Substrate processing method, method for manufacturing semiconductor device, program, and substrate processing device
By alternating pressure cycles and controlled gas supply in the etching process, the method addresses inefficiencies in semiconductor manufacturing etching, enhancing etching rate and uniformity while reducing gas usage.
Patent Information
- Application Number
- PCT/JP2026/014718
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-09-22
- Filing Date
- 2026-04-09
- Publication Date
- 2026-11-12
AI Technical Summary
Existing etching processes in semiconductor manufacturing face challenges in achieving a balance between etching rate, in-plane uniformity, and gas consumption, particularly in forming modified layers on substrate surfaces.
A method involving alternating steps of increasing and decreasing pressure in a processing chamber to form a modified layer on the substrate surface, followed by converting it into a volatile substance using specific gases, optimizing the etching process to improve efficiency and reduce gas consumption.
Enhances etching rate and in-plane uniformity while minimizing gas consumption and improving throughput by strategically controlling pressure and gas flow in the etching process.
Smart Images

Figure JP2026014718_12112026_PF_FP_ABST
Abstract
Description
Substrate processing method, semiconductor device manufacturing method, program, and substrate processing apparatus.
[0001] This disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a program, and a substrate processing apparatus.
[0002] In the manufacturing process of semiconductor devices, or as part of the substrate processing process, materials on a substrate are sometimes etched using multiple gases (see, for example, Patent Document 1).
[0003] Japanese Patent Publication No. 2021-158142
[0004] This disclosure provides a technology that enables improvement of the etching rate.
[0005] According to one aspect of the present disclosure, a technology is provided that includes: (a) a step of supplying a first gas to a substrate placed in a processing chamber while increasing the pressure in the processing chamber; (a2) a step of decreasing the pressure in the processing chamber after the completion of (a1); and a step of performing (a1) two or more times with (a2) in between to form a modified layer on the surface of a predetermined substance on the substrate; and (b) a step of supplying a second gas to the substrate to convert at least a portion of the modified layer into a volatile substance.
[0006] According to this disclosure, it becomes possible to improve the etching rate.
[0007] Figure 1 is a schematic diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, showing the processing furnace portion in a vertical cross-sectional view. Figure 2 is a schematic diagram of a controller of a substrate processing apparatus preferably used in one embodiment of the present disclosure, showing the controller's control system in a block diagram. Figure 3 is a flow chart showing a substrate processing process in one embodiment of the present disclosure. Figure 4 is a schematic diagram of the time change of pressure inside the processing chamber in an etching process in one embodiment of the present disclosure. Figure 5 is a schematic diagram of the time change of pressure inside the processing chamber in a part of an etching process of a modified example of the present disclosure.
[0008] <An Embodiment of the Disclosure> An embodiment of the disclosure will be described below, mainly with reference to Figures 1 to 4. Note that the drawings used in the following description are schematic, and the dimensional relationships and proportions of the elements shown in the drawings do not necessarily correspond to reality. Furthermore, the dimensional relationships and proportions of the elements do not necessarily correspond between multiple drawings.
[0009] (1) As shown in the configuration diagram 1 of the substrate processing apparatus, the processing furnace 202 has a heater 207 as a heating mechanism (temperature control unit). Inside the heater 207, a reaction tube 203 is arranged concentrically with the heater 207. The reaction tube 203 is formed in a cylindrical shape with a closed upper end and an open lower end. A processing chamber 201 is formed inside the reaction tube 203. The processing chamber 201 is configured to accommodate a wafer 200 as a substrate. Processing of the wafer 200 is performed in this processing chamber 201.
[0010] Gas supply pipes 232a and 232b are equipped with, in order from the upstream side of the gas flow, mass flow controllers (MFCs) 241a and 241b, which are flow control devices (flow control units), and valves 243a and 243b, which are on-off valves. Gas supply pipe 232c is connected downstream of valve 243a on gas supply pipe 232a. Gas supply pipe 232c is connected downstream of valve 243b on gas supply pipe 232b. Gas supply pipes 232c and 232c are equipped with, in order from the upstream side of the gas flow, MFCs 241c and 241c, and valves 243c and 243c, respectively.
[0011] Inside the processing chamber 201, nozzles 249a and 249b are provided so as to penetrate the lower side wall of the reaction tube 203. Gas supply holes 250a and 250b are provided on the sides of nozzles 249a and 249b, respectively, for supplying gas. Multiple gas supply holes 250a and 250b are provided extending from the lower to the upper part of the reaction tube 203. Gas supply pipes 232a and 232b are connected to nozzles 249a and 249b, respectively.
[0012] Gas supply pipe 232a is equipped with a first gas supply source containing a first element, an MFC 241a, a valve 243a, and a nozzle 249a in that order. Gas supply pipe 232b is equipped with a second gas supply source containing a second element, an MFC 241b, a valve 243b, and a nozzle 249b in that order. Gas supply pipes 232c and 232d are equipped with inert gas supply sources, MFCs 241c and 241d, valves 243c and 243d, gas supply pipes 232b and 232a, and nozzles 249b and 249a in that order. The inert gas acts as a purge gas, carrier gas, diluent gas, etc.
[0013] A first supply system is configured to supply the first gas to the wafer 200 (or inside the processing chamber 201), mainly consisting of a gas supply pipe 232a, an MFC 241a, and a valve 243a. A second supply system is configured to supply the second gas to the wafer 200 (or inside the processing chamber 201), mainly consisting of a gas supply pipe 232b, an MFC 241b, and a valve 243b. An inert gas supply system is configured to supply the inert gas to the wafer 200 (or inside the processing chamber 201), mainly consisting of gas supply pipes 232c, 232d, MFCs 241c, 241d, and valves 243c, 243d.
[0014] Of the various supply systems described above, any or all of them may be configured as an integrated supply system in which valves 243a to 243d and MFCs 241a to 241d are integrated. The integrated supply system is connected to each of the gas supply pipes 232a to 232d, and the supply operation of various gases into the gas supply pipes 232a to 232d, i.e., the opening and closing operation of valves 243a to 243d and the flow rate adjustment operation by MFCs 241a to 241d, is controlled by a controller 121, which will be described later. The integrated supply system 248 is configured as an integrated or segmented integrated unit, and can be attached to and detached from the gas supply pipes 232a to 232d, etc., in units of the integrated unit, and is configured so that maintenance, replacement, and expansion of the integrated supply system can be performed in units of the integrated unit.
[0015] An exhaust pipe 231 for exhausting the atmosphere inside the processing chamber 201 is connected to the lower side wall of the reaction tube 203. A vacuum pump 246, which acts as an exhaust device, is connected to the exhaust pipe 231 via a pressure sensor 245, which acts as a pressure detector (pressure detection unit) for detecting the pressure inside the processing chamber 201, and an APC (Auto Pressure Controller) valve 244, which acts as a pressure regulator (pressure adjustment unit). The APC valve 244 can be opened and closed while the vacuum pump 246 is operating to perform vacuum exhaust and stop vacuum exhaust inside the processing chamber 201. Furthermore, while the vacuum pump 246 is operating, the valve opening can be adjusted based on the pressure information detected by the pressure sensor 245 to adjust the pressure inside the processing chamber 201. The APC valve 244 is an example of an exhaust valve whose opening can be continuously controlled within a predetermined range. For example, if the minimum opening degree that the APC valve 244 can control is defined as 0%, and the maximum opening degree that the APC valve 244 can achieve is defined as 100%, then if the APC valve 244 can continuously control the opening degree within the range of 0% to 100%, then the predetermined range is expressed as 0% to 100%. The APC valve 244 is, for example, a butterfly valve. The exhaust system mainly consists of the exhaust pipe 231, the pressure sensor 245, and the APC valve 244. A vacuum pump 246 may also be included in the exhaust system. In this specification, numerical range notations such as "0% to 100%" mean that the lower limit and upper limit are included in that range. Therefore, for example, "0% to 100%" means "0% or more and 100% or less." The same applies to other numerical ranges.
[0016] Below the reaction tube 203, a seal cap 219 is provided as a furnace opening cover capable of airtightly closing the lower end opening of the reaction tube 203. An O-ring 220 is provided on the upper surface of the seal cap 219 as a sealing member that contacts the lower end of the reaction tube 203. Below the seal cap 219, a rotating mechanism 267 for rotating the boat 217, which will be described later, is installed. The rotating mechanism 267 is connected to the boat 217 via a rotating shaft 255, passing through the seal cap 219, and the boat 217 and the wafer 200 are rotated by rotating the rotating shaft 255. The seal cap 219 is raised and lowered vertically by a boat elevator 115, which is a lifting mechanism installed outside the reaction tube 203. The boat elevator 115 is configured as a transport device (transport mechanism) that moves the wafer 200 in and out of the processing chamber 201 by raising and lowering the seal cap 219.
[0017] The boat 217, which serves as a substrate support, is configured to support multiple wafers 200, for example 25 to 200 wafers 200, in a multi-stage arrangement, aligned vertically in a horizontal position and with their centers aligned, that is, arranged with spacing between them. The boat 217 is made of a heat-resistant material such as quartz. An insulating plate 218 is supported in a multi-stage arrangement in a horizontal position at the bottom of the boat 217. In this specification, numerical ranges such as "25 to 200 wafers" mean that the lower and upper limits are included within that range. Therefore, for example, "25 to 200 wafers" means "25 wafers or more and 200 wafers or less." The same applies to other numerical ranges.
[0018] A temperature sensor 263 is installed inside the reaction tube 203 to detect temperature. By adjusting the power supply to the heater 207 based on the temperature information detected by the temperature sensor 263, the temperature inside the processing chamber 201 can be adjusted to the desired temperature distribution.
[0019] As shown in Figure 2, the controller 121, which is the control unit (control means), is configured as a computer equipped with a CPU (Central Processing Unit) 121a, RAM (Random Access Memory) 121b, storage device 121c, and I / O port 121d. The RAM 121b, storage device 121c, and I / O port 121d are configured to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122, configured as, for example, a touch panel, is connected to the controller 121.
[0020] The storage device 121c is composed of, for example, flash memory, an HDD (Hard Disk Drive), etc. The storage device 121c contains, in a readable format, control programs that control the operation of the substrate processing device, and process recipes that describe the procedures and conditions for the etching process, which will be described later. The process recipe is a combination of steps in the etching process, described later, that cause the controller 121 to execute and obtain a predetermined result, and functions as a program. Hereinafter, process recipes and control programs will be collectively referred to simply as "programs" (program products). Similarly, process recipes will be simply referred to as "recipes." In this specification, the term "program" may include only recipes, only control programs, or both. The RAM 121b is configured as a memory area (work area) where programs and data read by the CPU 121a are temporarily held.
[0021] The I / O port 121d is connected to the MFCs 241a to 241d, valves 243a to 243d, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotating mechanism 267, boat elevator 115, etc.
[0022] The CPU 121a is configured to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to input of operation commands from the input / output device 122. The CPU 121a is configured to control the flow rate adjustment operation of various gases by the MFCs 241a to 241d, the opening and closing operation of valves 243a to 243d, the opening and closing operation of the APC valve 244 and the pressure adjustment operation of the APC valve 244 based on the pressure sensor 245, the starting and stopping of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotating mechanism 267, and the raising and lowering operation of the boat 217 by the boat elevator 115, etc., in accordance with the contents of the read recipe.
[0023] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 onto a computer. The external storage device 123 includes, for example, magnetic disks such as HDDs, optical disks such as CDs, and semiconductor memory such as USB memory. The storage device 121c and the external storage device 123 are configured as computer-readable recording media on which the program is recorded. Hereinafter, these will be collectively referred to simply as recording media. In this specification, when the term recording media is used, it may include only the storage device 121c, only the external storage device 123, or both. Note that the program may be provided to the computer using communication means such as the Internet or a dedicated line, without using the external storage device 123.
[0024] (2) Substrate Processing Process An example of etching a predetermined substance on a wafer 200 as one step in the semiconductor device manufacturing process using the processing furnace 202 of the substrate processing apparatus described above will be explained with reference to Figures 3 and 4. In the following explanation, the operation of each part constituting the substrate processing apparatus is controlled by the controller 121.
[0025] Figure 3 is a flowchart of the substrate processing process. As shown in Figure 3, the substrate processing process involves steps S1, S2, S3, S4, and S5.
[0026] The term "wafer" used in the present disclosure may refer to the wafer itself, or may refer to a laminate of the wafer and a predetermined layer or film formed on the surface thereof. The expression "surface of a wafer" as used in the present specification may refer to the surface of the wafer itself, or may refer to the surface of a predetermined layer or the like formed on the wafer. When the phrase "forming a predetermined layer on a wafer" is described in the present specification, it may mean directly forming the predetermined layer on the surface of the wafer itself, or may mean forming the predetermined layer on a layer or the like already formed on the wafer. The use of the term "substrate" in the present specification has the same meaning as the use of the term "wafer".
[0027] (Step S1: Substrate loading step) A plurality of wafers 200 on which a predetermined substance to be etched is formed are loaded (wafer charge) into a boat 217. Thereafter, the boat 217 supporting the plurality of wafers 200 is lifted by a boat elevator 115 and carried into a processing chamber 201 (boat load). In this state, a seal cap 219 seals the lower end of a reaction tube 203 via an O-ring 220.
[0028] (Step S2: Pressure and temperature adjustment step) The interior of the processing chamber 201, that is, the space where the wafers 200 are present, is evacuated (pressure-reduced exhaust) by a vacuum pump 246 so as to reach a desired processing pressure (degree of vacuum). Further, the wafers 200 in the processing chamber 201 are heated by a heater 207 so as to reach a desired processing temperature. In addition, rotation of the wafers 200 by a rotation mechanism 267 is started. The operation of the vacuum pump 246, the heating of the wafers 200, and the rotation of the wafers 200 are all continuously performed at least until the processing on the wafers 200 is completed.
[0029] The processing temperature in the present specification means the temperature of the wafer 200 or the temperature inside the processing chamber 201, and the processing pressure means the pressure inside the processing chamber 201. Further, the processing time means the duration for which the corresponding processing is continued. These also apply to the following description.
[0030] Here, the predetermined substance containing the predetermined element M to be etched is, for example, an oxide of the predetermined element M. The predetermined element M is, for example, a metal element or a metalloid element. Therefore, the predetermined substance is, for example, a metal oxide, a metalloid oxide, a mixture or a laminate thereof, or the like.
[0031] As the metal element, at least one or more of aluminum (Al), zirconium (Zr), hafnium (Hf), titanium (Ti), yttrium (Y), lanthanum (La), tantalum (Ta), niobium (Nb), ruthenium (Ru), vanadium (V), zinc (Zn), manganese (Mn), cobalt (Co), and the like can be used. As the metalloid element, at least one or more of silicon (Si), germanium (Ge), gallium (Ga), indium (In), and the like can be used. As the predetermined substance, a substance containing two or more of these metal elements and metalloid elements may be used.
[0032] (Step S3: Etching Step) In step S3, at least a part of the predetermined substance on the wafer 200 is etched using a plurality of gases. In step S3, at least a part of the predetermined substance on the wafer 200 may be etched by, for example, ALE (Atomic Layer Etching). Specifically, a first gas is supplied to the wafer 200 to form a modified layer containing the predetermined element M on the surface of the predetermined substance. Thereafter, a second gas is supplied to the wafer 200 to convert at least a part of the modified layer into a volatile substance containing the predetermined element M. As a result, at least a part of the predetermined substance is etched. Here, the "volatile substance" in the present disclosure refers to a substance that enters a gas phase state under the conditions in the processing chamber 201 in at least a part of step S3.
[0033] Step S3 includes at least step S31 and step S33. In the following description, step S3 will be described by taking as an example a case where a processing cycle in which step S31, step S32, step S33, and step S34 are sequentially performed is performed a predetermined number of times. Here, FIG. 4 schematically shows the temporal change of the pressure in the processing chamber 201 in each step during step S3.
[0034] [Step S31: First Gas Supply Process] In step S31, step S311 is performed two or more times, with step S312 in between, to form a modified layer containing a predetermined element M on at least a portion of the surface of a predetermined substance on the wafer 200. The following explanation will be given using the case in which step S312 is started simultaneously with the end of step S311 as shown in Figure 4.
[0035] <Step S311> As shown in Figure 4, in step S311, the pressure inside the processing chamber 201 is increased while the first gas is supplied to the wafer 200 placed inside the processing chamber 201. As a result, a modified layer is formed on a portion of the surface of the predetermined material.
[0036] Specifically, valve 243a is opened, and the first gas flows into the gas supply pipe 232a. The flow rate of the first gas is regulated by MFC 241a and supplied to the processing chamber 201 via nozzle 249a. Valves 243c and 243d are also opened, and inert gas flows into the gas supply pipes 232c and 232d. The flow rate of the inert gas is regulated by MFC 241c and 241d and supplied to the processing chamber 201 via nozzles 249a and 249b. The first gas and inert gas supplied to the processing chamber 201 are exhausted through the exhaust pipe 231 via APC valve 244, which is controlled to increase the pressure inside the processing chamber 201.
[0037] Examples of processing conditions in step S311 include: processing temperature: 200 to 900°C, preferably 300 to 800°C; maximum pressure: 1 to 200 torr, preferably 5 to 100 torr; first gas supply flow rate: 0.1 to 10 slm; inert gas supply flow rate (each gas supply pipe): 0.1 to 10 slm; processing time: 5 to 200 seconds, preferably 10 to 100 seconds. The processing temperature in subsequent steps can be the same as in this step, for example.
[0038] As the first gas, for example, a gas containing fluorine (F), a halogen element as the first element in its molecular structure (F-containing gas) can be used. 2 ) gas, nitrogen trifluoride (NF 3) gas, hydrogen fluoride (HF) gas, carbon tetrafluoride (CF 4 ) gas, tungsten hexafluoride (WF 6 ) gas, hexafluoroacetylacetone (C 5 H 2 F 6 O 2 ) or the like, at least one or more of which can be used.
[0039] As the inert gas, in addition to nitrogen (N 2 ) gas, a rare gas such as argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas or the like can be used. One or more of these can be used as the inert gas.
[0040] Specifically, when a gas containing F is used as the first gas, for example, a modified layer containing a fluoride of a predetermined element M is formed on the surface of a predetermined substance that is an oxide of the predetermined element M.
[0041] <Step S312> As shown in FIG. 4, in step S312, after the end of step S311, the pressure in the processing chamber 201 is reduced.
[0042] Specifically, the gas is exhausted from the exhaust pipe 231 via the APC valve 244 controlled so that the pressure in the processing chamber 201 decreases. At this time, the valves 243c and 243d are opened to flow the inert gas into the gas supply pipes 232c and 232d. At this time, the first gas may or may not be supplied to the wafer 200 disposed in the processing chamber 201. When supplying the first gas, the valve 243a is opened to flow the first gas into the gas supply pipe 232a. The flow rate of the first gas is adjusted by the MFC 241a, and the first gas is supplied into the processing chamber 201 through the nozzle 249a. When not supplying the first gas, the valve 243a is kept closed.
[0043] Note that after step S311 performed at the end of step S31, step S312 may be performed under conditions different from those of the previous step S312, or step S312 may be replaced with another process. For example, after step S311 performed at the end of step S31, the exhaust in the processing chamber 201 may be performed under the same conditions as step S32 described later.
[0044] Examples of processing conditions in step S312 include: Minimum pressure: 0.1 to 20 torr, preferably 1 to 10 torr; First gas supply flow rate: 0.1 to 10 slm; Inert gas supply flow rate (each gas supply pipe): 0.1 to 10 slm; Processing time: 5 to 200 seconds, preferably 10 to 100 seconds. The processing temperature in subsequent steps can be the same as in this step, for example.
[0045] In step S31, as shown in Figure 4, step S311 is repeated two or more times with step S312 in between. Step S31 forms a modified layer on at least a portion of the surface of the predetermined substance on the wafer 200. It is preferable to repeat steps S311 and S312 until the modified layer is sufficiently formed.
[0046] By supplying the first gas while increasing the pressure inside the processing chamber 201, the proportion of molecules of the first gas supplied into the processing chamber 201 that are exhausted from the processing chamber 201 without contributing to the formation of the reformed layer can be reduced. Therefore, the etching rate can be improved. This can also be rephrased as being able to obtain an etching rate similar to that of the conventional method while reducing at least one of the supply amount of the first gas and the supply time of the first gas compared to the conventional method. Therefore, it becomes possible to reduce the consumption of the first gas and improve throughput.
[0047] Here, as the period for increasing the pressure in the processing chamber 201 lengthens, the first gas in the processing chamber 201 becomes more easily heated. In other words, the proportion of first gas molecules in the processing chamber 201 that have received thermal energy and become more reactive increases. Therefore, the formation of the modified layer progresses more easily in the central part of the wafer 200 compared to the edge part of the wafer 200 where there are many first gas molecules that have just been supplied into the processing chamber 201. Consequently, the longer the period during which the first gas is difficult to discharge from the processing chamber 201, the more likely the film thickness of the predetermined substance after etching will have a concave distribution. That is, the uniformity of the etching process within the surface of the wafer 200 (hereinafter referred to as in-plane uniformity) tends to decrease. On the other hand, if the period for increasing the pressure in the processing chamber 201 is short, it is difficult to form a sufficient amount of modified layer, and the etching rate tends to decrease.
[0048] By performing step S311 two or more times with step S312 in between, the supply of the first gas while increasing the pressure in the processing chamber 201 over a relatively short period of time can be performed multiple times. Therefore, both the etching rate and in-plane uniformity can be improved.
[0049] In step S312, as the pressure decreases, the proportion of molecules of the first gas supplied into the processing chamber 201 that are exhausted from the processing chamber 201 without contributing to the formation of the modified layer increases. For this reason, it is preferable to reduce the flow rate of the first gas supplied to the wafer 200 in at least a part of step S312 compared to the flow rate of the first gas supplied to the wafer 200 in step S311, or to not supply the first gas to the wafer 200 at all. This makes it possible to improve the etching rate while suppressing the consumption of the first gas.
[0050] Furthermore, it is preferable to reduce the flow rate of the first gas supplied to the wafer 200 throughout step S312 compared to the flow rate of the first gas supplied to the wafer 200 in step S311, or to not supply the first gas to the wafer 200 at all. It is also preferable not to supply the first gas to the wafer 200 for at least a portion of step S312. By doing so, the etching rate can be improved while further suppressing the consumption of the first gas. Moreover, it is preferable not to supply the first gas to the wafer 200 throughout step S312. This allows for a significant reduction in the consumption of the first gas while improving the etching rate.
[0051] It is preferable to make the time spent performing step S311 longer than the time spent performing step S312. This allows for longer formation of the modified layer while shortening the time spent performing step S312, which is less conducive to the formation of the modified layer. Therefore, the etching rate can be further improved while also improving throughput.
[0052] It is preferable to make the absolute value of the change in pressure inside the processing chamber per unit time in step S312 greater than the absolute value of the change in pressure inside the processing chamber per unit time in step S311. This allows for longer formation of the modified layer while shortening the time spent in step S312, which is less conducive to the formation of the modified layer. Therefore, throughput can be easily improved.
[0053] In at least a portion of step S311, it is preferable to control the APC valve 244 so that its opening degree is at the lower limit of a predetermined range. This makes it easier to further reduce the proportion of the first gas supplied into the processing chamber 201 that is exhausted from the processing chamber 201 without contributing to the formation of the reformed layer. Therefore, the etching rate can be further improved.
[0054] It is preferable to control the APC valve 244 so that its opening is maintained at the lower limit of a predetermined range for at least a portion of the duration of step S311. This makes it easier to significantly reduce the proportion of the first gas supplied into the processing chamber 201 that is exhausted from the processing chamber 201 without contributing to the formation of the reformed layer.
[0055] Now, consider the case where step S311 is performed while supplying plasma-enhanced chemical species (for example, the first gas or another gas that has been plasma-enhanced) to the wafer 200 (i.e., under plasma conditions). In this case, the material on the wafer 200 is more likely to be altered, i.e., damaged by the plasma, than when step S311 is performed without supplying plasma-enhanced chemical species to the wafer 200 (i.e., under non-plasma conditions). However, under non-plasma conditions, the formation of the modified layer is difficult, so throughput tends to decrease, and in-plane uniformity tends to decrease due to variations in the heating of the first gas on the surface of the wafer 200. According to the technology of this disclosure, it is possible to suppress the disadvantages of performing step S311 under non-plasma conditions while easily obtaining the advantages of performing step S311 under non-plasma conditions.
[0056] [Step S32: Removal Process] In step S32, reactive gases in the processing chamber 201 are removed between the end of step S31 and the start of step S33. Specifically, the opening of the APC valve 244 is controlled to evacuate the processing chamber 201. This removes unreacted first gases remaining in the processing chamber 201 and reaction by-products generated by the reaction between the first gases and the surface of the wafer 200 (i.e., the surface of a predetermined substance). At this time, valves 243c and 243d may be opened to maintain the supply of inert gas to the processing chamber 201. In other words, the processing chamber 201 may be purged. At this time, the inert gas acts as a purge gas. This allows for efficient removal of reactive gases from the processing chamber 201.
[0057] It is preferable to make the pressure in the processing chamber 201 at the end of step S312 higher than the pressure in the processing chamber 201 at the end of step S32. Even in this case, the etching rate can be sufficiently improved. In addition, since the time required to perform step S312 can be shortened, throughput can be further improved.
[0058] [Step S33: Second gas supply step] In step S33, the second gas is supplied to the wafer 200. This converts at least a portion of the modified layer into a volatile substance containing a predetermined element M.
[0059] Specifically, valve 243b is opened, and the second gas flows into the gas supply pipe 232b. The flow rate of the second gas is regulated by MFC 241b and supplied to the processing chamber 201 via nozzle 249b. Valves 243c and 243d are also opened, and inert gas flows into the gas supply pipes 232c and 232d. The flow rate of the inert gas is regulated by MFC 241c and 241d and supplied to the processing chamber 201 via nozzles 249a and 249b. The second gas and inert gas supplied to the processing chamber 201 are exhausted through the exhaust pipe 231 via APC valve 244.
[0060] Examples of processing conditions in step S33 include: processing pressure: 150 to 400 Pa, preferably 200 to 300 Pa; supply flow rate of the second gas: 0.1 to 10 slm; supply flow rate of the inert gas (each gas supply pipe): 0 to 10 slm; and processing time: 0.1 to 300 seconds, preferably 5 to 200 seconds.
[0061] As the second gas, for example, a gas containing chlorine (Cl) in its molecular structure (Cl-containing gas) can be used. 2 ), boron trichloride (BCl 3 ), carbon tetrachloride (CCl 4 ), thionyl chloride (SOCl 2 ), sulfuryl chloride (SO 2 Cl 2 ), phosgene (COCl 2 ), phosphorus trichloride (PCL 3 ), phosphorus pentachloride (PCL 5 ), silicon tetrachloride (SiCl 4 ), chlorodimethylaluminum (C 2 H 6 AlCl), Titanium tetrachloride (TiCl 4 ), aluminum trichloride (AlCl 3 ) etc. can be used. One or more of these can be used as the second gas.
[0062] It is preferable to perform step S33 under conditions that allow for easier exhaust of the gas in the processing chamber 201 than in step S311. This makes it easier to remove reaction products generated by the reaction originating from the second gas from the processing chamber 201. As a result, impurities are less likely to remain on the surface of the predetermined substance after the etching process. In addition, reaction products adhering to the surface of the wafer 200 can suppress inhibition of the reaction by the first and second gases.
[0063] [Step S34: Removal Process] In step S32, the reactive gas in the processing chamber 201 is removed between the end of step S33 and the start of the next step S34. Specifically, the processing chamber 201 is evacuated or purged using the procedure exemplified in step S33.
[0064] [Performed a predetermined number of times] The cycle of performing steps S31 to S34 described above is performed a predetermined number of times (n times, where n is an integer of 1 or more). As a result, at least a portion of the predetermined substance is removed from the wafer 200. That is, at least a portion of the predetermined substance is etched.
[0065] (Step S4: Pressure and Temperature Adjustment Process) Inert gas is supplied into the processing chamber 201 from gas supply pipes 232c and 232d, respectively, and exhausted from exhaust pipe 231. This purges the processing chamber 201, removing any remaining gases and reaction by-products (after-purging). Subsequently, the atmosphere inside the processing chamber 201 is replaced with inert gas (inert gas replacement), and the pressure inside the processing chamber 201 is returned to atmospheric pressure (atmospheric pressure return).
[0066] (Step S5: Substrate unloading process) The seal cap 219 is lowered by the boat elevator 115, and the lower end of the reaction tube 203 is opened. Then, the processed wafer 200, supported by the boat 217, is unloaded from the lower end of the reaction tube 203 to the outside of the reaction tube 203 (boat unloading). The processed wafer 200 is removed from the boat 217 (wafer discharge).
[0067] (3) Modified Examples Modified examples of the above-described embodiments will be explained below. The following will mainly explain the differences between these modified examples and the above-described embodiments, and will omit explanations of the similarities. In addition, in these modified examples, elements that are substantially the same as those described above will be denoted by the same reference numerals, and their explanations will be omitted.
[0068] Figure 5 schematically shows the time change of pressure in the processing chamber 201 at each step in step S31 of the modified example. In step S31 of the embodiment described above, step S312 started simultaneously with the end of step S311. In contrast, in step S31 of this modified example, as shown in Figure 5, step S313 is further included between the end of step S311 and the start of step S312.
[0069] <Step S313> As shown in Figure 5, in step S313, the pressure inside the processing chamber 201 is kept constant. At this time, the first gas may or may not be supplied to the wafer 200 having the predetermined substance inside the processing chamber 201. In either case, at least some of the effects described above can be obtained.
[0070] The following explanation will use the case where the first gas is supplied in step S313, or in other words, where the supply of the first gas continues from step S311, as an example.
[0071] In step S313, valve 243a is opened, and the first gas flows into the gas supply pipe 232a. The flow rate of the first gas is regulated by MFC 241a and supplied to the processing chamber 201 via nozzle 249a. Valves 243c and 243d are also opened, and inert gas flows into the gas supply pipes 232c and 232d. The flow rate of the inert gas is regulated by MFC 241c and 241d and supplied to the processing chamber 201 via nozzles 249a and 249b. The first gas and inert gas supplied to the processing chamber 201 are exhausted through the exhaust pipe 231 via APC valve 244, which is controlled to maintain a constant pressure in the processing chamber 201.
[0072] Examples of processing conditions in step S313 include: Maximum pressure: 1 to 200 torr, preferably 5 to 100 torr Supply flow rate of the first gas: 0.1 to 10 slm Supply flow rate of the inert gas (each gas supply pipe): 0.1 to 10 slm Processing time: 5 to 200 seconds, preferably 10 to 100 seconds.
[0073] In step S313, the pressure inside the processing chamber 201 is kept constant. Therefore, in step S313, at least one of the following is performed: the flow rate of the first supply and inert gas supplied into the processing chamber 201 (total supply flow rate) is made smaller than in step S311, and the amount of gas exhausted from the processing chamber 201 (exhaust flow rate) is made larger. In either case, in step S313, the formation of the reformed layer by the first gas per unit time is made less likely than in step S311.
[0074] Therefore, in step S31 of this modified example, it is preferable to make the time spent performing step S311 longer than the time spent performing step S313, as shown in Figure 5. This allows for longer formation of the modified layer while shortening the time spent performing step S313, in which formation of the modified layer is less likely to occur. Consequently, the etching rate can be further improved while improving throughput.
[0075] It is preferable to control the APC valve 244 so that the opening degree of the APC valve 244 in step S313 is greater than the opening degree of the APC valve 244 in step S311. This makes it easier to reduce the proportion of the first gas supplied into the processing chamber 201 in step S311 that is exhausted from the processing chamber 201 without contributing to the formation of the reformed layer.
[0076] (4) Other aspects of this disclosure. One aspect of this disclosure has been described in detail above. However, this disclosure is not limited to the aspects described above and can be modified in various ways without departing from its essence.
[0077] The embodiments and modifications described above have been explained using the case where an oxide of a predetermined element M is used as the predetermined substance. However, the technology of this disclosure is not limited thereto. For example, the elemental form of the predetermined element M or a nitride of the predetermined element may be used as the predetermined substance. Furthermore, when etching the elemental form of the predetermined element M or a nitride of the predetermined element, for example, an oxidizing gas may be used as the first gas and a halogen-based gas as the second gas. In addition, etching of the predetermined substance may be performed by appropriately selecting a first gas and / or second gas not mentioned above. Even in these cases, at least some of the effects described above can be obtained.
[0078] As the oxidizing gas, for example, gases containing oxygen (O) and hydrogen (H) can be used. As an example of an O and H-containing gas, water vapor (H) 2 O gas), hydrogen peroxide (H 2 O 2 ) gas, hydrogen (H 2 ) gas + oxygen (O 2 ) Gas, H 2 Gas + Ozone (O 3 ) gases can be used. In addition to gases containing O and H, oxygen (O)-containing gases can be used as oxidizing gases. For example, O 2 Gas, O 3 Gas, nitrous oxide (N) 2 O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO) 2 ) gas, carbon monoxide (CO) gas, carbon dioxide (CO) gas 2 Gases such as ) can be used. Note that gases containing O and H are also a type of O-containing gas. One or more of these can be used as the oxidizing gas.
[0079] As halogenated gases, for example, the F-containing gas or Cl-containing gas mentioned above can be used.
[0080] In addition, in the above-described embodiments and modifications, at least one of the first gas and the second gas may be a gas excited by plasma. In this case as well, at least some of the effects described above can be obtained.
[0081] Furthermore, it is preferable that the recipes used for substrate processing be prepared individually according to the processing content and stored in the storage device 121c via a telecommunications line or external storage device 123. When starting substrate processing, it is preferable that the CPU 121a appropriately selects the appropriate recipe from among the multiple recipes stored in the storage device 121c according to the processing content. This makes it possible to form films of various film types, composition ratios, film quality, and film thickness with good reproducibility using a single substrate processing device. In addition, it is possible to reduce the burden on the operator and start substrate processing quickly while avoiding operational errors.
[0082] The above-mentioned recipes are not limited to newly created ones; they may also be prepared, for example, by modifying existing recipes already installed in the board processing device. When modifying a recipe, the modified recipe may be installed in the board processing device via a telecommunications line or a recording medium containing the recipe. Alternatively, existing recipes already installed in the board processing device may be directly modified by operating the input / output device 122 provided in the existing board processing device.
[0083] Furthermore, the above-described embodiments described an example of processing a film using a batch-type substrate processing apparatus that processes multiple wafers 200 at once. This disclosure is not limited to the above-described embodiments. For example, it can be suitably applied when processing a film using a single-wafer substrate processing apparatus that processes one or several wafers 200 at once. Furthermore, the above-described embodiments described an example of processing a film using a substrate processing apparatus having a hot-wall type processing furnace. This disclosure is not limited to the above-described embodiments and can be suitably applied when processing a film using a substrate processing apparatus having a cold-wall type processing furnace.
[0084] Even when using these substrate processing devices, processing can be performed using the same processing procedures and conditions as described above for the embodiments and modifications, and the same effects as described above for the embodiments and modifications can be obtained.
[0085] Furthermore, the above-described embodiments and modifications can be used in appropriate combinations. The processing procedure and processing conditions in this case can be the same as, for example, the processing procedure and processing conditions of the above-described embodiments and modifications.
[0086] 200 Wafers (substrates) 201 Processing room
Claims
1. A substrate processing method comprising: (a) a step of supplying a first gas to a substrate placed in a processing chamber while increasing the pressure in the processing chamber; (a2) a step of reducing the pressure in the processing chamber after the completion of (a1), wherein (a1) is performed two or more times with (a2) in between, to form a modified layer on the surface of a predetermined substance on the substrate; and (b) a step of supplying a second gas to the substrate and converting at least a portion of the modified layer into a volatile substance.
2. The substrate processing method according to claim 1, wherein in at least a portion of (a2), the flow rate of the first gas supplied to the substrate is less than the flow rate of the first gas supplied to the substrate in (a1), or the first gas is not supplied to the substrate.
3. The substrate processing method according to claim 1, wherein the time spent performing (a1) is longer than the time spent performing (a2).
4. The substrate processing method according to claim 1, wherein the amount of decrease in pressure inside the processing chamber per unit time in (a2) is greater than the amount of increase in pressure inside the processing chamber per unit time in (a1).
5. The substrate processing method according to claim 1, wherein the processing chamber is connected to an exhaust device via an exhaust valve whose opening degree can be continuously controlled within a predetermined range, and in at least a portion of (a1), the exhaust valve is controlled so that the opening degree of the exhaust valve is the lower limit of the predetermined range.
6. The substrate processing method according to claim 5, wherein the exhaust valve is controlled so that the opening degree of the exhaust valve is maintained at the lower limit value for at least a portion of the period of (a1).
7. A substrate processing method according to any one of claims 1 to 6, wherein (a1) is performed without supplying plasma-generated chemical species to the substrate.
8. A substrate processing method according to any one of claims 1 to 6, further comprising the step of removing reactive gases in the processing chamber between the end of (a) and the start of (b), wherein the pressure in the processing chamber at the end of (a2) is higher than the pressure in the processing chamber at (c).
9. The substrate processing method according to any one of claims 1 to 6, wherein (b) is performed under conditions that allow the gas in the processing chamber to be more easily exhausted than in (a1).
10. The substrate processing method according to any one of claims 1 to 6, wherein (a) starts simultaneously with the completion of (a1).
11. The substrate processing method according to any one of claims 1 to 6, further comprising (a) a step of keeping the pressure in the processing chamber constant between the end of (a1) and the start of (a2).
12. The substrate processing method according to claim 11, wherein the time spent performing (a1) is longer than the time spent performing (a3).
13. The substrate processing method according to any one of claims 1 to 4, wherein (a) further comprises the step of making the pressure in the processing chamber constant between the end of (a1) and the start of (a2), the processing chamber is connected to an exhaust device via an exhaust valve whose opening degree can be continuously controlled within a predetermined range, and the exhaust valve is controlled such that the opening degree of the exhaust valve in (a3) is greater than the opening degree of the exhaust valve in (a1).
14. The substrate processing method according to any one of claims 1 to 6, wherein the first gas contains fluorine in its molecular structure and the second gas contains chlorine in its molecular structure.
15. A method for manufacturing a semiconductor device, comprising: (a) a step of supplying a first gas to a substrate placed in a processing chamber while increasing the pressure in the processing chamber; (a2) a step of reducing the pressure in the processing chamber after the completion of (a1), wherein (a1) is performed two or more times with (a2) in between, to form a modified layer on the surface of a predetermined substance on the substrate; and (b) a step of supplying a second gas to the substrate to convert at least a portion of the modified layer into a volatile substance.
16. A program that causes a substrate processing apparatus to execute a procedure by computer, the procedure comprising: (a) a procedure of supplying a first gas to a substrate placed in a processing chamber while increasing the pressure in the processing chamber; (a2) a procedure of decreasing the pressure in the processing chamber after the completion of (a1), wherein (a1) is performed two or more times with (a2) in between, to form a modified layer on the surface of a predetermined substance on the substrate; and (b) a procedure of supplying a second gas to the substrate and converting at least a portion of the modified layer into a volatile substance.
17. A substrate processing apparatus comprising: a processing chamber in which a substrate is disposed; a first supply system for supplying a first gas to the substrate; a second supply system for supplying a second gas to the substrate; a pressure adjustment unit for controlling the pressure inside the processing chamber; and a control unit configured to control the first supply system, the second supply system, and the pressure adjustment unit so as to perform a process comprising: (a) (a1) a process of supplying the first gas to the substrate while increasing the pressure inside the processing chamber; (a2) a process of reducing the pressure inside the processing chamber after the completion of (a1), wherein (a1) is performed two or more times with (a2) in between, thereby forming a modified layer on the surface of a predetermined substance on the substrate; and (b) a process of supplying the second gas to the substrate and converting at least a portion of the modified layer into a volatile substance.