A method for preparing modified nano zirconium sol
Through the preparation and application of modified nanozirconium sol, the film layer uneven problem caused by electron accumulation during zirconium-based film formation is solved, the bonding force and corrosion resistance of the paint film and metal substrate are improved, and heavy metal pollution is avoided. A more environmentally friendly surface treatment effect is achieved.
Patent Information
- Application Number
- CN202211710016.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Electronic accumulation during zirconium-based film formation leads to uneven distribution of zirconium-based film layer, affecting the adhesion and corrosion resistance of paint films. Existing solutions such as the introduction of trace copper elements poses a risk of environmental pollution.
Modified nanozirconium sol is used as the surface adjuster to form a microcathode through electrostatic adsorption of zirconium ions, adjust the surface reaction activity of metal substrates, and react with zirconium ions through the coordination of aminosilane and epoxy silane to form a nanozirconium sol. Used to pretreat the metal surface to improve uniformity and mechanical bonding force of the zirconium-based film layer.
The pulling bonding force and salt spray corrosion resistance of the coating paint film and metal substrate are significantly improved, heavy metal pollution is reduced, and the use of nano-zirconium sol does not affect the pH stability of subsequent processes.
Smart Images

Figure CN115961276B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing modified nano zirconium sol. Background Art
[0002] In the process of gradually replacing phosphating, metal non-phosphorus pretreatment agents have reduced a large amount of wastewater discharge and made outstanding contributions to environmental protection. Among them, zirconium-based film-forming technology, as a typical representative of non-phosphorus surface treatment, occupies a pivotal position in non-phosphorus pretreatment agents. Compared with traditional metal surface treatment processes such as phosphating and passivation technology, non-phosphorus pretreatment agents have incomparable advantages in environmental protection, less pollution to the environment, and will not cause eutrophication of water bodies. They have obvious advantages in consumption, cost, maintenance, etc. After continuous development in recent years, non-phosphorus technology can already meet the needs of most coating industries and has great potential.
[0003] The zirconium salt film formation process is a chemical deposition process accompanied by an electrochemical reaction. First, the reaction between the metal substrate and hydrogen ions causes the consumption of hydrogen ions, resulting in an increase in the pH of the local microenvironment, which causes the hydrolysis of zirconium ions to shift to the right, resulting in the chemical deposition of zirconium hydroxide particles, and forming an amorphous zirconium-based film layer. At the same time as the chemical deposition, the entire zirconium-based film formation process is also accompanied by an electrochemical process. The substrate corrosion produces a polarization process of electron accumulation, which significantly reduces the deposition rate of the micro-cathode area on the surface of the substrate, resulting in uneven distribution of the zirconium-based film layer, thereby causing the negative effects of poor adhesion of the paint film and decreased corrosion resistance. In response to this phenomenon, there are currently two main solutions: using a depolarizer and increasing the number of micro-cathodes. Both of them are to reduce the accumulation of electrons in the film formation process on the surface of the metal substrate by improving the depolarization ability. Among them, the path to increase the number of micro-cathodes is often achieved by introducing trace copper elements into the bath, which has a significant improvement in the uniformity of the film layer. Although the copper content in the bath is very small, copper, as a heavy metal element, still causes pollution problems to the environment. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a modified nano zirconium sol. The nano sol synthesized by the method uses zirconium element as raw material, and no heavy metal ions are introduced. The modified nano zirconium sol is used to adjust the metal surface before the metal phosphorus-free surface treatment, which can significantly improve the pulling bonding strength between the coating film and the metal substrate, and also has a significant promoting effect on the salt spray corrosion resistance of the coating film.
[0005] Technical solution: The preparation method of the modified nano zirconium sol described in the present invention is specifically as follows: 4-8g of concentrated nitric acid and 0.3-0.6g of zirconium nitrate pentahydrate solid are added to 100mL of deionized water, and after stirring to dissolve, 0.1-0.2g of aminosilane and 0.05-0.1g of epoxysilane are added at room temperature, and after sufficient stirring, the silanol groups are fully coordinated with the zirconium ions; finally, a pH adjuster is slowly added dropwise to the reaction solution to adjust the pH of the reaction system to 5-6 (the purpose of adjusting the pH of the reaction system is to ensure the storage stability of the sol), and the modified nano zirconium sol is obtained after the reaction.
[0006] Wherein, the mass concentration of the concentrated nitric acid is 65-68%.
[0007] Wherein, the aminosilane is one of KH-540, KH-550, KH-602 or KH-792 or a mixture of several thereof.
[0008] The stirring speed after adding silane was 800 rpm for 3 hours.
[0009] Wherein, the pH regulator is one of triethanolamine, ammonia water or ethylenediamine; preferably, an organic amine substance is used, which is conducive to the control of the particle size of the nanosol.
[0010] The surface regulator based on modified nano zirconium sol contains 50 g of modified nano zirconium sol per liter of the surface regulator, and the balance is deionized water.
[0011] When in use, sodium hydroxide and nitric acid solutions are used to adjust the pH of the surface adjuster to 5. The pH of the surface adjuster is adjusted to 5. On the one hand, it is close to the pH of the subsequent process to avoid drastic pH changes of the subsequent tank liquid caused by liquid carryover; on the other hand, the metal substrate is treated within this pH range, and the paint film after coating has better salt spray resistance.
[0012] Mechanism of action: When the modified nano zirconium sol of the present invention is used as a surface adjuster, due to the electrostatic adsorption effect (pre-film formation) of the zirconium sol, a micro cathode can be pre-generated on the surface of the metal substrate, which is conducive to the occurrence of depolarization, thereby ensuring the uniformity of the zirconium-based film formation process.
[0013] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the present invention uses zirconium sol that does not contain heavy metal ions as a metal reactivity regulator, which reduces environmental pressure while improving the pull-out bonding strength between the coating film and the metal substrate, and at the same time improves the salt spray corrosion resistance of the subsequent coating film; the added sol can, on the one hand, adjust the reactivity of the surface of the metal substrate, and increase the roughness of the film surface by forming micro-protrusions on the zirconium-based film layer, thereby improving the mechanical bonding strength between the subsequent coating film and the metal substrate; on the other hand, the added sol contains reactive active groups, which can react with the film-forming substance of the paint film to form chemical crosslinks, thereby improving the interfacial bonding strength through covalent bonds. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is the SEM morphology of the modified nano zirconium sol prepared in Example 1;
[0015] Figure 2 Schematic diagram of the morphology of the film layer with the participation of modified nanosol and the film layer without the participation of modified nanosol. DETAILED DESCRIPTION
[0016] All components in the surface treatment agent formula of the present invention are commercially available products: nitric acid, 68%, purchased from Sinopharm Chemical Reagent Co., Ltd.; zirconium nitrate pentahydrate, triethanolamine, KH-550, KH560, commercially available, with a purity of 95%+.
[0017] Example 1
[0018] The preparation method of the modified nano zirconium sol of the present invention is specifically as follows:
[0019] 100 mL of deionized water was added to a 250 mL three-necked round-bottom flask, and 6 g of concentrated nitric acid (mass concentration of 68%) and 0.45 g of solid zirconium nitrate pentahydrate were weighed and added to the flask, stirred to dissolve, and the reaction temperature was controlled at 30°C. Then, 0.15 g of aminosilane KH-550 and 0.05 g of epoxysilane KH-560 were added thereto, and stirred at 800 rpm for 3 h to allow the silanol group to fully coordinate with the zirconium ion; triethanolamine solution (the mass concentration of the triethanolamine aqueous solution was 0.1% to achieve the purpose of slowly changing the pH) was slowly added dropwise to the above reaction solution, the pH of the reaction system was adjusted to 5, the reaction temperature (30°C) and the stirring rate (800 rpm) were maintained, and the reaction was carried out for 5 h to obtain a modified nano-zirconium sol.
[0020] The particle size of the prepared modified nano zirconium sol is 15-20 nm, the particles are spherical, the particles are dispersed, and there is basically no agglomeration phenomenon. Figure 1 shown.
[0021] Application of the modified nano zirconium sol prepared in Example 1 as a surface conditioning agent:
[0022] Test plate: Use commercially available standard cold-rolled iron plate with specifications of (150mm×70mm×0.8mm).
[0023] Process flow:
[0024] Degreasing and deoiling → tap water washing → pure water washing → surface adjustment → phosphorus-free surface treatment → electrophoretic coating → high temperature curing
[0025] Brief introduction of each process:
[0026] Degreasing treatment: Use a commercially available heated cold-rolled plate degreasing agent to soak the cold-rolled plate at 50°C for 5 minutes, supplemented by manual swinging and scrubbing to ensure the surface is degreased and clean.
[0027] Washing after degreasing: Wash in tap water at room temperature for 1 minute, or in pure water for 1 minute.
[0028] Surface conditioning: Immerse the cold rolled iron plate in the surface conditioning agent at room temperature for 1 minute, with intermittent shaking during the period.
[0029] Phosphorus-free surface treatment: KR-S210 and KR-S211 from Nanjing Kerun Company, treated for 3 minutes at room temperature.
[0030] Electrophoretic coating: HT8000C water-based cathode electrophoretic coating produced by Xiangjiang Guanxi Coating Company on the market, the film thickness is controlled at 20-22μm. The electrophoretic test plate after washing is cured at 170℃ for 20 minutes, and then taken out and dried at room temperature.
[0031] A surface conditioning agent was prepared based on the modified nano zirconium sol prepared in Example 1: each liter of the surface conditioning agent contained 50 g of the modified nano zirconium sol, and the remainder was deionized water. The pH of the surface conditioning agent was adjusted to 5 using sodium hydroxide and nitric acid solutions.
[0032] The coating test panels without surface adjustment were compared simultaneously (the only difference between Comparative Example 1 and Example 1 is that surface adjustment was not performed before phosphorus-free surface treatment, and the rest of the processes are exactly the same as Example 1). Example 1 in Table 1 is a sample after surface adjustment of the present invention, and Comparative Example 1 is a sample without surface adjustment. Figure 2 As shown, the surface morphology of the zirconium-based film layer that has been pretreated with a surface adjuster has changed. From the cross-sectional image of the film layer, we can see the generation of film protrusions (improving the uniformity of film formation of the zirconium-based film layer) and the change in roughness (increasing the mechanical bonding strength between the paint film and the metal substrate). On the one hand, it can improve the uniformity of film formation of the zirconium-based film layer, and on the other hand, it can increase the mechanical bonding strength between the paint film and the metal substrate.
[0033] Table 1
[0034]
Claims
1. A surface conditioning agent based on modified nano zirconium sol, characterized in that: Each liter of surface conditioning agent contains 50-60g of modified nano zirconium sol, and the balance is deionized water; The modified nano-zirconium sol is prepared by the following method: 4-8 g of concentrated nitric acid and 0.3-0.6 g of zirconium nitrate pentahydrate solid are added to 100 mL of deionized water, stirred and dissolved, and then 0.1-0.2 g of aminosilane and 0.05-0.1 g of epoxysilane are added at room temperature. After sufficient stirring, the silanol groups are fully coordinated with the zirconium ions; finally, a pH regulator is slowly added dropwise to the reaction solution to adjust the pH of the reaction system to 5-6, and the modified nano-zirconium sol is obtained after the reaction.
2. The surface conditioning agent based on modified nano zirconium sol according to claim 1, characterized in that: The mass concentration of the concentrated nitric acid is 65-68%.
3. The surface conditioning agent based on modified nano zirconium sol according to claim 1, characterized in that: The aminosilane is one of KH-540, KH-550, KH-602 or KH-792 or a mixture of several thereof.
4. The surface conditioning agent based on modified nano zirconium sol according to claim 1, characterized in that: After adding silane, stir at a speed of 800-850 rpm for 3-4 hours.
5. The surface conditioning agent based on modified nano zirconium sol according to claim 1, characterized in that: The pH regulator is one of triethanolamine, ammonia water or ethylenediamine.
6. The surface conditioning agent based on modified nano zirconium sol according to claim 1, characterized in that: When using a surface conditioner, use sodium hydroxide and nitric acid solution to adjust the pH of the surface conditioner to 5~6.
Citation Information
Patent Citations
Environment-friendly metal surface treating agent and using method thereof
CN101701336A
Preparation method of zirconium oxide aerogel
CN103011280A
Process of silane-zirconium salt conversion treatment before metal cathode electrophoresis coating
CN103031584A
Silane-nanoceramic composite surface conditioning agent
CN104988563A
Magnetic microsphere for aqueous magnetorheological fluid and preparation method of such magnetic microsphere
CN106710775A