Composite sodium metal negative plate and preparation method and application thereof
The preparation of composite sodium metal negative electrode sheets by cold calendering method using composite sodium/sodium-M alloy/sodium halide composite materials in sodium metal batteries has solved the problem of sodium dendrite and poor processability, and achieved high capacity and long cycle life Sodium metal battery performance.
Patent Information
- Application Number
- CN202411378516.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Due to the high reduction of sodium metal, sodium, the sodium metal battery leads to side reactions and loose porous solid electrolyte interface formation, which affects stability, and the processability of sodium metal, difficulty in storage and transportation, and the growth of sodium dendrites accelerates.
Using composite sodium metal negative electrode sheet, made of sodium/sodium-M alloy/sodium halide composite material, the metal halide powder is uniformly distributed between sodium foils by cold calendering method to form sodium foil-metal halide-sodium foil "Sandwich "Structure, improving the deposition and transport performance of sodium ions.
It inhibits the side reaction between the sodium metal negative electrode and the electrolyte, slows down dendrites, improves moldability and processing performance, realizes a sodium metal battery with high capacity and long cycle life, and improves sodium ion deposition kinetics and electricity. Chemical properties.
Smart Images

Figure CN119008848A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium metal batteries, and in particular relates to a composite sodium metal negative electrode sheet and a preparation method and application thereof. Background Art
[0002] Sodium metal batteries have attracted great attention due to their high energy density, abundant sodium resources and potential low cost, but they still face some challenges that affect their commercialization. On the one hand, the high reducibility of metallic sodium leads to continuous side reactions between the negative electrode and the electrolyte, producing unstable solid electrolyte interfaces (SEI). Over time, these SEIs will develop into loose and porous layer structures during the cycle, destroying the Na + Diffusion and accelerated growth of sodium dendrites. On the other hand, sodium metal is usually stored in kerosene in the form of sodium blocks, which corrodes quickly in the air, and the low metal bond energy of sodium leads to poor processability, making the electrode very difficult to manufacture. Since sodium metal has low hardness and high viscosity, it will deform and adhere to it when in contact with it with a slight applied pressure, which creates difficulties for the storage or transportation of sodium foil. Therefore, it is urgent to develop a sodium metal negative electrode to solve the problem of sodium dendrites and solve the problems in the processing, storage, transportation and application of sodium metal. Summary of the invention
[0003] In order to overcome the deficiencies in the prior art, the present invention aims to provide a composite sodium metal negative electrode sheet and a preparation method and application thereof.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A composite sodium metal negative electrode sheet, which is a sodium / sodium-M alloy / sodium halide composite material, wherein the sodium-M alloy and the sodium halide are uniformly dispersed in the metallic sodium bulk phase; wherein the sodium-M alloy is a Na-Sn alloy, a Na-In alloy, a Na-Bi alloy or a Na-Zn alloy, and the sodium halide is NaF, NaCl, NaBr or NaI.
[0005] Preferably, the thickness of the composite sodium metal negative electrode sheet is 20-500 μm.
[0006] A method for preparing a composite sodium metal negative electrode sheet, the preparation steps are as follows: (1) Dry the metal halide powder and set it aside for later use, and prepare two pieces of sodium foil at the same time; the metal halide is a halide of Sn, In, Bi or Zn; (2) In a glove box protected by an inert atmosphere, the dried metal halide powder is evenly distributed between two sodium foils, stacked together in a "sandwich" structure of sodium foil-metal halide-sodium foil, cold rolled → folded in half → cold rolled, and the "cold rolled → folded in half → cold rolled" process is repeated multiple times to obtain a composite foil; (3) The composite foil is punched into an electrode sheet of a desired diameter using a punching machine to obtain a composite sodium metal negative electrode sheet.
[0007] Preferably, in step (2), the metal halide powder is added in batches, that is, the specific process of step (2) is: in a glove box protected by an inert atmosphere, take a portion of the dried metal halide powder, evenly distribute it between two sodium foils, stack them together in a sodium foil-metal halide-sodium foil "sandwich" structure, cold roll → evenly distribute a portion of the metal halide powder on the upper sodium foil after cold roll → fold it in half → cold roll, repeat "cold roll → evenly distribute a portion of the metal halide powder on the upper sodium foil after cold roll → fold it in half → cold roll" multiple times to obtain a composite foil.
[0008] Preferably, in a glove box protected by an inert atmosphere, H2O <0.1 ppm and O2 <0.1 ppm.
[0009] Preferably, in step (1), the metal halide powder is dried at a temperature of 60-80° C. for 48-72 hours.
[0010] Preferably, in step (1), the mass ratio of metal halide powder to two sodium foils is (5-8):100, more preferably, the mass ratio of metal halide powder to two sodium foils is (20-60):100, and most preferably, the mass ratio of metal halide powder to two sodium foils is 40:100.
[0011] An application of the composite sodium metal negative electrode sheet in a sodium metal battery.
[0012] Preferably, the sodium metal battery is a button-type full battery or a soft-pack full battery; The assembly process of the button-type full battery is as follows: in a glove box protected by an inert atmosphere, the positive electrode sheet is placed in the positive electrode shell, the electrolyte is added, the separator is placed, the electrolyte is added again, and then the composite sodium metal negative electrode sheet is placed on the separator, and finally the nickel foam and the negative electrode shell are placed, and pressed to obtain the button-type full battery; The assembly process of the soft-pack full battery is as follows: in a glove box protected by an inert atmosphere, NSF composite sodium metal negative electrode sheet-electrolyte-diaphragm-electrolyte-positive electrode sheet are stacked layer by layer in order, and then transferred to two pieces of aluminum foil, and the cut tabs are placed, and finally packaged with a heat sealer to obtain a soft-pack full battery; The positive electrode sheet is prepared according to the following process: taking the total mass percentage as 100%, weighing 70-80% of the positive electrode active material, 10-20% of the conductive agent and 10-20% of the binder respectively, adding an appropriate amount of dispersant to form a slurry, grinding evenly until the slurry is shiny, then spreading it evenly on aluminum foil, drying it, and cutting it to obtain a positive electrode sheet.
[0013] Preferably, the positive electrode active material is one or more of sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium iron pyrophosphate, sodium iron sulfate, sodium copper iron manganate, and sodium nickel iron manganate; the conductive agent is one or more of acetylene black, Super P Li, Ketjen black, and carbon nanotubes; the binder is one or more of PVDF, PTFE, polyacrylic acid, styrene-butadiene rubber, polyethylene oxide, sodium carboxymethyl cellulose, and alginate; the dispersant is one or more of 1-methyl-2-pyrrolidone, dimethyl sulfoxide, NN-dimethylformamide, NN-dimethylacetamide, acetone, anhydrous ethanol, and water; the electrolyte is a soluble salt organic solution; the diaphragm is a composite diaphragm of one or more of polyethylene, polypropylene microporous membrane, glass fiber diaphragm, and polyacrylonitrile diaphragm.
[0014] The operating temperature of the cold rolling described in the present invention is room temperature.
[0015] The preparation principle of the composite sodium metal negative electrode sheet of the present invention is: MX+Na→NaM+NaX (MX represents metal halide, NaM represents sodium-M alloy, M is Sn, In, Bi or Zn, and X is F, Cl, Br or I). The chemical property of metal Na is active and can spontaneously react with metal halide. The formed sodium-M alloy and sodium halide can improve the affinity of sodium ions, regulate the deposition of sodium ions, and improve the processability of the composite sodium metal negative electrode sheet.
[0016] Beneficial effects: (1) The present invention utilizes the spontaneous reaction between metallic sodium and metal halide to prepare a composite sodium metal negative electrode sheet by a simple repeated cold rolling and folding method of sodium foil and metal halide powder. In this process, abundant and fresh sodium halide and sodium-M alloy are produced. The sodium-M alloy can regulate the Na + The deposition of Na + The affinity of sodium halide is the most effective Na on the sodium negative electrode because of its high mechanical strength. + Conductor and stabilizer, the high ionic conductivity of sodium halide can achieve fast ion transport and good rate performance on the entire negative electrode sheet, while the low electronic conductivity further inhibits dendrite growth; the synergistic effect of the two can not only inhibit the side reaction between the sodium metal negative electrode and the electrolyte and the growth of sodium dendrites, but also promote the Na + The rapid transport of the composite sodium metal negative electrode sheet has higher formability compared to the soft and sticky sodium metal; (2) The sodium-M alloy and sodium halide formed in situ in the present invention are uniformly implanted into the metallic sodium, and the thickness of the composite sodium metal negative electrode sheet can be precisely controlled by adjusting the spacing between the two rollers of the cold-pressed delayed roller press. In the later stage, different molds can be used to cut into various shapes according to actual needs. Therefore, the composite sodium metal negative electrode sheet of the present invention has excellent processing performance; (3) The button-type full cell assembled with a composite sodium metal negative electrode sheet provides 108.9 mAh g at 1 C. -1 The assembled soft-pack battery provides 94.87 mAh g at 1C. -1 High capacity and 95.04% high capacity retention rate; (4) The present invention improves the sodium ion deposition kinetics and electrochemical performance, provides a novel alloy strategy for Na metal chemical modification, promotes the commercialization of sodium metal batteries, and shows high technical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 : Schematic diagram of the preparation process of the NSF composite sodium metal negative electrode sheet in Example 1 of the present invention.
[0018] Figure 2 : XRD spectrum of the NSF composite sodium metal negative electrode sheet prepared in Example 1 of the present invention.
[0019] Figure 3 :Effects of different metal halide ratios on battery performance: (a) EIS graphs of NSF|NSF and Na|Na symmetric batteries with different ratios; (b) EIS graphs of NSF|NSF and Na|Na symmetric batteries with different ratios at 1 mA cm -2 Deposition / dissolution curves at different current densities.
[0020] Figure 4 : Comparison of the cycling performance of NVP|NSF and NVP|Na button-type full batteries assembled in Example 1 of the present invention at 1C.
[0021] Figure 5 : Comparison of rate capacities of NVP|NSF and NVP|Na button-type full batteries assembled in Example 1 of the present invention.
[0022] Figure 6 : Charge and discharge curves of the NVP|NSF button-type full battery assembled in Example 1 of the present invention at different cycle numbers.
[0023] Figure 7 : Cycling performance of the NVP|NSF soft-pack full battery assembled in Example 1 of the present invention at 1C. DETAILED DESCRIPTION
[0024] The following is a clear and complete description of the technical solution of the present invention in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] Na / Na 15 The preparation steps of Sn4 / NaF (NSF) composite sodium metal negative electrode sheet are as follows: (1) Place SnF2 powder in a 60°C forced air drying oven and dry for 48 hours, then transfer to an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm) and place it there. At the same time, prepare two pieces of sodium foil in a mass ratio of SnF2 powder to two pieces of sodium foil = 40:100. The two pieces of sodium foil have the same shape and size. (2) In an argon glove box, Figure 1 As shown (the composite network refers to the sodium-Sn alloy Na 15 The composite of Sn4 and sodium fluoride NaF) is made by stacking the dried SnF2 powder and two pieces of sodium foil together to form a Na-SnF2-Na "sandwich" structure, which is pressed together by mechanical rolling using a roller press (cold rolling), and then folded in half, and then cold rolled, and cold rolling is repeated → folded in half → cold rolled to obtain a composite foil with a thickness of 50 μm; during this period, the thickness of the composite foil is changed by adjusting the spacing between the two rollers of the roller press; (3) The obtained composite foil is punched into an electrode sheet with a diameter of 12 mm using a punching machine, which is the target composite sodium metal negative electrode sheet, marked as NSF, for structural characterization and electrochemical testing.
[0027] Example 2
[0028] The difference from Example 1 is that in step (1), the mass ratio of SnF2 powder to two pieces of sodium foil is changed to SnF2 powder: two pieces of sodium foil = 20:100; the rest is the same as Example 1.
[0029] Example 3
[0030] The difference from Example 1 is that in step (1), the mass ratio of SnF2 powder to two pieces of sodium foil is changed to SnF2 powder: two pieces of sodium foil = 60:100; the rest is the same as Example 1.
[0031] Example 4
[0032] The difference from Example 1 is that SnCl2 powder is used instead of SnF2 powder.
[0033] The composite sodium metal negative electrode sheet prepared in this embodiment is Na / Na 15 Sn4 / NaCl (NSC).
[0034] Example 5
[0035] The difference from Example 1 is that SnBr2 powder is used instead of SnF2 powder.
[0036] The composite sodium metal negative electrode sheet prepared in this embodiment is Na / Na 15 Sn4 / NaBr (NSB).
[0037] Example 6
[0038] The difference from Example 1 is that SnI2 powder is used instead of SnF2 powder.
[0039] The composite sodium metal negative electrode sheet prepared in this embodiment is Na / Na 15 Sn4 / NaI (NSI).
[0040] Product structure characterization The NSF composite sodium metal negative electrode sheet prepared in Example 1 of the present invention was characterized by XRD. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that Na and SnF2 are successfully converted into Na 15 Sn4 and NaF. At the same time, due to the stoichiometric excess of metallic sodium, a strong diffraction peak of metallic sodium was still observed in the XRD spectrum of NSF, indicating the synthesis of NSF.
[0041] Product performance characterization 1. Effect of different metal halide ratios on battery performance The NSF composite sodium metal negative electrode sheet prepared in Examples 1 to 3 of the present invention is used for the assembly of NSF|NSF symmetric batteries (button type): in an argon glove box, the NSF composite sodium metal negative electrode sheet is placed in the positive electrode shell, 55 μL of electrolyte is added, and then a diaphragm is placed, and 55 μL of electrolyte is added again. Then, the NSF composite sodium metal negative electrode sheet is placed on the diaphragm, and finally, nickel foam and the negative electrode shell are placed, and the entire battery is pressed; the electrolyte is an organic solution of 1M NaClO4, and the solvent is a mixed solvent of EC (ethylene carbonate) and PC (propylene carbonate) in a volume ratio of 1:1, and 5 wt% FEC (fluoroethylene carbonate) is added to the mixed solvent; the diaphragm is a glass fiber diaphragm.
[0042] A Na|Na symmetric battery (button type) was assembled according to the above process using a pure sodium sheet instead of the NSF composite sodium metal negative electrode sheet as a control battery.
[0043] Figure 3 Effects of different metal halide ratios on battery performance: (a) EIS graphs of NSF|NSF and Na|Na symmetric batteries with different ratios; (b) EIS graphs of NSF|NSF and Na|Na symmetric batteries with different ratios at 1 mA cm -2 Deposition / dissolution curves under current density; in the figure, 20% NSF, 40% NSF, and 60% NSF correspond to NSF|NSF symmetric batteries assembled from NSF composite sodium metal negative electrode sheets obtained in Example 2, Example 1, and Example 3, respectively, and Na corresponds to Na|Na symmetric batteries assembled from pure sodium sheets. Figure 3 a shows that the interfacial impedances of NSF|NSF symmetric batteries assembled with 20% NSF, 40% NSF, and 60% NSF are 68.1 Ω, 32.78 Ω, and 71.1 Ω, respectively, all of which exhibit smaller interfacial impedances than that of Na|Na symmetric batteries (125.7 Ω). Among them, the interfacial impedance of the NSF|NSF symmetric battery assembled with 40% NSF is the smallest (32.78 Ω). Figure 3 b Display: Output at 1 mA cm -2 At a current density of 20%, the Na|Na symmetric battery showed the largest overpotential (0.12 V) and short-circuited after 125 h. The NSF|NSF symmetric batteries assembled with three ratios of 20% NSF, 40% NSF and 60% NSF all showed lower charge and discharge overpotentials of 0.10 V, 0.05 V and 0.08 V, respectively. Among them, the NSF|NSF symmetric battery assembled with 40% NSF showed the lowest cycle overpotential (0.05 V) and could stably charge and discharge for more than 400 h. In short, the impedance and polarization voltage of the NSF|NSF symmetric batteries at the three mass ratios (20% NSF, 40% NSF, 60% NSF) were smaller than those of Na|Na, indicating the superiority of the NSF negative electrode, and the NSF with a mass ratio of 40% NSF had the smallest impedance, the lowest polarization voltage and the longest cycle life at the three ratios, showing the best cycle stability.
[0044] (II) Full battery performance test The NSF composite sodium metal negative electrode sheet prepared in Example 1 of the present invention was used for the assembly of NVP|NSF button-type full batteries: in an argon glove box, the NVP positive electrode sheet was placed in the positive electrode shell, 55 μL of electrolyte was added, and then the diaphragm was placed, and 55 μL of electrolyte was added again. Then, the NSF composite sodium metal negative electrode sheet was placed on the diaphragm, and finally, the nickel foam and the negative electrode shell were placed, and the entire battery was pressed; the electrolyte was an organic solution of 1M NaClO4, and the solvent was a mixed solvent of EC (ethylene carbonate) and PC (propylene carbonate) in a volume ratio of 1:1, and 5 wt% FEC (fluoroethylene carbonate); the diaphragm is a glass fiber diaphragm; the NVP positive electrode sheet is prepared according to the following process: according to the mass ratio of 8:1:1, the positive electrode active material, the conductive agent and the binder are respectively weighed, and an appropriate amount of dispersant is added to form a slurry, and the slurry is evenly ground until it is bright, and then spread on aluminum foil and evenly coated, placed in a 60°C forced air drying oven for 6h, and a mold with a diameter of 13 mm is selected to cut to obtain an NVP positive electrode sheet; wherein, the positive electrode active material is sodium vanadium phosphate (NVP), the conductive agent is conductive carbon black (Super PLi), the binder is polyvinylidene fluoride, and the dispersant is 1-methyl-2-pyrrolidone.
[0045] The NVP|Na button-type full cell was assembled according to the above process using pure sodium sheet instead of NSF composite sodium metal negative electrode sheet as a control cell.
[0046] The NSF composite sodium metal negative electrode sheet prepared in Example 1 of the present invention is used for the assembly of NVP|NSF soft-pack batteries: in an argon glove box, the NSF composite sodium metal negative electrode sheet-55μL electrolyte-diaphragm-55μL electrolyte-NVP positive electrode sheet are stacked layer by layer in the order, and then the stacked battery is clamped with plastic tweezers, transferred to two pieces of aluminum foil, and the cut tabs are placed, and finally packaged with a heat sealer. Among them, the NVP positive electrode sheet, electrolyte, and diaphragm are the same as the aforementioned NVP|NSF button-type full battery.
[0047] The NVP|NSF button-type full battery and NVP|Na button-type full battery were charged and discharged at different current densities on a blue electric tester to investigate the charge and discharge specific capacity and cycle stability of the button-type full battery.
[0048] Figure 4 This is a comparison chart of the cycle performance of NVP|NSF and NVP|Na button-type full batteries assembled in Example 1 of the present invention at 1C. Figure 4 It can be seen that the NVP|NSF button cell delivers 108.9 mAh g at a rate of 1 C in the first cycle. -1 The high capacity of the battery was 107.9 mAh g at the 100th cycle. -1High capacity, the capacity at the 200th cycle is 106.6 mAh g -1 , the capacity at the 300th cycle is 105.9 mAh g -1 The capacity retention rate is as high as 97.2%. In addition, the capacity and coulombic efficiency curve of the NVP|NSF button-type full cell remains stable during the cycle. In contrast, the NVP|Na button-type full cell shows a much lower capacity and a significant capacity decay during the cycle, with a capacity of only 66.0 mAh g at the 300th cycle. -1 , the capacity retention rate is only 65.6%. The coulombic efficiency of NVP|Na button-type full cells is not much different from that of NVP|NSF button-type full cells.
[0049] Figure 5 This is a comparison chart of the rate capacity of NVP|NSF and NVP|Na button-type full batteries assembled in Example 1 of the present invention. Figure 5 It can be seen that the capacity of the NVP|NSF button-type full battery at the initial 0.1C is 100.8mAh g -1 , 94.3mAh g at 0.5C -1 , 90.0mAh g at 1C -1 , 83.9 mAh g at 2C -1 , 76.9 mAh g at 5C -1 , 67.6 mAh g at 10C -1 , and the capacity at the 50th cycle back to 0.1C is 95.3 mAh g -1 , with a capacity retention of 94.5%, indicating good rate performance. In contrast, the capacity of the NVP|Na battery is much lower, especially at high rates, with a capacity of 93.7 mAh g at 0.1C. -1 , 84.05 mAh g at 0.5C -1 , 79.3 mAh g at 1C -1 , 74.7 mAh g at 2C -1 , 68.8 mAh g at 5C -1 , 60.5 mAh g at 10C -1 , with a capacity retention rate of only 64.5%.
[0050] Figure 6 The charge and discharge curves of the NVP|NSF button-type full battery assembled in Example 1 of the present invention at different cycle times. Figure 6 It can be seen that the cut-off voltages of the 10th and 100th cycles are similar, indicating that this button-type full battery has good cycle stability.
[0051] Figure 7 The cycle performance of the NVP|NSF soft-pack full battery equipped in Example 1 of the present invention at 1C. Figure 7 It can be seen that in the first cycle, 94.87 mAh g -1 The high capacity of the battery was 90.16 mAh g at the 100th cycle. -1 The high capacity, stable curve and coulombic efficiency are always maintained during the cycle, and the capacity retention rate is as high as 95.04%. The illustration shows that the assembled full battery can successfully light up the light bulb.
Claims
1. A composite sodium metal negative electrode sheet, Features: The composite sodium metal negative electrode sheet is a sodium / sodium-M alloy / sodium halide composite material, and the sodium-M alloy and the sodium halide are uniformly dispersed in the metallic sodium bulk phase; wherein the sodium-M alloy is a Na-Sn alloy, a Na-In alloy, a Na-Bi alloy or a Na-Zn alloy, and the sodium halide is NaF, NaCl, NaBr or NaI.
2. The composite sodium metal negative electrode sheet according to claim 1, Features: The thickness of the composite sodium metal negative electrode sheet is 20~500μm.
3. A method for preparing the composite sodium metal negative electrode sheet as claimed in claim 1, It is characterized in that The preparation steps are as follows: (1) Dry the metal halide powder and set it aside for later use, and prepare two pieces of sodium foil at the same time; the metal halide is a halide of Sn, In, Bi or Zn; (2) In an inert atmosphere-protected glove box, the dried metal halide powder is evenly distributed between two sodium foils, stacked together in a "sandwich" structure of sodium foil-metal halide-sodium foil, cold rolled → folded in half → cold rolled, and the "cold rolled → folded in half → cold rolled" is repeated multiple times to obtain a composite foil; (3) The composite foil is punched into an electrode sheet of a desired diameter using a punching machine to obtain a composite sodium metal negative electrode sheet.
4. The method for preparing the composite sodium metal negative electrode sheet according to claim 3, It is characterized in that In step (2), the metal halide powder is added in batches, that is, the specific process of step (2) is: in a glove box protected by an inert atmosphere, take a portion of the dried metal halide powder, evenly distribute it between two sodium foils, stack them together in a sodium foil-metal halide-sodium foil "sandwich" structure, cold roll → evenly distribute a portion of the metal halide powder on the upper sodium foil after cold roll → fold it in half → cold roll, repeat "cold roll → evenly distribute a portion of the metal halide powder on the upper sodium foil after cold roll → fold it in half → cold roll" for multiple times to obtain a composite foil.
5. The method for preparing the composite sodium metal negative electrode sheet according to claim 3 or 4, Features: In an inert atmosphere glove box, H 2 O <0.1 ppm, O 2 <0.1 ppm.
6. The method for preparing the composite sodium metal negative electrode sheet according to claim 3 or 4, Features: In step (1), the metal halide powder is dried at a temperature of 60 to 80° C. for a time of 48 to 72 hours.
7. The method for preparing the composite sodium metal negative electrode sheet according to claim 3 or 4, Features: In step (1), the mass ratio of metal halide powder to two pieces of sodium foil is (5-80):
100.
8. The method for preparing the composite sodium metal negative electrode sheet according to claim 7, Features: In step (1), the mass ratio of metal halide powder to two pieces of sodium foil is (20-60):
100.
9. Use of the composite sodium metal negative electrode sheet as claimed in claim 1 or 2 in a sodium metal battery.
10. Use of the composite sodium metal negative electrode sheet according to claim 9 in a sodium metal battery, Features: The sodium metal battery is a button-type full battery or a soft-pack full battery; The assembly process of the button-type full battery is as follows: in a glove box protected by an inert atmosphere, the positive electrode sheet is placed in the positive electrode shell, the electrolyte is added, the separator is placed, the electrolyte is added again, and then the composite sodium metal negative electrode sheet is placed on the separator, and finally the nickel foam and the negative electrode shell are placed, and pressed to obtain the button-type full battery; The assembly process of the soft-pack full battery is as follows: in a glove box protected by an inert atmosphere, NSF composite sodium metal negative electrode sheet-electrolyte-diaphragm-electrolyte-positive electrode sheet are stacked layer by layer in order, and then transferred to two pieces of aluminum foil, and the cut tabs are placed, and finally packaged with a heat sealer to obtain a soft-pack full battery; The positive electrode sheet is prepared according to the following process: taking the total mass percentage as 100%, weighing 70-80% of the positive electrode active material, 10-20% of the conductive agent and 10-20% of the binder respectively, adding an appropriate amount of dispersant to form a slurry, grinding evenly until the slurry is shiny, then spreading it evenly on aluminum foil, drying it, and cutting it to obtain a positive electrode sheet.
Citation Information
Patent Citations
Ion-electron hybrid conductive metal sodium negative electrode and preparation method thereof
CN111430660A
Pre-lithiated and pre-sodium-modified composite negative electrode material as well as preparation method and application thereof
CN115036444A
High-entropy sodium alloy negative electrode, preparation method and sodium battery
CN118448585A
Lithium / sodium ion battery negative electrode having a dual-gradient structure, and preparation method therefor
WO2024114471A1
Cited By
Composite negative electrode for low-temperature sodium metal battery and preparation method of composite negative electrode
CN119560499A
Sodium metal composite negative electrode material and preparation method and application thereof