A kind of thermal film and its preparation method

By introducing protective film, isolation layer and intermediate layer into thermal film, using materials such as UV glue and polyvinyl alcohol, the problems of adhesion, insufficient waterproofness and poor scratch resistance are solved, and higher barrier performance is achieved and scratch resistance, improving the effect of image diagnosis.

CN111098618BActive Publication Date: 2024-11-22南阳柯丽尔科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010047617.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-16
Publication Date
2024-11-22
Estimated Expiration
2040-01-16

AI Technical Summary

Technical Problem

During use, existing thermal films have problems such as adhesion, insufficient waterproofness and poor scratch resistance, which affects the image diagnosis effect.

Method used

The thermal film design adopts a multi-layer structure, including a protective film, an isolation layer, an intermediate layer and a thermal layer. The isolation layer is composed of UV glue, an ultraviolet absorber, an antioxidant and a surfactant. The intermediate layer is composed of polyvinyl alcohol, Made of water and surfactant, the film's barrier properties and solvent resistance are improved by the combination of these layers, and the frictional resistance is reduced.

Benefits of technology

It significantly improves the anti-adhesion, barrier properties and scratch resistance of the thermal film, enhances the waterproof performance, ensures the clarity and stability of the image, and avoids adhesion contamination and scratch problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111098618B_ABST
    Figure CN111098618B_ABST
Patent Text Reader

Abstract

The invention discloses a thermal film and a preparation method thereof, and belongs to the technical field of thermal printing materials. A thermal film comprises a substrate, a protective film is arranged on one side of the substrate, a back film is arranged on the other side, a thermal layer is arranged between the protective film and the substrate, and an isolation layer and an intermediate layer are arranged in sequence between the protective film and the thermal layer. The thermal film of the invention does not stick during printing and has good machine passability; at the same time, it has good waterproof performance and excellent scratch resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal printing materials, and in particular relates to a thermal film and a preparation method thereof. Background Art

[0002] Thermal film is a medical film for thermal printing. It is generally imaged using an organic thermal coating. Some films have poor adhesion between the base and the thermal imaging layer. At the same time, the slippery performance and anti-static effect are poor, which leads to adhesion during printing and poor performance during machine passing. Therefore, the back side needs to be coated to improve the slippery performance and anti-static function, which is costly. Compared with general label printers and fax machines, the thermal printers used in image diagnosis have higher print head temperatures and longer printing times when recording, so they provide more heat. During the printing process, the film must be heated and developed by the print head. The substances on the protective layer of the film will inevitably sublimate. The steam condenses near the print head when it is cold. After a long period of accumulation, the print head becomes dirty. In severe cases, the film will have cards, scratches and artifacts, affecting the film's diagnostic effect.

[0003] Patent document with publication number CN108215559A discloses a thermal recording material and a preparation method thereof, wherein the material comprises a transparent support, wherein a base layer, a thermal imaging layer and a protective layer are sequentially arranged on one side of the support, and an adhesive and a removable backing paper are sequentially arranged on the other side of the support. The material is prepared by coating a thermal imaging layer coating liquid and a protective layer coating liquid on the support and drying them, and then coating an adhesive on the other side and then compounding a release paper; the protective layer contains an acrylic resin, a crosslinking agent, a crosslinking agent cosolvent and other auxiliary agents. The thermal recording material coating process of the invention is simple, and the thermal recording material prepared has good transparency, barrier properties and thermal printing adaptability.

[0004] The patent document with publication number CN107267046A discloses a thermal film and its preparation method and application. The first aspect of the present invention provides a thermal film, which includes a protective layer, a thermal imaging layer, a substrate layer, and a back layer from top to bottom; the thermal imaging layer at least includes color-developing microcapsules, dye microcapsules, a color-developing auxiliary agent, and an adhesive. The second aspect of the present invention provides a method for preparing the thermal film, which at least includes the following steps: coating the thermal imaging layer and the back layer on both sides of the substrate layer by coating technology; then coating the protective layer on the other side of the thermal imaging layer, and obtaining the thermal film after drying. The third aspect of the present invention provides the application of thermal film in the field of medical imaging.

[0005] Patent document with publication number CN109734942A discloses a medical thermal film and a preparation method thereof, wherein the film comprises a polyester substrate, one side of the polyester substrate is provided with an antistatic layer, and the other side is provided with an imaging layer and a protective layer in sequence. The present invention solves the problem that the existing thermal film is complicated to prepare and has a high cost. The thermal film preparation method of the present invention is simple and easy to implement, significantly improves production efficiency, and greatly reduces production costs. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a thermal film with better scratch resistance and waterproof performance.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0008] A heat-sensitive film comprises a substrate, a protective film is arranged on one side of the substrate, a back film is arranged on the other side, a heat-sensitive layer is arranged between the protective film and the substrate, and an isolation layer and an intermediate layer are arranged in sequence between the protective film and the heat-sensitive layer.

[0009] Preferably, the raw materials in the isolation layer and their weight parts are composed as follows: 60-80 parts of UV glue, 1-10 parts of ultraviolet absorber, 1-8 parts of antioxidant, 0-8 parts of surfactant, and 5-15 parts of solvent.

[0010] Preferably, the raw materials in the intermediate layer and their weight parts are as follows: 10-20 parts of polyvinyl alcohol, 1-12 parts of water, and 0.5-5 parts of surfactant.

[0011] A method for preparing a thermal film comprises the following steps:

[0012] Step S1: preparing a protective film coating liquid, an isolation layer coating liquid, an intermediate layer coating liquid, a heat-sensitive layer coating liquid and a back film coating liquid respectively;

[0013] Step S2: Install the substrate on the film storage rack of the coating machine as required, start the coating machine, and uniformly coat the heat-sensitive layer coating liquid, the intermediate layer coating liquid, the isolation layer coating liquid and the protective film coating liquid on one side of the substrate in turn, and dry and solidify them; then uniformly coat the back film coating liquid on the other side of the substrate, and dry and solidify them; roll and cut to obtain a finished product.

[0014] Preferably, the isolation layer coating liquid is prepared by weighing UV glue, ultraviolet absorber, antioxidant, surfactant and solvent in sequence, mixing, and emulsifying at high speed for 30-40 minutes.

[0015] Preferably, the intermediate layer coating liquid is prepared by weighing polyvinyl alcohol, water and a surfactant in sequence, mixing them, and emulsifying at a high speed for 30-40 minutes.

[0016] Preferably, the method for preparing the heat-sensitive layer coating solution comprises the following steps:

[0017] 1) Under slow stirring, add colorless dye microcapsules, developer, polyvinyl alcohol, acrylic resin, styrene acrylic emulsion and surfactant in sequence, stirring each time until the raw materials are evenly mixed before adding the next one;

[0018] 2) After all the additions are completed, adjust the viscosity of the coating solution with water;

[0019] 3) Use a wound filter to filter, and let it stand for 4-10 hours under slow stirring to remove bubbles until the bubbles are completely removed, and the coating liquid is obtained.

[0020] Preferably, the step of adjusting the viscosity of the coating liquid with water is to adjust the viscosity of the coating liquid with water to a viscosity of 12-16 seconds as measured by a viscosity cup.

[0021] Preferably, the weight proportions of the raw materials in the heat-sensitive layer are: 5-10 parts of polyvinyl alcohol, 2-5 parts of acrylic resin, 1-5 parts of styrene-acrylic emulsion, 0.5-2 parts of surfactant, and the remainder is colorless dye microcapsules and developer, with a total of 100 parts.

[0022] Preferably, the weight ratio of the colorless dye microcapsules to the developer is 1:(2-7).

[0023] The main structure of existing thermal films is composed of a support, a thermal imaging layer, a protective layer, a back layer (UV absorbing layer), etc. The main problem of thermal films in use lies in the inherent technical problems of direct thermal imaging: contact printing, the film is in close contact with the print head during printing, and there is continuous friction; the actual formation time of the image unit is about 10ms. To achieve a high heat transfer in such a short time, a relatively high pressure must be required between the print head and the film. The design pressure of most medical printers is about 40arm; to ensure the diagnostic effect, the basic requirements of medical imaging films are a maximum density of more than 3.2 and a printing time of about 10ms. Therefore, the actual instantaneous temperature of the print head can reach more than 270°C, and the maximum temperature of some printers with higher requirements can even reach 340-360°C. Although the contact time is short, it is inevitable that the additives on the surface of the film will fall off and contaminate the print head. As the dust, additives and other components on the surface of the film fall off and accumulate on the surface of the print head, the contaminated print head contacts the film, and scratches of different densities will be generated according to the different contamination conditions, affecting the image diagnosis. In order to obtain high-resolution and uniform printed images and disperse the high pressure on the thermal recording layer during film printing, CN200780026224.8 proposes to adhere nano-scale pigment particles to the surface of surface-modified hollow spherical pigment particles. However, these hollow spherical particles are easily adhered during the printing process due to the close contact between the print head and the thermal recording material, thereby increasing the friction resistance during printing; CN03819149.0 proposes that in order to more effectively protect all thermal recording layers under various environments, it is required that the water-based resin and cross-linking agent in the protective layer be combined and cured. Since these cross-linking agents basically complete cross-linking under low temperature conditions, it is difficult to ensure good stability over time after combining with the water-based resin in the protective layer. Therefore, the long-term aging problem caused by coating must be considered. The water-based resin emulsion with a specific composition (copolymer resin emulsion) and structure is applied to the protective layer of the thermal recording material, which can well protect the thermal recording layer from the external environment. It has been recognized that providing a protective layer composed of a water-soluble resin and a cross-linking agent on the thermal recording layer to overcome the apparent disadvantages has been recognized by everyone, but the water resistance is rarely insufficient, and the protective layer is easily dissolved to produce image loss. CN200710148988.6 proposes using diacetone-modified polyvinyl alcohol as the main adhesive of the protective layer, but the viscosity of the solution increases significantly over time, and the water resistance is not greatly improved. In general, both domestic and foreign countries have conducted relatively detailed research on the problems of adhesion, waterproofing and scratching of thermal films during use, and proposed different solutions, but the comprehensive performance of existing thermal films in terms of waterproofing and scratch resistance needs to be improved.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The thermal film of the present invention has excellent anti-scratch performance. Compared with the existing thermal film, in addition to the four-layer structure of the protective film layer, the thermal layer, the substrate and the back film layer, an isolation layer and an intermediate layer are sequentially arranged between the protective film and the thermal layer, and the isolation layer is made of ultraviolet curing glue (UV glue), ultraviolet absorber, antioxidant and surfactant, which plays the role of preventing the moisture of each layer located below the isolation layer from migrating upward and anti-oxidation and anti-aging; the intermediate layer is made of polyvinyl alcohol, water and surfactant, and the layer has solvent resistance, which plays the role of preventing the solvent located above the intermediate layer from damaging the thermal layer; by adding the isolation layer and the intermediate layer, and matching them with a coating formula of a specific composition, the permeability change of the thermal layer and the protective film layer is greatly reduced, thereby increasing the active ingredients of the surface layer used to protect the thermal layer, improving the barrier performance, being able to solve the adhesion problem to a great extent, reducing the friction resistance during printing, and thus avoiding the adhesion and pollution of the print head due to the shedding of materials, and significantly improving the anti-adhesion performance, barrier performance and anti-scratch performance of the thermal film.

[0026] The thermal film of the present invention has good waterproof property. The existing thermal film generally adopts a protective layer composed of a water-soluble resin and a cross-linking agent to overcome the surface defects, but the water resistance is slightly insufficient and the protective layer is easily dissolved to produce image loss. Therefore, in addition to setting an isolation layer between the protective film and the thermal layer, the present invention also sets an intermediate layer between the isolation layer and the thermal layer. The intermediate layer is made of polyvinyl alcohol, water and a surfactant, has solvent resistance, and prevents the solvent located on the upper part of the intermediate layer from damaging the thermal layer, thereby improving the waterproof performance of the thermal film.

[0027] The maximum density of the thermal film of the present invention is 2.8-2.9, the haze is less than 40%, the transparency is about 64%, and the protective film, the isolation layer, the middle layer, the thermal layer, the substrate and the back film are all well bonded; the thermal film does not stick during the printing process and has good machine passability; at the same time, it has good waterproof performance and excellent scratch resistance. Compared with thermal films of brands such as Fuji, Kodak, and Agfa, it has obvious advantages.

[0028] Instruction Manual

[0029] Figure 1 : A schematic diagram of the structure of the thermal film of the present invention;

[0030] Among them: 1-substrate, 2-protective film, 3-isolation layer, 4-intermediate layer, 5-back film, 6-thermosensitive layer. DETAILED DESCRIPTION

[0031] In order to better understand the present invention, the content of the present invention is further clearly described below in conjunction with the embodiments, but the protection content of the present invention is not limited to the following embodiments. In the following description, a large number of specific details are given in order to provide a more thorough understanding of the present invention.

[0032] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0033] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0034] The present invention provides a thermal film, comprising a substrate 1, a protective film 2 is arranged on one side of the substrate 1, a back film 5 is arranged on the other side, a thermal layer 6 is arranged between the protective film 2 and the substrate 1, and an isolation layer 3 and an intermediate layer 4 are arranged in sequence between the protective film 2 and the thermal layer 6, that is, from top to bottom, the protective film 2, the isolation layer 3, the intermediate layer 4, the thermal layer 6, the substrate 1 and the back film 5 are arranged in sequence.

[0035] Protective film:

[0036] The protective film 2 has UV glue as the main component, and one or more combinations of lubricants, solvents, fillers and surfactants can be added as needed, which can extend the image retention time and reduce the pressure of the print head on the photosensitive layer during thermal processing; and by adding a proper amount of lubricant, filler and / or surfactant to reduce the friction coefficient and improve the lubrication ability, it is ensured that the friction coefficient of the film when it contacts the print head during thermal imaging is reduced, thereby avoiding adhesion and contamination of the print head due to material shedding.

[0037] The present invention does not particularly limit the lubricant, solvent, filler and surfactant used, and the type and amount thereof can be appropriately selected within the scope that does not harm the purpose of the present invention. As a lubricant, it is selected from one of the following or any combination of several: zinc stearate, stearic acid amide, dimethyl silicone oil, polyethylene wax, paraffin. As a solvent, it can be ethyl acetate, ethanol, ethylene glycol, etc. As a filler, it can be inorganic materials such as calcium carbonate, magnesium carbonate, kaolin, aluminum hydroxide, calcined kaolin, clay, nano-silica, etc., or it can be organic materials such as polymethyl methacrylate microspheres (PMMA microspheres). As a surfactant, it is selected from one of the following or any combination of several: BYK-UV3535, BYK-UV3505, BYK-UV3570, BYK-378.

[0038] The raw materials and their weight parts in the protective film are as follows: 75-85 parts of UV glue, 3-8 parts of lubricant, 1-5 parts of filler, 0-5 parts of surfactant, and 7-12 parts of solvent.

[0039] The preparation method of the protective film coating liquid is as follows: the raw materials are mixed and then emulsified at high speed. Preferably, the emulsification time is 30-40 minutes.

[0040] Isolation layer:

[0041] The isolation layer 3 contains at least the following raw materials: UV glue, ultraviolet absorber and antioxidant, and surfactant can be added as needed, and mixed with a suitable solvent. The isolation layer 3 prevents the water in the layers below the isolation layer 3 from migrating upward and has the functions of anti-oxidation and anti-aging.

[0042] The present invention does not particularly limit the UV absorber, antioxidant, surfactant and solvent used to form the isolation layer coating liquid, and the type and amount thereof can be appropriately selected within the scope that does not harm the purpose of the present invention. As the UV absorber, it can be UV-1164, UV-120. As the antioxidant, it can be a phenolic antioxidant, a phosphite, a thioester, etc., such as antioxidant 1010, antioxidant 1076, antioxidant CA, 2,6-di-tert-butyl-4-methylphenol, ICC Dover S-9228. The solvent is water. As the surfactant, it is selected from one of the following or any combination of several: BYK-UV3535, BYK-UV3505, BYK-UV3570, BYK-378.

[0043] The raw materials and their weight parts in the isolation layer are as follows: 60-80 parts of UV glue, 1-10 parts of ultraviolet absorber, 1-8 parts of antioxidant, 0-8 parts of surfactant and 5-15 parts of solvent.

[0044] The isolation layer coating liquid is obtained by weighing the raw materials in sequence, mixing, and emulsifying at high speed. Preferably, the emulsification time is 30-40 minutes.

[0045] Middle layer:

[0046] The intermediate layer 4 contains at least polyvinyl alcohol, and an appropriate amount of surfactant may be added as needed to prepare an aqueous solution. This layer is solvent-resistant and prevents the solvent located on the upper part of the intermediate layer 4 from damaging the heat-sensitive layer 6.

[0047] The present invention does not particularly limit the surfactant used in the intermediate layer coating solution, and its type and amount can be appropriately selected within the range that does not impair the purpose of the present invention. The surfactant is selected from one or a combination of any of the following: sodium perfluorononenyloxybenzenesulfonate (OBS), surfactant 1292, and surfactant 1283.

[0048] The raw materials in the middle layer and their weight parts are as follows: 10-20 parts of polyvinyl alcohol, 1-12 parts of water, and 0.5-5 parts of surfactant.

[0049] The intermediate layer coating liquid is obtained by weighing each raw material in sequence, mixing, and emulsifying at high speed for 30-40 minutes.

[0050] Thermal layer:

[0051] The heat-sensitive layer 6 develops color after being heated and is an imaging layer. The layer contains at least the following raw materials: colorless dye microcapsules, developer, acrylic resin, styrene-acrylic emulsion, and a proper amount of surfactant is added as needed, and the viscosity is adjusted with water.

[0052] The present invention has no particular limitation on the surfactant used to form the heat-sensitive layer coating solution. The surfactant may be sodium perfluorononenyloxybenzenesulfonate (OBS), surfactant 1283, surfactant 1292, or BYK-348.

[0053] The raw materials and their weight parts in the heat-sensitive layer are composed of 5-10 parts of polyvinyl alcohol, 2-5 parts of acrylic resin, 1-5 parts of styrene-acrylic emulsion, 0.5-2 parts of surfactant, and the rest are colorless dye microcapsules and color developer, with a total of 100 parts.

[0054] The weight ratio of the colorless dye microcapsules to the color developer is 1:(2-7).

[0055] The colorless dye microcapsules are prepared by the following method, which specifically includes the following steps:

[0056] S1. Oil phase preparation:

[0057] S11, dissolving the colorless dye 2-phenylamino-3-methyl-6-dibutylaminofluoran in solvent oil, and heating until completely dissolved;

[0058] S12, cooling to room temperature, adding isocyanate and stirring to mix well;

[0059] S2. Preparation of aqueous phase:

[0060] S21, dissolving polyvinyl alcohol in water to prepare an aqueous solution with a mass concentration of 15%-20%;

[0061] S22, take 60 kg of the aqueous solution in step S21, add 40 kg of the oil phase under high-speed emulsification, and emulsify for 20-30 minutes;

[0062] S23, the emulsified dispersion is collected into a stirring kettle, a curing agent is added with low-speed stirring, the temperature is raised to 60° C., and the reaction is carried out for 4-5 hours;

[0063] S24, after the reaction is completed, the particle size is measured, and no color is produced when mixed with a color developer;

[0064] S25. Cool down to room temperature and set aside.

[0065] The above normal temperature refers to: temperature 25° C.-30° C. The unit of mass concentration is: g / ml.

[0066] The solvent oil includes one or more of ethyl acetate, butyl butyrate, α-methylnaphthalene, β-methylnaphthalene, cyclohexanone or dibutyl phthalate, and its main function is to dissolve the colorless dye.

[0067] The curing agent includes one or more of tetraethylenepentamine, diethylenetriamine, hexamethylenediamine, propylene glycol or glycerol, and its main function is to undergo a cross-linking reaction with the liquid wall material, and solidify and form the capsule wall of the microcapsule. The principle is that the amine group or hydroxyl group in the curing agent can undergo a cross-linking reaction with the isocyanate group in the wall material. The reaction process does not involve formaldehyde, and has the advantages of being environmentally friendly and efficient.

[0068] Preferably, the mass ratio of 2-phenylamino-3-methyl-6-dibutylaminofluoran to isocyanate is 1:(1-2); the mass ratio of solvent oil to 2-phenylamino-3-methyl-6-dibutylaminofluoran is (3-4):1; in the aqueous phase, in terms of mass percentage, polyvinyl alcohol is 60-70%, curing agent is 5-10%, and the balance is water.

[0069] The particle size of the leuco dye microcapsules is 0.5-0.7 μm.

[0070] The color developer can be listed as: 4,4′-isopropylidene diphenol, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4′-dihydroxydiphenyl sulfone, 2,4′-dihydroxydiphenyl sulfone, 4-hydroxy-4′-isopropoxydiphenyl sulfone, 3,3′-diallyl-4,4′-dihydroxydiphenyl sulfone, benzyl 4-hydroxybenzoate, N-(p-tolylsulfonyl)-N'-(3-p-tolylsulfonyloxy-phenyl)urea, and color developer H-503.

[0071] The method for preparing a heat-sensitive layer coating liquid comprises the following steps:

[0072] 1) Under slow stirring, add colorless dye microcapsules, developer, polyvinyl alcohol, acrylic resin, styrene acrylic emulsion and surfactant in sequence, stirring each time until the raw materials are evenly mixed before adding the next one;

[0073] 2) After all the additions are completed, adjust the viscosity of the coating solution with water;

[0074] 3) Use a wound filter to filter, and let it stand for 4-10 hours under slow stirring to remove bubbles until the bubbles are completely removed, and the coating liquid is obtained.

[0075] As a preferred embodiment of the present invention, the viscosity of the coating liquid obtained by adjusting the viscosity of the coating liquid with water is to adjust the viscosity of the coating liquid obtained by using water to a viscosity of 12-16 seconds measured by a Tu 4 viscosity cup. Tu 4 viscosity cup is designed according to the requirements of the GB1723-79 national standard coating viscosity determination method, and is a viscosity cup widely used in this field. Under certain temperature conditions, the time for a quantitative sample to flow out of a hole of a specified diameter is measured, expressed in seconds (s). The present invention can be any value between 12-16 seconds.

[0076] Substrate: The substrate 1 is a film support, which is a polyester film base.

[0077] Back film:

[0078] The back film 5 contains at least the following raw materials: acrylic resin, propylene glycol methyl ether acetate (PMA) and polyvinyl alcohol. The raw materials are mixed, water is added, and emulsified to prepare a coating liquid. A proper amount of filler and surfactant can also be added as needed. The filler can be selected from calcium carbonate, magnesium carbonate, kaolin, aluminum hydroxide, calcined kaolin, clay, silicon dioxide, etc., preferably silicon dioxide, so that the back film 5 has good heat resistance in actual use and has a suitable friction coefficient to improve the printing quality. The average particle size of silicon dioxide is selected to be 30-50 nanometers. The surfactant can be sodium perfluorononenyloxybenzenesulfonate (OBS), surfactant 1283, surfactant 1292, BYK-333.

[0079] The raw materials and their weight parts in the back film are composed of 20-40 parts of acrylic resin, 20-40 parts of PMA resin balls, 0-8 parts of fillers, 10-20 parts of polyvinyl alcohol, and 0-10 parts of surfactant.

[0080] The present invention also provides a method for preparing a thermal film, comprising the following steps:

[0081] Step S1: preparing a protective film coating liquid, an isolation layer coating liquid, an intermediate layer coating liquid, a heat-sensitive layer coating liquid and a back film coating liquid respectively;

[0082] Step S2: Install the substrate 1 on the film storage rack of the coating machine as required, start the coating machine, and uniformly coat the heat-sensitive layer coating liquid, the intermediate layer coating liquid, the isolation layer coating liquid and the protective film coating liquid on one side of the substrate 1 in turn, and dry and solidify them; then uniformly coat the back film coating liquid on the other side of the substrate 1, and dry and solidify them; roll and cut to obtain a finished product.

[0083] The coating method of the protective film 2, the isolation layer 3, the intermediate layer 4, the heat-sensitive layer 6 and the back film 5 of the thermal film of the present invention can be one or more combinations of slide extrusion coating, doctor blade coating, curtain coating, reverse roller coating, gravure coating, air knife coating or wire rod coating.

[0084] The following specific examples are given to further illustrate the thermal film of the present invention, but they are not all embodiments of the present invention. "Parts" and "%" in the examples, if not otherwise specified, represent "parts by mass" and "mass percentage" respectively.

[0085] Example 1: Preparation of Leuco Dye Microcapsules

[0086] The preparation method of leuco dye microcapsules comprises the following steps:

[0087] S1. Oil phase preparation:

[0088] S11, dissolving the colorless dye 2-phenylamino-3-methyl-6-dibutylaminofluoran in ethyl acetate, and heating until completely dissolved;

[0089] S12, cooling to room temperature, adding isocyanate and stirring to mix well;

[0090] S2. Preparation of aqueous phase:

[0091] S21, dissolving polyvinyl alcohol in water to prepare an aqueous solution with a mass concentration of 18%;

[0092] S22, taking 60 kg of the aqueous solution in step S21, adding 40 kg of the oil phase under high-speed emulsification, and emulsifying for 25 minutes;

[0093] S23, the emulsified dispersion was placed in a stirring kettle, diethylenetriamine was added with low-speed stirring, the temperature was raised to 60° C., and the reaction was carried out for 4.5 hours;

[0094] S24, after the reaction is completed, the particle size is measured, and no color is produced when mixed with a color developer;

[0095] S25. Cool down to room temperature and set aside.

[0096] Among them, the mass ratio of 2-phenylamino-3-methyl-6-dibutylaminofluoran and isocyanate is 1:1.5; the mass ratio of ethyl acetate to 2-phenylamino-3-methyl-6-dibutylaminofluoran is 3:1; in the aqueous phase, in terms of mass percentage, polyvinyl alcohol is 65%, diethylenetriamine is 7%, and the balance is water.

[0097] The above normal temperature refers to: temperature 25° C.-30° C. The unit of mass concentration is: g / ml.

[0098] The particle size of the leuco dye microcapsules is 0.5-0.7 μm.

[0099] Example 2

[0100] See also Figure 1 A thermal film comprises a substrate 1, a protective film 2 is arranged on one side of the substrate 1, a back film 5 is arranged on the other side, a thermal layer 6 is arranged between the protective film 2 and the substrate 1, and an isolation layer 3 and an intermediate layer 4 are arranged in sequence between the protective film 2 and the thermal layer 6.

[0101] A method for preparing a thermal film comprises the following steps:

[0102] Step S1: preparing a protective film coating liquid, an isolation layer coating liquid, an intermediate layer coating liquid, a heat-sensitive layer coating liquid and a back film coating liquid respectively;

[0103] The protective film coating liquid is obtained by weighing 80 parts of UV glue, 5 parts of dimethyl silicone oil, 10 parts of ethyl acetate and 2 parts of nano silicon dioxide in sequence, mixing, and emulsifying at high speed for 30 minutes;

[0104] The isolation layer coating liquid is obtained by weighing 75 parts of UV glue, 2 parts of ultraviolet absorber UV-1164, 6 parts of antioxidant 1076, 7 parts of surfactant OBS and 12 parts of water in sequence, mixing, and emulsifying at high speed for 30 minutes;

[0105] The intermediate layer coating liquid was obtained by weighing 15 parts of polyvinyl alcohol, 9 parts of water and 2 parts of surfactant OBS in sequence, mixing, and emulsifying at high speed for 30 minutes;

[0106] The heat-sensitive layer coating solution is obtained by the following preparation method:

[0107] 1) Under slow stirring, add 14.3 parts of colorless dye microcapsules, 71.5 parts of 4,4'-isopropylidene diphenol, 7 parts of polyvinyl alcohol, 3 parts of acrylic resin, 3 parts of styrene acrylic emulsion and 1.2 parts of surfactant OBS in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0108] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 12 seconds;

[0109] 3) Filter with a wire-wound filter and allow to stand for 7 hours with slow stirring until the bubbles are completely discharged.

[0110] The back film coating liquid is obtained by weighing 30 parts of acrylic resin, 38 parts of PMA resin beads, 5 parts of silicon dioxide, 15 parts of polyvinyl alcohol and 6 parts of surfactant OBS in sequence, mixing, and emulsifying at high speed for 30 minutes;

[0111] Step S2: Install the substrate 1 on the film storage rack of the coating machine as required, start the coating machine, and uniformly coat the heat-sensitive layer coating liquid, the intermediate layer coating liquid, the isolation layer coating liquid and the protective film coating liquid on one side of the substrate 1 in turn, and dry and solidify them; then uniformly coat the back film coating liquid on the other side of the substrate 1, and dry and solidify them; roll and cut to obtain a finished product.

[0112] Example 3

[0113] The difference between this embodiment and embodiment 1 is that:

[0114] The protective film coating liquid is obtained by weighing 75 parts of UV glue, 3 parts of polyethylene wax, 7 parts of ethanol, 1 part of aluminum hydroxide and 2 parts of BYK-UV3535 in sequence, mixing, and emulsifying at high speed for 35 minutes.

[0115] The isolation layer coating liquid is obtained by weighing 78 parts of UV glue, 5 parts of ultraviolet absorber UV-120, 5 parts of 2,6-di-tert-butyl-4-methylphenol, 8 parts of surfactant OBS and 13 parts of solvent in sequence, mixing, and emulsifying at high speed for 32 minutes.

[0116] The intermediate layer coating liquid was obtained by weighing 18 parts of polyvinyl alcohol, 10 parts of water and 4 parts of surfactant OBS in sequence, mixing them, and emulsifying at a high speed for 35 minutes.

[0117] The heat-sensitive layer coating liquid is obtained by the following preparation method:

[0118] 1) Under slow stirring, add 16.5 parts of colorless dye microcapsules, 66 parts of 1,1-bis(4-hydroxyphenyl)ethane, 8 parts of polyvinyl alcohol, 4 parts of acrylic resin, 4 parts of styrene-acrylic emulsion and 1.5 parts of surfactant OBS in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0119] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 13 seconds;

[0120] 3) Use a wound filter to filter and let it stand for 9 hours with slow stirring to remove bubbles until all the bubbles are completely discharged.

[0121] The back film coating liquid was obtained by weighing 35 parts of acrylic resin, 35 parts of PMA resin beads, 7 parts of silica, 18 parts of polyvinyl alcohol and 8 parts of surfactant OBS in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0122] Example 4

[0123] The difference between this embodiment and embodiment 1 is that:

[0124] The protective film coating liquid is obtained by weighing 85 parts of UV glue, 8 parts of stearic acid amide, 12 parts of ethyl acetate, 5 parts of PMMA microspheres and 3 parts of BYK-UV3505 in sequence, mixing, and emulsifying at high speed for 40 minutes.

[0125] The isolation layer coating liquid is obtained by weighing 80 parts of UV glue, 10 parts of ultraviolet absorber UV-1164, 8 parts of antioxidant CA, 6 parts of surfactant OBS and 15 parts of water in sequence, mixing, and emulsifying at high speed for 35 minutes.

[0126] The intermediate layer coating liquid was obtained by weighing 20 parts of polyvinyl alcohol, 12 parts of water and 5 parts of surfactant OBS in sequence, mixing them, and emulsifying at a high speed for 40 minutes.

[0127] The heat-sensitive layer coating liquid is obtained by the following preparation method:

[0128] 1) Under slow stirring, add 26 parts of colorless dye microcapsules, 52 parts of 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 10 parts of polyvinyl alcohol, 5 parts of acrylic resin, 5 parts of styrene-acrylic emulsion and 2 parts of surfactant OBS in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0129] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 14 seconds;

[0130] 3) Use a wound filter to filter and let it stand for 10 hours with slow stirring to remove bubbles until all the bubbles are completely discharged.

[0131] The back film coating liquid is obtained by weighing 40 parts of acrylic resin, 40 parts of PMA resin beads, 8 parts of silica, 20 parts of polyvinyl alcohol and 10 parts of surfactant OBS in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0132] Example 5

[0133] The difference between this embodiment and embodiment 1 is that:

[0134] The protective film coating liquid is obtained by weighing 82 parts of UV glue, 4 parts of dimethyl silicone oil, 9 parts of ethyl acetate, 2 parts of PMMA microspheres and 5 parts of BYK-UV3570 in sequence, mixing, and emulsifying at high speed for 38 minutes.

[0135] The isolation layer coating liquid is obtained by weighing 70 parts of UV glue, 6 parts of ultraviolet absorber UV-120, 4 parts of 2,6-di-tert-butyl-4-methylphenol and 9 parts of water in sequence, mixing, and emulsifying at high speed for 40 minutes.

[0136] The intermediate layer coating liquid was obtained by weighing 16 parts of polyvinyl alcohol, 8 parts of water and 12833 parts of a surfactant in sequence, mixing them, and emulsifying at a high speed for 35 minutes.

[0137] The heat-sensitive layer coating solution is obtained by the following preparation method:

[0138] 1) Under slow stirring, add 22 parts of colorless dye microcapsules, 65 parts of 2,4'-dihydroxydiphenyl sulfone, 7 parts of polyvinyl alcohol, 3 parts of acrylic resin, 2 parts of styrene-acrylic emulsion and 1 part of surfactant 1283 in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0139] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 15 seconds;

[0140] 3) Use a wound filter to filter and let it stand for 5 hours with slow stirring to remove bubbles until all the bubbles are completely discharged.

[0141] The back film coating liquid was obtained by weighing 28 parts of acrylic resin, 28 parts of PMA resin beads, 2 parts of silica, 15 parts of polyvinyl alcohol and 12835 parts of surfactant in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0142] Example 6

[0143] The difference between this embodiment and embodiment 1 is that:

[0144] The protective film coating liquid is obtained by weighing 78 parts of UV glue, 5 parts of dimethyl silicone oil, 10 parts of ethyl acetate, 3 parts of PMMA microspheres and 4 parts of BYK-UV3570 in sequence, mixing, and emulsifying at high speed for 35 minutes.

[0145] The isolation layer coating liquid is obtained by weighing 68 parts of UV glue, 4 parts of ultraviolet absorber UV-120, 3 parts of antioxidant 1010, 3 parts of surfactant 1292 and 7 parts of water in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0146] The intermediate layer coating liquid was obtained by weighing 12 parts of polyvinyl alcohol, 6 parts of water and 1292 1 part of a surfactant in sequence, mixing them, and emulsifying at a high speed for 38 minutes.

[0147] The heat-sensitive layer coating solution is obtained by the following preparation method:

[0148] 1) Under slow stirring, add 11.5 parts of colorless dye microcapsules, 80 parts of 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, 5 parts of polyvinyl alcohol, 2 parts of acrylic resin, 1 part of styrene-acrylic emulsion and 0.5 parts of surfactant 1292 in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0149] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 16 seconds;

[0150] 3) Use a wound filter to filter and let it stand for 5 hours with slow stirring to remove bubbles until all the bubbles are completely discharged.

[0151] The back film coating liquid was obtained by weighing 26 parts of acrylic resin, 25 parts of PMA resin beads, 4 parts of silica and 13 parts of polyvinyl alcohol in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0152] Example 7

[0153] The difference between this embodiment and embodiment 1 is that:

[0154] The protective film coating liquid is obtained by weighing 76 parts of UV glue, 6 parts of zinc stearate, 11 parts of ethanol, 5 parts of nano-silicon dioxide and 1 part of BYK-378 in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0155] The isolation layer coating liquid is obtained by weighing 65 parts of UV glue, 3 parts of ultraviolet absorber UV-120, 282 parts of ICCDoverS-92, 1 part of surfactant OBS and 6 parts of water in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0156] The intermediate layer coating liquid was obtained by weighing 14 parts of polyvinyl alcohol, 4 parts of water and 0.5 parts of surfactant OBS in sequence, mixing them, and emulsifying at a high speed for 30 minutes.

[0157] The heat-sensitive layer coating solution is obtained by the following preparation method:

[0158] 1) Under slow stirring, add 11.5 parts of colorless dye microcapsules, 80 parts of 4-hydroxybenzoic acid benzyl ester, 6 parts of polyvinyl alcohol, 3 parts of acrylic resin, 3 parts of styrene acrylic emulsion and 0.8 parts of surfactant OBS in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0159] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 15 seconds;

[0160] 3) Use a wire-wound filter to filter, and let it stand for 4 hours with slow stirring to remove bubbles until all the bubbles are completely discharged.

[0161] The back film coating liquid is obtained by weighing 25 parts of acrylic resin, 32 parts of PMA resin beads, 3 parts of silica, 10 parts of polyvinyl alcohol and 3 parts of surfactant OBS in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0162] Example 8

[0163] The difference between this embodiment and embodiment 1 is that:

[0164] The protective film coating liquid is obtained by weighing 83 parts of UV glue, 4 parts of dimethyl silicone oil, 8 parts of ethyl acetate, 4 parts of nano-silicon dioxide and 5 parts of BYK-378 in sequence, mixing, and emulsifying at high speed for 40 minutes.

[0165] The isolation layer coating liquid is obtained by weighing 62 parts of UV glue, 1 part of ultraviolet absorber UV-1164, 1 part of 2,6-di-tert-butyl-4-methylphenol, 2 parts of surfactant OBS and 5 parts of water in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0166] The intermediate layer coating liquid was obtained by weighing 10 parts of polyvinyl alcohol, 2 parts of water and 0.8 parts of surfactant OBS in sequence, mixing them, and emulsifying at a high speed for 30 minutes.

[0167] The heat-sensitive layer coating liquid is obtained by the following preparation method:

[0168] 1) Under slow stirring, add 12 parts of colorless dye microcapsules, 71.4 parts of N-(p-tolylsulfonyl)-N'-(3-p-tolylsulfonyloxy-phenyl)urea, 8 parts of polyvinyl alcohol, 5 parts of acrylic resin, 2 parts of styrene-acrylic emulsion and 1.6 parts of surfactant OBS in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0169] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 14 seconds;

[0170] 3) Use a wound filter to filter and let it stand for 6 hours with slow stirring to remove bubbles until all the bubbles are removed.

[0171] The back film coating liquid was obtained by weighing 23 parts of acrylic resin, 20 parts of PMA resin beads, 12 parts of polyvinyl alcohol and 2 parts of surfactant OBS in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0172] Example 9

[0173] The difference between this embodiment and embodiment 1 is that:

[0174] The protective film coating liquid is obtained by weighing 81 parts of UV glue, 7 parts of polyethylene wax, 9 parts of ethyl acetate, 3 parts of nano-silicon dioxide and 4 parts of BYK-UV3535 in sequence, mixing, and emulsifying at high speed for 35 minutes.

[0175] The isolation layer coating liquid is obtained by weighing 73 parts of UV glue, 9 parts of UV-120, 7 parts of antioxidant CA, 5 parts of surfactant 1283 and 10 parts of water in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0176] The intermediate layer coating liquid was obtained by weighing 10 parts of polyvinyl alcohol, 1 part of water and 2.5 parts of surfactant 1283 in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0177] The heat-sensitive layer coating solution is obtained by the following preparation method:

[0178] 1) While stirring slowly, add 12 parts of colorless dye microcapsules, 71.4 parts of color developer H-503, 9 parts of polyvinyl alcohol, 2 parts of acrylic resin, 3 parts of styrene-acrylic emulsion and 1.8 parts of surfactant 1283 in sequence, stirring each time until the raw materials are evenly added before adding the next one;

[0179] 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 16 seconds;

[0180] 3) Use a wound filter to filter and let it stand for 5 hours with slow stirring to remove bubbles until all the bubbles are completely discharged.

[0181] The back film coating liquid was obtained by weighing 20 parts of acrylic resin, 23 parts of PMA resin beads, 6 parts of silica, 16 parts of polyvinyl alcohol and 1 part of surfactant 1283 in sequence, mixing, and emulsifying at high speed for 30 minutes.

[0182] Comparative Example 1

[0183] The difference between Comparative Example 1 and Example 2 is that in the method for preparing the heat-sensitive layer coating liquid, the viscosity of the obtained coating liquid is adjusted with water to a viscosity of 20 seconds as measured by a Coating 4 viscosity cup.

[0184] Comparative Example 2

[0185] The difference between Comparative Example 1 and Example 2 is that the composition of the heat-sensitive layer coating liquid omits the styrene-acrylic emulsion.

[0186] Comparative Example 3

[0187] The difference between Comparative Example 1 and Example 2 is that in the composition of the heat-sensitive layer coating liquid, the weight ratio of the colorless dye microcapsules to the developer is 1:8.

[0188] Comparative Example 4

[0189] The difference between Comparative Example 1 and Example 2 is that the isolation layer 3 is omitted.

[0190] The coating method used for the samples is curtain coating, and the coating weights of the protective film, isolation layer, middle layer, heat-sensitive layer and back film are 20, 25, 15, 120, and 20 g / m2 respectively. 3 .

[0191] Film performance measurement:

[0192] 1. The thermal films prepared in Examples 2-9 and Comparative Examples 1-4 were sampled and tested, wherein:

[0193] 1) Experimental conditions: The samples must be equilibrated at a temperature of (23±2)°C and a relative humidity of (50±5)% for 2 hours before processing.

[0194] 2) Sampling: The sample should be sampled after reaching equilibrium under condition 1. Take a piece of film from the unopened package at random and cut it into several pieces with a width of 3.5 cm as test pieces.

[0195] 3) Test piece processing: Use a thermal processing device to heat the prepared film to a specified temperature for 3 seconds.

[0196] 4) Density measurement: Use X-Rite310T transmission densitometer to test film density.

[0197] 5) Haze: measured using Shenguang WGT-S haze meter.

[0198] 6) Waterproof test: Immerse all the test samples in deionized water. After soaking for 4 hours at room temperature, observe the surface transparency and whitish state. Then take out the rear surface and rub it vigorously with fingers 10 times to test the waterproof degree of the protective layer.

[0199] Waterproof evaluation criteria:

[0200] A: Transparent, the coating surface is smooth and no material is wiped off, and it has excellent waterproofness;

[0201] B: Slightly whitish, the coating surface is smooth, no material is wiped off, and the waterproof property is good;

[0202] C: White, the coating surface is melted and easily rubbed off, and the waterproof property is poor.

[0203] 7) Back layer machineability test: During film printing, if there is no sticking when passing through the machine, it is marked as ○; if there is sticking, it is marked as ×.

[0204] 8) Scratch resistance test: If there are no scratches during film printing, the scratch resistance is excellent; if there are slight scratches, the scratch resistance is good; if there are large scratches, the scratch resistance is poor.

[0205] 9) Transparency test: measured using Shenguang WGT-S haze meter.

[0206] The above test results are recorded in Table 1.

[0207] Table 1 Performance test results

[0208]

[0209] From the above test results, it can be seen that the maximum density of the thermal film of the present invention is 2.8-2.9, the haze is less than 40%, the transmittance is about 64%, and the layers are well bonded; the film does not stick during printing and has good machine passability; at the same time, it has excellent scratch resistance.

[0210] 2. The performance test of the thermal film of the present invention is compared with that of the thermal film available on the market. The test indicators are the same as above. The results are recorded in Table 2.

[0211] Table 2 Performance test comparison results

[0212]

[0213] The results in Table 2 show that the various indicators in the table of the thermal film of the present invention are excellent in comprehensive performance compared with Fuji, Kodak and Agfa thermal films. Compared with Fuji film, the present invention has excellent scratch resistance and small haze; compared with Kodak film, the present invention has excellent water resistance, high density, high transparency and low haze; compared with Agfa, the present invention has excellent water resistance and scratch resistance. In general, the thermal film of the present invention has excellent performance in water resistance and scratch resistance, and its maximum density, transparency and haze are also outstanding compared with brand products.

[0214] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A thermal film, comprising a substrate, a protective film disposed on one side of the substrate, a back film disposed on the other side, a thermal layer disposed between the protective film and the substrate, characterized in that: An isolation layer and an intermediate layer are sequentially arranged between the protective film and the heat-sensitive layer, wherein: The raw materials and their weight parts in the isolation layer are as follows: 60-80 parts of UV glue, 1-10 parts of ultraviolet absorber, 1-8 parts of antioxidant, 1-8 parts of surfactant, and 5-15 parts of solvent; The raw materials and their weight parts in the intermediate layer are as follows: 10-20 parts of polyvinyl alcohol, 1-12 parts of water, and 0.5-5 parts of surfactant; The method for preparing the heat-sensitive layer coating liquid comprises the following steps: 1) Under slow stirring, add colorless dye microcapsules, color developer, polyvinyl alcohol, acrylic resin, styrene acrylic emulsion and surfactant in sequence, the weight ratio of colorless dye microcapsules to color developer is 1: (2-7), and add the next one after stirring until the raw materials are evenly mixed; 2) After all the additions are completed, adjust the viscosity of the coating solution with water until the viscosity measured by the coating 4 viscosity cup is 12-16 seconds; 3) Use a wound filter to filter, and let it stand for 4-10 hours under slow stirring to remove bubbles until the bubbles are completely removed, and the coating liquid is obtained.

2. A method for preparing a thermal film according to claim 1, characterized in that: The following steps are involved: Step S1: preparing a protective film coating liquid, an isolation layer coating liquid, an intermediate layer coating liquid, a heat-sensitive layer coating liquid and a back film coating liquid respectively; Step S2: Install the substrate on the film storage rack of the coating machine as required, start the coating machine, and uniformly coat the heat-sensitive layer coating liquid, the intermediate layer coating liquid, the isolation layer coating liquid and the protective film coating liquid on one side of the substrate in turn, and dry and solidify them; then uniformly coat the back film coating liquid on the other side of the substrate, and dry and solidify them; roll and cut to obtain a finished product.

3. The method for preparing a thermal film according to claim 2, characterized in that: The preparation method of the isolation layer coating liquid is as follows: UV glue, ultraviolet absorber, antioxidant, surfactant and solvent are weighed in sequence, mixed, and emulsified at high speed for 30-40 minutes.

4. The method for preparing a thermal film according to claim 3, characterized in that: The preparation method of the intermediate layer coating liquid is: polyvinyl alcohol, water and surfactant are weighed in sequence, mixed, and emulsified at high speed for 30-40 minutes.