A method for preparing carbon nanotube / copper composite wire
Through electrophoretic deposition and multiple folding hot pressing processes, combined with drawing and annealing treatment, the problem of degradation of the conductivity of CNTs/Cu composite materials was solved, and carbon nanotube/copper composite wire with excellent strength and conductivity was prepared to realize The uniform dispersion and efficient combination of CNTs and copper are achieved.
Patent Information
- Application Number
- CN202210839080.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-07-18
AI Technical Summary
In the prior art, when preparing carbon nanotube reinforced copper-based composite materials, the conductivity decreases with the increase of CNTs content. The carbon nanotube/copper composite materials prepared by powder metallurgy process are not suitable for use in silk material production, and the materials are dispersed and heated. During the pressing process, the problem of agglomeration and interface bonding are prone to occur.
Electrophoretic deposition and dispersed CNTs, and the drawing blank was prepared by repeated folding and hot pressing. Combined with drawing and annealing treatment, CNTs/Cu composite wire material with excellent strength and conductivity was prepared. Specific steps include ultrasonic dispersing of acidified CNTs and hydrated aluminum nitrate in anhydrous ethanol, folding and hot pressing after electrophoretic deposition, and then drawing and annealing to improve the binding effect of CNTs and copper.
The electrical conductivity and tensile strength of CNTs/Cu composite wires are improved, and the problems of CNTs agglomeration and interface bonding are avoided, and composite materials with excellent strength and conductivity are obtained.
Smart Images

Figure CN115255020B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a carbon nanotube / copper composite wire material, and belongs to the technical field of material processing. Background Art
[0002] Since its discovery in 1991, CNTs have attracted widespread attention due to their excellent mechanical properties, electrical properties, and physical and chemical properties. CNTs are a nanoscale tubular structure material composed of carbon atoms with a large aspect ratio of up to 1.32×10 8 :1, and is one of the materials with the largest aspect ratio known so far; due to the special structure of CNTs at the nanoscale, CNTs become an ideal reinforcement material. Currently, composite materials reinforced with CNTs have been successfully applied in the fields of automobiles, aerospace, and industrial machinery. Therefore, the research on CNTs is a research hotspot. So far, due to the special structure and excellent performance of CNTs, CNTs have become a common reinforcement for metal-based composite materials.
[0003] In the research of metal matrix composite materials, a large number of studies have shown that the performance of the reinforced metal matrix composite materials has been greatly improved by compounding CNTs into metal materials such as magnesium, aluminum, titanium, and copper. Copper matrix composite materials are particularly suitable for use in the electrical field because of their good electrical conductivity, high wear resistance, and high corrosion resistance. Therefore, CNTs / Cu composite wires have broad application prospects. Although traditional fiber reinforcements can increase the strength of materials, they often reduce their electrical conductivity. Therefore, the development of copper matrix composite materials with excellent electrical conductivity and high strength is one of the current problems that need to be solved urgently.
[0004] In the process of preparing carbon nanotube-reinforced metal-based composites, it is often inevitable to encounter problems such as CNTs agglomeration, the interface bonding between CNTs reinforcement and metal matrix is hindered, and the CNTs structure is destroyed during dispersion and hot pressing. In recent years, there have been a large number of studies and reports showing that the use of powder metallurgy to prepare CNTs / Cu composites can greatly improve the strength of metal-based materials, but its conductivity will decrease. For example, Wang Yan found in the preparation and performance research of carbon nanotube / copper composites that the conductivity of carbon nanotube / copper composites decreases with the increase of CNTs content. Therefore, the carbon nanotube / copper composites prepared by powder metallurgy are not suitable for the production of wires. Therefore, it is of great significance to develop a new method for preparing carbon nanotube-reinforced copper-based composite wires by electrophoretic deposition. Summary of the invention
[0005] In order to solve the above-mentioned problems, the purpose of the present invention is to provide a method for preparing a carbon nanotube / copper composite wire with excellent strength and conductivity, which is to first disperse CNTs by electrophoretic deposition, then repeatedly fold and hot press to prepare a drawn blank, and obtain a CNTs / Cu composite wire by drawing and annealing, which specifically includes the following steps:
[0006] (1) The acidified CNTs are added to anhydrous ethanol for ultrasonic dispersion, and then hydrated aluminum nitrate is added for further ultrasonic dispersion, so that the CNTs and hydrated aluminum nitrate are fully dispersed to prepare a uniformly dispersed electrophoresis solution; the Al in the electrophoresis solution 3+ It is easy to attract hydroxyl and carboxyl groups, making CNTs easier to attach to Al 3+ Move toward the cathode to improve the efficiency of electrophoretic deposition.
[0007] (2) Using copper foil as cathode and stainless steel plate as anode, electrophoretic deposition is performed to obtain copper foil with CNTs deposited thereon; CNTs are effectively and evenly deposited on the surface of the copper foil, effectively avoiding stress and defects caused by uneven distribution of CNTs, which helps to improve the strength of the CNTs / Cu composite material and facilitates the recombination of CNTs and Cu during the next step of hot pressing.
[0008] (3) folding the copper foil obtained in step (2) for multiple times, and then hot pressing, repeating the folding and hot pressing steps multiple times to fully combine the CNTs and copper to form a CNTs / Cu composite blank, and forging the composite blank into a CNTs / Cu composite rod; since the surface area of the copper foil increases during hot pressing, the oxide film that has not been cleaned off in step (1) is torn apart, exposing more fresh copper foil surface to fully composite with the CNTs, and the obtained composite material has a better interface bonding effect, thereby improving its conductivity and tensile strength.
[0009] (4) placing the CNTs / Cu composite rod obtained in step (3) into a drawing device for drawing to obtain a CNTs / Cu composite wire, annealing the drawn wire, and then cooling it in a furnace to obtain a CNTs / Cu composite wire.
[0010] Preferably, the concentration of CNTs in the electrophoresis solution in step (1) of the present invention is 0.01-0.03 g / L, and the concentration of hydrated aluminum nitrate is 0.02-0.06 g / L.
[0011] Preferably, the ultrasonic frequency in step (1) of the present invention is in the range of 25 to 70 KHz.
[0012] Preferably, in step (2) of the present invention, the distance between the anodes is 3 cm, the DC voltage is maintained at 30 V, and the deposition is performed for 30 minutes.
[0013] Preferably, the hot pressing temperature of the present invention is selected to be 300-500° C., the hot pressing pressure is selected to be 80-100t, the hot pressing is repeated 3-5 times, the heat preservation time is 2-4h, and then the furnace is cooled.
[0014] Preferably, the annealing treatment temperature in step (4) of the present invention is in the range of 200 to 400° C. and the time is 1 to 3 hours.
[0015] Preferably, in step (4) of the present invention, the diameter of the solid round rod is 5 mm, and the diameter of the wire is 2 mm.
[0016] The present invention deposits CNTs by electrophoretic deposition to achieve the purpose of uniformly dispersing CNTs on the surface of copper foil, thereby solving the problem that the use of powder metallurgy to prepare CNTs-reinforced metal-based composite wires only unilaterally improves mechanical properties while reducing conductivity; in addition, during the preparation process of the present invention, the material is first maintained under a certain pressure for a certain period of time and then hot-pressed. This process can effectively squeeze out the air, avoid the formation of oxide films and defects, and obtain CNTs / Cu composite wires with improved strength and conductivity.
[0017] Beneficial effects of the present invention:
[0018] (1) The process method described in the present invention is simple, easy to operate and has low cost. The present invention achieves the effect of uniformly dispersing CNTs on copper foil by electrophoretic deposition, avoids poor composite effect caused by CNTs agglomeration, and realizes effective combination of copper foil and CNTs.
[0019] (2) The present invention enables CNTs to better contact with fresh metal through multiple folding and hot pressing, effectively eliminates oxygen at the bonding interface, and obtains a high interface bonding rate, thereby solving the problem of unilaterally improving strength but reducing conductivity when using powder metallurgy technology to prepare carbon nanotube-reinforced metal-based composite materials.
[0020] (3) The present invention effectively utilizes the excellent properties of CNTs and realizes the direct composite of metal matrix and CNTs through multiple hot pressing processes, effectively avoiding the generation of defects such as oxidation inclusions and holes, and obtaining a metal matrix composite material with improved conductivity and strength. This composite material with both excellent strength and conductivity is drawn into wires, and then annealed to obtain CNTs / Cu composite wires with both excellent strength and conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the process flow of the present invention;
[0022] Figure 2 This is the SEM image of the composite blank fracture obtained in Example 1;
[0023] Figure 3 This is the SEM image of the composite blank fracture obtained in Example 2;
[0024] Figure 4 This is the SEM image of the fracture of the composite blank obtained in Example 3. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to the contents described above;
[0026] The material used in the experiment in the embodiment of the present invention is a high-purity copper foil with a thickness of 0.2 mm, a length of 20 mm, and a width of 20 mm. In the actual process, the size of the copper foil is determined according to the needs.
[0027] Example 1
[0028] A method for preparing a carbon nanotube / copper composite wire material specifically comprises the following steps:
[0029] (1) Preparation of copper foil: Surface treatment of the copper foil is performed. The copper foil is cleaned with dilute hydrochloric acid to remove the surface oxide layer and oil stains, and the surface of the copper foil is polished to ensure that the copper foil is smooth and flat. In this embodiment, high-purity copper foil is selected with specifications of 0.2 mm thick, 20 mm wide and 20 mm long.
[0030] (2) Acidification of CNTs: Mix 25 ml of concentrated sulfuric acid and 75 ml of concentrated nitric acid, add 1 g of original CNTs, and ultrasonically vibrate in a water bath at 60°C for 5 h. Then pour the mixed acid solution into distilled water, dilute and filter. Then, continue to mix the filtered CNTs with distilled water and stir, then wash and filter. Repeat this process until the solution becomes neutral. Finally, dry the CNTs in a vacuum oven for use to obtain functionalized CNTs.
[0031] (3) Weigh 0.01 g of the acid-washed carbon nanotubes, dissolve them in 1000 ml of ethanol and disperse them ultrasonically for 3 h at an ultrasonic frequency of 25 kHz. Then, take 0.02 g of hydrated aluminum nitrate and disperse them ultrasonically for another 1 h to prepare a uniformly dispersed electrophoresis solution.
[0032] (4) Electrophoretic deposition: With copper foil as cathode and stainless steel plate as anode, electrophoretic deposition was performed at a certain voltage to obtain copper foil with CNTs deposited thereon. The distance between the anode and cathode was kept at 3 cm, and electrophoretic deposition was performed at a voltage of 30 V for 30 min.
[0033] (5) Vacuum hot pressing: Fold the copper foil in step (4) twice, then put it into a vacuum hot press, set appropriate temperature and pressure for pressing, repeat 3 steps of folding and hot pressing to fully combine CNTs and copper to form a CNTs / Cu composite blank; the hot pressing temperature is 300°C, the hot pressing pressure is 80t, and the hot pressing time is 2h each time.
[0034] (6) The CNTs / Cu composite blank in (5) is placed in a mold to form a 5 mm CNTs / Cu composite rod. The rod-shaped material is placed in a drawing device for drawing to form a CNTs / Cu composite wire with a diameter of 2 mm. The drawn wire is placed in an annealing furnace, annealed at 200°C for 1 h, and then cooled in the furnace.
[0035] Performance test: Conduct electrical conductivity and mechanical properties of the manufactured wires, and compare them with the electrical conductivity and tensile properties of pure copper.
[0036] The conductivity of pure copper foil was measured to be 95% IACS, and the conductivity of CNTs / Cu composite wire after annealing was 96.9% IACS, which was 2% higher than that of pure copper.
[0037] The tensile strength of pure copper was measured to be 183 MPa, and the tensile strength of the final CNTs / Cu composite wire was 196 MPa, which was 7.1% higher than that of pure copper.
[0038] Figure 2 This is the SEM image of the composite billet fracture obtained in Example 1. It can be seen from the figure that there are obvious dimples at the fracture of the billet, and the billet has debonded. After the billet is forged into a rod, it is drawn and annealed to obtain a CNTs / Cu composite wire. At this time, the strength and conductivity of the CNTs / Cu composite wire are improved compared to pure copper.
[0039] Example 2
[0040] A method for preparing a carbon nanotube / copper composite wire material specifically comprises the following steps:
[0041] (1) Preparation of copper foil: Surface treatment of the copper foil is performed. The copper foil is cleaned with dilute hydrochloric acid to remove the surface oxide layer and oil stains, and the surface of the copper foil is polished to ensure that the copper foil is smooth and flat. In this embodiment, high-purity copper foil is selected with specifications of 0.2 mm thick, 20 mm wide and 20 mm long.
[0042] (2) Acidification of CNTs: Mix 25 ml of concentrated sulfuric acid and 75 ml of concentrated nitric acid, add 1 g of original CNTs, and ultrasonically vibrate in a water bath at 60°C for 5 h. Then pour the mixed acid solution into distilled water, dilute and filter. Then, continue to mix the filtered CNTs with distilled water and stir, then wash and filter. Repeat this process until the solution becomes neutral. Finally, dry the CNTs in a vacuum oven for use to obtain functionalized CNTs.
[0043] (3) Weigh 0.02 g of the acid-washed carbon nanotubes, dissolve them in 1000 ml of ethanol and disperse them ultrasonically for 3 h at an ultrasonic frequency of 50 kHz. Then take 0.04 g of hydrated aluminum nitrate and disperse them ultrasonically for another 1 h to prepare a uniformly dispersed electrophoresis solution.
[0044] (4) Electrophoretic deposition: With copper foil as cathode and stainless steel plate as anode, electrophoretic deposition was performed at a certain voltage to obtain copper foil with CNTs deposited thereon; the distance between the anode and cathode was kept at 3 cm, and electrophoretic deposition was performed at a voltage of 30 V for 30 min.
[0045] (5) Vacuum hot pressing: Fold the copper foil in step (4) twice and then put it into a vacuum hot press. The hot pressing temperature is 400°C and the hot pressing pressure is 90t. The hot pressing is kept for 3 hours each time. Folding and hot pressing are repeated 4 times to fully combine CNTs and copper to form a CNTs / Cu composite blank.
[0046] (6) The CNTs / Cu composite blank in (5) is placed in a mold to form a 5 mm CNTs / Cu composite rod, the rod-shaped material is placed in a drawing device for drawing to form a 2 mm CNTs / Cu composite wire, and the drawn wire is placed in an annealing furnace for annealing at 300 ° C for 2 h, and then cooled in the furnace.
[0047] Performance test: Conduct electrical conductivity and mechanical properties of the manufactured wires, and compare them with the electrical conductivity and tensile properties of pure copper.
[0048] The electrical conductivity of the high-purity copper foil was measured to be 95% IACS, and the electrical conductivity of the CNTs / Cu composite wire after annealing was 98.1% IACS, which was 3.2% higher than that of pure copper.
[0049] The tensile strength of pure copper was measured to be 183 MPa, and the tensile strength of the final CNTs / Cu composite wire was 213 MPa, which was 16.4% higher than that of pure copper.
[0050] Figure 3 This is the SEM image of the composite billet fracture obtained in Example 2. It can be seen from the figure that the number of dimples at the fracture is further increased compared with that in Example 1, obvious bridging phenomenon occurs, and the debonding phenomenon is not obvious. The strength and conductivity of the CNTs / Cu composite wire finally obtained are significantly improved compared with those in Example 1.
[0051] Example 3
[0052] A method for preparing a carbon nanotube / copper composite wire material specifically comprises the following steps:
[0053] (1) Preparation of copper foil: Surface treatment of the copper foil is performed. The copper foil is cleaned with dilute hydrochloric acid to remove the surface oxide layer and oil stains, and the surface of the copper foil is polished to ensure that the copper foil is smooth and flat. In this embodiment, high-purity copper foil is selected with specifications of 0.2 mm thick, 20 mm wide and 20 mm long.
[0054] (2) Acidification of CNTs: Mix 25 ml of concentrated sulfuric acid and 75 ml of concentrated nitric acid, add 1 g of original CNTs, and ultrasonically vibrate in a water bath at 60°C for 5 h. Then pour the mixed acid solution into distilled water, dilute and filter. Then, continue to mix the filtered CNTs with distilled water and stir, then wash and filter. Repeat this process until the solution becomes neutral. Finally, dry the CNTs in a vacuum oven for use to obtain functionalized CNTs.
[0055] (3) Weigh 0.03 g of the acid-washed carbon nanotubes, dissolve them in 1000 ml of ethanol and disperse them ultrasonically for 3 h at an ultrasonic frequency of 75 kHz. Then, take 0.06 g of hydrated aluminum nitrate and disperse them ultrasonically for another 1 h to prepare a uniformly dispersed electrophoresis solution.
[0056] (4) Electrophoretic deposition: With copper foil as cathode and stainless steel plate as anode, electrophoretic deposition was performed at a certain voltage to obtain copper foil with CNTs deposited thereon; the distance between the anode and cathode was kept at 3 cm, and electrophoretic deposition was performed at a voltage of 30 V for 30 min.
[0057] (5) Vacuum hot pressing: Fold the copper foil in step (4) twice and then put it into a vacuum hot press. Set the hot pressing temperature to 500°C and the hot pressing pressure to 100t. Keep the hot pressing temperature for 4 hours each time. Repeat the folding and hot pressing for 5 times to fully combine the CNTs and copper to form a CNTs / Cu composite blank.
[0058] (6) The CNTs / Cu composite blank in (5) is placed in a mold to form a 5 mm CNTs / Cu composite rod. The rod-shaped material is placed in a drawing device for drawing to form a 2 mm CNTs / Cu composite wire. The drawn wire is placed in an annealing furnace, annealed at 400 °C for 3 h, and then cooled in the furnace.
[0059] Performance test: Conduct electrical conductivity and mechanical properties of the manufactured wires, and compare them with the electrical conductivity and tensile properties of pure copper.
[0060] The electrical conductivity of the high-purity copper foil was measured to be 95% IACS, and the electrical conductivity of the CNTs / Cu composite wire after annealing was 99% IACS, which was 4.2% higher than that of pure copper.
[0061] The tensile strength of pure copper was measured to be 183 MPa, and the tensile strength of the final CNTs / Cu composite wire was 231 MPa, which was 26.2% higher than that of pure copper.
[0062] Figure 4 This is the SEM image of the fracture of the composite billet obtained in Example 3. It can be seen from the figure that, compared with Example 2, the dimples at the fracture are further increased, the bridging phenomenon is more obvious, and the debonding phenomenon almost disappears. The billet is forged, drawn and annealed to obtain CNTs / Cu composite wires. At this time, the strength and conductivity of the composite wires are the best.
[0063] The strength and conductivity of the CNTs / Cu composite wires obtained in the above three embodiments are improved compared with pure copper, and from Example 1 to Example 3, the strength and conductivity of the CNTs / Cu composite wires obtained are gradually increased. This is mainly due to the different hot pressing parameters. The higher the hot pressing temperature and the greater the pressure, the better the bonding effect of CNTs and the copper matrix in the obtained CNTs / Cu composite wire, and the reinforcement effect of CNTs is fully exerted. Moreover, the better the bonding effect, the smaller the contact resistance between CNTs and the copper matrix, which is more conducive to the improvement of conductivity.
Claims
1. A method for preparing a carbon nanotube / copper composite wire, characterized in that: The specific steps include: (1) adding the acidified CNTs into anhydrous ethanol for ultrasonic dispersion, and then adding hydrated aluminum nitrate for further ultrasonic dispersion, so that the CNTs and hydrated aluminum nitrate are fully dispersed to prepare a uniformly dispersed electrophoresis solution; (2) Using copper foil as cathode and stainless steel plate as anode, electrophoretic deposition is performed to obtain copper foil with CNTs deposited on it; (3) folding the copper foil obtained in step (2) for multiple times, and then hot pressing, repeating the folding and hot pressing steps for multiple times to fully combine the CNTs and copper to form a CNTs / Cu composite blank, and then forging the composite blank into a CNTs / Cu composite rod; (4) placing the CNTs / Cu composite rod obtained in step (3) into a drawing device for drawing to obtain a CNTs / Cu composite wire, annealing the drawn wire, and then cooling it in a furnace to finally obtain a CNTs / Cu composite wire; The hot pressing temperature is selected to be 300-500°C, the hot pressing pressure is selected to be 80-100t, the hot pressing is repeated 3-5 times, the heat preservation time is 2-4h, and then the furnace is cooled; The annealing temperature ranges from 200 to 400°C and the time ranges from 1 to 3 hours.
2. The method for preparing the carbon nanotube / copper composite wire according to claim 1, characterized in that: The acidification process of the CNTs in step (1) is as follows: concentrated sulfuric acid and concentrated nitric acid are mixed in a volume ratio of 3:1, and original CNTs are added in a ratio of 1 g of carbon nanotubes per 100 ml of acid solution, and the mixture is placed in a water bath at 60°C. After ultrasonic vibration for 5 hours, the mixed acid solution is poured into distilled water, diluted and filtered, and then the CNTs obtained by filtration are further mixed with distilled water and stirred, and then washed and filtered. This process is repeated until the solution becomes neutral, and finally the CNTs are dried in a vacuum oven for use to obtain functionalized CNTs.
3. The method for preparing the carbon nanotube / copper composite wire according to claim 1 or 2, characterized in that: In the electrophoresis solution of step (1), the concentration of CNTs is 0.01-0.03 g / L, and the concentration of hydrated aluminum nitrate is 0.02-0.06 g / L.
4. The method for preparing the carbon nanotube / copper composite wire according to claim 3, characterized in that: The ultrasonic frequency range in step (1) is 25 to 70 kHz.
5. The method for preparing the carbon nanotube / copper composite wire according to claim 4, characterized in that: In step (2), the distance between the cathode and the anode was 3 cm, the DC voltage was maintained at 30 V, and the deposition was performed for 30 min.
6. The method for preparing the carbon nanotube / copper composite wire according to claim 5, characterized in that: In step (4), the diameter of the solid round rod is 5 mm, and the diameter of the wire is 2 mm.