Substrate processing method, method for manufacturing semiconductor device, program, and substrate processing device

The method forms oxide layers with varying affinities for substance M, allowing selective etching of specific substances on semiconductor substrates, enhancing manufacturing precision and efficiency.

WO2026234845A1PCT designated stage Publication Date: 2026-11-12KOKUSAI DENKI KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/034194
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-09-26
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing etching technologies struggle to selectively remove specific substances from substrates containing multiple materials, such as silicon oxide and silicon nitride films, during semiconductor manufacturing.

Method used

A substrate processing method involving the formation of oxide layers with different affinities for a substance M, followed by adsorption and reaction with an etching agent to selectively remove the first oxide layer, while leaving the second oxide layer intact.

Benefits of technology

Enables selective etching of specific substances on semiconductor substrates, improving precision and efficiency in semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2025034194_12112026_PF_FP_ABST
    Figure JP2025034194_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a substrate processing method comprising the steps of: (a) obtaining a substrate including an oxide, a non-oxide, a first oxide layer formed on a surface of the oxide, an exposed surface of the first oxide layer having a first end that has a first affinity for a substance M, and a second oxide layer formed on a surface of the non-oxide, an exposed surface of the second oxide layer having a second end that has a second affinity for substance M lower than the first affinity for the substance M; (b) adsorbing the substance M onto the surface of the first oxide layer by exposing the substrate to the substance M ; and (c) removing the first oxide layer and at least part of the oxide, by supplying an etching agent to the substrate and using a reaction product obtained by a reaction between the etching agent and the substance M adsorbed on the surface of the first oxide layer.
Need to check novelty before this filing date? Find Prior Art

Description

Substrate processing method, semiconductor device manufacturing method, program, and substrate processing apparatus.

[0001] This disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a program, and a substrate processing apparatus.

[0002] As part of the manufacturing process for semiconductor devices, etching of the substrate surface is sometimes performed (see, for example, Patent Document 1).

[0003] Japanese Patent Publication No. 2023-137735

[0004] This disclosure provides a technology that enables the selective etching of a specific substance among multiple substances contained in a substrate.

[0005] According to one aspect of the present disclosure, a technology is provided comprising the steps of: (a) providing a substrate comprising an oxide, a non-oxide, a first oxide layer formed on the surface of the oxide and having a first terminus on its exposed surface having a first affinity for substance M, and a second oxide layer formed on the surface of the non-oxide and having a second terminus on its exposed surface having a second affinity for substance M that is lower than the first affinity; (b) exposing the substrate to substance M so that substance M is adsorbed onto the surface of the first oxide layer; and (c) supplying an etching agent to the substrate and removing the first oxide layer and at least a portion of the oxide by a reaction product obtained by the reaction between the etching agent and substance M adsorbed on the surface of the first oxide layer.

[0006] According to this disclosure, it becomes possible to selectively etch a specific substance from among several substances contained in the substrate.

[0007] Figure 1 is a schematic diagram of a substrate processing apparatus 100 preferably used in one embodiment of the present disclosure. Figure 2 is a schematic diagram of the vertical processing furnace of a film processing apparatus 500 included in the substrate processing apparatus 100 preferably used in one embodiment of the present disclosure, and shows the processing furnace 202 portion in a vertical cross-sectional view. Figure 3 is a schematic diagram of the controller 121 of the processing apparatus preferably used in one embodiment of the present disclosure, and shows the control system of the controller 121 in a block diagram. Figure 4(a) is a schematic cross-sectional view showing the surface portion of a wafer 200 in one embodiment of the present disclosure on which oxide X and non-oxide Y are formed. Figure 4(b) is a schematic cross-sectional view showing the surface portion of the wafer 200 after step a1 in step A is performed. Figure 4(c) is a schematic cross-sectional view showing the surface portion of the wafer 200 after step a2 in step A is performed. Figure 4(d) is a schematic cross-sectional view showing the surface portion of the wafer 200 after step B is performed. Figure 4(e) is a schematic cross-sectional view showing the surface portion of the wafer 200 during step C is performed. Figure 4(f) is a schematic cross-sectional view showing the surface portion of wafer 200 after step C has been performed. Figure 4(g) is a schematic cross-sectional view showing the surface portion of wafer 200 after step F has been performed. Figure 4(h) is a schematic cross-sectional view showing the surface portion of wafer 200 after step D has been performed. Figure 4(i) is a schematic cross-sectional view showing the surface portion of wafer 200 during step E has been performed. Figure 4(j) is a schematic cross-sectional view showing the surface portion of wafer 200 after step E has been performed.

[0008] <An Embodiment of the Disclosure> An embodiment of the disclosure will be described below, mainly with reference to Figures 1 to 3 and Figures 4(a) to 4(j). Note that the drawings used in the following description are all schematic, and the dimensional relationships and ratios of the elements shown in the drawings do not necessarily correspond to reality. Furthermore, the dimensional relationships and ratios of the elements do not necessarily correspond between multiple drawings.

[0009] (1) Configuration of the substrate processing apparatus 100 As shown in Figure 1, the substrate processing apparatus 100 mainly comprises a film processing apparatus 500, an exposure apparatus 600, and a transport chamber 700.

[0010] The film processing apparatus 500 is a device that performs film deposition, modification, etching, etc., on the wafer 200 as part of the substrate processing process described later. Depending on the process performed, the film processing apparatus 500 may also be called, for example, a film deposition apparatus, a modification apparatus, or an etching apparatus. The exposure apparatus 600 is a device that performs exposure processing on the wafer 200 as part of the substrate processing process described later. The transport chamber 700 is an area where the wafer 200 is transported between the film processing apparatus 500 and the exposure apparatus 600.

[0011] (i) Configuration of the film processing apparatus 500: As shown in Figure 2, the processing furnace 202 has a heater 207 as a temperature regulator (heating unit). The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) the gas with heat.

[0012] A reaction tube 203 is arranged inside the heater 207, concentrically with the heater 207. The reaction tube 203 is formed in a cylindrical shape with a closed upper end and an open lower end. Below the reaction tube 203, a manifold 209 is arranged concentrically with the reaction tube 203. The processing vessel (reaction vessel) is mainly composed of the reaction tube 203 and the manifold 209. A processing chamber 201 is formed in the hollow cylindrical part of the processing vessel. The processing chamber 201 is configured to accommodate a wafer 200 as a substrate. Processing of the wafer 200 is performed in this processing chamber 201.

[0013] Within the processing chamber 201, nozzles 249a to 249c, which serve as the first to third supply units, are provided so as to penetrate the side walls of the manifold 209. Gas supply pipes 232a to 232c are connected to nozzles 249a to 249c, respectively.

[0014] Gas supply pipes 232a to 232c are equipped with mass flow controllers (MFCs) 241a to 241c and valves 243a to 243c, respectively, in order from the upstream side of the gas flow. Downstream of valve 243a in gas supply pipe 232a, gas supply pipes 232d and 232f are connected, respectively. Downstream of valve 243b in gas supply pipe 232b, gas supply pipes 232e and 232g are connected, respectively. Downstream of valve 243c in gas supply pipe 232c, gas supply pipe 232h is connected. Gas supply pipes 232d to 232h are equipped with MFCs 241d to 241h and valves 243d to 243h, respectively, in order from the upstream side of the gas flow.

[0015] Nozzles 249a to 249c are provided in the space between the inner wall of the reaction tube 203 and the wafer 200, extending from the lower to the upper part of the inner wall of the reaction tube 203, rising upward in the direction of wafer 200 arrangement. Gas supply holes 250a to 250c are provided on the sides of nozzles 249a to 249c, respectively, for supplying gas. Each of the gas supply holes 250a to 250c is capable of supplying gas toward the wafer 200. Multiple gas supply holes 250a to 250c are provided extending from the lower to the upper part of the reaction tube 203.

[0016] From the gas supply pipe 232a, the raw material is supplied into the processing chamber 201 via the MFC 241a, valve 243a, and nozzle 249a. The raw material is used as one of the film-forming agents.

[0017] From the gas supply pipe 232b, the reforming agent is supplied into the processing chamber 201 via the MFC 241b, valve 243b, and nozzle 249b.

[0018] From the gas supply pipe 232c, an oxidizing agent or substance M is supplied into the processing chamber 201 via the MFC 241c, valve 243c, and nozzle 249c. The oxidizing agent is used as one of the film-forming agents.

[0019] Etching agent is supplied from the gas supply pipe 232d into the processing chamber 201 via the MFC 241d, valve 243d, gas supply pipe 232a, and nozzle 249a.

[0020] From the gas supply pipe 232e, the catalyst is supplied into the processing chamber 201 via the MFC 241e, valve 243e, gas supply pipe 232b, and nozzle 249b. The catalyst is used as one of the film-forming agents.

[0021] Inert gas is supplied from gas supply pipes 232f to 232h into the processing chamber 201 via MFCs 241f to 241h, valves 243f to 243h, gas supply pipes 232a to 232c, and nozzles 249a to 249c, respectively. The inert gas acts as a purge gas, carrier gas, diluent gas, etc.

[0022] The raw material supply system is mainly composed of gas supply pipe 232a, MFC 241a, and valve 243a. The reformer supply system is mainly composed of gas supply pipe 232b, MFC 241b, and valve 243b. The oxidizer supply system or substance M supply system is mainly composed of gas supply pipe 232c, MFC 241c, and valve 243c. The etching agent supply system is mainly composed of gas supply pipe 232d, MFC 241d, and valve 243d. The catalyst supply system is mainly composed of gas supply pipe 232e, MFC 241e, and valve 243e. The inert gas supply system is mainly composed of gas supply pipes 232f to 232h, MFCs 241f to 241h, and valves 243f to 243h. Note that nozzles connected to the gas supply pipes that constitute the above-mentioned various supply systems may be included in each of the supply systems.

[0023] An exhaust port 231a for exhausting the atmosphere inside the processing chamber 201 is provided at the lower part of the side wall of the reaction tube 203. An exhaust pipe 231, which serves as an exhaust passage, is connected to the exhaust port 231a. A vacuum pump 246, which serves as a vacuum evacuation device, is connected to the exhaust pipe 231 via a pressure sensor 245, which serves as a pressure detector (pressure detection unit) for detecting the pressure inside the processing chamber 201, and an APC (Auto Pressure Controller) valve 244, which serves as a pressure regulator (pressure adjustment unit). The APC valve 244 can be opened and closed while the vacuum pump 246 is operating to evacuate the processing chamber 201 and stop the vacuum evacuation. Furthermore, while the vacuum pump 246 is operating, the pressure inside the processing chamber 201 can be adjusted by adjusting the valve opening based on the pressure information detected by the pressure sensor 245. The exhaust system mainly consists of the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. The vacuum pump 246 may be included in the exhaust system.

[0024] Below the manifold 209, a seal cap 219 is provided as a furnace opening cover capable of airtightly closing the lower end opening of the manifold 209. Below the seal cap 219, a rotating mechanism 267 for rotating the boat 217 is installed. The rotating shaft 255 of the rotating mechanism 267 is connected to the boat 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the boat 217. The boat elevator 115, which serves as a lifting mechanism, is configured as a transport device (transport mechanism) that moves the seal cap 219 up and down to transport the wafer 200 into and out of the processing chamber 201.

[0025] The boat 217, which serves as a substrate support, is configured to support multiple wafers 200, for example 25 to 200 wafers 200, in a horizontal position and aligned vertically with their centers aligned, in a multi-tiered arrangement, that is, arranged with spacing between them. A multi-tiered insulation plate 218 is supported at the bottom of the boat 217.

[0026] A temperature sensor 263 is installed inside the reaction tube 203 to detect temperature. By adjusting the power supply to the heater 207 based on the temperature information detected by the temperature sensor 263, the temperature inside the processing chamber 201 can be adjusted to the desired temperature distribution.

[0027] (ii) Configuration of the exposure apparatus 600 The exposure apparatus 600 comprises a light source that emits light energy, a photomask held between the light source and the wafer 200, a wafer support stand that supports the wafer 200, and an optical system that irradiates the wafer 200 with light energy via the photomask.

[0028] (iii) Configuration of the transport chamber 700 As shown in Figure 1, the transport chamber 700 is located between the film processing apparatus 500 and the exposure apparatus 600 via gate valves 10a and 10b. A transport mechanism 750 for transporting wafers 200 is provided inside the transport chamber 700. The transport mechanism 750 places the wafer 200 on a substrate mounting part provided on an arm and transports the wafer 200 between the film processing apparatus 500 and the exposure apparatus 600.

[0029] (iv) Control Unit

[0030] As shown in Figure 3, the controller 121, which is the control unit (control means) for the film processing apparatus 500, the exposure apparatus 600, and the transport chamber 700, is configured as a computer equipped with a CPU (Central Processing Unit) 121a, RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, storage device 121c, and I / O port 121d are configured to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122, configured as, for example, a touch panel, is connected to the controller 121. An external storage device 123 can also be connected to the controller 121.

[0031] The storage device 121c is composed of, for example, flash memory, HDD (Hard Disk Drive), SSD (Solid State Drive), etc. The storage device 121c contains, in a readable format, control programs that control the operation of the substrate processing device, and process recipes that describe the procedures and conditions for substrate processing, as described later. The process recipe functions as a program, combining the procedures in the substrate processing described later so that the controller 121 causes the substrate processing device to execute them and obtain a predetermined result. Hereinafter, process recipes and control programs will be collectively referred to simply as "programs" (program products). Similarly, process recipes will be simply referred to as "recipes." In this specification, the term "program" may include only recipes, only control programs, or both. The RAM 121b is configured as a memory area where programs and data read by the CPU 121a are temporarily held.

[0032] The I / O port 121d is connected to the MFCs 241a to 241h, valves 243a to 243h, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotating mechanism 267, boat elevator 115, etc.

[0033] The CPU 121a is configured to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to input of operation commands from the input / output device 122. The CPU 121a is configured to control the flow rate adjustment operation of various substances (various gases) by the MFCs 241a to 241h, the opening and closing operation of valves 243a to 243h, the opening and closing operation of the APC valve 244 and the pressure adjustment operation of the APC valve 244 based on the pressure sensor 245, the starting and stopping of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotating mechanism 267, and the raising and lowering operation of the boat 217 by the boat elevator 115, etc., in accordance with the contents of the read recipe.

[0034] The controller 121 can be configured by installing the above-mentioned program, which is recorded and stored in the external storage device 123, into a computer. The external storage device 123 includes, for example, magnetic disks such as HDDs, optical disks such as CDs, and semiconductor memory such as USB memory and SSDs. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these will be collectively referred to simply as recording media. In this specification, when the term recording media is used, it may include only the storage device 121c, only the external storage device 123, or both. Note that the program may be provided to the computer using communication means such as the Internet or a dedicated line, without using the external storage device 123.

[0035] (2) Substrate Processing Process Using the substrate processing apparatus 100 described above, a method for processing a substrate as one step in the semiconductor device manufacturing process, that is, an example of a processing sequence for selectively etching the surface of the wafer 200 as a substrate, will be explained mainly with reference to Figures 4(a) to 4(j). In the following explanation, the operation of each part constituting the substrate processing apparatus 100 is controlled by the controller 121.

[0036] As shown in Figure 4(a), a non-oxide Y is formed in a predetermined region on the substrate 200a that constitutes the wafer 200, and an oxide X is formed in other regions. In the following, as an example, we will describe a case in which a single-crystal Si substrate (oxygen-free) is formed on the surface of the wafer 200 as the substrate 200a, and a silicon nitride film (SiN film) as the non-oxide Y and a silicon oxide film (SiO film) as the oxide X are formed on the substrate 200a.

[0037] In the processing sequence of this embodiment, (a) step A provides (prepares) a wafer 200 comprising an oxide X, a non-oxide Y, a first oxide layer α1 formed on the surface of the oxide X and having a first end on its exposed surface having a first affinity for substance M, and a second oxide layer α2 formed on the surface of the non-oxide Y and having a second end on its exposed surface having a second affinity for substance M that is lower than the first affinity; (b) step B exposes the wafer 200 to substance M so that substance M is adsorbed onto the surface of the first oxide layer α1; and (c) step C supplies an etching agent to the wafer 200 and removes the first oxide layer α1 and at least a portion of the oxide X by a reaction product obtained by the reaction between the etching agent and substance M adsorbed on the surface of the first oxide layer α1.

[0038] The following example describes the case in which, in step A, raw materials are supplied to a wafer 200 in which the surfaces of oxide X and non-oxide Y are exposed to form a first oxide layer α1 and a second oxide layer α2. More specifically, the case in which oxide layer A (first oxide layer α1 and second oxide layer α2) is formed by executing a predetermined number of cycles (n times, where n is an integer of 1 or more) that include step x1 of supplying raw materials and step x2 of supplying an oxidizing agent to a wafer 200 in which the surfaces of oxide X and non-oxide Y are exposed. More specifically, the case in which raw materials and a catalyst are supplied in step x1, and an oxidizing agent and a catalyst are supplied in step x2 is described.

[0039] Furthermore, in the following example, we will describe a case in which, after performing a predetermined number of cycles including steps x1 and x2 in step A, (a-1) step a1 is performed by supplying a modifier to the first oxide layer α1 and the second oxide layer α2 to form second ends on the exposed surface of the first oxide layer α1 and the exposed surface of the second oxide layer α2, respectively, and (a-2) step a2 is performed after step a1 by selectively exposing the exposed surface of the first oxide layer α1 to convert the second ends on the exposed surface of the first oxide layer α1 to first ends.

[0040] Furthermore, the following example describes the case in which, after step C, step F is performed to convert the second terminator remaining on the exposed surface of the second oxide layer α2 into the first terminator by selectively exposing the exposed surface of the second oxide layer α2.

[0041] Furthermore, the following example describes the case where, after step C (more specifically after step F), step D is performed by exposing the wafer 200 to substance M, thereby adsorbing substance M onto the surface of the second oxide layer α2.

[0042] Furthermore, in the following example, we will describe the case in which, after step D, an etching agent is supplied to the wafer 200, and step E is performed to remove the second oxide layer α2 by the reaction product obtained by the reaction between the etching agent and the substance M adsorbed on the surface of the second oxide layer α2.

[0043] In this embodiment, steps A (steps x1, x2, a1, a2), B, C, F, D, and E, described later, are mainly performed in this order. Steps x1, x2, a1 in step A, steps B, C, D, and E are performed inside the film processing apparatus 500, while steps a2 and F in step A are performed inside the exposure apparatus 600.

[0044] In this specification, the processing sequence described above may also be shown as follows for convenience. The same notation will be used in the following descriptions of variations and other embodiments.

[0045] (Raw material + catalyst → oxidizing agent + catalyst) × n → modifier → lamp light → substance M → etching agent → lamp light → substance M → etching agent

[0046] In this specification, the term "wafer" may refer to the wafer itself or to a laminate of a wafer and a predetermined layer or film formed on its surface. In this specification, the term "surface of the wafer" may refer to the surface of the wafer itself or to the surface of a predetermined layer formed on the wafer. In this specification, when it is stated that "a predetermined layer is formed on the surface of the wafer," it may mean that the predetermined layer is formed directly on the surface of the wafer itself or that the predetermined layer is formed on a layer or other layer already formed on the wafer. In this specification, the term "substrate" has the same meaning as when it is used with the term "wafer."

[0047] As used herein, the term "agent" includes at least one of gaseous substances and liquid substances. Liquid substances include mist-like substances. That is, each of the film-forming agents (raw materials, oxidizing agents, catalysts), modifiers, and etching agents may contain gaseous substances, liquid substances such as mist-like substances, or both.

[0048] As used herein, the term "layer" includes at least one of continuous layers and discontinuous layers. For example, the first oxide layer α1 and the second oxide layer α2 may include continuous layers, discontinuous layers, or both.

[0049] In this specification, when describing the adsorption or reaction of film-forming agents, modifiers, and etching agents to the surface of the wafer 200, it may include not only the mode in which they adsorb or react to the wafer surface while remaining undecomposed, but also the mode in which they decompose or intermediates generated by the detachment of their ligands adsorb or react to the wafer 200 surface.

[0050] In this specification, the term "selectively adsorbing" is not limited to the case where adsorption occurs only to one surface and not to the other. This meaning includes cases where the amount, rate, probability, etc., of adsorption to one surface is relatively larger than the amount, rate, probability, etc., of adsorption to the other surface. In other words, this meaning includes cases where adsorption occurs preferentially to one surface over the other. Similarly, the term "selectively etching" is not limited to the case where etching occurs only to one surface and not to the other. This meaning includes cases where the amount, rate, probability, etc., of etching performed on one surface is relatively larger than the amount, rate, probability, etc., of etching performed on the other surface. In other words, this meaning includes cases where etching is performed preferentially to one surface over the other.

[0051] In the following embodiments, for the sake of explanation, substance M will be water (H 2 Based on examples of applying O), high affinity for substance M is sometimes referred to as "hydrophilicity," low affinity as "hydrophobicity," a treatment to increase affinity as "hydrophilization," and a treatment to decrease affinity as "hydrophobicization." However, substance M in this disclosure is H 2 The terms "hydrophilic," "hydrophobic," "hydrophilization," and "hydrophobicization" are not limited to O, but apply to H as a substance M. 2 This can include the magnitude of affinity when substances other than oxygen are applied, or the equivalent meaning of a treatment that alters affinity.

[0052] (Wafer Charging and Boat Loading) Once multiple wafers 200 are loaded into the boat 217, the boat 217 supporting the multiple wafers 200 is transported into the processing room 201 by the boat elevator 115 (boat loading), as shown in Figure 1.

[0053] (Pressure and Temperature Adjustment) After boat loading is complete, the processing chamber 201, i.e., the space where the wafer 200 is located, is evacuated (reduced pressure exhaust) by the vacuum pump 246 so that it reaches the desired pressure (vacuum level). The wafer 200 in the processing chamber 201 is also heated by the heater 207 so that it reaches the desired processing temperature. The rotation of the wafer 200 by the rotation mechanism 267 is also started. The exhaust of the processing chamber 201, the heating of the wafer 200, and the rotation are all carried out continuously at least until the processing of the wafer 200 is completed.

[0054] Then, steps A, B, C, F, D, and E are performed in order. In step A, steps x1, x2, a1, and a2 are performed in order.

[0055] [Step A] In Step A, first, raw materials and an oxidizing agent are supplied to the wafer 200 in the processing chamber 201, that is, the wafer 200 in which the surfaces of oxide X and non-oxide Y are exposed, and an oxide layer A is formed on the surfaces of oxide X and non-oxide Y. Specifically, step x1 of supplying raw materials and catalyst, and step x2 of supplying oxidizing agent and catalyst are performed sequentially.

[0056] [Step x1] In this step, raw materials and catalyst are supplied to the wafer 200.

[0057] Specifically, valves 243a and 243e are opened, and the raw material and catalyst are flowed into the gas supply pipes 232a and 232e, respectively. The flow rates of the raw material and catalyst are adjusted by MFCs 241a and 241e, respectively, and supplied into the processing chamber 201 via nozzles 249a and 249b, and exhausted from exhaust port 231a. At this time, the raw material and catalyst are supplied to the wafer 200. At this time, valves 243f to 243h may also be opened to supply inert gas into the processing chamber 201 via nozzles 249a to 249c, respectively.

[0058] Examples of processing conditions when supplying raw materials and catalysts in this step include: Processing temperature: room temperature (25°C) to 200°C, preferably room temperature to 150°C, more preferably room temperature to 100°C; Processing pressure: 133 to 1333 Pa; Processing time: 1 to 120 seconds, preferably 1 to 60 seconds; Raw material supply flow rate: 0.001 to 2 slm; Catalyst supply flow rate: 0.001 to 2 slm; Inert gas supply flow rate (per gas supply pipe): 0 to 20 slm.

[0059] In this specification, numerical ranges such as "25 to 200°C" mean that the lower and upper limits are included within that range. For example, "25 to 200°C" means "25°C or more and 200°C or less." The same applies to other numerical ranges. In this specification, processing temperature means the temperature of the wafer 200 or the temperature inside the processing chamber 201, and processing pressure means the pressure inside the processing chamber 201, in other words, the pressure of the space in which the wafer 200 is located. Processing time means the time for which the processing is continued. Also, if the supply flow rate includes 0 slm, 0 slm means the case in which the substance (gas) is not supplied. These also apply in the following explanations.

[0060] By supplying a raw material containing, for example, silicon (Si) to the wafer 200 under the processing conditions described above, a Si-containing layer as a first layer is formed on the surfaces of oxide X and non-oxide Y.

[0061] After forming the first layer on the surfaces of oxide X and non-oxide Y, valves 243a and 243e are closed to stop the supply of raw materials and catalyst to the processing chamber 201, respectively. Then, the processing chamber 201 is evacuated to remove any remaining gaseous substances. At this time, valves 243f to 243h are opened to supply inert gas to the processing chamber 201 via nozzles 249a to 249c. The inert gas supplied from nozzles 249a to 249c acts as a purge gas, thereby purging the processing chamber 201.

[0062] For example, a Si-containing substance can be used as the raw material. Examples of the Si-containing substance include substances containing halogen and Si, that is, halosilanes. Halogens include chlorine (Cl), fluorine (F), bromine (Br), iodine (I) and the like. Examples of the halosilane that can be used include chlorosilane, fluorosilane, bromosilane, iodosilane and the like.

[0063] As the raw material, for example, monochlorosilane (SiH 3 Cl), dichlorosilane (SiH 2 Cl 2 ), trichlorosilane (SiHCl 3 ), tetrachlorosilane (SiCl 4 ), hexachlorodisilane (Si 2 Cl 6 ), octachlorotrisilane (Si 3 Cl 8 ) and other chlorosilanes can be used.

[0064] In addition to these, for example, a substance containing an amino group and Si, that is, aminosilane, can also be used as the raw material.

[0065] As the raw material, for example, tetrakis(dimethylamino)silane (Si[N(CH 3 ) 2 4 ), tris(dimethylamino)silane, bis(diethylamino)silane (Si[N(C 2 H 5 ) 2 2 H 2 ), bis(tert-butylamino)silane (SiH 2 [NH(C 4 H 9 )] 2 ), (diisopropylamino)silane (SiH 3 [N(C 3 H 7 ) 2 ) and other aminosilanes can also be used.

[0066] One or more of these can be used as the raw material. ​​

[0067] As a catalyst, for example, a substance containing an amine compound can be used.

[0068] For example, as a catalyst, pyridine (C 5 H 5 N), aminopyridine (C 5 H 6 N 2 ), picolin (C 6 H 7 N), Lutidine (C 7 H 9 N), pyrimidine (C 4 H 4 N 2 Cyclic amines such as (C) can be used. Also, for example, triethylamine ((C) can be used as a catalyst. 2 H 5 ) 3 N), diethylamine ((C 2 H 5 ) 2 NH), monoethylamine ((C 2 H 5 ) NH 2 ), trimethylamine ((CH 3 ) 3 Chain-like amines such as N) can be used.

[0069] One or more of these can be used as catalysts. This also applies to step x2, which will be described later.

[0070] Examples of inert gases include nitrogen (N 2 Other gases such as argon (Ar), helium (He), neon (Ne), and xenon (Xe) can be used. One or more of these can be used as the inert gas. This also applies to each of the steps described later.

[0071] [Step x2] In this step, an oxidizing agent and a catalyst are supplied to the wafer 200, that is, the wafer 200 on which the first layer is formed on the surface of oxide X and non-oxide Y.

[0072] Specifically, valves 243c and 243e are opened, and the oxidizer and catalyst are flowed into the gas supply pipes 232c and 232e, respectively. The flow rates of the oxidizer and catalyst are adjusted by MFCs 241c and 241e, respectively, and supplied into the processing chamber 201 via nozzles 249c and 249b, and exhausted from the exhaust port 231a. At this time, the oxidizer and catalyst are supplied to the wafer 200. At this time, valves 243f to 243h may also be opened to supply inert gas into the processing chamber 201 via nozzles 249a to 249c, respectively.

[0073] Examples of processing conditions when supplying the oxidizing agent and catalyst in this step include: Processing temperature: room temperature (25°C) to 200°C, preferably room temperature to 150°C, more preferably room temperature to 100°C; Processing pressure: 133 to 1333 Pa; Processing time: 1 to 120 seconds, preferably 1 to 60 seconds; Oxidizing agent supply flow rate: 0.001 to 2 slm; Catalyst supply flow rate: 0.001 to 2 slm; Inert gas supply flow rate (per gas supply pipe): 0 to 20 slm.

[0074] By supplying an oxidizing agent to the wafer 200 under the processing conditions described above, at least a portion of the first layer is oxidized. As a result, a second layer is formed on the surface of oxide X and non-oxide Y, in which the first layer is oxidized and OH terminations are formed on the surface.

[0075] After oxidizing the first layer to transform it into the second layer, valves 243c and 243e are closed to stop the supply of the oxidizer and catalyst to the processing chamber 201, respectively. Then, using a processing procedure similar to the purging in step x1, any gaseous substances remaining in the processing chamber 201 are removed from the processing chamber 201.

[0076] As an oxidizing agent, for example, an oxygen (O)-containing substance can be used. 2 ), ozone (O 3 ), nitrous oxide ( 2 O), nitric oxide (NO), nitrogen dioxide (NO) 2 ), carbon monoxide (CO), carbon dioxide (CO) 2 ) etc. can be used.

[0077] Furthermore, as an oxidizing agent, for example, substances containing oxygen (O) and hydrogen (H) can be used. Examples of gases containing oxygen and hydrogen (H) include water vapor (H). 2 O), hydrogen peroxide (H 2 O 2 ), H 2 and O 2 A mixture of H 2 and O 3 A mixture of the above can be used. That is, as the O and H-containing substance, a mixture of the O-containing substance and the H-containing substance can also be used. In this case, a deuterium (D)-containing substance can also be used instead of the H-containing substance. As the D-containing substance, deuterium (D 2 ) can also be used.

[0078] One or more of these can be used as the oxidizing agent.

[0079] [Performed a predetermined number of times] By performing the above steps x1 and x2 in this order non-simultaneously (which can also be rephrased as alternating or intermittently) for n cycles (where n is 1 or an integer of 2 or more), an oxide layer A with an OH-terminated surface can be formed on the surfaces of oxide X and non-oxide Y formed on the wafer 200 (see Figure 4(b)). For example, when using the above raw materials and oxidizing agent, a SiO layer can be formed as the oxide layer A on the surfaces of oxide X and non-oxide Y. In this embodiment, the oxide layer formed on the surface of oxide X is referred to as the first oxide layer α1, and the oxide layer formed on the surface of non-oxide Y is referred to as the second oxide layer α2 (see Figure 4(b)). It is preferable to repeat the above cycle multiple times. That is, it is preferable to make the thickness of the second layer formed per cycle thinner than the desired film thickness, and to repeat the above cycle multiple times until the thickness of the oxide layer A formed by stacking the second layers reaches the desired thickness.

[0080] [Step a1] In this step, a modifier is supplied to the wafer 200, that is, the wafer 200 in which a first oxide layer α1 is formed on the surface of oxide X and a second oxide layer α2 is formed on the surface of non-oxide Y.

[0081] Specifically, valve 243b is opened, and the reforming agent is allowed to flow into the gas supply pipe 232b. The reforming agent's flow rate is adjusted by MFC 241b, and it is supplied into the processing chamber 201 via nozzle 249b and exhausted from exhaust port 231a. At this time, the reforming agent is supplied to the wafer 200. At this time, valves 243f to 243h may also be opened to supply inert gas into the processing chamber 201 via nozzles 249a to 249c, respectively.

[0082] Examples of processing conditions when supplying the modifier in this step include: Processing temperature: room temperature (25°C) to 200°C, preferably room temperature to 150°C, more preferably room temperature to 100°C; Processing pressure: 5 to 2000 Pa, preferably 10 to 1000 Pa; Processing time: 1 second to 120 minutes, preferably 30 seconds to 60 minutes; Modifier supply flow rate: 0.001 to 3 slm, preferably 0.001 to 0.5 slm; Inert gas supply flow rate (per gas supply pipe): 0 to 20 slm.

[0083] By supplying a modifier to the wafer 200 under the processing conditions described above, the modifier reacts with OH groups (OH terminations), which are adsorption sites present on the surfaces of the first oxide layer α1 and the second oxide layer α2, thereby forming second terminations on the exposed surfaces of the first oxide layer α1 and the second oxide layer α2 (see Figure 4(b)). For example, if the modifier contains atoms of a predetermined element and hydrocarbon groups bonded to these atoms, these atoms and the hydrocarbon groups bonded to them chemically adsorb onto the OH groups present on the surfaces of the first oxide layer α1 and the second oxide layer α2, terminating the surfaces with hydrocarbon groups. As a result, the surfaces of the first oxide layer α1 and the second oxide layer α2 become hydrophobic. If the hydrocarbon group contained in the modifier is a methyl group, then methyl group terminations are formed as second terminations on the surfaces of the first oxide layer α1 and the second oxide layer α2. In this way, the surface of the wafer 200 is hydrophobic via oxide layer A (first oxide layer α1 and second oxide layer α2).

[0084] (After-purging and return to atmospheric pressure) After forming the second termination on the exposed surfaces of the first oxide layer α1 and the second oxide layer α2, the valve 243b is closed to stop the supply of the modifier into the treatment chamber 201. Then, using the same treatment procedure as in step x1, any remaining gaseous substances in the treatment chamber 201 are removed from the treatment chamber 201. After that, the atmosphere in the treatment chamber 201 is replaced with an inert gas, and the pressure in the treatment chamber 201 is returned to atmospheric pressure.

[0085] (Boat unloading and wafer discharge) The seal cap 219 is then lowered by the boat elevator 115, and the lower end of the manifold 209 is opened. The wafer 200 is then discharged from the lower end of the manifold 209 to the outside of the reaction tube 203. After the wafer 200 has been discharged to the outside of the reaction tube 203, it is removed from the boat 217 by the transport mechanism 750.

[0086] The wafer 200, removed from the boat 217 by the transport mechanism 750, is placed on a mounting table located inside the exposure apparatus 600 via the transport chamber 700.

[0087] As a modifier, it is preferable to use a compound represented by the following formula 1.

[0088] [R 11 ]n 1 - (X 1 ) - [R 12 ]m 1 : Equation 1 In Equation 1 above, R 11 is X 1 Represents the first substituent directly bonded to R, 12 is X 1 This represents a second substituent directly bonded to X 1 n represents a tetravalent atom selected from the group containing carbon (C) atoms, Si atoms, germanium (Ge) atoms, and tetravalent metal atoms, 1 represents an integer from 1 to 3, and m 1 represents an integer between 1 and 3, and n 1 +m 1 = 4. Examples of tetravalent metal atoms include titanium (Ti), zirconium (Zr), hafnium (Hf), molybdenum (Mo), and tungsten (W).

[0089] In Formula 1, R which is the first substituent 11 , that is, the number of n 1 is an integer of 1 to 3, more preferably 2 or 3. When n 1 is 2 or 3, R as the first substituent 11 may each be the same or different.

[0090] R 11 The first substituent represented by is preferably a hydrocarbon group, a hydrogen group (-H), an alkoxy group, a fluoro group, or a fluoroalkyl group. Among them, as the first substituent represented by R 11 , a hydrogen group and a hydrocarbon group are preferable, and a hydrocarbon group is particularly preferable. Here, the hydrocarbon group may be an aliphatic hydrocarbon group such as an alkyl group, an alkenyl group, or an alkynyl group, or may be an aromatic hydrocarbon group.

[0091] The alkyl group as a partial structure in the hydrocarbon group and the alkoxy group as the first substituent is preferably an alkyl group having 1 to 4 carbon atoms. The alkyl group may be linear or branched.

[0092] In Formula 1, R which is the second substituent 12 , that is, the number of m 1 is an integer of 1 to 3, more preferably 1 or 2. When m 1 is 2 or 3, R as the second substituent 12 may each be the same or different.

[0093] R 12 The second substituent represented by is preferably a substituent that enables chemisorption of the modifier to adsorption sites (for example, OH termination) on the surface of the oxide layer A.

[0094] R 12 Examples of the second substituent represented by include an amino group, a chloro group, a bromo group, an iodo group, a hydroxy group, and the like. Among them, R 12As the second substituent represented by , an amino group is preferable, and a substituted amino group is more preferable. In particular, from the viewpoint of the adsorptivity of the modifier to the oxide layer A, R 12 It is preferable that all of the second substituents represented by are substituted amino groups.

[0095] The substituent that the substituted amino group has is preferably an alkyl group, more preferably an alkyl group having 1 to 5 carbon atoms, and particularly preferably an alkyl group having 1 to 4 carbon atoms. The alkyl group contained in the substituted amino group may be linear or branched. The number of substituents that the substituted amino group has is 1 or 2, and preferably 2.

[0096] X 1 The atom to which the first substituent and the second substituent represented by are directly bonded is preferably a C atom, a Si atom, or a Ge atom. This is because when X 1 is any one of a C atom, a Si atom, and a Ge atom, at least one of the properties selected from high adsorptivity of the modifier to the surface of the oxide layer A, and high chemical stability of the modifier after adsorption to the surface of the oxide layer A, that is, the residue derived from the modifier, can be obtained. Further, as X 1 , a Si atom is more preferable. This is because when X 1 is a Si atom, both properties of high adsorptivity of the modifier to the surface of the oxide layer A and high chemical stability of the modifier after adsorption to the surface of the oxide layer A, that is, the residue derived from the modifier, can be obtained in a well-balanced manner.

[0097] The compound represented by Formula 1 has been described above, but the modifier is not limited to the compound represented by Formula 1. For example, the atom to which the first substituent and the second substituent are directly bonded may be a metal atom capable of bonding to 5 or more ligands. The modifier may be composed of a molecule including the aforementioned first substituent, the aforementioned second substituent, and two or more atoms to which the first substituent and the second substituent are directly bonded.

[0098] Specific examples of the modifier include (dimethylamino)trimethylsilane: (CH 3 ) 2 NSi(CH 3 )3 (Ethylamino)trimethylsilane: (C 2 H 5 ) HNSi (CH 3 ) 3 (Propylamino)trimethylsilane: (C 3 H 7 ) 2 HNSi(CH 3 ) 3 , (butylamino)trimethylsilane: (C 4 H 9 ) 2 HNSi(CH 3 ) 3 (Diethylamino)trimethylsilane: (C 2 H 5 ) 2 NSi(CH 3 ) 3 (Dipropylamino)trimethylsilane: (C 3 H 7 ) 2 NSi(CH 3 ) 3 (Dibutylamino)trimethylsilane: (C 3 H 7 ) 2 NSi(CH 3 ) 3 (dimethylamino)dimethylsilane: (CH 3 ) 2 NSiH(CH 3 ) 2 (Ethylamino)dimethylsilane: (C 2 H 5 )HNSiH(CH 3 ) 2 , (propylamino)dimethylsilane: (C 3 H 7 ) 2 HNSiH(CH 3 ) 2 (Butylamino)dimethylsilane: (C 4 H 9 ) 2 HNSiH(CH 3 ) 2 (Diethylamino)dimethylsilane: (C 2 H 5 ) 2 NSiH(CH3 ) 2 (Dipropylamino)dimethylsilane: (C 3 H 7 ) 2 NSiH(CH 3 ) 2 (Dibutylamino)dimethylsilane: (C 3 H 7 ) 2 NSiH(CH 3 ) 2 (dimethylamino)methylsilane: (CH 3 ) 2 NSiH 2 (CH 3 ), (diethylamino)methylsilane: (C 2 H 5 ) 2 NSiH 2 (CH 3 ), (dipropylamino)methylsilane: (C 3 H 7 ) 2 NSiH 2 (CH 3 ), (dibutylamino)methylsilane: (C 3 H 7 ) 2 NSiH 2 (CH 3 ), (dimethylamino)diethylsilane: (CH 3 ) 2 NSiH(C 2 H 5 ) 2 (Diethylamino)diethylsilane: (C 2 H 5 ) 2 NSiH(C 2 H 5 ) 2 (Dipropylamino)diethylsilane: (C 3 H 7 ) 2 NSiH(C 2 H 5 ) 2 (Dibutylamino)diethylsilane: (C 3 H 7 ) 2 NSiH(C 2 H 5 ) 2(dimethylamino)ethylsilane: (CH 3 ) 2 NSiH 2 (C 2 H 5 ), (diethylamino)ethylsilane: (C 2 H 5 ) 2 NSiH 2 (C 2 H 5 ), (dipropylamino)ethylsilane: (C 3 H 7 ) 2 NSiH 2 (C 2 H 5 ), (dibutylamino)ethylsilane: (C 3 H 7 ) 2 NSiH 2 (C 2 H 5 ), (dipropylamino)silane: [(C 3 H 7 ) 2 N] SiH 3 , (dibutylamino)silane: [(C 4 H 9 ) 2 N] SiH 3 , bis(dimethylamino)dimethylsilane: [(CH 3 ) 2 N] 2 Si(CH 3 ) 2 , bis(ethylamino)dimethylsilane: [(C 2 H 5 ) HN] 2 Si(CH 3 ) 2 , bis(propylamino)dimethylsilane: [(C 3 H 7 ) 2 [HN] 2 Si(CH 3 ) 2 , bis(butylamino)dimethylsilane: [(C 4 H 9 ) 2 [HN] 2 Si(CH 3 ) 2, bis(diethylamino)dimethylsilane: [(C 2 H 5 ) 2 N] 2 Si(CH 3 ) 2 , bis(dipropylamino)dimethylsilane: [(C 3 H 7 ) 2 N] 2 Si(CH 3 ) 2 , bis(dibutylamino)dimethylsilane: [(C 3 H 7 ) 2 N] 2 Si(CH 3 ) 2 , bis(dimethylamino)methylsilane: [(CH 3 ) 2 N] 2 SiH(CH 3 ), bis(ethylamino)methylsilane: [(C 2 H 5 ) HN] 2 SiH(CH 3 ), bis(propylamino)methylsilane: [(C 3 H 7 ) 2 [HN] 2 SiH(CH 3 ), bis(butylamino)methylsilane: [(C 4 H 9 ) 2 [HN] 2 SiH(CH 3 ), bis(diethylamino)methylsilane: [(C 2 H 5 ) 2 N] 2 SiH(CH 3 ), (dimethylamino)trimethoxysilane: (CH 3 ) 2 NSi(OCH) 3 ) 3、 (Dimethylamino)triethoxysilane: (CH 3 ) 2 NSi(OC 2 H 5 ) 3、(Dimethylamino)triprotoxysilane: (CH 3 ) 2 NSi(OC 3 H 7 ) 3、 (Dimethylamino)tributotoxylane: (CH 3 ) 2 NSi(OC 4 H 9 ) 3 Examples of aminosilane-based substances include the following. One or more of these can be used as a modifier.

[0099] In step a1, the first substituent mainly adsorbs onto the surface of oxide layer A, thereby constituting at least a portion of the hydrophobic termination. However, the hydrophobic termination formed on the surface of oxide layer A may consist of only a portion of the first substituent, or it may also consist of other atoms.

[0100] [Step a2] In this step, exposure is performed on the wafer 200 in the exposure apparatus 600, that is, the wafer 200 in which the second termination has been formed on the exposed surface of the first oxide layer α1 and the second oxide layer α2. Specifically, the wafer 200 placed on the mounting table is moved to the wafer support using a moving mechanism provided in the exposure apparatus 600, and then a photomask is placed on the wafer 200 so as to face the light source. After that, light energy is irradiated from the light source onto the wafer 200 through the photomask. By selectively irradiating (exposing) the exposed surface of the first oxide layer α1 with light energy through the photomask, the second termination that had been formed on the exposed surface of the first oxide layer α1 is converted into a first termination (see Figure 4(c)).

[0101] In this specification, the first terminal is a terminal having a first affinity for substance M supplied in step B described later, and the second terminal is a terminal having a second affinity for substance M that is lower than the first affinity. For example, if substance M is H 2If the value is O, the surface of the first oxide layer α1 is hydrophilized by selectively exposing the exposed surface of the first oxide layer α1 in step a2. If the second terminus formed on the surface of the first oxide layer α1 is a methyl group terminus, two hydrogen atoms are removed from this methyl group terminus, and it is converted into a CH terminus (hydrophilic terminus) as the first terminus.

[0102] The light energy irradiated onto the wafer 200 is not particularly limited as long as it can make the hydrophobic surface hydrophilic, and for example, ultraviolet light, electron beams, etc. can be used. Of the light energy, vacuum ultraviolet light is preferred.

[0103] The wavelength of the light energy can be any wavelength that can make the hydrophobic surface hydrophilic, and is appropriately selected depending on the type of material of the hydrophobic layer (specifically, the first oxide layer α1 on which a second term is formed on the surface). Typically, it is preferably 100 nm to 250 nm, and more preferably 150 nm to 200 nm.

[0104] Examples of light energy include lamp light emitted from excimer lamps, low-mercury lamps, and the like, which are used as light sources.

[0105] The same points regarding light energy will be discussed in step F, which will be described later.

[0106] After converting the second end formed on the exposed surface of the first oxide layer α1 to the first end, the moving mechanism moves the wafer 200 from the wafer support to the mounting table inside the exposure apparatus 600. The transport mechanism 750 carries the wafer 200 placed on the mounting table out of the exposure apparatus 600, and loads it into the boat 217 via the transport chamber 700.

[0107] (Wafer charging and boat loading) Subsequently, the wafers 200 are loaded into the boat 217 using the same procedure as described above for wafer charging and boat loading, and then transported into the processing room 201.

[0108] (Pressure and temperature adjustment) Subsequently, the pressure and temperature inside the processing chamber 201 are adjusted using the same procedure as described above for pressure and temperature adjustment.

[0109] [Step B] In this step, substance M is supplied to the wafer 200 in the processing chamber 201, that is, the wafer 200 in which the second termination formed on the exposed surface of the first oxide layer α1 has been converted to the first termination.

[0110] Specifically, valve 243c is opened and substance M is flowed into gas supply pipe 232c. The flow rate of substance M is adjusted by MFC 241c and supplied into processing chamber 201 via nozzle 249c, and exhausted from exhaust port 231a. At this time, substance M is supplied to wafer 200, and wafer 200 is exposed to substance M (supply of substance M, exposure). At this time, valves 243f to 243h may be opened to supply inert gas into processing chamber 201 via nozzles 249a to 249c, respectively.

[0111] Examples of processing conditions when supplying substance M in this step include: Processing temperature: room temperature (25°C) to 200°C, preferably room temperature to 150°C, more preferably room temperature to 100°C; Processing pressure: 5 to 2000 Pa, preferably 10 to 1000 Pa; Processing time: 0.1 to 120 minutes, preferably 1 to 60 minutes; Supply flow rate of substance M: 0.01 to 20 slm, preferably 0.01 to 10 slm; Inert gas supply flow rate (per gas supply pipe): 0 to 20 slm, preferably 0 to 10 slm.

[0112] Under the processing conditions described above, by supplying (exposing) the wafer 200 to substance M, substance M can be selectively adsorbed onto the surface of the first oxide layer α1 (see Figure 4(d)). This is because the first termination formed on the surface of the first oxide layer α1 has a higher affinity for substance M than the second termination formed on the surface of the second oxide layer α2.

[0113] The substance M adsorbed onto the surface of the first oxide layer α1 reacts with the etching agent supplied into the processing chamber 201 in step C, described later, to produce a predetermined reaction product (etching species), thereby promoting the etching reaction on the surface of the first oxide layer α1. In other words, the substance M adsorbed onto the first oxide layer α1 functions as a reaction promoter that accelerates the etching reaction carried out in step C.

[0114] After selectively adsorbing substance M onto the surface of the first oxide layer α1, the valve 243c is closed to stop the supply of substance M into the processing chamber 201. Then, using a processing procedure similar to the purging in step x1, any gaseous substances remaining in the processing chamber 201 are removed from the processing chamber 201.

[0115] For example, water (H 2 O), water vapor (H 2 O gas) and H 2 O 2 Substances containing O and H, such as those listed above, can be used. One or more of these can be used as substance M. This also applies to step D, which will be described later.

[0116] [Step C] In this step, an etching agent is supplied to the wafer 200 in the processing chamber 201, that is, to the wafer 200 on which substance M has been selectively adsorbed on the surface of the first oxide layer α1.

[0117] Specifically, valve 243d is opened, and the etching agent is flowed into the gas supply pipe 232d. The etching agent's flow rate is adjusted by MFC 241d, and it is supplied into the processing chamber 201 via nozzle 249a and exhausted from exhaust port 231a. At this time, the etching agent is supplied to the wafer 200 (etching agent supply). At this time, valves 243f to 243h may be opened to supply inert gas into the processing chamber 201 via nozzles 249a to 249c, respectively.

[0118] Under the processing conditions described later, by supplying an etching agent to the wafer 200, the reaction product obtained by the reaction between the etching agent and the substance M that forms the first oxide layer α1 can etch the first oxide layer α1 and at least a portion of the oxide X (see Figures 4(e) and 4(f)).

[0119] For example, if both the first oxide layer α1 and oxide X are silicon oxide (SiO 2 ) containing substance M which has been pre-adsorbed onto the first oxide layer α1 is H 2If the etching agent supplied to the processing chamber 201 contains O and also contains hydrogen fluoride (HF) as an F-containing substance, then under the conditions described later, the reaction shown in the following formula can proceed. That is, in step C, substance M (H 2 The reaction product obtained by the reaction of O) and the etching agent (HF) 2 - This allows etching of the first oxide layer α1 (SiO layer) and at least a portion of the oxide X (SiO film) (see Figures 4(e) and 4(f)).

[0120] 2HF+H 2 O → HF 2 - +H 3 O + SiO 2 +2HF 2 - +2H 3 O + → SiF 4 +4H 2 O

[0121] As described above, according to this disclosure, etching of the first oxide layer α1 and oxide X on the surface of the wafer 200 is performed using an etching agent (HF) supplied into the processing chamber 201 and a trace amount of substance M (H) that was previously adsorbed on the wafer 200. 2 O) or part of its molecular structure (H x The reaction can be initiated by the interaction between O (where x is a real number less than 2) and .

[0122] When etching of the first oxide layer α1 and oxide X begins, a small amount of substance M (H) that was previously adsorbed onto the wafer 200 is removed. 2 O), etc., are consumed. However, in the reaction system in step C, the first oxide layer α1 and oxide X are etched to form substance M (e.g., H 2 O) is generated. Therefore, in step C, the above reaction is repeated in a chain reaction without additionally supplying substance M, etc., into the processing chamber 201, making it possible to etch the first oxide layer α1 and oxide X.

[0123] Examples of processing conditions when supplying the etching agent in this step include: Processing temperature: room temperature (25°C) to 170°C, preferably 25 to 150°C; Processing pressure: 10 to 4000, preferably 500 to 2000 Pa; Processing time: 1 to 120 minutes, preferably 10 to 100 minutes; Etching agent supply flow rate: 0.5 to 3 slm, preferably 1 to 2 slm; Inert gas supply flow rate (per gas supply pipe): 0 to 10 slm, preferably 1 to 5 slm.

[0124] Under the processing conditions described above, by supplying an etching agent to the wafer 200, the first oxide layer α1 and at least a portion of the oxide X are etched, and at least a portion of the surface of the substrate 200a, which was covered with oxide X, can be exposed. A third termination is formed on the surface of the exposed substrate 200a (see Figure 4(f)). The third termination is a termination that has a third affinity for substance M that is lower than the first affinity. For example, when the above-described F-containing substance is used as the etching agent, an F-terminus or an H-terminus is formed as a third termination on the surface of the substrate 200a.

[0125] (After-purging and return to atmospheric pressure) After etching the first oxide layer α1 and oxide X, the valve 243d is closed to stop the supply of etching agent to the processing chamber 201. Then, using the same procedure as the after-purging and return to atmospheric pressure described above, any gaseous substances remaining in the processing chamber 201 are removed from the processing chamber 201, and the pressure inside the processing chamber 201 is returned to normal pressure.

[0126] (Boat unloading and wafer discharge) Subsequently, the boat 217 is removed from the reaction tube 203 using the same procedure as described above for boat unloading and wafer discharge, and the wafer 200 is removed from the boat 217 by the transport mechanism 750.

[0127] The wafer 200, removed from the boat 217 by the transport mechanism 750, is placed on a mounting table located inside the exposure apparatus 600 via the transport chamber 700.

[0128] As mentioned above, an F-containing substance can be used as an etching agent, for example, an F and H-containing substance such as HF can be used. Also, for example, as an etching agent, fluorine (F 2 ), nitrogen trifluoride (NF 3 ), chlorine trifluoride (ClF 3 ), chlorine fluoride (ClF), etc., can be used. One or more of these can be used as etching agents. This also applies to step E described later.

[0129] [Step F] In this step, exposure is performed on the wafer 200 in the exposure apparatus 600, that is, the wafer 200 from which the first oxide layer α1 and oxide X have been etched. Specifically, the wafer 200 placed on the mounting table is moved to the wafer support using a moving mechanism provided in the exposure apparatus 600, and then a photomask is placed on the wafer 200 so as to face the light source. After that, light energy is irradiated from the light source onto the wafer 200 through the photomask. By selectively irradiating (exposing) the exposed surface of the second oxide layer α2 with light energy through the photomask, the second termination remaining on the exposed surface of the second oxide layer α2 is converted into the first termination (see Figure 4(g)).

[0130] After converting the second end formed on the exposed surface of the second oxide layer α2 to the first end, the moving mechanism moves the wafer 200 from the wafer support to the mounting table inside the exposure apparatus 600. The transport mechanism 750 carries the wafer 200 placed on the mounting table out of the exposure apparatus 600, and loads it into the boat 217 via the transport chamber 700.

[0131] (Wafer charging and boat loading) Subsequently, the wafers 200 are loaded into the boat 217 using the same procedure as described above for wafer charging and boat loading, and then transported into the processing room 201.

[0132] (Pressure and temperature adjustment) Subsequently, the pressure and temperature inside the processing chamber 201 are adjusted using the same procedure as described above for pressure and temperature adjustment.

[0133] [Step D] In this step, the wafer 200 in the processing chamber 201, that is, the wafer 200 in which the second termination formed on the exposed surface of the second oxide layer α2 has been converted to the first termination, is supplied (exposed) to the substance M. Specifically, the wafer 200 is exposed to the substance M using the same procedure and processing conditions as in step B.

[0134] Under the processing conditions described above, by supplying (exposing) the wafer 200 to substance M, substance M can be selectively adsorbed onto the surface of the second oxide layer α2 (see Figure 4(h)). This is because the first termination formed on the surface of the second oxide layer α2 has a higher affinity for substance M than the third termination formed on the surface of the substrate 200a.

[0135] The action in this step is the same as in step B described above. However, step B targets the first oxide layer α1, while step D targets the second oxide layer α2. That is, in step D, the substance M adsorbed on the second oxide layer α2 reacts with the etching agent supplied into the processing chamber 201 in the subsequent step E, producing a predetermined reaction product (etching species), thereby promoting the etching reaction on the second oxide layer α2.

[0136] After selectively adsorbing substance M onto the surface of the second oxide layer α2, the valve 243c is closed to stop the supply of substance M into the processing chamber 201. Then, using a processing procedure similar to the purging in step x1, any gaseous substances remaining in the processing chamber 201 are removed from the processing chamber 201.

[0137] [Step E] In this step, an etching agent is supplied to the wafer 200 in the processing chamber 201, that is, to the wafer 200 on which substance M has been selectively adsorbed on the surface of the second oxide layer α2. Specifically, the etching agent is supplied to the wafer 200 using the same procedure and processing conditions as in step C.

[0138] Under the processing conditions described above, by supplying an etching agent to the wafer 200, the second oxide layer α2 can be etched by the reaction product obtained from the reaction between the etching agent and the substance M adsorbed on the surface of the second oxide layer α2 (see Figures 4(i) and 4(j)).

[0139] The basic process of the etching reaction in this step is the same as the process in step C described above. For example, the second oxide layer α2 is silicon oxide (SiO 2 ) containing substance M which has been pre-adsorbed onto the second oxide layer α2 is H 2 If the etching agent supplied into the processing chamber 201 contains O and contains HF as an F-containing substance, then, similar to step C, substance M (H 2 The reaction product (HF) produced by the reaction of O) and the etching agent (HF) 2 - The second oxide layer α2 can be etched via (etc.) (see Figures 4(i) and 4(j)).

[0140] (After-purging and return to atmospheric pressure) After etching the second oxide layer α2, valve 243d is closed to stop the supply of etching agent to the processing chamber 201. Then, using the same procedure as the after-purging and return to atmospheric pressure described above, any gaseous substances remaining in the processing chamber 201 are removed from the processing chamber 201, and the pressure inside the processing chamber 201 is returned to normal pressure.

[0141] (Boat unloading and wafer discharge) Subsequently, the boat 217 is removed from the reaction tube 203 using the same procedure as described above for boat unloading and wafer discharge, and the wafer 200 is removed from the boat 217 by the transport mechanism 750.

[0142] (3) Effects of this embodiment According to this embodiment, one or more of the following effects can be obtained.

[0143] (a) By performing steps A to C, oxide X can be selectively etched relative to non-oxide Y (see Figure 4(f)).

[0144] (b) In step A, step x1 is performed in advance to form a second oxide layer α2 on the non-oxide Y, and then step a1 is performed to form a second terminator (hydrophobic terminator) on the second oxide layer α2. By performing step x1 in advance to form a second oxide layer α2 on the non-oxide Y in this way, it becomes easy to uniformly form a region on the non-oxide Y in which the second terminator is formed.

[0145] (c) In step A, by performing a cycle including step x1 and step x2 a predetermined number of times, it becomes easy to form the first oxide layer α1 and the second oxide layer α2 uniformly and with a desired thickness.

[0146] (d) In step A, step a1 is performed in advance to form a second terminator on the exposed surfaces of the first oxide layer α1 and the second oxide layer α2, and then in step a2, the exposed surface of the first oxide layer α1 is selectively exposed to light, thereby making it possible to selectively form a region on the oxide X in which the first terminator is formed.

[0147] (e) In step a2, by performing exposure through a photomask, the desired region can be made into the region where the first termination is formed.

[0148] (f) Using an F-containing substance as the etching agent, and using an O and H-containing substance (e.g., H) as substance M. 2 By using gas O, in step C, the oxide X can be efficiently etched by the reaction product obtained from the reaction between substance M and the etching agent.

[0149] (g) By making the second terminator a terminator containing a methyl group, the affinity for substance M (especially O and H-containing substances) can be reduced. Alternatively, by converting the second terminator to the first terminator through the exposure treatment in step a2, the affinity for substance M can be increased.

[0150] (h) By including a compound having an atom of a predetermined element and a methyl group bonded to the atom of the predetermined element in step a1, a methyl group termination as a second termination can be efficiently formed on the exposed surfaces of the first oxide layer α1 and the second oxide layer α2.

[0151] (i) In step C, the supply of the etching agent is continued until at least a portion of the surface of the substrate 200a, which was covered with oxide X, is exposed, thereby removing the oxide X from the substrate 200a and exposing the surface of the substrate 200a.

[0152] (j) In step C, a third terminal having a third affinity for substance M that is lower than the first affinity is formed on the surface of the substrate 200a, thereby making it easy to selectively etch the second oxide layer α2 in step E without performing any new hydrophobic treatment on the surface of the substrate 200a.

[0153] (k) By performing step D, which involves adsorbing substance M onto the surface of the second oxide layer α2 after step C, the etching process of the second oxide layer α2 in step E can be accelerated.

[0154] (l) After step C, step F is performed, in which the exposed surface of the second oxide layer α2 is selectively exposed to light, thereby selectively converting the second terminator remaining on the surface of the second oxide layer α2 into a first terminator with high affinity for substance M (e.g., hydrophilic).

[0155] (m) After step D, step E is performed to supply an etching agent to the wafer 200 and etch the second oxide layer α2, thereby selectively etching the remaining second oxide layer α2.

[0156] <Other Aspects of the Disclosure> The aspects of the Disclosure have been described in detail above. However, the Disclosure is not limited to the aspects described above and can be modified in various ways without departing from its essence.

[0157] In the above-described embodiment, the example given was that in step a1, the surface of the wafer 200 is hydrophobized via the oxide layer A by supplying the above-described modifier to the wafer 200; however, the disclosure is not limited thereto. For example, a second terminator (methyl group terminator) may be formed on the surface of the oxide layer A by vaporizing hexamethyldisilazane (HMDS) onto the wafer 200. The same effects as in the above-described embodiment can be obtained in this embodiment as well.

[0158] In the above-described embodiment, the example given was that in step a2, a photomask is used to hydrophilize the surface of the hydrophobic first oxide layer α1, but the disclosure is not limited thereto. For example, a resist pattern may be formed on the exposed surface of the hydrophobic first oxide layer α1, and light energy may be selectively irradiated onto the exposed surface. Alternatively, for example, in the processing chamber 201, for example, O 2 Heat treatment while supplying (O 2 The surface of the hydrophobic first oxide layer α1 may be made hydrophilic by performing an annealing treatment. The same applies in step F. The same effects as in the above-described embodiment can be obtained in this embodiment as well.

[0159] Although not specifically described in the above embodiments, the processing temperature may be varied during the execution of step B. Specifically, the processing temperature may be maintained at a first temperature for a predetermined time from the start of step B, and then lowered to a second temperature lower than the first temperature. Alternatively, the temperature inside the processing chamber 201 may be varied after the execution of step B. Specifically, the processing temperature may be maintained at a first temperature during the execution of step B, and then lowered to a second temperature lower than the first temperature after the execution of step B. The same effects as in the above embodiments can be obtained in this embodiment as well. Furthermore, in this embodiment, by lowering the temperature inside the processing chamber 201, the substance M can be condensed on the surface of the first oxide layer α1. This promotes the generation of reaction products in step C and accelerates the etching of the first oxide layer α1, etc. The same applies to step D.

[0160] Although not specifically described in the above embodiments, in step C, it is preferable to stop supplying the etching agent while at least a portion of the second oxide layer α2 remains. The same effects as in the above embodiments can be obtained in this embodiment as well. Furthermore, in this embodiment, it is possible to prevent the non-oxide Y from being etched.

[0161] Although not specifically described in the above embodiments, in step C, it is preferable to continue supplying the etching agent until at least a portion of the surface of the non-oxide Y, which was covered by the second oxide layer α2, is exposed. The same effects as in the above embodiments can be obtained in this embodiment as well. Furthermore, in this embodiment, the second oxide layer α2 on the non-oxide Y can be removed simultaneously with the first oxide layer α1 and the oxide X.

[0162] Although not specifically described in the above embodiments, in step C, it is preferable to supply the etching agent under conditions (for example, by adjusting the processing temperature, partial pressure of the etching agent, and thickness of the second oxide layer α2) such that at least a portion of the substrate surface 200a coated with oxide X and at least a portion of the non-oxide surface Y coated with the second oxide layer α2 are exposed at approximately the same time. In this embodiment, the same effects as in the above embodiments can be obtained. Furthermore, in this embodiment, the second oxide layer α2 on the non-oxide Y can be removed simultaneously in a single etching process along with the first oxide layer α1 and oxide X without performing an additional process (step E).

[0163] It is preferable that the recipes used for each process are prepared individually according to the processing content, recorded and stored in the storage device 121c via a telecommunications line or external storage device 123. When starting each process, it is preferable that the CPU 121a appropriately selects the appropriate recipe from among the multiple recipes recorded and stored in the storage device 121c according to the processing content. This makes it possible to form films of various film types, composition ratios, film quality, and film thickness with good reproducibility using a single substrate processing device. Furthermore, it reduces the burden on the operator and allows each process to be started quickly while avoiding operational errors.

[0164] The above-mentioned recipes are not limited to newly created ones; they may also be prepared, for example, by modifying existing recipes already installed in the board processing device. When modifying a recipe, the modified recipe may be installed in the board processing device via a telecommunications line or a recording medium on which the recipe is stored. Alternatively, existing recipes already installed in the board processing device may be directly modified by operating the input / output device 122 provided in the existing board processing device.

[0165] This disclosure is not limited to the embodiments described above, and can be suitably applied, for example, when forming a film using a single-wafer substrate processing apparatus that processes one or more substrates at a time. Furthermore, this disclosure is not limited to the embodiments described above, and can be suitably applied when forming a film using a substrate processing apparatus having a cold-wall type processing furnace. Even when using these substrate processing apparatuses, each process can be carried out using the same processing procedures and processing conditions as in the embodiments and modifications described above, and the same effects as in the embodiments and modifications described above can be obtained.

[0166] The above-described embodiments and modifications can be used in combination as appropriate. The processing procedure and processing conditions in this case can be the same as, for example, the processing procedure and processing conditions of the above-described embodiments and modifications.

[0167] 200 Wafer (substrate) 200a Underlayment X Oxide Y Non-oxide α1 First oxide layer α2 Second oxide layer

Claims

(a) A step of providing a substrate comprising: an oxide; a non-oxide; a first oxide layer formed on the surface of the oxide, the exposed surface of which has a first termination having a first affinity for substance M; and a second oxide layer formed on the surface of the non-oxide, the exposed surface of which has a second termination having a second affinity for substance M that is lower than the first affinity; (b) A step of exposing the substrate to the substance M so that the substance M is adsorbed onto the surface of the first oxide layer, (c) A step of supplying an etching agent to the substrate and removing the first oxide layer and at least a portion of the oxide by a reaction product obtained by the reaction of the etching agent with the substance M adsorbed on the surface of the first oxide layer, A substrate processing method having the following characteristics.   The first oxide layer and the second oxide layer are A substrate in which the surfaces of the oxide and the non-oxide are exposed is formed by supplying raw materials to it. The substrate processing method according to claim 1.   The first oxide layer and the second oxide layer are A predetermined number of cycles are performed on a substrate in which the surfaces of the oxide and the non-oxide are exposed, which include a step of supplying raw materials and a step of supplying an oxidizing agent. The substrate processing method according to claim 1.   The first termination and the second termination are (a-1) A step of supplying a modifier to the first oxide layer and the second oxide layer to form the second end on the exposed surface of the first oxide layer and the exposed surface of the second oxide layer, respectively. (a-2) After (a-1), a step of selectively exposing the exposed surface of the first oxide layer to the second end on the exposed surface of the first oxide layer to the first end, Formed by executing, The substrate processing method according to claim 1. The exposure in (a-2) is performed by irradiating the substrate with lamp light through a photomask. The substrate processing method according to claim 4.   The etching agent contains a fluorine-containing substance, and the substance M contains an oxygen- and hydrogen-containing substance. The substrate processing method according to claim 1.   (b) The substrate is exposed to water vapor, The substrate processing method according to claim 6.   The second terminator is a terminator containing a methyl group. The substrate processing method according to claim 1.   The modifier comprises a compound having an atom of a predetermined element and a methyl group bonded to the atom of the predetermined element. In (a-1), the second terminator is formed by the adsorption of atoms of the predetermined element and methyl groups bonded to atoms of the predetermined element onto the exposed surface of the first oxide layer and the exposed surface of the second oxide layer. The substrate processing method according to claim 4.   (c) In this case, the supply of the etching agent is stopped while at least a portion of the second oxide layer remains. The substrate processing method according to claim 1.   (c) The supply of the etching agent is continued until the surface of the non-oxide that was covered by the second oxide layer is exposed. The substrate processing method according to claim 1.   The oxide is formed on the substrate that constitutes the substrate, (c) The supply of the etching agent is continued until the surface of the substrate that was covered with the oxide is exposed. The substrate processing method according to claim 1.   (c) The etching agent is supplied under conditions such that the timing at which the surface of the substrate covered with the oxide is exposed and the timing at which the surface of the non-oxide material covered with the second oxide layer is exposed are substantially the same. The substrate processing method according to claim 12.   The aforementioned substrate is non-oxide, (c) A third terminal having a third affinity for the substance M that is lower than the first affinity is formed on the surface of the substrate. The substrate processing method according to claim 12. (d) The process further comprises the step of exposing the substrate to the substance M after (c) to adsorb the substance M onto the surface of the second oxide layer, The substrate processing method according to claim 1.   (e) The further step is to supply the etching agent to the substrate after (d), and remove the second oxide layer with the reaction product obtained by the reaction between the etching agent and the substance M adsorbed on the surface of the second oxide layer. The substrate processing method according to claim 15.   (f) The process further comprises the step of selectively exposing the exposed surface of the second oxide layer after (c) to convert the second end remaining on the exposed surface of the second oxide layer to the first end, The substrate processing method according to claim 1.   (a) A step of providing a substrate comprising: an oxide; a non-oxide; a first oxide layer formed on the surface of the oxide, the exposed surface of which has a first termination having a first affinity for substance M; and a second oxide layer formed on the surface of the non-oxide, the exposed surface of which has a second termination having a second affinity for substance M that is lower than the first affinity; (b) A step of exposing the substrate to the substance M so that the substance M is adsorbed onto the surface of the first oxide layer, (c) A step of supplying an etching agent to the substrate and removing the first oxide layer and at least a portion of the oxide by a reaction product obtained by the reaction of the etching agent with the substance M adsorbed on the surface of the first oxide layer, A method for manufacturing a semiconductor device having [a certain feature].   (a) A procedure for providing a substrate comprising an oxide, a non-oxide, a first oxide layer formed on the surface of the oxide and having a first termination on its exposed surface having a first affinity for substance M, and a second oxide layer formed on the surface of the non-oxide and having a second termination on its exposed surface having a second affinity for substance M that is lower than the first affinity, (b) A procedure to adsorb the substance M onto the surface of the first oxide layer by exposing the substrate to the substance M, (c) A procedure to supply an etching agent to the substrate and remove the first oxide layer and at least a portion of the oxide by a reaction product obtained by the reaction of the etching agent with the substance M adsorbed on the surface of the first oxide layer, A program that causes a circuit board processing unit to execute commands via a computer.   A material supply system that supplies material M to the substrate, An etching agent supply system that supplies an etching agent to the substrate, (a) A process for providing a substrate comprising an oxide, a non-oxide, a first oxide layer formed on the surface of the oxide and having a first termination on its exposed surface having a first affinity for the substance M, and a second oxide layer formed on the surface of the non-oxide and having a second termination on its exposed surface having a second affinity for the substance M that is lower than the first affinity, (b) A process of supplying the substance M to the substrate to adsorb the substance M onto the surface of the first oxide layer, (c) A process of supplying the etching agent to the substrate and removing the first oxide layer and at least a portion of the oxide by a reaction product obtained by the reaction of the etching agent with the substance M adsorbed on the surface of the first oxide layer, A control unit configured to control the substance M supply system and the etching agent supply system to perform the following actions: A substrate processing apparatus having