Resist underlayer film forming composition

By using the resist lower film formed by the resin and acid catalyst composition, the standing wave problem caused by substrate reflection in lithography is solved, and the planarization and anti-reflection effects are achieved on the recessed or segmented substrate, thereby improving lithography Process accuracy and efficiency.

CN112513738BActive Publication Date: 2024-11-26NISSAN CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN201980050814.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-31
Filing Date
2019-07-18
Publication Date
2024-11-26
Estimated Expiration
2039-07-18

AI Technical Summary

Technical Problem

The conventional resist lower layer film for photolithography is exposed to standing waves due to substrate reflection, which affects the pattern shape and resolution, and it is difficult to form a planarized film on the recessed or segmented substrate.

Method used

Using a composition containing a resin and a specific acid catalyst or a salt thereof, the resin has a -C(=O)-O-based repeating structural unit in the main chain and side chain, and the pKa value of the acid catalyst is less than -0.5, for forming the non- The resist underlayer film mixed with the photoresist layer and does not contain a crosslinking agent to reduce sublimation generation.

Benefits of technology

The solvent resistance and high fillability of the resist lower layer film are achieved, and the planarization film can be formed on the recessed or segmented substrate, and the anti-reflection effect caused by substrate reflection is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002923435170000031
    Figure BDA0002923435170000031
  • Figure BDA0002923435170000041
    Figure BDA0002923435170000041
  • Figure BDA0002923435170000071
    Figure BDA0002923435170000071
Patent Text Reader

Abstract

An object of the present application is to provide a resist underlayer film-forming composition for forming a resist underlayer film that can be suitably used as an antireflection film and a planarization film in a photolithography process for manufacturing a semiconductor device. The solution is a composition for forming a resist underlayer film, which contains a resin, an acid catalyst or a salt thereof, and a solvent, and the resist underlayer film forming composition does not contain a cross-linking agent as a monomer, the resin has a repeating structural unit containing at least one -C(=O)-O- group in the main chain and a repeating structural unit containing at least one hydroxyl group in the side chain, or has a repeating structural unit containing at least one -C(=O)-O- group in the main chain and at least one hydroxyl group in the side chain, and these repeating structural units do not have an organic group containing an epoxy ring or an oxetane ring, the acid catalyst or a salt thereof is 0.1 to 10 parts by mass relative to 100 parts by mass of the resin, and when the acid catalyst is a monobasic acid, the acid dissociation constant pKa in water at 25°C is less than -0.5, or when the acid catalyst is a polybasic acid, the acid dissociation constant pKa1 in water at 25°C is less than -0.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resist underlayer film-forming composition for forming a resist underlayer film for lithography, wherein the resist underlayer film for lithography can be used not only as an antireflection film during exposure but also as a planarization film for flatly filling recesses or steps. Background Art

[0002] In the manufacture of semiconductor devices, microfabrication is performed by photolithography using a photoresist composition. In recent years, the integration of semiconductor devices has been progressing, and the active light used has also been shortened from KrF excimer laser (248nm) to ArF excimer laser (193nm).

[0003] However, KrF excimer laser or ArF excimer laser (incident light) incident on the resist film before the resist pattern is formed is reflected by the substrate surface, thereby generating standing waves in the resist film. It is known that due to the influence of the standing waves, the shape of the pattern edge collapses and the resist pattern of the desired shape cannot be formed. That is, the existence of standing waves causes the size variation and poor resolution of the resist pattern.

[0004] In addition, for example, a composition for forming an underlayer film for lithography containing a linear polymer having 2,4-dihydroxybenzoic acid introduced into the main chain and a solvent (see Patent Document 1), and a composition for forming an anti-etching agent underlayer film for lithography containing a polymer having a benzaldehyde structure or a naphthaldehyde structure introduced into the main chain via an ester structure or an ether structure, a sulfonic acid compound, and a solvent (see Patent Document 2) are disclosed.

[0005] The resist underlayer film obtained from these compositions has performance as an antireflection film, and a rectangular resist pattern can be obtained even when using an ArF excimer laser light source.

[0006] In addition, as the pattern rules of semiconductor devices are becoming increasingly fine, a dual damascene process has been studied as a method for forming wiring on a semiconductor substrate in order to solve the problem of wiring delay in semiconductor devices. The substrate using this process is usually formed with a recess or step such as a hole or a groove structure. Therefore, in order to manufacture a semiconductor device with fine pattern rules, a resist lower layer film is required that can fill the recess on the substrate with the recess or step and form a flat coating film without step. However, in Patent Documents 1 and 2, the flattening property of the resist lower layer film (anti-reflective film) is not disclosed.

[0007] For example, a composition for forming a resist underlayer film for lithography containing an alicyclic epoxy compound having a light absorption site such as a benzene ring, a thermal acid generator for promoting a crosslinking reaction, and a solvent is disclosed (see Patent Document 3). By using this composition, a resist underlayer film capable of flattening the unevenness of a substrate having holes by filling it can be obtained.

[0008] In addition, a resist underlayer film containing a crosslinking polymer and an amine salt of α-difluoromethanesulfonic acid as a thermal acid generator is disclosed (Patent Document 4). By using this composition, a resist pattern with improved border can be obtained.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: International Publication No. 2009 / 057458

[0012] Patent Document 2: International Publication No. 2011 / 004721

[0013] Patent Document 3: International Publication No. 2016 / 158509

[0014] Patent Document 4: Japanese Patent Application Publication No. 2008-039815 Summary of the invention

[0015] Problems to be solved by the invention

[0016] In view of the above problems, the object of the present invention is to provide a resist underlayer film-forming composition that can be used in the manufacture of semiconductor devices. That is, the object of the present invention is to provide a resist underlayer film-forming composition for forming a resist underlayer film that does not mix with a photoresist layer applied and formed on an upper layer and has solvent resistance.

[0017] In particular, the purpose of the present invention is to provide a composition for forming a resist underlayer film, which is used to form a resist underlayer film that can be used not only as an anti-reflection film for reducing reflection of exposure light from a substrate to a resist layer in a photolithography process for manufacturing a semiconductor device, but also as a planarizing film for planarizing a semiconductor substrate having recesses or steps.

[0018] Means of solving problems

[0019] The first embodiment of the present invention is a composition for forming a resist underlayer film, which contains a resin, an acid catalyst or a salt thereof, and a solvent, wherein the resin has a repeating structural unit containing at least one -C(=O)-O- group in the main chain and a repeating structural unit containing at least one hydroxyl group in the side chain, or has a repeating structural unit containing at least one -C(=O)-O- group in the main chain and at least one hydroxyl group in the side chain, and these repeating structural units do not have an organic group containing an epoxy ring or an oxetane ring, and the acid catalyst or a salt thereof is 0.1 to 10 parts by mass relative to 100 parts by mass of the resin, and when the acid catalyst is a monobasic acid, the acid dissociation constant pKa in water at 25°C is less than -0.5, or when the acid catalyst is a polybasic acid, the acid dissociation constant pKa1 in water at 25°C is less than -0.5.

[0020] The salt of the acid catalyst is, for example, trifluoromethanesulfonate.

[0021] The cationic component of the trifluoromethanesulfonate is, for example, a primary ammonium to quaternary ammonium ion, a pyridinium ion which may have a substituent, Ion, optionally substituted imidazole Ion, iodine with substituents ions, sulfonium ions which may have a substituent, or pyranonium ions which may have a substituent ion.

[0022] The resin is, for example, a copolymer having a repeating structural unit represented by the following formula (1-1) and a repeating structural unit represented by the following formula (1-2).

[0023]

[0024] (Where R 1 and R 2 Each independently represents a divalent organic group containing a linear, branched or cyclic functional group having 2 to 20 carbon atoms, and the organic group may have at least one sulfur atom, nitrogen atom or oxygen atom, i and j each independently represent 0 or 1, and the two Qs each represent a single bond, an -O- group or a -C(=O)-O- group, wherein when both i and j are 0, at least one of the two Qs represents a -C(=O)-O- group.

[0025] In the repeating structural unit represented by the formula (1-1), R 1 For example, it represents a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, or represents a linear, branched or cyclic divalent organic group having 2 to 20 carbon atoms which may have at least one sulfur atom or oxygen atom, or represents a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocyclic ring having 3 to 12 carbon atoms, wherein the heterocyclic ring has at least one sulfur atom or oxygen atom.

[0026] In the repeating structural unit represented by the formula (1-2), R 2 For example, it represents a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, or represents a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocyclic ring having 3 to 12 carbon atoms, wherein the heterocyclic ring has at least one sulfur atom or oxygen atom.

[0027] The resist underlayer film-forming composition of the present invention may further contain a compound represented by the following formula (2), formula (3) or formula (4).

[0028]

[0029] (wherein, X represents a carbonyl group or a methylene group, l and m each independently represent an integer of 0 to 5 satisfying the relationship 3≦l+m≦10, R 3 and R 4 Each independently represents an alkylene or alkenylene group having 1 to 4 carbon atoms or a single bond, and n and p each independently represent an integer of 2 to 4. The substituent in formula (4) may be substituted at any position of positions 1 to 8 of the naphthalene ring.

[0030] Furthermore, the resist underlayer film-forming composition of the present invention may further contain a surfactant.

[0031] Effects of the Invention

[0032] According to the present invention, a resist underlayer film-forming composition for forming a resist underlayer film having solvent resistance and which does not mix with a photoresist layer formed as an upper layer by coating can be provided.

[0033] The resist underlayer film forming composition of the present invention does not contain low molecular weight compounds such as a crosslinking agent, so the amount of sublimates during baking can be reduced, and high filling properties inside the concave portion can be achieved without generating voids (gaps). Therefore, according to the present invention, a resist underlayer film forming composition for forming a resist underlayer film capable of flattening a substrate having a concave portion or a step can be provided.

[0034] Furthermore, according to the present invention, it is possible to provide a resist underlayer film-forming composition for forming a resist underlayer film which can be preferably used as an antireflection film for reducing reflection of exposure light from a substrate to a resist layer.

[0035] Specific embodiments of the invention

[0036] The resist underlayer film-forming composition of the present invention contains a resin, a specific amount of an acid catalyst or a salt thereof having an acid dissociation constant pKa or pKa1 of -0.5 or less in water at 25°C, and a solvent, and can be cured to form a resist underlayer film even without containing a crosslinking agent as a monomer. Here, the above-mentioned monomer is a monomer having no repeating unit, and polymers and oligomers obtained by polymerizing multiple monomers do not belong to monomers. In addition, the resist underlayer film-forming composition of the present invention can form a resist underlayer film with excellent planarization properties on a semiconductor substrate having a concave portion or a step difference by using the acid catalyst.

[0037] Examples of the monomer crosslinking agent not contained in the resist underlayer film-forming composition of the present invention include melamine compounds, guanamine compounds, glycoluril compounds, urea compounds and aromatic compounds having two or more at least one group selected from the group consisting of methylol, alkoxymethyl and acyloxymethyl groups in one molecule; and epoxy compounds, oxetane compounds, isocyanate compounds, blocked isocyanate compounds, azide compounds, alkenyl ether compounds, acryl-based compounds and methacryloyl-based compounds having two or more at least one group selected from the group consisting of epoxy, oxetane, isocyanate, blocked isocyanate, azide, alkenyl ether, acryloxy and methacryloyloxy groups in one molecule.

[0038] In the present specification, a component whose content is less than the detection limit as a result of quantitative analysis of the resist underlayer film-forming composition of the present invention is defined as not containing the component.

[0039] Hereinafter, the components contained in the resist underlayer film forming composition of the present invention will be described in detail.

[0040] [Acid catalyst or its salt]

[0041] The acid catalyst or its salt which is an essential component of the resist underlayer film forming composition of the present invention is not particularly limited as long as it is an acid catalyst or its salt which has an acid dissociation constant pKa of less than -0.5 in water at 25°C when the acid catalyst is a monobasic acid, or has an acid dissociation constant pKa1 of less than -0.5 in water at 25°C when the acid catalyst is a polybasic acid.

[0042] The smaller the value of the acid dissociation constant pKa is, the stronger the acidity is, and the more preferred it is for the present invention. Here, the acid dissociation constant pKa is the negative common logarithm of the equilibrium constant Ka of the acid ionization equilibrium, that is, pKa = -log 10 Ka. When the acid catalyst is a polyacid, the equilibrium constant Ka of the acid can be obtained in multiple numbers (Ka1, Ka2, Ka3, ...) according to the dissociation order, but in the present invention, the negative common logarithm of the equilibrium constant Ka1 of the acid ionization equilibrium of the first stage, that is, the acid catalyst whose acid dissociation constant pKa1 is less than -0.5 is selected.

[0043] Examples of acid catalysts having an acid dissociation constant pKa or pKa1 of -0.5 or less include p-toluenesulfonic acid (pKa = -2.8), p-phenolsulfonic acid (pKa1 = -2.59), 5-sulfosalicylic acid (pKa1 = -2.81), and trifluoromethanesulfonic acid (pKa = -14.0) or their salts.

[0044] The cation components of the salts of these acids are not particularly limited, and examples thereof include those derived from aliphatic primary to tertiary amines, heteroamines, aromatic amines, heterocyclic amines, nitrogen-containing compounds having a hydroxyl group, nitrogen-containing compounds having a hydroxyphenyl group, alcoholic nitrogen-containing compounds, quaternary ammonium compounds, iodine, The cation of the onium compound, sulfonium compound, pyranium compound, etc., preferably includes primary ammonium to quaternary ammonium ions, pyridinium ions which may have a substituent, Ion, optionally substituted imidazole Ion, iodine with substituents ions, sulfonium ions which may have a substituent, or pyranonium ions which may have a substituent Here, the substituent is not particularly limited, and examples thereof include methyl, ethyl, propyl, butyl, fluoro, phenyl, and benzyl.

[0045] As the acid catalyst, a salt of trifluoromethanesulfonic acid is particularly preferred, and examples thereof include compounds represented by the following formula.

[0046]

[0047] The acid catalyst of the present invention has a very low volatilization amount when the resin in the resist underlayer film forming composition is crosslinked by baking. Therefore, since the resist underlayer film forming composition of the present invention does not contain low molecular weight volatile components such as a crosslinking agent, the amount of sublimates generated during baking can be reduced, and a flat resist underlayer film without gaps such as voids can be formed.

[0048] In the resist underlayer film-forming composition of the present invention, the content of the acid catalyst or its salt is, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the resin. When the content of the acid catalyst or its salt is less than 0.1 parts by mass relative to 100 parts by mass of the resin, the effect of the present invention may not be obtained. When the content of the acid catalyst or its salt is greater than 10 parts by mass relative to 100 parts by mass of the resin, the amount of sublimates generated during baking increases, so gaps such as voids may sometimes be generated, and the effect of the present invention may not be obtained.

[0049] [Resin]

[0050] The resin as an essential component of the resist underlayer film forming composition of the present invention is not particularly limited as long as it has a repeating structural unit containing at least one -C(=O)-O- group in the main chain and a repeating structural unit containing at least one hydroxyl group in the side chain, or a repeating structural unit containing at least one -C(=O)-O- group in the main chain and at least one hydroxyl group in the side chain, and there is no particular restriction on the resin having no organic group containing an epoxy ring or an oxetane ring in these repeating structural units. Here, as an organic group containing an epoxy ring or an oxetane ring, for example, glycidyl and oxetane can be cited. In addition, a resin without the organic group refers to a resin without a glycidyl group, an oxetane group, etc. The weight average molecular weight of the resin is, for example, 500 to 50,000, preferably 900 to 50,000.

[0051] Since the resin does not have an organic group containing an epoxy ring or an oxetane ring having high reactivity, the resist underlayer film-forming composition of the present invention is excellent in storage stability.

[0052] The resin as an essential component of the resist underlayer film-forming composition of the present invention is preferably a copolymer having a repeating structural unit represented by the above formula (1-1) and a repeating structural unit represented by the above formula (1-2).

[0053] More preferably, the group R in formula (1-1) 1 It is a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, or a linear, branched or cyclic divalent organic group having 2 to 20 carbon atoms and having at least one sulfur atom or oxygen atom, or a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocyclic ring having 3 to 12 carbon atoms, and the heterocyclic ring has at least one sulfur atom or oxygen atom.

[0054] More preferably, the group R in formula (1-2) 2 It is a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, or a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocyclic ring having 3 to 12 carbon atoms, and the heterocyclic ring has at least one sulfur atom or oxygen atom.

[0055] Aromatic rings and heterocyclic rings have absorptivity to KrF excimer laser or ArF excimer laser used in the photolithography process. Therefore, the resist underlayer film obtained from the resist underlayer film-forming composition of the present invention can be well used as an antireflection film because it has at least one aromatic ring or heterocyclic ring in the repeating structural unit represented by formula (1-2).

[0056] Examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a tetracene ring, a triphenylene ring, a pyran ring, and ring, preferably a benzene ring and a naphthalene ring.

[0057] Examples of the heterocyclic ring include a triazine ring, a cyanuric ring, a pyrimidine ring, an imidazole ring, and a carbazole ring.

[0058] The copolymer may be a commercially available product or a copolymer synthesized by a known method using a commercially available product.

[0059] For example, the resin of the present invention may be a copolymer of at least one compound represented by the following formula (A) and at least one diepoxy compound represented by the following formula (B):

[0060]

[0061] (Where R 1 , i and j have the same meanings as above. )

[0062]

[0063] (Where R 2 and Q represent the same meanings as above. ).

[0064] That is, at least one compound represented by formula (A) and at least one diepoxy compound represented by formula (B) are dissolved in an organic solvent at an appropriate molar ratio, and polymerization is carried out in the presence of a catalyst as required, thereby obtaining a copolymer having a repeating structural unit represented by the formula (1-1) and a repeating structural unit represented by the formula (1-2).

[0065] The compound represented by the formula (A) is not particularly limited, and examples thereof include compounds represented by the following formulae.

[0066]

[0067] The diepoxy compound represented by the formula (B) is not particularly limited, and examples thereof include the following diepoxy compounds.

[0068]

[0069] Examples of the copolymer having a repeating structural unit represented by the above formula (1-1) and a repeating structural unit represented by the following formula (1-2) include copolymers having repeating structural units represented by the following formulas (1a) to (1n).

[0070]

[0071]

[0072] [Compound represented by formula (2), formula (3) or formula (4)]

[0073] The resist underlayer film forming composition of the present invention may contain a compound represented by the formula (2), formula (3) or formula (4) as an optional component. Examples of the compound represented by the formula (2) include compounds represented by the following formulas (2-1) to (2-20).

[0074]

[0075] Examples of the compound represented by the formula (3) include compounds represented by the following formulas (3-1) to (3-22).

[0076]

[0077] Examples of the compound represented by the formula (4) include compounds represented by the following formulas (4-1) to (4-9).

[0078]

[0079] The resist underlayer film-forming composition of the present invention may contain the compound represented by the formula (2), formula (3) or formula (4) in an amount of, for example, 0.01 to 60 parts by mass, preferably 0.1 to 20 parts by mass, based on 100 parts by mass of the resin.

[0080] By containing the compound represented by formula (2), formula (3) or formula (4), the resist underlayer film formed from the resist underlayer film-forming composition of the present invention can improve resistance to aqueous hydrogen peroxide solution. Thus, the resist underlayer film formed from the resist underlayer film-forming composition of the present invention can be used as a mask in an etching process and a cleaning process using aqueous hydrogen peroxide solution.

[0081] The resist underlayer film-forming composition of the present invention may contain a surfactant as an optional component in order to improve the coating property on the substrate. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether, polyoxyethylene-polyoxypropylene block copolymers, sorbic acid monolaurate, sorbitan monopalmitate, sorbitan monostearate, and sorbitan monooleate. , sorbitan fatty acid esters such as sorbitan trioleate and sorbitan tristearate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tristearate, and other polyoxyethylene sorbitan fatty acid esters such as nonionic surfactants, EFTOP (registered trademark) EF301, EFTOP EF303, EF352 (manufactured by Mitsubishi Microelectronics Co., Ltd.), MITSUBISHIファック〔Registered Trademark〕F171, メガファックF173, メガファックR-30 , メガファックR-30N, メガファックR-40-LM (produced by DIC Co., Ltd.),フロラードFC430, フロラードFC431 (manufactured by スリーエムジャパン Co., Ltd.), Fluorine-based surfactants such as Asahigard (registered trademark) AG710, Surflon (registered trademark) S-382, Surflon SC101, Surflon SC102, Surflon SC103, Surflon SC104, Surflon SC105, Surflon SC106 (produced by AGC Co., Ltd.), and organosiloxane polymer KP341 (produced by Shin-Etsu Chemical Co., Ltd.). These surfactants may be added alone or in combination of two or more.

[0082] When the above-mentioned surfactant is used, the content of the surfactant is, for example, 0.01 to 5 parts by mass, or preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the resin.

[0083] The resist underlayer film-forming composition of the present invention can be prepared by dissolving the above-mentioned components in an appropriate solvent and used in a uniform solution state. As such solvent, for example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, acetic acid methyl cellosolve, acetic acid ethyl cellosolve, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-hydroxyethyl propionate, 2-hydroxy-2-methylethyl propionate, ethoxyethyl acetate, hydroxyethyl acetate, 2-hydroxy-3-methylbutyric acid methyl ester, 3-methoxymethyl propionate, 3-methoxyethyl propionate, 3-ethoxyethyl propionate, 3-ethoxymethyl propionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone can be used. These solvents can be used alone or in combination of two or more. Furthermore, these solvents may be mixed with a high boiling point solvent such as propylene glycol monobutyl ether and propylene glycol monobutyl ether acetate.

[0084] The prepared composition is preferably used after filtering through a filter having a pore size of, for example, 0.2 μm, 0.1 μm, or 0.05 μm. The resist underlayer film-forming composition of the present invention has excellent storage stability when stored for a long period of time at room temperature. Example

[0085] Hereinafter, specific examples of the resist underlayer film forming composition of the present invention will be described using the following Examples, but the present invention is not limited thereto.

[0086] The apparatus used for measuring the weight average molecular weight of the reaction products obtained in the following synthesis examples.

[0087] Equipment: HLC-8320GPC produced by Tosoh Corporation

[0088] GPC column: TSKgel Super-MultiporeHZ-N (2 columns)

[0089] Column temperature: 40°C

[0090] Flow rate: 0.35ml / min

[0091] Eluent: Tetrahydrofuran

[0092] Standard sample: Polystyrene

[0093] <Synthesis example 1>

[0094] To 65.05 g of propylene glycol monomethyl ether (hereinafter referred to as PGME in this specification), 10.00 g of 1,6-bis(2,3-epoxypropane-1-yloxy)naphthalene (produced by DIC Corporation, trade name: HP-4032D), 7.72 g of 1,8-octanedioic acid, and 0.54 g of ethyltriphenylphosphonium bromide as a catalyst were added, and then reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene-equivalent weight average molecular weight was 4,400. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1a).

[0095]

[0096] <Synthesis example 2>

[0097] 8.00 g of a diepoxy compound (trade name: RE303S-L (produced by Nippon Kayaku Co., Ltd.), 7.94 g of 1,8-octanedioic acid, and 0.46 g of ethyltriphenylphosphonium bromide as a catalyst were added to 65.57 g of PGME, and then reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 4,500. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1b).

[0098]

[0099] <Synthesis Example 3>

[0100] 9.00 g of YX4000 (Mitsubishi Chemical Co., Ltd.), 6.89 g of 1,8-octanedioic acid, and 0.45 g of ethyltriphenylphosphonium bromide as a catalyst were added to 65.35 g of PGME, and the mixture was reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the weight average molecular weight in terms of standard polystyrene was 5,600. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1c).

[0101]

[0102] <Synthesis example 4>

[0103] 18.00 g of the trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.) as a diepoxy compound, 11.96 g of 1,8-octanedioic acid, 0.78 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.23 g of hydroquinone as a free radical scavenger were added to 123.90 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 6,500. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1d).

[0104]

[0105] <Synthesis Example 5>

[0106] 10.00 g of a diepoxy compound (trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.), 5.72 g of 1,6-adipic acid, 0.44 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.13 g of hydroquinone as a free radical scavenger were added to 65.15 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 5,900. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1e).

[0107]

[0108] <Synthesis Example 6>

[0109] 10.00 g of the trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.) as a diepoxy compound, 7.67 g of 1,10-decanedioic acid, 0.44 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.13 g of hydroquinone as a free radical scavenger were added to 72.62 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 5,400. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1f).

[0110]

[0111] <Synthesis Example 7>

[0112] 10.00 g of trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.) as a diepoxy compound, 5.66 g of cis-1,4-cyclohexanedicarboxylic acid, 0.44 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.13 g of hydroquinone as a free radical scavenger were added to 64.88 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 5,400. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1g).

[0113]

[0114] <Synthesis example 8>

[0115] 6.00 g of the trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.) as a diepoxy compound, 3.79 g of 1,3-adamantanedicarboxylic acid, 0.26 g of ethyltriphenylphosphine bromide as a catalyst, and 0.078 g of hydroquinone as a free radical scavenger were added to 40.51 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 2,200. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1h).

[0116]

[0117] <Synthesis Example 9>

[0118] 6.00 g of a diepoxy compound (trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.), 2.72 g of 2,3-norbornanedicarboxylic acid, 0.26 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.078 g of hydroquinone as a radical scavenger were added to 36.25 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 1,600. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1i).

[0119]

[0120] <Synthesis Example 10>

[0121] 10.00 g of monoallyl diglycidyl isocyanate (produced by Shikoku Chemical Industry Co., Ltd., trade name: MA-DGIC), 7.89 g of 3,3'-dithiodipropionic acid (produced by SC Organic Chemical Co., Ltd., trade name: DTDPA), and 0.33 g of ethyltriphenylphosphonium bromide as a catalyst were added to 72.88 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 5,300. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1j).

[0122]

[0123] <Synthesis Example 11>

[0124] To 110.51 g of PGME were added 15.00 g of diglycidyl terephthalate (manufactured by Nagasechem, trade name: EX-711), 11.65 g of 3,3'-dithiodipropionic acid (manufactured by SC Organic Chemicals, trade name: DTDPA), and 0.98 g of ethyltriphenylphosphonium bromide as a catalyst, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the weight average molecular weight in terms of standard polystyrene was 4,900. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1k).

[0125]

[0126] <Synthesis Example 12>

[0127] 15.00 g of 1,6-bis(2,3-epoxypropane-1-yloxy)naphthalene (manufactured by DIC Corporation, trade name: HP-4032D), 23.10 g of monoallyl diglycidyl isocyanate (manufactured by Shikoku Chemical Industry Co., Ltd., product name: MA-DGIC), 31.72 g of 3,3'-dithiodipropionic acid (manufactured by SC Organic Chemical Co., Ltd., trade name: DTDPA), and 2.55 g of ethyltriphenylphosphonium bromide as a catalyst were added to 289.49 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the weight average molecular weight converted to standard polystyrene was 4,500. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1n).

[0128]

[0129] <Synthesis Example 13>

[0130] 40.00 g of the trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.) as a diepoxy compound, 18.58 g of cis-1,2-cyclohexanedicarboxylic acid, 3.48 g of ethyltriphenylphosphine bromide as a catalyst, and 0.52 g of hydroquinone as a free radical scavenger were added to 146.03 g of PGME, and then reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 2,200. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (11).

[0131]

[0132] <Synthesis Example 14>

[0133] 40.00 g of YX4000 (Mitsubishi Chemical Co., Ltd.), 19.54 g of cis-1,2-cyclohexanedicarboxylic acid, and 4.01 g of ethyltriphenylphosphonium bromide as a catalyst were added to 148.30 g of PGME, and then reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 1.900. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1m).

[0134]

[0135] <Synthesis Example 15>

[0136] To 57.97 g of PGME were added 20.00 g of diepoxy compound (trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.), 16.65 g of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (produced by Konishi Chemical Industry Co., Ltd., trade name: BPA-CA), 1.74 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.26 g of hydroquinone as a free radical scavenger, and then reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene-equivalent weight average molecular weight was 16,000. The obtained reaction product was estimated to be a composite having a repeating structural unit represented by the following formula (1p).

[0137]

[0138] <Synthesis Example 16>

[0139] 30.00 g of the trade name: RE810-NM (produced by Nippon Kayaku Co., Ltd.) as a diepoxy compound, 22.16 g of 1,8-octanedioic acid, 1.27 g of ethyltriphenylphosphine bromide as a catalyst, and 0.38 g of hydroquinone as a free radical scavenger were added to 215.23 g of PGME, and then reacted at 105° C. for 24 hours to obtain a solution containing a reaction product. The obtained reaction product was subjected to GPC analysis, and the standard polystyrene conversion weight average molecular weight was 5,000. The obtained reaction product was estimated to be a copolymer having a repeating structural unit represented by the following formula (1o).

[0140]

[0141] [Preparation of Resist Underlayer Film-forming Composition]

[0142] <Example 1>

[0143] PGME 3.46 g, propylene glycol monomethyl ether acetate (hereinafter referred to as PGMEA in this specification) 2.83 g, pyridinium trifluoromethanesulfonate 2.69 g of a solution containing 0.56 g of the copolymer obtained in Synthesis Example 1 (the solvent was PGME used in the synthesis) were mixed. 0.021 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0006 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were added to obtain a 5.8 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0144] <Example 2>

[0145] PGME 3.37 g, PGMEA 2.83 g, pyridinium trifluoromethanesulfonate were mixed with 3.79 g of a solution containing 0.56 g of the copolymer obtained in Synthesis Example 2 (the solvent was PGME used in the synthesis). 0.021 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0006 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were added to obtain a 5.8 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0146] <Example 3>

[0147] PGME 3.52 g, PGMEA 2.83 g, and pyridinium trifluoromethanesulfonate were mixed with 3.63 g of a solution containing 0.56 g of the copolymer obtained in Synthesis Example 3 (the solvent was PGME used in the synthesis). A 5.8 mass % solution was prepared by mixing 0.021 g of 1,2-difluoro-2-nitropropene (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0006 g of a surfactant (produced by DIC Corporation, trade name: R-30N). The solution was filtered through a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0148] <Example 4>

[0149] PGME 110.47 g, PGMEA 110.47 g, pyridinium trifluoromethanesulfonate 126.18 g of a solution containing 20.66 g of the copolymer obtained in Synthesis Example 4 (the solvent was PGME used in the synthesis) were mixed. 0.77 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.021 g of a surfactant (produced by DIC Co., Ltd., trade name: R-30N) were prepared to prepare a 6.5 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0150] <Example 5>

[0151] PGME 7.97 g, PGMEA 5.66 g, pyridinium trifluoromethanesulfonate were mixed with 6.33 g of a solution containing 1.08 g of the copolymer obtained in Synthesis Example 5 (the solvent was PGME used in the synthesis). 0.040 g of (Tokyo Chemical Industry Co., Ltd.) and 0.0011 g of a surfactant (DIC Co., Ltd., trade name: R-30N) were prepared to prepare a 5.6 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0152] <Example 6>

[0153] PGME 7.71 g, PGMEA 5.66 g, and pyridinium trifluoromethanesulfonate were mixed with 6.59 g of a solution (the solvent was PGME used in the synthesis) containing 1.08 g of the copolymer obtained in Synthesis Example 6. 0.040 g of (Tokyo Chemical Industry Co., Ltd.) and 0.0011 g of a surfactant (DIC Co., Ltd., trade name: R-30N) were prepared to prepare a 5.6 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0154] <Example 7>

[0155] 9.12 g of PGME, 7.05 g of PGMEA, and pyridinium trifluoromethanesulfonate were mixed with 8.78 g of a solution containing 1.44 g of the copolymer obtained in Synthesis Example 7 (the solvent was PGME used in the synthesis). 0.054 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0014 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 6.0 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0156] <Example 8>

[0157] 9.28 g of PGME, 7.05 g of PGMEA, and pyridinium trifluoromethanesulfonate were mixed with 8.61 g of a solution containing 1.44 g of the copolymer obtained in Synthesis Example 8 (the solvent was PGME used in the synthesis). 0.054 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0014 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 6.0 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0158] <Example 9>

[0159] PGME 10.06 g, PGMEA 7.05 g, pyridinium trifluoromethanesulfonate 7.84 g of a solution containing 1.44 g of the copolymer obtained in Synthesis Example 9 (the solvent was PGME used in the synthesis) were mixed. 0.054 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0014 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 6.0 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0160] <Example 10>

[0161] 3.44 g of PGME, 2.80 g of PGMEA, and pyridinium trifluoromethanesulfonate were mixed with 3.74 g of a solution containing 0.64 g of the copolymer obtained in Synthesis Example 10 (the solvent was PGME used in the synthesis). 0.024 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.00064 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 6.6 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0162] <Example 11>

[0163] PGME 3.11 g, PGMEA 2.80 g, pyridinium trifluoromethanesulfonate and 1.5 g pyridinium chloride were mixed with 4.06 g of a solution containing 0.64 g of the copolymer obtained in Synthesis Example 11 (the solvent was PGME used in the synthesis). 0.024 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.00064 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 6.6 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0164] <Example 12>

[0165] 6.29 g of PGME and pyridinium trifluoromethanesulfonate were mixed with 3.66 g of a solution containing 0.61 g of the copolymer obtained in Synthesis Example 12 (the solvent was PGME used in the synthesis). 0.023 g of hydroxyethyl ester (produced by Tokyo Chemical Industry Co., Ltd.), 0.030 g of gallic acid hydrate (produced by Tokyo Chemical Industry Co., Ltd.), and 0.00061 g of surfactant (produced by DIC Co., Ltd., trade name: R-30N) were prepared into a 6.6 mass % solution. The solution was filtered with a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a composition for forming a resist underlayer film.

[0166] <Example 13>

[0167] PGME 7.39 g, PGMEA 4.24 g, pyridinium trifluoromethanesulfonate 3.34 g of a solution containing 0.86 g of the copolymer obtained in Synthesis Example 13 (the solvent was PGME used in the synthesis) were mixed. 0.024 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.00086 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 5.9 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0168] <Example 14>

[0169] 7.48 g of PGME, 4.23 g of PGMEA, and pyridinium trifluoromethanesulfonate were mixed with 3.26 g of a solution containing 0.86 g of the copolymer obtained in Synthesis Example 14 (the solvent was PGME used in the synthesis). 0.024 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.00086 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 5.9 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0170] <Example 15>

[0171] PGME 6.21 g, 5-sulfosalicylic acid (Tokyo Chemical Industry Co., Ltd.) 0.022 g, and surfactant (DIC Co., Ltd., trade name: R-30N) 0.00060 g were mixed with 3.77 g of a solution containing 0.60 g of the copolymer obtained in Synthesis Example 10 (the solvent was PGME used in the synthesis) to prepare a 6.2 mass % solution. The solution was filtered with a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0172] <Example 16>

[0173] 35.31 g of PGME, 28.32 g of PGMEA, and pyridinium trifluoromethanesulfonate were mixed with 36.15 g of a solution containing 5.38 g of the copolymer obtained in Synthesis Example 16 (the solvent was PGME used in the synthesis). 0.22 g of chlorinated polyol (produced by Tokyo Chemical Industry Co., Ltd.) and 0.0054 g of a surfactant (produced by DIC Corporation, trade name: R-30N) were prepared to prepare a 5.6 mass % solution. The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film-forming composition.

[0174] <Comparative Example 1>

[0175] PGME 2.50 g, PGMEA 2.81 g, tetramethoxymethyl glycoluril (trade name: Paudalink 1174, manufactured by Japan Science Instruments Co., Ltd.) 0.13 g, pyridinium trifluoromethanesulfonate 0.50 g of a solution containing 0.50 g of the copolymer obtained in Synthesis Example 4 (the solvent was PGME used in the synthesis) 0.13 g, pyridinium trifluoromethanesulfonate 0.50 g of a solution containing 0.50 g of the copolymer obtained in Synthesis Example 4 (Tokyo Chemical Industry Co., Ltd.

[0176] A 6.5 mass % solution was prepared by mixing 0.019 g of a crosslinking agent (produced by DIC Corporation, trade name: R-30N) and 0.0005 g of a surfactant (produced by DIC Corporation, trade name: R-30N). The solution was filtered through a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a composition for forming a resist underlayer film. This comparative example contains a monomer crosslinking agent.

[0177] <Comparative Example 2>

[0178] 3.86 g of PGME, 2.79 g of PGMEA, 0.14 g of tetramethoxymethyl glycoluril (trade name: Paudalink 1174, manufactured by Japan Science Instruments Co., Ltd.) as a monomer crosslinking agent, and pyridinium trifluoromethanesulfonate were mixed with 3.19 g of a solution containing 0.54 g of the copolymer obtained in Synthesis Example 10 (the solvent was PGME used in the synthesis). 0.020 g of (Tokyo Chemical Industry Co., Ltd.) and 0.0005 g of a surfactant (DIC Co., Ltd., trade name: R-30N) were prepared to prepare a 7.0 mass % solution. The solution was filtered with a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a composition for forming a resist underlayer film. This comparative example contains a monomer crosslinking agent.

[0179] <Comparative Example 3>

[0180] 1.27 g of PGME, 1.41 g of PGMEA, and pyridinium trifluoromethanesulfonate were mixed with 2.31 g of a solution containing 0.28 g of the copolymer obtained in Synthesis Example 15 (the solvent was PGME used in the synthesis). 0.011 g of (Tokyo Chemical Industry Co., Ltd.) and 0.0003 g of a surfactant (DIC Co., Ltd., trade name: R-30N) were prepared to prepare a 5.8 mass % solution. The solution was filtered with a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film forming composition. This comparative example is an example in which the copolymer does not contain a -C(=O)-O- group.

[0181] <Comparative Example 4>

[0182] PGME 6.33 g, trifluoroacetic acid (produced by Tokyo Chemical Industry Co., Ltd.) 0.022 g, and surfactant (produced by DIC Co., Ltd., trade name: R-30N) 0.00058 g were mixed with 3.65 g of a solution containing 0.58 g of the copolymer obtained in Synthesis Example 10 (the solvent was PGME used in the synthesis) to prepare a 6.0 mass % solution. The solution was filtered with a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film-forming composition. This comparative example is an example in which the pKa of the acid catalyst used is greater than -0.5.

[0183] [Dissolution test in photoresist solvent]

[0184] The compositions for forming an anti-etching underlayer film prepared in Examples 1 to 16 and Comparative Examples 1 to 4 were respectively applied on a silicon wafer by a spin coater. Then, the anti-etching underlayer film (film thickness 0.2 μm) was formed by baking on a hot plate at a temperature shown in Table 1 below for 1 minute. These anti-etching underlayer films were immersed in the solvents PGME and PGMEA used in the photoresist solution. The evaluation results are shown in Table 1 below, and the case of being insoluble in the two solvents is recorded as "○", and the case of being soluble in the two solvents is recorded as "×".

[0185] [Optical parameter test]

[0186] The resist underlayer film forming composition prepared in Examples 1 to 16 and Comparative Examples 1 to 4 is applied to a silicon wafer using a spin coater. Then, it is baked on a hot plate at a temperature shown in Table 1 below for 1 minute to form a resist underlayer film (film thickness 0.2 μm). Then, an optical ellipsometer (VUV-VASE VU-302, produced by JAW Oollam) is used to measure the refractive index (n value) and attenuation coefficient (k value) of these resist underlayer films at wavelengths of 193 nm and 248 nm. The results are shown in Table 1 below. In order for the above-mentioned resist underlayer film to have sufficient anti-reflection function, it is desired that the k value at a wavelength of 193 nm is greater than 0.1.

[0187] Table 1

[0188]

[0189] [Coating test on step substrate]

[0190] As an evaluation of planarization, the coating thickness of the groove area (TRENCH) with a groove width of 200nm and an interval of 600nm and the open area (OPEN) without patterning are compared on a SiO2 substrate with a film thickness of 230nm. The resist lower film forming composition of Examples 1 to 16, Comparative Example 1 and Comparative Example 2 is coated on the above substrate with a film thickness of 200nm, and then baked on a hot plate at the temperature shown in Table 1 for 1 minute to form a resist lower film (film thickness 0.2μm). The step coverage of the substrate was observed using a scanning electron microscope (S-4800) produced by Hitachi HiTech Nologiz (Strain), and the film thickness difference (the coating step difference between the groove area and the open area, referred to as "deviation") of the step substrate was measured, thereby evaluating the planarization. The film thickness of the groove area and the open area and the coating step difference are shown in Table 2. The smaller the coating step value, the higher the flattening property evaluation. The coating step values ​​shown in Table 2 below are marked as "○" when they are less than 40 nm, and "×" when they are greater than 40 nm. The flattening property evaluation results are shown in Table 1 above.

[0191] Table 2

[0192]

[0193] By comparing the planarization properties, it can be seen that the coating step difference between the groove area and the open area of ​​Examples 1 to 16 is smaller than the coating step difference between the groove area and the open area of ​​Comparative Examples 1 and 2, so it is believed that the resist underlayer film obtained by the resist underlayer film forming composition of Examples 1 to 16 has good planarization properties.

[0194] Industrial Applicability

[0195] The resist underlayer film forming composition of the present invention, after being coated on a substrate, shows high reflowability through a baking process, and can be evenly coated on a substrate having a step difference to form a flat film. In addition, since it has a suitable antireflection effect, it is useful as a resist underlayer film forming composition.

Claims

1. A resist underlayer film-forming composition comprising a resin, an acid catalyst or a salt thereof, and a solvent, wherein the resist underlayer film-forming composition does not contain a crosslinking agent as a monomer, The resin has a repeating structural unit containing at least one -C(=O)-O- group in the main chain and a repeating structural unit containing at least one hydroxyl group in the side chain, or a repeating structural unit containing at least one -C(=O)-O- group in the main chain and at least one hydroxyl group in the side chain, and these repeating structural units do not contain an organic group containing an epoxy ring or an oxetane ring, The acid catalyst or its salt is 0.1 to 10 parts by mass relative to 100 parts by mass of the resin, and when the acid catalyst is a monobasic acid, the acid dissociation constant pKa in 25°C water is less than -0.5, or when the acid catalyst is a polybasic acid, the acid dissociation constant pKa1 in 25°C water is less than -0.

5. 2 . The resist underlayer film forming composition according to claim 1 , wherein the salt of the acid catalyst is a trifluoromethanesulfonate.

3. The resist underlayer film-forming composition according to claim 2, wherein the cation component of the trifluoromethanesulfonate is a primary to quaternary ammonium ion, a pyridinium ion which may have a substituent, Ion, optionally substituted imidazole Ion, iodine with substituents ions, sulfonium ions which may have a substituent, or pyranonium ions which may have a substituent ion.

4. The resist underlayer film-forming composition according to any one of claims 1 to 3, wherein the resin is a copolymer having a repeating structural unit represented by the following formula (1-1) and a repeating structural unit represented by the following formula (1-2), In the formula, R 1 and R 2 Each independently represents a divalent organic group containing a linear, branched or cyclic functional group having 2 to 20 carbon atoms, and the organic group may have at least one sulfur atom, nitrogen atom or oxygen atom, i and j each independently represent 0 or 1, and the two Qs each represent a single bond, an -O- group or a -C(=O)-O- group, wherein, When both i and j are 0, at least one of the two Qs represents a -C(=O)-O- group.

5. The resist underlayer film-forming composition according to claim 4, wherein in the repeating structural unit represented by the formula (1-1), R 1 represents a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, or R 1 represents a linear, branched or cyclic divalent organic group having 2 to 20 carbon atoms and having at least one sulfur atom or oxygen atom, or R 1 It represents a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocyclic ring having 3 to 12 carbon atoms, wherein the heterocyclic ring has at least one sulfur atom or oxygen atom.

6. The resist underlayer film-forming composition according to claim 4, wherein in the repeating structural unit represented by the formula (1-2), R 2 It represents a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, or a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocyclic ring having 3 to 12 carbon atoms, wherein the heterocyclic ring has at least one sulfur atom or oxygen atom.

7. The resist underlayer film-forming composition according to any one of claims 1 to 3, further comprising a compound represented by the following formula (2), formula (3) or formula (4): In the formula, X represents a carbonyl group or a methylene group, l and m each independently represent an integer of 0 to 5 satisfying the relationship 3≤l+m≤10, and R 3 and R 4 Each independently represents an alkylene group or alkenylene group having 1 to 4 carbon atoms or a single bond, and n and p each represent an integer of 2 to 4. The substituent in formula (4) may be substituted at any position among positions 1 to 8 of the naphthalene ring. 8 . The resist underlayer film forming composition according to claim 1 , further comprising a surfactant.

Citation Information

Patent Citations

  • Resist undercoat film material, and resist undercoat film substrate and pattern forming method using the same

    JP2008039815A

  • Composition for forming resist underlayer film and method of forming resist pattern from the same

    WO2009057458A1

  • Composition for forming resist underlayer film and method for forming resist pattern using same

    WO2011004721A1

  • Cationically polymerizable resist underlayer film forming composition

    WO2016158509A1

  • Resist underlayer film-forming composition containing copolymer that has triazine ring and sulfur atom in main chain

    CN105849642A