Connecting structure and method for manufacturing the connecting structure

By placing conductive particles and resin composition on the electrodes and performing crimping and photocuring, the problems of poor conduction and short circuit in high-fine and high-density connections are solved, and high-precision electrodes are realized connect.

CN110098167BActive Publication Date: 2024-12-31MIKUNI ELECTORON CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN201910081189.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-01-31
Filing Date
2019-01-28
Publication Date
2024-12-31
Estimated Expiration
2039-01-28

AI Technical Summary

Technical Problem

When the existing anisotropic conductive film is connected to a circuit in a highly refined and dense electronic device, irregular arrangement of conductive particles leads to poor conduction and short circuit problems, and the heating and curing connection method causes a difference in thermal expansion coefficient and leads to electrode bias. shift.

Method used

By configuring conductive particles and resin compositions on the electrodes and curing them by crimping and photocuring, the pressure deformation of the conductive particles in the opposite direction is ensured to form a conductive path, while using different resin materials to control thermal expansion and suppress thermal expansion. Short circuit.

Benefits of technology

Reliable conductive connection between highly refined and dense electrodes is achieved, and electrode offset caused by the difference in thermal expansion coefficient is avoided, thereby improving the accuracy and reliability of the connection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110098167B_ABST
    Figure CN110098167B_ABST
Patent Text Reader

Abstract

The subject of the present invention is to ensure the conductivity between electrodes and to suppress the situation where adjacent electrodes are short-circuited with each other. The method for making a connection structure of the present invention includes: arranging conductive particles and a first composition on a first electrode arranged on a first surface of a first member, arranging a second composition in an area other than the first electrode of the first surface, arranging the second surface of a second member arranged with a second electrode and the first surface in a manner such that "the conductive particles and the first composition contact the second electrode, and the second composition contacts the area other than the second electrode of the second surface", pressing the first member and the second member, and curing the first composition and the second composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a connection structure having an electrode connection structure formed of a conductive composition, and a method for producing the connection structure. Background Art

[0002] When electronic components such as integrated circuits are mounted on substrates, such as COG (Chip on Glass) connections that directly connect integrated circuits to glass substrates of liquid crystal displays, and FOG (Film on Glass) connections that connect flexible printed substrates to glass substrates of flat panel displays, anisotropic conductive films (ACF; Anisotropic Conductive Film) containing conductive particles are generally widely used. Anisotropic conductive film is a film of thermosetting resin in which fine conductive particles are dispersed. By sandwiching the anisotropic conductive film between aligned electrodes and performing thermocompression bonding, the conductive particles located between the electrodes can form a conductive path. On the other hand, the insulating properties of the thermosetting resin can be used to suppress short circuits of adjacent electrodes in the surface direction of the substrate. That is, the anisotropic conductive film has the anisotropy of "forming conductivity in the pressurized direction (the direction of the two electrodes) and maintaining insulation in the non-pressurized direction (the surface direction of the substrate)". Due to such characteristics, the anisotropic conductive film can connect a plurality of electrodes provided on an integrated circuit, a printed substrate, a glass substrate, etc. in batches, and can maintain insulation between electrodes adjacent to each other in the surface direction of the substrate.

[0003] However, with the high precision and high density of connection circuits in electronic devices in recent years, the reliability of connections using anisotropic conductive films has become a problem. That is, if the size of the electrode to be connected becomes smaller, the number of conductive particles that contribute to conduction between a pair of electrodes will decrease, and the connection reliability between the electrodes cannot be fully obtained. In addition, if the distance between adjacent electrodes in the surface direction of the substrate becomes narrower, the conductive particles will contact both sides of the adjacent electrodes, and the insulation reliability cannot be fully obtained. For this reason, Patent Document 1 discloses an anisotropic conductive film in which conductive particles are dispersed by applying a magnetic field or the like, thereby being separated from other conductive particles.

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-167106 Summary of the invention

[0007] [Problems to be solved by the invention]

[0008] However, in anisotropic conductive films, when the substrates are thermally pressed together, the arrangement of the conductive particles is irregular and scattered, so that it is not possible to fully eliminate the poor conduction caused by the absence of conductive particles between electrodes and the short circuit caused by the conductive particles contacting between adjacent electrodes. Furthermore, since a heat curing connection method is adopted, in principle, a dimensional change caused by the difference in thermal expansion coefficients between the upper and lower substrates occurs, and it is not possible to eliminate the problem of the electrodes formed on the upper and lower substrates being offset from each other.

[0009] One embodiment of the present invention is completed in view of the existing problems as described above, and one of its purposes is to ensure the conductivity between opposing electrodes through a simple process and to prevent adjacent electrodes from short-circuiting even if the electrodes arranged on an integrated circuit, a printed substrate, a glass substrate, etc. are highly refined and highly dense.

[0010] [Methods for solving the problem]

[0011] A method for producing a connection structure involved in one embodiment of the present invention includes: disposing conductive particles and a first composition on a first electrode disposed on a first surface of a first component, disposing a second composition in an area other than the first electrode on the first surface, disposing the second surface of a second component disposed with a second electrode and the first surface opposite to each other in a manner such that "the conductive particles and the first composition are in contact with the second electrode, and the second composition is in contact with an area other than the second electrode on the second surface", pressing the first component and the second component, and curing the first composition and the second composition.

[0012] A method for producing a connecting structure involved in one embodiment of the present invention includes: configuring a second composition in an area other than a first electrode configured on a first surface of a first component, configuring conductive particles and the first composition on the first electrode, arranging the second surface of the second component configured with the second electrode and the first surface opposite to each other in a manner of "the conductive particles and the first composition are in contact with the second electrode, and the second composition is in contact with the area other than the second electrode on the second surface", pressing the first component and the second component, and curing the first composition and the second composition.

[0013] A method for producing a connection structure involved in one embodiment of the present invention includes: configuring conductive particles and a first composition on a first electrode configured on a first surface of a first component, configuring a second composition in an area other than the second electrode configured on a second surface of a second component, arranging the first surface and the second surface opposite to each other in a manner such that "the conductive particles and the first composition are in contact with the second electrode, and the second composition is in contact with an area other than the first electrode of the first surface", pressing the first component and the second component, and curing the first composition and the second composition.

[0014] A method for producing a connecting structure involved in one embodiment of the present invention includes: configuring a second composition in an area other than a first electrode configured on a first surface of a first component, configuring conductive particles and the first composition on a second electrode configured on a second surface of a second component, arranging the first surface and the second surface opposite to each other in a manner of "the conductive particles and the first composition are in contact with the first electrode, and the second composition is in contact with an area other than the second electrode on the second surface", pressing the first component and the second component, and curing the first composition and the second composition.

[0015] A connection structure involved in one embodiment of the present invention includes: a first surface of a first component, a first electrode arranged on the first surface, a second surface of a second component facing the first surface, a second electrode opposite to the first electrode and arranged on the second surface, conductive particles and a first resin arranged between the first electrode and the second electrode, and a second resin arranged between an area other than the first electrode on the first surface and an area other than the second electrode on the second surface, and the first resin is different from the second resin.

[0016] [Effects of the invention]

[0017] According to one embodiment of the present invention, even if the electrodes arranged in the electronic components are highly refined and highly dense, the conductivity between the electrodes facing each other can be ensured by a simple process, and the short circuit between adjacent electrodes can be suppressed. Furthermore, since the heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a figure which shows the structure of the connection structure body which concerns on one Embodiment of this invention.

[0019] Figure 2 The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0020] Figure 3The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0021] Figure 4 The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0022] Figure 5 The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0023] Figure 6 The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0024] Figure 7 The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0025] Figure 8 The diagrams are for explaining a method for producing a connection structure according to one embodiment of the present invention.

[0026] Fig. 9 It is a figure which shows the structure of the connection structure body which concerns on one Embodiment of this invention.

[0027] Fig.10 It is a figure which shows the structure of the connection structure body which concerns on one Embodiment of this invention.

[0028] Fig.11 It is a diagram showing an example of a connection structure according to an embodiment of the present invention.

[0029] Fig.12 It is a diagram showing an example of a connection structure according to an embodiment of the present invention.

[0030] Fig.13 It is a diagram showing an example of a connection structure according to an embodiment of the present invention.

[0031] Fig.14 It is a diagram showing an example of a connection structure according to an embodiment of the present invention.

[0032] Fig.15 It is a diagram showing an example of a connection structure according to an embodiment of the present invention.

[0033] Fig.16 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0034] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, etc. However, the present invention includes a variety of different forms and is not limited to the following exemplary embodiments. The drawings attached to this specification are sometimes schematically represented by the width, thickness, shape, etc. of each part compared with the actual form in order to make the description clearer, but it is only an example and does not necessarily limit the content of the present invention. In addition, in the present invention, when a specific element recorded in a certain figure is the same or corresponding to a specific element recorded in other figures, the same symbol is sometimes marked (or a, b, etc. are marked after the number recorded as the symbol), and repeated descriptions are appropriately omitted. Furthermore, the text marked "the first" and "the second" of each element is a convenient mark used to distinguish each element, and has no further meaning unless otherwise specified.

[0035] In this specification, when a certain component or region is located "above (or below)" another component or region, unless otherwise specified, it includes not only the case where it is located directly above (or directly below) another component or region, but also the case where it is located above (or below) another component or region. That is, it also includes the case where another component is included between the above (or below) another component or region and the certain component or region.

[0036] In this specification, a connection structure in a COG connection in which an integrated circuit (second electronic component) is connected to a glass substrate of a liquid crystal display (first electronic component) is shown as an example. However, the present invention is not limited thereto, and a connection structure in a FOG connection in which a flexible printed substrate is connected to a glass substrate of a flat panel display may also be used. In this case, the second electronic component may also be a flexible printed substrate such as TAB (Tape Automated Bonding) or COF (Chip on film).

[0037] <First embodiment>

[0038] [Structure of the connection structure]

[0039] Figure 1 The structure of a connection structure according to one embodiment of the present invention is shown. Figure 1 (A) is a plan view of a connection structure according to one embodiment of the present invention. Figure 1 (B) Yes Figure 1 (A) AA' cross-section. Figure 1 (C) Yes Figure 1 (B) is an enlarged cross-sectional view of the conductive particles in the region B.

[0040] like Figure 1As shown in (A) and (B), the first electronic component 101 includes a terminal 104, a first insulating film 106, a second insulating film 108, and a first electrode 110 on the connection surface (first surface) of the first member 102. The second electronic component 111 is mounted on the connection surface (first surface) of the first electronic component 101. The second electronic component 111 includes a second electrode 114 on the connection surface (second surface) of the second member 112. The first surface of the first electronic component 101 and the second surface of the second electronic component 111 are arranged facing each other. The connection structure 100 is responsible for the physical connection between the first electronic component 101 and the second electronic component 111, and the electrical connection between the first electrode 110 and the second electrode 114. The connection structure 100 includes the first surface of the first member 102, the first electrode 110, the second surface of the second member 112, the second electrode 114, the conductive particles 10, the first resin 20, and the second resin 30.

[0041] A plurality of first electrodes 110 are disposed on the first surface of the first member 102. A second insulating film 108 is disposed on the first surface of the first member 102 in a region other than the region where the first electrodes 110 are disposed. A plurality of second electrodes 114 corresponding to the plurality of first electrodes 110 are disposed on the second surface of the second member 112. An insulating film may also be disposed on the second surface of the second member 112 in a region other than the region where the second electrodes 114 are disposed.

[0042] A plurality of first electrodes 110 and a plurality of second electrodes 114 are arranged opposite to each other. A plurality of conductive particles 10 and a first resin 20 are arranged between the opposing first electrodes 110 and second electrodes 114. A plurality of conductive particles 10 are arranged in a surface direction (D2-D3 surface direction) between the opposing first electrodes 110 and second electrodes 114. One conductive particle 10 is arranged in a facing direction (D1 direction) between the first electrode 110 and second electrode 114 between the opposing first electrodes 110 and second electrodes 114. Each conductive particle 10 contacts the opposing first electrode 110 and second electrode 114. Figure 1As shown in (C), the conductive particle 10 is deformed by pressure in the direction of the electrodes facing each other (D1 direction) between the first electrode 110 and the second electrode 114 by the following method for producing a connection structure. That is, the distance between the first electrode 110 and the second electrode 114 in the direction of the electrodes facing each other (D1 direction) is approximately the same as the height of the conductive particle 10 in the direction of the electrodes facing each other (D1 direction). The height of the conductive particle 10 in the direction of the electrodes facing each other (D1 direction) is deformed by pressure by about 10% to 40%. By applying stress between the first electrode 110, the conductive particle 10, and the second electrode 114, the first resin 20 is excluded from the contact portion between the first electrode 110 and the conductive particle 10, and the contact portion between the second electrode 114 and the conductive particle 10. Furthermore, even if a natural oxide film is formed on the first electrode 110, the conductive particles 10, or the second electrode 114 and the surface is insulated, the natural oxide film can be broken and a conductive path can be formed by pressing the first electrode 110 and the second electrode 114 with the conductive particles 10 interposed therebetween. Furthermore, by deforming the conductive particles 10, the contact area between the first electrode 110 and the conductive particles 10 and the contact area between the second electrode 114 and the conductive particles 10 can be increased. By configuring in this way, the conductive particles 10 can electrically connect the first electrode 110 and the second electrode 114.

[0043] A plurality of conductive particles 10 are dispersed in the first resin 20 between the first electrode 110 and the second electrode 114. Each conductive particle 10 is surrounded by the first resin 20 in the surface direction (D2-D3 surface direction) between the first electrode 110 and the second electrode 114. The first resin 20 is an insulating resin. Therefore, the connection structure 100 has insulating properties in the surface direction (D2-D3 surface direction). However, a plurality of conductive particles 10 arranged between the opposing first electrode 110 and the second electrode 114 and adjacent in the surface direction (D2-D3 surface direction) may also contact each other. When the conductive particles 10 adjacent in the surface direction (D2-D3 surface direction) contact each other, the adjacent conductive particles 10 are also electrically connected to each other. By configuring in this way, the conductive particles 10 can more reliably electrically connect the opposing first electrode 110 and the second electrode 114. The distance between adjacent conductive particles 10 can be appropriately controlled by adjusting the concentration of the conductive particles 10 mixed in the first composition 20 ′ described below.

[0044] like Figure 1As shown in (A) and (B), a plurality of conductive particles 10 and a first resin 20 are arranged on the upper surface of the first electrode 110 (or the lower surface of the second electrode 114). When observed in the opposite direction of the electrodes (D1 direction), a plurality of conductive particles 10 and a first resin 20 are arranged in each certain area. In the present embodiment, the diameter of the conductive particles 10 observed in the opposite direction of the electrodes (D1 direction) is within the range of 2 μm or more and 10 μm or less. Preferably, the number of areas where conductive particles 10 and the first resin 20 are arranged on the upper surface of one first electrode 110 (or the lower surface of the second electrode 114) is 1 or more, and each area is separated by 5 μm or more. The number of conductive particles 10 in one area where conductive particles 10 and the first resin 20 are arranged is preferably 1 or more and 7 or less. The number of conductive particles 10 arranged in one area is more preferably 3, and the second most preferably 7. When viewed in the opposing direction of the electrodes (direction D1), the number of the conductive particles 10 disposed between the first electrode 110 and the second electrode 114 that face each other is preferably 7 particles / 400 μm. 2 More than 20 pieces / 400μm 2 When the number of conductive particles 10 is less than 7 / 400 μm 2 When the number of the conductive particles 10 is more than 20 / 400 μm, the connection resistance value may tend to vary. 2 When the number of conductive particles 10 is greater than 20 / 400 μm, the amount of pressure deformation of the conductive particles 10 decreases due to load dispersion, and the natural oxide film in the connection area cannot be broken, resulting in a high connection resistance. 2 By configuring in this way, the conductive particles 10 can reliably connect the first electrode 110 and the second electrode 114 facing each other, and can prevent short circuits between a plurality of first electrodes 110 adjacent to each other in the plane direction (D2-D3 plane direction), between a plurality of second electrodes 114 adjacent to each other in the plane direction (D2-D3 plane direction), and between the first electrode 110 and the second electrode 114 not facing each other.

[0045] In the present embodiment, the shape of the region where the conductive particles 10 and the first resin 20 are arranged observed in the opposite direction of the electrodes (D1 direction) is circular. However, this is not limited to this, and the region where the conductive particles 10 and the first resin 20 are arranged can adopt any shape as long as the above conditions are met. In the present embodiment, two regions where the conductive particles 10 and the first resin 20 are arranged are arranged on the upper surface of one first electrode 110 (or the lower surface of one second electrode 114). In addition, seven conductive particles 10 are arranged in one region. However, this is not limited to this, and the number of regions where the conductive particles 10 and the first resin 20 are arranged on the upper surface of one first electrode 110 (or the lower surface of one second electrode 114) as long as the above conditions are met, can be appropriately adjusted according to the area of ​​the upper surface of the first electrode 110 (or the lower surface of the second electrode 114), the area of ​​the region where the conductive particles 10 and the first resin 20 are arranged, and the size of the conductive particles 10. The number of the conductive particles 10 to be arranged in one region may be adjusted as appropriate as long as the above conditions are satisfied, depending on the size and concentration of the conductive particles 10 .

[0046] The second resin 30 is further arranged between the first surface of the first member 102 and the second surface of the second member 112. The second resin 30 is arranged in an area other than between the first electrode 110 and the second electrode 114 facing each other. The second resin 30 is arranged between an area other than the first electrode of the first surface and an area other than the second electrode of the second surface. That is, the second resin 30 is arranged between and around a plurality of first electrodes 110 adjacent in the surface direction (D2-D3 surface direction) (between and around a plurality of second electrodes 114 adjacent in the surface direction (D2-D3 surface direction)). In addition, the second resin 30 is also arranged in an area other than the area where the conductive particles 10 and the first resin 20 are arranged between the first electrode 110 and the second electrode 114. The second resin 30 is arranged between and around a plurality of areas where the conductive particles 10 and the first resin 20 are adjacent in the surface direction (D2-D3 surface direction). In other words, the conductive particles 10 and the first resin 20 are surrounded by the second resin 30 in the surface direction (D2-D3 surface direction). That is, when observed in the opposite direction of the electrodes (D1 direction), the plurality of conductive particles 10 are surrounded by the first resin 20, and the first resin 20 is surrounded by the second resin 30. The second resin 30 is an insulating resin. Therefore, the connection structure 100 has insulating properties in the surface direction (D2-D3 surface direction). By configuring in this way, the second resin 30 can reliably insulate between the plurality of first electrodes 110 adjacent in the surface direction (D2-D3 surface direction), between the plurality of second electrodes 114 adjacent in the surface direction (D2-D3 surface direction), and between the first electrode 110 and the second electrode 114 that are not facing each other.

[0047] The boundary between the first resin 20 and the second resin 30 can be confirmed by observing the cross section of the connection structure 100. Since the first resin 20 and the second resin 30 have different compositions, the boundary between the first resin 20 and the second resin 30 can also be determined by using a processing / observation device such as a focused ion beam processing and observation device (FIB), a scanning electron microscope (SEM), or a transmission electron microscope (TEM).

[0048] When the first composition 20' and the second composition 30' described below are difficult to dissolve in each other, the boundary between the first resin 20 and the second resin 30 can be confirmed as an interface. When the first composition 20' and the second composition 30' have similar compositions and the interface disappears in the following steps, a boundary layer in which the first resin 20 and the second resin 30 are mixed may be observed.

[0049] The first electronic element 101 may be, for example, a flat panel display such as a liquid crystal display, an organic EL display, or a plasma display, and the first member 102 may be, for example, an insulating substrate such as a glass substrate or a transparent film substrate. The first electrode 110 may be, for example, an external connection terminal provided on the display. The first electrode 110 and the terminal 104 may also be formed by transparent conductive materials such as ITO (indium tin oxide), IZO (indium zinc oxide), metals such as copper (Cu), aluminum (Al), molybdenum (Mo), titanium (Ti), and alloys containing at least one of them (Mo-Ti alloy, etc.), and laminated structures of these materials (Mo / Cu laminated structure, Mo-Ti alloy / Cu laminated structure, Mo / Al laminated structure, Mo / Al / Mo laminated structure, Al / Ti laminated structure, etc.).

[0050] The second electronic element 111 may also be a Si chip formed with an integrated circuit. In this case, the second electrode 114 is equivalent to an external connection terminal (pad) provided on the integrated circuit. The second member 112 is preferably a silicon substrate, a SiC substrate, a sapphire substrate, a plastic substrate, etc. The second electrode 114 is preferably formed by gold (Au) or gold plating on the surface of copper (Cu). In the case where the second electronic element 111 is, for example, a flexible printed substrate, the second member 112 is, for example, preferably an insulating polymer film such as polyimide or para-polyamide. The second electrode 114 is, for example, equivalent to an external connection terminal provided on a flexible printed substrate, generally formed of copper (Cu), and gold-plated on the surface.

[0051] There is no particular limitation on the size of the first electrode 110 and the second electrode 114 observed in the opposite direction (D1 direction). There is no particular limitation on the distance between the plurality of first electrodes 110 adjacent to each other in the surface direction (D2-D3 surface direction) (the distance between the plurality of second electrodes 114 adjacent to each other in the surface direction), for example, it can be 5 μm or more. By adopting such a structure, the first electrode 110 and the second electrode 114 can be electrically connected without damaging the insulation. In the present embodiment, the first electrode 110 and the second electrode 114 are arranged in a row at one end of the first electronic component 101 and the second electronic component 111 with their short sides arranged side by side. However, this is not limited to this, and the first electrode 110 and the second electrode 114 can also be arranged in multiple columns, and can also be arranged in a zigzag lattice shape.

[0052] The conductive particles 10 contained in the connection structure 100 may also be oblate spherical. The diameter (major diameter) of the conductive particles 10 observed in the direction opposite to the electrodes (D1 direction) is in the range of 2 μm to 10 μm. The conductive particles 10 may also be originally spherical with the major diameter as the diameter, and may be deformed to be flat in the direction opposite to the electrodes (D1 direction) in the range of 10% to 40% relative to 100% of the major diameter by the following connection structure production method. The diameter (major diameter) and the amount of pressure deformation of the conductive particles 10 may be appropriately selected from the above ranges according to the types of the first electronic component 101 and the second electronic component 111, the production methods of each connection structure, etc. In the present embodiment, the conductive particles 10 are as follows. Figure 1 (D) shows a perfect sphere. However, it is not limited to this. For example, Figure 1 As shown in (E), it is a spherical shape with a plurality of protrusions on the surface (a spike shape). By having fine protrusions on the surface of a spherical shape like this, it is more preferable because, for example, the natural oxide film in the connection area can be broken.

[0053] The material of the conductive particles 10 is not particularly limited, and can be appropriately selected from well-known conductive particles. Figure 1 As shown in (D) and (E), metal-coated particles may be used, and the metal-coated particles have coating layers 10b and 10c that coat a particle core 10a obtained by coating a high-hardness resin material with a rubber-like elastic resin or a high-hardness inorganic material with a rubber-like inorganic elastic body with a metal such as nickel (Ni), copper (Cu), and gold (Au). The metal coating may be formed into a Ni / Cu stacked structure, a Ni / Au stacked structure, or a Cu / Au stacked structure by, for example, a drum sputtering method, a metal nanoparticle plating method, an electroless plating method, an ultrasonic plating method, or the like.

[0054] The first resin 20 and the second resin 30 are formed by curing the first composition 20' and the second composition 30' containing different materials. The materials of the first composition 20' and the second composition 30' are not particularly limited, and can be appropriately selected from well-known curable resin materials. In the present embodiment, the curable resin materials of the first composition 20' and the second composition 30' both contain free radical polymerization resins. As free radical polymerization resin materials, preferably (meth) acrylic monomers or (meth) acrylate oligomers, more preferably ester-type bonds. (Meth) acrylic oligomers have at least one or more (meth) acryloyl groups, for example, epoxy acrylate, acrylic urethane, polyester acrylate, polybutadiene acrylate, polyol acrylate, polyether acrylate, silicone resin acrylate, melamine acrylate, etc. can be used. It can be any of monofunctional and multifunctional, and more preferably contains multifunctional monomers or oligomers. The curable resin material may be composed of two or more selected from (meth)acrylate monomers and (meth)acrylate oligomers.

[0055] As the curable resin material of the second composition 30', a material with a low volume shrinkage during curing is particularly preferred. Therefore, the (meth) acrylic acid monomer compound, for example, may also contain an amide hydroxymethyl structural part, and may also contain a dendritic polymer or a hyperbranched polymer structural part. During photocuring, the (meth) acrylic acid monomer compound having an amide hydroxymethyl structural part polymerizes with each other as the carbon-carbon double bonds derived from (meth) acrylic acid, and the methylene-oxygen of the amide hydroxymethyl structural part is cut off. Therefore, the second composition 30' comprises a (meth) acrylic acid monomer compound having at least one amide hydroxymethyl structural part composed of -CO-NH-CH2-O- in the molecule as a curing component, thereby further suppressing the volume shrinkage of the second resin 30 caused by curing the second composition 30', and suppressing the warping caused by the difference in bending rigidity between the first electronic component 101 and the second electronic component 111. By including a dendritic polymer or hyperbranched polymer structure having acryloyl groups arranged in the branches, the van der Waals distance between the branches is shorter than the van der Waals distance of a normal molecule. Therefore, the second composition 30' includes a dendritic polymer or hyperbranched polymer structure having acryloyl groups arranged as a curing component, so that the volume shrinkage of the second resin 30 caused by curing the second composition 30' can be further suppressed, and the warping caused by the difference in bending rigidity between the first electronic component 101 and the second electronic component 111 can be suppressed.

[0056] As the curable resin material of the second composition 30', it is preferred to use a fluorene-based acrylate. The second composition 30' may also include an ene / thiol-based curable resin as a curing component, and the ene / thiol-based curable resin contains a compound having an ethylenically unsaturated double bond and a thiol compound, and at least one of these components may also include a compound having a 9,9-diarylfluorene skeleton. As a 9,9-diarylfluorene compound, a 9,9-diarylfluorene compound having an ethylenically unsaturated bond and / or a 9,9-diarylfluorene compound having a mercapto group may also be included. As an ethylenically unsaturated compound, for example, 9,9-di(4-acryloyloxyethoxyphenyl)fluorene (manufactured by Osaka Gas Chemical (Co., Ltd.), OGSOL EA-0200), phenoxyethyl acrylate (manufactured by Kyoeisha Chemical (Co., Ltd.), Light-Acrylate POA) may also be used. As the thiol compound, for example, pentaerythritol tetrakis(3-mercaptobutyrate) (produced by Showa Denko Co., Ltd., Karenz MT PE1) can also be used. The second composition 30' contains such a curable resin material, so that the volume shrinkage of the second resin 30 caused by curing the second composition 30' can be further suppressed, and the warping caused by the difference in bending rigidity between the first electronic component 101 and the second electronic component 111 can be suppressed.

[0057] As the curable resin material of the second composition 30', a material obtained by treating an ene / thiol curable resin with an oxidizing compound may also be used. The ene / thiol curable resin includes: an ene compound having two or more functional groups selected from the group consisting of allyl ether groups, vinyl ether groups, acrylate groups and methacrylate groups in the molecule, or a mixture of two or more of the above ene compounds; and a thiol compound having two or more thiol groups in one molecule. As a compound having two or more mercapto groups in one molecule, esters of mercaptocarboxylic acid and polyols, aliphatic polythiols and aromatic polythiols, and other polythiols may be included, and one or more of them may be used. For the oxidizing compound treatment, it is preferably carried out using a gas with oxidizing ability. The gas with oxidizing ability is a compound that has the properties of a gas under the temperature and pressure conditions of the oxidizing compound treatment and has oxidizing ability. As the gas with oxidizing ability, air, oxygen, ozone, etc. may be used, and a mixed gas containing part of them may also be used. By treating the photocurable resin material with an oxidizing compound, the second composition 30' can improve its stability over time.

[0058] The materials of the first composition 20' and the second composition 30' further include a photocuring initiating component. The photocuring initiating component can be any compound that generates free radicals by irradiating ultraviolet rays or visible light as a photoradical initiator. As an ultraviolet free radical initiator, for example, acetophenone-based initiators, benzoin ether-based initiators, benzophenone-based initiators, α-diketone-based initiators, and thioxanthone-based initiators can be used. As a visible light free radical initiator, for example, camphorquinone-based compounds and acylphosphine oxide compounds can be used. In addition, it can also be a component that is classified as an ultraviolet free radical initiator but can be used together with a sensitizer to initiate visible light free radicals. The sensitizer can be used appropriately as needed. As a sensitizer, a known compound can be used, for example, an amine compound and (meth) acrylates of alkanolamines can be used. A variety of photocuring initiating components and sensitizers can be used together. For example, an ultraviolet free radical initiator and a visible light free radical initiator can be used together to expand the wavelength region in which curing can be performed. The photocuring initiating component is more preferably a photo-radical initiator that generates free radicals within a range of 300 nm to 500 nm of wavelength of irradiated light. The photocuring initiating component is formulated so that the curable resin material can be cured at room temperature within a light irradiation time of preferably about 3 seconds or less, more preferably 1 second or less. In addition, the curable resin material is also appropriately selected so that it can be cured at room temperature within such a time.

[0059] In the present embodiment, the first composition 20' and the second composition 30' more preferably further include a shielding curing active compound, such as a chain transfer agent. The chain transfer agent transfers the free radicals generated by light irradiation to the shielding portion that the light does not directly reach. The chain transfer agent can, for example, use a compound containing at least one selected from a carbamate bond, a urea bond, or an isocyanate group, and at least one alkoxysilyl group. In the photocuring reaction using the above-mentioned chain transfer agent, a polyol having a hydroxyl group as an anion is produced as a by-product. The polyol causes an ester exchange reaction with the alkoxysilyl group contained in the chain transfer agent, thereby further curing. That is, by including a chain transfer agent, free radical curing and anion curing are simultaneously produced, and the shielding portion that the light does not directly reach can be cured.

[0060] By making the first composition 20' and the second composition 30' contain a shielding portion curable active compound, the first composition 20' and the second composition 30' can be reliably cured even under conditions such as the materials and connection methods of the first electronic component 101, the second electronic component 111, the first electrode 110, and the second electrode 114, where the first composition 20' and the second composition 30' cannot be cured by the action of the photocuring initiating component generated by light irradiation alone.

[0061] In the present embodiment, the material of the first composition 20' may further include an anaerobic curing initiation component. The anaerobic curing initiation component may use a known system including an organic peroxide and a curing accelerator. For example, the organic peroxide may use hydrogen peroxides, ketone peroxides, diacyl peroxides, peroxyesters, etc. As a curing accelerator, for example, o-benzoylsulfonyl imide (saccharin), hydrazine compounds, amine compounds, thiol compounds, etc. may be used. A variety of anaerobic curing initiation components and curing accelerators may also be used together.

[0062] In the present embodiment, the first composition 20' is surrounded by the first surface (including the first electrode 110), the second surface (including the second electrode 114), and the second composition 30'. Furthermore, the first composition 20' contacts the first electrode 110, the second electrode 114, and the conductive particles 10. When the first composition 20' includes an anaerobic curing initiating component, since the first electrode 110, the second electrode 114, and the conductive particles 10 contain a transition metal component, the peroxide is decomposed by the redox reaction of the curing accelerator and the transition metal ions, thereby initiating anaerobic curing of the first composition 20'.

[0063] By making the first composition 20' further include an anaerobic curing initiating component, the first composition 20' can be reliably cured even under conditions such as the materials and connection methods of the first electronic component 101, the second electronic component 111, the first electrode 110, and the second electrode 114, where the first composition 20' cannot be cured using only the action of the photocuring initiating component generated by light irradiation.

[0064] Additives can be used appropriately as needed to improve or change properties such as fluidity, coating characteristics, preservation, curing characteristics, and physical properties after curing. As additives, known compounds can be used, for example, silane coupling agents, diluents, modifiers, surfactants, storage stabilizers, defoamers, leveling agents, etc. can be listed, but are not limited to these. As silane coupling agents, for example, epoxy systems, amino systems, mercapto-sulfide systems, urea systems, etc. can be used, but are not particularly limited. By adding silane coupling agents, the adhesion on the interface of organic materials and inorganic materials is improved.

[0065] The viscosity of the first composition 20' is higher than the viscosity of the second composition 30'. The viscosity of the first composition 20' is 5×10 3 cP or more and 5×10 5 The viscosity of the second composition 30' is 2×10 3 cP or more and 2×10 5cP or less. The difference between the viscosity of the first composition 20' and the viscosity of the second composition 30' is at least 2 times. The viscosity of the first composition 20' and the second composition 30' can also be controlled by the degree of polymerization of the resin material contained in the first composition 20' and the second composition 30'. The viscosity of each composition can be appropriately selected from the above range according to the type of the first electronic component 101 and the second electronic component 111, the method for making the connection structure, the method for configuring the composition, etc. When the viscosity of the first composition 20' is less than 5×10 3 cP, the uniform dispersibility of the conductive particles 10 deteriorates, and sedimentation or aggregation is easily generated. By making the viscosity of the first composition 20' higher than the viscosity of the second composition 30', the flow of the conductive particles 10 mixed in the first composition 20' can be suppressed, so that the conductive particles 10 can be efficiently arranged between the first electrode 110 and the second electrode 114. Therefore, the connection reliability between the first electrode 110 and the second electrode 114 can be ensured.

[0066] The first resin 20 and the second resin 30 are formed by curing the first composition 20' and the second composition 30'. The volume shrinkage of the first resin 20 generated by curing the first composition 20' and the volume shrinkage of the second resin 30 generated by curing the second composition 30' are preferably 4% or less, and more preferably 2% or less. When the volume shrinkage of the first resin 20 and the second resin 30 is greater than 4%, internal shrinkage stress is generated, and warping is easily generated due to the difference in bending rigidity between the first electronic component 101 and the second electronic component 111, thereby reducing the physical connection reliability of the first electronic component 101 and the second electronic component 111.

[0067] The first resin 20 preferably has high adhesion to conductive materials such as metal materials and metal oxide materials. The first resin 20 preferably has high adhesion to metal materials forming the first electrode 110 and the second electrode 114, for example, preferably has high adhesion to Au and ITO. The second resin 30 preferably has high adhesion to resin materials. The second resin 30 preferably has high adhesion to insulating film materials forming the first surface of the first component 102 and the second surface of the second component 112, for example, preferably has high adhesion to insulating materials such as polyimide, para-polyamide film, P-SiNx, and glass. The adhesion of the first resin 20 is preferably within a range of 500 N / m or more. The adhesion of the second resin 30 is preferably within a range of 700 N / m or more. The adhesion, glass transition temperature, and hardness of each resin can be appropriately selected according to the types of the first electronic component 101 and the second electronic component 111, and the method for making the connection structure. By selecting the first resin 20 and the second resin 30 according to the materials of the adherends, the bonding strength between the first surface of the first member 102 and the second surface of the second member 112 can be further improved. Therefore, the physical connection reliability between the first electronic component 101 and the second electronic component 111 can be improved.

[0068] [Method for producing a connected structure]

[0069] Next, use Figure 2 to Figure 5 , a method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figure 2 to Figure 5 Detailed description will be given of a method for forming the connection structure 100 .

[0070] First, a plurality of conductive particles 10 and a first composition 20' are arranged in a given area on the first electrode 110. The plurality of conductive particles 10 and the first composition 20' are mixed and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, it is particularly preferred to use a pad printing method using a pad transfer printing material. Figure 2 to Figure 5 , a method of arranging the plurality of conductive particles 10 and the first composition 20 ′ will be described.

[0071] Figure 2 This shows a step of placing a mixture of a plurality of conductive particles 10 and a first composition 20 ′ on a printing plate 220 . Figure 3 yes Figure 2C-C' cross-sectional view. In the present embodiment, the printing plate 220 is a flat gravure plate, for example, a waterless plate. The printing plate 220 has a recess 226 corresponding to an area where a plurality of conductive particles 10 and a first composition 20' are arranged on the first surface of the first member 102. The printing plate 220 includes a lyophilic layer 222 and a lyophobic layer 224. The lyophobic layer 224 is arranged on the liquid contact surface and has an opening. The lyophobic layer 224 exposes the lyophilic layer 222 at the opening. That is, the lyophobic layer 224 is arranged on the upper surface of the printing plate 220, and the lyophilic layer 222 is arranged on the bottom surface of the recess 226.

[0072] The material of the lyophilic layer 222 may be, for example, aluminum oxide (Al2O3). The material of the lyophobic layer 224 is preferably, for example, an elastic silicone resin. The depth of the recess 226 is approximately the same as the thickness of the lyophobic layer 224. The depth of the recess 226 only needs to be greater than the diameter of the conductive particle 10. In addition to the horizontal plate, the printing plate 220 may also be a glass flat gravure plate, a stainless steel flat gravure plate, a sapphire flat gravure plate, or a zirconium oxide flat gravure plate. The recesses 226 observed on the upper surface of the printing plate 220 are preferably spaced apart by more than 5 μm. When the recesses 226 are less than 5 μm apart, the lyophobic layer 224 separating the adjacent recesses 226 is easily damaged, thereby reducing the durability of the printing plate 220.

[0073] In the present embodiment, the shape of the recess 226 observed in the opposite direction of the electrode (D1 direction) is circular. In addition, the recess 226 has the same shape in the depth direction. That is, the recess 226 has a shape obtained by cutting a cylinder from the printing plate 220. However, this is not limited to this, and the shape of the recess 226 can be any shape as long as the depth is within the above range.

[0074] In this embodiment, a mixture of the conductive particles 10 and the first composition 20' is placed on a printing plate 220 using a roller 210. Figure 2 (A)~(C) and Figure 3 As shown in (A) to (C), the roller 210 moves while rotating from one end to the other end of the printing plate 220 so that the outer peripheral surface of the roller 210 contacts the upper surface of the printing plate 220 (the upper surface of the liquid-repellent layer 224 ), thereby arranging the conductive particles 10 and the first composition 20 ′ in the recessed portion 226 .

[0075] The concentration of the conductive particles 10 mixed in the first composition 20' is preferably in the range of 20% by volume or more and 60% by volume or less relative to the total volume of the conductive particles 10 and the first composition 20'. When the amount of the conductive particles 10 blended is less than 20% by volume, it is difficult to fill a sufficient amount of the conductive particles 10 into the recess 226. When the amount of the conductive particles 10 blended is greater than 60% by volume, the operability is deteriorated, making it difficult to fill the mixture of the conductive particles 10 and the first composition 20' into the recess 226. The conductive particles 10 and the first composition 20' are filled into the recess 226 of the printing plate 220 by arranging the mixture of the conductive particles 10 and the first composition 20' using the roller 210. Since the recess 226 has a depth in the above range, one conductive particle 10 can be held in the depth direction (D1 direction) of the recess 226. The number of conductive particles 10 arranged in one concave portion 226 is preferably 1 or more and 7 or less. The number of conductive particles 10 arranged in one concave portion 226 is more preferably 3, and the next most preferably 7. By arranging in this way, in the step of transferring the mixture of the conductive particles 10 and the first composition 20' to the pad described below, the conductive particles 10 and the first composition 20' can be efficiently transferred to the pad.

[0076] Since the recessed portion 226 has an opening of the elastic liquid-repellent layer 224, even if the conductive particles 10 abut against the liquid-repellent layer 224 due to the movement of the roller 210, the conductive particles 10 can be held in the recessed portion 226 without being damaged. Since the recessed portion 226 has the liquid-philic layer 222 at the bottom, the first composition 20' can be held. On the other hand, since the liquid-repellent layer 224 is disposed on the upper surface of the printing plate 220, the first composition 20' is repelled.

[0077] Figure 4 2 shows the process of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the printing plate 220 to the pad 230. Figure 4 As shown in (A) to (C), the conductive particles 10 and the first composition 20' filled in the concave portion 226 are transferred to the rubber head 230 by pushing the rubber head 230 in a direction substantially perpendicular to the printing plate 220 and pulling the rubber head 230 away in a direction substantially perpendicular to the printing plate 220. Since the viscosity of the first composition 20' is 5×10 3 cP or more and 5×10 5 Since the conductive particles 10 mixed in the first composition 20 ′ are within the range of cP or less, the conductive particles 10 can be held on the surface of the pad 230 .

[0078] The material of the pad 230 is preferably, for example, a silicone resin having elasticity. The shape of the pad 230 preferably has at least a convex structure. The shape of the pad 230 can be appropriately formed according to the shapes of the first electronic component 101 and the printing plate 220 .

[0079] Figure 5 (A) to (B) represent the process of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the rubber head 230 to the first electrode 110. Figure 5 As shown in (A) to (B), the mixture of the conductive particles 10 and the first composition 20' transferred to the glue head 230 is transferred to the first electrode 110 by pushing the glue head 230 in a direction substantially perpendicular to the first electrode 110 and pulling the glue head 230 away in a direction substantially perpendicular to the first electrode 110. On the first surface of the first member 102, the conductive particles 10 and the first composition 20' form a convex structure in the direction opposite to the electrodes (D1 direction). Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP or more and 5×10 5 Since the range of cP or less is 1.5 cP, the conductive particles 10 mixed in the first composition 20' can be held on the first electrode 110. By using such a method, the conductive particles 10 and the first composition 20' can be accurately arranged in a predetermined region on the first electrode 110.

[0080] Next, the second composition 30' is disposed on the first surface of the first member 102. Figure 5 As shown in (C), the second composition 30' is arranged in an area other than the first electrode 110 on the first surface of the first member 102. Moreover, the second composition 30' is also arranged in an area other than the area on the first electrode 110 where the plurality of conductive particles 10 and the first composition 20' are arranged. That is, the second composition 30' is arranged on the first surface of the first member 102 in an area other than the area where the plurality of conductive particles 10 and the first composition 20' are arranged. The first composition 20' and the conductive particles 10 forming the convex structure on the first surface of the first member 102 are buried with the aid of the second composition 30'. Although not shown in the figure, in this embodiment, the second composition 30' is arranged using a pad printing method in the same manner as the arrangement of the mixture of the conductive particles 10 and the first composition 20'. However, it is not limited to this, and the method of arranging the second composition 30' can also use an existing method as long as it can be coated differently from the area other than the area where the plurality of conductive particles 10 and the first composition 20' are arranged. For example, inkjet, coating using a dispenser, offset printing, or the like can be used.

[0081] The viscosity of the second composition 30' is 2×10 3 cP or more and 2×105 The viscosity of the first composition 20' only needs to be higher than the viscosity of the second composition 30', and the difference in viscosity is at least 2 times. Thus, the flow of the conductive particles 10 mixed in the first composition 20' can be suppressed, so that the conductive particles 10 can be retained on the first electrode 110.

[0082] Next, the second member 112 is mounted on the first surface of the first member 102. Figure 5 As shown in (D), the first surface of the first member 102 and the second surface of the second member 112 are arranged to face each other in such a manner that the corresponding plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposed. The first member 102 and the second member 112 are pressed so that the first surface of the first member 102 and the second surface of the second member 112 are pressed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20', and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because of its higher viscosity than the second composition 30'. The conductive particles 10 and the first composition 20 ′ disposed on the first electrode 110 are in contact with the second electrode 114 , and the second composition 30 ′ disposed on the first surface other than the first electrode 110 is in contact with the second surface other than the second electrode 114 .

[0083] like Figure 5 As shown in (E), the first member 102 and the second member 112 are further pressed, so that the first surface of the first member 102 and the second surface of the second member 112 are pushed in a direction substantially perpendicular to each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower parts of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10 and the elastic force of the first composition 20' and the second composition 30'.

[0084] Here, the pressure is applied until the conductive particle 10 is deformed into an oblate spheroid due to the pressure from the first electrode 110 and the second electrode 114. The pressure deformation amount of the conductive particle 10 is controlled within a range of 10% or more and 40% or less relative to 100% of the major axis of the conductive particle 10. At this time, by applying stress between the first electrode 110, the conductive particle 10, and the second electrode 114, the first composition 20' between the first electrode 110 and the conductive particle 10, and between the second electrode 114 and the conductive particle 10 is removed. Furthermore, even if a natural oxide film is formed on the first electrode 110, the conductive particle 10, or the second electrode 114 and the surface is insulated, the first electrode 110 and the second electrode 114 can be pressed and bonded with the conductive particle 10 sandwiched therebetween, thereby breaking through the natural oxide film and forming a conductive path. By deforming the conductive particles 10, the contact area between the first electrode 110 and the conductive particles 10 and the contact area between the second electrode 114 and the conductive particles 10 can be increased. By disposing the conductive particles 10 in this manner, the conductive particles 10 can electrically connect the first electrode 110 and the second electrode 114.

[0085] In the state where the first member 102 and the second member 112 are pressed, the connection structure 100 is irradiated with light. The wavelength region of the light is preferably ultraviolet and / or visible light region, and ultraviolet light is more preferred in particular. The wavelength region of the light can be appropriately selected according to the photocuring initiating components contained in the first composition 20' and the second composition 30'. The direction of light irradiation can be appropriately selected from the first electronic component 101 side or the second electronic component 111 side according to the wavelength region of the light and the materials of the first member 102 and the second member 112. In addition, it is also preferred to irradiate from both sides, and irradiation from the side without a shield is also effective. The irradiation time of light can be appropriately selected according to the photocuring initiating components and curable resin materials contained in the first composition 20' and the second composition 30'. Generally, it is preferably about 3 seconds or less, and more preferably about 1 second or less. In other words, the light irradiation intensity, photocuring initiating components, and curable resin materials are appropriately selected in such a manner that room temperature curing can be performed within such a time.

[0086] By light irradiation, most of the first composition 20' and the second composition 30' contained in the connection structure 100 are cured at room temperature. However, there may be insufficient curing between the first electrode 110 and the second electrode 114 where light does not fully reach. Therefore, the material of the first composition 20' more preferably includes a shielding portion curing active compound or an anaerobic curing initiating component. By including a shielding portion curing active compound or an anaerobic curing initiating component, room temperature curing can be promoted even in the portion where light does not fully reach. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting such a structure, the first surface of the first electronic component 101 can be physically connected to the second surface of the second electronic component 111.

[0087] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged in the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.

[0088] <Second embodiment>

[0089] The structure of the connection structure involved in this embodiment is the same as that of the connection structure involved in the first embodiment. The method for preparing the connection structure involved in this embodiment is the same as the method for preparing the connection structure involved in the first embodiment, except that the order of the process of configuring the mixture of the plurality of conductive particles 10 and the first composition 20' and the process of configuring the second composition 30' are exchanged. The same description as that of the first embodiment is omitted, and only the parts different from the method for preparing the connection structure involved in the first embodiment are described here.

[0090] [Method for producing a connected structure]

[0091] use Figure 6 A method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figure 6 Detailed description will be given of a method for forming the connection structure 100.

[0092] First, the second composition 30' is disposed on the first surface of the first member 102. Figure 6As shown in (A) to (B), the second composition 30' is arranged in an area other than the first electrode 110 on the first surface of the first member 102. Furthermore, the second composition 30' is also arranged in an area other than the area on the first electrode 110 where a plurality of conductive particles 10 and the first composition 20' are arranged as described below. That is, the second composition 30' is arranged on the first surface of the first member 102 in an area other than the area where a plurality of conductive particles 10 and the first composition 20' are arranged. On the first surface of the first member 102, the second composition 30' forms a convex structure in the opposite direction of the electrodes (D1 direction). Although not shown in the figure, in this embodiment, the second composition 30' is arranged using a pad printing method. However, it is not limited to this, and the method of configuring the second composition 30' can use an existing method as long as it can be coated differently from the area other than the area where a plurality of conductive particles 10 and the first composition 20' are arranged. For example, inkjet or coating using a dispenser, offset printing, etc. can be used.

[0093] The viscosity of the second composition 30' is 2×10 3 cP or more and 2×10 5 This can suppress the flow of the second composition 30'.

[0094] Next, a plurality of conductive particles 10 and a first composition 20' are arranged in a given area on the first electrode 110. The plurality of conductive particles 10 and the first composition 20' are mixed and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, it is particularly preferred to use a pad printing method of a pad transfer printing material. The area and method for arranging the mixture of the plurality of conductive particles 10 and the first composition 20' are the same as the method for preparing the connection structure involved in the first embodiment, so the description is omitted here.

[0095] Figure 6 (C) to (D) show the process of transferring the rubber head 230 to the first electrode 110 by pad printing. Figure 6 As shown in (C) to (D), the mixture of the conductive particles 10 and the first composition 20' transferred to the glue head 230 is transferred to the first electrode 110 by pushing the glue head 230 in a direction substantially perpendicular to the first electrode 110 and pulling the glue head 230 away in a direction substantially perpendicular to the first electrode 110. The second composition 30' forming the convex structure on the first surface of the first member 102 is embedded by means of the first composition 20' and the conductive particles 10. Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP or more and 5×10 5Since the range of cP or less is 0.1, the conductive particles 10 mixed in the first composition 20' can be held on the first electrode 110. By using such a method, the conductive particles 10 and the first composition 20' can be reliably arranged in a predetermined region on the first electrode 110.

[0096] Next, the second electronic component 111 is mounted on the first surface of the first electronic component 101. Figure 6 As shown in (E), the first surface of the first member 102 and the second surface of the second member 112 are arranged to face each other in such a manner that the corresponding plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposed. The first member 102 and the second member 112 are pressed so that the first surface of the first member 102 and the second surface of the second member 112 are pressed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20', and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because of its higher viscosity than the second composition 30'. The conductive particles 10 and the first composition 20 ′ disposed on the first electrode 110 are in contact with the second electrode 114 , and the second composition 30 ′ disposed on the first surface other than the first electrode 110 is in contact with the second surface other than the second electrode 114 .

[0097] like Figure 6 As shown in (F), the first member 102 and the second member 112 are further pressed, so that the first surface of the first member 102 and the second surface of the second member 112 are pushed along the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower parts of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'. By adopting such a structure, the first electrode 110 and the second electrode 114 can be electrically connected.

[0098] In a state where the first member 102 and the second member 112 are pressed, the connection structure 100 is irradiated with light, so that the first composition 20' and the second composition 30' are cured. The method of curing the first composition 20' and the second composition 30' is the same as the method for preparing the connection structure involved in the first embodiment, so the description is omitted here. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting such a structure, the first surface of the first electronic component 101 and the second surface of the second electronic component 111 can be physically connected.

[0099] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged in the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.

[0100] <Third embodiment>

[0101] The structure of the connection structure involved in this embodiment is the same as that of the connection structure involved in the first embodiment. The method for preparing the connection structure involved in this embodiment is the same as the method for preparing the connection structure involved in the first embodiment, except that the second composition 30' is arranged in the area other than the second electrode 114 on the second surface. The same description as that of the first embodiment is omitted, and only the parts different from the method for preparing the connection structure involved in the first embodiment are described here.

[0102] [Method for producing a connected structure]

[0103] use Figure 7 , a method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figure 7 Detailed description will be given of a method for forming the connection structure 100 .

[0104] First, a plurality of conductive particles 10 and a first composition 20' are arranged in a given area on the first electrode 110. The plurality of conductive particles 10 and the first composition 20' are mixed and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, it is particularly preferred to use a pad printing method of a pad transfer printing material. The area and method for arranging the mixture of the plurality of conductive particles 10 and the first composition 20' are the same as the method for preparing the connection structure involved in the first embodiment, so the description is omitted here.

[0105] Figure 7 (A) to (B) show the process of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the pad 230 to the first electrode 110 by pad printing. Figure 7As shown in (A) to (B), the mixture of the conductive particles 10 and the first composition 20' transferred to the glue head 230 is transferred to the first electrode 110 by pushing the glue head 230 in a direction substantially perpendicular to the first electrode 110 and pulling the glue head 230 away in a direction substantially perpendicular to the first electrode 110. On the first surface of the first member 102, the conductive particles 10 and the first composition 20' form a convex structure in the direction opposite to the electrodes (D1 direction). Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP or more and 5×10 5 Since the range of cP or less is 0.1, the conductive particles 10 mixed in the first composition 20' can be held on the first electrode 110. By using such a method, the conductive particles 10 and the first composition 20' can be reliably arranged in a predetermined region on the first electrode 110.

[0106] Next, the second composition 30' is disposed on the second surface of the second member 112. Figure 7 As shown in (C) to (D), the second composition 30' is arranged in an area other than the second electrode 114 on the second surface of the second member 112. Furthermore, the second composition 30' is also arranged in an area other than the area on the second electrode 114 where a plurality of conductive particles 10 and the first composition 20' are arranged as described below. That is, the second composition 30' is arranged on the second surface of the second member 112 in an area other than the area where a plurality of conductive particles 10 and the first composition 20' are arranged. On the second surface of the second member 112, the second composition 30' forms a convex structure in the opposite direction of the electrodes (D1 direction). Although not shown in the figure, in this embodiment, the second composition 30' is arranged using a pad printing method. However, it is not limited to this, and the method of arranging the second composition 30' can use an existing method as long as it can be coated differently from the area other than the area where a plurality of conductive particles 10 and the first composition 20' are arranged. For example, inkjet or coating using a dispenser, offset printing, etc. can be used.

[0107] The viscosity of the second composition 30' is 2×10 3 cP or more and 2×10 5 This can suppress the flow of the second composition 30'.

[0108] Next, the second electronic component 111 is mounted on the first surface of the first electronic component 101. Figure 7As shown in (E), the first surface of the first member 102 and the second surface of the second member 112 are arranged to face each other in such a manner that the corresponding plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposed. The first composition 20' forming a convex structure on the first surface of the first member 102 and the conductive particles 10 are embedded by means of the second composition 30' forming a convex structure on the second surface of the second member 112. The first member 102 and the second member 112 are pressed so that the first surface of the first member 102 and the second surface of the second member 112 are pressed in a direction substantially perpendicular to the respective surfaces. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20', and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because of its higher viscosity than the second composition 30'. The conductive particles 10 and the first composition 20 ′ disposed on the first electrode 110 are in contact with the second electrode 114 , and the second composition 30 ′ disposed on the second surface other than the second electrode 114 is in contact with the first surface other than the first electrode 110 .

[0109] like Figure 7 As shown in (F), the first member 102 and the second member 112 are further pressed, so that the first surface of the first member 102 and the second surface of the second member 112 are pushed in the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower parts of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'. By adopting such a structure, the first electrode 110 and the second electrode 114 can be electrically connected.

[0110] In a state where the first member 102 and the second member 112 are pressed, the connection structure 100 is irradiated with light to cure the first composition 20' and the second composition 30'. The method for curing the first composition 20' and the second composition 30' is the same as the method for preparing the connection structure involved in the first embodiment, so the description is omitted here. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting such a structure, the first surface of the first electronic component 101 and the second surface of the second electronic component 111 can be physically connected.

[0111] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged in the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.

[0112] <Fourth embodiment>

[0113] The structure of the connection structure involved in this embodiment is the same as that of the connection structure involved in the first embodiment. The method for producing the connection structure involved in this embodiment is the same as the method for producing the connection structure involved in the first embodiment, except that the second composition 30' is arranged in the area other than the first electrode 110 of the first member 102, and the plurality of conductive particles 10 and the first composition 20' are arranged on the second electrode 114 of the second member 112. The same description as that of the first embodiment is omitted, and only the parts different from the method for producing the connection structure involved in the first embodiment are described here.

[0114] [Method for producing a connected structure]

[0115] use Figure 8 A method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figure 8 Detailed description will be given of a method for forming the connection structure 100 .

[0116] First, the second composition 30' is disposed on the first surface of the first member 102. Figure 8As shown in (A) to (B), the second composition 30' is arranged in an area other than the first electrode 110 on the first surface of the first member 102. Furthermore, the second composition 30' is also arranged in an area other than the area on the first electrode 110 where a plurality of conductive particles 10 and the first composition 20' are arranged as described below. That is, the second composition 30' is arranged on the first surface of the first member 102 in an area other than the area where a plurality of conductive particles 10 and the first composition 20' are arranged. On the first surface of the first member 102, the second composition 30' forms a convex structure in the opposite direction of the electrodes (D1 direction). Although not shown in the figure, in this embodiment, the second composition 30' is arranged using a pad printing method. However, it is not limited to this, and the method of configuring the second composition 30' can use an existing method as long as it can be coated differently from the area other than the area where a plurality of conductive particles 10 and the first composition 20' are arranged. For example, inkjet or coating using a dispenser, offset printing, etc. can be used.

[0117] The viscosity of the second composition 30' is 2×10 3 cP or more and 2×10 5 This can suppress the flow of the second composition 30'.

[0118] Next, a plurality of conductive particles 10 and a first composition 20' are arranged in a given area on the second electrode 114. The plurality of conductive particles 10 and the first composition 20' are mixed and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, it is particularly preferred to use a pad printing method of a pad transfer printing material. The area and method for arranging the mixture of the plurality of conductive particles 10 and the first composition 20' are the same as the method for preparing the connection structure involved in the first embodiment, so the description is omitted here.

[0119] Figure 8 (C) to (D) represent the process of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the pad 230 to the second electrode 114 by pad printing. Figure 8 As shown in (C) to (D), the mixture of the conductive particles 10 and the first composition 20' transferred to the glue head 230 is transferred to the second electrode 114 by pushing the glue head 230 in a direction substantially perpendicular to the second electrode 114 and pulling the glue head 230 away in a direction substantially perpendicular to the second electrode 114. On the second surface of the second member 112, the conductive particles 10 and the first composition 20' form a convex structure in the direction opposite to the electrodes (D1 direction). Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP or more and 5×10 5Since the range of cP or less is 1.5 cP, the conductive particles 10 mixed in the first composition 20' can be held on the second electrode 114. By using such a method, the conductive particles 10 and the first composition 20' can be accurately arranged in a predetermined region on the second electrode 114.

[0120] Next, the second electronic component 111 is mounted on the first surface of the first electronic component 101. Figure 8 As shown in (E), the first surface of the first member 102 and the second surface of the second member 112 are arranged to face each other in such a manner that the corresponding plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposed. The second composition 30' forming a convex structure on the first surface of the first member 102 is embedded by means of the first composition 20' forming a convex structure on the second surface of the second member 112 and the conductive particles 10. The first member 102 and the second member 112 are pressed so that the first surface of the first member 102 and the second surface of the second member 112 are pressed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20', and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because of its higher viscosity than the second composition 30'. The conductive particles 10 and the first composition 20 ′ disposed on the second electrode 114 are disposed in contact with the first electrode 110 , and the second composition 30 ′ disposed in a region other than the first electrode 110 on the first surface is disposed in contact with a region other than the second electrode 114 on the second surface.

[0121] like Figure 8 As shown in (F), the first member 102 and the second member 112 are further pressed, so that the first surface of the first member 102 and the second surface of the second member 112 are pushed in the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower parts of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'. By adopting such a structure, the first electrode 110 and the second electrode 114 can be electrically connected.

[0122] In a state where the first member 102 and the second member 112 are pressed, the connection structure 100 is irradiated with light to cure the first composition 20' and the second composition 30'. The method for curing the first composition 20' and the second composition 30' is the same as the method for preparing the connection structure involved in the first embodiment, so the description is omitted here. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting such a structure, the first surface of the first electronic component 101 and the second surface of the second electronic component 111 can be physically connected.

[0123] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged in the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.

[0124] <Fifth embodiment>

[0125] The structure of the connection structure according to this embodiment is the same as that of the connection structure according to the first embodiment except that the region where the second resin 30 is disposed contains insulating particles 40. The same description as that of the first embodiment is omitted, and only the parts different from the connection structure according to the first embodiment are described here.

[0126] [Structure of the connection structure]

[0127] Fig. 9 The structure of a connection structure according to one embodiment of the present invention is shown. Fig. 9 (A) is a plan view of a connection structure according to one embodiment of the present invention. Fig. 9 (B) Yes Fig. 9 (A) D-D' cross-section. Fig. 9 (C) Yes Fig. 9 (B) is an enlarged cross-sectional view of the conductive particles in the region E.

[0128] like Fig. 9 As shown in (A) and (B), the connection structure 100a involved in this embodiment includes the first surface of the first member 102, the first electrode 110, the second surface of the second member 112, the second electrode 114, the conductive particles 10, the first resin 20, the second resin 30, and the insulating particles 40.

[0129] The second resin 30 and the plurality of insulating particles 40 are arranged between the first surface of the first member 102 and the second surface of the second member 112. The second resin 30 and the plurality of insulating particles 40 are arranged in a region other than between the first electrode 110 and the second electrode 114 facing each other. The second resin 30 and the plurality of insulating particles 40 are arranged between the region other than the first electrode of the first surface and the region other than the second electrode of the second surface. That is, the second resin 30 and the plurality of insulating particles 40 are arranged between and around the plurality of first electrodes 110 adjacent in the plane direction (D2-D3 plane direction) (between and around the plurality of second electrodes 114 adjacent in the plane direction). Furthermore, the second resin 30 and the insulating particles 40 are also arranged in a region other than the region where the conductive particles 10 and the first resin 20 are arranged between the first electrode 110 and the second electrode 114. The second resin 30 and the insulating particles 40 are arranged between and around the regions where the plurality of conductive particles 10 and the first resin 20 are arranged adjacent to each other in the plane direction (D2-D3 plane direction). The plurality of insulating particles 40 are dispersed in the second resin 30. When viewed in the direction opposite to the electrodes (D1 direction), each conductive particle 10 is surrounded by the first resin 20, and each insulating particle 40 is surrounded by the second resin 30. Furthermore, the conductive particles 10 and the first resin 20 are surrounded by the second resin 30 and the insulating particles 40 in the plane direction (D2-D3 plane direction).

[0130] In the area between the first and second opposing surfaces, other than the area where the conductive particles 10 and the first resin 20 are arranged, a plurality of insulating particles 40 are arranged in the surface direction (D2-D3 surface direction). In the area between the first and second opposing surfaces, other than the area where the conductive particles 10 and the first resin 20 are arranged, one insulating particle 40 is arranged in the opposing direction (D1 direction) between the first and second surfaces. Each insulating particle 40 may also contact the first and second opposing surfaces. The insulating particles 40 may also be deformed by applying pressure to the opposing direction (D1 direction) of the electrodes between the first and second surfaces using the method for making a connection structure. By applying stress between the first surface, the insulating particles 40, and the second surface, the stress applied between the first electrode 110, the conductive particles 10, and the second electrode 114 can be dispersed, thereby further improving the reliability of the connection structure 100a.

[0131] The insulating particles 40 contained in the connection structure 100a may also be spherical. The diameter (major diameter) of the insulating particles 40 observed in the opposite direction of the electrode (D1 direction) may also be in the range of 0.1 μm or more and 10 μm or less. There is no particular limitation on the material of the insulating particles 40, and it can be appropriately selected from well-known insulating particles. The diameter (major diameter) of the insulating particles 40 can be appropriately selected from the range according to the size and material of the conductive particles 10, the material of the first composition 20' and the second composition 30', the viscosity, the method for making the connection structure, etc.

[0132] exist Fig. 9 In the figure, the insulating particles 40 contained in the connection structure 100a are shown as spherical, but may also be fibrous, for example. Cellulose nanofibers may also be used as the material of the insulating particles 40. By using such insulating particles 40, the strength and rigidity against peeling are improved, and the reliability of the physical connection between the first electronic component 101 and the second electronic component 111 is improved.

[0133] When observing the opposing direction of the electrodes (D1 direction), the concentration of the insulating particles 40 in the region other than the region where the conductive particles 10 and the first resin 20 are arranged between the opposing first and second surfaces is preferably in the range of 10 volume % or more and 50 volume % or less relative to the total volume of the insulating particles 40 and the second composition 30'. By configuring in this way, the insulating particles 40 can prevent short circuits between a plurality of first electrodes 110 adjacent in the surface direction (D2-D3 surface direction), between a plurality of second electrodes 114 adjacent in the surface direction (D2-D3 surface direction), and between the first electrode 110 and the second electrode 114 not facing each other. In addition, the flow of the conductive particles 10 mixed in the first composition 20' can be suppressed, so that the conductive particles 10 are efficiently arranged between the first electrode 110 and the second electrode 114. Therefore, the insulation reliability and connection reliability of the connection structure 100a can be ensured.

[0134] [Method for producing a connected structure]

[0135] The method for preparing a connection structure according to an embodiment of the present invention is the same as the method for preparing a connection structure according to the first embodiment, except that a mixture of a plurality of insulating particles 40 and a second composition 30' is arranged instead of the second composition 30'. The same description as the first embodiment is omitted, and only the parts different from the method for preparing a connection structure according to the first embodiment are described here. In addition, this embodiment is not limited to this, and can also be applied to the second to fourth embodiments.

[0136] The plurality of insulating particles 40 are mixed with the second composition 30' and arranged by offset printing. Since the mixture of the insulating particles 40 and the second composition 30' contains the insulating particles 40, pad printing using a pad transfer printing material is particularly preferred.

[0137] The concentration of the insulating particles 40 mixed in the second composition 30' is preferably in a range of 10% by volume or more and 50% by volume or less relative to the total volume of the insulating particles 40 and the second composition 30'. When the amount of the insulating particles 40 is less than 10% by volume, it is difficult to configure a sufficient number of insulating particles 40. When the amount of the insulating particles 40 is greater than 50% by volume, the operability deteriorates and it is difficult to configure the mixture of the insulating particles 40 and the second composition 30'. The method of configuring the mixture of the plurality of insulating particles 40 and the second composition 30' is the same as the method of configuring the mixture of the plurality of conductive particles 10 and the first composition 20', so the description is omitted here.

[0138] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure conductivity between opposing electrodes and suppress short circuits between adjacent connection electrodes through a simple process even if electrodes arranged in an electronic component are highly refined and highly dense.

[0139] <Sixth embodiment>

[0140] The structure of the connection structure according to this embodiment is the same as that of the connection structure according to the first embodiment except that the region where the first resin 20 is disposed further includes conductive nanoparticles 50. The same description as that of the first embodiment is omitted, and only the parts different from those of the connection structure according to the first embodiment are described here.

[0141] [Structure of the connection structure]

[0142] Fig.10 The structure of a connection structure according to one embodiment of the present invention is shown. Fig.10 (A) is a plan view of a connection structure according to one embodiment of the present invention. Fig.10 (B) Yes Fig.10 (A) F-F' cross-section. Fig.10 (C) Yes Fig.10 (B) is an enlarged cross-sectional view of the conductive particles in the region G.

[0143] like Fig.10As shown in (A) and (B), the connection structure 100 b according to this embodiment includes the first surface of the first member 102 , the first electrode 110 , the second surface of the second member 112 , the second electrode 114 , the conductive particles 10 , the first resin 20 , the second resin 30 , and the conductive nanoparticles 50 .

[0144] A plurality of conductive particles 10, a plurality of conductive nanoparticles 50, and a first resin 20 are arranged between the first electrode 110 and the second electrode 114 that are opposite to each other. A plurality of conductive particles 10 and a plurality of conductive nanoparticles 50 are arranged in a plane direction (D2-D3 plane direction) between the first electrode 110 and the second electrode 114 that are opposite to each other. One conductive particle 10 and a plurality of conductive nanoparticles 50 are arranged in a direction of facing the electrodes (D1 direction) between the first electrode 110 and the second electrode 114 that are opposite to each other. Each conductive particle 10 contacts a plurality of conductive nanoparticles 50, the first electrode 110 and the second electrode 114 that are opposite to each other. Fig.10 As shown in (C), the conductive particle 10 is deformed by pressure between the first electrode 110 and the second electrode 114 along the opposing direction of the electrodes (D1 direction) by using the method for producing a connected structure. At this time, a plurality of conductive nanoparticles 50 may be arranged between the conductive particle 10 and the first electrode 110, or between the conductive particle 10 and the second electrode 114. The distance between the first electrode 110 and the second electrode 114 in the opposing direction of the electrodes (D1 direction) is substantially the same as the height of the conductive particle 10 in the opposing direction of the electrodes (D1 direction). When stress is applied between the first electrode 110, the conductive particle 10, and the second electrode 114, a plurality of conductive nanoparticles 50 may be arranged at the contact portion between the first electrode 110 and the conductive particle 10, and at the contact portion between the second electrode 114 and the conductive particle 10. Even if a natural oxide film is formed on the first electrode 110, the conductive particles 10, or the second electrode 114 and the surface is insulated, by arranging a plurality of conductive nanoparticles 50 when the first electrode 110 and the second electrode 114 are crimped with the conductive particles 10 sandwiched therebetween, it is possible to break through the films and form a conductive path. Furthermore, by arranging a plurality of conductive nanoparticles 50, it is possible to increase the contact area between the first electrode 110 and the conductive particles 10, and the contact area between the second electrode 114 and the conductive particles 10. By arranging a plurality of conductive nanoparticles 50 in this way, the conductive particles 10 can more reliably connect the first electrode 110 and the second electrode 114, thereby improving the connection reliability of the connection structure 100b.

[0145] A plurality of conductive particles 10 and a plurality of conductive nanoparticles 50 are dispersed in the first resin 20 between the first electrode 110 and the second electrode 114. Each conductive nanoparticle 50 and conductive particle 10 is surrounded by the first resin 20 between the first electrode 110 and the second electrode 114. The first resin 20 is an insulating resin. Therefore, the connection structure 100b has insulating properties in the surface direction (D2-D3 surface direction). However, the plurality of conductive nanoparticles 50 may also contact a plurality of conductive particles 10 that are arranged between the first electrode 110 and the second electrode 114 facing each other and are adjacent in the surface direction (D2-D3 surface direction). When the conductive particles 10 that are adjacent in the surface direction (D2-D3 surface direction) contact the plurality of conductive nanoparticles 50, the electrical connection of the adjacent conductive particles 10 can be improved. By configuring in this way, the conductive particles 10 and the conductive nanoparticles 50 can more reliably electrically connect the first electrode 110 and the second electrode 114 facing each other.

[0146] The conductive nanoparticles 50 included in the connection structure 100b may also be spherical. The diameter of the conductive nanoparticles 50 may also be 10 -3 μm or more and 10 -1 μm or less. As the material of the conductive nanoparticles 50, it can be appropriately selected from well-known conductive particles. As the material of the conductive nanoparticles 50, Ni-based nanoparticles that are not easily oxidized and have little migration are preferred, but Cu-based nanoparticles can also be used. It can also be a core & shell structured nanoparticle whose core is a Cu-based metal and whose shell is formed by a Ni-type metal. The diameter and material of the conductive nanoparticles 50 can be appropriately selected from the above range according to the size and material of the conductive particles 10, the material of the first composition 20' and the second composition 30', the viscosity, the method for preparing the connected structure, etc.

[0147] [Method for producing a connected structure]

[0148] The method for preparing a connection structure according to one embodiment of the present invention is the same as the method for preparing a connection structure according to the first embodiment except that a mixture of a plurality of conductive particles 10, a plurality of conductive nanoparticles 50 and a first composition 20' is arranged instead of a plurality of conductive particles 10 and a first composition 20'. The same description as the first embodiment is omitted, and only the parts different from the method for preparing a connection structure according to the first embodiment are described here. In addition, this embodiment is not limited to this, and can also be applied to the second embodiment to the fourth embodiment.

[0149] The conductive particles 10, conductive nanoparticles 50 and the first composition 20' are mixed and arranged by offset printing. Since the mixture of the conductive particles 10, conductive nanoparticles 50 and the first composition 20' contains the conductive particles 10, pad printing using a pad transfer printing material is particularly preferred.

[0150] The concentration of the conductive nanoparticles 50 mixed in the first composition 20' is preferably in a range of 0.1% by weight or more and 10% by weight or less relative to the total volume of the plurality of conductive particles 10, the plurality of conductive nanoparticles 50 and the first composition 20'. When the amount of the conductive nanoparticles 50 blended is less than 0.1% by weight, it is difficult to configure a sufficient number of the conductive nanoparticles 50. When the amount of the conductive nanoparticles 50 blended is greater than 10% by weight, the operability deteriorates, making it difficult to configure the mixture of the plurality of conductive particles 10, the plurality of conductive nanoparticles 50 and the first composition 20'. The method of configuring the mixture of the plurality of conductive particles 10, the plurality of conductive nanoparticles 50 and the first composition 20' is the same as the method of configuring the mixture of the plurality of conductive particles 10 and the first composition 20', so the description is omitted here.

[0151] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure conductivity between opposing electrodes and suppress short circuits between adjacent connection electrodes through a simple process even if electrodes arranged in an electronic component are highly refined and highly dense.

[0152] The present invention is not limited to the above-described embodiments, and can be appropriately modified within the scope of the gist. In addition, the various embodiments can be appropriately combined.

[0153] [Example 1]

[0154] Fig.11 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.11 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 1 of the present invention. Fig.11 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure according to Example 1 of the present invention. The parameters of the connection structure of Example 1 are as follows.

[0155] Width (short side) of first electrode 110 (A1) = 12 μm

[0156] Distance between first electrodes 110 (B1) = 9 μm

[0157] · Span of the first electrode 110 (A1+B1=C1)=21 μm

[0158] Length (long side) of first electrode 110 (D1) = 84 μm

[0159] Area of ​​the first electrode 110 (A1×D1)=1008 μm 2

[0160] · Area of ​​one region where the conductive particles 10 and the first resin 20 are arranged = 64 μm 2

[0161] Total area of ​​the region where the conductive particles 10 and the first resin 20 are arranged per electrode = 448 μm 2

[0162] The number of regions where the conductive particles 10 and the first resin 20 are arranged per electrode = 7

[0163] The number of conductive particles 10 arranged per region where the conductive particles 10 and the first resin 20 are arranged = 3

[0164] The number of conductive particles 10 arranged per one electrode = 21 particles.

[0165] [Example 2]

[0166] Fig.12 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.12 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 2 of the present invention. Fig.12 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure according to Example 2 of the present invention. The parameters of the connection structure of Example 2 are as follows.

[0167] Width (short side) of first electrode 110 (A2) = 9 μm

[0168] Distance between first electrodes 110 (B2) = 6 μm

[0169] · Span of the first electrode 110 (A2+B2=C2)=15 μm

[0170] Length (long side) of first electrode 110 (D2) = 78 μm

[0171] The area of ​​the first electrode 110 (A2×D2)=702 μm 2

[0172] · Area of ​​one region where the conductive particles 10 and the first resin 20 are arranged = 40 μm 2

[0173] Total area of ​​the region where the conductive particles 10 and the first resin 20 are arranged per electrode = 280 μm 2

[0174] The number of regions where the conductive particles 10 and the first resin 20 are arranged per electrode = 7

[0175] The number of conductive particles 10 arranged per region where the conductive particles 10 and the first resin 20 are arranged = 2

[0176] The number of conductive particles 10 arranged per electrode = 14 particles.

[0177] [Example 3]

[0178] Fig.13 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.13 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 3 of the present invention. Fig.13 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure according to Example 3 of the present invention. The parameters of the connection structure of Example 3 are as follows.

[0179] Width (short side) of first electrode 110 (A3) = 12 μm

[0180] Distance between first electrodes 110 (B3) = 9 μm

[0181] · Span of the first electrode 110 (A3+B3=C3) = 21 μm

[0182] Length (long side) of first electrode 110 (D3) = 105 μm

[0183] Area of ​​the first electrode 110 (A3×D3)=1260 μm 2

[0184] · Area of ​​one region where the conductive particles 10 and the first resin 20 are arranged = 113 μm 2

[0185] Total area of ​​the region where the conductive particles 10 and the first resin 20 are arranged per electrode = 791 μm 2

[0186] The number of regions where the conductive particles 10 and the first resin 20 are arranged per electrode = 7

[0187] The number of conductive particles 10 arranged per region where the conductive particles 10 and the first resin 20 are arranged = 7

[0188] The number of conductive particles 10 disposed per first electrode 110 = 49 particles.

[0189] [Example 4]

[0190] Fig.14 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.14 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 4 of the present invention. Fig.14 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure according to Example 4 of the present invention. The parameters of the connection structure of Example 4 are as follows.

[0191] Width (short side) of first electrode 110 (A4) = 9 μm

[0192] Distance between first electrodes 110 (B4) = 6 μm

[0193] · Span of the first electrode 110 (A4+B4=C4) = 15 μm

[0194] Length (long side) of first electrode 110 (D4) = 84 μm

[0195] The area of ​​the first electrode 110 (A4×D4)=756 μm 2

[0196] · Area of ​​one region where the conductive particles 10 and the first resin 20 are arranged = 64 μm 2

[0197] Total area of ​​the region where the conductive particles 10 and the first resin 20 are arranged per electrode = 448 μm 2

[0198] The number of regions where the conductive particles 10 and the first resin 20 are arranged per electrode = 7

[0199] The number of conductive particles 10 arranged per region where the conductive particles 10 and the first resin 20 are arranged = 3

[0200] The number of conductive particles 10 arranged per one electrode = 21 particles.

[0201] [Example 5]

[0202] Fig.15 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.15 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 5 of the present invention. Fig.15 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure according to Example 5 of the present invention. The parameters of the connection structure of Example 5 are as follows.

[0203] Width (short side) of first electrode 110 (A5) = 21 μm

[0204] Distance between first electrodes 110 (B5) = 10 μm

[0205] · Span of the first electrode 110 (A5+B5=C5)=31 μm

[0206] · Length (long side) of first electrode 110 (D5) = 21 μm

[0207] Area of ​​the first electrode 110 (A5×D5)=441 μm 2

[0208] · Area of ​​region α where conductive particles 10 and first resin 20 are arranged = 64 μm 2

[0209] Total area of ​​region α where conductive particles 10 and first resin 20 are arranged per electrode = 128 μm 2

[0210] The number of regions α where the conductive particles 10 and the first resin 20 are arranged = 2

[0211] The number of conductive particles 10 arranged in each region α = 3

[0212] · Area of ​​region β where conductive particles 10 and first resin 20 are arranged = 40 μm 2

[0213] Total area of ​​region β where conductive particles 10 and first resin 20 are arranged per electrode = 80 μm

[0214] The number of regions β where the conductive particles 10 and the first resin 20 are arranged = 2

[0215] The number of conductive particles 10 arranged in each region β = 2

[0216] The number of conductive particles 10 arranged per one electrode = 10 particles.

[0217] [Example 6]

[0218] Fig.16 It is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.16 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 6 of the present invention. Fig.16 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure according to Example 6 of the present invention. The parameters of the connection structure of Example 6 are as follows.

[0219] Width (short side) of first electrode 110 (A6) = 15 μm

[0220] Distance between first electrodes 110 (B6) = 10 μm

[0221] · Span of the first electrode 110 (A6+B6=C6)=25 μm

[0222] · Length (long side) of first electrode 110 (D6) = 30 μm

[0223] Area of ​​the first electrode 110 (A6×D6)=450 μm 2

[0224] · Area of ​​one region where the conductive particles 10 and the first resin 20 are arranged = 113 μm 2

[0225] Total area of ​​the region where the conductive particles 10 and the first resin 20 are arranged per electrode = 226 μm 2

[0226] The number of regions where the conductive particles 10 and the first resin 20 are arranged per electrode = 2

[0227] The number of conductive particles 10 arranged per region where the conductive particles 10 and the first resin 20 are arranged = 7

[0228] The number of conductive particles 10 arranged per one electrode = 14 particles.

[0229] As shown in Examples 1 to 6, according to one embodiment of the present invention, even if electrodes arranged in electronic components are highly refined and highly dense, conductivity between opposing electrodes can be ensured by a simple process and short circuits between adjacent electrodes can be suppressed.

[0230] Explanation of symbols

[0231] 10 Conductive particles

[0232] 20 1st resin

[0233] 20' Composition 1

[0234] 30 2nd resin

[0235] 30' Composition 2

[0236] 40 Insulating particles

[0237] 50 Conductive Nanoparticles

[0238] 100, 100a, 100b connection structure

[0239] 101 No.1 Electronic Components

[0240] 102 Component 1

[0241] 104 terminal

[0242] 106 1st insulating film

[0243] 108 Second insulating film

[0244] 110 1st electrode

[0245] 111 Second Electronic Components

[0246] 112 Component 2

[0247] 114 Second electrode

[0248] 210 Roller

[0249] 220 Printing Plate

[0250] 222 Lyophilic layer

[0251] 224 Liquid-repellent layer

[0252] 226 concavity

[0253] 230 Rubber Head

Claims

1. A method for manufacturing a connection structure, comprising: On the first electrode disposed on the first surface of the first member, a first composition containing conductive particles is divided into a plurality of regions and disposed such that the number of the conductive particles in each region is 1 or more and 7 or less, The second composition is arranged in a region other than a region on the first surface where the first composition is arranged, The second electrode disposed on the second surface of the second member is disposed opposite to the first electrode. The first member and the second member are pressed so that the conductive particles come into contact with the first electrode and the second electrode in a state where the first composition containing the conductive particles is sandwiched between the first electrode and the second electrode, and The first composition and the second composition are cured in a state where the conductive particles are in contact with the first electrode and the second electrode.

2. A method for manufacturing a connection structure, comprising: The second composition is disposed in a region other than the first electrode disposed on the first surface of the first member and in a region other than the plurality of regions on the first electrode. On the first electrode, the first composition containing conductive particles is divided into the plurality of regions and arranged such that the number of the conductive particles in each region is 1 or more and 7 or less, The second electrode disposed on the second surface of the second member is disposed opposite to the first electrode. The first member and the second member are pressed so that the conductive particles come into contact with the first electrode and the second electrode in a state where the first composition containing the conductive particles is sandwiched between the first electrode and the second electrode, and The first composition and the second composition are cured in a state where the conductive particles are in contact with the first electrode and the second electrode.

3. A method for manufacturing a connection structure, comprising: On the first electrode disposed on the first surface of the first member, a first composition containing conductive particles is divided into a plurality of regions and disposed such that the number of the conductive particles in each region is 1 or more and 7 or less, The second composition is disposed in a region other than the second electrode disposed on the second surface of the second member and in a region other than the region corresponding to the plurality of regions on the second electrode. The second electrode is arranged opposite to the first electrode. The first member and the second member are pressed so that the conductive particles come into contact with the first electrode and the second electrode in a state where the first composition containing the conductive particles is sandwiched between the first electrode and the second electrode, and The first composition and the second composition are cured in a state where the conductive particles are in contact with the first electrode and the second electrode.

4. A method for manufacturing a connection structure, comprising: The second composition is disposed in a region other than the first electrode disposed on the first surface of the first member and in a region other than the plurality of regions on the first electrode. On the second electrode disposed on the second surface of the second member, the first composition containing conductive particles is divided into regions corresponding to the plurality of regions so that the number of the conductive particles in each region is 1 or more and 7 or less, The second electrode is arranged opposite to the first electrode. The first member and the second member are pressed so that the conductive particles come into contact with the first electrode and the second electrode in a state where the first composition containing the conductive particles is sandwiched between the first electrode and the second electrode, and The first composition and the second composition are cured in a state where the conductive particles are in contact with the first electrode and the second electrode.

5. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition containing the conductive particles is divided into the plurality of regions and arranged so that the conductive particles are arranged at a size of 400 μm per region. 2 At least 7 or more and 20 or less are arranged on the first electrode.

6. The method for manufacturing a connection structure according to claim 5, wherein: The first composition contacts the first electrode and the second electrode.

7. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The conductive particles and the first composition are arranged by offset printing.

8. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The conductive particles and the first composition are arranged by pad printing.

9. The method for manufacturing a connection structure according to claim 8, wherein: The pad printing method uses a flat plate gravure.

10. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The viscosity of the first composition is higher than the viscosity of the second composition.

11. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The conductive particles are disposed on the first electrode together with the first composition in a state where the conductive particles are mixed in the first composition in an amount ranging from 20% by volume to 60% by volume.

12. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition includes conductive nanoparticles.

13. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition includes a radical polymerizable resin.

14. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The second composition includes an ene / thiol curable resin containing an ethylenically unsaturated compound and a thiol compound, wherein a curing component of at least one of the ethylenically unsaturated compound and the thiol compound is a 9,9-diarylfluorene compound.

15. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition and the second composition contain a photocuring initiating component.

16. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition and the second composition are cured by light irradiation.

17. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition and the second composition contain a shielding portion curable active compound.

18. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition contains an anaerobic curing initiating component.

19. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The second composition contains insulating particles.

20. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The pressing of the first member and the second member is performed simultaneously with the curing of the first composition and the second composition.

21. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The conductive particles are brought into contact with the first electrode and the second electrode by the pressing of the first member and the second member.

22. A connection structure comprising: the first surface of the first component; a first electrode disposed on the first surface; a second surface of the second member, which faces the first surface; a second electrode, which is opposite to the first electrode and is disposed on the second surface; The first resin containing conductive particles is arranged in a plurality of regions between the first electrode and the second electrode so that the number of the conductive particles in each region is not less than 1 and not more than 7; a second resin disposed between a region of the first surface other than the first electrode and a region of the second surface other than the second electrode, and a region other than the plurality of regions between the first electrode and the second electrode; The first resin is different from the second resin.

23. The connection structure according to claim 22, wherein: When viewed in the opposing direction of the first electrode and the second electrode, there are 7 electrodes / 400 μm between the first electrode and the second electrode. 2 More than 20 pieces / 400μm 2 The following ranges include the above-mentioned conductive particles.

Citation Information

Patent Citations

  • Anisotropic conductive film, and connection structure

    JP2015167106A

  • Anisotropic conductive material, connection structure, and connection structure producing method

    CN102484326A

  • Circuit device and its producing method

    CN1532919A

  • Film transistor, wiring substrate, display device and electronic device

    CN1655377A

  • Method for connecting LSI chip

    JP1992253348A