Chemical vapor deposition of quaternary aluminum scandium gallium nitride layers for iii-nitride high electron mobility transistors

The deposition of AlScGaN layers by MOCVD addresses material growth challenges in III-nitride HEMTs, achieving high-quality layers with enhanced 2DEG densities and electron mobilities for improved transistor performance.

WO2026235742A1PCT designated stage Publication Date: 2026-11-12RGT UNIV OF CALIFORNIA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2025/051102
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2025-10-15
Publication Date
2026-11-12

Smart Images

  • Figure US2025051102_12112026_PF_FP_ABST
    Figure US2025051102_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Quaternary aluminum scandium gallium nitride (AlScGaN) layers are deposited by chemical vapor deposition (CVD) in a nitride semiconductor growth chamber for electronics and transistor semiconductor structures. The addition of Ga enables higher quality material than AlScN while retaining the two-dimensional electron gas (2DEG) charges and electron mobilities of AlScN. The AlScGaN layers can be used as functional layers in structures with III-nitride or other III-V semiconductor materials, thereby providing higher performance and reliability than existing high charge 2DEG-based structures, without the material growth problems of AlScN materials. Moreover, CVD is the preferred growth method for commercial applications.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CHEMICAL VAPOR DEPOSITION OF QUATERNARY ALUMINUM SCANDIUM GALLIUM NITRIDE LAYERS FOR III-NITRIDE HIGH ELECTRON MOBILITY TRANSISTORS AND OTHER ELECTRONIC DEVICES

[0002] CROSS REFERENCE TO RELATED APPLICATION

[0003] This application claims the benefit under 35 U.S.C. Section 119(e) of the following co-pending and commonly-assigned application:

[0004] U.S. Provisional Patent Application Serial No. 63 / 802,248, filed on May 8, 2025, by Vineeta R. Muthuraj, Claire E. Vozel, Stacia Keller, Umesh K. Mishra and Steven P. DenBaars, entitled “CHEMICAL VAPOR DEPOSITION OF QUATERNARY ALUMINUM SCANDIUM GALLIUM NITRIDE LAYERS FOR III-NITRIDE HIGH ELECTRON MOBILITY TRANSISTORS AND OTHER ELECTRONIC DEVICES,” docket number G&C 30794.0877USP1 (UC 2025-387-i);

[0005] which application is incorporated by reference herein.

[0006] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH AND DEVELOPMENT

[0007] This invention was made with Government support under Grant No. N00164-23-9-G056 awarded by the Naval Surface Warfare Center. The Government has certain rights in this invention.

[0008] BACKGROUND OF THE INVENTION

[0009] 1. Field of the Invention.

[0010] This invention relates to chemical vapor deposition (CVD) of quaternary aluminum scandium gallium nitride (AlScGaN) for Ill-nitride devices.2. Description of the Related Art.

[0011] Group Ill-nitride semiconductors, such as gallium nitride (GaN), aluminum nitride (AIN), and indium nitride (InN), are widely used in high-power and high-frequency electronic applications due to their strong spontaneous and piezoelectric polarization effects, high electron mobilities, wide bandgaps, high electrical breakdown fields, and thermal stability.

[0012] Ill-nitride semiconductors are used to achieve high power, high current transistors. High-electron-mobility transistors (HEMTs) based on Ill-nitride materials typically utilize a heterostructure composed of a relatively wide-bandgap barrier layer and a relatively narrow-bandgap channel layer. The transistor structure requires a barrier material layer to create a high density of electric charge known as a 2-dimensional electron gas (2DEG) that can be manipulated in fabricated devices. At the heterointerface, a discontinuity in polarization, arising from both spontaneous and strain-induced piezoelectric components, leads to the formation of the 2DEG within the channel. This 2DEG enables high electron mobility, often exceeding 2000 cm2 / V s at room temperature, due to reduced impurity and alloy scattering.

[0013] Aluminum gallium nitride (Al GaN) is the most common barrier layer in III-nitride HEMTs and can support 2DEG sheet densities in the range of approximately 8 x 1012cm'2to 1.5 x 1013cm'2. However, the increasing demand for higher power density and current capability in electronic devices necessitates barrier materials that can support higher sheet carrier concentrations. Alternative barrier materials include AIN, indium aluminum nitride (InAlN), indium aluminum gallium nitride (InAlGaN), and more recently, aluminum scandium nitride (AlScN), which also exhibits ferroelectric behavior.

[0014] AIN can theoretically support sheet charges as high as 6 x io13cm'2, but suffers from low critical thickness when grown on GaN, limiting its practical use. InAlN and InAlGaN allow for lattice-matched barrier compositions on GaN and can achieve 2DEG sheet densities of 2 x io13cm'2to 3 x io13cm'2with reduced strain. However, InAlN is difficult to grow epitaxially, and the incorporation of indiumintroduces issues such as low miscibility, surface roughness, and leakage. InAlGaN mitigates some of these issues by incorporating gallium to improve crystal quality and reduce alloy scattering, but the presence of indium still presents leakage and reliability concerns.

[0015] Sc-containing nitride materials are a recent interest for achieving high charge and power. For example, AlScN has emerged as a promising alternative due to its high polarization and potential for high 2DEG densities between 2 x 1013cm'2and 5 x 1013cm'2in AlScN / GaN heterostructures. Additionally, AlScN can be lattice-matched to GaN, enabling high-performance device design. AlScN layers have been grown using both molecular beam epitaxy (MBE) and metalorganic chemical vapor deposition (MOCVD), although MOCVD growth has historically been limited by the low vapor pressure of available scandium precursors. However, the ternary compound AlScN presents many material growth challenges, such as interface roughness, and high impurity levels in the AlScN layer.

[0016] Introducing gallium intentionally into the AlScN barrier - thereby forming a quaternary alloy AlScGaN, offers potential improvements similar to those observed in InAlGaN. Gallium acts as a surfactant, improving surface morphology and crystalline quality. Furthermore, due to its ionic radius falling between that of Al3+and Sc3+, gallium can relieve in-plane strain and allow for additional composition engineering flexibility. However, unintentional Ga incorporation can negatively impact device performance.

[0017] To date, there have been no reported demonstrations of MOCVD-grown quaternary AlScGaN heterostructures or their electrical performance in GaN-based devices. Given MOCVD’s advantages in throughput and scalability for industrial manufacturing, successful growth and integration of AlScGaN by MOCVD represents a critical step toward commercialization of scandium-containing Ill-nitride HEMTs.SUMMARY OF THE INVENTION

[0018] In this invention, quaternary AlScGaN layers are deposited by CVD in a nitride semiconductor growth chamber for transistor and other electronic device structures. Layers of this material have not previously been demonstrated by CVD. The addition of Ga enables higher quality material than AlScN while retaining high 2DEG charges and electron mobilities. The AlScGaN layers can be used as functional layers in transistor structures with Ill-nitride or other III-V semiconductor materials.

[0019] The quaternary AlScGaN enables transistors with required high performance levels without the material growth problems that other semiconductor barrier materials (such as AlScN) have. Chemical vapor deposition is the preferred growth method for commercial applications, so with the disclosed method, it is possible to deposit AlScGaN layers in an industrial setting. The higher quality layers enable high performance devices with higher reliabilities than existing high charge 2DEG-based transistors.

[0020] BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Referring now to the drawings in which like reference numbers represent corresponding parts throughout:

[0022] FIG. l is a schematic of an exemplary device structure with a metal-polar (Illpolar) growth orientation.

[0023] FIG. 2 is a schematic of an exemplary device structure with a Nitrogen-polar (N-polar) growth orientation.

[0024] FIG. 3 is a graph of AlScGaN thickness vs. triethylgallium (TEGa) flow (pmol min'1) showing growth rate data.

[0025] FIG. 4 is a graph of sheet density ns (cm'2) vs. TEGa flow (pmol min'1) vs. electron mobility showing Hall measurement data.

[0026] FIG. 5 is a graph of Intensity counts vs. co * showing x-ray diffraction (XRD) data for TEGa at 10 pmol min'1and 7.5 pmol min'1.FIG. 6 is an atomic force microscopy (AFM) image at 2 pm showing a rootmean-square (RMS) roughness of 0.61 nm.

[0027] DETAILED DESCRIPTION OF THE INVENTION

[0028] In the following description of the preferred embodiment, reference is made to the accompanying drawings which form a part hereof, and in which is shown by way of illustration a specific embodiment in which the invention may be practiced. It is to be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present invention.

[0029] Overview

[0030] This invention provides the first demonstration of MOC VD-grown AlScGaN / AlN / GaN heterostructures with exceptional electrical properties, enabling enhanced 2DEG performance in advanced electronic devices.

[0031] Devices

[0032] FIG. l is a schematic of an exemplary HEMT device structure with a metalpolar (Ill-polar) growth orientation. The fabrication process for the device structure begins with the epitaxial growth by MOCVD of a heterostructure on a substrate 101, wherein the heterostructure is comprised of a semi-insulating (S.I.) GaN channel layer 102; an optional interlayer (not shown), deposited on or above the S.I. GaN channel layer 102, selected from binary, ternary, or quaternary III-V compounds; and an AlScGaN barrier layer 103, deposited on or above the optional interlayer and / or the S.I. GaN channel layer 102, consisting of a quaternary III-V semiconductor alloy having the formula AlxScyGai-x-yN, where 0 < x < 1, 0 <y < 0.5, and x + y < 1. A 2DEG 104 forms at an interface between the S.I. GaN channel layer 102 and the AlScGaN barrier layer 103 (when the optional interlayer is not present), or at an interface between the S.I. GaN channel layer 102 and the optional interlayer (when the optional interlayer is present), facilitating high electron mobility. A gate dielectric105 is deposited on or above the AlScGaN barrier layer 103, and etching is performed to define the device regions and form mesa structures. A gate metal 106 is deposited on the gate dielectric 105 to form the gate electrode 106, and ohmic contacts 107, 108 are formed on the S.I. GaN channel layer 102 for the source and drain terminals 107, 108.

[0033] FIG. 2 is a schematic of an exemplary device structure with a Nitrogen-polar (N-polar) growth orientation that is inverted as compared to FIG. 1. The fabrication process for the device structure begins with the epitaxial growth by MOCVD of a heterostructure on a substrate 201, wherein the heterostructure is comprised of an S.I. GaN base layer 202 deposited on or above a substrate 201; an AlScGaN barrier layer 203, deposited on or above the S.I. GaN base layer 202, consisting of a quaternary III-V semiconductor alloy having the formula AlxScyGai-x-yN, where 0 < x < 1, 0 < y < 0.5, and x + y < 1; an optional interlayer (not shown), deposited on or above the AlScGaN barrier layer 203, selected from binary, ternary, or quaternary III-V compounds; and a GaN channel layer 204 deposited on or above the optional interlayer and / or the AlScGaN barrier layer 203. A 2DEG 205 forms at an interface between the GaN channel layer 204 and the AlScGaN barrier layer 203 (when the optional interlayer is not present), or at an interface between the GaN channel layer 204 and the optional interlayer (when the optional interlayer is present), facilitating high electron mobility. A gate dielectric 206 is deposited on or above the GaN channel layer 204, and etching is performed to define the device regions and form mesa structures. A gate metal is deposited on the gate dielectric 206 to form the gate electrode 207, and ohmic contacts 208, 209 are formed on the GaN channel layer 204 for the source and drain terminals 208, 209.

[0034] Examples for using MOCVD-grown AlScGaN in electronic devices may include the following:

[0035] 1. As a HEMT barrier layer in Ill-nitride 2DEG-based devices of Illpolar, N-polar, nonpolar, or semipolar orientations. Devices may incorporate layers ofother III-V semiconductor materials, where the group-III element may be B, Al, Sc, Ga, Y, or In, and the group-V element may be N, P, or As. Structures include:

[0036] a. Single barrier (all with possible cap / passivation layers such as GaN or silicon nitride (SiNx):

[0037] i. AlScGaN / GaN.

[0038] ii. Structures including interlayers between the AlScGaN and the GaN base layer, which may be binary, ternary, or quaternary alloys of III-V elements (group-III = B, Al, Sc, Ga, Y, In, group-V = N, P, As). If the interlayer is AlScGaN, it has a different composition from the AlScGaN barrier.

[0039] b. Multi-channel transistor structures comprised of a plurality of alternating AlScGaN barrier layers and one or more additional III-V semiconductor layers that form a superlattice, for example, using GaN as the base layer and as a channel layer:

[0040] i. AlScGaN / W-Y superlattices (W = B, Al, Sc, Y, In, Y = N, P, As).

[0041] ii. AlScGaN / W-X-Y superlattices where W-X-Y is a ternary III-V compound (group-III = B, Al, Sc, Ga, Y, In, group-V = N, P, As).

[0042] iii. AlScGaN / W-X-Y-Z superlattices where W-X-Y-Z is a quaternary III-V compound. If the W-X-Y-Z interlayer is AlScGaN, its composition is different from the AlScGaN barrier layer.

[0043] iv. The superlattice barrier layers can be composed multiple layers as described above.

[0044] c. Composite barriers using GaN as the base layer: barriers of multiple materials for single channel devices:

[0045] i. The barrier may include two or more layers where at least one layer is AlScGaN. The other layer(s) are binary, ternary, or quaternary alloys of III-V semiconductor materials, where the group-Ill elements may be B, Al, Sc, Ga, Y, or In, and the group-V elements may be N, P, or As.

[0046] ii. The structure may include an interlayer between the composite barrier and the GaN channel that consists of binary, ternary, or quaternary alloys of III-V semiconductor materials, where the group-III elements may be B, Al, Sc, Ga, Y, or In, and the group-V elements may be N, P, or As.

[0047] 2. Polarization doping by growing graded composition AlScGaN layers along a growth direction to induce polarization doping and form a three-dimensional carrier gas, resulting in 3D electron or hole gases for n- or p- type conduction.

[0048] 3. Lattice-matched or polarization-matched back-barriers for HEMTs, for reduced strain and enhanced thermal stability, for example, the AlScGaN barrier layer has a composition that is engineered to be lattice-matched or polarization-matched to the GaN channel layer for reduced strain and enhanced thermal stability.

[0049] 4. The layer structures may include channel layers other than GaN and the channel or channels can be composed of other III-V compounds (group-III = B, Al, Sc, Ga, Y, In, group-V = N, P, As).

[0050] Methods

[0051] In one example, AlScGaN layers were deposited by MOCVD on or above a c-sapphire in N2 carrier gas using NH3 as the nitrogen precursor, trimethylaluminum (TMA1) as the aluminum precursor, trimethylgallium (TMGa) or tri ethylgallium (TEGa) as the gallium precursor, and bis(ethylcyclopentadienyl)scandium ((EtCp)2Sc(dbt)) as the scandium precursor. The growth pressure was 150 Torr and temperatures of 900 °C or 950 °C were used.

[0052] First, a GaN base layer was grown on or above the substrate at atmospheric pressure using trimethylgallium (TMGa) or triethylgallium (TEGa) and NH3, and a growth temperature of 1190 °C. Afterward, the temperature was lowered to the AlScGaN growth temperature, a nominally 0.7 nm thick optional interlayer of AIN oranother III-V compound was deposited on or above the GaN base layer using TMA1 and NH3, and then the AlScGaN barrier layer was deposited on or above the interlayer and / or the GaN base layer by metalorganic chemical vapor deposition (MOCVD) using precursors comprising: trimethylaluminum (TMA1), trimethylgallium (TMGa) or triethylgallium (TEGa), bis(ethylcyclopentadienyl)scandium ((EtCp)2Sc(dbt)), and ammonia (NH3), wherein the flow rates of TMGa or TEGa, TMA1, and (EtCp)2Sc(dbt) are adjusted to control the relative Al, Ga, and Sc content, and the growth temperature is between 900 °C and 1000 °C and the growth pressure is approximately 150 Torr. Specifically, the composition of the AlScGaN layer was modulated by adjusting the TMGa or TEGa flow while holding the TMA1, (EtCp)2Sc(dbt), and NH3 flows constant. The NH3 flow was 134 mmol min'1, the (EtCp)2Sc(dbt) flow was 10 pmol min'1, the TMA1 flow was 1.2 pmol min'1, and the TMGa or TEGa flow was varied from 2.5 pmol min'1to 10 pmol min'1.

[0053] Alternatively, the AlScGaN layers can be grown using other suitable precursors to supply Al, Sc, Ga, and N. Possible substrates include sapphire, SiC, bulk GaN, bulk AIN, or Si.

[0054] The result is a HEMT heterostructure fabricated by the method, wherein the heterostructure exhibits a two-dimensional electron gas (2DEG) with a sheet carrier density nsgreater than 1.5 x 1013cm'2, an electron mobility p greater than 1500 cm2 / V s, or a sheet resistance Rsless than 200 Q / n.

[0055] Experimental Results

[0056] Various experimental results were obtained by the inventors, including:

[0057] • an AlScGaN barrier layer having a thickness between 4 nm and 25 nm;

[0058] • an AlScGaN barrier layer having a thickness between 25 nm and 200 nm;

[0059] • an AIN interlayer with a thickness of 0.5 nm to 5 nm;• a heterostructure exhibiting a 2DEG with a sheet carrier density nsgreater than 1.5 x 1013cm'2and an electron mobility p greater than 1500 cm2 / V s, or a sheet resistance Rsless than 200 Q / n; and

[0060] • AlScGaN layers exhibit a root-mean-square (RMS) roughness as measured by AFM across a 2 gm x 2 gm scan area that is greater than 0 nm and less than 0.7 nm, and more preferably less than or equal to 0.5 nm.

[0061] Hall effect measurements were conducted on AlScGaN / AlN / GaN heterostructures using pressed indium contacts on 1 x 1 cm2square pieces with van der Pauw geometry. The surface morphologies and roughness of the AlScGaN layers were assessed using AFM. The structural characteristics of the heterostructures were measured using XRD, and AlScGaN layer thicknesses were measured using x-ray reflectivity (XRR).

[0062] FIG. 3 is a graph of AlScGaN thickness vs. TEGa flow (pmol min'1) showing growth rate data.

[0063] FIG. 4 is a graph of sheet carrier density ns (cm'2) vs. TEGa flow (pmol min'1) vs. electron mobility p showing Hall effect measurement data.

[0064] FIG. 5 is a graph of Intensity, counts vs. co, * showing XRD data for TEGa flow at 10 pmol min'1and 7.5 pmol min'1.

[0065] FIG. 6 is an AFM image of the AlScGaN layers showing an RMS roughness over a 2 pm x 2 pm scan area of 0.61 nm.

[0066] Advantages and Benefits

[0067] This invention has the advantages and benefits of increased 2DEG sheet charge compared to AlGaN / GaN HEMTs with higher electron mobilities than AlScN / GaN and InAlN / GaN 2DEG heterostructures with the same sheet charge.References

[0068] The following patent application publications are incorporated by reference herein:

[0069] [1] U.S. Patent Application Publication No. 2024 / 0274435 Al, filed April 4, 2024, by S. Leone, C. Manz, H. Menner, J. Wiegert, and J. Ligl, published August 15, 2024, and entitled “Method and apparatus for manufacturing a semiconductor layer and substrate provided therewith.”

[0070] [2] U.S. Patent Application Publication No. US 2024 / 0395921 Al, filed August 24, 2022, by Z. Mi, P. Wang, D. Wang, and E. Ahmadi, published November 28, 2024, and entitled “Semiconductor heterostructures with scandium Ill-nitride layer.”

[0071] Conclusion

[0072] This concludes the description of the preferred embodiment of the present invention. The foregoing description of one or more embodiments of the invention has been presented for the purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Many modifications and variations are possible in light of the above teaching. It is intended that the scope of the invention be limited not by this detailed description, but rather by the claims appended hereto.

Claims

IN THE CLAIMS:

1. A high-electron-mobility transistor (HEMT) heterostructure, comprising:a GaN channel layer;an AlScGaN barrier layer consisting of a quaternary III-V semiconductor alloy having the formula AlxScyGai-x-yN, where 0 <x < l, 0 <y < 0.5, and x + y < 1; and an optional interlayer, positioned between the GaN channel layer and the AlScGaN barrier layer, selected from binary, ternary, or quaternary III-V compounds;wherein a two-dimensional electron gas (2DEG), formed at an interface between the GaN channel layer and the AlScGaN barrier layer when the optional interlayer is not present, or formed at an interface between the GaN channel layer and the optional interlayer when the optional interlayer is present, exhibits a sheet carrier density nsgreater than 1.5 x 1013cm'2and an electron mobility p greater than 1500 cm2 / V s.

2. The heterostructure of claim 1, wherein the 2DEG has a sheet resistance Rsless than 200 Q / n.

3. The heterostructure of claim 1, wherein the optional interlayer comprises a thin AIN interlayer with a thickness of 0.5 nm to 5 nm.

4. The heterostructure of claim 1, wherein the AlScGaN barrier layer exhibits a root-mean-square (RMS) surface roughness as measured by atomic force microscopy (AFM) across a 2 pm x 2 pm scan area that is less than 0.5 nm.

5. The heterostructure of claim 1, wherein the AlScGaN barrier layer has a thickness between 4 nm and 25 nm.

6. The heterostructure of claim 1, wherein the AlScGaN barrier layer has a thickness between 25 nm and 200 nm.

7. The heterostructure of claim 1, wherein the AlScGaN barrier layer further comprises one or more additional III-V semiconductor layers forming a composite barrier.

8. The heterostructure of claim 7, wherein the composite barrier is a superlattice.

9. The heterostructure of claim 1, wherein the AlScGaN barrier layer is used in a multi-channel transistor comprised of a plurality of alternating AlScGaN barrier layers and one or more additional III-V semiconductor layers that form a superlattice.

10. The heterostructure of claim 9, wherein the one or more additional III-V semiconductor layers comprise one or more GaN layers.

11. The heterostructure of claim 1, wherein the AlScGaN barrier layer has a composition that is engineered to be lattice-matched or polarization-matched to the GaN channel layer for reduced strain and enhanced thermal stability.

12. The heterostructure of claim 1, wherein the AlScGaN barrier layer is graded in composition along a growth direction to induce polarization doping and form a three-dimensional carrier gas.

13. The heterostructure of claim 1, wherein the AlScGaN barrier layer has a crystal orientation selected from Ill-polar, N-polar, nonpolar, or semipolar orientations.

14. A method of fabricating a HEMT heterostructure, comprising: forming a GaN base layer on a substrate;optionally depositing an interlayer of AIN or another III-V compound on or above the GaN base layer;depositing a barrier layer of quaternary AlScGaN on or above the interlayer and / or GaN base layer by metalorganic chemical vapor deposition (MOCVD) using precursors comprising:trimethylaluminum (TMA1),trimethylgallium (TMGa) or triethylgallium (TEGa), bis(ethylcyclopentadienyl)scandium ((EtCp)2Sc(dbt)), and ammonia (NH3);wherein the flow rates of TMGa or TEGa, TMA1, and (EtCp)2Sc(dbt) are adjusted to control the relative Al, Ga, and Sc content, andwherein the growth temperature is between 900 °C and 1000 °C and the growth pressure is approximately 150 Torr.

15. A HEMT hetero structure fabricated by the method of claim 14, wherein the heterostructure exhibits a two-dimensional electron gas (2DEG) with a sheet carrier density nsgreater than 1.5 x 1013cm'2, an electron mobility p greater than 1500 cm2 / V s, or a sheet resistance Rsless than 200 Q / n.

16. A method, compri sing :fabricating a high-electron-mobility transistor (HEMT) heterostructure comprised of:a GaN channel layer;an AlScGaN barrier layer consisting of a quaternary III-V semiconductor alloy having the formula AlxScyGai-x-yN, where 0 < x < l, 0 < y < 0.5, and x + y < 1; andan optional interlayer, positioned between the GaN channel layer and the AlScGaN barrier layer, selected from binary, ternary, or quaternary III-V compounds;wherein a two-dimensional electron gas (2DEG), formed at an interface between the GaN channel layer and the AlScGaN barrier layer when the optional interlayer is not present, or formed at an interface between the GaN channel layer and the optional interlayer when the optional interlayer is present, exhibits a sheet carrier density nsgreater than 1.5 x 1013cm'2and an electron mobility p greater than 1500 cm2 / V s.

17. The method of claim 16, wherein the 2DEG has a sheet resistance Rsless than 200 Q / n.