A plasmon-enhanced local avalanche ultraviolet photodetector and preparation method thereof
By etching the micropore structure in the P layer of the wide bandgap semiconductor ultraviolet photodetector and preparing metal nanoparticle arrays, the local avalanche area is enhanced by using the plasmon field to solve the problem of high avalanche breakdown voltage of traditional detectors. Lower avalanche voltage and higher quantum efficiency are achieved.
Patent Information
- Application Number
- CN202210497724.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-05-09
AI Technical Summary
The traditional planar PiN structure APD wide bandgap semiconductor ultraviolet photodetector has an APD wide bandgap semiconductor ultraviolet photodetector, because the incident light part is absorbed by the P layer, the quantum efficiency is not high enough, and a high bias voltage (usually higher than 100V) is required to generate an avalanche, resulting in an avalanche. The breakdown voltage is high.
By etching microporous structures of different sizes on the P layer of the device and preparing metal nanoparticle arrays on the surface of the device, the local avalanche area is enhanced by using the plasmon field to reduce the avalanche voltage.
The local avalanche of the device is realized, reducing the avalanche breakdown voltage to between 30V and 40V, improving the quantum efficiency, and reducing the operating voltage of the device.
Smart Images

Figure CN115000238B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor detection devices, and in particular relates to a plasmon-enhanced local avalanche ultraviolet photodetector and a preparation method thereof. Background Art
[0002] With the rapid development of the times, wide bandgap semiconductors, as a new generation of semiconductor materials, have the advantages of large bandgap width, high saturated electron drift velocity, and high breakdown electric field. They have very broad application prospects in many fields such as new energy power, aerospace, scientific research, and medical care. At the same time, wide bandgap semiconductor ultraviolet photodetectors have the advantages of smaller size, higher detection rate, and the ability to detect sunlight blindness. They have great application potential in ultraviolet communications, space science, and environmental monitoring. The research on new high-performance wide bandgap semiconductor ultraviolet photodetectors has become one of the key research topics in optoelectronics in developed countries. Based on the above advantages, wide bandgap semiconductor devices can work in harsh environments (such as high temperature, high pressure or high radiation) without any radiation damage to themselves.
[0003] However, with the rapid development of semiconductor technology, the demand for devices in various fields is constantly increasing, so more attention should be paid to improving device performance. The traditional planar PiN structure APD wide bandgap semiconductor ultraviolet photodetector has a low quantum efficiency because the incident light is partially absorbed by the P layer, and the generated photogenerated carriers fail to enter the depletion region. At the same time, a very high bias voltage (usually higher than 100V) is required for the device to produce avalanche. Therefore, the present invention designs a plasmon-enhanced local avalanche ultraviolet photodetector, which is mainly to etch micropore structures of different sizes in the P layer of the device to achieve local avalanche of the device, and at the same time prepare a metal nanoparticle array on the surface of the device, and use the plasmon field to enhance the expansion of the local avalanche area, causing the non-avalanche or about-to-avalanche area to avalanche in advance, thereby reducing the avalanche voltage of the device, providing an additional way to reduce the avalanche breakdown voltage of the wide bandgap semiconductor ultraviolet detector, and providing a feasible solution for future high-performance wide bandgap semiconductor ultraviolet detectors. Summary of the invention
[0004] The purpose of the present invention is to provide an ultraviolet photodetector for plasmon-enhanced local avalanche and a preparation method thereof, which utilizes surface plasmon field enhancement to induce electric field enhancement in the lower wide bandgap semiconductor through a principle similar to a MOS structure, so as to achieve a high field condition for avalanche: on the one hand, the originally small local avalanche area at the micropore is enlarged; on the other hand, it mainly induces the non-avalanche area or the area about to avalanche to reach the high field condition for avalanche, thereby realizing the local avalanche of the device and reducing the avalanche breakdown voltage of the device.
[0005] The present invention provides a method for preparing a plasmon-enhanced local avalanche ultraviolet photodetector, comprising the following steps:
[0006] 1) Using chemical vapor transport homoepitaxial method on N + An N-type buffer layer and an i-type absorption layer are sequentially grown on a wide bandgap semiconductor substrate, and a P-type layer is then grown by chemical vapor deposition;
[0007] 2) etching a tilted terrace on a wide bandgap semiconductor epitaxial wafer of a PiN structure by photolithography and ICP etching;
[0008] 3) etching the microporous structure by photolithography and ICP etching;
[0009] 4) growing a silicon dioxide passivation layer and opening windows by thermal oxidation and chemical vapor deposition;
[0010] 5) Fabricating P-electrode and N-electrode by photolithography and magnetron sputtering;
[0011] 6) A PS mask is prepared on the surface using a PS microsphere solution, a metal film is deposited on the PS mask, and a surface metal nanoparticle array is obtained after peeling off the PS mask.
[0012] In step 1), the doping concentration of the N-type buffer layer may be 1×10 17 / cm 3 -5×10 20 / cm 3 , the thickness may be 0.5 to 3 μm; the doping concentration of the i-type absorption layer may be 1×10 14 / cm 3 ~2×10 16 / cm 3 , the thickness can be 1 to 20 μm; the P + The doping concentration of the type layer can be 1×10 17 / cm 3 ~5×10 20 / cm 3 , the thickness can be 0.1~1μm.
[0013] In step 3), the micropores are opened from the P-type layer to the i-type absorption layer, so that the P-type layer is engraved through to the i-type absorption layer. The function of the micropore structure is to cause local avalanche of the device, mainly because the local electric field at the edge of the micropore is higher; the size and spacing of the micropores are changed according to the excitation effect of the surface plasmon, so that it can achieve the best excitation effect in the ultraviolet band and enhance the local avalanche with the maximum efficiency.
[0014] In step 4), the thickness of the silicon dioxide passivation layer is 10 to 500 nm.
[0015] In step 6), the diameter of the PS microsphere can be 100-1000nm; the thickness of the metal film can be 5-50nm; the shape of the metal nanoparticles can be spherical, disc-shaped, triangular prism-shaped and other shapes, and the size and spacing of the metal nanoparticles can be selected by computational simulation; the metal nanoparticles can be selected from metal materials such as Al, Ag, Au, etc. that can excite surface plasmons in the ultraviolet band; the metal nanoparticle array is evenly distributed on the device surface, the bottom of the micropores and the side walls of the micropores to better induce field enhancement in the semiconductor. When ultraviolet light is incident on the device surface at different angles, photon energy can be obtained in both the horizontal and vertical directions, thereby maximizing the field enhancement of the surface plasmons. When applied to APDs including structures such as PiN, SAM, and SACM, the size and spacing of the surface metal nanoparticle array are obtained by computational simulation to maximize the plasmon field intensity excited by the ultraviolet band light source.
[0016] The present invention provides an ultraviolet photoelectric detector, which is prepared by the preparation method of the ultraviolet photoelectric detector for plasmon enhanced local avalanche.
[0017] The present invention etches micropores first after etching the inclined table, then grows a silicon dioxide passivation layer, and finally obtains a surface metal nanoparticle array through deposition and peeling. This sequence is beneficial to reducing the dark current of the device.
[0018] When the device is working, ultraviolet rays irradiate the device at different angles. First, due to the different angles of incidence, especially the oblique incidence, there can be light components in both the horizontal and vertical directions, thereby maximizing the stimulation of surface plasmon field enhancement; second, there is a local avalanche effect in a smaller area at the edge of the micropore structure; third, by stimulating the surface plasmon field enhancement to induce a lower electric field in the wide bandgap semiconductor, on the one hand, it can expand the local avalanche area of the device, and on the other hand, make the non-avalanche area or the area about to avalanche reach the conditions for premature avalanche, thereby realizing the local avalanche of the device and greatly reducing the avalanche breakdown voltage of the device.
[0019] The preparation method of the present invention is applicable to APD photodetectors including structures such as PiN, SAM, and SACM, but is not limited to such devices. For APDs with different structures, the surface metal material, the size of metal nanoparticles, and the spacing are selected and distinguished through computational simulation to better realize the local avalanche of ultraviolet photoelectric devices and reduce the avalanche voltage. Only suitable materials and sizes can stimulate surface plasmon field enhancement and achieve the conditions of local avalanche, thereby reducing the avalanche voltage of the device, otherwise the effect is not good.
[0020] The present invention induces the electric field in a wide bandgap semiconductor by exciting a plasmon field enhancement through metal nanoparticles, thereby expanding the avalanche region of the device, inducing the device to reach an avalanche condition in advance, and reducing the avalanche breakdown voltage to between 30V and 40V. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a cross-sectional schematic diagram of a PiN structure wide bandgap semiconductor APD ultraviolet photodetector with plasmon enhanced local avalanche according to an embodiment of the present invention.
[0022] Figure 2 Schematic diagram of a top view of a PiN structured wide bandgap semiconductor APD ultraviolet photodetector with plasmon enhanced local avalanche according to an embodiment of the present invention.
[0023] Figure 3 It is a cross-sectional schematic diagram of a wide-bandgap semiconductor APD ultraviolet photodetector with a plasmon-enhanced local avalanche SACM structure according to an embodiment of the present invention.
[0024] Figure 4 Schematic diagram of the device effect of the PiN structure wide bandgap semiconductor APD ultraviolet photodetector with plasmon enhanced local avalanche according to an embodiment of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the following embodiments will further illustrate the present invention in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. On the contrary, the present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention as defined by the claims.
[0026] Example 1
[0027] The cross-sectional view of the PiN structure wide bandgap semiconductor APD ultraviolet photodetector with plasmon enhanced local avalanche implemented by the present invention is as follows: Figure 1 As shown, the top view is Figure 2 shown.
[0028] The ultraviolet photodetector is provided with N electrode 01, highly doped N +The invention comprises a wide bandgap semiconductor substrate 02, an N-type layer 03, a lightly doped i-type layer 04, a highly doped P-type layer 05, a P-type electrode 06, a silicon dioxide passivation layer, and a metal nanoparticle array 07. The metal nanoparticle array can be made of metal materials such as Al, Ag, and Au that can excite surface plasmons. The shape of the metal nanoparticle array can be spherical, disc-shaped, triangular prism-shaped, and the size and spacing of the metal nanoparticles need to be obtained through reasonable calculation and simulation; the opening 08 is a hole opened from the P layer to the i layer, so that the P layer is engraved through the i layer. The function of the micropore structure is to cause local avalanche of the device, mainly because the local electric field at the edge of the micropore is high. When ultraviolet light is incident on the detector chip at different angles, the surface metal particles excite the plasmon field to enhance, which can induce the area with originally low electric field in the device to reach the high field condition of avalanche: on the one hand, it expands the originally small local avalanche area at the micropore; on the other hand, it mainly induces the non-avalanche area or the area about to avalanche to reach the high electric field condition of avalanche.
[0029] The specific preparation steps of the ultraviolet photodetector are as follows:
[0030] (1) In highly doped N + The N-type layer 03 and the i-type layer 04 are epitaxially grown on the wide bandgap semiconductor substrate 02 by chemical vapor deposition in sequence. The doping concentration of the N-type layer can be 1×10 17 / cm 3 -5×10 20 / cm 3 , the thickness can be 0.5μm-3μm, and the doping concentration of the i-type layer can be 1×10 14 / cm 3 -2×10 16 / cm 3, The thickness can be 1 μm-20 μm.
[0031] (2) A P-type layer 05 is formed on the upper surface of the i-type layer by chemical vapor deposition. The doping concentration of the P-type layer can be 1×10 17 / cm 3 ~5×10 20 / cm 3 , the thickness can be 0.1 to 1 μm. Then the entire epitaxial wafer is cleaned according to the RCA standard.
[0032] (3) The inclined terrace 17 is etched using photolithography and ICP etching techniques.
[0033] (4) Using photoresist as a barrier layer, the micropore structure 19 is etched by photolithography and magnetron sputtering ICP etching technology, with an etching depth of about 0.1 to 1 μm. The optimal micropore size is obtained through simulation, which is mainly used to achieve local avalanche conditions.
[0034] (5) A silicon dioxide passivation layer is grown on the device surface using thermal oxidation and chemical vapor deposition techniques, wherein the thickness of the thermally oxidized silicon dioxide is 10 to 200 nm, and the chemical vapor deposition of silicon dioxide and silicon nitride is 100 to 1000 nm thick.
[0035] (6) A window 18 is opened by photolithography and ICP etching technology. The depth of the window opening is 200 to 2000 nm, which is the thickness of the silicon dioxide and silicon nitride grown by chemical vapor deposition in step (5).
[0036] (7) Using photolithography technology, BOE solution corrodes the silicon dioxide layer at the P electrode, and magnetron sputtering metal forms the P electrode 06.
[0037] (8) Etching the back side highly doped N + A wide bandgap semiconductor substrate is used and metal is magnetron sputtered to form an N electrode.
[0038] (9) A PS mask is prepared on the surface using a PS microsphere solution, wherein the diameter of the PS microsphere is 100 to 1000 nm.
[0039] (10) A layer of metal Al film is deposited on the PS mask using electron beam evaporation technology. The thickness of the metal Al film is about 5 to 50 nm.
[0040] (11) Finally, the PS mask was peeled off using a tetrahydrofuran solution to prepare a surface metal Al nanoparticle array.
[0041] Example 2
[0042] The SACM structure wide bandgap semiconductor APD ultraviolet photodetector with plasmon enhanced local avalanche implemented by the present invention has a cross-sectional view as shown in FIG. Figure 3 The specific preparation steps are as follows:
[0043] (1) On a highly doped N+ type wide bandgap semiconductor substrate 02, an absorption layer 32, a charge layer 33, and a multiplication layer 34 are epitaxially grown in sequence by chemical vapor deposition. The doping concentration of the absorption layer can be 1×10 14 / cm 3 ~1×10 16 / cm 3 , the thickness can be 1 to 10 μm, and the doping concentration of the charge layer can be 1×10 17 / cm 3 ~1×10 20 / cm 3 The thickness can be 0.1 to 1 μm, and the doping concentration of the multiplication layer can be 1×10 14 / cm 3 ~1×10 16 / cm 3The thickness can be 0.1 to 1 μm. (2) Forming P on the surface of the multiplication layer by chemical vapor deposition + Type 35, P + The doping concentration of the type layer can be 1×10 18 / cm 3 ~2×10 20 / cm 3 The thickness can be 0.1 to 1 μm. Then the epitaxial wafer is cleaned according to the RCA standard.
[0044] (3) Same as step (3) of Example 1.
[0045] (4) Etching the micropore structure, using 5214E photoresist as a barrier layer, etching from the top to the absorption layer, with an etching depth of about 0.3-3 μm. The difference from Example 1 is that the etching depths are different and the optimal micropore sizes are different, but both are for achieving local avalanche conditions.
[0046] (5) to (11) are the same as steps (5) to (11) in Example 1.
[0047] Specific process of device preparation:
[0048] The above RCA standard cleaning, the specific steps are:
[0049] ①Use toluene, acetone and ethanol to ultrasonically process for 5 to 10 minutes, repeat 4 times, and then rinse with deionized water;
[0050] ② After boiling with No. 3 solution at 250°C for 15 to 30 minutes, rinse with hot and cold deionized water; the No. 3 solution is in a volume ratio of H2SO4:H2O2=4:1;
[0051] ③ Soak the sample in diluted hydrofluoric acid for 3 to 5 minutes, and then rinse with hot and cold deionized water; the dilute hydrofluoric acid has a volume ratio of HF:H2O=1:20;
[0052] ④ After boiling with No. 1 solution for 5 to 10 minutes, rinse with hot and cold deionized water; the No. 1 solution has a volume ratio of NH3·H2O:H2O2:H2O=1:1:4;
[0053] ⑤ Soak the sample in diluted hydrofluoric acid for 3 to 5 minutes, then rinse with hot and cold deionized water;
[0054] ⑥ After boiling with No. 2 solution for 5 to 10 minutes, rinse with hot and cold deionized water, and then blow dry with nitrogen for later use; the volume ratio of the No. 2 solution is HCl: H2O2: H2O = 1:1:4.
[0055] The specific steps of tilted mesa etching are: using photoresist reflow technology, spinning (4620), pre-baking, exposing with the first mask plate, developing, and rinsing to form a mesa pattern, then post-baking to collapse the photoresist, and finally forming a mesa structure through ICP etching. The etching is carried out through two cycles, and the back of the wafer needs to be oiled.
[0056] The specific steps of etching micropores are: using photoresist as a mask, adopting the technology of reverse glue, spinning glue (5214E), pre-baking, exposing with a second mask plate, flooding, developing, and rinsing to form a pattern of etched micropores. There is no photoresist at the position where the holes need to be etched, and the photoresist is used as a barrier layer where the micropores do not need to be etched. Finally, the micropore array is obtained on the surface of the device through ICP etching technology.
[0057] The specific steps for the growth of the passivation layer are as follows: after etching the micropores, the passivation layer is grown. Silicon dioxide exists on the device surface, the bottom of the micropores and the sidewalls, which is used to reduce leakage and light reflection. First, a layer of silicon dioxide is grown as a sacrificial layer by alternating oxidation with dry oxygen, wet oxygen and dry oxygen; take out the sample that has been oxidized for the first time, put it into a buffered hydrofluoric acid solution for corrosion, remove the oxide layer formed by the first oxidation, and rinse it with deionized water; put the wafer into the oxidation furnace, and grow a dense silicon dioxide layer with a thickness of 10 to 200 nm by alternating oxidation with dry oxygen, wet oxygen and dry oxygen again; PECVD grows SiO2 with a thickness of 100 to 1000 nm; PECVD grows Si3N 4, Thickness 100~1000nm.
[0058] The specific steps of opening the window are as follows: the barrier layer is the SiO2 and Si3N4 grown by PECVD mentioned above, and the window pattern is formed by spinning (4620), pre-baking, exposing with a third mask plate, and developing, and then hardening the photoresist, and finally forming the window by ICP etching.
[0059] The specific steps for preparing the P electrode and the N electrode are as follows: use the fourth mask plate to photolithography the P-type electrode area on the photosensitive surface area, and use a buffered hydrofluoric acid solution to etch away the oxide layer at the electrode, and use magnetron sputtering Ti / Al / Ti / Au multilayer metal as the P-type electrode; the N-type ohmic contact is formed on the back of the substrate, and the specific steps are as follows: first, use photoresist to protect the front of the device, then use a buffered hydrofluoric acid solution to etch away the natural oxide layer on the back of the substrate, and then magnetron sputter Ni / Au as the N-type electrode; finally, the two electrodes are annealed at high temperature to form a good ohmic contact.
[0060] Pad preparation: Use the fifth mask plate to form the pad area by photolithography, and then magnetron sputter Ti / Au as the device's pad.
[0061] Preparation of surface metal nanoparticle arrays: First, a PS mask is prepared on the device surface using a PS microsphere suspension with a diameter of 100 to 1000 nm. Then, a metal film with a thickness of 5 to 50 nm is evaporated on the mask surface using electron beam evaporation technology. The PS mask is then peeled off using a tetrahydrofuran solution to obtain a surface metal nanoparticle array. The metal particles are present on the device surface, at the bottom of the micropores, and on the sidewalls of the micropores, and are arranged evenly and orderly.
[0062] When ultraviolet light is incident on the detector chip at different angles, the surface metal particles excite the plasmon field, which can induce the originally low electric field area in the device to reach the high field condition of avalanche. On the one hand, it expands the originally small local avalanche area at the microhole; on the other hand, it mainly induces the non-avalanche area or the area about to avalanche to reach the high electric field condition of avalanche.
[0063] The present invention induces the electric field in the wide bandgap semiconductor by exciting the plasmon field with metal nanoparticles, thereby expanding the avalanche region of the device, inducing the device to reach the avalanche condition in advance, and reducing the avalanche breakdown voltage to 30-40V; see the effect Figure 4 .
[0064] The above embodiments are only preferred embodiments of the present invention and cannot be considered to limit the scope of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.
Claims
1. A method for preparing a plasmon-enhanced local avalanche ultraviolet photodetector, characterized in that The following steps are involved: 1) Using chemical vapor transport homoepitaxial method on N + An N-type buffer layer and an i-type absorption layer are sequentially grown on a wide bandgap semiconductor substrate, and a P-type layer is then grown by chemical vapor deposition; 2) Etching the inclined terrace on the wide bandgap semiconductor epitaxial wafer of PiN structure by photolithography and ICP etching; 3) etching a microporous structure by photolithography and ICP etching; the microporous structure is opened from the P-type layer to the i-type absorption layer, so that the P-type layer is etched through to the i-type absorption layer, and the size and spacing of the microporous structure are set according to the excitation effect of the surface plasmon; 4) Using thermal oxidation and chemical vapor deposition techniques to grow a silicon dioxide passivation layer on the device surface, and using photolithography and ICP etching techniques to open windows; The specific steps of growing the silicon dioxide passivation layer are as follows: growing the passivation layer after etching the micropores, silicon dioxide exists on the device surface, the bottom of the micropores and the sidewalls, and its function is to reduce leakage and reflection of light. First, a layer of silicon dioxide is grown as a sacrificial layer by alternating oxidation with dry oxygen, wet oxygen and dry oxygen; taking out the sample that has been oxidized for the first time, putting it into a buffered hydrofluoric acid solution for corrosion, removing the oxide layer formed by the first oxidation, and rinsing it with deionized water; putting the wafer into an oxidation furnace, and growing a dense silicon dioxide layer again by alternating oxidation with dry oxygen, wet oxygen and dry oxygen; growing SiO2 by PECVD; growing Si3N4 by PECVD; The specific steps of the window opening are as follows: the barrier layer is the SiO2 and Si3N4 grown by PECVD, the window opening pattern is formed by spinning, pre-baking, exposure with a mask, and development, then hardening the photoresist to harden it, and finally forming the window by ICP etching; 5) The P electrode and N electrode are made by photolithography and magnetron sputtering. The specific steps are: use a mask to photolithography the P-type electrode area on the photosensitive surface area, and use a buffered hydrofluoric acid solution to etch off the oxide layer at the electrode, and use magnetron sputtering Ti / Al / Ti / Au multilayer metal as the P-type electrode; the N-type ohmic contact is formed on the back of the substrate. The specific steps are: first, use photoresist to protect the front of the device, then use a buffered hydrofluoric acid solution to etch off the natural oxide layer on the back of the substrate, and then magnetron sputter Ni / Au as the N-type electrode; finally, the two electrodes are annealed at high temperature to form a good ohmic contact; 6) Prepare a PS mask on the surface using a PS microsphere solution, deposit a metal film on the PS mask, and obtain a surface metal nanoparticle array after peeling off the PS mask. The specific steps are: first, prepare a PS mask on the device surface using a PS microsphere suspension, then evaporate a layer of metal film on the mask surface using electron beam evaporation technology, and then peel off the PS mask using a tetrahydrofuran solution to obtain a surface metal nanoparticle array; The diameter of the PS microsphere is 100 to 1000 nm; the shape of the metal nanoparticles is spherical, disc-shaped or triangular prism-shaped to better match the size; the material of the metal nanoparticles is selected from Al, Ag or Au; the metal nanoparticle array is evenly distributed on the device surface, the bottom of the micropores and the side walls of the micropores to better induce field enhancement in the semiconductor. When ultraviolet light is incident on the device surface at different angles, photon energy is obtained in both the horizontal and vertical directions, thereby maximizing the excitation surface plasmon field enhancement.
2. The method for preparing a plasmon-enhanced local avalanche ultraviolet photodetector according to claim 1, characterized in that In step 1), the doping concentration of the N-type buffer layer is 1×10 17 / cm 3 ~5×10 20 / cm 3 , the doping concentration of the i-type absorption layer is 1×10 14 / cm 3 ~2×10 16 / cm 3 , the doping concentration of the P-type layer is 1×10 17 / cm 3 ~5×10 20 / cm 3 .
3. The method for preparing a plasmon-enhanced local avalanche ultraviolet photodetector according to claim 1, characterized in that In step 1), the thickness of the N-type buffer layer is 0.5-3 μm; the thickness of the i-type absorption layer is 1-20 μm; and the thickness of the P-type layer is 0.1-1 μm.
4. The method for preparing a plasmon-enhanced local avalanche ultraviolet photodetector according to claim 1, characterized in that In step 4), the thickness of the silicon dioxide passivation layer is 10 to 1000 nm.
5. The method for preparing a plasmon-enhanced local avalanche ultraviolet photodetector according to claim 1, characterized in that In step 6), the thickness of the metal film is 5 to 50 nm. 6 . The plasmon-enhanced local avalanche ultraviolet photodetector prepared by the preparation method as claimed in any one of claims 1 to 5 .
Citation Information
Patent Citations
Deep ultraviolet MSM detector based on local surface plasmon effect and preparation method
CN110364584A
4H-SiC ultraviolet photoelectric detector with etched micropore structure and preparation
CN112117337A