Processing method, production method for semiconductor device, processing device, and program

By controlling pressure and sequential substance introduction, the method enhances etching efficiency and reproducibility in semiconductor substrate processing, addressing inefficiencies in existing etching technologies.

WO2026234827A1PCT designated stage Publication Date: 2026-11-12KOKUSAI DENKI KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/022011
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-06-18
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing etching methods for semiconductor substrates are inefficient, lacking a systematic approach to enhance the etching process and achieve uniform and reproducible results.

Method used

A method involving controlled pressure changes and the sequential supply of reactive substances to promote etching reactions, including increasing pressure to adsorb a substance X onto the substrate, followed by reducing pressure and introducing an etching agent to generate etching species for efficient substrate etching.

Benefits of technology

This approach enables efficient and uniform etching of semiconductor substrates by stabilizing the adsorption of reactive substances, ensuring thorough etching without excess consumption, thereby improving etching efficiency and reproducibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2025022011_12112026_PF_FP_ABST
    Figure JP2025022011_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention includes (a) a step for raising the pressure of a space that contains a substrate to a first pressure, (b) a step for supplying a substance X that reacts with an etching agent to promote an etching reaction to the space that contains the substrate, thereby producing a state in which the space that contains the substrate as at the first pressure contains the substance X and causing the substance X to be adsorbed onto the substrate, (c) a step for lowering the pressure of the space that contains the substrate to a second pressure that is lower than the first pressure, and (d) a step for supplying the etching agent to the space that contains the substrate as at a third pressure that is equal to or lower than the second pressure, thereby causing the etching agent to react with the substance X that has been adsorbed onto the substrate to generate an etching species, and using the etching species to etch the surface of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Processing method, method for manufacturing a semiconductor device, processing apparatus, and program

[0001] This disclosure relates to processing methods, methods for manufacturing semiconductor devices, processing apparatuses, and programs.

[0002] As part of the manufacturing process for semiconductor devices, etching of the substrate surface is sometimes performed (see, for example, Patent Document 1).

[0003] Japanese Patent Publication No. 2023-137735

[0004] This disclosure provides a technology that enables efficient etching of the surface of a substrate.

[0005] According to one aspect of the present disclosure, a technology is provided comprising: (a) a step of increasing the pressure of a space containing a substrate to a first pressure; (b) a step of supplying a substance X that reacts with an etching agent to promote an etching reaction to the space containing the substrate, thereby creating a state in which the substance X is present in the space containing the substrate at the first pressure, and adsorbing the substance X onto the substrate; (c) a step of decreasing the pressure of the space containing the substrate to a second pressure lower than the first pressure; and (d) a step of supplying the etching agent to the space containing the substrate at a third pressure lower than or equal to the second pressure, thereby reacting the etching agent with the substance X adsorbed on the substrate to generate etching species, and etching the surface of the substrate using the etching species.

[0006] According to this disclosure, it becomes possible to efficiently etch the surface of a substrate.

[0007] Figure 1 is a schematic diagram of a vertical processing furnace of a processing apparatus preferably used in one embodiment of the present disclosure, showing the processing furnace 202 portion in a vertical cross-sectional view. Figure 2 is a schematic diagram of a vertical processing furnace of a processing apparatus preferably used in one embodiment of the present disclosure, showing the processing furnace 202 portion in a cross-sectional view along line A-A in Figure 1. Figure 3 is a schematic diagram of a controller 121 of a processing apparatus preferably used in one embodiment of the present disclosure, showing the control system of the controller 121 in a block diagram. Figure 4 is a diagram showing the gas supply and pressure control sequence in one embodiment of the present disclosure. Figure 5 is a diagram showing the gas supply and pressure control sequence in another embodiment of the present disclosure. Figure 6 is a diagram showing the gas supply and pressure control sequence in another embodiment of the present disclosure. Figure 7 is a diagram showing the gas supply and pressure control sequence in another embodiment of the present disclosure.

[0008] <An Embodiment of the Disclosure> An embodiment of the disclosure will be described below, mainly with reference to Figures 1 to 4. Note that the drawings used in the following description are schematic, and the dimensional relationships and ratios of the elements shown in the drawings do not necessarily correspond to reality. Furthermore, the dimensional relationships and ratios of the elements do not necessarily correspond between multiple drawings.

[0009] (1) As shown in the configuration diagram 1 of the processing apparatus, the processing furnace 202 of the processing apparatus has a heater 207 as a temperature regulator (heating unit). The heater 207 is cylindrical and is mounted vertically by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) the gas with heat.

[0010] Inside the heater 207, a reaction tube 203 is arranged concentrically with the heater 207. The reaction tube 203 is made of, for example, quartz (SiO₂). 2) or a heat-resistant material such as silicon carbide (SiC), and is formed in a cylindrical shape with a closed upper end and an open lower end. Below the reaction tube 203, a manifold 209 is disposed concentrically with the reaction tube 203. The manifold 209 is made of a metal material such as stainless steel (SUS), and is formed in a cylindrical shape with an open upper end and an open lower end. The upper end portion of the manifold 209 is engaged with the lower end portion of the reaction tube 203, and is configured to support the reaction tube 203. An O-ring 220a serving as a sealing member is provided between the manifold 209 and the reaction tube 203. The reaction tube 203 is installed vertically similarly to the heater 207. A processing container (reaction container) is mainly constituted by the reaction tube 203 and the manifold 209. A processing chamber 201 is formed in the cylindrical hollow portion of the processing container. The processing chamber 201 is configured to be capable of accommodating a wafer 200 serving as a substrate. Processing for the wafer 200 is performed in this processing chamber 201.

[0011] In the processing chamber 201, nozzles 249a to 249c serving as first to third supply units are respectively provided so as to penetrate the side wall of the manifold 209. The nozzles 249a to 249c are also referred to as first to third nozzles, respectively. The nozzles 249a to 249c are made of a heat-resistant material such as quartz or SiC. Gas supply pipes 232a to 232c are connected to the nozzles 249a to 249c, respectively. The nozzles 249a to 249c are different nozzles, and each of the nozzles 249a and 249c is provided adjacent to the nozzle 249b.

[0012] Gas supply pipes 232a to 232c are equipped with mass flow controllers (MFCs) 241a to 241c and valves 243a to 243c, respectively, which are flow control devices (flow control units), starting from the upstream side of the gas flow. Downstream of valve 243a in gas supply pipe 232a, gas supply pipes 232d and 232f are connected, respectively. Downstream of valve 243b in gas supply pipe 232b, gas supply pipes 232e and 232g are connected, respectively. Downstream of valve 243c in gas supply pipe 232c, gas supply pipe 232h is connected. Gas supply pipes 232d to 232h are equipped with MFCs 241d to 241h and valves 243d to 243h, respectively, starting from the upstream side of the gas flow. Gas supply pipes 232a to 232h are made of a metal material such as SUS.

[0013] As shown in Figure 2, the nozzles 249a to 249c are respectively provided in an annular space in plan view between the inner wall of the reaction tube 203 and the wafer 200, along the inner wall of the reaction tube 203 from the lower part to the upper part thereof, so as to rise upward in the arrangement direction of the wafers 200. That is, the nozzles 249a to 249c are respectively provided in a region laterally of the wafer arrangement region where the wafers 200 are arranged, which horizontally surrounds the wafer arrangement region, so as to extend along the wafer arrangement region. In plan view, the nozzle 249b is disposed to face an exhaust port 231a, which will be described later, in a straight line across the center of the wafer 200 in the processing chamber 201. The nozzles 249a and 249c are disposed so as to sandwich a straight line L passing through the centers of the nozzle 249b and the exhaust port 231a from both sides along the inner wall of the reaction tube 203 (the outer peripheral portion of the wafer 200). The straight line L is also a straight line passing through the centers of the nozzle 249b and the wafer 200. That is, it can also be said that the nozzle 249c is provided on the side opposite to the nozzle 249a across the straight line L. The nozzles 249a and 249c are arranged in line symmetry with the straight line L as the axis of symmetry. Gas supply holes 250a to 250c for supplying gas are respectively provided on the side surfaces of the nozzles 249a to 249c. Each of the gas supply holes 250a to 250c is opened so as to face (oppose) the exhaust port 231a in plan view, and is capable of supplying gas toward the wafer 200. A plurality of the gas supply holes 250a to 250c are provided from the lower portion to the upper portion of the reaction tube 203.

[0014] A fluorine (F)-containing substance is supplied from the gas supply pipe 232a into the processing chamber 201 via the MFC 241a, the valve 243a, and the nozzle 249a. The F-containing substance is used as one of etching agents.

[0015] A raw material is supplied from the gas supply pipe 232b into the processing chamber 201 via the MFC 241b, the valve 243b, and the nozzle 249b. The raw material is used as one of film-forming agents.

[0016] From the gas supply pipe 232c, the dopant agent is supplied into the processing chamber 201 via the MFC 241c, valve 243c, and nozzle 249c. The dopant agent is used as one of the film-forming agents.

[0017] From the gas supply pipe 232d, substance X is supplied into the processing chamber 201 via the MFC 241d, valve 243d, gas supply pipe 232a, and nozzle 249a.

[0018] From the gas supply pipe 232e, the reducing agent is supplied into the processing chamber 201 via the MFC 241e, valve 243e, gas supply pipe 232b, and nozzle 249b.

[0019] Inert gas is supplied from gas supply pipes 232f to 232h into the processing chamber 201 via MFCs 241f to 241h, valves 243f to 243h, gas supply pipes 232a to 232c, and nozzles 249a to 249c, respectively. The inert gas acts as a purge gas, carrier gas, diluent gas, etc.

[0020] The F-containing substance supply system is mainly composed of gas supply pipe 232a, MFC 241a, and valve 243a. The raw material supply system is mainly composed of gas supply pipe 232b, MFC 241b, and valve 243b. The dopant agent supply system is mainly composed of gas supply pipe 232c, MFC 241c, and valve 243c. The substance X supply system is mainly composed of gas supply pipe 232d, MFC 241d, and valve 243d. The reducing agent supply system is mainly composed of gas supply pipe 232e, MFC 241e, and valve 243e. The inert gas supply system is mainly composed of gas supply pipes 232f to 232h, MFC 241f to 241h, and valves 243f to 243h. The F-containing substance supply system is also called the etching agent supply system. The raw material supply system and the dopant supply system, either partially or entirely, are also referred to as the film-forming agent supply system. The inert gas supply system is also referred to as the purge gas supply system.

[0021] Of the various supply systems described above, any or all of them may be configured as an integrated supply system 248, which is comprised of valves 243a to 243h and MFCs 241a to 241h. The integrated supply system 248 is connected to each of the gas supply pipes 232a to 232h, and the supply operation of various substances (various gases) into the gas supply pipes 232a to 232h, i.e., the opening and closing operation of valves 243a to 243h and the flow rate adjustment operation by MFCs 241a to 241h, is controlled by a controller 121, which will be described later. The integrated supply system 248 is configured as an integrated or segmented integrated unit, and can be attached to and detached from the gas supply pipes 232a to 232h in units of the integrated unit, and is configured so that maintenance, replacement, and expansion of the integrated supply system 248 can be performed in units of the integrated unit.

[0022] An exhaust port 231a for exhausting the atmosphere inside the processing chamber 201 is provided at the lower part of the side wall of the reaction tube 203. As shown in Figure 2, the exhaust port 231a is located in a position opposite (facing) the nozzles 249a to 249c (gas supply holes 250a to 250c) with the wafer 200 in between, in a plan view. The exhaust port 231a may be provided along the upper part of the side wall of the reaction tube 203, that is, along the wafer arrangement region. An exhaust pipe 231 is connected to the exhaust port 231a. A vacuum pump 246, which is a vacuum exhaust device, is connected to the exhaust pipe 231 via a pressure sensor 245, which is a pressure detector (pressure detection unit) for detecting the pressure inside the processing chamber 201, and an APC (Auto Pressure Controller) valve 244, which is a pressure regulator (pressure adjustment unit). A pressure release system 300 for releasing the pressure inside the processing chamber 201 is further connected to the exhaust pipe 231. The pressure release system 300 is configured to release the pressure inside the processing chamber 201 by releasing the gas inside the processing chamber 201 to the outside of the processing chamber 201 when the pressure inside the processing chamber 201 reaches a predetermined pressure that is equal to or greater than atmospheric pressure. The APC valve 244 can be opened and closed while the vacuum pump 246 is operating to perform vacuum evacuation and stop vacuum evacuation inside the processing chamber 201. Furthermore, while the vacuum pump 246 is operating, the valve opening can be adjusted based on the pressure information detected by the pressure sensor 245 to adjust the pressure inside the processing chamber 201. The exhaust system mainly consists of the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. The vacuum pump 246 and the pressure release system 300 may also be included in the exhaust system.

[0023] Below the manifold 209, a seal cap 219 is provided as a furnace opening cover capable of hermetically closing the lower end opening of the manifold 209. The seal cap 219 is made of a metal material such as SUS and is formed in a disc shape. An O-ring 220b is provided on the upper surface of the seal cap 219 as a sealing member that contacts the lower end of the manifold 209. Below the seal cap 219, a rotating mechanism 267 for rotating the boat 217, which will be described later, is installed. The rotating shaft 255 of the rotating mechanism 267 passes through the seal cap 219 and is connected to the boat 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the boat 217. The seal cap 219 is configured to be raised and lowered vertically by a boat elevator 115, which is installed outside the reaction tube 203 as a lifting mechanism. The boat elevator 115 is configured as a transport device (transport mechanism) that moves the wafer 200 into and out of the processing chamber 201 by raising and lowering the seal cap 219.

[0024] Below the manifold 209, a shutter 219s is provided as a furnace opening cover that can airtightly close the lower end opening of the manifold 209 when the seal cap 219 is lowered and the boat 217 is removed from the processing chamber 201. The shutter 219s is made of a metal material such as SUS and is formed in a disc shape. An O-ring 220c is provided on the upper surface of the shutter 219s as a sealing member that contacts the lower end of the manifold 209. The opening and closing operation of the shutter 219s (such as lifting and lowering or rotating) is controlled by the shutter opening and closing mechanism 115s.

[0025] The boat 217, which serves as a substrate support, is configured to support multiple wafers 200, for example 25 to 200 wafers 200, in a horizontal position and aligned vertically with their centers aligned, in a multi-stage arrangement, that is, arranged with spacing between them. The boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the boat 217, a multi-stage insulation plate 218, also made of a heat-resistant material such as quartz or SiC, is supported.

[0026] A temperature sensor 263 is installed inside the reaction tube 203 as a temperature detector. By adjusting the amount of power supplied to the heater 207 based on the temperature information detected by the temperature sensor 263, the temperature inside the processing chamber 201 is adjusted to the desired temperature distribution. The temperature sensor 263 is installed along the inner wall of the reaction tube 203.

[0027] As shown in Figure 3, the controller 121, which is the control unit (control means), is configured as a computer equipped with a CPU (Central Processing Unit) 121a, RAM (Random Access Memory) 121b, storage device 121c, and I / O port 121d. The RAM 121b, storage device 121c, and I / O port 121d are configured to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122, configured as, for example, a touch panel, is connected to the controller 121. An external storage device 123 can also be connected to the controller 121. The processing unit may be configured to have one control unit or multiple control units. That is, the control for performing the processing sequence described later may be performed using one control unit or using multiple control units. Furthermore, the multiple control units may be configured as a control system connected to each other by a wired or wireless communication network, and the entire control system may perform the control necessary to carry out the processing sequence described later. In this specification, the term "control unit" may refer to a single control unit, a plurality of control units, or a control system composed of a plurality of control units.

[0028] The storage device 121c is composed of, for example, flash memory, HDD (Hard Disk Drive), SSD (Solid State Drive), etc. The storage device 121c contains, in a readable format, control programs that control the operation of the processing device, and process recipes that describe the procedures and conditions for the substrate processing described later. The process recipe functions as a program, combining the procedures in the substrate processing described later so that the controller 121 causes the processing device to execute them and obtain a predetermined result. Hereinafter, process recipes and control programs will be collectively referred to simply as "programs" (program products). Similarly, process recipes will be simply referred to as "recipes." In this specification, the term "program" may include only recipes, only control programs, or both. The RAM 121b is configured as a memory area (work area) where programs and data read by the CPU 121a are temporarily held.

[0029] The I / O port 121d is connected to the MFCs 241a to 241h, valves 243a to 243h, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotary mechanism 267, boat elevator 115, shutter opening / closing mechanism 115s, pressure release system 300, etc.

[0030] The CPU 121a is configured to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to input of operation commands from the input / output device 122. The CPU 121a is configured to control operations such as flow rate adjustment of various substances (various gases) by MFCs 241a to 241h, opening and closing of valves 243a to 243h, opening and closing of APC valve 244 and pressure adjustment operation by APC valve 244 based on pressure sensor 245, starting and stopping of vacuum pump 246, temperature adjustment operation of heater 207 based on temperature sensor 263, rotation and rotation speed adjustment operation of boat 217 by rotation mechanism 267, raising and lowering of boat 217 by boat elevator 115, opening and closing of shutter 219s by shutter opening / closing mechanism 115s, and pressure release operation in processing chamber 201 by pressure release system 300, in accordance with the contents of the read recipe.

[0031] The controller 121 can be configured by installing the above-mentioned program, which is recorded and stored in the external storage device 123, into a computer. The external storage device 123 includes, for example, magnetic disks such as HDDs, optical disks such as CDs, and semiconductor memory such as USB memory and SSDs. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these will be collectively referred to simply as recording media. In this specification, when the term recording media is used, it may include only the storage device 121c, only the external storage device 123, or both. Note that the program may be provided to the computer using communication means such as the Internet or a dedicated line, without using the external storage device 123.

[0032] (2) Processing Process Using the processing apparatus described above, an example of a processing sequence in which a substrate is processed as one step in the manufacturing process (manufacturing method) of a semiconductor device, namely, a process of etching the surface of the wafer 200 as a substrate and a process of growing a film on the wafer 200 after the surface has been etched, will be explained mainly with reference to Figure 4. In the following explanation, the operation of each part constituting the processing apparatus is controlled by the controller 121. The processing apparatus will also be referred to as a substrate processing apparatus, etching processing apparatus, etching apparatus, film deposition processing apparatus, or film deposition apparatus, depending on the processing content. The processing method will also be referred to as a substrate processing method, etching processing method, etching method, film deposition processing method, or film deposition method, depending on the processing content.

[0033] In this embodiment, the processing sequence includes: (a) step A, which increases the pressure of the space where the wafer 200 is located to a first pressure; (b) step B, which involves supplying a substance X that reacts with an etching agent to promote the etching reaction to the space where the wafer 200 is located, thereby creating a state in which the substance X is present in the space where the wafer 200 is located at the first pressure, and adsorbing the substance X onto the wafer 200; (c) step C, which decreases the pressure of the space where the wafer 200 is located to a second pressure lower than the first pressure; and (d) step D, which involves supplying an etching agent to the space where the wafer 200 is located at a third pressure lower than the second pressure, thereby reacting the etching agent with the substance X adsorbed on the wafer 200 to generate etching species, and using these etching species to etch the surface of the wafer 200.

[0034] Here, it is preferable that steps A and B be performed with at least a partial overlap in time. In the following example, we will describe the case in which step B is performed during step A, when the pressure in the space where the wafer 200 is located is being increased to the first pressure, and when the pressure in the space where the wafer 200 is located has reached the first pressure.

[0035] Furthermore, the following example describes a case where, after performing step D, step E is further performed by supplying a film-forming agent to the wafer 200 whose surface has been etched, thereby forming a film on the wafer 200.

[0036] In this specification, the term "wafer" may refer to the wafer itself or to a laminate of a wafer and layers or films formed on its surface. In this specification, the term "surface of the wafer" may refer to the surface of the wafer itself or to the surface of a film or other film formed on the wafer. In this specification, when it is stated that "a film is formed on the surface of the wafer," it may mean that a film is formed directly on the surface of the wafer itself or that a film is formed on a film or other film already formed on the wafer. In this specification, the term "substrate" has the same meaning as when it is used with the term "wafer."

[0037] In this specification, the terms "agent" and "substance" include at least one of gaseous substances and liquid substances. Liquid substances include mist-like substances. That is, each of substance X, etching agent (F-containing substance), reducing agent, and film-forming agent (raw material, dopant agent) may contain a gaseous substance, a liquid substance such as a mist-like substance, or both.

[0038] (Boat Loading) First, multiple wafers 200 are loaded (wafer charging) into the boat 217.

[0039] Oxides may be formed on the surface of wafer 200. These oxides are silicon oxide films (SiO₂) of non-stoichiometric composition. x A film (where x is a real number less than 2) and a silicon oxide film (SiO) of stoichiometric composition. 2 It may contain at least one of the following (films). Furthermore, the oxide may contain at least one of the following: native oxide film and chemical oxide film. x membranes and SiO 2 The film will collectively be referred to as an SiO film below. Oxides may contain elements other than Si and O.

[0040] After the wafer charging is complete, the shutter 219s is moved by the shutter opening / closing mechanism 115s, opening the lower end opening of the manifold 209 (shutter open). Then, as shown in Figure 1, the boat 217 supporting the wafer 200 is lifted by the boat elevator 115 and loaded into the processing chamber 201 (boat loading). In this state, the seal cap 219 seals the lower end of the manifold 209 via the O-ring 220b. With the boat loading complete, the substrate to be processed, i.e., the wafer 200 having oxide on its surface, is prepared (placed) in the processing chamber 201.

[0041] (Temperature Adjustment) After the boat loading is complete, the wafer 200 in the processing chamber 201 is heated by the heater 207 to reach the desired processing temperature. At this time, the amount of power supplied to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263 so that the processing chamber 201 has the desired temperature distribution (temperature adjustment). Also, the rotation of the wafer 200 by the rotation mechanism 267 is started (wafer rotation). Both the temperature adjustment and rotation of the wafer 200 are continued at least until the processing of the wafer 200 is completed. Depending on the processing temperature, it may not be necessary to heat the wafer 200 with the heater 207. The space in which the wafer 200 is located, that is, the space in the processing chamber 201, is also called the processing space.

[0042] (Step A) After temperature adjustment, or in parallel with temperature adjustment, the processing chamber 201, i.e., the space where the wafer 200 is located, is pressurized to a predetermined first pressure. At this time, inert gas is supplied into the processing chamber 201 to raise the pressure inside the processing chamber 201 to the first pressure, and the opening degree of the APC valve 244 is controlled to adjust the amount of exhaust gas from the processing chamber 201.

[0043] Specifically, the valves 243f to 243h are opened, and an inert gas is caused to flow into the gas supply pipes 232f to 232h. The flow rate of the inert gas is adjusted by MFCs 241f to 241h, the inert gas is supplied into the processing chamber 201 via nozzles 249a to 249c, and is exhausted from the exhaust port 231a. At this time, the pressure inside the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information.

[0044] By performing this step, the pressure inside the processing chamber 201 can be gradually increased, and the pressure inside the processing chamber 201 can be made to reach a predetermined first pressure.

[0045] When the first pressure exceeds the atmospheric pressure, step F of temporarily restricting the function of the pressure release system 300 before or during the execution of step A 1 may be further performed. Alternatively, step F of adjusting the threshold pressure at which the pressure release system 300 operates before or during the execution of step A 2 may be further performed. Note that step F 1 includes temporarily disabling (stopping) the function of the pressure release system 300. In addition, step F 2 includes maintaining the function of the pressure release system 300 without disabling (stopping) it, and changing the threshold value at which the system operates. When performing step F 2 , for example, the threshold pressure at which the pressure release system 300 operates is set to a pressure higher than the first pressure. Specifically, for example, when the first pressure is set to 110000 to 140000 Pa, the threshold pressure at which the pressure release system 300 operates can be set to 120000 to 150000 Pa, which is a pressure higher than the first pressure. Step F 1 or step F 2By doing so, the pressure release system 300 can be prevented from being activated in steps A and B. This makes it possible to effectively set the pressure in the processing chamber 201 to a desired pressure that exceeds atmospheric pressure. Furthermore, it is possible to avoid the pressure in the processing chamber 201 falling below the first pressure after it has reached the first pressure, and to effectively maintain the pressure in the processing chamber 201 at the first pressure. Note that step F 1 or step F 2 This only needs to be continued while steps A and B are being performed, and can be canceled (not performed) in subsequent steps, for example, from step D onward.

[0046] Examples of processing conditions when pressurizing the processing chamber 201 in step A include: processing temperature: 25 to 170°C, preferably 25 to 150°C; pressure after pressurization (first pressure): 100,000 to 150,000, preferably 101,325 to 140,000 Pa; processing time: 1 to 20 minutes, preferably 5 to 10 minutes; inert gas supply flow rate (per gas supply pipe): 0.5 to 10 slm, preferably 1 to 5 slm.

[0047] In this specification, numerical ranges such as "25 to 170°C" mean that the lower and upper limits are included within that range. For example, "25 to 170°C" means "25°C or more and 170°C or less." The same applies to other numerical ranges. In this specification, processing temperature means the surface temperature of the object being processed. In this specification, processing pressure means the pressure inside the processing chamber 201. In addition, processing time means the time during which the processing is continued. Furthermore, if the supply flow rate includes 0 slm, 0 slm means the case in which the substance (gas) is not supplied. These also apply in the following explanations.

[0048] Furthermore, if the first pressure is lower than 100,000 Pa, it may become difficult to stably adsorb and fix substance X to the wafer 200 uniformly and firmly in step B, which will be described later. By setting the first pressure to 100,000 Pa or higher, this tendency can be mitigated, making it possible to stably and reproducibly adsorb and fix substance X to the wafer 200 uniformly and firmly in step B. By setting the first pressure to 101,325 Pa or higher, and even higher, by setting the pressure to a pressure exceeding 101,325 Pa, it becomes possible to stably and reproducibly adsorb and fix substance X to the wafer 200 uniformly and firmly in step B.

[0049] Furthermore, if the first pressure is set higher than 150,000 Pa, the time required to reduce the pressure inside the processing chamber 201 to the second pressure in step C, described later, will be longer, which may affect productivity. By setting the first pressure to 150,000 Pa or less, this tendency can be mitigated, making it possible to reduce the time required to reduce the pressure inside the processing chamber 201 to the second pressure in step C to a time that does not affect productivity. By setting the first pressure to 140,000 Pa or less, it is possible to reduce the time required to reduce the pressure inside the processing chamber 201 to the second pressure in step C to a time that has even less impact on productivity.

[0050] Based on these considerations, it is desirable that the first pressure be, for example, 100,000 Pa or more and 150,000 Pa or less, preferably 101,325 Pa or more and 140,000 Pa or less, and more preferably greater than 101,325 Pa and 140,000 Pa or less.

[0051] Furthermore, the higher the first pressure, the greater the amount of saturated water vapor in the processing chamber 201, increasing the amount of substance X present in the processing chamber 201 and making the atmosphere in the processing chamber 201 rich in substance X. As a result, in step B described later, it becomes possible to uniformly and firmly adsorb and fix substance X to the wafer 200 more stably and reproducibly. In this respect, it is desirable that the first pressure be equal to or higher than atmospheric pressure.

[0052] As an inert gas, nitrogen (N2 Other gases such as argon (Ar), helium (He), neon (Ne), and xenon (Xe) can be used. One or more of these can be used as the inert gas. This also applies to each of the steps described later.

[0053] (Step B) In Step B, substance X is supplied into the processing chamber 201 to create a state in which substance X is present in the processing chamber 201 at a first pressure, causing substance X to be adsorbed onto the wafer 200. It is preferable that Step A and Step B overlap at least partially in time. As described above, Figure 4 shows the case in which Step B is performed both during the pressure increase to the first pressure in the processing chamber 201 in Step A, and when the pressure in the processing chamber 201 has reached the first pressure.

[0054] Specifically, valve 243d is opened, and substance X is flowed into the gas supply pipe 232d. The flow rate of substance X is adjusted by MFC 241d and supplied into the processing chamber 201 via nozzle 249a, and exhausted from exhaust port 231a. At this time, substance X is supplied to the wafer 200 from the side of the wafer 200, and the surface of the wafer 200 and the surface of the components in the processing chamber 201 are exposed to substance X (supply and exposure of substance X). At this time, valves 243f to 243h may be opened to supply inert gas into the processing chamber 201 via nozzles 249a to 249c, respectively.

[0055] By performing this step under the processing conditions described later, that is, by supplying substance X to the wafer 200 under the same pressure conditions as in step A, it becomes possible to uniformly and firmly adsorb and fix substance X to the wafer 200. Furthermore, it becomes possible to adsorb substance X to the components in the processing chamber 201, thereby ensuring that substance X is also present in the processing chamber 201.

[0056] After supplying substance X into the processing chamber 201 for a predetermined time, the valve 243d is closed to stop the supply of substance X into the processing chamber 201.

[0057] Examples of processing conditions when supplying substance X in step B include: processing temperature: 25 to 170°C, preferably 25 to 150°C; processing pressure (first pressure): 100,000 to 150,000, preferably 101,325 to 140,000 Pa; processing time: 1 to 20 minutes, preferably 5 to 10 minutes; substance X supply flow rate: 0.5 to 5 slm, preferably 3 to 5 slm; inert gas supply flow rate (per gas supply pipe): 0.5 to 10 slm, preferably 1 to 5 slm.

[0058] Substance X is water vapor (H 2 O) and hydrogen peroxide (H 2 O 2 Hydrogen (H) and oxygen (O)-containing substances (H and O-containing gases) such as ) can be used.

[0059] (Step C) After Step B is completed, the pressure inside the processing chamber 201, i.e., the space where the wafer 200 is located, is reduced to a second pressure lower than the first pressure. At this time, the supply of inert gas to the processing chamber 201 is continued to reduce the pressure inside the processing chamber 201 to the second pressure, and the opening of the APC valve 244 is controlled to adjust the amount of exhaust gas from the processing chamber 201. By performing this step, it is possible to gradually reduce the pressure inside the processing chamber 201 and bring the pressure inside the processing chamber 201 to a predetermined second pressure. It is preferable that the pressure inside the processing chamber 201 does not fall below the third pressure described later between the time Steps A and B are performed and the time Step D described later is performed.

[0060] By performing this step under the processing conditions described later, it becomes possible to remove any excess substance X remaining in the processing chamber 201. Note that performing this step may cause some of the substance X adsorbed onto the wafer 200 and the components in the processing chamber 201 in step B to detach. However, by firmly adsorbing a sufficient amount of substance X onto the wafer 200 and the components in the processing chamber 201 in step B, it becomes possible to retain the amount of substance X necessary to advance the etching reaction in step D, described later, while it remains adsorbed onto the wafer 200 and the components in the processing chamber 201.

[0061] Examples of processing conditions when reducing the pressure inside the processing chamber 201 in step C include: processing temperature: 25 to 170°C, preferably 25 to 150°C; pressure after pressure reduction (second pressure): 100 to 5000, preferably 500 to 3000 Pa; processing time: 1 to 20 minutes, preferably 5 to 10 minutes; inert gas supply flow rate (per gas supply pipe): 0 to 10 slm, preferably 1 to 5 slm.

[0062] The second pressure is preferably lower than atmospheric pressure. Furthermore, the second pressure is preferably higher than the pressure reached when the vacuum pump 246 completely evacuates the processing chamber 201 (the ultimate vacuum pressure), and also higher than the processing pressure (fourth pressure) in step D, which will be described later.

[0063] Furthermore, if the second pressure is set lower than 100 Pa, for example to the vacuum target pressure, a large portion of the substance X adsorbed on the wafer 200 may desorb in step C. By setting the second pressure higher than the vacuum target pressure, preferably to 100 Pa or higher, this tendency can be mitigated, and it is possible to effectively suppress the desorption of a large portion of the substance X adsorbed on the wafer 200 in step C. By setting the second pressure higher than the fourth pressure, preferably to 500 Pa or higher, it is possible to more effectively suppress the desorption of a large portion of the substance X adsorbed on the wafer 200 in step C.

[0064] Furthermore, if the second pressure is set higher than 5000 Pa, for example, to above atmospheric pressure, the time required to bring the pressure inside the processing chamber 201 to the third pressure in step D will be longer, which may affect productivity. By setting the second pressure to a pressure below atmospheric pressure, preferably 5000 Pa or less, this tendency can be mitigated, making it possible to set the time required to bring the pressure inside the processing chamber 201 to the third pressure in step D to a time that does not affect productivity. By setting the second pressure to 3000 Pa or less, and even further to 2000 Pa or less, it is possible to set the time required to bring the pressure inside the processing chamber 201 to the third pressure in step D to a time that has even less impact on productivity.

[0065] For these reasons, it is desirable that the second pressure be higher than the vacuum pressure and the fourth pressure described later, and lower than atmospheric pressure. For example, it is desirable that it be 100 Pa or more and 5000 Pa or less, preferably 500 Pa or more and 3000 Pa or less, and more preferably 500 Pa or more and 2000 Pa or less.

[0066] (Step D) Subsequently, the etching agent is supplied into the processing chamber 201, which is set to a third pressure lower than or equal to the second pressure.

[0067] Specifically, valve 243a is opened and etching agent is flowed into gas supply pipe 232a. The etching agent's flow rate is adjusted by MFC 241a and supplied into processing chamber 201 via nozzle 249a, and exhausted from exhaust port 231a. At this time, etching agent is supplied to the wafer 200 from the side of the wafer 200, and the wafer 200 is exposed to the etching agent (etching agent supply, exposure). At this time, valves 243f to 243h may be opened to supply inert gas into processing chamber 201 via nozzles 249a to 249c, respectively.

[0068] By supplying an etching agent to the wafer 200 under the processing conditions described later, the etching agent reacts with the substance X that was previously adsorbed onto the wafer 200 and the components in the processing chamber 201 in step B, thereby etching the surface of the wafer 200.

[0069] For example, if the oxide on the surface of wafer 200 is silicon oxide (SiO 2 ) containing substance X which has been pre-adsorbed onto the wafer 200 or components in the processing chamber 201, and water (H 2 When the etching agent supplied into the processing chamber 201 contains O) and contains hydrogen fluoride (HF) as an F-containing substance, the reaction shown in the following formula can be carried out under the processing conditions described later. That is, substance X (H 2 Etching species (HF) obtained by reaction of O) and etching agent (HF) 2 - Using such as, an oxide (SiO2) is formed on the surface of the wafer 200. 2 This makes it possible to etch and remove the material.

[0070] 2HF+H 2 O → HF 2 - +H 3 O + SiO 2 +2HF 2 - +2H 3 O + → SiF 4 +4H 2 O

[0071] As described above, according to this disclosure, the oxide (SiO) on the surface of the wafer 200 2 The etching of the wafer is performed using an etching agent (HF) supplied into the processing chamber 201 and a substance X (H) that has been pre-adsorbed onto the wafer 200 and the components in the processing chamber 201. 2 The reaction between O) and can be used as a trigger to start the process. When the etching of the oxide starts, the substance X(H) that has been previously adsorbed onto the wafer 200 or the components in the processing chamber 201 is triggered. 2 O) is consumed.

[0072] However, in the reaction system in step D, water (H) is removed by etching of the oxide. 2 O) is generated. Therefore, in step D, the above reaction is repeated in a chain reaction without supplying additional substance X into the processing chamber 201, making it possible to etch the oxide on the surface of the wafer 200. Note that if additional substance X is supplied into the processing chamber 201 in step D, the amount of substance X in this reaction system becomes excessive, which may actually hinder the progress of the etching reaction.

[0073] As described above, by performing step B, a sufficient amount of substance X can be firmly adsorbed onto the wafer 200 and the components in the processing chamber 201. As a result, when step D is started after step C has been performed, the amount of substance X necessary to advance the etching reaction can be adsorbed onto the wafer 200 and the components in the processing chamber 201 in a substantially uniform amount across the entire arrangement direction of the wafer 200. Therefore, the effect of substance X in promoting the etching reaction is obtained uniformly among the multiple wafers 200 in the processing chamber 201, thereby improving the uniformity of the etching amount on the surface of the wafer 200.

[0074] After etching the surface of the wafer 200, that is, after etching the oxide on the surface of the wafer 200, the valve 243a is closed to stop the supply of the etching agent into the processing chamber 201.

[0075] Examples of processing conditions when supplying the etching agent in step D include: Processing temperature: 25 to 170°C, preferably 25 to 150°C; Processing pressure (third pressure): 100 to 4000, preferably 500 to 2000 Pa; Processing time: 1 to 120 minutes, preferably 10 to 100 minutes; Etching agent supply flow rate: 0.5 to 3 slm, preferably 1 to 2 slm; Inert gas supply flow rate (per gas supply pipe): 0 to 10 slm, preferably 1 to 5 slm.

[0076] The third pressure is preferably lower than atmospheric pressure. Furthermore, it is desirable that the third pressure be higher than the pressure reached when the vacuum pump 246 completely evacuates the processing chamber 201 (the ultimate vacuum pressure), and higher than the processing pressure (fourth pressure) in step D described later.

[0077] Furthermore, if the third pressure is set lower than 100 Pa, for example to the vacuum target pressure, a large portion of the substance X adsorbed on the wafer 200 may desorb in step D. By setting the third pressure higher than the vacuum target pressure, preferably to 100 Pa or higher, this tendency can be mitigated, and it is possible to effectively suppress the desorption of a large portion of the substance X adsorbed on the wafer 200 in step D. By setting the third pressure higher than the fourth pressure, preferably to 500 Pa or higher, it is possible to more effectively suppress the desorption of a large portion of the substance X adsorbed on the wafer 200 in step D.

[0078] Furthermore, if the third pressure is set higher than 4000 Pa, for example, above atmospheric pressure, abnormal etching may occur in step D, damaging the components placed in the processing chamber 201 and generating a large amount of particles. By setting the third pressure to a pressure below atmospheric pressure, preferably 4000 Pa or less, this tendency can be mitigated, and it is possible to effectively suppress abnormal etching in step D, damaging the components placed in the processing chamber 201 and generating a large amount of particles. By setting the third pressure to 2000 Pa or less, it is possible to more effectively suppress abnormal etching in step D, damaging the components placed in the processing chamber 201 and generating a large amount of particles.

[0079] For these reasons, it is desirable that the third pressure be higher than the vacuum pressure and the fourth pressure described later, and lower than atmospheric pressure. For example, it is desirable that it be between 100 Pa and 4000 Pa, and more preferably between 500 Pa and 2000 Pa.

[0080] It is preferable that the third pressure be less than or equal to the second pressure. For example, the third pressure may be set to the same pressure as the second pressure, or it may be set to a lower pressure than the second pressure. Figure 4 shows the case where the third pressure is set to the same pressure as the second pressure.

[0081] Furthermore, while lowering the processing temperature below 25°C (room temperature) can increase the etching rate, if other processes such as film deposition are performed at least before or after the etching process, the time required to change the processing temperature between the etching process and the other process (heating time and / or cooling time) may become too long, potentially reducing productivity. By setting the processing temperature to 25°C or higher, it is possible to maintain a high etching rate while shortening the time required to change the processing temperature between processes, thereby suppressing the decrease in productivity.

[0082] Furthermore, raising the processing temperature above 170°C can significantly reduce the time required to change processing temperatures between processes, but it can also lead to a decrease in productivity due to an excessively low etching rate. By keeping the processing temperature below 170°C, it is possible to suppress the decrease in etching rate while maintaining the significant reduction in processing temperature time between processes, thereby suppressing the decrease in productivity. By keeping the processing temperature below 150°C, it is possible to further suppress the decrease in etching rate while maintaining the significant reduction in processing temperature time between processes, thereby suppressing the decrease in productivity. By keeping the processing temperature below 130°C, it is possible to significantly suppress the decrease in etching rate while maintaining the significant reduction in processing temperature time between processes, thereby suppressing the decrease in productivity.

[0083] Based on these considerations, it is desirable that the processing temperature be 25°C or higher and 170°C or lower, preferably 25°C or higher and 150°C or lower, and more preferably 25°C or higher and 130°C or lower.

[0084] As mentioned above, fluorine-containing substances (fluorine-containing gases) can be used as etching agents, and fluorine-containing substances (fluorine- and fluorine-containing gases) such as HF can be used. In addition, fluorine (F) can be used as an etching agent. 2 ), nitrogen trifluoride (NF 3 ), chlorine trifluoride (ClF 3), F-containing substances (F-containing gases) such as chlorine fluoride (ClF), F and N-containing substances (F and N-containing gases), and F and Cl-containing substances (F and Cl-containing gases) can be used. One or more of these can be used as the etching agent.

[0085] (Reducing agent cycle purging) After step D is completed, cycle purging using a reducing agent is performed.

[0086] Specifically, the valve 243e is opened and closed intermittently to supply a reducing agent to the processing chamber 201 via the nozzle 249b for a predetermined number of times (reducing agent cycle purging). This removes any gaseous substances remaining in the processing chamber 201, thereby maintaining a clean surface for the wafer 200 and the processing chamber 201.

[0087] At this time, an inert gas may be supplied into the processing chamber 201 together with the reducing agent. Alternatively, cycle purging may be performed using the inert gas and / or the reducing agent. When cycle purging is performed in this manner, the purging of the processing chamber 201 by supplying at least one of the inert gas and / or the reducing agent to the processing chamber 201 and the exhaust (vacuum exhaust) of the processing chamber 201 may be performed alternately a predetermined number of times, preferably multiple times. Alternatively, with the processing chamber 201 exhausted, the supply of the reducing agent to the processing chamber 201 and the supply of the inert gas to the processing chamber 201 may be performed alternately a predetermined number of times, preferably multiple times. Alternatively, with the processing chamber 201 exhausted, one of the inert gas and / or the reducing agent may be continuously supplied into the processing chamber 201 while the other of the inert gas and / or the reducing agent is supplied intermittently a predetermined number of times (multiple times).

[0088] Figure 4 shows the case where, after step D is completed, the processing chamber 201 is evacuated, and an inert gas is continuously supplied to the processing chamber 201 while the reducing agent is supplied to the processing chamber 201 intermittently multiple times.

[0089] These measures enable the efficient and effective removal of residual substances from the treatment chamber 201. When an inert gas is used as the purge gas, the treatment chamber 201 is purged primarily by physical action. On the other hand, when a reducing agent is used as the purge gas, not only physical action but also chemical action can be produced, further enhancing the purging effect. When performing cycle purging, the opening and closing of valves 243f to 243h and valve 243e are controlled as appropriate in accordance with the supply timing of the inert gas or reducing agent. Alternatively, instead of cycle purging, a normal purge may be performed by continuously supplying the inert gas or reducing agent into the treatment chamber 201 and exhausting the contents.

[0090] As a reducing agent, hydrogen (H 2 ), deuterium (D 2 ) and other H-containing substances (H-containing gases) or deuterium (D)-containing substances (D-containing gases) can be used. One or more of these can be used as reducing agents. This also applies to each of the steps described later.

[0091] (Reducing agent purging, temperature and pressure adjustment) After the reducing agent cycle purging is completed, the output of the heater 207 is adjusted so that the temperature inside the processing chamber 201 and the wafer 200 reaches the desired processing temperature (temperature adjustment). At this time, the valve 243e is opened and the reducing agent is supplied into the processing chamber 201 via the nozzle 249b (reducing agent purging). This makes it possible to maintain a clean state on the surface of the wafer 200 and inside the processing chamber 201. The pressure inside the processing chamber 201 during the reducing agent cycle purging and reducing agent purging is preferably lower than the third and fourth pressures, for example, it can be 10 to 90 Pa, preferably 10 to 50 Pa.

[0092] When the temperature inside the processing chamber 201 and the wafer 200 approaches or reaches the desired processing temperature, valve 243e is closed to stop the supply of reducing agent into the processing chamber 201. Valves 243f to 243h are opened to supply inert gas into the processing chamber 201 through nozzles 249a to 249c, respectively. In parallel, the opening degree of the APC valve 244 is controlled to adjust the exhaust volume into the processing chamber 201, thereby increasing the pressure inside the processing chamber 201 to a predetermined fourth pressure (pressure adjustment).

[0093] (Step E) After the processing chamber 201 reaches a predetermined processing temperature and stabilizes at a predetermined fourth pressure, the raw material, which is a film-forming agent, is supplied to the wafer 200 whose surface has been etched.

[0094] Specifically, valve 243b is opened and the raw material flows into the gas supply pipe 232b. The flow rate of each raw material is adjusted by MFC 241b and supplied into the processing chamber 201 via nozzle 249b, and exhausted from exhaust port 231a. At this time, the raw material as a film-forming agent is supplied to the wafer 200 from the side of the wafer 200, and the wafer 200 is exposed to the raw material (raw material supply, exposure). At this time, valves 243f to 243h may be opened and inert gas may be supplied into the processing chamber 201 via nozzles 249a to 249c. Alternatively, valve 243e may be opened and a reducing agent may be supplied into the processing chamber 201 via nozzle 249b.

[0095] By supplying raw materials to the wafer 200 under the processing conditions described later, a film of a desired thickness can be formed on the surface of the etched wafer 200. For example, if the surface of the wafer 200 exposed by the etching process is composed of single-crystal Si, and the raw materials and reducing agents described later are used, it becomes possible to grow and form an epitaxial Si film as a film on the surface of the wafer 200. When the reducing agent is supplied to the wafer 200 together with the raw materials, the surface of the wafer 200 and the inside of the processing chamber 201 can be kept clean, allowing for proper epitaxial growth and the formation of a high-purity epitaxial Si film.

[0096] After forming a film of the desired thickness on the surface of the wafer 200, valve 243b is closed to stop the supply of raw materials into the processing chamber 201. If a reducing agent was being supplied to the wafer 200, valve 243e is closed to stop the supply of the reducing agent into the processing chamber 201.

[0097] Examples of processing conditions when supplying raw materials in step E include: Processing temperature: 500 to 650°C, preferably 550 to 600°C Processing pressure (fourth pressure): 4 to 200 Pa, preferably 1 to 120 Pa Processing time: 10 to 120 minutes, preferably 20 to 60 minutes Raw material supply flow rate: 0.1 to 5 slm, preferably 0.2 to 3 slm Reducing agent supply flow rate: 0 to 20 slm, preferably 1 to 10 slm Inert gas supply flow rate (per gas supply pipe): 0 to 10 slm, preferably 0.1 to 5 slm.

[0098] As a raw material, for example, silicon (Si)-containing substances (Si-containing gases) can be used. As a raw material, monochlorosilane (SiH 3 Cl), dichlorosilane (SiH 2 Cl 2 ), trichlorosilane (SiHCl 3 ), tetrachlorosilane (SiCl 4 ), hexachlorodisilane (Si 2 Cl 6 Chlorosilenes such as ) can be used. In addition, monosilane (SiH) can be used as a raw material. 4 ), disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), tetrasilane (Si 4 H 10 Silicon hydride such as ) can be used. One or more of these can be used as raw materials.

[0099] Examples of reducing agents include H 2 , D 2 H-containing substances (H-containing gases) and D-containing substances (D-containing gases) can be used. One or more of these can be used as reducing agents.

[0100] (After-purging and return to atmospheric pressure) After step E is completed, with the processing chamber 201 evacuated, inert gas is supplied to the processing chamber 201 as a purge gas from nozzles 249a to 249c and exhausted from exhaust port 231a. This purges the processing chamber 201, removing any remaining gases and reaction by-products (after-purging). Subsequently, the atmosphere inside the processing chamber 201 is replaced with inert gas (inert gas replacement), and the pressure inside the processing chamber 201 is returned to normal pressure (return to atmospheric pressure).

[0101] (Boat Unloading) The seal cap 219 is then lowered by the boat elevator 115, opening the lower end of the manifold 209. The processed wafers 200, supported by the boat 217, are then unloaded from the lower end of the manifold 209 to the outside of the reaction tube 203 (boat unloading). After boat unloading, the shutter 219s is moved, and the lower end opening of the manifold 209 is sealed by the shutter 219s via the O-ring 220c (shutter closing). After boat unloading, the processed wafers 200 are removed from the boat 217 (wafer discharge).

[0102] The processing step in one aspect of this disclosure is thus completed.

[0103] Furthermore, in this embodiment, steps D and E can be performed continuously in the same processing container (in situ). Performing the series of processes in situ ensures that the wafer 200 is not exposed to the atmosphere during the process, and that stable processing can be performed consistently while the wafer 200 remains under vacuum.

[0104] (3) Effects of this embodiment According to this embodiment, one or more of the following effects can be obtained.

[0105] (a) By performing steps A to D described above, it becomes possible to etch the surface of the substrate efficiently. It also becomes possible to etch the surface of the substrate uniformly. Furthermore, it becomes possible to shorten the total processing time and increase productivity in substrate processing.

[0106] Specifically, by performing steps A to C, substance X can be uniformly and firmly adsorbed and fixed onto the substrate and components within the processing chamber, and furthermore, the uniform adsorption of the required amount of substance X onto the substrate and components within the processing chamber can be maintained.

[0107] This allows etching to begin in step D while maintaining uniform adsorption of the required amount of substance X onto the substrate and components within the processing chamber, that is, while suppressing insufficient adsorption or variation in the amount of substance X adsorbed onto the substrate and components within the processing chamber. As a result, a decrease in the etching rate and variation in the amount of etching can be suppressed, making it possible to efficiently etch the surface of the substrate. Furthermore, it is possible to improve the uniformity of the amount of etching within the substrate surface and the uniformity of the amount of etching between substrates. Moreover, it is possible to suppress damage to components placed in the space where the substrate is located.

[0108] Furthermore, this allows the etching process in step D to be performed at a higher temperature than when the etching process is performed without steps A to C. As a result, it becomes possible to bring the processing temperature in the etching process in step D closer to the processing temperature in the film deposition process in step E. This reduces the time required to change the processing temperature between the etching process and the film deposition process, i.e., the heating time and cooling time. As a result, the total processing time can be reduced, and productivity in substrate processing can be increased.

[0109] (b) The first pressure is set to be equal to or higher than atmospheric pressure, and the second and third pressures are set to be lower than atmospheric pressure. This makes it possible to produce the above-mentioned effects more effectively.

[0110] (c) The second and third pressures are set to pressures higher than the pressure that can be reached when the space containing the substrate is completely vacuumed by the vacuum pump (ultimate vacuum pressure). This makes it possible to produce the above-mentioned effects more effectively.

[0111] (g) After steps A and B are performed, and before step D is performed, ensure that the pressure in the space where the substrate is located does not fall below the third pressure. This effectively suppresses the desorption of much of the substance X adsorbed onto the substrate in step B before step D is performed.

[0112] (h) Steps A and B are performed with at least a partial overlap in time. This makes it possible to effectively adsorb and fix substance X to the substrate uniformly and firmly.

[0113] (i) Step B is performed both during the pressure increase of the space containing the substrate to the first pressure in step A, and when the space containing the substrate has reached the first pressure. This makes it possible to effectively adsorb and fix substance X to the substrate uniformly and firmly.

[0114] (j) In step B, substance X is adsorbed onto the component placed in the space where the substrate is located, and substance X is also present in the space where the substrate is located. As a result, in step D, not only substance X adsorbed on the substrate, but also substance X adsorbed on the component placed in the space where the substrate is located, and substance X present in the space where the substrate is located can be reacted with the etching agent, making it possible to generate a larger number of etching species. As a result, the etching rate can be improved, and etching of the substrate surface can be performed more efficiently.

[0115] (k) The etching agent contains fluorine, and substance X contains H and O. Alternatively, the etching agent contains H and F. In either of these cases, the above-mentioned effects can be produced more effectively.

[0116] (l) In step D, the oxide on the surface of the substrate is etched. The oxide includes a silicon oxide film of stoichiometric or non-stoichiometric composition. The oxide also includes at least one of a native oxide film and a chemical oxide film. In either case, the above-mentioned effects can be produced more effectively.

[0117] (m) In step E, a film-forming agent is supplied to the substrate whose surface has been etched. This allows a film to be formed on the substrate whose surface has been etched and cleaned, and makes it possible to reduce the concentration of impurities (oxygen concentration, etc.) at the interface between the substrate and the film.

[0118] (n) The second pressure in step C and the third pressure in step D are made higher than the fourth pressure in step E. This effectively suppresses the desorption of much of the substance X adsorbed onto the substrate in step B in steps C and D.

[0119] (o) Step F, which temporarily restricts the function of the pressure relief system that releases pressure in the space where the substrate is located, before or during step A, if the first pressure exceeds atmospheric pressure. 1 Further, step F adjusts the pressure threshold at which the pressure relief system that releases pressure in the space where the substrate is located is activated, either before or during step A. 2 This is done. In either of these cases, the pressure release system can be kept from being activated in steps A and B. This makes it possible to effectively raise the pressure in the space where the substrate is located to a desired pressure that exceeds atmospheric pressure. Furthermore, it is possible to avoid the pressure in the space where the substrate is located falling below the first pressure after it has reached the first pressure, and to effectively maintain the pressure in the space where the substrate is located at the first pressure.

[0120] (j) The above-mentioned effects can also be obtained when a predetermined substance is arbitrarily selected from the above-mentioned substances X, etching agents, reducing agents, film-forming agents, and inert gases.

[0121] <Other Aspects of the Disclosure> The aspects of the Disclosure have been described in detail above. However, the Disclosure is not limited to the aspects described above and can be modified in various ways without departing from its essence.

[0122] For example, as shown in Figure 5, step B may be performed only during the pressure increase to the first pressure in the space where the substrate is located in step A, and step B may not be performed once the space where the substrate is located has reached the first pressure.

[0123] Alternatively, as shown in Figure 6, for example, step B may be omitted during step A when the pressure in the space containing the substrate is being increased to the first pressure, and step B may be performed only when the space containing the substrate has reached the first pressure.

[0124] In other words, step B may be performed during the pressure increase of the space containing the substrate to the first pressure in step A, or when the space containing the substrate has reached the first pressure. In these cases as well, steps A and B will overlap at least partially in time, and the same effects as in the above-described embodiment will be obtained.

[0125] Furthermore, as shown in Figure 7, for example, step B is performed both during the pressure increase of the space containing the substrate to the first pressure in step A, and when the space containing the substrate has reached the first pressure, and also during the execution of step C. In other words, steps A and B may be performed with at least a partial overlap in time, and steps C and B may also be performed with at least a partial overlap in time. In this case as well, the same effects as in the above-described embodiment can be obtained.

[0126] Furthermore, in step E, for example, an amorphous Si film, a poly Si film, or a mixed crystalline Si film of amorphous and poly may be formed on the substrate in addition to the epitaxial Si film. That is, in step E, an amorphous film, a polycrystalline film, or a mixed crystalline film of these may be formed on the substrate in addition to the epitaxial film. In these cases as well, the same effects as those of the embodiments described above can be obtained.

[0127] Furthermore, for example, in step E, a dopant agent may be supplied to the substrate as a film-forming agent in addition to the raw materials. The dopant agent can be supplied from the film-forming agent supply system described above. As the dopant agent, a substance containing any of the Group 15 elements such as phosphorus (P) and arsenic (As), and any of the Group 13 elements such as boron (B) can be used. As the dopant agent, phosphine (PH) 3 ), Arsine (Ash 3 ), diborane (B 2 H 6 ), trichloroborane (BCl 3 P-containing substances (P-containing gas), As-containing substances (As-containing gas), and B-containing substances (B-containing gas) can be used. One or more of these can be used as the dopant agent. The same effects as in the above-described embodiment can be obtained in this embodiment as well. Furthermore, according to this embodiment, it is possible to form a dopant-doped film (P, As, B, etc.) on a substrate.

[0128] Furthermore, for example, in step E, a material containing semiconductor elements other than Si may be used to form a semiconductor element-containing film on the substrate. For example, monogermanic (GeH) may be used as a raw material. 4 Alternatively, a germanium (Ge)-containing substance (Ge-containing gas) such as ) may be used to form a Ge-containing film on the substrate. Alternatively, for example, a Si-containing substance and a Ge-containing substance may be used as raw materials to form a Si and Ge-containing film on the substrate. Alternatively, for example, a metal element-containing substance (metal element-containing gas) such as tungsten (W), molybdenum (Mo), aluminum (Al), titanium (Ti), zirconium (Zr), hafnium (Hf), or tantalum (Ta) may be used as raw materials to form a metal element-containing film on the substrate. In these cases as well, the same effects as those described above can be obtained.

[0129] Furthermore, in step E, for example, instead of performing a process to form a film on the substrate, a process to modify the surface of the substrate to a predetermined surface may be performed, or a process to etch the surface of the substrate may be performed. In these cases as well, the same effects as in the embodiments described above can be obtained.

[0130] It is preferable that the recipes used for each process be prepared individually according to the processing content, recorded and stored in the storage device 121c via a telecommunications line or external storage device 123. When starting each process, it is preferable that the CPU 121a appropriately selects the appropriate recipe from among the multiple recipes recorded and stored in the storage device 121c according to the processing content. This allows the processing device to perform various processes with high reproducibility. Furthermore, it reduces the burden on the operator and allows each process to be started quickly while avoiding operational errors.

[0131] The above-mentioned recipes are not limited to newly created ones; they may also be prepared, for example, by modifying existing recipes already installed on the processing unit. When modifying a recipe, the modified recipe may be installed on the processing unit via a telecommunications line or a recording medium on which the recipe is stored. Alternatively, existing recipes already installed on the processing unit may be directly modified by operating the input / output device 122 provided on the existing processing unit.

[0132] The above-described embodiments illustrate an example of processing using a batch-type processing apparatus that processes multiple substrates at once. This disclosure is not limited to the above-described embodiments and can also be applied to processing using a single-wafer processing apparatus that processes one or several substrates at once. Furthermore, the above-described embodiments illustrate an example of processing using a processing apparatus having a hot-wall type processing furnace. This disclosure is not limited to the above-described embodiments and can also be applied to processing using a processing apparatus having a cold-wall type processing furnace.

[0133] Even when using these processing devices, each process can be carried out using the same processing procedures and conditions as described above for the embodiments and modifications, and the same effects as described above for the embodiments and modifications can be obtained.

[0134] The above-described embodiments and modifications can be used in combination as appropriate. The processing procedure and processing conditions in this case can be the same as, for example, the processing procedure and processing conditions of the above-described embodiments and modifications.

[0135] 200 wafers (substrates)

Claims

1. A processing method comprising: (a) a step of increasing the pressure of a space containing a substrate to a first pressure; (b) a step of supplying a substance X that reacts with an etching agent to promote an etching reaction to the space containing the substrate, thereby creating a state in which the substance X is present in the space containing the substrate at the first pressure, and adsorbing the substance X onto the substrate; (c) a step of decreasing the pressure of the space containing the substrate to a second pressure lower than the first pressure; and (d) a step of supplying the etching agent to the space containing the substrate at a third pressure lower than or equal to the second pressure, thereby reacting the etching agent with the substance X adsorbed on the substrate to generate etching species, and etching the surface of the substrate using the etching species.

2. The processing method according to claim 1, wherein the first pressure is set to be equal to or greater than atmospheric pressure, or higher than atmospheric pressure, and the second and third pressures are set to be lower than atmospheric pressure.

3. The processing method according to claim 1, wherein the second pressure and the third pressure are set to pressures higher than the pressure achieved when the space in which the substrate is present is completely vacuumed by the vacuum pump.

4. The processing method according to claim 1, wherein the first pressure is 100,000 Pa or more and 150,000 Pa or less.

5. The processing method according to claim 1, wherein the second pressure is 100 Pa or more and 5000 Pa or less.

6. The processing method according to claim 1, wherein the third pressure is 100 Pa or more and 4000 Pa or less.

7. The processing method according to claim 1, wherein the pressure in the space where the substrate is located does not fall below the third pressure after (a) and (b) and before (d) is performed.

8. The processing method according to claim 1, wherein (a) and (b) are performed with at least a partial overlap in time.

9. The processing method according to claim 1, wherein (b) is performed during the pressurization of the space containing the substrate to the first pressure in (a), and in at least one of the states in which the space containing the substrate has reached the first pressure.

10. (b) The processing method according to claim 1, wherein the substance X is adsorbed onto a member placed in the space where the substrate exists, and the substance X is also present in the space where the substrate exists.

11. The treatment method according to claim 1, wherein the etching agent contains fluorine, and the substance X contains hydrogen and oxygen.

12. The processing method according to claim 11, wherein the etching agent comprises hydrogen and fluorine.

13. (d) The processing method according to claim 1, wherein the oxide on the surface of the substrate is etched.

14. The treatment method according to claim 13, wherein the oxide comprises a silicon oxide film having a stoichiometric or non-stoichiometric composition.

15. The treatment method according to claim 13, wherein the oxide comprises at least one of a native oxide film and a chemical oxide film.

16. (e) The processing method according to any one of claims 1 to 15, further comprising the step of supplying a film-forming agent to the substrate whose surface has been etched to form a film on the substrate.

17. The processing method according to claim 16, wherein the pressure in the space where the substrate is located in (e) is defined as the fourth pressure, and the second pressure and the third pressure are each set higher than the fourth pressure.

18. The processing method according to any one of claims 1 to 15, further comprising the step of temporarily restricting the function of a pressure release system that releases pressure in the space in which the substrate is located, before performing (f)(a).

19. The processing method according to any one of claims 1 to 15, further comprising the step of adjusting the pressure threshold at which a pressure release system for releasing pressure in the space in which the substrate is located is activated, before performing (f)(a).

20. A method for manufacturing a semiconductor device, comprising: (a) a step of increasing the pressure of a space containing a substrate to a first pressure; (b) a step of supplying a substance X that reacts with an etching agent to promote an etching reaction to the space containing the substrate, thereby creating a state in which the substance X is present in the space containing the substrate at the first pressure, and adsorbing the substance X onto the substrate; (c) a step of decreasing the pressure of the space containing the substrate to a second pressure lower than the first pressure; and (d) a step of supplying the etching agent to the space containing the substrate at a third pressure lower than or equal to the second pressure, thereby reacting the etching agent with the substance X adsorbed on the substrate to generate etching species, and etching the surface of the substrate using the etching species.

21. A processing apparatus comprising: a pressure regulator for adjusting the pressure in a space containing a substrate; an etching agent supply system for supplying an etching agent to the space containing the substrate; a substance X supply system for supplying a substance X that reacts with the etching agent to promote an etching reaction to the space containing the substrate; and a control unit configured to control the pressure regulator, the substance X supply system, and the etching agent supply system so as to perform: (a) a process of increasing the pressure in the space containing the substrate containing the substrate to a first pressure; (b) a process of supplying the substance X to the space containing the substrate to create a state in which the substance X is present in the space containing the substrate at the first pressure, thereby adsorbing the substance X onto the substrate; (c) a process of decreasing the pressure in the space containing the substrate to a second pressure lower than the first pressure; and (d) a process of supplying the etching agent to the space containing the substrate at a third pressure lower than the second pressure, thereby reacting the etching agent with the substance X adsorbed on the substrate to generate etching species, and etching the surface of the substrate using the etching species.

22. A program that causes a processing device to execute the following steps via a computer: (a) a step of increasing the pressure of the space in which a substrate is present to a first pressure; (b) a step of supplying a substance X that reacts with an etching agent to promote an etching reaction to the space in which the substrate is present to create a state in which the substance X is present in the space in which the substrate is present at the first pressure, thereby adsorbing the substance X onto the substrate; (c) a step of decreasing the pressure of the space in which the substrate is present to a second pressure lower than the first pressure; and (d) a step of supplying the etching agent to the space in which the substrate is present to a third pressure lower than or equal to the second pressure, thereby reacting the etching agent with the substance X adsorbed on the substrate to generate etching species, and etching the surface of the substrate using the etching species.