Porous transport layer, membrane electrode assembly, water electrolysis device, and fuel cell

The porous transport layer with a microporous layer on a conductive substrate addresses the issues of membrane damage and high costs by ensuring effective gas diffusion and durability, achieving improved water electrolysis performance.

WO2026239902A1PCT designated stage Publication Date: 2026-11-19TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016446
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-01-28
Filing Date
2026-04-24
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing porous transport layers in water electrolysis devices are expensive and prone to damage the electrolyte membrane due to fuzziness, leading to reduced performance and high production costs.

Method used

A porous transport layer with a microporous layer on a conductive porous substrate, featuring voids with specific diameters and contact angles, and no through-holes, to enhance gas diffusivity and prevent membrane damage, while being cost-effective.

Benefits of technology

The solution effectively suppresses membrane damage, improves gas diffusion, and reduces production costs by using a cost-effective design with enhanced conductivity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-M000002
    Figure JPOXMLDOC01-APPB-M000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a porous transport layer that suppresses piercing of the electrolyte membrane by a conductive porous base material when used in a membrane electrode assembly, that has excellent gas diffusion properties, and that can be manufactured at a low cost. The present invention relates to a porous transport layer comprising a microporous layer on at least one side of a conductive porous base material that contains carbon fiber, wherein the microporous layer has voids with an average diameter of 3-70 μm, and the contact angle between the microporous layer and water is 70-180°.
Need to check novelty before this filing date? Find Prior Art

Description

Porous transport layer, membrane electrode assembly, water electrolysis device, and fuel cell

[0001] The present invention relates to a porous transport layer used in water electrolysis devices and fuel cells, and to a membrane electrode assembly, a water electrolysis device, and a fuel cell using the porous transport layer.

[0002] In recent years, methods for producing hydrogen through the electrolysis of water (water electrolysis), particularly those that use renewable energy as the power source for water electrolysis to produce clean hydrogen with a low environmental impact, have attracted attention. While there are several methods for water electrolysis, polymer electrolyte membrane (PEM) water electrolysis devices are being widely developed because they can utilize the technology of polymer electrolyte fuel cells (PEFCs) and can produce high-purity hydrogen.

[0003] The cell (water electrolysis cell) of a PEM-type water electrolysis apparatus has a structure in which a membrane electrode assembly (MEA) is formed by bonding catalyst layers to both sides of a solid polymer electrolyte membrane, sandwiching both sides of the MTL (Plastic Transport Layer), and further sandwiching the MEA with separators. In other words, in a PEM-type water electrolysis apparatus cell, the layer sandwiched between the catalyst layer and the separator is called the porous transport layer. For the porous transport layer, conductive porous substrates such as carbon paper or carbon felt, or metal porous sintered bodies made of titanium, are used in terms of conductivity and mechanical strength. Metal porous sintered bodies have the advantage of being resistant to corrosion, but are expensive. For this reason, a porous substrate made of carbon is sometimes used, especially on the cathode side where corrosion of carbon due to oxidation reactions does not occur. When a porous substrate made of carbon is used, the water electrolysis cell is fastened under high pressure, so the fuzz on the surface of the porous substrate may damage the polymer electrolyte membrane, causing deterioration of the polymer electrolyte membrane starting from that point, and potentially reducing the water electrolysis performance. Therefore, in order to cover the fuzzy surface of the porous substrate, a porous transport layer is sometimes used that consists of a microporous layer placed on top of a conductive porous substrate.

[0004] The porous transport layer used in water electrolysis devices requires low electrical resistance to reduce electrode overvoltage and high gas diffusivity to efficiently discharge the gas generated by water electrolysis. Furthermore, to reduce hydrogen production costs, the components of the water electrolysis device are desirable to be inexpensive, and the porous transport layer is therefore required to be as inexpensive as possible.

[0005] As a porous transport layer used in water electrolysis devices, Patent Document 1 discloses a porous metal gas diffusion layer characterized by being made of a porous metal sheet for solid polymer fuel cells. Patent Document 2 discloses a diffusion layer comprising a porous substrate made of a conductive material and a coating containing a metal oxide.

[0006] Japanese Patent Publication No. 2022-145670 Japanese Patent Publication No. 2023-76968

[0007] The conductive porous substrate made of a metal porous body disclosed in Patent Document 1 has the problem of being expensive due to high material costs and challenges in productivity.

[0008] The metal oxide coating described in Patent Document 2 is insufficient to cover the fuzziness of the conductive porous substrate and has the problem of damaging the electrolyte membrane.

[0009] Therefore, the present invention aims to provide a porous transport layer that can be manufactured at low cost while suppressing damage to the electrolyte membrane.

[0010] The present invention employs the following means to solve the above problems: (1) A porous transport layer having a microporous layer on at least one side of a conductive porous substrate containing carbon fibers, wherein the microporous layer has voids with an average diameter of 3 μm to 70 μm, and the contact angle between the microporous layer and water is 70° to 180°. (2) The porous transport layer according to (1), wherein there are no through holes in the microporous layer that penetrate from the surface of the microporous layer to the conductive porous substrate. (3) The porous transport layer according to (1) or (2), wherein the microporous layer has voids with an average diameter of 9 μm to 55 μm. (4) The porous transport layer according to any one of (1) to (3), wherein the area ratio occupied by voids with a diameter of 3 μm to 70 μm on the surface of the microporous layer is 0.1% to 50%. (5) A porous transport layer according to any one of (1) to (4), wherein the area ratio occupied by voids with a diameter of 3 μm or more and 70 μm or less in the cross-section of the microporous layer is 0.1% or more and 50% or less. (6) A porous transport layer according to any one of (1) to (4), wherein the area ratio occupied by voids with a diameter of 3 μm or more and 70 μm or less in the cross-section of the microporous layer is 0.5% or more and 20% or less. (7) A porous transport layer according to any one of (1) to (6), wherein the contact angle between the microporous layer and water is 130° or more and 180° or less. (8) A porous transport layer according to any one of (1) to (7), wherein the thickness of the conductive porous substrate is 0.3 mm or more. (9) A porous transport layer according to any one of (1) to (8), wherein the ratio obtained by dividing the pore volume in the range of pore diameters in the range of 3 μm or more and 100 μm or less by the pore volume in the range of pore diameters in the range of 3 μm or more and 180 or less is 4 or more and 180 or less. (10) A porous transport layer according to any one of (1) to (9), wherein the contact angle between the conductive porous substrate and air in water is greater than the contact angle between the microporous layer and air in water. (11) A porous transport layer according to any one of (1) to (10), wherein the conductive porous substrate does not allow water containing 20% ​​by mass of ethanol to permeate, but allows water containing 40% by mass of ethanol to permeate, and the microporous layer does not allow water containing 40% by mass of ethanol to permeate. (12) A porous transport layer whose mass loss after heat treatment at 400°C for 1 hour under air is 5 g / m². 2 A porous transport layer as described in any of (1) to (11) below. (13) A mass loss of 1 g / m² when immersed in hot water at 85°C for 5 hours.2 A porous transport layer according to any of (1) to (12) below. (14) A membrane electrode assembly using a porous transport layer according to any of (1) to (13). (15) A water electrolysis device using a porous transport layer according to any of (1) to (13). (16) A fuel cell using a porous transport layer according to any of (1) to (13).

[0011] According to the present invention, it is possible to suppress the penetration of the conductive porous substrate into the electrolyte membrane when used in a membrane electrode assembly, and to provide a porous transport layer that has excellent gas diffusion properties and can be manufactured at low cost.

[0012] This is a schematic cross-sectional view showing one example of the configuration of the porous transport layer of the present invention. This is a schematic top view of the porous transport layer of the present invention as seen from the microporous layer side. This is a schematic top view of the porous transport layer of the present invention as seen from the microporous layer side.

[0013] The porous transport layer of the present invention will be described in detail below, but the present invention is not limited to the embodiments described below.

[0014] <Conductive Porous Substrate> The conductive porous substrate used in the porous transport layer of the present invention contains carbon fibers. Examples of conductive porous substrates containing carbon fibers include carbon paper, carbon felt, carbon fiber fabric, carbon fiber paper, and carbon fiber nonwoven fabric. Among these, carbon paper is preferred because it is a conductive porous substrate obtained by binding a carbon fiber paper with resin carbides, and it has excellent properties for absorbing dimensional changes in the thickness direction of the electrolyte membrane (i.e., "springiness").

[0015] Examples of carbon fibers that can be preferably used in conductive porous substrates include polyacrylonitrile (PAN) type, pitch type, and rayon type. Among these, PAN type carbon fibers and pitch type carbon fibers are preferred because they have excellent mechanical strength. These fibers may also be mixed with natural or synthetic fibers such as rayon fibers, acrylic fibers, and cellulose fibers.

[0016] When using carbon fiber papermaking or carbon paper as a conductive porous substrate, the average length of the carbon fiber single fibers is preferably 3 mm or more and 20 mm or less. By setting the average length of the single fibers to 3 mm or more, more preferably 5 mm or more, the mechanical strength and conductivity of the conductive porous substrate can be improved. On the other hand, by setting the average length of the single fibers to 20 mm or less, more preferably 15 mm or less, the dispersion of carbon fibers during papermaking is improved, and a homogeneous conductive porous substrate can be obtained.

[0017] The thickness of the conductive porous substrate is preferably 0.3 mm or more. By making the thickness of the conductive porous substrate preferably 0.3 mm or more, more preferably 0.4 mm or more, even more preferably 0.5 mm or more, and most preferably 1.0 mm or more, the pressure can be uniformly distributed in the in-plane direction, thereby increasing the compressive strength of the conductive porous substrate, and increasing the contact area between the porous transport layer and the catalyst layer, which reduces contact electrical resistance and improves water electrolysis performance. In addition, the gas diffusion pathways increase, which increases gas diffusivity in the in-plane direction. Furthermore, it is possible to prevent the destruction or deterioration of the electrolyte membrane due to localized pressure. On the other hand, by making the thickness of the conductive porous substrate preferably 5.0 mm or less, more preferably 3.0 mm or less, the increase in electrical resistance of the porous transport layer due to excessive thickness can be suppressed. In this invention, the thickness of the conductive porous substrate is the value measured using a micrometer or the like while applying a load of 0.15 MPa. When measuring the thickness of a conductive porous substrate in a porous transport layer, the porous transport layer can be heated in air at 500°C for one hour, then scraped off to remove the microporous layer, and only the conductive porous substrate can be extracted to measure its thickness.

[0018] <Microporous Layer> The porous transport layer of the present invention has a microporous layer on at least one side of the conductive porous substrate. By providing a microporous layer, the surface of the conductive porous substrate can be covered with a smoother surface, which improves the adhesion between the catalyst layer and the porous transport layer and enhances conductivity. In addition, it has the effect of preventing damage to the electrolyte membrane due to fraying of the conductive porous substrate when fastened under high pressure in a water electrolysis cell.

[0019] The microporous layer of the present invention has voids with an average diameter of 3 μm to 70 μm. Here, voids in the microporous layer refer to spaces observed in a cross-section obtained by cutting the microporous layer parallel to the thickness direction, where components constituting the microporous layer (hereinafter simply referred to as microporous layer components) are absent. Since the microporous layer is inherently a layer with numerous fine voids, in this specification, when referring to "voids," voids with a diameter of 1 μm or more are excluded, and voids with a diameter of less than 1 μm that are inherently present in the microporous layer are excluded. The presence of voids in the microporous layer increases the gas permeability of the microporous layer, allowing for efficient discharge of gas generated by water electrolysis, thereby improving water electrolysis performance. Furthermore, the presence of voids makes it less likely for the gas discharge path to be blocked by water, as described later, thus enabling high water electrolysis performance. Specifically, by setting the average diameter of the voids to 3 μm or more, preferably 9 μm or more, it becomes possible to suppress blockage of the gas discharge path while increasing gas permeability, and by setting the average diameter of the voids to 70 μm or less, preferably 55 μm or less, it becomes possible to increase the conductivity and strength of the microporous layer. In this specification, the average diameter of the voids refers to the average value of the diameters of multiple voids observed in a cross-section obtained by cutting the microporous layer parallel to the thickness direction, i.e., in a two-dimensional plane.

[0020] In this invention, one method for measuring the diameter of a void is to calculate the equivalent circular diameter of the void present in a cross-section from a two-dimensional image of a cross-section obtained by cutting the microporous layer parallel to the thickness direction. From the equivalent circular diameter obtained here, the average diameter of the void can be statistically derived. As an example, a cross-section obtained by cutting the microporous layer parallel to the thickness direction using an ion milling apparatus, etc., is obtained using a scanning electron microscope at a magnification that allows observation of the void, for example, 1,000 times. Next, the area of ​​each void present in the microporous layer in the image is measured using the image analysis software "ImageJ", and the equivalent circular diameter of the void is calculated from the following formula (1), and this is taken as the diameter of the void. The average value of the calculated diameters of each void is then taken as the average diameter of the void. For voids with an open top, such as through holes described later, the line connecting the uppermost positions where the left and right sides of the void begin to be surrounded by the microporous layer component is set as the boundary line. The area of ​​the region defined by closing the opening with this boundary line is defined as the area of ​​the void, and the diameter of the circle calculated from equation (1) is defined as the diameter of the void. Note that the diameter of the void observed in the cross-section is measured as a value slightly smaller than the diameter of the void observed in three dimensions. For example, if the diameter of the void in the cross-section is 3 μm or more and 70 μm or less, it corresponds to a diameter of the void observed in three dimensions of approximately 5 μm or more and 90 μm or less. However, in this invention, the diameter of the void refers only to the value obtained from the two-dimensional image of the cross-section.

[0021]

[0022] Furthermore, it is preferable that there are no through-holes in the microporous layer that penetrate from the surface of the microporous layer to the conductive porous substrate. In other words, it is preferable that there are no through-holes in the microporous layer that penetrate from the surface of the microporous layer to the conductive porous substrate, and that only voids other than through-holes exist. This allows the microporous layer to sufficiently cover the conductive porous substrate, and enhances the effect of preventing damage to the electrolyte membrane due to fuzzing of the conductive porous substrate. Note that through-holes are a concept included in voids, and among them, those that penetrate from the surface of the microporous layer to the conductive porous substrate. A method for checking the presence or absence of through-holes will be explained. An image is obtained using a scanning electron microscope at a magnification that allows observation of voids, for example, 1,000 times, of a cross-section of the microporous layer cut parallel to the thickness direction using an ion milling device or the like. Next, the parts of the image that do not contain microporous layer components are checked. Using the image analysis software "ImageJ", voids present in the microporous layer in the image are identified and the presence or absence of voids corresponding to through-holes is checked. Here, voids and through-holes are explained in Figure 1. Figure 1 is a schematic cross-sectional view showing an example of a porous transport layer. The porous transport layer 10 has a microporous layer 2 on one side of a conductive porous substrate 1, and further has voids in the microporous layer 2 where there are no microporous layer components. Of these voids, those shown as voids 3 and 4 in Figure 1 are voids other than through holes that do not penetrate to the conductive porous substrate. On the other hand, those shown as through holes 5 and 6 in Figure 1 are voids that penetrate from the surface of the microporous layer to the conductive porous substrate. Furthermore, in this invention, "there are no through holes in the microporous layer that penetrate from the surface of the microporous layer to the conductive porous substrate" means that when the above-mentioned cross-section of the microporous layer is cut parallel to the thickness direction at a total of 10 locations in the porous transport layer, arranged in 2 rows x 5 columns evenly spaced apart from each other as shown in Figure 3, no through holes are observed at any of the observation locations. Figure 3 is a top view of the porous transport layer 10 as seen from the microporous layer 2 side. By creating cross-sections cut parallel to the thickness direction along lines A-A' and B-B', and checking for the presence or absence of through-holes at 10 observation points 26, it is possible to determine whether or not through-holes exist in the porous transport layer.

[0023] Furthermore, it is preferable from the viewpoint of gas permeability that voids with an average diameter of 3 μm to 70 μm exist on the surface of the microporous layer. Here, it is preferable that the area ratio occupied by voids with a diameter of 3 μm to 70 μm on the surface of the microporous layer is 0.1% to 50%. By setting the above area ratio to preferably 0.1% or more, and more preferably 0.5% or more, the gas permeability of the microporous layer is further increased. On the other hand, by setting the above area ratio to preferably 50% or less, and more preferably 20% or less, the contact surface between the microporous layer and the catalyst layer is increased, making the water electrolysis reaction more likely to occur. Here, voids present on the surface of the microporous layer refer to the parts of the surface where no microporous layer components are present when viewed from the surface of the microporous layer. Also, the diameter of the void refers to the equivalent circular diameter of the void. As mentioned above, it is preferable that these voids present on the surface are voids that do not penetrate the microporous layer in the thickness direction, that is, they are not through holes, but the above area ratio is calculated without excluding (including) through holes. This document describes a method for measuring the area ratio of voids with a diameter of 3 μm to 70 μm on the surface of a microporous layer. For the surface of the microporous layer of a porous transport layer, a scanning electron microscope is used to acquire an image magnified to a level sufficient to observe the voids, for example, 1,000 times (field of view size of 100 μm or more). Using the image analysis software "ImageJ," the area of ​​voids with a diameter of 3 μm to 70 μm in the image is measured, and the ratio of the area of ​​these voids to the surface area of ​​the microporous layer is calculated as the area ratio of voids with a diameter of 3 μm to 70 μm on the surface of the microporous layer. The area ratio is measured for 10 images in a 2x5 grid, evenly spaced arrangement, and the arithmetic mean is taken as the area ratio of voids with a diameter of 3 μm to 70 μm on the surface of the microporous layer of the porous transport layer. An example of 10 images in a 2x5 grid, evenly spaced arrangement, is shown in Figure 2. Figure 2 is a top view of the porous transport layer 10 as seen from the microporous layer 2 side, and is an example of 10 observation points 16 in a 2x5 grid, evenly spaced apart from each other.

[0024] The area ratio occupied by voids with a diameter of 3 μm to 70 μm in the cross-section of the microporous layer is preferably 0.1% to 50%. By setting the above area ratio to preferably 0.1% or more, and more preferably 0.5% or more, the gas permeability of the microporous layer is further increased. On the other hand, by setting the above area ratio to preferably 50% or less, and more preferably 20% or less, the strength of the microporous layer is maintained, puncture of the electrolyte membrane due to fuzzing of the conductive porous substrate is suppressed, and short circuits can be further prevented. As mentioned above, it is preferable that the voids present in these cross-sections are voids that do not penetrate the microporous layer in the thickness direction, i.e., they are not through holes, but the above area ratio is calculated without excluding (including) through holes. A method for measuring the area ratio occupied by voids with a diameter of 3 μm to 70 μm in the cross-section of the microporous layer will be described. An image is obtained using a scanning electron microscope at a magnification that allows observation of voids, for example, 1,000 times, of the cross-section obtained by cutting the microporous layer of the porous transport layer parallel to the thickness direction using an ion milling apparatus or the like. For the image in question, the area of ​​voids with a diameter of 3 μm or more and 70 μm or less in the image is measured using the image analysis software "ImageJ". The ratio of the area of ​​these voids to the total area of ​​the cross-section of the microporous layer is calculated and defined as the area ratio occupied by voids with a diameter of 3 μm or more and 70 μm or less in the cross-section of the microporous layer. The above area ratio is measured for a total of 10 images in 2 rows x 5 columns that are evenly spaced apart, and the arithmetic mean is defined as the area ratio occupied by voids with a diameter of 3 μm or more and 70 μm or less in the cross-section of the microporous layer of the porous transport layer. An example of a total of 10 locations in 2 rows x 5 columns that are evenly spaced apart is shown in Figure 3. Figure 3 is a top view of the porous transport layer 10 as seen from the microporous layer 2 side. The cross-sections cut parallel to the thickness direction along the A-A' line or B-B' line at the 10 observation points 26 are examples of a total of 10 locations in 2 rows x 5 columns that are evenly spaced apart.

[0025] As a method for forming voids in a microporous layer, for example, a microporous layer composition containing a pore-forming agent can be prepared, the microporous layer composition can be coated onto a conductive porous substrate, and then sintered to burn off the pore-forming agent. The material of the pore-forming agent is not particularly limited as long as it burns off or shrinks under the sintering conditions of the porous transport layer to form voids in the microporous layer. Examples include acrylic resins, styrene resins, starch, polylactic acid resins, sublimable low molecular weight materials, and microballoons. Here, sublimable low molecular weight materials are usually low molecular weight organic powders with a molecular weight of 1,000 or less that sublimate and burn off at the sintering temperature. Examples of sublimable low molecular weight materials include anthracene, pentacene, and phenanthrene. Furthermore, microballoons are hollow particles that expand significantly when heated, forming voids around them, and eventually the resin portion decomposes or shrinks due to thermal decomposition, leaving only the voids. Examples include "Matsumoto Sphere®" (manufactured by Matsumoto Oil & Fat Pharmaceutical Co., Ltd.) and "Expancel®" (manufactured by Nippon Philite Co., Ltd.).

[0026] When using a pore-forming agent, it is preferable to use a material whose carbonization yield after burning off by thermal decomposition, melting and volatilization, sublimation, etc., at 350°C, which is a common sintering condition for porous transport layers, is 20% or less. By setting the carbonization yield of the pore-forming agent to 20% or less at 350°C, it becomes easier to form voids within the microporous layer. Examples of such pore-forming agents include polymethyl methacrylate (PMMA). The carbonization yield at 350°C can be measured using a TGA apparatus such as the EXTRATGA6200 manufactured by SII. Specifically, using this apparatus, the temperature is raised from 50°C to 350°C at a heating rate of 2°C / min in air, held at 350°C for 10 minutes, and the carbonization yield at 350°C is obtained by dividing the mass after holding by the original mass and multiplying by 100.

[0027] In a composition for a microporous layer, the amount of pore-forming agent is preferably 10 parts by mass or more and 500 parts by mass or less, when the amount of solids excluding the pore-forming agent is 100 parts by mass. By preferably adding 10 parts by mass or more, and more preferably 30 parts by mass or more, a sufficient amount of voids can be obtained. On the other hand, by preferably adding 500 parts by mass or less, and more preferably 350 parts by mass or less, the strength of the microporous layer can be maintained. Furthermore, if the composition for a microporous layer contains conductive particles, the amount of pore-forming agent in the composition for a microporous layer is preferably 10 parts by mass or more and 500 parts by mass or less, and more preferably 30 parts by mass or more and 350 parts by mass or less, when the amount of conductive particles is 100 parts by mass.

[0028] The microporous layer preferably contains conductive particles to improve conductivity. By including conductive particles, the conductivity of the porous transport layer can be improved, and an improvement in water electrolysis performance can be expected. From the viewpoint of cost, the conductive particles preferably contain carbon material, but other conductive particles may be included as needed. Examples of conductive particles made of carbon material include carbon black, graphite particles, carbon nanotubes, carbon nanofibers, chopped carbon fibers, and graphene, but carbon black is particularly preferred because it contains fewer impurities. Examples of other conductive particles include those made of metal, such as metal powder, foamed metal, and foamed metal alloy. Examples of constituent metals include titanium, nickel, aluminum, stainless steel, and alloys mainly composed of at least one of these metals, but titanium and titanium alloys are particularly preferred.

[0029] The primary particle diameter of the conductive particles is preferably 100 nm or less. By setting the primary particle diameter of the conductive particles to preferably 100 nm or less, more preferably 60 nm or less, and even more preferably 40 nm or less, the surface of the microporous layer becomes dense, the surface quality of the microporous layer can be enhanced, and piercing of the electrolyte membrane by the conductive porous base material can be suppressed. In addition, the primary particle diameter of the conductive particles is preferably 20 nm or more. By setting the primary particle diameter of the conductive particles to 20 nm or more, the conductivity of the microporous layer can be improved. In addition, the viscosity of the composition for a microporous layer when forming the microporous layer tends to decrease, so that the composition for a microporous layer easily penetrates into the conductive porous base material, and the conductivity of the porous transport layer can also be enhanced, thereby improving the electrolytic performance of the water electrolysis cell.

[0030] Here, the primary particle diameter of the conductive particles can be obtained by preparing a cross-section observation sample using an ion milling apparatus, magnifying it at a high magnification (for example, 200,000 times or more) with a microscope such as a scanning electron microscope to take a photograph, measuring the diameters of 10 randomly selected primary particles, and averaging the measured values. As the ion milling apparatus, for example, IM4000 (manufactured by Hitachi High-Technologies Corporation) can be used.

[0031] The microporous layer of the porous transport layer of the present invention has a contact angle with water of 70° to 180°. By setting the contact angle with water to 70° or more, preferably 90° or more, more preferably 120° or more, even more preferably 130° or more, and even more preferably 140° or more, the water electrolysis performance of the water electrolysis cell can be improved. In the present invention, the reason why the water electrolysis performance of the water electrolysis cell is improved by having the contact angle between the microporous layer and water within the above range is presumed to be as follows: In a water electrolysis cell, during the water electrolysis reaction, protons move from the anode side to the cathode side through the electrolyte membrane, and at that time, water also moves along with the protons. Therefore, there is a possibility that the hydrogen gas discharge path in the porous transport layer on the cathode side may be blocked by water that has moved along with the protons. If the hydrogen gas discharge path in the porous transport layer is blocked by water, it can cause problems such as inhibition of the water electrolysis reaction and cross-leakage of hydrogen gas. To suppress blockage by water, it is important that the porous transport layer has high drainage capacity. As described above, the microporous layer of the porous transport layer of the present invention has high water repellency with a contact angle with water of 70° to 180°, thus providing excellent drainage. Therefore, it is presumed that the water electrolysis performance of a water electrolysis cell can be improved by using the porous transport layer of the present invention. However, the present invention is not limited in any way by the above presumption.

[0032] The microporous layer of the porous transport layer of the present invention preferably contains a water-repellent resin. Thereby, the water repellency of the microporous layer is improved, and the drainage performance of the porous transport layer can be enhanced based on the presumed mechanism described above. From the viewpoints of chemical stability, water repellency and the like, a fluororesin having a fluoroalkyl chain or the like is preferred as the water-repellent resin. Examples of the fluororesin include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), ETFE (tetrafluoroethylene-ethylene copolymer), PVDF (polyvinylidene fluoride), and PVF (polyvinyl fluoride), among which PTFE or FEP that exhibits high water repellency is preferred. The content of the water-repellent resin in the microporous layer is not particularly limited, but is preferably 0.5 mass% or more and 40.0 mass% or less. Setting the content of the water-repellent resin in the microporous layer to 0.5 mass% or more can enhance water repellency, and setting it to 40.0 mass% or less can suppress electrical resistance. The content of the water-repellent resin in the microporous layer can be measured, for example, by thermally decomposing microporous layer powder scraped from the surface of the porous transport layer using pyrolysis GC / MS.

[0033] In general, since fluororesins are insoluble in water, organic solvents and the like, it is preferable to use a dispersion liquid of the water-repellent resin processed into fine particles when producing the composition for a microporous layer. Examples of the dispersion liquid of particulate water-repellent resin include "Polyflon (registered trademark)" D-210C, "Neoflon (registered trademark)" ND-110 (all manufactured by Daikin Industries, Ltd.), 120-JRB, and 31-JR (all manufactured by Mitsui Chemours Fluoroproducts Co., Ltd.).

[0034] The thickness of the microporous layer is preferably 10 μm or more and 80 μm or less. By making the thickness of the microporous layer preferably 10 μm or more, more preferably 15 μm or more, the conductive porous substrate can be sufficiently covered, and the fuzzing of the conductive porous substrate can be suppressed, thereby preventing damage to the electrolyte membrane and improving durability. On the other hand, by making the thickness of the microporous layer preferably 80 μm or less, more preferably 70 μm or less, and even more preferably 60 μm or less, gas permeability in the direction perpendicular to the surface can be increased, and water electrolysis performance can be improved. In this invention, the thickness of the microporous layer refers to the value obtained by subtracting the thickness of the conductive porous substrate from the thickness of the porous transport layer, and the thickness of the parts in which the microporous layer has permeated the conductive porous substrate is not added to the thickness of the microporous layer. In this invention, the thickness of the microporous layer can be calculated by measuring the thickness of the conductive porous substrate when the conductive porous substrate is placed on a smooth surface plate and a pressure of 0.15 MPa is applied, then similarly measuring the thickness of the porous transport layer on which the microporous layer is formed, and subtracting the thickness of the conductive porous substrate from the thickness of the porous transport layer. When measuring the thickness of the microporous layer from the state of the porous transport layer, the thickness of the conductive porous substrate is measured after heating it in air at 500°C for 1 hour and then removing (scraping off) the microporous layer. The thickness is then calculated as the difference between this measurement and the thickness of the porous transport layer before the microporous layer was removed.

[0035] The porous transport layer of the present invention can be manufactured by forming a microporous layer on at least one surface of a conductive porous substrate by coating, drying, sintering, etc., a microporous layer composition containing the aforementioned pore-forming agent and conductive particles.

[0036] The composition for the microporous layer may contain a dispersion medium such as water or an organic solvent, but water is preferred as the dispersion medium. The composition for the microporous layer may also contain, as a dispersant such as a surfactant, polyalkylene glycol, carboxyl vinyl polymer, polyester, polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, polyacrylic acid, polyacrylate, polystyrene sulfonate, polyalkylene polyamine, polyvinylimidazoline, cellulose derivative, alginate, guar gum, xanthan gum, carrageenan, pectin, gelatin, starch, etc., either individually or in a mixture of two or more.

[0037] The coating of microporous layer compositions onto conductive porous substrates can be performed using various commercially available coating devices. Coating methods such as screen printing, rotary screen printing, spray aeration, intaglio printing, gravure printing, die coating, bar coating, and blade coating can be used.

[0038] It is preferable to coat a conductive porous substrate with a microporous layer composition to form a microporous layer precursor (coating film before drying), then place it in a dryer set to a temperature of 80 to 180°C and dry it for 2 to 30 minutes. After further drying, it is preferable to place it in a muffle furnace, firing furnace, or high-temperature dryer and sinter it at a temperature of, for example, 300 to 400°C for 1 to 60 minutes to melt the water-repellent resin and form a microporous layer by using it as a binder between conductive particles. In this sintering, it is preferable that the porosizing agent is burned away by thermal decomposition, melting and volatilization, or sublimation, thereby forming voids.

[0039] When the porous transport layer of the present invention is used in a water electrolysis apparatus, it is preferable that the microporous layer is insoluble in water, which is the target of electrolysis. By employing a microporous layer that is insoluble in water, it is possible to suppress the delamination of the microporous layer starting from the dissolved portion, which reduces adhesion to the electrolyte membrane and thus reduces the electrolysis performance.

[0040] <Porous Transport Layer> The porous transport layer of the present invention is preferably used as the porous transport layer on the cathode side in a water electrolysis cell. The cathode has a lower potential compared to the anode and does not require high oxidation resistance, so there is an advantage that the porous transport layer of the present invention has a low possibility of corrosion when used as the porous transport layer on the cathode side.

[0041] In the porous transport layer of the present invention, it is preferable that the ratio b / a (hereinafter sometimes abbreviated as "pore volume ratio b / a") obtained by dividing the pore volume a in the range of pore diameters from 10 nm to 1 μm by the pore volume b in the range of pore diameters from 3 μm to 100 μm is between 4 and 180. Here, pore volume refers to the pore volume per unit area of ​​the porous transport layer. As described above, in order to obtain good water electrolysis performance, it is important to suppress clogging of the porous transport layer by water accompanying the water electrolysis reaction. When a water electrolysis cell is operated continuously, water continuously moves to the porous transport layer on the cathode side during operation, so there is a risk that the water electrolysis performance will deteriorate due to clogging by water. By setting the pore volume ratio b / a to preferably 4 or higher, and more preferably 20 or higher, that is, by reducing the number of pores with a diameter of 10 nm to 1 μm, which are likely to be clogged by water, and increasing the number of pores with a diameter of 3 μm to 100 μm, which are less likely to be clogged by water, the deterioration of water electrolysis performance due to clogged water can be suppressed. On the other hand, by setting the pore volume ratio b / a to preferably 180 or lower, and more preferably 120 or lower, the strength of the porous transport layer can be maintained, and the deterioration of water electrolysis performance due to damage to the conductive paths in the porous transport layer caused by compression when assembling the water electrolysis cell or pressure caused by the discharge of hydrogen gas and water when the water electrolysis cell is operated continuously can be suppressed. The pore diameter and pore volume of the porous transport layer can be calculated by measuring the pore diameter distribution using a mercury intrusion porosimeter.

[0042] In the porous transport layer of the present invention, it is preferable that the contact angle between the conductive porous substrate and air in water is greater than the contact angle between the microporous layer and air in water, that is, that the wettability of the conductive porous substrate in water is greater than that of the microporous layer. The contact angle with air in water is the contact angle between a solid and a bubble in water, measured by the so-called underwater bubble method. By making the contact angle between the conductive porous substrate and air in water greater than the contact angle between the microporous layer and air in water, water moving to the cathode side during the electrolytic reaction can be smoothly discharged from the microporous layer to the conductive porous substrate, thereby suppressing blockage by water in the porous transport layer and improving the water electrolysis performance of the water electrolysis cell. In particular, since a large amount of water moves to the cathode side in water electrolysis, it is important to control the wettability of the microporous layer and the conductive porous substrate in water in order to suppress blockage by water in the porous transport layer. Therefore, it is considered that a favorable effect can be obtained by making the wettability in water, that is, the contact angle with air in water, as described above. Furthermore, maintaining the above-described relationship between the contact angle with air in water is also effective in suppressing the deterioration of water electrolysis performance during continuous operation of the water electrolysis cell. This is thought to be because water moving to the cathode side during the electrolysis reaction can be smoothly discharged from the microporous layer to the conductive porous substrate. Therefore, it is particularly preferable that the contact angle between the conductive porous substrate and air in water is 100° or more, and even more preferably 110° or more, than the contact angle between the microporous layer and air in water.

[0043] In the porous transport layer of the present invention, it is preferable that the conductive porous substrate does not allow water containing 20% ​​by mass of ethanol to permeate, but allows water containing 40% by mass of ethanol to permeate, while the microporous layer does not allow water containing 40% by mass of ethanol to permeate. Here, "permeation" refers to the seeping of the aforementioned water containing 20% ​​by mass or 40% by mass of ethanol (hereinafter abbreviated as "solvent") into the porous transport layer. Specifically, it refers to the contact angle becoming 10° or less within 1 second after dropping 5 μL of the solvent onto the surface of the conductive porous substrate or the microporous layer. The above relationship in the permeability of each solvent in the conductive porous substrate and microporous layer of the porous transport layer of the present invention makes it possible to suppress deterioration of water electrolysis performance when the water electrolysis cell is operated continuously. As described above, in order to obtain good water electrolysis performance, it is important to suppress clogging of the porous transport layer by water accompanying the water electrolysis reaction. When the water electrolysis cell is operated continuously, water continuously moves to the porous transport layer on the cathode side during operation, so there is a risk that water clogging will occur and the water electrolysis performance will deteriorate. In a porous transport layer, water is discharged from the microporous layer toward the conductive porous substrate. Therefore, if the water permeability to the conductive porous substrate is higher than that of the microporous layer, water is more easily discharged from the microporous layer toward the conductive porous substrate, thus suppressing deterioration of water electrolysis performance. On the other hand, if the water permeability to the conductive porous substrate is too high, water becomes difficult to discharge from the conductive porous substrate, which can cause blockage in the porous transport layer and deteriorate water electrolysis performance. For this reason, it is preferable that the permeability of each solvent to the conductive porous substrate and the microporous layer be in the relationship described above.

[0044] The porous transport layer of the present invention exhibits a mass reduction of 5 g / m² when heat-treated at 400°C for 1 hour under atmospheric conditions. 2is preferably not more than the above value. As described above, examples of the method for forming voids in the microporous layer or the method for forming voids on the surface of the microporous layer include a method of burning out a pore-forming agent, but when residues derived from the pore-forming agent or the like are present in the porous transport layer, the component may degrade the catalyst in the catalyst layer of the membrane electrode assembly described later during continuous operation of the water electrolysis cell, leading to deterioration of water electrolysis performance. Therefore, it is preferable that the residue of the relevant component is as small as possible. Specifically, the mass reduction of the porous transport layer when the porous transport layer is heat-treated at 400°C for 1 hour in the atmosphere is preferably 5 g / m 2 or less, more preferably 3 g / m 2 or less, still more preferably 1 g / m 2 or less.

[0045] The porous transport layer of the present invention preferably has a mass reduction of 1 g / m 2 or less when subjected to immersion treatment in hot water at 85°C for 5 hours. When a component that dissolves in hot water is present in the porous transport layer, this component may degrade the catalyst in the catalyst layer constituting the membrane electrode assembly described later, leading to deterioration of water electrolysis performance. Therefore, it is preferable that the residue of the relevant component is as small as possible. Specifically, the mass reduction of the porous transport layer when the porous transport layer is subjected to immersion treatment in hot water at 85°C for 5 hours is preferably 1 g / m 2 or less, more preferably 0.5 g / m 2 or less, still more preferably 0.1 g / m 2 or less. The mass reduction of the porous transport layer when the porous transport layer is immersed in hot water at 85°C for 5 hours can be calculated by subtracting the mass of the porous transport layer that has been dried to remove water after immersion from the mass of the porous transport layer before immersion.

[0046] <Membrane Electrode Assembly> A membrane electrode assembly is one aspect of the present invention and refers to one that uses the porous transport layer of the present invention. Specifically, a membrane electrode assembly of the present invention can be formed by bonding the porous transport layer of the present invention to at least one side of an electrolyte membrane having catalyst layers on both sides. Arranging the porous transport layer so that the microporous layer side is in contact with the catalyst layer is preferable because it increases the contact area between the catalyst layer and the porous transport layer, reduces contact electrical resistance, and prevents damage to the electrolyte membrane. As the electrolyte membrane, one with high proton conductivity and oxidation resistance and low gas crossover is preferred. As the electrolyte membrane, one made of fluorine-based polymers or hydrocarbon-based polymers is known, and either of these can be used.

[0047] In the film electrode assembly of the present invention, it is preferable that the cathode catalyst layer and the anode catalyst layer are composed of different materials. For example, it is preferable to use platinum or a platinum-cobalt alloy as catalyst particles in the cathode catalyst layer. For example, it is preferable to use a noble metal such as iridium, ruthenium, rhodium, palladium, or osmium, or an alloy or oxide thereof, in the anode catalyst layer.

[0048] <Water Electrolysis Device> A water electrolysis device is one aspect of the present invention and refers to one that uses the porous transport layer of the present invention. Specifically, a water electrolysis device of the present invention can be formed by constructing and using a water electrolysis cell having separators on both sides of the membrane electrode assembly of the present invention.

[0049] <Fuel Cells> Fuel cells are one aspect of the present invention and refer to those using the porous transport layer of the present invention. Specifically, a fuel cell of the present invention can be formed by arranging separators on both sides of the membrane electrode assembly of the present invention. The fuel cell of the present invention includes not only the single cells described above, but also stacks of these single cells.

[0050] The present invention will be described below with reference to examples and comparative examples.

[0051] [Measurement Method] (1) Measurement of the thickness of the microporous layer The conductive porous substrate was placed on a smooth surface plate, and under pressure of 0.15 MPa, the thickness of 10 different locations on the conductive porous substrate was measured, and the average value was taken as the thickness of the conductive porous substrate. Next, the thickness of the porous transport layer in which the microporous layer was formed was measured and calculated in the same way as the conductive porous substrate. Then, the thickness of the microporous layer [μm] was calculated by subtracting the thickness of the conductive porous substrate from the thickness of the porous transport layer.

[0052] (2) Measurement of the diameter of voids in the microporous layer From the porous transport layer cut to 300 mm x 300 mm, as shown in Figure 3, 10 sections were cut out in 2 rows x 5 columns, with each section measuring 10 mm x 10 mm and spaced 10 mm apart from the others. Ten cross-sectional observation samples were prepared by cutting the porous transport layer parallel to the thickness direction using an ion milling device IM4000 (manufactured by Hitachi High-Tech Corporation). Next, using a scanning electron microscope VHX-D510 (manufactured by Keyence Corporation), one image of the cross-section of the microporous layer was acquired for each cross-sectional observation sample, magnified 1,000 times. Next, the area of ​​the voids present in the microporous layer in the image of each cross-sectional observation sample was measured using the image analysis software "ImageJ", and the equivalent circular diameter of each void was calculated based on the following formula. The same procedure was performed for all 10 cross-sectional observation samples.

[0053]

[0054] Next, we checked whether any of the measured samples contained voids with a diameter of 3 μm to 70 μm or voids with a diameter of 9 μm to 55 μm. Furthermore, from the voids for which the diameter was calculated, we extracted only those with a diameter of 1 μm or more and calculated the arithmetic mean, which was defined as the average diameter of the voids [μm].

[0055] (3) Measurement of the maximum dimension in the thickness direction of voids in the microporous layer (and confirmation of the presence or absence of through holes) For the samples prepared in (2) above, the dimensions of the voids in the microporous layer in the image in the thickness direction of the microporous layer were measured, and the presence or absence of through holes was observed. The same procedure was performed for all 10 samples for cross-sectional observation, and the maximum value among all measurements was taken as the maximum dimension [μm] in the thickness direction of voids in the microporous layer, and the presence or absence of through holes was also recorded.

[0056] (4) Measurement of the contact angle between the microporous layer and water. 5 μL of deionized water droplets were dropped onto 10 randomly selected points on the microporous layer in an environment of 20°C and 60% humidity. An automatic contact angle meter DM-501 (manufactured by Kyowa Interface Science Co., Ltd.) was used to measure the contact angle [°] at each point 1.0 second after dropping. The average of the 10 measured values ​​was taken as the contact angle between the microporous layer and water.

[0057] (5) Measurement of the area ratio occupied by voids with a diameter of 3 μm to 70 μm on the surface of the microporous layer From the porous transport layer cut out to 300 mm × 300 mm, as shown in Figure 2, a total of 10 locations were cut out in 2 rows × 5 columns with a measurement area size of 10 mm × 10 mm and spaced 10 mm apart from each other, to be used as measurement samples. Next, using a scanning electron microscope VHX-D510 (manufactured by Keyence Corporation), one image of the microporous layer side surface of each measurement sample was acquired, magnified 1,000 times. Next, the area of ​​voids present in the image of each measurement sample was measured using the image analysis software "ImageJ", and after extracting voids with a diameter of 3 μm to 70 μm based on the method described in (2) above, the ratio of the area occupied by voids with a diameter of 3 μm to 70 μm to the surface area of ​​the microporous layer in each sample was individually calculated. The area percentage [%] of voids with a diameter of 3 μm to 70 μm on the surface of the microporous layer was calculated by expressing the arithmetic mean ratio of the area of ​​voids with a diameter of 3 μm to 70 μm to the surface area of ​​the microporous layer obtained from a total of 10 measurement samples.

[0058] (6) Measurement of the area ratio occupied by voids with a diameter of 3 μm to 70 μm in the cross-section of the microporous layer In the same manner as in (2) above, images of the cross-sections of 10 cross-sectional observation samples magnified 1,000 times were obtained. Next, the area of ​​voids present in the image of each cross-sectional observation sample was measured using the image analysis software "ImageJ", and after extracting voids with a diameter of 3 μm to 70 μm based on the method described in (2) above, the ratio of the area occupied by voids with a diameter of 3 μm to 70 μm to the cross-sectional area of ​​the microporous layer in each sample was calculated individually. The arithmetic mean of the ratio of the area occupied by voids with a diameter of 3 μm to 70 μm to the cross-sectional area of ​​the microporous layer obtained for a total of 10 measurement samples was expressed as a percentage to obtain the area ratio [%] occupied by voids with a diameter of 3 μm to 70 μm in the cross-section of the microporous layer.

[0059] (7) Measurement of air permeability resistance was performed using a Gahl-type densometer (Toyo Seiki Seisakusho Co., Ltd. G-B3C). A porous transport layer cut to a size of 50 mm x 50 mm was set in the measuring instrument, and the permeation time at an air permeation rate of 300 mL was measured. Ten samples were measured in the same manner, and the average value of the permeation time was taken as the air permeability resistance [seconds]. The smaller the air permeability resistance, the better the porous transport layer is in terms of gas diffusion.

[0060] (8) Measurement of short circuit rate Ten samples were prepared by cutting the porous transport layer to a size of 40 mm x 40 mm. A high-density polyethylene film (50 mm x 50 mm, thickness 20 μm) was placed on the microporous layer side of the porous transport layer of these samples so that the centers of the porous transport layer and the high-density polyethylene film coincided, and rigid electrodes of smooth, gold-plated metal (each with an area of ​​9 cm²) were placed on the top and bottom. 2 These were sandwiched between two electrodes, and an average pressure of 4.0 MPa was applied. In this state, when a current of 2.0 V was passed through the upper and lower electrodes, the current between the upper and lower electrodes was measured. The same measurement was performed on 10 samples, and samples with a current of 1 mA or more were considered short-circuited. The fewer the short-circuited samples, the better the porous transport layer is considered to be at preventing punctures. The number of short-circuited samples was judged as follows, with A to D being considered good. A: 1 or less. B: 2. C: 3. D: 4 to 7. E: 8 or more.

[0061] (9) Electrolyte membrane with catalyst layer for measuring cell voltage (electrolyte membrane is "Nafion®" (registered trademark)) 117, iridium catalyst as catalyst for anode catalyst layer (iridium content 2.25 mg / cm³) 2 ), platinum catalyst as catalyst for the cathode catalyst layer (platinum amount 1 mg / cm³) 2 A membrane electrode assembly was fabricated by laminating a commercially available porous titanium sintered plate as the anode-side porous transport layer on the anode catalyst layer side and the porous transport layer under evaluation as the cathode-side porous transport layer on the cathode catalyst layer side. The membrane electrode assembly was laminated so that the microporous layer side of the porous transport layer was in contact with the cathode catalyst layer.

[0062] The membrane electrode assembly prepared above is placed in a Fuel Cell Store water electrolysis cell "Electrolyzer Hardware-Square" (electrode area 50 cm²). 2 The device was set up and the cell was fastened so that the average pressure on the membrane electrode assembly was 4 MPa. Deionized water with an electrical conductivity of 1 μS / cm or less was supplied to both the cathode electrode and the anode electrode, which were set to a cell temperature of 60°C, at a flow rate of 0.2 L / min at atmospheric pressure, and 2 A / cm² was applied. 2 A constant current of 2 A / cm was used to perform the electrolysis reaction of water, generating hydrogen gas and oxygen gas. 2 In the constant current measurement, the cell voltage [V] after one hour was measured and judged as follows. In the constant current measurement, the lower the cell voltage, the better the water electrolysis characteristics, so A to D were considered to be good cell voltages. A: Less than 2.2V. B: 2.2V or more and less than 2.3V. C: 2.3V or more and less than 2.4V. D: 2.4V or more and less than 2.5V. E: 2.5V or more and less than 2.6V. F: 2.6V or more.

[0063] Also, 2 A / cm 2In the constant current measurement, the cell voltage [V] after 100 hours was measured, and the difference between the cell voltage after 1 hour and the cell voltage after 100 hours was measured and judged as follows. In constant current measurement, the smaller the change in cell voltage, the better the water electrolysis characteristics, so A to D were considered to be good cell voltage changes. A: Less than 40mV. B: 40mV or more and less than 60mV. C: 60mV or more and less than 80mV. D: 80mV or more and less than 100mV. E: 100mV or more and less than 150mV. F: 150mV or more.

[0064] (10) Measurement of pore volume ratio b / a Five samples of porous transport layer cut to a size of 20 mm × 30 mm were prepared, and the pore size distribution was obtained by measuring the pore size in the range of measurement pressure from 6 kPa to 123 MPa (pore size from 10 nm to 200 μm) using the mercury intrusion method. The measuring device used was an Autopore 9520 manufactured by Shimadzu Corporation. The pore volume in the range of pore size from 10 nm to 1 μm was determined by subtracting the cumulative pore volume in the range of pore size exceeding 1 μm from the cumulative pore volume in the range of pore size exceeding 1 μm. The pore volume in the range of pore size from 3 μm to 100 μm was determined by subtracting the cumulative pore volume in the range of pore size exceeding 100 μm from the cumulative pore volume in the range of pore size exceeding 100 μm. For each sample, the ratio of the pore volume in the pore diameter range of 3 μm to 100 μm was calculated by dividing the pore volume in the pore diameter range of 10 nm to 1 μm by the pore volume in the pore diameter range of 3 μm to 100 μm. The arithmetic mean of the pore volume ratios for the five samples was then defined as the pore volume ratio b / a (the ratio obtained by dividing the pore volume a in the pore diameter range of 10 nm to 1 μm in the porous transport layer by the pore volume b in the pore diameter range of 3 μm to 100 μm).

[0065] (11) Evaluation of permeability 5 μL of ion-exchanged water containing 40% by mass of ethanol was dropped onto 10 randomly selected points each on a conductive porous substrate and a microporous layer in an environment of 20°C and 60% humidity. An automatic contact angle meter DM-501 (manufactured by Kyowa Interface Science Co., Ltd.) was used to measure the contact angle [°] at each point 1.0 second after dropping. If the average of the measurements from each of the 10 points was 10° or less, it was determined that the conductive porous substrate or microporous layer had permeated the ion-exchanged water. Furthermore, 5 μL of ion-exchanged water containing 20% ​​by mass of ethanol was dropped onto 10 different randomly selected points on the conductive porous substrate in an environment of 20°C and 60% humidity, and the permeability was evaluated using the same method and criteria.

[0066] (12) Method for measuring and calculating the mass loss when a porous transport layer is heat-treated at 400°C for 1 hour under air. Five samples of the porous transport layer, each measuring 100 mm x 100 mm, are placed in a muffle furnace. The temperature is raised from room temperature to 400°C under air and held at 400°C for 1 hour. After removing the samples from the muffle furnace, the difference between the mass before heat treatment and the mass after heat treatment is divided by the area of ​​the sample to calculate the mass loss [g / m²]. 2 The following was calculated. The average mass loss of the five samples was then used as the mass loss when the porous transport layer was heat-treated at 400°C for 1 hour under air.

[0067] (13) Method for measuring and calculating the mass loss when a porous transport layer is immersed in 85°C hot water for 5 hours A stainless steel beaker containing deionized water was placed in a water bath containing deionized water, and the temperature of the water bath was adjusted so that the water temperature in the stainless steel beaker reached 85°C. Five samples of the porous transport layer, cut to a size of 100 mm x 100 mm, were immersed in the deionized water in the stainless steel beaker for 5 hours. The samples after immersion were placed in a drying oven and dried at 110°C for 30 minutes. The difference between the mass before treatment and the mass after treatment was divided by the area of ​​the sample to calculate the mass loss [g / m²]. 2 The following was calculated. The average mass loss of the five samples was then used as the mass loss when the porous transport layer was immersed in 85°C hot water for 5 hours.

[0068] (14) Measurement of the contact angle of microporous layers and conductive porous substrates with air in water The contact angle of microporous layers and conductive porous substrates with air in water was measured by the water bubble method. Specifically, in an environment of 20°C and 60% humidity, the sample to be measured (microporous layer or conductive porous substrate) was fixed in a measuring cell with the surface facing downwards and horizontal, and the cell was filled with deionized water. Then, 30 μL of air was introduced from below the sample to form bubbles on the sample surface, and after 3 seconds, the contact angle [°] with air in water was measured using an automatic contact angle meter DM-501 (manufactured by Kyowa Interface Science Co., Ltd.). This measurement was performed at 10 random locations, and the average value of the contact angles at the 10 locations was taken as the contact angle of the microporous layer or conductive porous substrate with air in water.

[0069] [Example 1] A microporous layer composition was prepared using carbon black (primary particle size 24 nm) as conductive particles, carboxymethylcellulose (DN-400H; manufactured by Daicel Mirise Co., Ltd.) as a dispersant, polytetrafluoroethylene (PTFE) ("Polyflon®" D-210C; manufactured by Daikin Industries, Ltd.; containing 60% by mass of PTFE in the dispersion medium (water)) as a water repellent, pore-forming agent A (PMMA particles, average particle size 4 μm), and purified water, while adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 12.0 parts by mass / 76.0 parts by mass. The above microporous layer composition was then used to prepare a 2.0 mm thick carbon paper (conductive porous substrate, basis weight 1,050 g / m²). 2 A porous transport layer having a microporous layer on one side of a conductive porous substrate was obtained by coating the substrate with a slit die coater so that the thickness of the microporous layer after sintering was 50 μm, drying at 120°C, and then sintering at 350°C for 30 minutes under nitrogen. The obtained porous transport layer was evaluated according to the measurement method described above, and the results are shown in Table 1.

[0070] [Example 2] A porous transport layer was obtained in the same manner as in Example 1, except that pore-forming agent B (PMMA particles, average particle size 8 μm) was used instead of pore-forming agent A when preparing the composition for the microporous layer. The results of evaluation according to the measurement method described above are shown in Table 1.

[0071] [Example 3] A porous transport layer was obtained in the same manner as in Example 1, except that pore-forming agent C (PMMA particles, average particle size 15 μm) was used instead of pore-forming agent A when preparing the composition for the microporous layer. The results of evaluation according to the measurement method described above are shown in Table 1.

[0072] [Example 4] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was prepared by adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 3.0 parts by mass / 85.0 parts by mass. The results of evaluation according to the measurement method described above are shown in Table 1.

[0073] [Example 5] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was prepared by adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 6.0 parts by mass / 82.0 parts by mass. The results of evaluation according to the measurement method described above are shown in Table 1.

[0074] [Example 6] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was prepared by adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 15.0 parts by mass / 73.0 parts by mass. The results of evaluation according to the measurement method described above are shown in Table 1.

[0075] [Example 7] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was prepared by adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 18.0 parts by mass / 70.0 parts by mass. The results of evaluation according to the measurement method described above are shown in Table 1.

[0076] [Example 8] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was prepared by adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 0.05 parts by mass / 12.0 parts by mass / 79.55 parts by mass. The results of evaluation according to the measurement method described above are shown in Table 1.

[0077] [Example 9] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was prepared by adjusting the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water to 6.0 parts by mass / 2.4 parts by mass / 0.2 parts by mass / 12.0 parts by mass / 79.4 parts by mass. The results of evaluation according to the measurement method described above are shown in Table 1.

[0078] [Example 10] A porous transport layer was obtained in the same manner as in Example 1, except that pore-forming agent D (PMMA particles, average particle size 27 μm) was used instead of pore-forming agent A when preparing the composition for the microporous layer. The results of evaluation according to the measurement method described above are shown in Table 2.

[0079] [Example 11] A porous transport layer was obtained in the same manner as in Example 1, except that pore-forming agent E (PMMA particles, average particle size 40 μm) was used instead of pore-forming agent A when preparing the composition for the microporous layer. The results of evaluation according to the measurement method described above are shown in Table 2.

[0080] [Example 12] A porous transport layer was obtained in the same manner as in Example 11, except that when coating the microporous layer composition, the thickness of the microporous layer after sintering was 20 μm. The results of evaluation according to the measurement method described above are shown in Table 2. In the sample of this example, holes (through holes) penetrating from the surface of the microporous layer to the conductive porous substrate were observed.

[0081] [Example 13] As a conductive porous substrate, carbon paper with a thickness of 0.20 mm (basis weight 75 g / m²) was used. 2 A porous transport layer was obtained in the same manner as in Example 3, except that the following was used. The results of the evaluation according to the measurement method described above are shown in Table 2.

[0082] [Example 14] A porous transport layer was obtained in the same manner as in Example 1, except that when coating with the microporous layer composition, the thickness of the microporous layer after sintering was 8 μm. The results of evaluation according to the measurement method described above are shown in Table 2.

[0083] [Comparative Example 1] A porous transport layer was obtained in the same manner as in Example 1, except that when preparing the composition for the microporous layer, the mass ratio of conductive particles / dispersant / water repellent / purified water was adjusted to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 88.0 parts by mass, and no pore-forming agent was used. The results of evaluation according to the measurement method described above are shown in Table 2.

[0084] [Comparative Example 2] A porous transport layer was obtained in the same manner as in Example 1, except that pore-forming agent F (PMMA particles, average particle size 100 μm) was used instead of pore-forming agent A when preparing the composition for the microporous layer. The results of evaluation according to the measurement method described above are shown in Table 2. In this comparative example, holes (through-holes) penetrating from the surface of the microporous layer to the conductive porous substrate were observed. In addition, a short circuit occurred in the cell during the measurement of the cell voltage, so the cell voltage could not be evaluated.

[0085] [Comparative Example 3] A porous transport layer was obtained in the same manner as in Example 3, except that when preparing the composition for the microporous layer, the mass ratio of conductive particles / dispersant / pore-forming agent / purified water was adjusted to 6.0 parts by mass / 2.4 parts by mass / 12.0 parts by mass / 79.6 parts by mass, and no water-repellent agent was used. The results of evaluation according to the measurement method described above are shown in Table 2.

[0086] [Example 15] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was applied and dried, and then sintered at 350°C for 3 minutes under nitrogen. The results of evaluation according to the measurement method described above are shown in Table 3.

[0087] [Example 16] A porous transport layer was obtained in the same manner as in Example 3, except that the composition for the microporous layer was applied and dried, and then sintered at 350°C for 1 minute under nitrogen. The results of evaluation according to the measurement method described above are shown in Table 3.

[0088] [Example 17] A porous transport layer was obtained in the same manner as in Example 3, except that when preparing the composition for the microporous layer, the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water was adjusted to 6.0 parts by mass / 7.2 parts by mass / 3.6 parts by mass / 12.0 parts by mass / 71.2 parts by mass, and methylcellulose (methylcellulose 100; manufactured by Wako Pure Chemical Industries, Ltd.) was used as the dispersant. The results of evaluation according to the measurement method described above are shown in Table 3.

[0089] [Example 18] A porous transport layer was obtained in the same manner as in Example 3, except that when preparing the composition for the microporous layer, the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water was adjusted to 6.0 parts by mass / 14.4 parts by mass / 3.6 parts by mass / 12.0 parts by mass / 64.0 parts by mass, and methylcellulose (methylcellulose 50; manufactured by Wako Pure Chemical Industries, Ltd.) was used as the dispersant. The results of evaluation according to the measurement method described above are shown in Table 3.

[0090] [Example 19] Thickness 2.0 mm and basis weight 1,000 g / m 2 A porous transport layer was obtained in the same manner as in Example 7, except that a composition for the microporous layer was applied to carbon paper, adjusted so that the thickness of the microporous layer after sintering was 45 μm. The results of evaluation according to the measurement method described above are shown in Table 3.

[0091] [Example 20] When preparing a composition for a microporous layer, the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water was adjusted to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 24.0 parts by mass / 64.0 parts by mass, resulting in a thickness of 2.0 mm and a basis weight of 950 g / m². 2 A porous transport layer was obtained in the same manner as in Example 3, except that a composition for the microporous layer was applied to carbon paper, adjusted so that the thickness of the microporous layer after sintering was 40 μm. The results of evaluation according to the measurement method described above are shown in Table 3.

[0092] [Example 21] When preparing a composition for a microporous layer, the mass ratio of conductive particles / dispersant / water repellent / pore-forming agent / purified water was adjusted to 6.0 parts by mass / 2.4 parts by mass / 3.6 parts by mass / 30.0 parts by mass / 58.0 parts by mass, resulting in a thickness of 2.0 mm and a basis weight of 900 g / m². 2 A porous transport layer was obtained in the same manner as in Example 3, except that a composition for the microporous layer was applied to carbon paper, adjusted so that the thickness of the microporous layer after sintering was 35 μm. The results of evaluation according to the measurement method described above are shown in Table 3.

[0093] [Example 22] 2.0 mm thick carbon paper (conductive porous substrate, basis weight 1,050 g / m²) 2 A porous transport layer was obtained in the same manner as in Example 3, except that the carbon paper was immersed for 3 minutes in a water-repellent resin dispersion prepared by mixing 5 parts by mass of FEP resin ("Neoflon®" FEP Dispersion ND-110 (manufactured by Daikin Industries, Ltd.)) and 95 parts by mass of ion-exchanged water, the carbon paper was then removed from the water-repellent resin dispersion, excess water-repellent resin dispersion was removed, and the material was further dried at 100°C for 5 minutes before being used as the conductive porous substrate. The results of the evaluation according to the measurement method described above are shown in Table 3.

[0094] [Example 23] 2.0 mm thick carbon paper (conductive porous substrate, basis weight 1,050 g / m²) 2 A porous transport layer was obtained in the same manner as in Example 9, except that the carbon paper was immersed for 3 minutes in a water-repellent resin dispersion prepared by mixing 1 part by mass of FEP resin ("Neoflon®" FEP Dispersion ND-110 (manufactured by Daikin Industries, Ltd.)) and 99 parts by mass of ion-exchanged water, the carbon paper was then removed from the water-repellent resin dispersion, excess water-repellent resin dispersion was removed, and the material was further dried at 100°C for 5 minutes before being used as the conductive porous substrate. The results of the evaluation according to the measurement method described above are shown in Table 3.

[0095] [Example 24] 2.0 mm thick carbon paper (conductive porous substrate, basis weight 1,050 g / m²) 2A porous transport layer was obtained in the same manner as in Example 3, except that the carbon paper was immersed for 3 minutes in a water-repellent resin dispersion prepared by mixing 0.2 parts by mass of FEP resin ("Neoflon®" FEP Dispersion ND-110 (manufactured by Daikin Industries, Ltd.)) and 99.8 parts by mass of ion-exchanged water, the carbon paper was then removed from the water-repellent resin dispersion, excess water-repellent resin dispersion was removed, and the material was further dried at 100°C for 5 minutes before being used as the conductive porous substrate. The results of the evaluation according to the measurement method described above are shown in Table 3.

[0096]

[0097]

[0098]

[0099] 1 Conductive porous substrate 2 Microporous layer 3, 4 Voids 5, 6 Through holes 10 Porous transport layer 16, 26 Observation points

[0100] The porous transport layer of the present invention suppresses penetration of the electrolyte membrane by the conductive porous substrate when used in a membrane electrode assembly, and exhibits excellent gas diffusion properties. As a result, high electrolysis performance can be obtained in a water electrolysis apparatus equipped with the membrane electrode assembly. Furthermore, the porous transport layer of the present invention is CO 2 It can be used in electrolytic devices, ammonia electrolysis devices, fuel cells, etc., but is particularly suitable for use in the membrane electrode assembly of a PEM-type water electrolysis device.

Claims

1. A porous transport layer having a microporous layer on at least one side of a conductive porous substrate containing carbon fibers, wherein the microporous layer has voids with an average diameter of 3 μm or more and 70 μm or less, and the contact angle between the microporous layer and water is 70° or more and 180° or less.

2. The porous transport layer according to claim 1, wherein there are no through-holes in the microporous layer that penetrate from the surface of the microporous layer to the conductive porous substrate.

3. The porous transport layer according to claim 1, wherein the microporous layer has voids with an average diameter of 9 μm or more and 55 μm or less.

4. The porous transport layer according to claim 1, wherein the area ratio of voids with a diameter of 3 μm or more and 70 μm or less on the surface of the microporous layer is 0.1% or more and 50% or less.

5. The porous transport layer according to claim 1, wherein the area ratio occupied by voids with a diameter of 3 μm or more and 70 μm or less in the cross-section of the microporous layer is 0.1% or more and 50% or less.

6. The porous transport layer according to claim 1, wherein the area ratio occupied by voids with a diameter of 3 μm or more and 70 μm or less in the cross-section of the microporous layer is 0.5% or more and 20% or less.

7. The porous transport layer according to claim 1, wherein the contact angle between the microporous layer and water is 130° or more and 180° or less.

8. The porous transport layer according to claim 1, wherein the thickness of the conductive porous substrate is 0.3 mm or more.

9. The porous transport layer according to claim 1, wherein the ratio b / a, obtained by dividing the pore volume a of pores with a diameter in the range of 10 nm to 1 μm by the pore volume b of pores with a diameter in the range of 3 μm to 100 μm, is 4 to 180.

10. The porous transport layer according to claim 1, wherein the contact angle between the conductive porous substrate and air in water is greater than the contact angle between the microporous layer and air in water.

11. The porous transport layer according to claim 1, wherein the conductive porous substrate does not allow water containing 20% ​​by mass of ethanol to permeate, but allows water containing 40% by mass of ethanol to permeate, and the microporous layer does not allow water containing 40% by mass of ethanol to permeate.

12. Mass loss of 5 g / m² after heat treatment at 400°C for 1 hour under atmospheric conditions. 2 The porous transport layer according to claim 1, wherein the following applies:

13. Mass loss of 1 g / m² after immersion in 85°C hot water for 5 hours. 2 The porous transport layer according to claim 1, wherein the following applies:

14. A membrane electrode assembly using the porous transport layer described in claim 1.

15. A water electrolysis apparatus using the porous transport layer described in claim 1.

16. A fuel cell using the porous transport layer described in claim 1.