Composite hydrogel for photocuring cell-carrying 3D printing and preparation method and application thereof
By combining hyaluronic acid-glutamate polymer with other materials, a photocurable composite hydrogel is formed, which solves the problem of difficult to take into account both the biocompatibility and mechanical properties of the materials in the prior art, and achieves high precision, Biocompatible and mechanical properties tunable 3D printed hydrogel scaffolds suitable for the survival environment and tissue engineering of nerve cells.
Patent Information
- Application Number
- CN202210679971.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-16
AI Technical Summary
In the prior art, biocompatible and degradable materials used for three-dimensional tissue reconstruction are difficult to simultaneously possess high precision, biocompatible, low toxicity, adjustable mechanical properties, and suitable for cell adhesion and proliferation. Efficient photocuring molding.
By combining the amino group-containing L-glutamic acid with hyaluronic acid, a hyaluronic acid-glutamic acid polymer is formed, and combined with materials such as collagen, methacrylylated gelatin and sodium carboxymethylcellulose, to form Photocurable composite hydrogels are 3D printed using photoinitiators and ultraviolet light to build hydrogel scaffolds with good moldability.
The morphology of the 3D printed hydrogel scaffold with cell loading is controlled, with high moldability, excellent biocompatibility and adjustable mechanical properties, providing an environment conducive to the survival of nerve cells and providing a new type of light for tissue engineering. Cured material.
Smart Images

Figure CN114989455B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedical materials, and in particular to a composite hydrogel for photocuring cell-carrying 3D printing and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not be necessarily regarded as an admission or any form of suggestion that the information constitutes the prior art already known to those skilled in the art.
[0003] In tissue engineering technology, biocompatible, biodegradable materials are used as support matrices, as matrices for delivering cultured cells, or for three-dimensional (3D) tissue reconstruction.
[0004] Polymer hydrogels have a three-dimensional network and can absorb and retain a large amount of water while maintaining their three-dimensional structure due to the presence of a large number of hydrophilic groups. Due to their structure and composition similar to the natural extracellular matrix (ECM), hydrogels have been widely used in biological applications and the next generation of soft, strong and bio-integrated systems in wound dressings, electronics and soft machines. The polymer network of hydrogels is usually formed by covalent interactions or non-covalent interactions. However, covalent bonds or non-covalent bonds can contribute to the strength or toughness of hydrogels. In summary, it is very important to develop hydrogels suitable for cell adhesion, migration and proliferation by adding appropriate natural materials. In addition, it is particularly important to prepare scaffolds with high precision, good biocompatibility and providing carriers for three-dimensional cultured cells. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing a composite hydrogel and its application. The present invention prepares a composite hydrogel material for biological 3D printing with good biocompatibility, low toxicity, adjustable mechanical properties, high photocurable molding precision, and the ability to provide a carrier for three-dimensional cultured cells and promote cell adhesion and proliferation on a three-dimensional scaffold.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] In a first aspect, the present invention provides a method for preparing a composite hydrogel, comprising the following steps:
[0008] (1) L-glutamic acid containing an amino group is grafted onto the molecular chain of hyaluronic acid containing a carboxyl group through a peptide bond to obtain a hyaluronic acid-glutamic acid polymer (HA-Glu). The polymer introduces the relevant properties of glutamic acid while retaining the original properties of hyaluronic acid, thereby providing a favorable living environment for nerve cells; hyaluronic acid-glutamic acid polymer (HA-Glu), type I collagen (Col), and sodium chloride are dissolved in an HCl solution to form a mixed solution of hyaluronic acid-glutamic acid polymer and collagen (HA-Glu / Col mixed solution).
[0009] (2) dissolving a photoinitiator, phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP), in a NaCl solution and heating in a water bath to form a LAP solution;
[0010] (3) dissolving methacryloyl gelatin (GelMA) in the LAP solution and heating in a water bath until it is completely dissolved to form a methacryloyl gelatin solution;
[0011] (4) Dissolve sodium carboxymethyl cellulose (NaCMC) in the LAP solution and heat in a water bath until it is completely dissolved to form a sodium carboxymethyl cellulose solution.
[0012] (5) The HA-Glu / Col mixed solution of step (1), the methacrylated gelatin solution of step (3), and the sodium carboxymethyl cellulose solution of step (4) are mixed respectively, and then a light-blocking agent, tartrazine, is added, and the mixture is filtered and sterilized with a 0.22 μm sterile filter to finally obtain a composite hydrogel.
[0013] Further, the preparation method of hyaluronic acid-glutamic acid polymer is specifically as follows: in step (1), hyaluronic acid is dissolved in MES buffer at 55°C, and then 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) are added to the solution for activation at 37°C; after activation, L-glutamic acid hydrochloride is dissolved in the above solution at 37°C, and stirring is continued at 37°C for full reaction. Preferably, the mass volume concentration g / mL of the hyaluronic acid, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, N-hydroxysuccinimide and L-glutamic acid hydrochloride in the solution system is 1 (w / v)%, 0.72 (w / v)%, 0.44 (w / v)%, 1.46 (w / v)%, respectively.
[0014] Further, collagen was dissolved in HCl solution at 4°C, sodium chloride was added, the solution was heated to 37°C, hyaluronic acid-glutamic acid polymer was added to the solution and stirred until completely dissolved; pH was adjusted with 0.1 M NaOH at 37°C to finally obtain a mixed solution of hyaluronic acid-glutamic acid polymer and collagen.
[0015] The mass volume concentration of hyaluronic acid-glutamic acid polymer and collagen as solutes in the solution is 2%, wherein the mass ratio of hyaluronic acid-glutamic acid polymer to collagen is 1:7-7:1, more preferably, 1:1.
[0016] Furthermore, in step (2), the mass volume concentration of the photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite in the LAP solution is 0.25%.
[0017] Furthermore, in step (2), the water bath heating temperature is 60° C. and the heating time is 30 min.
[0018] Furthermore, in step (3), the mass volume concentration of the methacrylylated gelatin solution is 14%.
[0019] Furthermore, in step (3), the water bath heating temperature is 60°C.
[0020] Furthermore, in step (4), the mass volume concentration of the sodium carboxymethyl cellulose solution is 1.9%.
[0021] Furthermore, in step (4), the water bath heating temperature is 60°C.
[0022] Furthermore, in step (5), the volume fraction of the methacrylated gelatin solution in the composite solution is 42% (v / v).
[0023] Furthermore, in step (5), the volume fraction of the sodium carboxymethyl cellulose solution in the composite solution is 16% (v / v).
[0024] Furthermore, in step (5), the volume fraction of the mixed solution of hyaluronic acid-glutamic acid polymer and collagen in the composite solution is 42% (v / v).
[0025] Furthermore, in step (5), the concentration of the light-blocking agent tartrazine in the composite solution is 0.05% (w / v).
[0026] In a second aspect, the present invention provides a composite hydrogel prepared using the above method for photocuring cell-laden 3D printing.
[0027] In a third aspect, the present invention also provides a method for obtaining a composite hydrogel scaffold using the composite hydrogel, comprising the following steps:
[0028] Under a sterile environment, the composite hydrogel was evenly mixed with mouse NE-4C neural stem cells and then photocured by 3D printing under 405nm ultraviolet light to obtain a composite hydrogel scaffold.
[0029] Furthermore, the temperature of the deposition platform of the light-curing 3D printer is 29°C, and the temperature of the material tank is 29°C.
[0030] Furthermore, the layer height is 100um and the light intensity is 15mW / cm 2 , base layer number 5, base layer exposure time 20s, layer exposure time 20s.
[0031] Furthermore, the Z-axis speed is 25 mm / min, the peeling distance is 6 mm, the peeling speed is 25 mm / min, and the peeling recovery speed is 100 mm / min.
[0032] In a fourth aspect, the present invention also provides a composite hydrogel scaffold prepared by the above method.
[0033] By adopting the method of the present invention, the hyaluronic acid with a carboxyl group is connected with the glutamic acid with an amino group under the action of EDC and NHS activation to form a hyaluronic acid-glutamic acid polymer, which not only retains the original chemical properties of the hyaluronic acid, but also introduces the relevant properties of glutamic acid to provide a favorable living environment for nerve cells; under the irradiation of ultraviolet light with a wavelength of 405nm, the initiator absorbs light energy to generate free radicals, and the GelMA monomer and the free radical undergo a chain growth reaction, that is, covalent bonds are formed between GelMA molecules to generate a polymerization network, thereby forming a GelMA polymer network with good formability; the amino groups, hydroxyl groups and carboxyl groups of the sodium carboxymethyl cellulose, collagen and the hyaluronic acid-glutamic acid polymer in the scaffold can form hydrogen bonds, which help the network in the scaffold to be dynamically stable, thereby improving the structural stability of the scaffold.
[0034] The present invention has the following beneficial effects:
[0035] (1) The photocuring 3D bioprinting technology can be used to print cell-laden hydrogel scaffolds. The scaffolds have controllable morphology, good formability, high precision, and good stability.
[0036] (2) The added GelMA, as a photosensitive material, can construct a hydrogel scaffold through photocuring. It has RGD polypeptide to stimulate cell growth and differentiation, provide adhesion sites for cells, and has excellent biocompatibility. The added NaCMC can increase the mechanical properties of the hydrogel scaffold and ensure that the hydrogel remains stable after curing. The prepared hyaluronic acid-glutamic acid polymer not only retains the original chemical properties of hyaluronic acid, can resist tissue compression and cell damage, and act as a damper, but also introduces the relevant properties of glutamate, which can be used as a supplement for the nerve center and cerebral cortex. It has a certain effect on the treatment of nerve damage and can provide a favorable living environment for nerve cells. The added collagen is one of the main components of the extracellular matrix and has excellent low immunogenicity. The composite hydrogel has the comprehensive properties of excellent biocompatibility, rapid gelation, and good formability, providing a new type of photocurable material for tissue engineering.
[0037] (3) The scaffold printing process is simple and can be completed in a short time. The porosity and mechanical properties of the 3D printed hydrogel scaffold can be adjusted by adjusting the ratio of HA-Glu and Col in the hydrogel system. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The drawings in the specification, which constitute a part of the present application, are used to provide further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0039] Figure 1 This is a diagram of a light-cured 3D printed bracket according to Example 3 of the present invention.
[0040] Figure 2 (a) is a schematic diagram of the hyaluronic acid-glutamic acid polymer prepared in Examples 1-5 of the present invention; Figure 2 (b) is the hydrogen nuclear magnetic resonance spectrum of the hyaluronic acid-glutamic acid polymer prepared in Example 1-5 of the present invention.
[0041] Figure 3 The microscopic morphology of the hydrogel prepared in Examples 1-5 of the present invention under a scanning electron microscope is shown in FIG. Figure 3 (a) GM / CMC / 1HA-Glu / 7Col hydrogel prepared in Example 1, Figure 3 (b) GM / CMC / 2HA-Glu / 6Col hydrogel prepared in Example 2, Figure 3 (c) GM / CMC / 4HA-Glu / 4Col hydrogel prepared in Example 3, Figure 3 (d) GM / CMC / 6HA-Glu / 2Col hydrogel prepared in Example 4, Figure 3 (e) GM / CMC / 7HA-Glu / 1Col hydrogel prepared in Example 5.
[0042] Figure 4 This is the swelling diagram of the hydrogel prepared in Examples 1-5 of the present invention.
[0043] Figure 5 This is a graph of the compression modulus of the hydrogels prepared in Examples 1-5 of the present invention.
[0044] Figure 6 The rheological properties of the hydrogels prepared in Examples 1-5 of the present invention are shown in FIG. Figure 6 (a) is a graph showing the variation of storage modulus G' and loss modulus G" of hydrogel with strain. Figure 6 (b) is the gelation kinetics curve of the hydrogel.
[0045] Figure 7 The relative proliferation rate RGR of cells cultured in the hydrogels prepared in Examples 1-5 of the present invention. DETAILED DESCRIPTION
[0046] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0047] The technical scheme and implementation process of the present invention are explained in detail through the following examples and accompanying drawings. The following examples are only used to illustrate the present invention, but not to limit the scope of the present invention.
[0048] As some embodiments of the present invention, a method for preparing a photocurable cell-carrying 3D printing composite hydrogel and a scaffold with the same are composed of the following raw materials: the volume ratio of the GelMA solution in the composite solution is 42% (v / v), wherein the concentration of the GelMA solution is 14% (w / v); the volume ratio of the NaCMC solution in the composite solution is 16% (v / v), wherein the concentration of the NaCMC solution is 1.9% (w / v); the volume ratio of the mixed solution of HA-Glu and Col (HA-Glu / Col mixed solution) in the composite solution is 42% (v / v), wherein the solution concentration of HA-Glu / Col as a solute is 2% (w / v), and the mass ratios of HA-Glu and Col are 1:7, 2:6, 4:4, 6:2, and 7:1, respectively; the concentration of LAP in the composite solution is 0.145% (w / v).
[0049] Example 1
[0050] (1) Preparation of hyaluronic acid-glutamic acid polymer (HA-Glu): 1 g of hyaluronic acid was dissolved in 100 ml of MES buffer (50 mM, pH 4.7), and the solution was heated to 55°C in a water bath for 30 min, with oscillation 3 times. Then the heating was stopped, and when the solution temperature reached 37°C, 0.72 g of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride (EDC) and 0.44 g of N-hydroxysuccinimide (NHS) were added to the solution, respectively, and activated for 15-20 min. After the activation, 1.46 g of L-glutamic acid hydrochloride was dissolved in the above solution at 37°C, and continued to stir at 37°C for 24 h for full reaction. After the reaction was completed, the mixture was transferred to a dialysis bag with a molecular weight of 12,000, first dialyzed in a 0.1 M NaCl aqueous solution for 12 hours, and then dialyzed in deionized water for 8 days, during which the deionized water was replaced every day. After dialysis, the solution was placed in a centrifuge at 5750r / min for 5 minutes. After centrifugation, the solution was placed in a rotary evaporator for rotary concentration. After concentration, the solution was divided into equal parts and transferred to an ultra-low temperature refrigerator for 2 hours. After freezing, the material was transferred to a freeze dryer without thawing and freeze-dried until completely dehydrated (about 2-3 days). Finally, the freeze-dried material was placed in a bottle and sealed and refrigerated for storage for use.
[0051] (2) Preparation of a mixed solution of hyaluronic acid-glutamic acid polymer (HA-Glu) and type I collagen (Col): 0.35 g of collagen (Col) was dissolved in 20 ml of 0.01 M HCl solution, the solution was cooled to 4°C in a water bath and stirred continuously for 15 min, and then 0.468 g of sodium chloride was added to the solution and stirred continuously for 5 min. The solution was then heated to 37°C, and 0.05 g of hyaluronic acid-glutamic acid polymer (HA-Glu) was added to the solution and stirred until completely dissolved. After the dissolution was completed, 0.1 M NaOH was used to adjust the pH to 5 at 37°C. Finally, a mixed solution of HA-Glu and Col (HA-Glu / Col mixed solution) was obtained, wherein the solution concentration of HA-Glu / Col as a solute was 2% (w / v), and the mass ratio of HA-Glu to Col was 1:7, i.e., 1HA-Glu / 7Col mixed solution.
[0052] (3) Preparation of LAP solution: 0.1 g of photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP) was dissolved in 40 ml of 0.4 M NaCl solution, and the solution was heated to 60° C. in a water bath for 30 min, during which it was shaken three times to form a LAP solution with a concentration of 0.25% (w / v).
[0053] (4) Preparation of methacryloyl gelatin (GelMA) solution: 1.4 g of GelMA was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a GelMA solution was formed. The solubility of the GelMA solution was 14% (w / v).
[0054] (5) Preparation of sodium carboxymethyl cellulose (NaCMC) solution: 0.19 g of NaCMC was dissolved in 10 ml of LAP solution, and heated in a water bath at 60° C., with shaking for 3 times. After the solution was completely dissolved, a NaCMC solution was formed, i.e., the solubility of the NaCMC solution was 1.9%.
[0055] (w / v).
[0056] (6) Preparation of composite solution: 4.2 ml of GelMA solution, 1.6 ml of NaCMC solution, and 4.2 ml of 1HA-Glu / 7Col mixed solution were placed in a container and stirred evenly, and then 0.005 g of light-blocking agent tartrazine was added. During this period, the mixture was heated in a water bath at 37°C and shaken three times. Finally, the mixture was sterilized by filtration with a 0.22 μm sterile filter to form a 10 ml composite solution, which was recorded as GM / CMC / 1HA-Glu / 7Col.
[0057] (7) DLP photocuring 3D printing prepared the composite solution to obtain a hydrogel scaffold: in a sterile environment, the composite solution was evenly mixed with mouse NE-4C neural stem cells, wherein the amount ratio of the composite solution to the mouse NE-4C neural stem cells was 1 mL: 1×106; a DLP printer was used for photocuring 3D printing to form a scaffold, wherein the deposition platform temperature of the photocuring 3D printer was 29°C, the material tank temperature was 29°C, the layer height was 100 um, and the light intensity was 15 mW / cm 2 , base layer number 5, base layer exposure time 20s, sheet layer exposure time 20s, Z-axis speed 25mm / min, peeling distance 6mm, peeling speed 25mm / min, peeling recovery speed 100mm / min.
[0058] Example 2
[0059] (1) Preparation of hyaluronic acid-glutamic acid polymer (HA-Glu): Same as Example 1.
[0060] (2) Preparation of a mixed solution of hyaluronic acid-glutamic acid polymer (HA-Glu) and type I collagen (Col): 0.3 g of collagen (Col) was dissolved in 20 ml of 0.01 M HCl solution, the solution was cooled to 4°C in a water bath and stirred continuously for 15 min, and then 0.468 g of sodium chloride was added to the solution and stirred continuously for 5 min. The solution was then heated to 37°C, and 0.1 g of hyaluronic acid-glutamic acid polymer (HA-Glu) was added to the solution and stirred until completely dissolved. After the dissolution was completed, 0.1 M NaOH was used to adjust the pH to 5 at 37°C. Finally, a mixed solution of HA-Glu and Col (HA-Glu / Col mixed solution) was obtained, wherein the solution concentration of HA-Glu / Col as a solute was 2% (w / v), and the mass ratio of HA-Glu to Col was 2:6, i.e., 2HA-Glu / 6Col mixed solution.
[0061] (3) Preparation of LAP solution: 0.1 g of photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP) was dissolved in 40 ml of 0.4 M NaCl solution, and the solution was heated to 60° C. in a water bath for 30 min, during which it was shaken three times to form a LAP solution with a concentration of 0.25% (w / v).
[0062] (4) Preparation of methacryloyl gelatin (GelMA) solution: 1.4 g of GelMA was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a GelMA solution was formed. The solubility of the GelMA solution was 14% (w / v).
[0063] (5) Preparation of sodium carboxymethyl cellulose (NaCMC) solution: 0.19 g of NaCMC was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a NaCMC solution was formed, and the solubility of the NaCMC solution was 1.9% (w / v).
[0064] (6) Preparation of composite solution: 4.2 ml of GelMA solution, 1.6 ml of NaCMC solution, and 4.2 ml of 2HA-Glu / 6Col mixed solution were placed in a container and stirred evenly, and then 0.005 g of light-blocking agent tartrazine was added. During this period, the mixture was heated in a water bath at 37°C and shaken three times. Finally, the mixture was sterilized by filtration with a 0.22 μm sterile filter to form a 10 ml composite solution, which was recorded as GM / CMC / 2HA-Glu / 6Col.
[0065] (7) DLP photocuring 3D printing prepared the composite solution to obtain a hydrogel scaffold: in a sterile environment, the composite solution was evenly mixed with mouse NE-4C neural stem cells, wherein the amount ratio of the composite solution to the mouse NE-4C neural stem cells was 1 mL: 1×106; a DLP printer was used for photocuring 3D printing to form a scaffold, wherein the deposition platform temperature of the photocuring 3D printer was 29°C, the material tank temperature was 29°C, the layer height was 100 um, and the light intensity was 15 mW / cm 2 , base layer number 5, base layer exposure time 20s, sheet layer exposure time 20s, Z-axis speed 25mm / min, peeling distance 6mm, peeling speed 25mm / min, peeling recovery speed 100mm / min.
[0066] Example 3
[0067] (1) Preparation of hyaluronic acid-glutamic acid polymer (HA-Glu): Same as in Example 1.
[0068] (2) Preparation of a mixed solution of hyaluronic acid-glutamic acid polymer (HA-Glu) and type I collagen (Col): 0.2 g of collagen (Col) was dissolved in 20 ml of 0.01 M HCl solution, the solution was cooled to 4°C in a water bath and stirred continuously for 15 min, and then 0.468 g of sodium chloride was added to the solution and stirred continuously for 5 min. The solution was then heated to 37°C, and 0.2 g of hyaluronic acid-glutamic acid polymer (HA-Glu) was added to the solution and stirred until completely dissolved. After the dissolution was completed, 0.1 M NaOH was used to adjust the pH to 5 at 37°C. Finally, a mixed solution of HA-Glu and Col (HA-Glu / Col mixed solution) was obtained, wherein the solution concentration of HA-Glu / Col as a solute was 2% (w / v), and the mass ratio of HA-Glu to Col was 4:4, i.e., 4HA-Glu / 4Col mixed solution.
[0069] (3) Preparation of LAP solution: 0.1 g of photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP) was dissolved in 40 ml of 0.4 M NaCl solution, and the solution was heated to 60° C. in a water bath for 30 min, during which it was shaken three times to form a LAP solution with a concentration of 0.25% (w / v).
[0070] (4) Preparation of methacryloyl gelatin (GelMA) solution: 1.4 g of GelMA was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a GelMA solution was formed. The solubility of the GelMA solution was 14% (w / v).
[0071] (5) Preparation of sodium carboxymethyl cellulose (NaCMC) solution: 0.19 g of NaCMC was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a NaCMC solution was formed, and the solubility of the NaCMC solution was 1.9% (w / v).
[0072] (6) Preparation of composite solution: 4.2 ml of GelMA solution, 1.6 ml of NaCMC solution, and 4.2 ml of 4HA-Glu / 4Col mixed solution were placed in a container and stirred evenly, and then 0.005 g of light-blocking agent tartrazine was added. During this period, the mixture was heated in a water bath at 37°C and shaken three times. Finally, the mixture was sterilized by filtration with a 0.22 μm sterile filter to form a 10 ml composite solution, which was recorded as GM / CMC / 4HA-Glu / 4Col.
[0073] (7) DLP photocuring 3D printing prepared the composite solution to obtain a hydrogel scaffold: in a sterile environment, the composite solution was evenly mixed with mouse NE-4C neural stem cells, wherein the amount ratio of the composite solution to the mouse NE-4C neural stem cells was 1 mL: 1×106; a DLP printer was used for photocuring 3D printing to form a scaffold, wherein the deposition platform temperature of the photocuring 3D printer was 29°C, the material tank temperature was 29°C, the layer height was 100 um, and the light intensity was 15 mW / cm 2 , base layer number 5, base layer exposure time 20s, sheet layer exposure time 20s, Z-axis speed 25mm / min, peeling distance 6mm, peeling speed 25mm / min, peeling recovery speed 100mm / min.
[0074] Example 4
[0075] (1) Preparation of hyaluronic acid-glutamic acid polymer (HA-Glu): Same as Example 1.
[0076] (2) Preparation of a mixed solution of hyaluronic acid-glutamic acid polymer (HA-Glu) and type I collagen (Col): 0.1 g of collagen (Col) was dissolved in 20 ml of 0.01 M HCl solution, the solution was cooled to 4°C in a water bath and stirred continuously for 15 min, and then 0.468 g of sodium chloride was added to the solution and stirred continuously for 5 min. The solution was then heated to 37°C, and 0.3 g of hyaluronic acid-glutamic acid polymer (HA-Glu) was added to the solution and stirred until completely dissolved. After the dissolution was completed, 0.1 M NaOH was used to adjust the pH to 5 at 37°C. Finally, a mixed solution of HA-Glu and Col (HA-Glu / Col mixed solution) was obtained, wherein the solution concentration of HA-Glu / Col as a solute was 2% (w / v), and the mass ratio of HA-Glu to Col was 6:2, i.e., 6HA-Glu / 2Col mixed solution.
[0077] (3) Preparation of LAP solution: 0.1 g of photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP) was dissolved in 40 ml of 0.4 M NaCl solution, and the solution was heated to 60° C. in a water bath for 30 min, during which it was shaken three times to form a LAP solution with a concentration of 0.25% (w / v).
[0078] (4) Preparation of methacryloyl gelatin (GelMA) solution: 1.4 g of GelMA was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a GelMA solution was formed. The solubility of the GelMA solution was 14% (w / v).
[0079] (5) Preparation of sodium carboxymethyl cellulose (NaCMC) solution: 0.19 g of NaCMC was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a NaCMC solution was formed, and the solubility of the NaCMC solution was 1.9% (w / v).
[0080] (6) Preparation of composite solution: 4.2 ml of GelMA solution, 1.6 ml of NaCMC solution, and 4.2 ml of 6HA-Glu / 2Col mixed solution were placed in a container and stirred evenly, and then 0.005 g of light-blocking agent tartrazine was added. During this period, the mixture was heated in a water bath at 37°C and shaken three times. Finally, the mixture was sterilized by filtration with a 0.22 μm sterile filter to form a 10 ml composite solution, which was recorded as GM / CMC / 6HA-Glu / 2Col.
[0081] (7) The composite solution prepared by DLP photocuring 3D printing was used to obtain a hydrogel scaffold: under a sterile environment, the composite solution was evenly mixed with mouse NE-4C neural stem cells, wherein the amount ratio of the composite solution to the mouse NE-4C neural stem cells was 1 mL: 1×106; the scaffold was formed by photocuring 3D printing using a DLP printer, wherein the deposition platform temperature of the photocuring 3D printer was 29°C, the material tank temperature was 29°C, the layer height was 100 um, the light intensity was 15 mW / cm2, the number of base layers was 5, the base layer exposure time was 20 s, the sheet layer exposure time was 20 s, the Z-axis speed was 25 mm / min, the peeling distance was 6 mm, the peeling speed was 25 mm / min, and the peeling recovery speed was 100 mm / min.
[0082] Example 5
[0083] (1) Preparation of hyaluronic acid-glutamic acid polymer (HA-Glu): Same as Example 1.
[0084] (2) Preparation of a mixed solution of hyaluronic acid-glutamic acid polymer (HA-Glu) and type I collagen (Col): 0.05 g of collagen (Col) was dissolved in 20 ml of 0.01 M HCl solution, the solution was cooled to 4°C in a water bath and stirred continuously for 15 min, and then 0.468 g of sodium chloride was added to the solution and stirred continuously for 5 min. The solution was then heated to 37°C, and 0.35 g of hyaluronic acid-glutamic acid polymer (HA-Glu) was added to the solution and stirred until completely dissolved. After the dissolution was completed, 0.1 M NaOH was used to adjust the pH to 5 at 37°C. Finally, a mixed solution of HA-Glu and Col (HA-Glu / Col mixed solution) was obtained, wherein the solution concentration of HA-Glu / Col as a solute was 2% (w / v), and the mass ratio of HA-Glu to Col was 7:1, i.e., 7HA-Glu / 1Col mixed solution.
[0085] (3) Preparation of LAP solution: 0.1 g of photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP) was dissolved in 40 ml of 0.4 M NaCl solution, and the solution was heated to 60° C. in a water bath for 30 min, during which it was shaken three times to form a LAP solution with a concentration of 0.25% (w / v).
[0086] (4) Preparation of methacryloyl gelatin (GelMA) solution: 1.4 g of GelMA was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a GelMA solution was formed. The solubility of the GelMA solution was 14% (w / v).
[0087] (5) Preparation of sodium carboxymethyl cellulose (NaCMC) solution: 0.19 g of NaCMC was dissolved in 10 ml of LAP solution, and the solution was heated in a water bath at 60° C. and shaken three times. After the solution was completely dissolved, a NaCMC solution was formed, and the solubility of the NaCMC solution was 1.9% (w / v).
[0088] (6) Preparation of composite solution: 4.2 ml of GelMA solution, 1.6 ml of NaCMC solution, and 4.2 ml of 7HA-Glu / 1Col mixed solution were placed in a container and stirred evenly, and then 0.005 g of light-blocking agent tartrazine was added. During this period, the mixture was heated in a water bath at 37°C and shaken three times. Finally, the mixture was sterilized by filtration with a 0.22 μm sterile filter to form a 10 ml composite solution, which was recorded as GM / CMC / 7HA-Glu / 1Col.
[0089] (7) DLP photocuring 3D printing prepared composite solution to obtain hydrogel scaffold: Under a sterile environment, the composite solution was evenly mixed with mouse NE-4C neural stem cells, wherein the amount ratio of the composite solution to the mouse NE-4C neural stem cells was 1 mL: 1×10 6 The DLP printer was used for photocuring 3D printing to form the bracket, wherein the deposition platform temperature of the photocuring 3D printer was 29°C, the material tank temperature was 29°C, the layer height was 100um, and the light intensity was 15mW / cm 2 , base layer number 5, base layer exposure time 20s, sheet layer exposure time 20s, Z-axis speed 25mm / min, peeling distance 6mm, peeling speed 25mm / min, peeling recovery speed 100mm / min.
[0090] The following tests are used to illustrate the advantages of the hydrogel material in the examples in the application of tissue engineering scaffolds or cell-loaded printed tissues.
[0091] Formability characterization: Example 3 Hydrogel material 3D printing porous scaffolds such as Figure 1 As shown, it can be found that the hydrogel scaffold exhibits a porous morphology and does not swell or break, and there is no blockage or collapse, and the structure is relatively stable.
[0092] Analysis of the new material HA-Glu: Example 1-5 The principle of preparing the new material HA-Glu is as follows Figure 2 As shown in (a), hyaluronic acid with a carboxyl group and glutamic acid with an amino group react under the action of activators EDC and NHS, and finally the carboxyl group and the amino group react to form a peptide bond, and glutamic acid is grafted onto the hyaluronic acid. Example 1-5 Preparation of HA-Glu new material H NMR spectrum is shown in Figure 2 As shown in (b), the peak at 4.79ppm is characterized by D2O, the peak at 2.00ppm is characterized by the methyl group -CH3 on the HA chain, and L1, L2, and L3 correspond to the three hydrocarbon groups on glutamic acid. The grafting rate of Glu grafted on HA is calculated by the following formula:
[0093]
[0094] This shows that Glu was successfully grafted onto HA.
[0095] Characterization of hydrogel microstructure: The hydrogel materials of Example 1, Example 2, Example 3, Example 4, and Example 5 were respectively subjected to photocuring, freeze drying, and gold spraying, and the internal polymer network of the hydrogel was studied using a field emission scanning electron microscope (JEOL, JSM-7610F) at an AC accelerating voltage of 5 kV. Figure 3As shown. Observation of the electron microscope image shows that all hydrogel components have a porous structure. When the Col content is high, the pore size is small, the pore wall is thin, and the cross section is fibrous. When the HA-Glu content increases, the pore size increases, the wall thickness increases, and the porosity increases. It can be observed that the structure changes from fibrous to lamellar. Therefore, the microstructure of the composite hydrogel can be changed by changing the ratio of HA-Glu to Col.
[0096] Characterization of swelling performance: The hydrogel materials of Example 1, Example 2, Example 3, Example 4, and Example 5 were respectively photocured and freeze-dried to prepare small cylinders with a diameter of 9 mm and a height of 5 mm. The cylindrical hydrogel samples were then freeze-dried and weighed (W0), and then immersed in a 37°C PBS solution to allow water absorption and swelling. Then, the samples were removed at different time points after incubation for 10 min, 30 min, 1 h, 2 h, 6 h, 12 h, 24 h, 36 h, 48 h, 72 h, and 96 h, and the samples with surface moisture removed were weighed (W0). n ). The expansion ratio can be calculated using equation (1) as follows:
[0097] W patio =(W n -W0) / W0×100%
[0098] The swelling ratio of each component hydrogel is as follows Figure 4 As shown in the figure, it can be found that the swelling rates of GM / CMC / 1HA-Glu / 7Col, GM / CMC / 2HA-Glu / 6Col, GM / CMC / 4HA-Glu / 4Col, GM / CMC / 6HA-Glu / 2Col, and GM / CMC / 7HA-Glu / 1Col hydrogels are 633%, 650%, 670%, 699%, and 720%, respectively. With the increase of HA-Glu content, the water absorption capacity of the hydrogel is improved. This is because there are a large number of carboxyl -COO groups on the HA main chain in HA-Glu. - In addition, there are also some carboxyl groups in the grafted Glu. Therefore, the increase in hydrophilic groups improves the water absorption capacity.
[0099] Mechanical properties characterization: The mechanical properties of the hydrogels of Examples 1-5 were characterized using a universal testing machine (ZLC-2D, Jinan XLC Testing Machine Co., Ltd.) at a loading rate of 2 mm / min and a 100 N load cell in air. Figure 5 As shown in the figure, with the increase of HA-Glu content, the elastic modulus of the hydrogel gradually increased, and the hardness of the hydrogel gradually increased, and its modulus ranged from 6.7kPa to 39.7kPa. Therefore, by changing the ratio of HA-Glu to Col, the elastic modulus of the composite hydrogel can be changed, and the modulus can be controlled.
[0100] Rheological characterization: Rheological analysis of the hydrogels of Examples 1-5 was performed at room temperature using Anton Paar MCr 302 and a 1° cone plate. During the experiment, silicone oil was used to seal the edges of the plate to prevent water loss. Figure 6 (a) shows the curves of the storage modulus (G') and loss modulus (G") of the cured hydrogel with strain. At small strains, it can be seen that the higher the HA-Glu content, the larger the G', and the harder the cured hydrogel. The higher the HA-Glu content, the smaller the strain value at the intersection of the G' and G" curves, and the easier it is for the cured hydrogel to break under the same strain conditions. Figure 6 (b) shows the gel kinetics curve of the hydrogel of Example 1-5, which is cured by light with a power of 25 mW / cm 2 Under the irradiation of ultraviolet light, the curing gel time and gel rate of the hydrogel liquid were tested. 0.5 ml of uniform solution was loaded onto the fixture, and a time scan was performed at a frequency of 1 Hz, with a strain of 1%. The ultraviolet light was turned on at 50 s and irradiated for 300 s. Figure 6 (b) Rheological data show that the GM / CMC / HA-Glu / Col hydrogel solutions of Examples 1-5 all completely gelled at 190 seconds. As the ratio of HA-Glu to Col changes, the gelation time of the solution does not change significantly, so the change in the HA-Glu / Col ratio does not affect the photocuring ability of the hydrogel. As the HA-Glu content increases, the modulus of the hydrogel after curing also increases, and the cured hydrogel is harder (consistent with the analysis of mechanical property characterization).
[0101] Cytotoxicity characterization: The biocompatibility of the material was verified by cell proliferation experiments, and the CCK-8 reagent was used to evaluate the activity of cells in the material extract. First, mouse NE-4C neural stem cells were inoculated into 96-well plates at a density of 3000 cells per well, cultured with complete culture medium (100 μl / well) for 24 hours, and then three groups of experiments were designed (positive control group, blank control group, experimental group). Among them, the blank control group continued to be cultured with complete culture medium, the positive control group was incubated with 0.65% phenol solution, and the experimental groups were GM / CMC / 1HA-Glu / 7Col, GM / CMC / 2HA-Glu / 6Col, GM / CMC / 4HA-Glu / 4Col, GM / CMC / 6HA-Glu / 2Col, and GM / CMC / 7HA-Glu / 1Col hydrogels of Examples 1-5, respectively. The above experiments were cultured for 7 days, and the solution was changed once a day. Use CCK-8 stock solution and the corresponding culture medium to prepare a working solution with a volume ratio of 1:10 and keep it away from light for later use. The detection process is: first take out the original culture medium in the well plate, then add 110 μl / well of CCK-8 working solution to the well plate, and place it in an incubator for 2 hours, avoiding the generation of bubbles during the process. Finally, use a multifunctional microplate reader (ReadMax 1900, Shanghai Flash Spectrum Biotechnology Co., Ltd.) to measure the absorbance of the test solution at a wavelength of 450nm on the seventh day, read the OD value, the number of samples is greater than 5, and repeat the experiment n=3. Then, use the Dixon test to eliminate outliers, and express these data as the mean standard deviation (SD). Finally, use the following equation to express the relative proliferation rate RGR of cells in percentage.
[0102] RGR=OD 450e / OD 450 b×100%
[0103] Among them, OD_450e is the average optical density measured by the sample extract; OD_450b is the average optical density of the blank group. The results are as follows Figure 7 The lower the survival rate value, the higher the cytotoxic potential of the test sample, and the cell toxicity level is shown in Table 1.
[0104] Combination Figure 7 From Table 1, we can find the relative proliferation rate RGR and toxicity level on the seventh day. The RGR of the positive control group was only 6.9%, and the cell level was 4, indicating that the sample was toxic. The RGR of the experimental group was more than 90%, and the cell level was 1, indicating that the hydrogel samples prepared by Examples 1-5 were non-toxic to cells. Therefore, it is shown that the prepared hydrogel system is not cytotoxic and has good biocompatibility.
[0105] Table 1 Cytotoxicity test results of hydrogel materials
[0106]
[0107] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a composite hydrogel, characterized in that: The following steps are involved: (1) L-glutamic acid containing an amino group is grafted onto the molecular chain of hyaluronic acid containing a carboxyl group through a peptide bond to obtain a hyaluronic acid-glutamic acid polymer (HA-Glu); the hyaluronic acid-glutamic acid polymer (HA-Glu), type I collagen (Col), and sodium chloride are dissolved in an HCl solution to form a mixed solution of the hyaluronic acid-glutamic acid polymer and collagen; The mass ratio of the hyaluronic acid-glutamic acid polymer to collagen is 1:7 to 7:1; (2) dissolving the photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite (LAP) in a NaCl solution and heating in a water bath to form a LAP solution; (3) Dissolving methacryloyl gelatin (GelMA) in the LAP solution and heating in a water bath until it is completely dissolved to form a methacryloyl gelatin solution; (4) Dissolve sodium carboxymethyl cellulose (NaCMC) in the LAP solution and heat in a water bath until it is completely dissolved to form a sodium carboxymethyl cellulose solution; (5) The HA-Glu / Col mixed solution of step (1), the GelMA solution of step (3), and the NaCMC solution of step (4) are mixed respectively, and then a light-blocking agent, tartrazine, is added, and the mixture is filtered and sterilized with a 0.22 μm sterile filter to finally obtain a composite hydrogel.
2. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (1), the preparation method of the hyaluronic acid-glutamic acid polymer is specifically as follows: dissolving hyaluronic acid in MES buffer at 55°C, and then adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) to the solution for activation at 37°C; after the activation, dissolving L-glutamic acid hydrochloride in the above solution at 37°C, and continuing to stir at 37°C for sufficient reaction.
3. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (1), the mass volume concentrations of hyaluronic acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, N-hydroxysuccinimide and L-glutamic acid hydrochloride in the solution system are 1%, 0.72%, 0.44% and 1.46%, respectively.
4. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (1), collagen is dissolved in HCl solution at 4°C, sodium chloride is added, the solution is heated to 37°C, and hyaluronic acid-glutamic acid polymer is added to the solution and stirred until completely dissolved; The pH was adjusted with 0.1 M NaOH at 37° C. to finally obtain a mixed solution of hyaluronic acid-glutamic acid polymer and collagen.
5. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (1), the mass volume concentration of the hyaluronic acid-glutamic acid polymer and collagen as solutes in the solution is 2%, wherein the mass ratio of the hyaluronic acid-glutamic acid polymer to the collagen is 1:
1.
6. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (2), the mass volume concentration of the photoinitiator phenyl-2,4,6-trimethylbenzoyl lithium phosphite in the LAP solution is 0.25%; in step (2), the water bath heating temperature is 60° C. and the heating time is 30 min.
7. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (3), the mass volume concentration of the methacrylated gelatin solution is 14%; in step (3), the water bath heating temperature is 60°C.
8. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (4), the mass volume concentration of the sodium carboxymethyl cellulose solution is 1.9%; in step (4), the water bath heating temperature is 60°C.
9. The method for preparing the composite hydrogel according to claim 1, characterized in that: In step (5), the volume fraction of the methacrylated gelatin solution in the composite solution is 42%; In step (5), the volume fraction of the sodium carboxymethyl cellulose solution in the composite solution is 16%; In step (5), the volume fraction of the mixed solution of hyaluronic acid-glutamic acid polymer and collagen in the composite solution is 42%; In step (5), the mass volume concentration of the light-blocking agent tartrazine in the composite solution is 0.05%.
10. A composite hydrogel for photocurable cell-laden 3D printing prepared according to the method of any one of claims 1 to 9.
11. A method for preparing a composite hydrogel scaffold, characterized in that: The steps include: In a sterile environment, the composite hydrogel according to claim 10 is uniformly mixed with mouse NE-4C neural stem cells, and then photocured 3D printing is performed under 405 nm ultraviolet light to obtain a composite hydrogel scaffold.
12. The method for preparing a composite hydrogel scaffold according to claim 11, characterized in that: The temperature of the deposition platform of the light-curing 3D printer is 29°C, and the temperature of the material tank is 29°C; Layer height 100 um, light intensity 15 mW / cm 2 , number of base layers: 5, exposure time of base layer: 20s, exposure time of sheet layer: 20s; Z-axis speed 25mm / min, peeling distance 6mm, peeling speed 25mm / min, peeling recovery speed 100mm / min.
13. A composite hydrogel scaffold prepared by the method according to any one of claims 11 to 12.
Citation Information
Patent Citations
Method for preparing injectable porous hydrogel microspheres by microfluidic ice crystal method and application of injectable porous hydrogel microspheres
CN112409553A
Photocuring molding composite hydrogel matrix precursor, preparation method thereof and stent with photocuring molding composite hydrogel matrix precursor
CN113679888A
Bionic hydrogel scaffold for tissue engineering skin construction and preparation method thereof
CN114276567A
Additive Manufacturing Of Cell-Laden Functional Hydrogel And Live Cell Constructs
US20220152279A1