A vitrification treatment method for lead-bismuth alloy nuclear waste
By oxidizing lead-bismuth alloy nuclear waste at high temperatures and using silicon compounds and boron compound additives to form heavy metal oxide glass, the problems of solidified body instability and insufficient compatibilization in the treatment of lead-bismuth alloy nuclear waste in the prior art are solved. Efficient and stable glass solidification formation and nuclear radiation shielding effects are achieved.
Patent Information
- Application Number
- CN202210612635.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-05-31
AI Technical Summary
Existing glass solidification technology is not suitable for lead-bismuth alloy nuclear waste. Traditional methods cannot form a stable glass solidified body, and cement solidification is detrimental to the volume expansion of the waste body, making it difficult to improve the durability of the waste.
By fully oxidizing the lead-bismuth alloy nuclear waste at high temperatures, using silicon compounds and boron compounds as additives to form heavy metal oxide glass, the lead and bismuth are oxidized and participate in the composition of the glass network, reducing the amount of additives and improving chemical stability and nuclear radiation shielding capabilities.
It achieves efficient solidification of lead-bismuth alloy nuclear waste, improves the containment rate and chemical stability of the glass solidified body, has excellent nuclear radiation shielding capabilities, has a simple process and low cost, and is suitable for the treatment of lead-bismuth alloy nuclear waste.
Smart Images

Figure BDA0003672514640000051 
Figure BDA0003672514640000061 
Figure HDA0003672514650000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radioactive nuclear waste treatment, and in particular to a glass solidification treatment method for lead-bismuth alloy nuclear waste. Background Art
[0002] Lead-bismuth alloy has good physical, thermal and chemical properties, and is the main candidate material for lead-cooled fast reactor coolant and ADS (Accelerator Driven Subcritical System) coolant and spallation target. When the reactor is in operation, the flowing liquid lead-bismuth alloy will cause a certain degree of corrosion to the structural materials, and the corrosion products will dissolve in the lead-bismuth alloy. Under the action of neutron activation, both the lead-bismuth alloy and the corrosion products will produce radioactive nuclides. In addition, if the fuel elements of the reactor are damaged, the fission products will also be released into the coolant, which will cause the lead-bismuth coolant to contain radioactive nuclides and generate lead-bismuth nuclear waste.
[0003] Lead-cooled fast reactors, as a typical representative of the fourth-generation nuclear energy system, are currently the focus of nuclear reactor research in countries around the world. Therefore, the treatment of lead-bismuth nuclear waste is particularly important. The chemical stability of lead-bismuth alloys is poor. If they come into contact with groundwater during the disposal process, it is easy to cause the migration of radioactive nuclides. Therefore, the lead-bismuth coolant containing radioactive nuclides needs to be solidified. At present, the treatment method of metal nuclear waste is usually to remelt or hot isostatic pressing, and then solidify it with cement. However, due to the poor chemical stability of lead-bismuth alloys themselves, hot isostatic pressing or remelting volume reduction treatment cannot improve the durability of the waste body. In addition, cement solidification significantly increases the volume of the waste body, which is not conducive to later disposal. In summary, it is necessary to develop a solidification method that can effectively treat lead-bismuth alloy nuclear waste.
[0004] The glass solidification method is a very good method for treating nuclear waste. In this method, nuclear waste and glass additives are first mixed in a certain proportion, then calcined and melted at high temperature to form a homogeneous glass liquid with the nuclear waste and glass additives, and finally cast to form a glass solid body. The specific principle can be referred to the review article published earlier by the inventor (Xu Kai. International Research Progress on Nuclear Waste Glass Solidification [J]. China Materials Progress, 2016, 35(7): 481). In this process, the toxic elements are fixed in the glass network structure at the atomic scale, effectively preventing them from migrating outward. In addition, the glass solid body with optimized formula design also has the advantages of corrosion resistance and high temperature resistance, making the glass solidification technology the only industrially applied high-level radioactive nuclear waste solidification treatment method in the world.
[0005] With the development of glass solidification technology, its application has gradually expanded to the solidification treatment of medium and low-level radioactive waste. For example, Li Lili and others invented a glass solidification body and a coordinated glass solidification method for non-combustible radioactive waste (CN113979642A). This technology provides a treatment method for the coordinated glass solidification of medium and low-level radioactive glass fibers with contaminated soil and concrete. Xu Kai and others invented a method for the coordinated glass solidification of medium and low-level radioactive glass fibers and combustible solid nuclear waste incineration ash (CN112382429A). This solution optimizes and designs the glass solidification formula based on the chemical composition characteristics of each nuclear waste, forming a formula library for the vitrification of medium and low-level radioactive mixed waste incineration ash in nuclear power plants.
[0006] Analysis shows that the existing glass solidification technology and glass solidification formula design are mainly aimed at oxide nuclear waste systems, while the main components of lead-bismuth alloy nuclear waste are metal lead and bismuth. This type of nuclear waste cannot form a stable glass solidification body after high-temperature treatment, which means that the traditional glass solidification method is not suitable for lead-bismuth alloy nuclear waste. Therefore, it is necessary to develop a glass solidification treatment method suitable for lead-bismuth alloy nuclear waste and develop a glass additive for solidifying lead-bismuth alloy. Summary of the invention
[0007] The present invention provides a glass solidification treatment method for lead-bismuth alloy nuclear waste, which comprises scheme a: heating and melting the lead-bismuth alloy nuclear waste and an additive, fully oxidizing the obtained material in a molten state, and finally cooling to obtain a glass solidified body; or scheme b: heating and melting the lead-bismuth alloy nuclear waste and fully oxidizing it, then adding an additive and continuing to heat to maintain the molten state, and finally cooling to obtain a glass solidified body.
[0008] Furthermore, the heating melting temperature of the mixture in scheme a is 700-1200° C., and the mixture is kept oxidized at this temperature for 0.5-10 hours.
[0009] Furthermore, in scheme b, the heating and melting temperature of the lead-bismuth alloy nuclear waste is 200-900°C, and it is kept warm for oxidation at this temperature for 0.5-5 hours. After adding the additive, the heating and melting temperature is 700-1200°C, and it is kept warm for 0.5-8 hours at this temperature.
[0010] Furthermore, the oxidation in scheme a or b is carried out in an oxygen-containing atmosphere, and the oxygen-containing gas is mixed into the molten liquid using a bubbling device or a stirring device to complete the oxidation reaction.
[0011] Furthermore, the additive is selected from at least one of silicon compounds and boron compounds.
[0012] Furthermore, the silicon compound is specifically SiO2, and the boron compound includes B2O3 and H3BO3.
[0013] Furthermore, the mass ratio of lead-bismuth alloy nuclear waste to additive is (100-x):x, where 4≤x≤30, preferably 95:5.
[0014] Furthermore, the lead-bismuth alloy nuclear waste originates from the lead-bismuth alloy coolant from the decommissioning of nuclear facilities (such as nuclear reactors or accelerator driven system cores).
[0015] Furthermore, the lead-bismuth alloy nuclear waste comprises (40-50) wt% of metal element Pb, (50-60) wt% of metal element Bi and no more than 5 wt% of contaminating nuclides.
[0016] Furthermore, the composition of the glass solidified body includes (25-50) wt% PbO, (35-60) wt% Bi2O3, no more than 30 wt% SiO2, no more than 35 wt% B2O3 and no more than 5 wt% of contaminating nuclide oxides.
[0017] In order to make lead-bismuth alloy nuclear waste suitable for glass solidification method, the present invention utilizes the characteristic that metal elements of lead and bismuth are easily oxidized at high temperature, introduces oxygen through an oxidation device and causes oxidation reaction at high temperature, so that lead-bismuth alloy is used as the network skeleton of radioactive waste glass in the form of oxide, thereby achieving the purposes of solidifying radioactive waste and safely disposing of nuclear facility decommissioning waste, and solving the problems of poor durability and capacity expansion of waste packages commonly existing in conventional treatment methods of metal nuclear waste.
[0018] Lead-bismuth alloy reactors use liquid lead-bismuth alloy as a coolant, which has the advantages of a low melting point. The melting temperature of lead-containing heavy metal oxide glass is generally lower than 1000°C. At this temperature, the volatilization of volatile radioactive nuclides can be effectively reduced, reducing the burden of tail gas treatment. In addition, heavy metal oxide glass has the characteristics of high density and is a commonly used nuclear radiation shielding window material. Lead-bismuth alloy coolants generally contain 45wt% of metal Pb and 55wt% of metal Bi. High-temperature oxidation is used to form ionic lead and bismuth, which can participate in the formation of the glass network, thereby reducing the amount of additives used. SiO2 and B2O3 are the basic components for forming the glass network and are also commonly used additives for forming heavy metal oxide glass. On the one hand, they can improve the forming ability of heavy metal oxide glass, and on the other hand, they can improve the chemical stability of the glass.
[0019] Compared with the traditional curing technology, the beneficial effects of the present invention are embodied in the following aspects:
[0020] (1) The lead-bismuth alloy is melted and oxidized at high temperature to form heavy metal ions, which then participate in the formation of a glass network, thereby reducing the amount of glass additives used. The resulting glass solid has a maximum inclusion rate of 96 wt% (in terms of oxide) for lead-bismuth waste;
[0021] (2) The test results show that the glass solidification body not only has good chemical stability, but also has excellent nuclear radiation shielding ability due to the presence of heavy metal ions;
[0022] (3) The method of the present invention has many advantages such as simple process, good effect and low cost, and has good technical feasibility and engineering application prospects in the treatment of lead-bismuth alloy nuclear waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a process flow chart of the present invention.
[0024] Figure 2 It is the XRD spectrum of the glass solidified body obtained in Example 1-3 of the present invention. DETAILED DESCRIPTION
[0025] In order to enable ordinary technicians in the field to fully understand the technical solutions and beneficial effects of the present invention, further description is given below in conjunction with specific embodiments and drawings.
[0026] The chemical composition of the lead-bismuth alloy raw material in Examples 1-4 of the present invention is: 44.72wt% Pb and 55.28wt% Bi. Simultaneously, TeO2 and NiO simulating nuclides are added to the alloy raw material in a total amount not exceeding 1.50wt%, wherein the addition amount of TeO2 is about 1.00wt% of the alloy raw material, and the addition amount of NiO is about 0.50wt% of the alloy raw material, thereby forming a lead-bismuth alloy simulating nuclear waste. The remaining raw materials are all commercially available unless otherwise specified.
[0027] Example 1
[0028] Reference Figure 1 In the process shown in the figure, 89g of lead-bismuth alloy simulated nuclear waste and 11g of SiO2 are added to a corundum crucible, and the corundum crucible is placed in an air atmosphere furnace and heated to 900°C to melt the material. After melting for 30 minutes, the stirring device is turned on for stirring. During the stirring process, oxygen enters the molten liquid and reacts with the metal element to produce an oxidation reaction. After stirring for 30 minutes, a uniform glass liquid is obtained, which is cast into a mold and cooled to form a glass solid body, and its chemical composition is shown in Table 1.
[0029] Table 1 Chemical composition of glass solidified bodies of Examples 1-4 (wt% of oxides)
[0030]
[0031] The solidified body obtained in this embodiment is homogeneous glassy when observed with naked eyes, and its X-ray diffraction pattern is as follows: Figure 2As shown in the figure, the spectrum is a typical amorphous diffraction peak. The density of the glass solid body measured by Archimedes drainage method is 7.16g / cm 3 .
[0032] The chemical stability of the glass solid body sample was evaluated according to the 7-day product consistency test (PCT) standard (ASTM C 1285-02), and the results are shown in Table 2. As can be seen from the table, the leaching values of each element in the glass solid body are all lower than 1 g / m 2 , meeting the chemical stability requirements of nuclear waste vitrified bodies.
[0033] Table 2 leaching results of PCT-7 glass solidified body of Example 1-3 (g / m 2 )
[0034]
[0035] Note: ND*Not Detected
[0036] Example 2
[0037] 475g of lead-bismuth alloy simulated nuclear waste, 15g of SiO2, and 10g of B2O3 (mass ratio 47.5:1.5:1) were added to a corundum crucible, and the corundum crucible was placed in an air atmosphere furnace and heated to 800°C to melt the material. After melting for 60 minutes, the stirring device was turned on for stirring. During the stirring process, oxygen entered the molten liquid and reacted with the metal element for oxidation. After stirring for 90 minutes, a uniform glass liquid was obtained, which was cast into a mold and cooled to obtain a glass solid body, and its chemical composition is shown in Table 1.
[0038] The solidified body obtained in this example is homogeneous glassy when observed with naked eyes, and its X-ray diffraction pattern ( Figure 2 ) is also a typical amorphous diffraction peak. The density of the glass solid body measured by Archimedes drainage method is 7.54 g / cm 3 Under the same test standards and conditions, the leaching values of each element in the glass solid body are all lower than 1g / m 2 (Table 2), meeting the chemical stability requirements of nuclear waste glass solidification.
[0039] Example 3
[0040] 192g of lead-bismuth alloy simulated nuclear waste and 8g of B2O3 were added to a corundum crucible, and the corundum crucible was placed in an air atmosphere furnace and heated to 750°C to melt the material. After melting for 30 minutes, the stirring device was turned on for stirring. During the stirring process, oxygen entered the molten liquid and reacted with the metal element for oxidation. After stirring for 60 minutes, a uniform glass liquid was obtained, which was cast into a mold and cooled to obtain a glass solid body, and its chemical composition is shown in Table 1.
[0041] The solidified body obtained in this example is homogeneous glassy when observed with naked eyes, and its X-ray diffraction pattern ( Figure 2 ) is also a typical amorphous diffraction peak. The density of the glass solid body measured by Archimedes drainage method is 7.73g / cm 3 Under the same test standards and conditions, the leaching values of each element in the glass solid body are all lower than 1g / m 2 (Table 2), meeting the chemical stability requirements of nuclear waste glass solidification.
[0042] Example 4
[0043] 270g of lead-bismuth alloy simulated nuclear waste was added to a corundum crucible, and the corundum crucible was placed in an air atmosphere furnace and heated to 800℃ to melt the material. During the stirring process, the stirring device was turned on. During the stirring process, oxygen entered the molten liquid and reacted with the metal element to produce an oxidation reaction. After 60 minutes of melting and stirring, 30g of SiO2 was added to the corundum crucible, and then the furnace temperature was raised to 900℃ and kept at this temperature. Stirring was continued for 30 minutes to obtain a uniform glass liquid, which was cast into a mold and cooled to obtain a glass solid body. Its chemical composition is shown in Table 1.
Claims
1. A method for vitrification treatment of lead-bismuth alloy nuclear waste, characterized in that The method comprises the following steps: The lead-bismuth alloy nuclear waste is mixed with additives, heated and melted, then fully oxidized, and finally cooled to obtain a glass solid; Alternatively, the lead-bismuth alloy nuclear waste is heated to melt and fully oxidized, and then additives are added to continue heating and melting, and finally cooled to obtain a glass solid.
2. The method according to claim 1, characterized in that: The mixture of lead-bismuth alloy nuclear waste and additives is heated to a melting temperature of 700-1200°C and is kept oxidized at this temperature for 0.5-10 hours.
3. The method according to claim 1, characterized in that: The heating and melting temperature of lead-bismuth alloy nuclear waste is 200-900°C, and it is kept warm for oxidation at this temperature for 0.5-5 hours; the heating and melting temperature after adding additives is 700-1200°C, and it is kept warm for 0.5-8 hours at this temperature.
4. The method according to claim 1, characterized in that: The material is oxidized in an oxygen-containing atmosphere, and the oxygen-containing gas is mixed into the molten liquid using a bubbling device or a stirring device to complete the oxidation reaction.
5. The method according to claim 1, characterized in that: The additive is selected from at least one of silicon compounds and boron compounds.
6. The method according to claim 5, characterized in that: The silicon compound is specifically SiO2, and the boron compound includes B2O3 and H3BO3.
7. The method according to claim 1, wherein: The mass ratio of lead-bismuth alloy nuclear waste to the additive is (100-x): x, where 4≤x≤30.
8. The method according to claim 7, characterized in that: The mass ratio of lead-bismuth alloy nuclear waste to additives is 95:
5.
9. The method according to claim 1, characterized in that: The lead-bismuth alloy nuclear waste is derived from the lead-bismuth alloy coolant of decommissioned nuclear facilities.
10. The method according to claim 1 or 9, characterized in that: The lead-bismuth alloy nuclear waste comprises (40-50) wt% of a metal element Pb, (50-60) wt% of a metal element Bi and no more than 5 wt% of nuclides.
11. The method according to claim 1, characterized in that: The composition of the glass solidified body includes (25-50) wt% PbO, (35-60) wt% Bi2O3, no more than 30 wt% SiO2, no more than 35 wt% B2O3 and no more than 5 wt% nuclide oxide.