A method for selectively preparing phenolic compounds by catalyzing guaiacol

By dispersing ruthenium-containing catalysts at the atomic level in hydrodeoxygenation reactions, the problems of poor selectivity and insufficient activity of existing catalysts are solved, efficient preparation of phenolic compounds is achieved, and the activity of the catalyst and product purity are improved.

CN115894177BActive Publication Date: 2024-10-18GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211295601.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-10-18
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing catalysts have poor selectivity in hydrodeoxygenation reactions. Traditional CoMoS and NiMoS catalysts are prone to deactivation. The cost of precious metal catalysts is high. In industrial applications, cheap metal nickel catalysts have dispersed product distribution and unsatisfactory reaction conditions.

Method used

Atomic-level dispersed ruthenium-containing catalysts are used to prepare nanoparticle ruthenium-containing catalysts through impregnation or impregnation-carbonization methods, which are used in the hydrodeoxygenation reaction of guaiacol to achieve highly selective synthesis of phenolic compounds.

Benefits of technology

The yield and selectivity of phenolic compounds are improved, the generation of benzene ring saturated products is reduced, and the catalyst has high activity and reusability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115894177B_ABST
    Figure CN115894177B_ABST
Patent Text Reader

Abstract

The invention discloses a method for selectively preparing phenolic compounds by catalyzing guaiacol. The method uses a ruthenium-containing catalyst to catalyze the hydrodeoxygenation reaction of guaiacol to achieve highly selective synthesis of phenolic compounds, and specifically comprises the following steps: dissolving guaiacol in an organic solvent to obtain a guaiacol solution, then adding a ruthenium-containing catalyst to the guaiacol solution, sealing and replacing the air in the reaction container with hydrogen, and finally introducing hydrogen not exceeding 5MPa into the reaction container, the reaction temperature is 200°C to 270°C, the reaction time is 0.5 to 12h, the mass of the ruthenium-containing catalyst is 1 to 50wt% of the mass of guaiacol, and phenolic compounds are obtained. The present invention uses a ruthenium-containing catalyst to prepare phenolic compounds (phenol, o-cresol, m-cresol and p-cresol) with high catalytic activity, and finally makes the prepared phenolic compounds have high yield and selectivity, and guaiacol has a high conversion rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of organic matter preparation, and in particular to a method for selectively preparing phenolic compounds by catalyzing guaiacol. Background technology:

[0002] Biomass energy is an important component of renewable energy, with the characteristics of large reserves, low pollution, and carbon neutrality. As an important component of biomass lignocellulose, lignin is composed of a variety of methoxyphenylpropane units and is a potential substitute for traditional aromatic hydrocarbon resources. The liquid products obtained from lignin cracking contain a large number of oxygen-containing compounds, especially a large number of guaiacol-based phenolic derivatives, and the lignin liquefaction products need to be treated by efficient catalytic hydrogenation and deoxygenation process.

[0003] At present, the research on bio-oil hydrodeoxygenation mainly uses lignin structural unit compounds as model compounds, and guaiacol is one of the commonly used model compounds. Traditional CoMoS and NiMoS catalysts are subject to certain restrictions in industrial application due to the easy deactivation of the catalyst. Precious metal catalysts are difficult to promote and use in industrial production due to their high cost. Cheap metal nickel is low in cost and is a commonly used hydrogenation catalyst in industry, but its selectivity is poor, and the product distribution is mostly relatively dispersed, usually including phenol compounds, benzene derivatives and benzene ring saturated products. There are also problems such as long reaction time and high reaction temperature in the reaction conditions. The existing problems need to be solved urgently. Summary of the invention:

[0004] The present invention solves the problems existing in the prior art and provides a method for selectively preparing phenolic compounds by catalyzing guaiacol. The present invention uses an atomic-level dispersed ruthenium-containing catalyst to prepare phenolic compounds (phenol, o-cresol, m-cresol and p-cresol) with high catalytic activity, and ultimately enables the prepared phenolic compounds to have a high yield and selectivity, and guaiacol to have a high conversion rate.

[0005] The present invention aims to provide a method for selectively preparing phenolic compounds by catalyzing guaiacol. A nanoparticle ruthenium-containing catalyst prepared by an impregnation method or an atomic-level dispersed ruthenium-containing catalyst prepared by an impregnation-carbonization method is used to catalyze the hydrodeoxygenation reaction of guaiacol, so as to achieve high-selective synthesis of phenolic compounds. The method specifically comprises the following steps: dissolving guaiacol in an organic solvent to obtain a guaiacol solution, then adding the ruthenium-containing catalyst to the guaiacol solution, sealing the reaction container, replacing the air in the reaction container with hydrogen, and finally introducing hydrogen at a pressure of no more than 5MPa into the reaction container. The reaction temperature is 230°C to 270°C, the reaction time is 0.5 to 12h, the mass of the ruthenium-containing catalyst is 1 to 50wt% of the mass of the guaiacol, and the phenolic compounds are obtained.

[0006] Preferably, the organic solvent is selected from at least one of n-hexane, n-octane, n-decane, dodecane and decahydronaphthalene. The reaction temperature of the above reaction is 230° C. to 270° C., the reaction time is 0.5 to 8 hours, and the hydrogen pressure is 0.5-3.0 MPa.

[0007] Preferably, the phenolic compounds include phenol, o-cresol, m-cresol and p-cresol.

[0008] Preferably, the mass of the ruthenium-containing catalyst is 30-50wt% of the mass of guaiacol, and the mass volume ratio of the ruthenium-containing catalyst to the organic solvent is 6.25 mg / mL.

[0009] Preferably, the ruthenium-containing catalyst is a nanoparticle ruthenium-containing catalyst in which ruthenium is loaded onto a carrier by impregnation using a solution of a ruthenium-containing compound, or an atomically dispersed ruthenium-containing catalyst prepared by an impregnation-carbonization method with face-centered cubic α-MoC as a carrier, and the amount of ruthenium loaded in the ruthenium-containing catalyst is 0.1 to 5 wt% of the catalyst mass. More preferably, the amount of ruthenium loaded in the ruthenium-containing catalyst is 0.1 to 3 wt% of the catalyst mass.

[0010] More preferably, the carrier is selected from at least one of α-MoC, MoO3, TiO2, ZrO2, Al2O3, SiO2, activated carbon and S-1 zeolite molecular sieve. The carrier (α-MoC) used in the impregnation method or impregnation-carbonization method is obtained by calcining ammonium molybdate at 500°C for 4 hours.

[0011] Further preferably, the impregnation method includes the following steps: dissolving the ruthenium-containing compound in a corresponding solvent to form a solution with a concentration of 0.01 to 4 wt%; then uniformly loading the ruthenium on the surface of the carrier by dropping and stirring, drying after stirring at room temperature, and calcining to obtain a reaction powder; reducing the reaction powder with a mixture of H2 and N2 at 450°C to 550°C for 3.5-4.5h to obtain a nanoparticle ruthenium-containing catalyst.

[0012] The impregnation method specifically includes the following steps: dissolving a ruthenium-containing compound in a corresponding solvent to prepare a solution with a concentration of 0.01-4wt%; then uniformly loading ruthenium on the surface of the carrier by dropping and stirring, stirring at room temperature for 12 hours; then evaporating to dryness while stirring at 80°C-120°C, drying in an oven at 80°C-120°C for 6-12 hours, and then calcining at 500°C for 4 hours to obtain a reaction powder; the reaction powder is heated from room temperature to 500°C at a heating rate of 5°C / min in a tube furnace with a mixture of H2 and N2, and reduced for 4 hours to obtain a nanoparticle ruthenium-containing catalyst, and the flow rate of the mixture is 90-110mL / min. The volume ratio of H2 to N2 in the mixture of H2 and N2 is 1:9. The solvent is water.

[0013] Further preferably, the impregnation-carbonization method comprises the following steps: dissolving a ruthenium-containing compound in a corresponding solvent to form a solution with a concentration of 0.01 to 4 wt%; then uniformly loading ruthenium on the surface of the precursor carrier (MoO3) by dropping and stirring, drying after stirring at room temperature, and calcining to obtain a reaction powder; carbonizing the reaction powder with a mixture of CH4 and H2 at 650°C-750°C for 1.5-2.5h, causing MoO3 to undergo a carburization and deoxidation phase transition, and obtaining a ruthenium-containing catalyst with an α-MoC carrier that is completely carbonized to a face-centered cubic crystal, in which the metal Ru is in an atomically dispersed state.

[0014] The impregnation-carbonization method specifically includes the following steps: dissolving a ruthenium-containing compound in a corresponding solvent to form a solution with a concentration of 0.01 to 4 wt%; then uniformly loading ruthenium on the surface of a precursor carrier (MoO3) by dropping and stirring, and stirring at room temperature for 12 hours; then evaporating to dryness while stirring at 80 to 120°C, drying in an oven at 80 to 120°C for 6 to 12 hours, and then calcining at 500°C for 4 hours to obtain a reaction powder; heating the reaction powder in a tubular furnace with a mixture of CH4 and H2 at a heating rate of 5°C / min from room temperature to 300°C, and at a heating rate of 1°C / min from 300°C to 700°C, and then carbonizing at 700°C for 2 hours to obtain an atomically dispersed ruthenium-containing catalyst with α-MoC as a carrier that is completely carbonized to a face-centered cubic crystal, and the flow rate of the mixed gas is 90 to 110 mL / min. The volume ratio of CH4 to H2 in the mixed gas of CH4 and H2 is 1:4. The solvent is water.

[0015] Preferably, the ruthenium-containing compound is ruthenium trichloride.

[0016] Compared with the prior art, the present invention has the following advantages:

[0017] 1. The ruthenium-containing catalyst proposed in the present invention is an atomic-level dispersed ruthenium-containing catalyst with α-MoC completely carbonized into a face-centered cubic crystal as a carrier. The ruthenium single atom is completely incorporated into the α-MoC lattice instead of being loaded on the carrier surface.

[0018] 2. The present invention uses guaiacol to prepare high-value phenol compounds (phenol, o-cresol, m-cresol and p-cresol) instead of common hydrocarbon substances such as benzene and cyclohexane. The ruthenium-containing catalyst has high catalytic activity, so that the selectivity of phenol compounds in the reaction products is very high, and almost no benzene ring hydrogenation products are produced.

[0019] 3. The reaction temperature of the method for selectively preparing phenolic compounds from catalyzing guaiacol proposed by the present invention is 230° C. to 270° C., and the reaction time is 0.5 to 12 h. Guaiacol can be efficiently converted, and the products are almost all phenolic substances. The catalyst has good reusability in intermittent reactor reactions and can operate for a long time on a fixed bed. Description of the drawings:

[0020] Figure 1 are XRD patterns of 1% Ru / α-MoC prepared in Example 1 and 1% Pt / α-MoC prepared in Comparative Example 1;

[0021] Figure 2 This is the TEM image of 1%Ru / α-MoC. Specific implementation method:

[0022] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.

[0023] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.

[0024] The ruthenium-containing catalyst of the present invention generally has a ruthenium loading of less than 1wt% to obtain a good effect. A certain amount of the ruthenium-containing catalyst is added to the reactant solution, and the air in the reactor is replaced with hydrogen after sealing, and finally a certain pressure of hydrogen (less than 5MPa) is introduced. The reactor temperature is controlled between 230°C and 270°C, and samples are taken after 0.5 to 12 hours of reaction, and the raw material conversion rate, the yield of each product and the selectivity are calculated.

[0025]

[0026]

[0027]

[0028] The qualitative analysis of the products was carried out by gas chromatography-mass spectrometry, and the amount of the remaining raw materials and various products in the reaction was analyzed by gas chromatography.

[0029] Example 1

[0030] 1wt% Ru / α-MoC catalyst was prepared by impregnation-carbonization method: ammonium molybdate was calcined at 500℃ for 4h to obtain a molybdenum trioxide carrier. Then 0.5460g of 3.7wt% ruthenium trichloride solution was added dropwise to 2g of molybdenum trioxide carrier and stirred at room temperature for 12h; then evaporated to dryness while stirring at 100℃, dried in an oven at 100℃ for 9h, and then calcined at 500℃ for 4h to obtain a reaction powder. The reaction powder was heated from room temperature to 300℃ at a heating rate of 5℃ / min in a tubular furnace using a mixture of CH4 and H2 (the volume ratio of CH4 to H2 is 1:4), and then from 300℃ to 700℃ at a heating rate of 1℃ / min, and then carbonized at 700℃ for 2h, with a flow rate of 100mL / min, to obtain a 1wt% Ru / α-MoC catalyst. The XRD pattern of the catalyst is shown in Figure 1 The TEM images of the catalysts are shown in Figure 2 As shown by Figure 2 It was found that the lattice spacings are 0.240 nm and 0.209 nm, respectively, corresponding to the (1 1 1) plane (0.247 nm) and (2 0 0) plane (0.214 nm) of α-MoC.

[0031] 100 mg of the catalyst was placed in a high-pressure batch reactor, and then 248 mg of guaiacol and 16 mL of n-hexane were added to the reactor. The reactor was sealed, purged with hydrogen for 7 times, and then 1.0 MPa of hydrogen was introduced. The reactor was heated to 250 ° C, stirred at 400 rpm, and the reaction was continued for 1 hour to obtain phenol compounds. The product yields are shown in Table 1.

[0032] Example 2

[0033] The reaction temperature was 230° C., the reaction time was 8 h, the catalyst preparation method, the amount of feed and the reaction conditions were the same as those in Example 1, and phenol compounds were obtained. The product yields are shown in Table 1.

[0034] Example 3

[0035] The reaction temperature was 270° C., the reaction time was 0.5 h, the catalyst preparation method, the amount of feed and the reaction conditions were the same as those in Example 1, and phenol compounds were obtained. The product yields are shown in Table 1.

[0036] Table 1. Time required for complete conversion of guaiacol at different reaction temperatures

[0037]

[0038] Example 4

[0039] The reaction pressure was 0.5 MPa, and the catalyst preparation method, feed amount and reaction conditions were the same as those in Example 1 to obtain phenol compounds. The product yields are shown in Table 2.

[0040] Example 5

[0041] The reaction pressure was 3 MPa, and the catalyst preparation method, feed amount and reaction conditions were the same as those in Example 1 to obtain phenol compounds. The product yields are shown in Table 2.

[0042] Table 2. Reaction results of guaiacol at different hydrogen pressures

[0043]

[0044]

[0045] Example 6

[0046] The reaction solvent was n-octane, and the catalyst preparation method, addition amount and reaction conditions were the same as those in Example 1 to obtain phenol compounds. The product yields are shown in Table 3.

[0047] Example 7

[0048] The reaction solvent was n-decane, and the catalyst preparation method, addition amount and reaction conditions were the same as those in Example 1 to obtain phenol compounds. The product yields are shown in Table 3.

[0049] Table 3. Reaction results of guaiacol in different solvents

[0050]

[0051] Example 8

[0052] The 0.1wt% Ru / α-MoC catalyst was prepared by the impregnation-carbonization method: ammonium molybdate was calcined at 500℃ for 4h to obtain a molybdenum trioxide carrier. Then 0.0541g of 3.7wt% ruthenium trichloride solution was added dropwise to 2g of molybdenum trioxide carrier, stirred at room temperature for 12h, evaporated to dryness while stirring at 110℃, dried in an oven at 80℃ for 12h, and calcined at 500℃ for 4h. The 0.1wt% Ru / α-MoC catalyst was obtained by carbonization at 700℃ for 2h in a tubular furnace with a CH4-H2 mixed gas (the volume ratio of CH4 to H2 is 1:4) to obtain a 0.1wt% Ru / α-MoC catalyst.

[0053] 100 mg of the catalyst was placed in a high-pressure batch reactor, and then 248 mg of guaiacol and 16 mL of n-hexane were added to the reactor. The reactor was sealed, purged with hydrogen for 7 times, and then 1.0 MPa of hydrogen was introduced. The reactor was heated to 250 ° C, stirred at 400 rpm, and the reaction was continued for 1 hour to obtain phenol compounds. The product yields are shown in Table 4.

[0054] Example 9

[0055] 3wt% Ru / α-MoC catalyst was prepared by impregnation-carbonization method: ammonium molybdate was calcined at 500℃ for 4h to obtain a molybdenum trioxide carrier. Then 1.6718g of 3.7wt% ruthenium trichloride solution was added dropwise to 2g of molybdenum trioxide carrier, stirred at room temperature for 12h, evaporated to dryness while stirring at 110℃, dried in an oven at 80℃ for 12h, and calcined at 500℃ for 4h. 3wt% Ru / α-MoC catalyst was obtained by carbonization at 700℃ for 2h in a tubular furnace with a CH4-H2 mixed gas (the volume ratio of CH4 to H2 was 1:4) to obtain a 3wt% Ru / α-MoC catalyst.

[0056] 100 mg of the catalyst was placed in a high-pressure batch reactor, and then 248 mg of guaiacol and 16 mL of n-hexane were added to the reactor. The reactor was sealed, purged with hydrogen for 7 times, and then 1.0 MPa of hydrogen was introduced. The reactor was heated to 250 ° C, stirred at 400 rpm, and the reaction was continued for 1 hour to obtain phenol compounds. The product yields are shown in Table 4.

[0057] Table 4. Reaction results of guaiacol on catalysts with different Ru loadings

[0058]

[0059] Example 10

[0060] The supported ruthenium-containing catalyst was prepared by impregnation method: 0.5460 g of 3.7 wt% ruthenium trichloride solution was added dropwise to 2 g of MoO3 carrier, stirred at room temperature for 12 h, evaporated to dryness while stirring at 110°C, dried in an oven at 80°C for 12 h, and calcined at 500°C for 4 h. The ruthenium-containing catalyst was reduced with H2-N2 mixed gas in a tubular furnace for 4 h to obtain the ruthenium-containing catalyst.

[0061] 100 mg of the catalyst was placed in a high-pressure batch reactor, and then 248 mg of guaiacol and 16 mL of n-hexane were added to the reactor. The reactor was sealed, purged with hydrogen for 7 times, and then 1.0 MPa of hydrogen was introduced. The reactor was heated to 250 ° C, stirred at 400 rpm, and the reaction was continued for 1 hour to obtain phenol compounds. The product yields are shown in Table 5.

[0062] Examples 11-13

[0063] Refer to Example 10, the difference is that the carriers of the ruthenium-containing catalyst are different, namely TiO2, ZrO2, and S-1 zeolite molecular sieve.

[0064] Table 5. Reaction results of guaiacol on ruthenium-containing catalysts on different supports

[0065]

[0066] Comparative Example 1

[0067] Preparation of 1wt% Pt / α-MoC catalyst by impregnation method: calcine ammonium molybdate at 500℃ for 4h to obtain a molybdenum trioxide carrier. Then add 1.3034g of 1.55wt% chloroplatinic acid solution dropwise to 2g of molybdenum trioxide carrier, stir at room temperature for 12h, evaporate to dryness while stirring at 110℃, dry in an oven at 80℃ for 12h, and calcine at 500℃ for 4h. Carbonize with CH4-H2 mixed gas at 700℃ for 2h in a tubular furnace to obtain 1wt% Pt / α-MoC catalyst. The XRD pattern of the catalyst is shown in Figure 1 shown.

[0068] Depend on Figure 1 It was concluded that the (1 1 1) and (2 0 0) crystal plane peaks of α-MoC were present, and no diffraction peaks belonging to metals were observed, indicating that the metals were highly dispersed on the support.

[0069] 100 mg of the catalyst was placed in a high-pressure batch reactor, and then 248 mg of guaiacol and 16 mL of n-hexane were added to the reactor. The reactor was sealed, purged with hydrogen for 7 times, and then 1.0 MPa of hydrogen was introduced. The reactor was heated to 250 ° C, stirred at 400 rpm, and the reaction was continued for 1 hour. The product yields were shown in Table 6.

[0070] Table 6. Reaction results of guaiacol with different catalyst loading metals

[0071]

[0072]

[0073] As can be seen from Tables 1 to 6, the ruthenium-containing catalyst prepared by the present invention can efficiently convert guaiacol into phenolic compounds, the product types are relatively simple, and there is almost no benzene ring saturated product. After reacting at 250°C for 1 hour, the conversion rate of guaiacol can reach 98.25%, and the selectivity of phenolic compounds is 80.81%.

[0074] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for selectively preparing phenolic compounds by catalyzing guaiacol, characterized in that: A ruthenium-containing catalyst catalyzes the hydrodeoxygenation reaction of guaiacol to achieve the synthesis of phenolic compounds. The ruthenium-containing catalyst is an atomic-level dispersed ruthenium-containing catalyst prepared by an impregnation-carbonization method and using α-MoC as a carrier in which MoO3 is completely carbonized into a face-centered cubic crystal. The loading amount of ruthenium in the ruthenium-containing catalyst is 0.1-5 wt% of the mass of the catalyst. The method specifically comprises the following steps: dissolving guaiacol in an organic solvent to obtain a guaiacol solution, then adding the ruthenium-containing catalyst to the guaiacol solution, sealing the reaction container, replacing the air in the reaction container with hydrogen, and finally introducing hydrogen at a pressure of no more than 5 MPa into the reaction container. The reaction temperature is 230°C-270°C, the reaction time is 0.5-12 h, the mass of the ruthenium-containing catalyst is 30-50 wt% of the mass of the guaiacol, and phenolic compounds are obtained. The phenolic compounds include phenol, o-cresol, m-cresol and p-cresol.

2. The method according to claim 1, characterized in that The organic solvent is selected from at least one of n-hexane, n-octane, n-decane, dodecane and decahydronaphthalene.

3. The method according to claim 1, characterized in that The mass of the ruthenium-containing catalyst is 30-50 wt% of the mass of guaiacol, and the mass volume ratio of the ruthenium-containing catalyst to the organic solvent is 6.25 mg / mL.

4. The method according to claim 1, characterized in that: The impregnation-carbonization method comprises the following steps: dissolving a ruthenium-containing compound in a corresponding solvent to prepare a solution with a concentration of 0.01-4 wt%; then uniformly loading ruthenium on the surface of a carrier by dropping and stirring, drying after stirring at room temperature, and calcining to obtain a reaction powder; carbonizing the reaction powder with a mixture of CH4 and H2 at 650°C-750°C for 1.5-2.5 h to obtain a ruthenium-containing catalyst with a face-centered cubic α-MoC carrier.

5. The method according to claim 4, characterized in that The ruthenium-containing compound is ruthenium trichloride.

Citation Information

Cited By

  • In2O3-TiO2 composite oxide catalyst as well as preparation method and application thereof

    CN120361885A