Method of producing a gas adsorbent media
The reaction of alkali silicate with an aqueous acidic salt solution at pH 4-6 forms a stable mesoporous silica gel, addressing the inefficiencies of conventional methods by producing a reliable gas adsorbent media with enhanced adsorption capabilities and tailored functionalities.
Patent Information
- Application Number
- PCT/US2026/027043
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional methods for producing silica gel as a gas adsorbent media are hazardous, inefficient, and result in inconsistent material properties due to the use of strong acids, leading to poor adsorption performance.
A method involving the reaction of alkali silicate with an aqueous acidic salt solution at pH 4-6 forms a stable mesoporous silica gel, using ammonium sulfate as a chemical buffer to maintain pH, eliminating the need for additional pH regulation and hazardous acids, and incorporating additives for enhanced performance.
This method produces a reliable and efficient gas adsorbent media with consistent properties, capable of adsorbing water vapor and contaminants, and can be tailored for specific applications by adding activated carbon or zeolites to enhance functionality.
Smart Images

Figure IMGF000013_0001_TABLE 
Figure IMGF000013_0002_TABLE 
Figure 00000018_0000
Abstract
Description
[0001] Method of producing a gas adsorbent media
[0002] TECHNICAL FIELD
[0003] The present disclosure relates to a method of producing a gas adsorbent media, a dehumidification block, and a dehumidification apparatus comprising gas adsorbent media obtained by the method.
[0004] BACKGROUND ART
[0005] Gas adsorbent media is often used in applications for dehumidification, purification, or adsorption. Silica gel is a commonly used desiccant due to ease of manufacturing and low cost. Tailoring the properties of silica gel, like pore volume or pore width, can be done through regulating the pH or ripening steps. Conventional methods to produce silica gels containing predominantly mesopores (i.e. pore widths of 2-50 nm) often utilize strong acids (such as sulfuric acid, hydrochloric acid, etc.) or ammoniated water, which are hazardous and toxic. Additionally, the use of acids requires constant regulation of the gelling pH to maintain a consistent product. Further, variations in conditions during the gelling process can lead to inconsistent material properties and poor adsorption performance.
[0006] There is thus a need for a more efficient and reliable method of producing a gas adsorbent media.
[0007] SUMMARY
[0008] It is an object of the present invention to mitigate, alleviate or eliminate one or more of the above-identified deficiencies and disadvantages in the prior art and solve at least the above mentioned problem. According to a first aspect of the invention there is provided a method of producing a gas adsorbent media comprising the step of bringing an alkali silicate into contact with an aqueous acidic salt solution, said acidic salt solution having a pH between 4-6, and allowing said acidic salt solution to react with the alkali silicate to form a solid, mesoporous silica gel. The acidic salt acts as a chemical buffer and maintains a stable pH leading to fast and reliable creation of a gas adsorbent media in the form of solid, mesoporous silica gel. The gas adsorbent media may suitably include a substrate for the solid, mesoporous silica gel.
[0009] According to a second aspect there is provided a dehumidification block comprising the solid, mesoporous silica gel gas adsorbent media.
[0010] According to a third aspect there is provided a dehumidification apparatus comprising the dehumidification block.Effects and features of the second and third aspects are to a large extent analogous to those described above in connection with the first aspect. Embodiments mentioned in relation to the first aspect are largely compatible with the second and third aspects.
[0011] The present disclosure will become apparent from the detailed description given below. The detailed description and specific examples disclose preferred embodiments of the disclosure by way of illustration only. Those skilled in the art understand from guidance in the detailed description that changes and modifications may be made within the scope of the disclosure. Hence, it is to be understood that the herein disclosed disclosure is not limited to the particular details or steps of the methods described since such details and method may vary. It is also to be understood that the terminology used herein is for purpose of describing particular embodiments only, and is not intended to be limiting.
[0012] BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Fig. 1 schematically illustrates a substrate element for gas adsorbent media according to the present invention;
[0014] Fig. 2 schematically illustrates a honeycomb matrix substrate of gas adsorbent media according to the present invention;
[0015] FIG. 3 schematically illustrates another structure of honeycomb matrix substrate of gas adsorbent media according to the present invention;
[0016] FIG. 4 shows a graph of the incremental pore volumes and cumulative pore volumes measured by nitrogen physisorption;
[0017] FIG. 5 shows a graph of the amount of water vapor adsorbed as a function of relative humidity at 25°C on mesoporous silica gel prepared with ammonium sulfate and different additives; FIG. 6 shows a graph of the amount of water vapor adsorbed as a function of relative humidity at 25°C on mesoporous silica gel prepared with different acidic salts.
[0018] DETAILED DESCRIPTION
[0019] The method of producing a gas adsorbent media according to the present invention comprises the step of bringing an alkali silicate into contact with an aqueous acidic salt solution. The acidic salt solution has a pH between 4-6 and is allowed to react with the alkali silicate to form a solid, mesoporous silica gel, wherein the acidic salt acts as a gelling agent. The produced gas adsorbent media is suitable for use in applications for dehumidification, filtration andadsorption, and the gas adsorbed may typically be, for example, water vapor, possibly containing various contaminants. Performing the reaction in aqueous solution containing alkali silicate and acidic salt ensures sufficient contact between the alkali silicate and acidic salt, thus providing a faster and more reliable process of creating mesoporous silica gel. The mesoporous silica gel forms as a result of the gelling pH being between 4-6. The acidic salt in the aqueous solution acts as a chemical buffer and maintains a stable pH, without any need of adding extra acid of acidic salt during the gelling process, in a way that would not be possible with conventional acids, such as sulfuric or hydrochloric acid, historically used to control pH in the gelling process. Additionally, this eliminates the need to use mesoporogens or surfactants that are commonly used to make mesoporous silica gels. Gelling at lower pH will result in microporous silica gel and at higher pH the obtained silica gel would be unstable and essentially nonporous.
[0020] A mesoporous silica gel may typically have a micropore volume <0.02 cm3 / g, a BET surface area of about 250 m2 / g, a total pore volume of about 0.30 cm3 / g, and an average pore size of about 8.5nm, where about 90% of pore volume is between 5-20nm.
[0021] The acidic salt solution may preferably be a solution of water and an acidic salt selected from the group consisting of ammonium sulfate, ammonium chloride, ammonium acetate, ammonium nitrate, magnesium sulfate, magnesium nitrate, zinc sulfate, copper sulfate, or a combination thereof. These acidic salts are capable of maintaining a stable pH between 4.5-6 and produce a mesoporous silica gel matrix. The acidic salt solution preferably has a pH between 4.5-6 and a concentration of 50-300 grams of acidic salt per liter of solution, not in excess of the saturation limit of the salt. There should preferably be at least a 1:1 molar balance of SiO2to acidic salt, and it is preferred to have an excess of acidic salt when reacting with alkali silicate as to maintain a stable pH throughout the course of the chemical reaction. Magnesium sulfate as the acidic salt produces a good mesoporous silica gel, but an extra processing step may typically be needed to remove insoluble magnesium hydroxide precipitate formed during the reaction, as illustrated in Formula (I) below.
[0022] MgSO4+ Na2SiO3+ H2O -> SiO2+ Na2SO4+ Mg(OH)2(I)
[0023] However, the acidic salt may more advantageously be ammonium sulfate having a pH in the acidic salt solution of preferably between 4.5-5. Ammonium sulfate has been observed to produce high-performing gas adsorbent media without contamination from insoluble precipitates. Mesoporous silica gel produced with ammonium sulfate as the gelling agent contains larger pores than silica gel made at lower pH. These larger pores adsorb water more weakly than the smaller pores, such that less energy is required to remove the water and regenerate the large pore silica gel.Ammonium sulfate dissolves in water to form a solution of approximately pH 4.5 without the addition of extra acid or other pH regulators. Ammonium cations (NH4+) can partially dissociate in water to form ammonia (NH3) and an acidic proton (H+), where the proton can then react with alkali silicate, e.g. sodium silicate, to form the silica gel matrix, as illustrated in Formula (II) below.
[0024] (NH4)2SO4(aq) + Na2SiO3(aq) -> H2O + SiO2(s) + Na2SO4+ 2NH3(g) (II)
[0025] The released ammonia can be returned to ammonium sulfate by the addition of sulfuric acid at the end of the process, thereby increasing sustainability and eliminating hazardous emissions.
[0026] It is preferred to maintain an excess of ammonium sulfate, to avoid depletion of NH4+cations in the solution as the reaction proceeds. There is no maximum concentration of ammonium sulfate in the solution as long as the ammonium sulfate can fully dissolve in water, which would be about 800 g / L at 40 °C for complete saturation. The acidic salt solution preferably has a concentration of 50-300 grams ammonium sulfate per liter solution.
[0027] The alkali silicate brought in contact with the aqueous acidic salt solution and reacted to form a solid, mesoporous silica gel is advantageously sodium silicate. Sodium silicate may be preferred because it has appropriate chemical properties, stability and pH, and is readily available and affordable. Alternatives to sodium silicate may be lithium silicate or potassium silicate or an alkoxysilane (e.g. tetraethoxysilane), but these are considered less promising as they are less widely available, more expensive, or produce volatile organics as emissions (e.g., ethanol from tetraethoxysilane).
[0028] In order to generate a fully set solid, mesoporous silica gel gas adsorbent media, the alkali silicate is preferably allowed to contact the acidic salt solution for time period of at least 20 minutes at a temperature of 15 °C to 60 °C. This provides time for the reaction to approach completion and leads to a sufficiently formed silica gel matrix with good performance. There is no upper time limit for the reaction, but up to 90-120 minutes may be preferred to ensure generation of a fully formed mesoporous silica gel matrix. The time needed for the reaction is closely related to the temperature of the acidic salt solution because higher temperatures will cause the reaction to proceed faster. A temperature of 35-45 °C may be advantageous to allow for faster reaction time than room temperature, while being sufficiently cold to not require additional safety precautions or too high energy consumption.
[0029] The mesoporous silica gel obtained by the above reaction of alkali silicate with the aqueous acidic salt solution may be somewhat unstable at high pH. This can be mitigated by further including a step of reacting the solid, mesoporous silica gel with an acidic solution to reduce the pH to a pH of about 1 to 4. This stabilizes the silica gel matrix, so that the mesoporous silica gel gas adsorbent media can maintain its high adsorption capacity also when exposed tohot air streams, for example during regeneration of mesoporous gas adsorbent having been used in an application for dehumidification, filtration or adsorption. The reaction of the solid, mesoporous silica gel with an acidic solution to reduce the pH to about 1-4, may preferably be performed as an acidic rinse, to remove excess sodium or ammonium salts and reduce the pH of the mesoporous silica gel media itself. The acidic solution may a weak aqueous solution sulfuric acid or hydrochloric acid, having a concentration of e.g. 0.1-10 % by weight.
[0030] However, instead of using a solution of weak sulfuric or hydrochloric acid as the acidic solution for this step, the acidic solution may advantageously be a solution of a multivalent salt, preferably an aluminum salt or a titanium salt, more preferably aluminum sulfate, aluminum chloride, aluminum nitrate, or titanium sulfate, or a combination thereof, where the solution of multivalent salt preferably has a pH of 1 to 4. Multivalent salts, such as those comprising aluminum or titanium cations spontaneously form a solution with a pH between 2-4 without the need for additional acid. A pH below 4 ensures that the multivalent cations are kept in solution and prevents precipitation.
[0031] In addition to removing excess sodium or ammonium salts and reducing pH of the silica gel media, the reaction with the solution of a multivalent salt also further improves long-term high-temperature thermal stability of the mesoporous silica gel gas adsorbent media due to incorporation of the multivalent cation into the silica gel matrix. When alkali silicate reacts to form a silica gel matrix, inherent "defects" are likely formed, that may be susceptible to breaking apart. Aluminum, and other multivalent cations, can react with such defects to "heal" them and make the silica gel matrix more difficult to break apart.
[0032] In order to remove excess salts and acid from the mesoporous silica gel, the method preferably further comprises a step of washing the mesoporous silica gel, preferably with water, e.g., deionized water, and then drying it. The washing removes substances that can cause damage in the mesoporous silica gel product or to metal surfaces that hold the mesoporous silica gel media in place. The washing can be carried out by placing the silica gel in a suitable container and pouring the washing solution, typically water or another appropriate solvent, over the silica gel until it is fully submerged. Gentle agitation of the container may facilitate the removal of undesired substances. The silica gel may be allowed to soak in the washing solution for a period, e.g. 10 to 30 minutes. Once the washing is complete, excess washing solution is drained from the silica gel. The silica gel can then be dried to desired final moisture content placing it on a tray to air dry at room temperature or at an elevated temperature, such as 100°C to 150°C. The dried silica gel may be stored in an airtight container to prevent moisture absorption from the environment, ensuring it remains dry and ready for use.
[0033] The alkali silicate that is to be brought into contact with the aqueous acidic salt solution and reacted to form a solid, mesoporous silica gel may suitably be provided as an aqueous solutioncontaining the alkali silicate. This further reduces any issue of possible insufficient moisture content during forming of the mesoporous silica gel, and thus creation of mesoporous silica gel is thus fast and more reliable.
[0034] The aqueous solution of alkali silicate, preferably, has a silicate concentration of about 3 to 60 weight percent calculated as silica based on the total weight of the aqueous solution. This concentration ensures that a sufficient amount of alkali silicate is present to give enough silica gel product to be useful, while avoiding that the aqueous solution alkali silicate becomes too viscous to work with due to too high concentration.
[0035] The method may advantageously comprise adding one or more additives to the aqueous alkali silicate solution, prior to bringing it into contact with the acidic salt solution to form a composite of solid, mesoporous silica gel and the one or more additives. The additives may preferably be activated carbon, zeolite, metal-organic framework, inorganic metal oxide, ora combination thereof. The additives can be added to alter the final properties of the mesoporous silica gel matrix. Typically, the mesoporous silica gel formed through reacting alkali silicate, e.g. sodium silicate, with ammonium sulfate is used for dehumidification. In such application activated carbons, zeolites (e.g., MFI (ZSM-5 type), FAU (X, Y, or USY type), LTA (3A, 4A, or 5A type), metal-organic frameworks (MOFs) (e.g., aluminum fumurate, MIL-160, MOF-303, MIL-100, UiO-66, or MOF-808), and inorganic metal oxides (e.g., titanium oxide (rutile or anatase), manganese oxide, aluminum oxide (alumina), or similar materials) can advantageously contribute in forming a composite that can remove volatile organic compounds (VOCs) or odor molecules, enhance water removal, or capture acid gases (e.g., CO2, SOX, NOX).
[0036] In the method of the present invention, the alkali silicate provided in the form of an aqueous solution containing alkali silicate may thus be added directly to the aqueous solution of acidic salt, i.e., introduced into a container holding a volume of the aqueous solution of acidic salt. This can suitably be done by dripping the aqueous alkali silicate solution into the aqueous acidic salt solution, i.e., adding the alkali silicate solution drop by drop into the acidic salt solution. The thus introduced alkali silicate is then allowed to react with the solution of acidic salt to form a solid, mesoporous silica gel gas adsorbent media. The rate of dripping may be controlled to maintain a steady and consistent addition, preventing any sudden changes in the reaction environment, to achieve a uniform particle size and structure in the resulting silica gel. By dripping the aqueous alkali silicate solution into the aqueous acidic salt solution a powdered mesoporous silica gel product may be obtained, which can be used for example as packed column adsorbent media for air treatment, or be formed into beads of various shapes and sizes, or be separately coated onto a substrate. Powdered mesoporous silica gel may benefit from being formed into mesoporous silica gel beads by addition of a binder, such as colloidal silica, alumina, or ceramic binder, to prevent dusting and material loss when brought into contact with an air stream during use. The mesoporous silica gel beads may further beused to form a gas adsorbent media block, e.g., by placing them in a mesh container or adsorption column.
[0037] Alternatively, the alkali silicate, provided in the form of an aqueous solution containing alkali silicate, may be brought into the form of a solid or semi-solid alkali silicate, i.e., a solid or semisolid alkali silicate precursor, prior to bringing it into contact with the aqueous solution of acidic salt, such that the alkali silicate in the form of solid or semi-solid alkali silicate can be brought into contact with the aqueous solution of acidic salt. The solid or semi-solid alkali silicate may suitably be immersed into the aqueous solution of acidic salt to allow the reaction forming the solid, mesoporous silica gel. By semi-solid alkali silicate is meant a concentrated liquid or gel or paste, retaining some fluidity but being significantly thicker and more cohesive than a typical liquid solution. A semi-solid alkali silicate is characterized by its intermediate state between liquid and solid, exhibiting properties such as high viscosity, plasticity, and the ability to hold shape to some extent, typically exhibiting a viscosity above 100,000 cP. Semisolid alkali silicate can be spread or molded but does not flow freely like a liquid. A solid alkali silicate is a drained and dried solution of alkali silicate, typically appearing as a crystalline or amorphous solid and rigid material, having a moisture content in equilibrium with the ambient air.
[0038] The solid or semi-solid alkali silicate may preferably be provided as a solid or semi-solid coating on a substrate. The substrate with the coating of solid or semi-solid alkali silicate will then suitably be immersed in the aqueous solution of acidic salt and will, after reaction, form a silica gel gas adsorbent media block comprising the solid, mesoporous silica gel.
[0039] The solid or semi-solid alkali silicate can be coated on a substrate by applying an aqueous solution of alkali silicate to a substrate, allowing the alkali silicate solution to drain to form a cohesive alkali silicate coating on the substrate, and thereafter drying the coated substrate to moisture content of 40-80 weight % based on the total weight of the cohesive alkali silicate coating. The alkali silicate can be applied to the substrate by impregnating the substrate material with the alkali silicate solution, for example by dragging the substrate through a trough filled with an alkali silicate solution or by pouring alkali silicate solution over the substrate. Excess alkali silicate solution can be removed by scraping off any excess if the substrate is flat, or if the substrate has channels, forcing air through the channels to push out excess solution. Removing excess moisture aides in obtaining a desired "stickiness" of the coated substrate so that elements of the substrate are strong enough to maintain any shaping or processing, but wet enough to adhere to adjacent elements. Fully dried elements will be strong, but won't stick together whereas very wet elements will stick together well, but won't have structural stability. If desired, the drying can be assisted by heat.
[0040] The substrate may be a solid panel or a three-dimensional structure having channels or cavities. Adhering the mesoporous silica gel to a substrate allows for customizing contact areawith a gas or air stream to be treated. The customization can be done by creating channels of different width or cutting a coated substrate to a desired size and shape.
[0041] In the present context, a solid panel is an essentially flat, solid piece of substrate material. It can have a rectangular circumference, but can also be circular, oval or have any other suitable circumferential shape. It can be in the form of a sheet (e.g. having a thickness of less than 10% of its circumference) or have a higher thickness to be shaped as a cuboid or cylinder (e.g. having a thickness of more than 10% of its circumference). Substrate sheets may have a thickness of 0.1 to 0.4 mm, preferably 0.17 to 0.18 mm, and may have a bulk density of less than 100 g / m2, preferably less than 35 g / m2.
[0042] Further, in the present context, a three-dimensional structure having channels or cavities therein is typically a structure extending in three dimensions and having a more complex internal or external geometry. The three-dimensional structure may have any suitable shape, such as a cylinder having any suitable base shape, or a cuboid, and may preferably include through-channels that can allow a gas flow to pass through the structure or cavities therein, may most preferably be a honeycomb structure comprising an array of parallel channels allowing transport of fluid through the honeycomb structure. The honeycomb structure is a geometric configuration that typically features a repeating pattern of parallel channels, which can be, e.g., hexagonal, square, rectangular, or triangular, maximizing space utilization and minimizing material use, providing a high strength-to-weight ratio. The array of parallel channels in a honeycomb structure creates a high contact area between the mesoporous silica gel gas adsorbent media and the gas or air stream to be treated. This serves to minimize pressure loss through the depth of the media allowing for high fluid velocities to be treated without a significant energy penalty due to flow resistance. A three-dimensional structure substrate may be composed by substrate sheet material. A honeycomb structure can be made by laminating a corrugated sheet material to a flat liner of substrate material as illustrated in Fig. 1. The flutes may have a height of 1-5 mm, a pitch of about 2-5 mm and a ratio of height / pitch of about 0.25-1. The laminated flute and flat sheet may preferably be formed into a honeycomb matrix comprising an elongated honeycomb element wound into a compact honeycomb cylinder shape, as illustrated in Fig. 2, or comprise a plurality of stacked honeycomb elements forming a honeycomb block, as illustrated in Fig. 3. Fig. 1 shows a flat liner (11) and corrugated flute sheet (12) of a substrate element (10) for gas adsorbent media. Fig. 2 shows a substrate element (10) of gas adsorbent media comprising a flat liner (11) and corrugated flute sheet (12) to form a honeycomb matrix (13) by winding the element around a central axis. Fig. 3 shows a honeycomb matrix substrate (15) formed by assembling a plurality of substrate elements (10) of gas adsorbent media comprising a flat liner (11) and corrugated flute sheet (12).
[0043] Regardless of the shape, the substrate is suitably comprised of fibrous material, preferably in the form of woven or nonwoven fibrous material, most preferably a fiberglass paper orceramic fiber paper. The substrate may be a porous material made from about 70-100%, preferably about 90%, heat resistant inorganic fibers having a diameter of about 3 to 15 microns. Typical fibers may be ceramic fiber, slag fiber, carbon fiber and / or glass fiber. In addition, the paper may contain up to about 15% natural or synthetic binders, such as methyl cellulose, polyvinyl alcohol, polyvinyl acetate, melamine, or mixtures thereof. The alkali silicate is adhered in gaps between the fibers and on the surface of the fibrous material.
[0044] Fiberglass paper and ceramic fiber paper can be easily formed into different shapes and structures, have good absorbency of the alkali silicate solution, do not soften significantly or disintegrate when wet, and are fire resistant. Other potential substrates, like cellulose or polymer papers, may be useful in some circumstances, but may be unstable when wet or in contact with alkali solutions, are expensive, and not fire resistant without further chemical treatment.
[0045] Thus, for example, in order to form the solid, mesoporous silica gel adsorbent media from sodium silicate solution, the substrate, preferably a composite honeycomb matrix substrate, is contacted with an aqueous solution containing acidic salts, preferably ammonium sulfate. The sodium silicate and ammonium sulfate salts react to form a solid, mesoporous silica gel coating on the substrate. Sodium sulfate, a by-product, excess ammonium sulfate, and mesoporous silica gel not supported in the paper may then be removed by washing. By suitably heating and drying the honeycomb matrix, the main constituent thereof, a solid, mesoporous silica gel adsorbent media, is obtained.
[0046] It has been found that to form a satisfactory mesoporous silica gel coating from the sodium silicate impregnated matrix, the temperature of the acidic salt solution and the pH of the solution are important interrelated factors which should preferably be considered together. For the above, and other purposes, the temperature of the bath may generally be controlled to be from 20 to 60 °C, preferably from 35-45 °C. In general, the reaction time may be from 15 minutes to 180 minutes. The pH is suitably maintained during the reaction between a pH of 4 to 5.5, and preferably 4.5, by the equilibrium that occurs between ammonium cations, sulfate anions, and water in solution.
[0047] Additionally, it may be useful to circulate the acidic salt solution through a honeycomb matrix substrate for at least 15 minutes, preferably 120 minutes, by evenly raising and lowering the honeycomb matrix from a bath of the acidic salt solution. If desired, the acid solution may be pumped through the honeycomb matrix instead of raising and lowering the matrix. Rather than employing a bath, the acidic salt solution can be circulated through the honeycomb matrix substrate. Optionally, the substrate may be passed under a waterfall of acidic salt solution to form the mesoporous silica gel media.Aluminum salts may also be employed, if desired, as their presence tends to stabilize the matrix of the silica gel pores and enhances the long term stability of the mesoporous silica gel. Aluminum sulfates, chlorides, nitrates, or phosphates may be employed to incorporate aluminum into the final matrix. This can be achieved by rinsing, dipping, washing, or otherwise contacting the solid, mesoporous silica gel coated substrate with an aqueous solution of aluminum salt. The final product is then comprised of a mesoporous, aluminosilicate containing 0.5-1.5wt% AI2O3 and 98.5-99.5wt% SiCh.
[0048] After the alkali silicate has been converted to a solid, mesoporous silica gel, it is washed to remove by-products and excess reactants. Thereafter, the substrate and the solid, mesoporous silica gel is suitably dried with air at appropriate flow rates and air temperatures to form an aerogel, by replacing the liquid in the pores of the mesoporous silica gel by air. The temperature and flow rates employed for this purpose are not critical. In general, an air temperature of about 150 °C and a flow velocity of about 200 feet per minute may be satisfactory.
[0049] The mesoporosity of the final silicate media is controlled by the pH and temperature of the acidic salt solution. By employing a pH of about 4.5 at a reaction temperature of about 40 °C the final silica gel coating may have a total pore volume of about 0.30 cm3 / g and a micropore volume of less than 0.02 cm3 / g. Additionally, the silica gel media may have a surface area, measured by the Brunauer-Emmett-Teller (BET) method, of between 260 to 300 m2 / g and an average pore diameter of about 8.5 nm with a relatively narrow pore size distribution where 90% of the total pore diameter is between 5-20 nm, see Fig. 4, showing a graph of incremental (open circles) pore volumes and cumulative (closed circles) pore volumes as a function of the pore width, calculated from nitrogen adsorption / desorption isotherms measured at -196 °C across a pressure range of 0.06-720 torr by the Barrett-Joyner-Halenda (BJH) method, which is a commonly used method to determine the average pore diameters for mesoporous materials.
[0050] When used in dehumidification applications the mesoporous silica gel medium of the present invention can be regenerated at relatively low temperatures, usually <100C, and preferably about 50 °C, using less energy than with typical humidity exchange materials. Lowering the gelling pH below about 4 results in a silica gel product with smaller pore diameters and more costly regeneration requirements.
[0051] Moreover, the properties of the solid, mesoporous silica gel adsorbent media can be tailored by addition of additives to the sodium silicate solution prior to coating the paper. For example, activated carbon may be added to the alkali silicate at 5 wt% on a dry weight basis relative to alkali silicate. Addition of activated carbon powder may be achieved by dispersion of activated carbon directly into a solution of sodium silicate, by powder coating onto the sodium silicate impregnated elements, by aerosolizing a mixture of activated carbon to coat a gas adsorbingelement, or by other such means. The activated carbon modified alkali silicate coated substrate elements can then be treated with an acidic salt solution, as described previously, to produce a solid, mesoporous gas adsorbing media. Addition of activated carbon does not alter the mesopore structure or in any way hinder the reaction of sodium silicate with ammonium sulfate, but does provide additional functionality to remove odorous compounds from a gas stream.
[0052] The present invention also relates to a dehumidification block comprising solid, mesoporous silica gel gas adsorbent media manufactured by the method described above. The block is typically formed by winding or stacking substrate elements coated in alkali silicate (e.g. sodium silicate), then immersing the block into a tank containing a solution of acidic salt (e.g. ammonium sulfate), stabilizing the block in a second acidic solution (e.g. aluminum sulfate solution), and then drying to obtain the final gas adsorbent media block.
[0053] The main industrial application of the mesoporous silica gel gas adsorbent media is to remove humidity and water from an air stream. The mesoporous silica gel produced by reacting alkali silicate with a solution of acidic salt produces a hydrophilic mesoporous silica gel product with large pores. This media can be used to remove moisture from an airstream with high humidity. The present invention also relates to a dehumidification apparatus comprising the dehumidification block, where the dehumidification block preferably is comprised in a dehumidification rotor, to be placed in a position in a system that passes moisture laden air through the block for a period of time, and then switches to a hot, dry air stream to remove the adsorbed moisture, and thus regenerate the gas adsorbent media.
[0054] To fit in a dehumidification rotor, the dehumidification block may be cut into a circle, or multiple circle sectors to be assembled, to form a round wheel shape, between 0.3 to 5 meters in diameter. The rotor is then placed inside a dehumidification assembly and rotated through various zones. A portion of the rotor first rotates through a process zone with cool, humid air at a specified rotation speed to dehumidify the air stream where the mesoporous silica gel adsorbs water. Then, the moisture-laden rotor passes through a heated air stream to remove the adsorbed water. The dry rotor then returns to the humid air stream to complete the cycle. This circular process allows for the continuous dehumidification of a humid air stream and production of a dry air stream.
[0055] EXPERIMENTS
[0056] Water adsorption capacities were measured at 25 °C and a relative humidity of 80%. Prior to water vapor exposure, mesoporous silica gel samples were dried at 150 °C in air for 30 minutes. Water accessible surface areas were calculated from water adsorption isotherms (Examples 1-4 are shown in Fig. 5) measured at 25 °C and a relative humidity range of 5-30% (1.2 - 7.2 torr) using the Brunauer-Emmett-Teller (BET) method.Examples 1-10
[0057] Examples 1-10 describe the procedure for producing solid, mesoporous silica gel gas adsorbent media using ammonium sulfate as the acidic salt (gelling agent).
[0058] Example 1
[0059] Fiberglass paper samples, having a bulk density of 35 g / m2and an organic content of <11%, were coated with an aqueous solution of sodium silicate (38% solids, 3.22 SiO2 / Na2O molar ratio) to obtain a loading of about 180 g / m2dry weight. The coated fiberglass paper samples were then partially dried to 50 wt% solids and contacted with 10 liters per kg coated paper of an aqueous solution containing 210 grams per liter of ammonium sulfate at a pH of 4.5 for 120 minutes at a bath temperature of 40 °C. The samples were washed with water and dried at 150 °C for 60 minutes to obtain a solid, mesoporous silica gel gas adsorbent media.
[0060] Example 2
[0061] Example 1 was repeated, but after the washing step and prior to drying the samples were contacted with 10 liters per kg coated paper of an aqueous solution containing 180 grams per liter of aluminum sulfate at a pH of 3.2 for 30 minutes at a bath temperature of 22C. The samples were then washed with water and dried at 150 °C for 60 minutes to obtain a solid, mesoporous aluminosilicate gas adsorbent media.
[0062] Example 3
[0063] The same fiberglass paper samples from Example 1 were coated with an aqueous solution of sodium silicate (38% solids, 3.22 SiO2 / Na2O molar ratio) containing 5 wt% activated carbon to obtain a loading of about 180 g / m2dry weight. The coated fiberglass paper samples were then partially dried to 50 wt% solids and contacted with 10 liters per kg coated paper of an aqueous solution containing 210 grams per liter of ammonium sulfate at a pH of 4.5 for 120 minutes at a bath temperature of 40 °C. The samples were washed with water and then contacted with 10 liters per kg coated paper of an aqueous solution containing 180 grams per liter of aluminum sulfate at a pH of 3.2 for 30 minutes at a bath temperature of 22 °C. The samples were then washed with water and dried at 150 °C for 60 minutes to obtain a solid, mesoporous aluminosilicate gel gas adsorbent media containing activated carbon.
[0064] Example 4
[0065] The same procedure as Example 3 was performed but using 20 wt% faujasite zeolites, which have a SiCh / A Ch ratio less than 3, in place of the activated carbon when preparing the sodium silicate coating mixture.
[0066] The results of Examples 1-4 are disclosed in Table 1.
[0067] Table 1Example Alkali silicate solution Acidic Salt Treatment Water Capacity Surface # Identity after gelling at 80% RH, Area reaction 25°C; wt% m2 / g 1 Sodium Silicate Ammonium - 32.8 281
[0068] Sulfate
[0069] 2 Sodium Silicate Ammonium Aluminum 34.4 278
[0070] Sulfate Sulfate
[0071] 3 Sodium Silicate + Ammonium Aluminum 30.9 303
[0072] 5 wt% activated carbon Sulfate Sulfate
[0073] 4 Sodium Silicate + Ammonium Aluminum 32.9 371
[0074] 20 wt% faujasite zeolites Sulfate Sulfate
[0075]
[0076] Examples 1-4 show that the ammonium sulfate gelling reactions produces a porous, silica gel product with a Type IV isotherm (Fig. 5) consistent with the predominance of mesoporous channels (Fig. 4). The mesoporous silica gel product formed from Example 1 adsorbs approximately 33 wt% of water vapor at 25°C and 80% relative humidity. The pore structure and water adsorption capacity remain unchanged if an aluminum sulfate washing step is used (Example 2) or if activated carbon is incorporated into the sodium silicate solution prior to reaction with ammonium sulfate (Example 3). Addition of hydrophilic faujasite zeolites (Example 4) does not alter the water capacity at high relative humidities as shown in Table 1, but does increase the water accessible surface area. Additional water adsorption is observed at low relative humidities (i.e., <20%) due to the presence of micropores in faujasite zeolites that are comprised of pores <1 nm in diameter that strongly adsorb water vapor. As a result, these data show that the final properties of the mesoporous silica gel composite media can be modified by addition of various additives without alteration of the underlying mesoporous silica gel matrix.
[0077] Examples 5-10
[0078] The same procedure as Example 1 was performed but using alternative acidic salt solutions. Table 2
[0079] Example # Acidic Salt Identity Water Capacity at 80% RH, 25°C; wt% Surface Area m2 / g
[0080] 1 Ammonium Sulfate 32.8 281
[0081] 5 Ammonium Chloride 25.9 250
[0082] 6 Ammonium Acetate 20.9 246
[0083] 7 Ammonium Nitrate 28.9 242
[0084] 8 Zinc Sulfate 6.0 47
[0085] 9 Copper Sulfate 4.0 36
[0086] 10 Magnesium Sulfate 25.8 307
[0087] 11 Magnesium Nitrate 12.0 229
[0088]
[0089] Table 2 and Fig. 6 show the results from water capacity measurements on silica gels obtained by varying the acidic salt identity. Examples 1, 5-7, 10, and 11 all produced silica gels with similar water accessible surface areas between around 230-300 m2 / g, but with varying water capacities at 25°C and 80% relative humidity. Gelling with ammonium sulfate resulted in a silica gel product with the highest water capacity (32.8 wt%) while materials prepared in Examples 5-7 with alternative ammonium salts showed similar, albeit lower, water capacities (21-29 wt%). Keeping the sulfate anion the same, but changing the cation produced largely nonporous silicas when transition metal cations were used (e.g., zinc or copper). Magnesium sulfate (Example 10), however, produced a mesoporous silica comparable to those prepared with ammonium salts while magnesium nitrate showed a reasonable surface area but a lower water capacity. Both magnesium salts suffered from precipitation of insoluble magnesium hydroxides that could only be completely removed by washing the mesoporous silica product in moderately strong acid (pH<3). Ultimately, the reaction of sodium silicate with a solution of aqueous ammonium sulfate resulted in a mesoporous silica gel with highly desirable water adsorption properties that was also free of insoluble impurities.
[0090] The person skilled in the art realizes that the present disclosure is not limited to the preferred examples and embodiments described above. The person skilled in the art further realizes that modifications and variations are possible within the scope of the appended claims.
Claims
CLAIMS1. A method of producing a gas adsorbent media comprising the steps of:Bringing an alkali silicate into contact with an aqueous acidic salt solution, said acidic salt solution having a pH between 4-6, and allowing said acidic salt solution to react with the alkali silicate to form a solid, mesoporous silica gel.
2. The method of claims 1, wherein the acidic salt solution is a solution of water and an acidic salt selected from the group consisting of ammonium sulfate, ammonium chloride, ammonium acetate, ammonium nitrate, magnesium sulfate, zinc sulfate, copper sulfate, or a combination thereof, said acidic salt solution preferably having a concentration of 50-300 grams acidic salt per liter solution and a pH between 4.5-6.
3. The method of claim 2, wherein the acidic salt is ammonium sulfate, preferably having a concentration of 50-300 grams ammonium sulfate per liter solution, and a pH between 4.5-5.
4. The method of any one of the preceding claims, wherein the alkali silicate is allowed to contact the acidic salt solution for time period of at least 20 minutes at a temperature of 15 °C to 60 °C.
5. The method of any one of the preceding claims, wherein the method further includes a step of reacting the solid, mesoporous silica gel with an acidic solution to reduce the pH to a pH of 1 to 4.
6. The method of claim 5, wherein the acidic solution is a solution of a multivalent salt, said multivalent salt preferably being an aluminum salt or a titanium salt, more preferably aluminum sulfate, aluminum chloride, aluminum nitrate, or titanium sulfate, or a combination thereof, and said solution of a multivalent salt preferably having a pH of 1 to 4.
7. The method of any one of the preceding claims, wherein the method further comprises a step of washing and drying.
8. The method of any one of the preceding claims, wherein the alkali silicate is sodium silicate.
9. The method of any one of the preceding claims, wherein the alkali silicate is provided as an aqueous solution containing alkali silicate, preferably having a silicate concentrationof about 3 to 60 weight percent calculated as silica gel based on the total weight of the aqueous solution.
10. The method of claim 9, comprising adding one or more additives to the aqueous solution containing alkali silicate, priorto bringing it into contact with the acidic salt solution, said one or more additives preferably being activated carbon, zeolite, metal-organic framework, inorganic metal oxide to form a composite of solid, mesoporous silica gel and one or more of said additives.
11. The method of any one of claims 9 or 10, wherein the aqueous solution containing alkali silicate is added to said solution of acidic salt, preferably by dripping, and is allowed to react with the solution of acidic salt to form a solid, mesoporous silica gas adsorbent media.
12. The method of any one of claims 9 or 10, wherein the aqueous solution containing alkali silicate is brought into the form of a solid or semi-solid alkali silicate, prior to bringing it into contact with the aqueous solution of acidic salt, said solid or semi-solid alkali silicate being immersed in the aqueous solution of acidic salt to form said solid, mesoporous silica gel.
13. The method of claim 12, wherein the solid or semi-solid alkali silicate is provided as a solid or semi-solid coating on a substrate, by:a. applying the aqueous solution of alkali silicate to a substrate;b. allowing said alkali silicate solution to drain to form a cohesive alkali silicate coating on the substrate; and thereafterc. drying said coated substrate to moisture content of 40-80 weight % based on the total weight of the cohesive alkali silicate coating.
14. The method of claim 13, wherein the substrate is a solid panel or a three-dimensional structure having channels or cavities, the substrate preferably being comprised of fibrous material, said fibrous material being in the form of woven or nonwoven fibrous paper-based material, preferably a fiberglass paper or ceramic fiber paper.
15. The method of claim 14, wherein the substrate is a honeycomb structure comprising an array of through channels allowing transport of fluid through the honeycomb structure.
16. A dehumidification block comprising solid, mesoporous silica gel gas adsorbent media, said dehumidification block being manufactured by the method of any one of the preceding claims.
17. A dehumidification apparatus comprising the dehumidification block of claim 16.
18. The dehumidification apparatus of claim 17, wherein the dehumidification block is comprised in a dehumidification rotor.