Silicon negative electrode material and preparation method thereof, negative electrode and lithium ion battery
By forming a small-molecule clad layer of benamidyl group on the surface of the silicon negative electrode material, the interfacial rupture caused by volume changes in the silicon negative electrode material during lithium embedding/delithation process is solved, and the cycling and kinetic performance of the battery is improved.
Patent Information
- Application Number
- CN202310141474.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-17
AI Technical Summary
The volume of the silicon negative electrode material changes greatly during the lithium embedding/delivering process, resulting in the cracking of the solid electrolyte interface layer and severe consumption of active lithium ions, limiting its market application. The formation speed of the passivation layer of existing additives is slow and uneven, resulting in Battery performance is poor.
By placing the silicon particle material with oxygen-containing groups on the surface in a benamid group small molecule solution, the benamid group small molecule reacts with the surface of the silicon particles to form a stable coating layer, and binds to a binder to inhibit the powdering of the electrode sheet. and break and participate in the formation of SEI film during charging and discharging, reducing electrolyte reaction.
The formed cladding layer improves the bonding degree between silicon particles and binder, and is stable on the electrode surface, prevents the electrode from contacting the electrolyte, significantly improves the mobility of lithium ions and the cycling performance of the battery, and reduces the increase in the battery impedance.
Smart Images

Figure CN115911342B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium battery technology, and in particular to a silicon negative electrode material and a preparation method thereof, a negative electrode and a lithium ion battery. Background Art
[0002] With the rapid development of electric vehicles and energy markets, people have put forward higher and higher requirements on the energy density of lithium-ion battery energy storage systems. Under this demand, compared with other negative electrode materials, silicon (Si) negative electrode materials have a very high specific capacity (4200mAhg -1 ), suitable voltage, abundant resources and cost, etc. However, the large volume change (~300%) of silicon during lithium insertion / extraction leads to the rupture of the solid electrolyte interface (SEI) layer. The newly exposed silicon surface further reacts with the electrolyte to consume a large amount of active lithium ions, which eventually leads to the rapid failure of Si negative electrode, which seriously limits its market application.
[0003] Although additives help to form an excellent passivation layer to protect the electrode from the corrosion of the electrolyte and improve the conductivity of lithium ions, thereby improving the electrochemical performance of the battery. However, there are still inevitable disadvantages. (1) Slow reaction speed: The additives only work when they diffuse to the electrode surface; and the driving force generated by the concentration gradient of the additives is very low, resulting in a very slow diffusion rate. (2) The passivation layer is uneven and discontinuous. The formation of the passivation layer depends on the location and distribution of active points on the electrode surface. (3) Significant side effects: After the battery is formed, 50%-70% of the film-forming additives remain in the electrolyte, which will lead to the continuous growth of the SEI film and increase the internal resistance. (4) The formed passivation layer has poor toughness: The SEI film that grows naturally by the decomposition of the electrolyte is mainly composed of inorganic components such as Li2CO3, LiF and Li2O. During the electrochemical cycle, it is easy to rupture as the volume of the electrode material expands and contracts.
[0004] In addition, in the process of preparing negative electrode sheets of silicon negative electrode materials, on the one hand, silicon is difficult to disperse due to its small particles, and is very easy to agglomerate. The bonding between particles is unstable and it is easy to fall off from the surface of the current collector. On the other hand, the volume expansion of silicon itself is large, which easily causes the electrode sheet to pulverize and break.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a silicon negative electrode material, a silicon negative electrode material, a negative electrode and a lithium ion battery.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a method for preparing a silicon negative electrode material, comprising:
[0009] The silicon particle material having oxygen-containing groups on the surface is placed in a benzamide-based small molecule solution;
[0010] The benzamide small molecules are allowed to fully react with the oxygen-containing groups on the surface of the silicon particles;
[0011] The solvent in the benzamide small molecule solution is volatilized, and the benzamide small molecules are coated on the surface of the silicon particles;
[0012] The benzamide-based small molecule is selected from at least one of 2-aminobenzamide, 3-nitrosobenzamide, 2-(trifluoromethyl)benzamide, 2-hydroxy-N-phenylbenzamide, 2-amino-5-nitrobenzamide, N,N-vinylbisbenzamide, 2-methoxy-4-aminobenzamide, 5-acetyl-2-hydroxybenzamide and 2-nitro-4-trifluoromethylbenzamide.
[0013] In an optional embodiment, the mass ratio of the phenylamide-based small molecules to the oxygen-containing silicon particle material is 0.01-0.2:1.
[0014] In an optional embodiment, the solvent in the benzamide-based small molecule solution is volatilized by:
[0015] The reaction system is placed at a temperature of 50 to 100°C and stirred under protective gas until the solvent is completely evaporated;
[0016] Preferably, the protective gas is nitrogen or an inert gas.
[0017] In an optional embodiment, after the solvent in the benzamide-based small molecule solution is volatilized, the method further comprises: baking the solid material obtained after the solvent is volatilized in a vacuum environment at a temperature of 70 to 120° C. for 5 to 12 hours.
[0018] In an optional embodiment, before placing the silicon particle material having oxygen-containing groups on the surface in the benzamide-based small molecule solution, the process further comprises:
[0019] The silicon particle material is placed in an oxygen atmosphere and pre-oxidized at a temperature of 100 to 500° C. for 2 to 6 hours to obtain a silicon particle material having oxygen-containing groups on the surface.
[0020] In an optional embodiment, before placing the silicon particle material having oxygen-containing groups on the surface in the benzamide-based small molecule solution, the process further comprises:
[0021] Dissolving the benzamide small molecule in a solvent to obtain a benzamide small molecule solution, wherein the solvent is selected from at least one of deionized water, ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran and N-methylpyrrolidone;
[0022] Preferably, the mass fraction of the benzamide small molecules in the benzamide small molecule solution is 2% to 10%;
[0023] Preferably, the process of dissolving the benzamide small molecules in a solvent to obtain a benzamide small molecule solution is carried out at a temperature of 30 to 100°C.
[0024] In an optional embodiment, the method for making the benzamide small molecule fully react with the oxygen-containing groups on the surface of the silicon particles is:
[0025] The silicon particle material having oxygen-containing groups on the surface is placed in a benzamide-based small molecule solution and then ultrasonicated for 0.5 to 2 hours with an ultrasonic power of 600-2400W.
[0026] In a second aspect, the present invention provides a silicon negative electrode material, which is prepared by the preparation method of any one of the aforementioned embodiments.
[0027] In a third aspect, the present invention provides a negative electrode, which is made of the silicon negative electrode material as described in the above embodiment.
[0028] In a fourth aspect, the present invention provides a lithium ion battery comprising the negative electrode according to the aforementioned embodiment.
[0029] The present invention has the following beneficial effects:
[0030] The method provided by the present invention can form a stable benzamide small molecule coating layer on the surface of silicon particles. The formation of the coating layer has the following advantages:
[0031] The multiple functional groups contained in the benzamide small molecules can combine with the hydroxyl groups in the binder polyvinyl alcohol and the hydroxyl or carboxyl groups on the surface of the silicon particles through hydrogen bonds and chemical bonds, playing the role of a "bridge" connecting silicon and the binder, making the silicon and the binder tightly combined, and inhibiting the powdering and breakage of the pole piece during the manufacturing process;
[0032] The solubility of benzamide small molecules in water is low, which also ensures that the coating layer can exist stably in the aqueous binder. Therefore, the coating layer formed on the silicon surface can exist stably on the surface of the silicon particles during the slurry coating process. Therefore, after the negative electrode is made, there is still a stable benzamide-based small molecule coating layer on the surface of the silicon particles. This coating layer can effectively prevent the direct contact between the silicon particles and the electrolyte, and play a role in protecting the electrode material; and the functional groups contained in the benzamide-based small molecules will participate in the formation of the SEI film during the charge and discharge process, and can reduce the continuous reaction of the electrolyte at the electrode interface during the charge and discharge process, effectively inhibit the impedance increase and active lithium consumption of the battery, and significantly improve the cycle performance of the battery; the functional groups contained in the benzamide-based small molecules can significantly increase the mobility of lithium ions and improve the kinetic performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0034] Figure 1 The first charge and discharge test results of Comparative Example 1 and Examples 1 to 3 are shown;
[0035] Figure 2 This is the rate performance test of Comparative Example 1 and Examples 1 to 3;
[0036] Figure 3 The EIS graphs after the rate performance tests of Comparative Example 1 and Examples 1 to 3 are shown;
[0037] Figure 4 This is the cycle performance test of Comparative Example 1 and Examples 1 to 3;
[0038] Figure 5 is a morphology diagram of the negative electrode sheet prepared in Example 1;
[0039] Figure 6 is a morphology diagram of the negative electrode sheet prepared in Example 11;
[0040] Figure 7 This is a morphology picture of the negative electrode sheet prepared in Comparative Example 1. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0042] The silicon negative electrode material and its preparation method, negative electrode and lithium ion battery provided in the embodiments of the present invention are described in detail below.
[0043] The method for preparing a silicon negative electrode material provided by an embodiment of the present invention comprises:
[0044] The silicon particle material having oxygen-containing groups on the surface is placed in a benzamide-based small molecule solution;
[0045] The benzamide small molecules are allowed to fully react with the oxygen-containing groups on the surface of the silicon particles;
[0046] The solvent in the benzamide small molecule solution is volatilized, and the benzamide small molecules are coated on the surface of the silicon particles;
[0047] The benzamide-based small molecule is selected from at least one of 2-aminobenzamide, 3-nitrosobenzamide, 2-(trifluoromethyl)benzamide, 2-hydroxy-N-phenylbenzamide, 2-amino-5-nitrobenzamide, N,N-vinylbisbenzamide, 2-methoxy-4-aminobenzamide, 5-acetyl-2-hydroxybenzamide and 2-nitro-4-trifluoromethylbenzamide.
[0048] The preparation method provided in the present application forms a coating layer by means of surface grafting and solvent volatilization, so that the above-mentioned specific benzamide-based small molecules are stably coated on the surface of silicon particles through chemical bonds. When the coating layer is used to prepare the negative electrode, the surface of the coating layer can be combined with the hydroxyl groups in the binder polyvinyl alcohol and the hydroxyl groups or carboxyl groups on the surface of the silicon particles through hydrogen bonds and chemical bonds due to the multiple functional groups contained in the benzamide-based small molecules, thus playing the role of a "bridge" connecting silicon and the binder, making the silicon and the binder tightly bonded, and inhibiting the powdering and breakage of the electrode during the manufacturing process. The solubility of benzamide small molecules in water is low, which also ensures that the coating layer can exist stably in the aqueous binder. Therefore, the coating layer formed on the silicon surface can exist stably on the surface of the silicon particles during the slurry coating process. Therefore, after the negative electrode is made, there is still a stable benzamide-based small molecule coating layer on the surface of the silicon particles, which can effectively prevent the direct contact between the silicon particles and the electrolyte, and play a role in protecting the electrode material; and the functional groups contained in the benzamide-based small molecules will participate in the formation of the SEI film during the charge and discharge process, which can reduce the continuous reaction of the electrolyte at the electrode interface during the charge and discharge process, effectively inhibit the impedance increase and active lithium consumption of the battery, and significantly improve the cycle performance of the battery; the functional groups contained in the benzamide-based small molecules can significantly increase the mobility of lithium ions and improve the kinetic performance of the battery.
[0049] The method provided in the present application for coating the surface of silicon particles with benzamide-based small molecules has a significantly better effect, especially for negative electrode materials. If it is applied to positive electrodes or separators, the following problems may occur:
[0050] 1. If used for positive electrode, due to the large polarity of such small molecules, they are easily soluble in polar solvents. In the market, N-methylpyrrolidone is mostly used as the solvent for positive electrode slurry. During the electrode preparation process, the small molecules will dissolve and fall off from the surface of silicon particles, and will not play a role. At the same time, oxidation may occur under high voltage and fail.
[0051] 2. If used for diaphragms, what may occur between the multi-functional groups and the diaphragm is not grafting, but a cross-linking reaction, which may lead to uneven tension inside the diaphragm and cause curling and bending. The tensile strength of multiple regions of the diaphragm is unevenly distributed, making it easy to rupture and fail.
[0052] The preparation method provided in this application is further described below.
[0053] The preparation method of silicon negative electrode material is specifically as follows:
[0054] S1. Pre-oxidation of silicon granular materials
[0055] The silicon particle material is placed in an oxygen atmosphere and pre-oxidized at a temperature of 100-500°C (e.g., 100°C, 110°C, 120°C, 130°C or 150°C) for 2-6h (e.g., 2h, 3h, 4h or 6h) to obtain a silicon particle material having oxygen-containing groups on the surface.
[0056] S2. Preparation of phenylamide-based small molecule solution
[0057] The benzamide small molecule is dissolved in a solvent at 30-100° C. (eg, 30° C., 50° C., 60° C., 80° C. or 100° C.) to obtain a benzamide small molecule solution after being fully dissolved.
[0058] The benzamide-based small molecule is selected from at least one of 2-aminobenzamide, 3-nitrosobenzamide, 2-(trifluoromethyl)benzamide, 2-hydroxy-N-phenylbenzamide, 2-amino-5-nitrobenzamide, N,N-vinylbisbenzamide, 2-methoxy-4-aminobenzamide, 5-acetyl-2-hydroxybenzamide and 2-nitro-4-trifluoromethylbenzamide;
[0059] The solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran and N-methylpyrrolidone;
[0060] Preferably, the mass fraction of the benzamide small molecule in the benzamide small molecule solution is 2% to 10% (eg, 2%, 5%, 8% or 10%). Silicon particles placed in the above concentration environment have a higher grafting efficiency.
[0061] S3, grafted phenylamide small molecules
[0062] The silicon particle material is placed in a benzamide-based small molecule solution, and the benzamide-based small molecules are fully reacted with the oxygen-containing groups on the surface of the silicon particles to achieve the effect of grafting the benzamide-based small molecules to the surface of the silicon particles.
[0063] Preferably, the materials are fed in a mass ratio of 0.01 to 0.2:1 (e.g., 0.01:1, 0.05:1, 0.1:1 or 0.2:1) of the benzamide small molecule to the oxygen-containing silicon particle material. Within this mass ratio range, the surface of the prepared silicon particles has a suitable amount of benzamide small molecule coating. If the benzamide small molecule is coated too much, the benzamide small molecule has a low conductivity and is deposited thickly on the surface of the silicon particles, resulting in a large battery impedance and poor performance; if the coating is too little, the performance improvement of the silicon negative electrode material is not obvious.
[0064] Preferably, the grafting is achieved by placing the silicon particle material in a benzamide-based small molecule solution, and then ultrasonicating for 0.5 to 2 hours (e.g., 0.5 hours, 1 hour, or 2 hours) at an ultrasonic power of 600-2400W (600W, 800W, 1000W, 1500W, 2000W, or 2400W).
[0065] S4, evaporate the solvent
[0066] After the ultrasonic treatment, the reaction system is placed at 50-100° C. (eg, 50° C., 60° C., 80° C. or 100° C.) and heated and stirred in the presence of protective gas until the solvent is completely evaporated to obtain a solid material.
[0067] Preferably, the protective gas is nitrogen or an inert gas.
[0068] By heating and drying the solvent to evaporate it, the solvent removal effect can be achieved very well. By drying at a suitable temperature, the benzamide small molecules will not evaporate and will not be wasted, thus ensuring that all the benzamide small molecules are coated on the surface of the silicon particles.
[0069] S5. Vacuum drying
[0070] The solid material obtained in the previous step is placed in a vacuum environment at a temperature of 70 to 120° C. (e.g., 70° C., 80° C., 90° C., 100° C. or 120° C.) and baked for 5 to 12 hours (e.g., 5 hours, 7 hours, 10 hours or 12 hours) to ensure that the moisture generated during the grafting process and the trace water present in the solvent are evaporated to finally obtain silicon particles coated with phenylamide small molecules.
[0071] The silicon negative electrode material provided in the embodiment of the present application is prepared by the preparation method provided in the embodiment of the present application.
[0072] The negative electrode provided in the embodiment of the present application is made using the silicon negative electrode material provided in the embodiment of the present application.
[0073] The lithium-ion battery provided in the embodiment of the present application includes the negative electrode provided in the embodiment of the present application.
[0074] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0075] Example 1
[0076] The method for preparing the silicon negative electrode material provided in this embodiment is specifically as follows:
[0077] The silicon particle material is placed in a tube furnace and pre-oxidized at 200° C. in an oxygen atmosphere for 3 h to obtain a silicon particle material having oxygen-containing groups on the surface;
[0078] Dissolve 0.5 g of p-2-aminobenzamide in 9.5 g of N-methylpyrrolidone to obtain a 5% benzamide small molecule solution after sufficient dissolution;
[0079] 10 g of silicon particles with oxygen-containing groups on the surface obtained after pre-oxidation were placed in a benzamide-based small molecule solution and subjected to ultrasonic treatment for 1 h at an ultrasonic power of 1500 W;
[0080] Then the reaction system was placed at 80°C and heated with stirring under nitrogen protection until the solvent was completely evaporated to obtain a solid material;
[0081] The solid material was placed in a vacuum drying oven and baked at 110° C. for 8 hours to obtain silicon particles coated with benzamide small molecules.
[0082] Example 2
[0083] The method for preparing the silicon negative electrode material provided in this embodiment is specifically as follows:
[0084] The silicon particle material is placed in a tube furnace and pre-oxidized at 100° C. in an oxygen atmosphere for 6 h to obtain a silicon particle material having oxygen-containing groups on the surface;
[0085] Dissolve 0.1 g of p-nitrosobenzamide in 4.9 g of N-methylpyrrolidone to obtain a 2% benzamide small molecule solution after sufficient dissolution;
[0086] 10 g of silicon particles with oxygen-containing groups on the surface obtained after pre-oxidation were placed in a benzamide-based small molecule solution and subjected to ultrasonic treatment for 0.5 h at an ultrasonic power of 600 W;
[0087] Then the reaction system was placed at 50°C and heated with stirring under nitrogen protection until the solvent was completely evaporated to obtain a solid material;
[0088] The solid material was placed in a vacuum drying oven and baked at 70° C. for 12 h to obtain silicon particles coated with benzamide small molecules.
[0089] Example 3
[0090] The method for preparing the silicon negative electrode material provided in this embodiment is specifically as follows:
[0091] The silicon particle material is placed in a tube furnace and pre-oxidized at 100° C. in an oxygen atmosphere for 6 h to obtain a silicon particle material having oxygen-containing groups on the surface;
[0092] Dissolve 1 g of p-2-(trifluoromethyl)benzamide in 9 g of N-methylpyrrolidone to obtain a 10% benzamide-based small molecule solution after sufficient dissolution;
[0093] 5 g of silicon particles with oxygen-containing groups on the surface obtained after pre-oxidation were placed in a benzamide-based small molecule solution and subjected to ultrasonic treatment for 2 h at an ultrasonic power of 2400 W;
[0094] Then the reaction system was placed at 100° C. and heated and stirred under nitrogen protection until the solvent was completely evaporated to obtain a solid material;
[0095] The solid material was placed in a vacuum drying oven and baked at 120° C. for 5 hours to obtain silicon particles coated with benzamide small molecules.
[0096] Example 4
[0097] This embodiment is substantially the same as embodiment 1, except that the benzamide-based small molecule is 2-hydroxy-N-phenylbenzamide.
[0098] Example 5
[0099] This embodiment is substantially the same as embodiment 1, except that the benzamide-based small molecule is 2-amino-5-nitrobenzamide.
[0100] Example 6
[0101] This embodiment is substantially the same as embodiment 1, except that the benzamide-based small molecule is N,N-vinylbisbenzamide.
[0102] Example 7
[0103] This embodiment is substantially the same as embodiment 1, except that the benzamide-based small molecule is 2-methoxy-4-aminobenzamide.
[0104] Example 8
[0105] This embodiment is substantially the same as embodiment 1, except that the benzamide-based small molecule is 5-acetyl-2-hydroxybenzamide.
[0106] Example 9
[0107] This embodiment is substantially the same as embodiment 1, except that the benzamide-based small molecule is 2-nitro-4-trifluoromethylbenzamide.
[0108] Example 10
[0109] This embodiment is substantially the same as embodiment 1, except that the amount of the benzamide small molecule used is 5 g.
[0110] Embodiment 11
[0111] This embodiment is basically the same as Embodiment 1, except that:
[0112] Based on Example 1, the last two steps are replaced as follows: After ultrasonic treatment, the silicon particles are filtered out from the solution, washed with deionized water for three times, and then placed in a vacuum drying oven and baked at 90° C. for 8 h.
[0113] Comparative Example 1
[0114] Silicon granules material without any treatment.
[0115] Experimental Example 1
[0116] The silicon negative electrode materials provided in Examples 1-11 and the comparative example were made into silicon half-cells, and their electrochemical properties were tested.
[0117] The preparation method of the silicon half-cell is specifically as follows:
[0118] Silicon particle negative electrode material, sodium carboxymethyl cellulose, and acetylene black were mixed evenly at a mass ratio of 70:15:15 to prepare an electrode slurry, which was then coated on a copper foil current collector and dried using a 2MPa / cm 2 The silicon half-cell was obtained by pressing and cutting the negative electrode sheets with a pressure of 10000 and using metal lithium as the counter electrode to assemble the half-cell. Figure 1-4 And as shown in Table 1.
[0119] Figure 1 Comparing the first charge and discharge curves of Examples 1 to 3 and Comparative Example 1, the reversible capacity of the uncoated silicon half-cell is 2679.9 mAh / g, and the first coulombic efficiency is relatively low at 89.6%. After the silicon negative electrode is modified with multi-functional amide small molecules, the reversible capacity reaches up to 3064.6 mAh / g, and the first coulombic efficiency is up to 92.3%. This is because the functional groups contained can form a stable SEI film in situ in one step during the first charge and discharge process, and mostly construct an artificial interface layer on the surface of the silicon particles, which reduces the continuous reaction of the electrolyte at the electrode interface, effectively reduces the consumption of active lithium, and improves the reversible capacity and first coulombic efficiency of the battery.
[0120] Figure 2 For the rate performance comparison of Examples 1 to 3 and Comparative Example 1, the reversible capacity retention rate of the uncoated silicon half-cell at a high current density of 20C is only 58.2%. After modification with multi-functional amide small molecules, the silicon half-cell exhibits excellent rate performance, up to 81%, because the SEI film formed by the special functional groups contained in the small molecules exhibits higher lithium ion conductivity.
[0121] Figure 3The EIS graphs after the rate performance test of Examples 1 to 3 and Comparative Example 1 are shown. Silicon exhibits significant volume expansion during high current charge and discharge, resulting in particle pulverization and rupture, SEI film repair, regeneration and thickening, and high impedance. The impedance of silicon is significantly reduced after modification, which is due to the fact that the SEI film formed after interface modification is thin, stable and has good lithium conductivity. On the one hand, it can effectively alleviate the volume expansion of silicon, and on the other hand, it also plays a role in reducing battery impedance.
[0122] Figure 4 The cycle performance comparison of Examples 1 to 3 and Comparative Example 1 shows that the capacity of the uncoated silicon negative electrode half-cell after 200 cycles is only 786.4 mAh / g. After modification with multi-functional amide small molecules, the cycle stability of the battery is significantly improved, and the capacity can reach up to 2068 mAh / g after 200 cycles.
[0123] Table 1 Comparison of electrochemical performance of Examples 1-11 and Comparative Example 1
[0124]
[0125]
[0126] It can be seen from the above table that the silicon negative electrode materials prepared in each embodiment of the present application have good electrochemical properties. By comparing Example 1 with Example 10, it can be found that the various electrochemical properties of Example 10 are worse than those of Example 1, and the amount of phenylamide small molecules used in Example 10 exceeds the preferred range required by the present application, which shows that in the process of silicon particles coating phenylamide small molecules, the silicon particles and phenylamide small molecules should have better effects when they are within a suitable ratio range; by comparing Example 11 with Example 1, the various electrochemical properties of Example 11 are significantly worse, which shows that the method of evaporating the solvent and then baking can produce a silicon negative electrode material with better electrochemical properties than the method of filtering out the silicon particles, washing and then drying.
[0127] Experimental Example 2
[0128] Photographing the morphology of the negative electrode sheets obtained in Example 1, Example 11 and Comparative Example 1. Figure 5-7 shown.
[0129] Figure 5 This is a morphology diagram of the negative electrode plate prepared in Example 1. It can be seen from the figure that the coating formed on the current collector of the negative electrode plate is dense and has almost no cracks.
[0130] Figure 6 and Figure 7The morphology pictures of the negative electrode sheets prepared in Example 11 and Comparative Example 1 are shown respectively. It can be seen from the pictures that the coating surfaces formed on the current collectors in Example 11 and Comparative Example 1 have many obvious cracks, especially in Comparative Example 1.
[0131] In summary, the preparation method of the silicon negative electrode material provided in the embodiment of the present application, through surface grafting and solvent volatilization, makes the benzamide small molecules stably coated on the surface of the silicon particles through chemical bonds to form a stable coating layer, which can make the silicon and the binder tightly combined in the negative electrode preparation process, and inhibit the pulverization and breakage of the electrode during the manufacturing process; the prepared coating layer can effectively prevent the direct contact between the silicon particles and the electrolyte, play a role in protecting the electrode material, and can also improve the electrochemical performance of the battery.
[0132] The silicon negative electrode material provided in the embodiment of the present application is prepared by the preparation method provided in the embodiment of the present application. Therefore, the silicon negative electrode material is not prone to pulverization and breakage during the negative electrode preparation process and has the characteristics of good electrochemical performance.
[0133] The negative electrode provided in the embodiment of the present application is made from the silicon negative electrode material provided in the present application, so the negative electrode has the advantage of good electrochemical performance.
[0134] The lithium-ion battery provided in the embodiment of the present application has better electrochemical performance because it includes the negative electrode provided in the embodiment of the present application.
[0135] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a silicon negative electrode material, characterized in that: include: The silicon particle material is placed in an oxygen atmosphere and pre-oxidized at a temperature of 100 to 500° C. for 2 to 6 hours to obtain a silicon particle material having oxygen-containing groups on the surface; The silicon particle material having oxygen-containing groups on the surface is placed in a benzamide-based small molecule solution; The silicon particle material having oxygen-containing groups on the surface is placed in a benzamide-based small molecule solution and then ultrasonicated for 0.5 to 2 hours at an ultrasonic power of 600 to 2400 W to allow the benzamide-based small molecules to fully react with the oxygen-containing groups on the surface of the silicon particles; The reaction system is placed at a temperature of 50-100° C. and protected by protective gas until the solvent is completely volatilized, and the solid material obtained after the solvent is volatilized is placed in a vacuum environment at a temperature of 70-120° C. and baked for 5-12 hours, so that the benzamide small molecules are coated on the surface of the silicon particles; The benzamide-based small molecule is selected from at least one of 2-aminobenzamide, 3-nitrosobenzamide, 2-(trifluoromethyl)benzamide, 2-amino-5-nitrobenzamide, N,N-vinylbisbenzamide, 2-methoxy-4-aminobenzamide and 2-nitro-4-trifluoromethylbenzamide; The mass ratio of the phenylamide-based small molecules to the oxygen-containing silicon particle material is 0.01-0.2:
1.
2. The method for preparing a silicon negative electrode material according to claim 1, characterized in that: The process of completely evaporating the solvent is carried out under stirring.
3. The method for preparing a silicon negative electrode material according to claim 2, characterized in that: The protective gas is nitrogen or an inert gas.
4. The method for preparing a silicon negative electrode material according to claim 1, characterized in that: Before placing the silicon particle material having oxygen-containing groups on the surface in the benzamide-based small molecule solution, the method further comprises: The benzamide small molecule is dissolved in a solvent to obtain the benzamide small molecule solution, and the solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran and N-methylpyrrolidone.
5. The method for preparing a silicon negative electrode material according to claim 1, characterized in that: The mass fraction of the benzamide small molecules in the benzamide small molecule solution is 2% to 10%.
6. The method for preparing a silicon negative electrode material according to claim 1, characterized in that: The process of dissolving the benzamide small molecule in a solvent to obtain the benzamide small molecule solution is carried out at a temperature of 30-100°C.
7. A silicon negative electrode material, characterized in that: The method is prepared according to any one of claims 1 to 6.
8. A negative electrode, characterized in that It is made from the silicon negative electrode material as claimed in claim 7.
9. A lithium ion battery, characterized in that: Comprising the negative electrode as claimed in claim 8.