor device, according to any one of claims 10 to 13, wherein in the seventh step, the second semiconductor film is processed such that the second semiconductor layer has a tapered shape with a taper angle of less than 90°.