Vacuum vapor deposition apparatus and device manufacturing method using same

The vacuum vapor deposition apparatus addresses inaccuracies in quantum device fabrication by ensuring uniform metal deposition angle and thickness, enhancing qubit integration and coherence through controlled substrate movement and an opening limiting member.

WO2026235238A1PCT designated stage Publication Date: 2026-11-12KOREA ADVANCED NANO FAB CENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2025/014979
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2025-09-24
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional vacuum vapor deposition methods result in varying metal deposition thickness and angle of incidence due to substrate positioning, leading to inaccuracies in fabricating quantum technology devices like Josephson devices, particularly affecting qubit integration and coherence.

Method used

A vacuum vapor deposition apparatus with an opening limiting member and controlled substrate movement, allowing precise deposition by ensuring uniform metal incidence angle and thickness across the substrate surface.

Benefits of technology

The apparatus significantly reduces deposition errors, enabling accurate fabrication of Josephson devices and qubits with improved coherence and reduced equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2025014979_12112026_PF_FP_ABST
    Figure KR2025014979_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a vacuum vapor deposition apparatus and a device manufacturing method using same. The disclosed vacuum vapor deposition apparatus may comprise: a source emitter that emits a source material in a vacuum chamber; an opening-defining member that is spaced apart from the source emitter in the Y-axis direction, has a surface disposed parallel to the XZ plane along the X-axis and the Z-axis perpendicular to the Y-axis in a basic arrangement, and has an opening through which the source material passes, the opening extending in the X-axis or the Z-axis direction; and a substrate holder which is spaced apart from the source emitter and on which is mounted a substrate on which the source material that has passed through the opening is deposited.
Need to check novelty before this filing date? Find Prior Art

Description

Vacuum vapor deposition apparatus and method for manufacturing devices using the same

[0001] The present invention relates to a deposition apparatus and device manufacturing technology, and more specifically, to a vacuum vapor deposition apparatus and a method for manufacturing a device using the same.

[0002] The national research and development projects that supported this invention are as follows.

[0003] Project ID 1711183984

[0004] Project Number 2023M3H3A1059080

[0005] Ministry of Science and ICT

[0006] Project Management Agency Name: National Research Foundation of Korea

[0007] Research Project Name: Original Technology Development Project

[0008] Research Project Title: Establishment of Quantum Device Manufacturing Infrastructure Based on General-Purpose Equipment

[0009] Project Implementing Organization Name: Korea Institute of Nanotechnology

[0010] Research Period: 2023.02.07 ~ 2025.12.31

[0011] In order for quantum computers to achieve a practical level capable of performing calculations impossible with classical von Neumann computers—that is, to secure quantum supremacy—at least hundreds to thousands of qubits (i.e., quantum bits) must be integrated. In fact, some companies have presented roadmaps to achieve 1,121 qubit integration by 2023 and are planning for up to one million qubit QPUs (quantum process units) in the long term. In the case of superconducting qubits, which are currently the most technologically advanced, an integration density of over 1,000 qubits has been achieved and is continuously evolving.

[0012] Superconducting qubits are classified into charge qubits, phase qubits, and flux qubits depending on their method, and all of them use Josephson devices as core active components. Among these, the charge qubit is evaluated as having the best performance, particularly in terms of long coherence time. Charge qubits are divided into transmon qubits and other charge qubits (general charge qubits) depending on their detailed design, and can be divided into fixed frequency qubits and tunable frequency qubits depending on the presence or absence of frequency control functions by the Josephson devices used. Currently, the fixed frequency transmon type demonstrates the best performance and has achieved an integration density of over 1,000 qubits. Here, the aforementioned frequency corresponds to the quantized energy interval (energy gap) of the superconducting qubit.

[0013] Charge qubits fabricated using superconducting circuits are fundamentally composed of capacitors and Josephson elements (Josephson junctions). The energy of the capacitor is interpreted as kinetic energy, and the energy of the Josephson element (Josephson junction) as potential energy. When the total energy of the system, i.e., the Hamiltonian, is quantized, the intervals between the resulting multiple energy levels can differ. Therefore, a superconducting circuit containing Josephson elements and capacitors can be utilized as a qubit with anharmonicity. Among the discontinuous energy levels, the lowest ground state and the first excited state can be used as the 0 state and 1 state, respectively. In this case, the Hamiltonian of the qubit ( ) can be given as in mathematical formula 1 below.

[0014] [Mathematical Formula 1]

[0015]

[0016] In mathematical formula 1, charging energy (E C ), Josephson energy (E J ), number operator( ) and offset charge (n g ) can be defined as shown in mathematical formulas 2 to 5 below.

[0017] [Mathematical Formula 2]

[0018]

[0019] [Mathematical Formula 3]

[0020]

[0021] [Mathematical Formula 4]

[0022]

[0023] [Mathematical Formula 5]

[0024]

[0025] In the mathematical equations above, C and Q (i.e., Q J ) are capacitance and charge, respectively, and I C is the critical current value of the Josephson junction, and Φ0 is the magnetic flux quanta. ε₀ is Dirac's constant, and e is the elementary charge. The magnetic flux quantum (Φ₀) is given by the following mathematical equation 6.

[0026] [Mathematical Formula 6]

[0027]

[0028] In mathematical equation 6, h is the Planck constant.

[0029] Using the above mathematical formulas, the eigenvalue of energy (energy level) is obtained as shown in mathematical formula 7 below.

[0030] [Mathematical Formula 7]

[0031]

[0032] Referring to Equation 7, the initial energy gap is √8E C E J value( It is determined by ), and thereafter, as the energy level increases, depending on the energy level From E C The value obtained by subtracting an integer multiple of the value corresponds to the energy difference between the two levels. In Equation 7, ω is the angular frequency and m is an integer.

[0033] From the above, the energy and anharmonicity of a qubit are E C and E J It can be seen that it is determined by a combination of values. In particular, energy values Even if the qubit energy is the same because it is identical, E C and E J It can be seen that the anharmonicity varies depending on the ratio.

[0034] In the case of a typical charged qubit, E C and E J is designed with similar values, and in this case, anharmonicity becomes significantly large. However, E C and E J In cases where they are similar, there is a problem where the coherence lifetime is shortened due to significant influence from charge noise. On the other hand, in the case of transmon qubits, E J / E C The ratio is determined to be approximately 30–50 or higher; in this case, it is hardly affected by charge noise, so the offset charge (n gWhile it has the advantage of eliminating the need for ), anharmonicity is reduced, and E C and E J If the value is not precisely controlled, the energy (E) that excites from the 0 state to the 1 state 0,1 A problem may arise where the energy can excite the 1st state to the 2nd state. The case where the energy used to excite the 0th state to the 1st state instead excites the 1st state to the 2nd state is called leakage.

[0035] Even if the anharmonicity is small, if only a single qubit is controlled, the microwave signal can be precisely controlled to prevent leakage; however, in devices such as QPUs that require multiple qubits, there may be cases where the microwave signal controlling a specific qubit ends up controlling an adjacent qubit. In particular, for example, E of the first qubit 0,1 (i.e., the energy that excites from the 0 state to the 1 state) is the E of the second qubit 1,2 If it is equal to (i.e., energy that excites from state 1 to state 2), the microwave signal controlling the first qubit can cause leakage of the second qubit.

[0036] Generally, the energy of a qubit can be determined between approximately 4 GHz and 8 GHz, taking into account factors such as operating temperature and dielectric loss, and the anharmonicity of the transmon can be around several hundred MHz, which is a few percent of the energy size. When the anharmonicity is only a few percent of the qubit energy, if the energy of the qubit has a variation of a few percent due to process variation (error), various forms of frequency interference can occur between qubits, which can be referred to as frequency collision or frequency crowding.

[0037] E due to process variation (error) C and E J Value dispersion can be an unavoidable problem, and among these, especially E J The dispersion of values ​​can cause problems. E J The value is ultimately I C It can be determined by the value, and I C The value is given as follows by the experimental Ambegaokar-Baratoff relation.

[0038] [Mathematical Formula 8]

[0039]

[0040] In Equation 8, Δ represents the superconducting gap energy, and Rn (normal resistance) is the resistance value of the Josephson junction measured at room temperature (room temperature resistance). Since Rn is a resistance value, it is determined by the structure of the Josephson device, such as the area of ​​the Josephson junction and the thickness of the insulating film; consequently, E J The value can be determined. E C Although the dispersion of values ​​can affect changes in device characteristics, in the case of transmon, since the capacitance is designed to be large, E C Rather than the dispersion of E J Dispersion can play a decisive role.

[0041] E J is I C Depends on the value and I C The value can be determined by the Rn value. The Rn value can be determined by the structure of the Josephson device, namely the area and the thickness of the insulating film. Therefore, in the fabrication of Josephson devices, it is necessary to reduce process errors and realize a junction surface (Josephson junction surface) of accurate size.

[0042] Josephson devices are typically fabricated through a process known as the Dolan process or the Manhattan process, both of which involve the deposition of superconducting metal by angle evaporation in two different directions.

[0043] To describe the Dolan process as an example, first, as illustrated in FIG. 1, two photoresists with different sensitivities to electron beam lithography, namely the first and second photoresists (110, 120), are formed sequentially on a substrate (100), and exposure and development are performed. Then, the first photoresist (110) located at the bottom is developed and removed more, thereby creating a cross-sectional profile in which an undercut is formed. Using this photoresist pattern, as illustrated in FIG. 2, a substrate (100) can be tilted at a specific angle to deposit a first metal film (130) (e.g., an Al film) for fabricating a Josephson device, and oxygen can be introduced to oxidize the surface portion of the first metal film (130) to form an oxide film (140) (e.g., an Al oxide film) of a certain thickness. Then, the substrate (100) can be tilted in a direction different from that of the first metal film (130) to deposit a second metal film (150) (e.g., an Al film). After this process, a Josephson device can be formed in which the first metal film (130) and the second metal film (150) overlap only partially, and an insulator, i.e., an oxide film (140), is located between them. A Josephson junction is defined in the region where the first metal film (130) and the second metal film (150) overlap each other. For convenience, the first photoresist (110) of Fig. 1 in Fig. 2 is not shown.

[0044] In this fabrication method, not only the size and height of the photoresist but also the deposition angle of the metal is an important factor in determining the size of the fabricated device. However, due to the structure of current electron beam evaporator equipment, the method of depositing material on an inclined surface has a problem in that the thickness of the deposited metal varies depending on the position of the substrate, and an even greater problem is that the deposition angle of the metal varies depending on the position of the substrate. In processes using a conventional electron beam evaporator, it is common to rotate the substrate in two ways—rotation and revolution—to deposit a uniform thin film, but since such rotation cannot be used in the fabrication of Josephson devices, the aforementioned problems may be unavoidable.

[0045] Referring to FIG. 3, if the metal source generation part (200 + 300) is assumed to be a rough point light source, the amount of flux (400) of the source material has symmetry with respect to the centerline, so it can be said that an equal amount of metal evaporates and proceeds on both sides with respect to the centerline. Here, reference numeral 200 represents a crucible containing the metal source material, and reference numeral 300 represents a crucible holder having an electron beam gun. However, if the substrate (100) is positioned at an angle, the cross-sectional areas of the parts of the substrate (100) located on the left and right sides become different from each other, so one half of the substrate (100) (the right half in the drawing) receives more flux (400) than the other half (the left half in the drawing), and as a result, the metal is deposited with a thick thickness. As one way to overcome these problems, a method such as that described in prior art 1 (WO 2022 / 067433 A1) has been proposed.

[0046] The second problem is that when deposition is performed with the substrate positioned at an angle, the angle of incidence of the metal source material being deposited varies depending on the position of the substrate. If the angle of incidence of the metal source material varies depending on the position of the substrate, the length and width of the metal pattern being deposited will vary depending on the position of the substrate. Consequently, the length and width of the Josephson device (Josephson junction) will vary depending on the position of the substrate. Although this deviation decreases as the distance between the metal source generator and the substrate increases, as the distance increases, not only does the waste of the source become more severe, but the cost of maintaining the vacuum of the deposition chamber also increases significantly. As a method to overcome the above problem, a method of correcting the design size of the Josephson device by setting different sizes for each position of the substrate so that the Josephson devices are fabricated to a desired size or the same size was presented in Prior Art 2 (Wafer-scale uniformity improvement of Dolan bridge Josephson junction by shadow evaporation bias correction, arXiv.2403.01894). However, in the case of pattern correction methods, there is a problem in that the pattern size must be corrected individually according to the position on the substrate, and correction must be performed whenever the position or size of the device changes.

[0047] The technical problem that the present invention aims to solve is to provide a vacuum vapor deposition apparatus that enables the fabrication of devices with more accurate and precise sizes by reducing the error (dispersion) in the deposition process depending on the position of the substrate, for example, in the manufacturing of quantum technology-related devices such as Josephson devices.

[0048] In addition, the technical problem that the present invention aims to solve is to provide a method for manufacturing a device using the vacuum vapor deposition apparatus described above.

[0049] The problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be understood by those skilled in the art from the description below.

[0050] According to one embodiment of the present invention, a vacuum vapor deposition apparatus using an evaporation method comprises: a source emitter that emits a source material through evaporation within a vacuum chamber; and an opening limiting member positioned above the source emitter within the vacuum chamber at a distance in the y-axis direction, wherein in a basic arrangement, the surface thereof is arranged parallel to an xz plane along the x-axis and z-axis perpendicular to the y-axis, and has an opening through which the source material passes, wherein the opening has a structure extending in the x-axis to z-axis direction in the basic arrangement. A vacuum vapor deposition apparatus using an evaporation method is provided, comprising: a substrate holder positioned within the vacuum chamber with the opening limiting member in between and spaced apart from the source emitter, wherein the substrate is mounted such that the surface of the substrate on which the source material passing through the opening is deposited faces downward; wherein the substrate holder is configured to be movable along at least one of a first parallel direction parallel to the substrate and a second parallel direction parallel to the substrate and perpendicular to the first parallel direction, wherein in the basic arrangement, the first parallel direction is parallel to the z-axis and the second parallel direction is parallel to the x-axis, and the substrate holder and the opening limiting member are configured to be rotatable about the z-axis.

[0051] The center of the source emitter and the center of the opening can be positioned on a vertical line.

[0052] The above substrate holder may be configured to rotate at a controlled angle with respect to the z-axis, in a first rotational direction and a second rotational direction opposite thereto, respectively.

[0053] The above opening may have a slit shape.

[0054] The above opening may be extended in the x-axis direction and may have a length along the x-axis and a width along the z-axis, and the substrate holder may be configured to be movable linearly along at least the first parallel direction.

[0055] The above opening may be extended in the z-axis direction and may have a length along the z-axis and a width along the x-axis, and the substrate holder may be configured to be movable linearly along at least the second parallel direction.

[0056] The above opening may have a length along either the x-axis or the z-axis and a width along the other of the x-axis and the z-axis, and the width of the opening may be in the range of about 0.1 to 10 cm.

[0057] The vacuum vapor deposition device described above can be configured to variably adjust the width of the opening.

[0058] When the center of the substrate is located on the center of the opening, the center of the substrate, the center of the opening, and the center of the source emitter can be arranged on a vertical line.

[0059] A shutter member may be further provided, disposed between the source emitter and the opening limiting member, for blocking or allowing the movement of the source material toward the opening limiting member or controlling it in another way.

[0060] The vacuum vapor deposition apparatus may further include a mechanical component to which the substrate holder and the opening limiting member are connected or coupled, and the mechanical component may be configured to allow the substrate holder to move along at least one of the first and second parallel directions, and may be configured to allow the substrate holder and the opening limiting member to rotate about the z-axis.

[0061] The vacuum vapor deposition apparatus may further include first and second mechanical components to which the substrate holder and the opening limiting member are connected or coupled, and the substrate holder and the opening limiting member may be disposed between the first and second mechanical components, and the first and second mechanical components may be configured to allow the substrate holder to move along at least one of the first and second parallel directions, and may be configured to allow the substrate holder and the opening limiting member to rotate about the z-axis.

[0062] The vacuum vapor deposition apparatus may further include a support member that directly or indirectly supports the substrate holder on the side opposite to where the opening limiting member is positioned.

[0063] The above opening limiting member may be configured to function as a gas injection part for injecting gas into the vacuum chamber.

[0064] The vacuum vapor deposition apparatus described above may be configured to perform a deposition process with the substrate holder rotated by a given angle with respect to the z-axis.

[0065] The vacuum vapor deposition apparatus described above may be configured to perform a deposition process over the entire effective area of ​​the substrate surface while continuously moving the substrate holder at a given speed.

[0066] The vacuum vapor deposition apparatus may be configured to perform a deposition process over the entire effective area of ​​the substrate surface in a step-and-repeat manner, and in the step-and-repeat manner, after performing a deposition process for the Nth area of ​​the substrate surface, the substrate holder may be moved and a deposition process for the N+1th area of ​​the substrate surface may be performed.

[0067] According to another embodiment of the present invention, a method for manufacturing a device is provided, comprising the step of depositing a material film using the vacuum vapor deposition apparatus described above.

[0068] The above device may include a Josephson device.

[0069] The above method for manufacturing the device may include the steps of: forming a first superconducting material film on the substrate while the substrate holder and the opening limiting member are rotated with respect to the z-axis at a first angle condition; forming an insulating film on the surface of the first superconducting material film; and forming a second superconducting material film on the insulating film while the substrate holder and the opening limiting member are rotated with respect to the z-axis at a second angle condition different from the first angle condition.

[0070] In each of the step of forming the first superconducting material film and the step of forming the second superconducting material film, the substrate holder can be moved along at least one of the first and second parallel directions.

[0071] According to an embodiment of the present invention, a vacuum vapor deposition apparatus can be implemented that enables the fabrication of a device with a more accurate and precise size by reducing the error (dispersion) of the deposition process according to the position of the substrate in the manufacture of a quantum technology-related device, such as a Josephson device. Furthermore, according to an embodiment of the present invention, a method for fabricating a device using the above-described vacuum vapor deposition apparatus can be implemented.

[0072] Conventional evaporators have a fundamental limitation in that the amount of metal deposited and the angle of incidence vary depending on the position of the substrate, due to the characteristic that the source travels radially (partially radially) at a constant angle from a metal source generator having a relatively small cross-sectional area and is deposited. Among these limitations, the problem of varying metal amounts can be partially mitigated by the aforementioned prior art 1, but the problem of varying angles of incidence, which is a more significant issue, has not been resolved at the equipment level, and a method for correcting the substrate pattern has been proposed in the aforementioned prior art 2. However, in the case of the pattern correction method, the pattern size must be corrected individually according to the position of the substrate, and there is a problem that correction must be performed whenever the position or size of the device changes.

[0073] According to one embodiment of the present invention, a vacuum vapor deposition apparatus and a related method can be implemented that can drastically reduce process error (dispersion) by using an opening limiting member, for example, having an opening in the shape of a slit, to allow the source material to pass only through the opening, and by moving the position of the substrate on which a predetermined mask pattern is formed, making the incident amount and incident angle of the source material uniform or nearly uniform across the entire effective area of ​​the substrate.

[0074] In addition, according to one embodiment of the present invention, since the distance between the source emitter and the substrate can be reduced, the excessive consumption of the source that occurs when deposition is performed only through the opening can be compensated for, and furthermore, as the equipment size is reduced, the effect of reducing equipment manufacturing costs and operating costs such as vacuum maintenance costs can be obtained.

[0075] However, the effects of the present invention are not limited to the above effects and can be extended in various ways without departing from the technical concept and scope of the present invention.

[0076] Figure 1 is a cross-sectional view showing the process of forming a photoresist pattern according to the Dolan process, which is one of the methods for fabricating Josephson junctions.

[0077] Figure 2 is a cross-sectional view showing a double angle evaporation process using a photoresist pattern having a Dolan bridge.

[0078] Figure 3 is a diagram illustrating the problem that the thickness of the metal deposited varies depending on the position of the substrate in angle evaporation.

[0079] FIGS. 4 and 5 are drawings that serve as the principle background of an embodiment of the present invention and explain how the angle of incidence of a source material deposited varies depending on the position of a tilted substrate.

[0080] FIG. 6 relates to an embodiment of the present invention and is a diagram exemplarily showing the fabrication process of a Josephson device.

[0081] FIGS. 7 and 8 are drawings that serve as the principle background of an embodiment of the present invention and explain how the angle of incidence of a source material deposited varies depending on the position of a tilted substrate.

[0082] Figure 9 is a diagram illustrating that the width of the Josephson element varies depending on the position shown in Figures 7 and 8.

[0083] Figure 10 is a diagram exemplarily showing the change in width of a Josephson junction along the z-axis direction of a substrate.

[0084] FIG. 11 is a drawing for explaining a vacuum vapor deposition apparatus using an evaporation method according to one embodiment of the present invention.

[0085] Figures 12 and 13 are drawings showing an enlarged view of a part of the configuration of the vacuum vapor deposition apparatus of Figure 11.

[0086] FIG. 14 is a plan view exemplarily showing an opening limiting member that can be applied to a vacuum vapor deposition apparatus according to one embodiment of the present invention.

[0087] FIG. 15 is a plan view exemplarily showing an opening limiting member that can be applied to a vacuum vapor deposition apparatus according to another embodiment of the present invention.

[0088] FIG. 16 is a drawing for explaining a vacuum vapor deposition apparatus using an evaporation method according to another embodiment of the present invention.

[0089] FIGS. 17a to 17c are cross-sectional views illustrating a method for manufacturing a device using a vacuum vapor deposition apparatus utilizing an evaporation method according to one embodiment of the present invention.

[0090] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0091] FIGS. 4 and 5 serve as the principle background for an embodiment of the present invention and are drawings intended to explain how the angle of incidence of a source material (metal) deposited varies depending on the position of a tilted substrate. FIGS. 4 and 5 are drawings exemplified for calculating the angle of incidence of a source material (metal) at a position r away from the center of the substrate along an inclined plane during the deposition of a first metal film (bottom metal) and a second metal film (top metal), respectively. FIG. 4 is a drawing intended to explain how the angle of incidence deposited varies depending on the position of the substrate during bottom metal angle evaporation, and FIG. 5 is a drawing intended to explain how the angle of incidence deposited varies depending on the position of the substrate during top metal angle evaporation.

[0092] Referring to Figures 4 and 5, even if the center of the substrate is positioned to achieve a desired deposition incidence angle, the incidence angle gradually increases at lower positions from the center, while conversely, the incidence angle gradually decreases at higher positions from the center.

[0093] When calculating the angles of metal incident on the center of the substrate and the ends of the x-axis, for a substrate diameter of approximately 20 cm (8-inch substrate), when the angle of incidence at the center of the substrate is 45°, the angle of incidence at the center remains unchanged for distances of 30 cm, 100 cm, and 150 cm between the center of the substrate and the metal source generator, respectively; however, the angles of incidence at the ends become 62° and 34°, 48.3° and 41.3°, and 47.8° and 42.4°. It can be seen that while the deviation in the angle of incidence decreases as the distance between the source generator and the substrate increases, a significant angle deviation exists even at a distance of 150 cm. If this distance is increased further, the deviation decreases, but the rate of decrease gradually diminishes; moreover, increasing the distance leads to a larger chamber size, which may be accompanied by the problem of increased cost and time required to create a vacuum. Depending on the size of the substrate, this deviation in the angle of incidence can cause the length of the Josephson device to vary by approximately 1–3% or more at different locations on the substrate.

[0094] FIG. 6 relates to an embodiment of the present invention and is a diagram illustrating the fabrication process of a Josephson device in an exemplary manner. Here, the reference numerals may be the same as those described in FIG. 1 and FIG. 2. Of the three drawings in FIG. 6, the top drawing is a plan view, and the two drawings below are cross-sectional views. For convenience, the first photoresist and the insulating film (e.g., oxide film) are not shown in FIG. 6. FIG. 6 is intended to explain the phenomenon in which the length of the Josephson junction fabricated varies depending on the position when the angle of incidence varies depending on the position of the substrate. In FIG. 6, "Position O" corresponds to the center of the substrate, and "Position A" and "Position B" correspond to positions A and B in FIG. 4 and FIG. 5.

[0095] Referring to Fig. 6, L is the length of the Josephson junction. JJis the length of the first metal film (bottom metal) (130) and the second metal film (top metal) (150), defined as the length from one end of the deposited metal to the end of the photoresist bridge, i.e., L B and L T The length of the photoresist bridge (L) from the sum of bridge It can be calculated by subtracting ). However, L B and L T Since it varies depending on the angle of metal deposition, if the angle of incidence varies depending on the position of the substrate, the length of the Josephson junction fabricated varies depending on the position of the substrate, which means that the frequency of the fabricated qubit will vary.

[0096] For example, the thickness of the first photoresist (t pr1 ) is 400 nm, and the length of the photoresist bridge (L bridge ) is 400 nm, and the thickness (t) of the first metal film (130) B When the () is set to 50 nm and the distance between the metal source generator and the center of the substrate is set to 80 cm, if the angle of incidence at the center of the substrate (100) is set to 45°, the angle of incidence at the lower end (lower side) 7.5 cm away from the center of the substrate (100) becomes 48.3°, and the angle of incidence at the higher end (higher side) 7.5 cm away becomes 41.3°.

[0097] Referring to the drawing and mathematical formula exemplified in FIG. 6, the length L of the Josephson joint JJ If we calculate, L at the center of the substrate JJ While is 350 nm, L at the lower point 15 cm from the center and the higher point 15 cm from the center JJare 345 nm and 358 nm, respectively, resulting in deviations of -1.4% and 2.3%. This calculation applies when the substrate is rotated so that the lower and higher sides of the substrate are reversed during the deposition of the first metal film (bottom metal) and the second metal film (top metal). If the substrate is rotated so that the lower side of the substrate during the deposition of the first metal film (bottom metal) remains the lower side during the deposition of the second metal film (top metal), then L JJ The deviation of is 20 to 25 percent or more.

[0098] Meanwhile, the variation in the width of the Josephson junction depending on the position of the substrate can be even more severe.

[0099] FIGS. 7 and 8 serve as the principle background for an embodiment of the present invention and are drawings to explain how the angle of incidence of a source material (metal) deposited varies depending on the position of a tilted substrate. FIGS. 7 and 8 illustrate drawings for calculating the angle of incidence of the metal according to the position of the substrate in the z-axis direction. FIG. 7 is a drawing to explain how the angle of incidence of deposition in the z-axis direction varies depending on the position in the z-axis direction from the center of the substrate, and FIG. 8 is a drawing to explain how the angle of incidence of deposition in the z-axis direction varies depending on the position in the z-axis direction from a position away from the center of the substrate in the x-axis direction.

[0100] Referring to FIGS. 7 and 8, a deviation in the incident angle in the z-axis direction of the substrate occurs, and this deviation acts in combination depending on the x-axis position, and this deviation causes a change in the width of the Josephson device. This change in the width of the Josephson device becomes more than approximately 7.3% when the distance between the source generator and the center of the substrate is 80 cm, even on a substrate of about 15 cm, thereby limiting the normal fabrication of the device.

[0101] FIG. 9 is a diagram illustrating how the width of a Josephson element varies depending on the position shown in FIG. 7 and FIG. 8. Of the four figures in FIG. 9, the top two figures are plan views, and the bottom two figures are cross-sectional views. FIG. 9 illustrates a diagram for calculating the width of a Josephson junction according to the angle of incidence. The width of the Josephson junction varies not only depending on the position in the z-axis direction but also on the position in the x-axis direction.

[0102] FIG. 10 is a diagram illustrating the variation in the width of a Josephson junction along the z-axis direction of a substrate. As can be seen in FIG. 10, at the center of the substrate where the incident angle of the metal source in the z-axis direction is perpendicular, the width of the Josephson junction is formed at 300 nm, which is the width of the photoresist pattern; however, as the distance along the z-axis direction increases, the variation in width can exceed approximately -7.3%. This deviation may decrease as the distance between the metal source generation unit and the substrate increases, but increasing the distance leads to greater waste of the source and significantly increases the cost of maintaining the vacuum of the deposition chamber. However, the degree of width variation shown in FIG. 10 is presented exemplarily under specific given conditions and may vary depending on the conditions.

[0103] Qubits utilizing superconducting circuits may include Josephson devices (Josephson junctions), and the characteristics of the qubit can be significantly influenced by the characteristics of the Josephson devices (Josephson junctions). For example, in the case of transmon, the E of the Josephson device J The energy gap of a qubit can be determined by the value, and anharmonicity can also be determined. E JThe value can be determined by the size of the Josephson device and the thickness of the insulating film, but the device size can be significantly affected not only by the size of the photoresist pattern but also by the angle of metal deposition (angle of incidence of the source). Due to the limitations of conventional metal deposition methods, the deposition angle varying at different locations on the substrate can be a problem. In the case of a 6-inch substrate, the variation in the width of the Josephson device can exceed 7.3%, and the variation can increase further as the substrate size increases. Considering that general quantum computers require a frequency variation of approximately 1–2% or less, the aforementioned dimensional variation (width variation) is a very large variation that can limit the implementation and operation of a normal quantum computer.

[0104] Embodiments of the present invention may provide, for example, a deposition apparatus and a related method for the uniform or accurate (precision) fabrication of a superconducting Josephson device. In particular, embodiments of the present invention may provide a deposition apparatus and a related method for ensuring the uniformity and / or precision of the Josephson junction size, which is essential for accurately controlling the frequency of a qubit, in the fabrication of a superconducting quantum qubit with a fixed frequency structure and a quantum process unit (QPU) using the same.

[0105] In an embodiment of the present invention, a technique or method can be provided that significantly reduces the variation in the deposition angle depending on the position of the substrate by installing an opening limiting member (a type of screen) having, for example, an opening in the form of a slit in the center in front of an inclined substrate, and performing deposition while moving the substrate. For example, in a deposition apparatus using an evaporation method, if an opening limiting member (screen) having a predetermined opening is installed on the front side of the substrate and deposition is performed only through said opening while moving the substrate in a predetermined manner, an apparatus and method can be implemented in which a source material (e.g., metal) is deposited at a uniform (or nearly uniform) angle of incidence. At this time, the deposition may proceed in a step-and-repeat manner in which unit deposition is performed to a desired thickness and the substrate is moved, or in a continuous deposition manner in which deposition is performed continuously while moving a substrate tilted at a certain angle. Generally, the size of a Josephson device is small, less than several hundred nanometers, and the size of a qubit is large, for example, about 0.5 cm to 1 cm. Therefore, if the width of the aperture is determined in the range of about 0.5 to 3 cm, a very uniform Josephson junction size can be obtained. The method according to the embodiment of the present invention can not only increase the uniformity of the incident angle of the deposited metal but also improve the thickness uniformity of the deposited metal.

[0106] FIG. 11 is a drawing for explaining a vacuum vapor deposition apparatus using an evaporation method according to one embodiment of the present invention.

[0107] Referring to FIG. 11, a vacuum vapor deposition apparatus using an evaporation method according to an embodiment of the present invention may include a source emitter (350) that emits a source material through evaporation within a vacuum chamber (1000). The source emitter (350) may include a source container (210) containing the source material and a source container holder (310) that holds the source material. The source container holder (310) may include an electron beam gun (e-beam gun) or other heating unit. The source material may be, for example, a metallic material. The source emitter (350) may be a type of evaporator unit, and the evaporator unit may be an electron beam (e-beam) evaporator unit or a thermal evaporator unit. Reference numeral 410 indicates a flux of the source material. The flux (410) may include a vaporized source material, that is, an evaporated source material.

[0108] The vacuum vapor deposition apparatus may include an opening-defining member (510) located above and spaced apart in the y-axis direction (height direction) with respect to the source emitter (350) within the vacuum chamber (1000). The opening-defining member (510) may be positioned in a basic arrangement such that its surface is parallel to the xz plane along the x-axis and z-axis perpendicular to the y-axis. The opening-defining member (510) may have an opening (H1) through which the source material passes, and the opening (H1) may have a structure extending in the x-axis or z-axis direction in the basic arrangement. The opening-defining member (510) may be a screen in which the opening (H1) is formed. The opening-defining member (510) may have a thin plate shape.

[0109] The above vacuum vapor deposition apparatus may include a substrate holder (520) positioned apart from a source emitter (350) with an opening limiting member (510) in between within a vacuum chamber (1000). A substrate (S1 in FIG. 12) may be mounted on the substrate holder (520). The substrate may be mounted such that the surface of the substrate on which the source material passing through the opening (H1) is deposited faces downward. The substrate for material deposition may be mounted on the lower surface of the substrate holder (520).

[0110] The substrate holder (520) may be configured to be movable along at least one of a first parallel direction parallel to the substrate and a second parallel direction parallel to the substrate and perpendicular to the first parallel direction. In the above basic arrangement, the first parallel direction may be parallel to the z-axis, and the second parallel direction may be parallel to the x-axis. In other words, in the arrangement state as shown in FIG. 11, the first parallel direction may be parallel to the z-axis, and the second parallel direction may be parallel to the x-axis. The substrate mounted on the substrate holder (520) may be movable along at least one of the first and second parallel directions.

[0111] Additionally, the substrate holder (520) and the opening limiting member (510) may be configured to be rotatable about the z-axis. The substrate holder (520) and the opening limiting member (510) may be rotatable about the z-axis in a first rotation direction and a second rotation direction opposite thereto. The substrate holder (520) may be configured to be rotatable about the z-axis at an angle controlled in the first rotation direction and the second rotation direction, respectively. For example, the substrate holder (520) may be configured to be rotatable about 90° about the z-axis in the first rotation direction and the second rotation direction, respectively. One of the first and second rotation directions may be clockwise, and the other may be counterclockwise. The substrate holder (520) and the opening limiting member (510) may rotate together to have the same or nearly the same angle of inclination with respect to the horizontal plane. A substrate mounted on the substrate holder (520) may rotate together with the substrate holder (520).

[0112] The source material emitted by the source emitter (350), i.e., the vaporized source material, can reach the surface of the substrate mounted on the substrate holder (520) through the opening (H1) and be deposited. During the material deposition process on the substrate, the substrate holder (520) may be moved in a predetermined direction. Additionally, the vacuum vapor deposition apparatus may be configured to perform the deposition process with the substrate holder (520) rotated by a given angle with respect to the z-axis.

[0113] According to one embodiment, the center of the source emitter (350) and the center of the opening (H1) may be positioned on a vertical line. The opening (H1) may, for example, have a slit shape. The opening (H1) may extend in the x-axis direction and may have a length along the x-axis and a width along the z-axis. Here, the length may be greater than or equal to the width. When the opening (H1) has a slit shape extending in the x-axis direction, the substrate holder (520) may be configured to be movable linearly along at least the first parallel direction. In the arrangement shown in FIG. 11, the substrate holder (520) may be movable linearly along at least the z-axis direction.

[0114] In other cases, the opening (H1) may be extended in the z-axis direction and may have a length along the z-axis and a width along the x-axis. Here, the length may be greater than or equal to the width. If the opening (H1) has a slit shape extended in the z-axis direction, the substrate holder (520) may be configured to be movable linearly along at least the second parallel direction. This case will be described in more detail later with reference to FIG. 15.

[0115] The opening (H1) may have a length along either the x-axis or the z-axis and a width along the other of the x-axis and the z-axis, and the width of the opening (H1) may be in the range of about 0.1 to 10 cm. The width of the opening (H1) may be determined, for example, within the range of about 0.5 to 3 cm or about 0.5 to 1.5 cm, but is not limited thereto. In some cases, the vacuum vapor deposition apparatus may be configured to variably adjust the width of the opening (H1). It may be possible to variably adjust the width of the opening (H1) by a mechanical means. The length of the opening (H1) may be a length that allows deposition to be performed on part or all of the diameter of the substrate. The length of the opening (H1) can be set to about 80% or more or about 90% or more of the diameter (width) of the substrate so that deposition can be performed over the entire effective area (effective surface area) of the substrate. In this case, it may be advantageous to perform deposition over the entire effective area (effective surface area) of the substrate while performing a single linear movement (movement of the substrate). However, depending on the case, the length of the opening (H1) may be set to less than 80% of the diameter (width) of the substrate.

[0116] According to one embodiment, when performing deposition while moving the substrate, when the center of the substrate is positioned on the center of the opening (H1), the center of the substrate, the center of the opening (H1), and the center of the source emitter (350) may be arranged on a vertical line. Here, the center of the source emitter (350) may refer to the emission center of the source container (210).

[0117] The above vacuum vapor deposition apparatus may further include a mechanical component (550) to which a substrate holder (520) and an opening limiting member (510) are connected or coupled. The mechanical component (550) may be configured to allow the substrate holder (520) to move along at least one of the first and second parallel directions. Additionally, the mechanical component (550) may be configured to allow the substrate holder (520) and the opening limiting member (510) to rotate about the z-axis. The mechanical component (550) itself may rotate about the z-axis. The mechanical component (550) may include a mechanical moving part. For example, the mechanical component (550) may include at least one of a linear actuator and a rotary actuator. A connecting member (522) connecting the substrate holder (520) and the mechanical component (550) may be further provided. The connecting member (522) may, for example, have a rod shape or a plate shape, or have other shapes.

[0118] Additionally, the vacuum vapor deposition apparatus may further include a support member (530) that directly or indirectly supports a substrate holder (520) on the opposite side from where the opening limiting member (510) is positioned. A substrate holder (520) may be positioned between the support member (530) and the opening limiting member (510). The support member (530) may include at least one structure such as a plate, a bar, or a rod. The support member (530) may support the substrate holder (520) from the rear side of the substrate holder (520). Thus, the movement of the substrate holder (520) can be made more stably by the support member (530). A rail member, for example, may be positioned between the substrate holder (520) and the support member (530). The support member (530) may rotate together with the substrate holder (520) and the opening limiting member (510) around the z-axis. Additionally, the support member (530) can be connected to or coupled to the mechanical component (550).

[0119] Additionally, depending on the case, the opening limiting member (510) may be configured to function as a gas injection unit for injecting gas into the vacuum chamber (1000). In this case, the opening limiting member (510) may include at least one gas injection passage for injecting oxygen gas, and oxygen gas may be injected into the vacuum chamber (1000) through the at least one gas injection passage. At this time, the oxygen gas may be used to form an oxide film (insulating film). When the opening limiting member (510) is configured to function as a gas injection unit, a predetermined gas can be easily injected into an area adjacent to the substrate through the opening limiting member (510), thereby making it easier to perform processes such as oxidation. However, the opening limiting member (510) having the function of a gas injection unit may be optional.

[0120] In addition, the vacuum vapor deposition apparatus may further include a shutter member (600) positioned between a source emitter (350) and an opening limiting member (510). The shutter member (600) may serve to block or allow the movement of the source material toward the opening limiting member (510), or to control it in other ways. The shutter member (600) may be referred to as a global shutter. The shutter member (600) can be used to control, for example, the ON / OFF of the deposition process. Although not illustrated, the vacuum vapor deposition apparatus may further be provided with an ion milling part for cleaning the surface of the substrate, an ultraviolet (UV) lamp required for oxidation, an oxygen supply device, other sensors, etc.

[0121] According to one embodiment, the vacuum vapor deposition apparatus may be configured to perform a deposition process over the entire effective area of ​​the substrate surface in a step-and-repeat manner. In this case, in the step-and-repeat manner, after performing a deposition process for the Nth area of ​​the substrate surface, the substrate holder (520) may be moved a certain amount, and then a deposition process may be performed for the N+1th area of ​​the substrate surface, and this process may be repeated. According to another embodiment, the vacuum vapor deposition apparatus may be configured to perform a deposition process over the entire effective area of ​​the substrate surface while continuously moving the substrate holder (520) at a given speed. In other words, the vacuum vapor deposition apparatus may perform deposition in a continuous deposition manner while moving the substrate.

[0122] FIGS. 12 and FIGS. 13 are drawings showing enlarged portions of the configuration of the vacuum vapor deposition apparatus of FIG. 11. FIG. 12 is a side view along the yz plane, and FIG. 13 is a side view along the xy plane.

[0123] Referring to FIGS. 12 and 13, an opening limiting member (510), a substrate holder (520), a support member (530), and a mechanical component (550) are illustrated. The opening limiting member (510), the substrate holder (520), the support member (530), and the mechanical component (550) may form a single assembly (500). A substrate (S1) may be mounted on the substrate holder (520), and a source material passing through the opening (H1) may be deposited on the target surface of the substrate (S1). The substrate (S1) may be a substrate structure having a predetermined mask pattern (photoresist pattern) formed on a base substrate. The structure of the substrate (S1) may be the same or similar as described, for example, with reference to FIGS. 1 and 2. The gap between the substrate (S1) and the opening limiting member (510) may be several cm or less, for example, about 1 cm or less. It may be preferable for the gap between the substrate (S1) and the opening limiting member (510) to be as small as possible.

[0124] FIG. 14 is a plan view exemplarily showing an opening limiting member (510) that can be applied to a vacuum vapor deposition apparatus according to one embodiment of the present invention.

[0125] Referring to FIG. 14, the opening limiting member (510) may have an opening (H1). The opening (H1) may extend in the x-axis direction and may have a length along the x-axis and a width along the z-axis. Here, the length may be greater than or equal to the width. If the opening (H1) has a slit shape extending in the x-axis direction, the substrate holder (520) may be configured to be movable linearly along at least the first parallel direction. In the basic arrangement, the first parallel direction may be a direction parallel to the z-axis. A deposition process on the substrate may be performed while moving the substrate mounted on the substrate holder (520) in the first parallel direction. The deposition process may be performed while exposing the substrate surface from one end to the other through the opening (H1).

[0126] FIG. 15 is a plan view exemplarily showing an opening limiting member (510) that can be applied to a vacuum vapor deposition apparatus according to another embodiment of the present invention.

[0127] Referring to FIG. 15, the opening limiting member (510) may have an opening (H1). The opening (H1) may extend in the z-axis direction and may have a length along the z-axis and a width along the x-axis. Here, the length may be greater than or equal to the width. If the opening (H1) has a slit shape extending in the z-axis direction, the substrate holder (520) may be configured to be movable linearly along at least the second parallel direction. In the basic arrangement, the second parallel direction may be a direction parallel to the x-axis. A deposition process on the substrate may be performed while moving the substrate mounted on the substrate holder (520) in the second parallel direction. The deposition process may be performed while exposing the substrate surface from one end to the other through the opening (H1).

[0128] However, the shape and arrangement of the opening (H1) described with reference to FIGS. 14 and 15 are exemplary and may vary depending on the case. The opening (H1) may have a square shape or other shapes. Additionally, the substrate holder (520) on which the substrate is mounted may be configured to move in the first parallel direction and the second parallel direction. Here, the movement may include linear reciprocating movement.

[0129] In an exemplary embodiment of the present invention, an opening limiting member (screen) having an opening extended in one of the x-axis and z-axis directions is placed between a substrate and a source emitter in a portion adjacent to the substrate so that deposition is performed only through said opening, and the deposition process can be completed on the front surface of the substrate by moving the substrate in a direction perpendicular to the direction of extension of the opening.

[0130] This method may be useful for eliminating or minimizing the variation in length or width of a Josephson device. As explained above, since the variation in width may be greater than the variation in length, in order to eliminate or minimize the variation in width, as exemplified in FIGS. 11 to 14, an opening limiting member having a slit-shaped opening extending in the x-axis direction in a portion adjacent to the substrate between the substrate and the source emitter can be placed, and the substrate can be moved in the z-axis direction to perform the deposition process.

[0131] The width of the above-mentioned opening can be determined by considering the desired angular deviation, for example, preferably between about 0.5 and 3 cm, and more preferably between about 0.5 and 1.5 cm, but is not limited thereto. For example, if the width of the slit-type opening is 1 cm, the deviation in the width of the Josephson device can be obtained at a value lower than about 0.5%, although this varies depending on other conditions. Generally, one or two qubits can be designed within the 1 cm range, and in the case of transmons, one or two Josephson junctions can be formed. Accordingly, the deviation in the width of the Josephson junction formed across the entire substrate can be controlled to within 0 to 0.5%.

[0132] Another advantage of the embodiment of the present invention is that the distance between the source emitter and the center of the substrate can be reduced due to such small deviation.

[0133] For example, when the substrate tilt angle is 45°, and the thickness of the second photoresist of the Dolan process pattern is designed to be 200 nm and the width of the Josephson junction to be 300 nm, and the distance between the source emitter and the center of the substrate is 80 cm, the width of the Josephson junction may differ by up to about 8.3%. If the distance between the source emitter and the center of the substrate is reduced to 50 cm or 30 cm, the difference increases to 13.3% and 22.2%, respectively.

[0134] On the other hand, in an embodiment of the present invention, when the width of the opening is set to 1 cm, the variation in the width of the Josephson junction can be significantly reduced to 1.1%, 0.7%, and 0.4% when the distance between the source emitter and the center of the substrate is 80 cm, 50 cm, and 30 cm, respectively, thereby making it possible to reduce the size of the vacuum chamber. For example, in the case of a chamber capable of depositing a single 8-inch substrate, reducing the distance between the source emitter and the center of the substrate from 80 cm to 50 cm or 30 cm can reduce the chamber size by 26% and 43%, respectively. Such a reduction in chamber size can lead to a reduction in manufacturing and maintenance costs for a Josephson junction fabrication chamber that requires maintaining a high vacuum. In particular, a Josephson junction fabrication chamber can perform the function of oxidizing metals in addition to metal deposition, and because it must control very thin oxide films, it is sensitive to contamination by impurities and has the characteristic of requiring a higher vacuum level compared to a general deposition chamber. In this regard, the effect of reducing the chamber size can be even greater.

[0135] According to an exemplary embodiment of the present invention, the assembly (500) of FIG. 12 can be rotated about 90° in the +x direction (first rotation direction) and the -x direction (second rotation direction) around the z-axis (rotation axis, i.e., rotation center) to enable deposition on an inclined substrate (wafer), i.e., angled deposition, and the center of the opening can be aligned with the center of the source emitter. When the assembly (500) is rotated around the z-axis, the high side and the low side of the substrate can be symmetrically positioned with respect to the center of the substrate.

[0136] When using only a portion of the vaporized source material through an opening, there may be concerns about increased source consumption; however, in the case of an angle evaporation process, since a large distance must be secured between the substrate and the source emitter, source consumption may fundamentally be higher compared to a general evaporation process. Furthermore, considering that the thickness of the deposited material is thin (non-limiting example, 40 to 100 nm) and the deposited metal (non-limiting example, Al, etc.) is inexpensive, the increase in source consumption due to the use of an opening may not be a major problem. Moreover, in the case of the embodiment of the present invention, the distance between the source emitter and the substrate can be easily reduced. Since the amount of source material reaching the substrate is inversely proportional to the square of the distance, reducing the distance between the substrate and the source emitter instead of using an opening can reduce source consumption and may be advantageous for reducing equipment manufacturing and operating costs.

[0137] FIG. 16 is a drawing illustrating a vacuum vapor deposition apparatus using an evaporation method according to another embodiment of the present invention. This embodiment is a modified version of FIG. 11.

[0138] Referring to FIG. 16, a vacuum vapor deposition apparatus according to the present embodiment may include first and second mechanical components (550a, 550b) to which a substrate holder (520) and an opening limiting member (510) are connected or coupled. The substrate holder (520) and the opening limiting member (510) may be disposed between the first and second mechanical components (550a, 550b). A first connecting member (522) connecting the substrate holder (520) and the first mechanical component (550a) may be disposed, and a second connecting member (524) connecting the substrate holder (520) and the second mechanical component (550b) may be disposed. The first connecting member (522) and the second connecting member (524) may be connected as one. The first and second mechanical components (550a, 550b) may be configured to allow the substrate holder (520) to move along at least one of the first and second parallel directions. Additionally, the first and second mechanical components (550a, 550b) may be configured to allow the substrate holder (520) and the opening limiting member (510) to rotate about the z-axis. When the first and second mechanical components (550a, 550b) are used, the movement and rotation of the substrate holder (520) can be performed more stably.

[0139] According to an embodiment of the present invention, a method for manufacturing a device may be provided, comprising the step of depositing a material film using the aforementioned vacuum vapor deposition apparatus. Herein, the device may include, as a non-limiting example, a Josephson device. The method for manufacturing the device may include the steps of forming a first superconducting material film on the substrate while the substrate holder and the opening limiting member are rotated with respect to the z-axis by a first angle condition, forming an insulating film on the surface of the first superconducting material film, and forming a second superconducting material film on the insulating film while the substrate holder and the opening limiting member are rotated with respect to the z-axis by a second angle condition different from the first angle condition. Additionally, in each of the step of forming the first superconducting material film and the step of forming the second superconducting material film, the substrate holder may be moved along at least one of the first and second parallel directions.

[0140] The first and second superconducting material films may comprise, for example, at least one superconducting metal selected from Al, TiN, Nb, Ta, and V. The insulating film may be an oxide, a nitride, or other insulating material. The oxide may be, for example, Al oxide, but is not limited thereto and may vary in various ways. If the insulating film is an oxide film, the oxide film may be formed, for example, through an oxidation process on the surface portion of the first superconducting material film.

[0141] FIGS. 17a to 17c are cross-sectional views illustrating a method for manufacturing a device using a vacuum vapor deposition apparatus utilizing an evaporation method according to one embodiment of the present invention.

[0142] Referring to FIG. 17a, the substrate structure may include a substrate (101) and a mask pattern disposed on the substrate (101). The mask pattern may include, for example, first and second photoresists (111, 121). The mask pattern may be formed to have a multilayer (double-layer) structure and an undercut structure as described in FIG. 1. Here, 'photoresist' may be referred to as 'electron beam resist,' and this may be applied equally throughout the entire specification. The mask pattern may be formed, for example, by electron beam lithography or by photolithography.

[0143] A first superconducting material film (131) can be formed on a substrate (101) while the substrate (101) is rotated to a first angle condition using a vacuum vapor deposition apparatus according to an embodiment of the present invention. At this time, a source material can be provided to the substrate (101) through the opening, and the substrate (101) can be moved in a predetermined direction during the deposition process.

[0144] Referring to FIG. 17b, an insulating film (141) can be formed on the surface of the first superconducting material film (131). The insulating film (141) can be formed within the vacuum vapor deposition apparatus. If the insulating film (141) is an oxide film, the oxide film can be formed, for example, through an oxidation process on the surface portion of the first superconducting material film (131). However, the method of forming the insulating film (141) is not limited thereto and may vary depending on the case.

[0145] Referring to FIG. 17c, a second superconducting material film (151) can be formed on a substrate (101) while the substrate (101) is rotated to a second angle condition using a vacuum vapor deposition apparatus according to an embodiment. At this time, a source material can be provided to the substrate (101) through the opening, and the substrate (101) can be moved in a predetermined direction during the deposition process. The second superconducting material film (151) can be formed on an insulating film (141) and can be formed to partially overlap with the first superconducting material film (131). A Josephson junction can be defined in the region where the second superconducting material film (151) and the insulating film (141) are in contact.

[0146] By forming a plurality of qubits on a substrate (101) on which a Josephson element is formed in the manner illustrated in FIGS. 17a to 17c, a circuit (qubit-based circuit) including a plurality of qubits can be fabricated. The plurality of qubits may be a plurality of superconducting qubits. Embodiments of the present invention may be applicable, for example, to quantum computers, quantum sensors, quantum communication, superconducting devices, etc.

[0147] According to the embodiments of the present invention described above, a vacuum vapor deposition apparatus can be implemented that enables the fabrication of devices with more accurate and precise sizes by reducing the error (dispersion) of the deposition process according to the position of the substrate in the manufacture of quantum technology-related devices, such as Josephson devices, for example. Furthermore, according to the embodiments of the present invention, a method for fabricating devices using the above-described vacuum vapor deposition apparatus can be implemented.

[0148] Conventional evaporators have a fundamental limitation in that the amount of metal deposited and the angle of incidence vary depending on the position of the substrate, due to the characteristic that the source travels radially (partially radially) at a constant angle from a metal source generator having a relatively small cross-sectional area and is deposited. Among these limitations, the problem of varying metal amounts can be partially mitigated by the aforementioned prior art 1, but the problem of varying angles of incidence, which is a more significant issue, has not been resolved at the equipment level, and a method for correcting the substrate pattern has been proposed in the aforementioned prior art 2. However, in the case of the pattern correction method, the pattern size must be corrected individually according to the position of the substrate, and there is a problem that correction must be performed whenever the position or size of the device changes.

[0149] According to one embodiment of the present invention, a vacuum vapor deposition apparatus and a related method can be implemented that can drastically reduce process error (dispersion) by using an opening limiting member, for example, having an opening in the shape of a slit, to allow the source material to pass only through the opening, and by moving the position of a substrate on which a predetermined mask pattern is formed, thereby making the incident amount and incident angle of the source material uniform or nearly uniform across the entire effective area of ​​the substrate. In addition, according to one embodiment of the present invention, since the distance between the source emitter and the substrate can be reduced, the excessive consumption of the source that occurs when deposition is performed only through the opening can be compensated for, and furthermore, as the equipment size is reduced, the effect of reducing equipment manufacturing costs and operating costs such as vacuum maintenance costs can be obtained.

[0150] This specification discloses preferred embodiments of the present invention. Although specific terms have been used, they are used merely in a general sense to facilitate the explanation of the technical content of the invention and to aid in understanding the invention, and are not intended to limit the scope of the invention. It is obvious to those skilled in the art that, in addition to the embodiments disclosed herein, other variations based on the technical concept of the present invention are possible. Those skilled in the art will understand that the vacuum vapor deposition apparatus and the method for manufacturing a device using the same according to the embodiments described with reference to FIGS. 11 to 17c can be variously substituted, changed, and modified within the scope of the technical concept of the present invention. For example, in the vacuum vapor deposition apparatus according to the embodiments, the opening limiting member may have two or more openings. As another example, the vacuum vapor deposition apparatus according to the embodiments may include two or more source emitters. Various other modifications may also be possible. Therefore, the scope of the invention should not be determined by the described embodiments but by the technical concept described in the claims.

Claims

1. As a vacuum vapor deposition apparatus using an evaporation method, A source emitter that releases a source substance through evaporation within a vacuum chamber; An opening limiting member positioned above and spaced apart in the y-axis direction with respect to the source emitter within the vacuum chamber, wherein in a basic arrangement, the surface thereof is arranged parallel to the xz plane along the x-axis and z-axis perpendicular to the y-axis, and has an opening through which the source material passes, and the opening has a structure extending in the x-axis to z-axis direction in the basic arrangement; and A substrate holder positioned within the vacuum chamber spaced apart from the source emitter with the opening limiting member in between, wherein the substrate is mounted such that the surface of the substrate on which the source material passing through the opening is deposited faces downward; A vacuum vapor deposition apparatus using an evaporation method, wherein the substrate holder is configured to be movable along at least one of a first parallel direction parallel to the substrate and a second parallel direction parallel to the substrate and perpendicular to the first parallel direction, and in the basic arrangement, the first parallel direction is parallel to the z-axis and the second parallel direction is parallel to the x-axis, and the substrate holder and the opening limiting member are configured to be rotatable about the z-axis.

2. In Paragraph 1, A vacuum vapor deposition apparatus in which the center of the source emitter and the center of the opening are positioned on a vertical line.

3. In Paragraph 1, A vacuum vapor deposition apparatus configured such that the substrate holder is rotatable at an angle controlled in a first rotational direction and a second rotational direction opposite thereto, respectively, with respect to the z-axis.

4. In Paragraph 1, The above-mentioned opening is a vacuum vapor deposition apparatus having a slit shape.

5. In Paragraph 1, The above opening extends in the x-axis direction and has a length along the x-axis and a width along the z-axis, The above substrate holder is configured to be linearly movable along at least the first parallel direction. A vacuum vapor deposition apparatus.

6. In Paragraph 1, The above opening extends in the z-axis direction and has a length along the z-axis and a width along the x-axis, A vacuum vapor deposition apparatus in which the substrate holder is configured to be linearly movable along at least the second parallel direction.

7. In Paragraph 1, The above opening has a length along either the x-axis or the z-axis and a width along the other of the x-axis and the z-axis, and A vacuum vapor deposition apparatus in which the width of the opening is in the range of 0.1 to 10 cm.

8. In Paragraph 1, The above vacuum vapor deposition apparatus is a vacuum vapor deposition apparatus configured to variably adjust the width of the opening.

9. In Paragraph 1, A vacuum vapor deposition apparatus in which, when the center of the substrate is located on the center of the opening, the center of the substrate, the center of the opening, and the center of the source emitter are arranged on a vertical line.

10. In Paragraph 1, A vacuum vapor deposition apparatus further comprising a shutter member disposed between the source emitter and the aperture limiting member, which blocks or allows the movement of the source material toward the aperture limiting member or controls it in another way.

11. In Paragraph 1, The above substrate holder and the above opening limiting member further include a mechanical component to which they are connected or coupled, and A vacuum vapor deposition apparatus in which the mechanical component is configured to allow the substrate holder to move along at least one of the first and second parallel directions, and the substrate holder and the opening limiting member are configured to rotate about the z-axis.

12. In Paragraph 1, The above substrate holder and the above opening limiting member further include first and second mechanical components to which they are connected or coupled, and the substrate holder and the above opening limiting member are disposed between the first and second mechanical components. A vacuum vapor deposition apparatus in which the first and second mechanical components are configured to allow the substrate holder to move along at least one of the first and second parallel directions, and the substrate holder and the opening limiting member are configured to rotate about the z-axis.

13. In Paragraph 1, A vacuum vapor deposition apparatus further comprising a support member that directly or indirectly supports the substrate holder on the opposite side where the opening limiting member is positioned.

14. In Paragraph 1, A vacuum vapor deposition apparatus configured such that the above-mentioned opening limiting member functions as a gas injection part for injecting gas into the vacuum chamber.

15. In Paragraph 1, The above vacuum vapor deposition apparatus is a vacuum vapor deposition apparatus configured to perform a deposition process with the substrate holder rotated by a given angle with respect to the z-axis.

16. In Paragraph 1, The above vacuum vapor deposition apparatus is configured to perform a deposition process over the entire effective area of ​​the substrate surface while continuously moving the substrate holder at a given speed.

17. In Paragraph 1, The above vacuum vapor deposition apparatus is configured to perform a deposition process over the entire effective area of ​​the substrate surface in a step-and-repeat manner, and A vacuum vapor deposition apparatus that, in the above step-and-repeat method, performs a deposition process on the Nth region of the substrate surface, moves the substrate holder, and performs a deposition process on the N+1th region of the substrate surface.

18. A method for manufacturing a device comprising the step of depositing a material film using a vacuum vapor deposition apparatus described in any one of claims 1 to 17.

19. In Paragraph 18, The above device is a method for manufacturing a device including a Josephson device.

20. In Paragraph 19, A step of forming a first superconducting material film on the substrate while rotating the substrate holder and the opening limiting member by a first angle condition with respect to the z-axis; A step of forming an insulating film on the surface of the first superconducting material film; and A method for manufacturing a device comprising the step of forming a second superconducting material film on an insulating film while rotating the substrate holder and the opening limiting member with respect to the z-axis to a second angle condition different from the first angle condition.

21. In Paragraph 20, A method for manufacturing a device in which the substrate holder is moved along at least one of the first and second parallel directions in each of the step of forming the first superconducting material film and the step of forming the second superconducting material film.