Boron-nitrogen reinforced metal coating resistant to intergranular corrosion and preparation method thereof

By adding Cr, B, N and other elements to the metal coating and using metal flux-core welding wire for laser cladding, the problem of intergranular corrosion in wire laser cladding technology is solved, and the high hardness and resistance of shaft parts are achieved Corrosion performance extends the service life of parts.

CN115976507BActive Publication Date: 2024-11-22XI AN RES INST OF INTELLIGENT REMANUFACTURING CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211691198.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-11-22
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

In the prior art, the silk laser cladding technology is difficult to meet the service requirements of shaft components in harsh environments, and is prone to intergranular corrosion, resulting in reduced mechanical strength of the metal coating and scrapped parts.

Method used

Boron-nitrogen-enhanced metal coating is used to strengthen the metal coating, and by adding elements such as Cr, B, N, etc., it forms nitrides such as TiB2, ε-(Fe, Cr)2N, Cr2N, CrN, etc., and combines stabilizing elements such as Ti and Nb to hinder the chromium carbide. Generate, improve the hardness and corrosion resistance of the coating, and laser cladding is performed through metal flux-core welding wire to expand the application range.

Benefits of technology

It achieves high hardness and corrosion resistance of shaft parts in harsh environments, extends the service life of parts, avoids the problem of strength reduction caused by intergranular corrosion, and is low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976507B_ABST
    Figure CN115976507B_ABST
Patent Text Reader

Abstract

The present invention discloses a boron-nitrogen-strengthened metal coating resistant to intergranular corrosion and a preparation method thereof, wherein a certain amount of Cr element is added to the metal coating to ensure excellent corrosion resistance of the metal coating; considering the limitation of a single C element in improving the hardness of the metal coating, B and N elements are additionally added in the present invention, and the hardness of the metal coating is improved by the composite strengthening effect of TiB2 boride and ε-(Fe, Cr)2N1-x, Cr2N, CrN and other nitrides; stabilizing elements such as Ti and Nb are added to generate niobium carbide or titanium carbide during the cladding process through their higher affinity, hindering the generation of chromium carbide, thereby restricting the formation of chromium-poor areas, and achieving the purpose of preventing intergranular corrosion. The coating is applied to shaft parts with harsh service environments, and the surface of the parts is modified to have both excellent corrosion resistance and high hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and in particular relates to a boron-nitrogen reinforced metal coating resistant to intergranular corrosion and a preparation method thereof. Background Art

[0002] Shaft components such as hydraulic supports and offshore platform columns in the coal mining industry need to rub against mating surfaces, so the metal coating needs to have sufficient hardness to resist failure due to friction and wear. In addition, surface modification is usually used in current engineering practice to improve the service performance of the above-mentioned structural parts. Wire laser cladding technology has become the most ideal technology for surface modification of the above-mentioned structural parts due to its advantages of low cost and high material utilization rate. However, such shaft parts have been in service for a long time in harsh working conditions with high humidity and a large amount of SO 2 , H 2 S and other complex corrosive media, intergranular corrosion is very likely to occur in some corrosive media, in which the stainless steel metal coating grain matrix, grain boundaries and intergranular compounds can form a micro-battery effect, which can lead to the loss of bonding between grains. This corrosion is different from other types of corrosion. This corrosion is selective corrosion damage. It is different from general selective corrosion in that this intergranular corrosion is on a microscopic scale, due to the difference in chemical composition between the surface and the inside of the grains and the presence of grain boundary impurities or internal stress. Intergranular corrosion destroys the bonding between grains, and the corrosion that expands inward along the interface between metal grains greatly reduces the mechanical strength of the metal. After the corrosion occurs, the surface of the metal and alloy still maintains a certain metallic luster, and there is no sign of damage, but the bonding between grains is significantly weakened, and the mechanical properties are deteriorated. When subjected to stress, it will break along the grain boundary and the strength will almost completely disappear, seriously affecting the normal service of parts. It leads to the scrapping and failure of the entire shaft component, seriously endangering the safe operation of the equipment.

[0003] The metal coating is prepared on the surface of the hydraulic support by wire laser cladding technology. In order to achieve high hardness and corrosion resistance of the metal coating, the chemical composition of the metal coating must be precisely controlled, resulting in a narrow process window in the preparation process. At the same time, the wire composition design is limited by the wire drawing process performance, and the composition design is limited. Some anti-intergranular corrosion elements are difficult to add. As a result, in actual use, the stainless steel metal coating will have the risk of intergranular corrosion, making it difficult for the prepared metal coating to meet the needs of shafts in harsh service environments. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a boron nitrogen strengthened metal coating resistant to intergranular corrosion and a preparation method thereof, so as to solve the problem that the wire laser cladding technology in the prior art is difficult to meet the service requirements and intergranular corrosion easily destroys the bonding between grains.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A boron-nitrogen reinforced metal coating for resisting intergranular corrosion, comprising, by mass fraction, C: 0.15-0.18%, Si: 0.20-0.40%, Mn: 0.3-0.6%, Cr: 18.50-19.7%, Ni: 1.50-2.0%, Mo: 1.1-1.60%, Ti: 0.50-1.00%, Nb: 0.50-0.75%, N: 0.30-0.45% and B: 0.20-0.70%, with the balance being Fe;

[0007] The surface hardness of the metal coating is 47-52HRC;

[0008] The boron-nitrogen strengthened metal coating contains boride, nitride, niobium carbide and titanium carbide.

[0009] A further improvement of the present invention is:

[0010] Preferably, the metal coating has a C-method corrosion rate measured by a sulfuric acid-ferric sulfate method of ≤1.0 mm / a.

[0011] Preferably, the metal coating is obtained by laser cladding a metal cored welding wire, wherein the metal cored welding wire is composed of a welding skin and a metal core powder, wherein the metal core powder is wrapped by the welding skin; and the metal core powder is arranged along the length direction of the welding skin.

[0012] Preferably, when the weld skin is a 430 stainless steel strip, the composition of the metal core powder is: C: 0.50-0.60wt.%, Si: 1.00-1.50wt.%, Mn: 1.50-2.00wt.%, Cr: 24.00-26.00wt.%, Ni: 5.00-6.00wt.%, Mo: 4.00-5.00wt.%, Nb: 2.00-2.50wt.%, Ti: 1.50-2.00wt.%, N: 1.00-1.50wt.%, B: 3.0-4.0wt.%, and the balance is Fe.

[0013] Preferably, when the weld skin is a 410 stainless steel strip, the composition of the metal core powder is: C: 0.50-0.60wt.%, Si: 0.90-1.40wt.%, Mn: 1.50-2.00wt.%, Cr: 34.50-38.00wt.%, Ni: 5.30-6.30wt.%, Mo: 4.00-5.00wt.%, Nb: 2.00-2.50wt.%, Ti: 1.50-2.00wt.%, N: 1.00-1.50wt.%, B: 3.0-4.0wt.%, and the balance is Fe.

[0014] Preferably, the filling rate of the metal cored welding wire is 30wt.%-33wt.%.

[0015] Preferably, the diameter of the metal cored welding wire is 1.0-1.2 mm.

[0016] A method for preparing a boron-nitrogen-reinforced metal coating that resists intergranular corrosion, wherein the boron-nitrogen-reinforced metal coating is prepared on a bracket by laser cladding a metal cored welding wire, wherein the metal cored welding wire is composed of a welding sheath and a metal core powder, and the metal core powder is wrapped by the welding sheath.

[0017] Preferably, the preparation process of the metal flux-cored welding wire is as follows: target metal flux-cored powder is weighed and arranged, and the metal flux-cored powder is wrapped with welding skin to obtain the metal flux-cored welding wire.

[0018] Preferably, the metal flux-cored welding wire is produced by drawing.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention discloses a boron-nitrogen-strengthened metal coating resistant to intergranular corrosion, wherein a certain amount of Cr element is added to the metal coating to ensure excellent corrosion resistance of the metal coating; considering the limitation of a single C element in improving the hardness of the metal coating, the present invention additionally adds B and N elements, and improves the hardness of the metal coating through the composite strengthening effect of TiB2 boride and ε-(Fe, Cr)2N1-x, Cr2N, CrN and other nitrides; adding stabilizing elements such as Ti and Nb, through their higher affinity, generates niobium carbide or titanium carbide during the cladding process, hinders the generation of chromium carbide, and further restricts the formation of chromium-poor areas, achieving the purpose of preventing intergranular corrosion. The coating is applied to shaft parts in harsh service environments, and by modifying the surface of the parts, it has both excellent corrosion resistance and high hardness.

[0021] Furthermore, the boron nitrogen strengthened metal coating is prepared by metal flux-cored welding wire, which uses easily available and low-cost stainless steel as the steel strip material, and uses a variety of alloy elements to achieve excellent performance of the metal coating; in order to expand the application scope of wire laser cladding, the present invention uses flux-cored welding wire in the form of stainless steel strip + metal powder to overcome the problem that it is difficult to add stabilizing elements such as Ti and Nb that resist intergranular corrosion due to work hardening of traditional wires, and finally achieves the coexistence of intergranular corrosion resistance and high hardness of the wire metal coating.

[0022] Furthermore, the present invention designs the flux core component so that the metal coating formed by the flux core and the 430 stainless steel strip or the 410 stainless steel strip after cladding can have sufficient strength and resistance to intergranular corrosion, thereby improving the overall performance of shaft parts. Compared with solid welding wire, the melting efficiency of the wire can be significantly improved during the laser cladding manufacturing process, and it has the advantages of high hardness and resistance to intergranular corrosion. The wire laser cladding technology based on the metal flux cored welding wire of the present invention also has the advantage of low cost compared with the traditional powder laser cladding technology.

[0023] The present invention also discloses a method for preparing a boron-nitrogen-strengthened metal coating that resists intergranular corrosion. The metal coating is prepared on the surface of a structural part by laser cladding a metal flux-cored welding wire. The metal wire material for laser cladding of the present invention is a flux-cored welding wire, and the metal coating finally prepared belongs to a martensitic stainless steel type material. By adding alloy elements and stabilizing elements that improve toughness, the material has good intergranular corrosion resistance and high hardness and plastic toughness, so that it can be prepared into a metal wire material by drawing. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The microstructure of the metal coating after laser cladding of the flux-cored welding wire prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0026] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0027] One of the embodiments of the present invention discloses a boron-nitrogen strengthened metal coating that is resistant to intergranular corrosion. The metal boron-nitrogen strengthened metal coating has the effect of resisting intergranular corrosion by optimizing its composition formula. The metal coating is a martensitic stainless steel type material. After the metal coating is laser clad on the surface of the hydraulic support cylinder by laser cladding wire, the hardness of the surface laser metal coating reaches HRC47-52, and the intergranular corrosion resistance of the surface laser metal coating is less than or equal to 1.0mm / a according to the C method in GB / T 4334.2-2020 using the sulfuric acid-ferric sulfate method. The standard requires that it is less than or equal to 1.2mm / a to be qualified.

[0028] The metal coating is made by TIG welding multi-layer cladding. Calculated by mass fraction, the metal coating consists of the following components: C: 0.15-0.18%; Si: 0.20-0.40%; Mn: 0.3-0.6%; Cr: 18.50-19.7%; Ni: 1.50-2.0%; Mo: 1.1-1.60%; Ti: 0.50-1.00%; Nb: 0.50-0.75%; N: 0.30-0.45%; B: 0.20-0.70%.

[0029] One of the embodiments of the present invention discloses a method for preparing a boron-nitrogen-reinforced metal coating resistant to intergranular corrosion. The preparation method comprises the following steps: subjecting a metal flux-cored welding wire to laser cladding treatment and then preparing the coating on the surface of a hydraulic support cylinder.

[0030] The present invention ensures the material's resistance to intergranular corrosion through the reasonable allocation of elements, while not only improving the material's hardness, but also having good plasticity and toughness, making it easy to draw and prepare into wire. Compared with existing martensitic stainless steel, the stainless steel component has excellent resistance to intergranular corrosion and higher hardness. The specific functions of the main alloying elements in the metal wire material formula of the present invention are as follows:

[0031] Chromium (Cr): Cr protects the metal coating from corrosion by acid and salt spray by forming a dense oxide film. The target structure of the metal coating of the present invention is a martensitic stainless steel structure. With a 430 stainless steel strip and a filling rate of 30-33wt.%, 24.00-28.00% of the Cr element is added to the powder. With a 410 stainless steel strip and a filling rate of 30-33wt.%, 34.50-38.00% of the Cr element is added to the powder.

[0032] Boron (B): B has a low solid solubility in ferrite and austenite, and excess B elements will form borides. Borides have very high hardness and can be used as hard phases in Fe-based alloys. In addition, B can also promote the growth of carbides, such as increasing the volume fraction of Cr7C3. Due to the high hardness of borides, it is necessary to control their content in the cladding metal. In the present invention, 3.00-4.00% of B elements are added to the powder in combination with 430 stainless steel strip or 410 stainless steel strip and a filling rate of 30-33wt.%.

[0033] Nitrogen (N): Due to the small size of N atoms and the similar radius to that of carbon atoms, N atoms can replace the lattice position of C in austenite to form interstitial solid solution, play a role in solid solution strengthening, and interact with other elements in steel to form dispersed nitrides to form dispersion strengthening. However, when the nitrogen content exceeds the solid solution limit of austenitic stainless steel, the excess N elements form boron nitride and chromium nitride with Cr and B elements. Since nitrogen has a strong effect on the formation and stability of austenite and can also expand the austenite phase region, it is necessary to control the addition of N elements to ensure the martensite content in the metal coating. In the present invention, 1.00-1.50% of N elements are added to the powder in combination with 430 stainless steel strip or 410 stainless steel strip and a filling rate of 30-33wt.%.

[0034] Nickel (Ni): Ni element can improve corrosion resistance and toughness of materials, and the addition of Ni can improve the fracture toughness of metal coatings. However, since Ni is an austenite stabilizing element, in order to ensure the martensitic structure of the metal coating, the content of Ni needs to be controlled in the present invention. In the present invention, 5.00-6.00% of Ni element is added to the powder in combination with 430 stainless steel 10 stainless steel strip and a filling rate of 30-33wt.%.

[0035] Niobium (Nb): Nb can be dissolved in the α-Fe matrix to play a role in solid solution strengthening. Secondly, Nb and C can react to form carbides, which play a strengthening role. However, when the amount of Nb added is large, the cold crack sensitivity of the metal coating is high, so it is necessary to control its addition amount. In the present invention, 2.00-2.50% of Nb element is added to the powder with a 430 stainless steel strip or a 410 stainless steel strip and a filling rate of 30-33wt.%.

[0036] Titanium (Ti): As a stabilizing element, titanium has a greater affinity with carbon than chromium. After titanium is added to steel, carbon preferentially combines with titanium to form titanium carbide (Tic), thus avoiding the precipitation of chromium carbide and causing chromium depletion at the grain boundary, thereby effectively preventing intergranular corrosion. Since titanium can combine with nitrogen to form titanium nitride, and titanium can combine with oxygen to form titanium dioxide, the amount of titanium added is limited to a certain extent. In actual production, in order to prevent intergranular corrosion, the amount of titanium added is generally calculated as follows: Ti=C*5~0.8%. In the present invention, 1.50-2.00% of the Ti element is added to the powder in combination with 430 stainless steel strip or 410 stainless steel strip and a filling rate of 30-33wt.%.

[0037] Molybdenum (Mo): Mo can be dissolved in the α-Fe matrix to play a role in solid solution strengthening. Mo can also improve the corrosion resistance of martensitic stainless steel. In the present invention, 4.00-5.00% of Mo element is added to the powder with a 430 stainless steel strip or a 410 stainless steel strip and a filling rate of 30-33wt.%.

[0038] Carbon (C): The C element can strongly increase the hardness of the metal coating and ensure the formation of martensite structure. However, as the C content increases, the cold crack sensitivity of the metal coating increases, so the C content needs to be strictly controlled. In the present invention, 1.00-1.50% of the C element is added to the powder with a 430 stainless steel strip or a 410 stainless steel strip and a filling rate of 30-33wt.%.

[0039] Silicon (Si) and manganese (Mn): Si and Mn have a combined deoxidation effect, which can reduce the oxygen content in the metal coating, prevent the generation of pores, and also improve the hardness of the metal coating. However, Mn is an austenite-forming element, so its content should be controlled. A large amount of Si addition will deteriorate the plasticity and toughness of the metal coating, which also needs to be controlled. In the present invention, 1.00-1.50% of Si elements and 1.50-2.00% of Mn elements are added to the powder in combination with 430 stainless steel strip and a filling rate of 30-33wt.%. In combination with 410 stainless steel strip and a filling rate of 30-33wt.%, 0.90-1.40% of Si elements and 1.50-2.00% of Mn elements are added to the powder.

[0040] The present invention discloses an embodiment in which a boron-nitrogen composite strengthened and intergranular corrosion resistant metal flux-cored welding wire for laser cladding is disclosed, which is mainly used for the preparation of metal coatings on the surface of parts with both intergranular corrosion resistance and high hardness performance requirements. The metal wire for laser cladding of the present invention is a flux-cored welding wire, and the metal coating finally prepared belongs to the martensitic stainless steel type material. By adding alloy elements that improve strength and toughness, the material has good intergranular corrosion resistance, high hardness and plastic toughness, so that it can be prepared into a metal wire by drawing.

[0041] The metal flux-cored welding wire comprises a flux core and a welding skin. Along the length direction of the welding wire, the outer surface of the flux core is covered by the welding skin, and the welding skin is a stainless steel strip. The flux core composition of the metal flux-cored welding wire of this structure is adjusted according to the different welding skins, so that the metal coating finally prepared can meet the target component requirements.

[0042] The preferred implementation of the present invention does not limit the technical solution of the present invention to this. Based on the main technical concept of the present invention, those skilled in the art only change the composition of the steel strip (for example, 430 stainless steel strip is replaced by 410 stainless steel strip, etc.) to change the composition of the powder, but if the chemical composition is the same after multi-layer cladding using the test method specified by the present invention, it still falls within the protection scope of the present invention. At the same time, based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0043] When the weld skin is made of 430 stainless steel strip, the following raw metal powders are weighed in mass percentage to prepare the flux core: in terms of mass fraction, the composition of the flux core is C: 0.50-0.60%; Si: 1.00-1.50%; Mn: 1.50-2.00%; Cr: 24.00-28.00%; Ni: 5.00-6.00%; Mo: 4.00-5.00%; Nb: 2.00-2.50%; Ti: 1.50-2.00%; N: 1.00-1.50%; B: 3.0-4.0%; the balance is Fe, and the sum of the mass percentages of the above components is 100%. The powder filling rate of the flux cored wire is 30wt.%-33wt.%.

[0044] When the weld skin is made of 410 stainless steel strip, the following raw metal powders are weighed in mass percentage to prepare the flux core: in terms of mass fraction, the composition of the flux core is, C: 0.50-0.60%; Si: 0.90-1.40%; Mn: 1.50-2.00%; Cr: 34.50-38.00%; Ni: 5.30-6.30%; Mo: 4.00-5.00%; Nb: 2.00-2.50%; Ti: 1.50-2.00%; N: 1.00-1.50%; B: 3.0-4.0%; the balance is Fe, and the sum of the mass percentages of the above components is 100%. The powder filling rate of the flux cored wire is 30wt.%-33wt.%.

[0045] The diameter of the metal flux-cored welding wire for laser cladding is φ1.0-1.2mm, and the laser cladding wire can be used for laser cladding treatment of the surface of the hydraulic support cylinder.

[0046] Specific embodiments of the present invention are given below to illustrate the implementation effects of the present invention through the embodiments.

[0047] Example 1

[0048] The metal flux core is prepared according to the following formula, calculated by mass fraction: C: 0.5; Si: 1.3%; Mn: 1.50%; Cr: 26%; Ni: 5.00%; Mo: 4.5%; Nb: 2%; B: 3.0%; Ti: 1.75%; N: 1.00%; the remainder is Fe, and the sum of the mass percentages of the above components is 100%. The prepared metal flux core is placed in a 430 stainless steel strip for wrapping, and the filling rate of the powder is controlled at 30wt.%, and the flux-cored welding wire is prepared by drawing.

[0049] The flux-cored welding wire is used for laser cladding, and the obtained laser cladding metal coating is: C: 0.153%; Si: 0.32%; Mn: 0.34%; Cr: 19.1%; Ni: 1.50%; Mo: 1.42%; B: 0.20%; Nb: 0.5%; Ti: 0.87%; N: 0.30, and the balance is iron.

[0050] Five different areas of the metal coating were tested for Rockwell hardness (HRC), which were 48.2, 49.7, 50, 49.3 and 49.2 respectively, with an average of 49.3.

[0051] The corrosion rate of the metal coating was measured by the sulfuric acid-ferric sulfate method according to GB / T 4334.2-2020 (C method), and the corrosion rate (mm / a) was 0.98.

[0052] Example 2

[0053] The metal flux core was prepared according to the following formula, calculated by mass fraction: C: 0.6; Si: 1.0%; Mn: 2.0%; Cr: 24%; Ni: 6.00%; Mo: 4%; Nb: 2.5%; B: 4.0%; Ti: 1.5%; N: 1.50%; the remainder was Fe, and the sum of the mass percentages of the above components was 100%. The prepared metal flux core was placed in a 430 stainless steel strip for wrapping, and the filling rate of the powder was controlled at 32wt.%, and the flux-cored welding wire was prepared by drawing.

[0054] The laser cladding metal coating prepared by laser cladding with the flux-cored welding wire is: C: 0.18%; Si: 0.2%; Mn: 0.58%; Cr: 18.5%; Ni: 1.97%; Mo: 1.14%; B: 0.7%; Nb: 0.68%; Ti: 0.5%; N: 0.45, and the balance is iron.

[0055] Five different areas of the metal coating were tested for Rockwell hardness (HRC), which were 54.4, 53.1, 52.7, 50.3 and 53.4 respectively, with an average of 52.8.

[0056] The corrosion rate of the metal coating was measured by the sulfuric acid-ferric sulfate method according to GB / T 4334.2-2020 (C method), and the corrosion rate (mm / a) was 0.81.

[0057] Example 3

[0058] The metal flux core was prepared according to the following formula, calculated by mass fraction: C: 0.55; Si: 1.5%; Mn: 1.7%; Cr: 28%; Ni: 5.50%; Mo: 5%; Nb: 2.3%; B: 3.5%; Ti: 1.5%; N: 1.30%; the remainder was Fe, and the sum of the mass percentages of the above components was 100%. The prepared metal flux core was placed in a 430 stainless steel strip for wrapping, and the filling rate of the powder was controlled at 33wt.%, and the flux-cored welding wire was prepared by drawing.

[0059] The flux-cored welding wire is used for laser cladding, and the obtained laser cladding metal coating is: C: 0.17%; Si: 0.4%; Mn: 0.45%; Cr: 19.7%; Ni: 1.82%; Mo: 1.6%; B: 0.51%; Nb: 0.62%; Ti: 1.0%; N: 0.39, and the balance is iron.

[0060] Five different areas of the metal coating were tested for Rockwell hardness (HRC), which were 49.8, 48.7, 49.5, 51.2 and 52 respectively, with an average of 50.2.

[0061] The corrosion rate of the metal coating was measured by the sulfuric acid-ferric sulfate method according to GB / T 4334.2-2020 (method C), and the corrosion rate was 0.94 mm / a.

[0062] The laser metal coating prepared in Example 3 has a structure as follows Figure 1 As shown: the cladding layer is mainly composed of cellular dendrites, the organization is martensite, including dendrite segregation Cr-rich phase and complex carbides (NbC, TiB2, Cr2N, CrN, TiC, etc.), and the organization is evenly distributed.

[0063] Example 4

[0064] The metal flux core is prepared according to the following formula, calculated by mass fraction: C: 0.5; Si: 0.9%; Mn: 1.78%; Cr: 34.5%; Ni: 5.30%; Mo: 4.5%; Nb: 2.5%; B: 3.5%; Ti: 1.5%; N: 1.0%; the remainder is Fe, and the sum of the mass percentages of the above components is 100%. The prepared metal flux core is placed in a 410 stainless steel strip for wrapping, and the filling rate of the powder is controlled at 30wt.%, and the flux-cored welding wire is prepared by drawing.

[0065] The flux-cored welding wire is used for laser cladding, and the obtained laser cladding metal coating is: C: 0.165%; Si: 0.22%; Mn: 0.45%; Cr: 18.6%; Ni: 1.53%; Mo: 1.39%; B: 0.43%; Nb: 0.7%; Ti: 0.5%; N: 0.34, and the balance is iron.

[0066] Five different areas of the metal coating were tested for Rockwell hardness (HRC), which were 49.8, 48.9, 51.2, 48.9 and 49.6 respectively, with an average of 49.7.

[0067] The corrosion rate of the metal coating was measured by the sulfuric acid-ferric sulfate method according to GB / T 4334.2-2020 (C method), and the corrosion rate (mm / a) was 0.95.

[0068] Example 5

[0069] The metal flux core was prepared according to the following formula, calculated by mass fraction: C: 0.6; Si: 1.4%; Mn: 2.0%; Cr: 38%; Ni: 6.30%; Mo: 4%; Nb: 2%; B: 4.0%; Ti: 2%; N: 1.50%; the remainder was Fe, and the sum of the mass percentages of the above components was 100%. The prepared metal flux core was placed in a 410 stainless steel strip for wrapping, and the filling rate of the powder was controlled at 32wt.%, and the flux-cored welding wire was prepared by drawing.

[0070] The flux-cored welding wire is used for laser cladding, and the obtained laser cladding metal coating is: C: 0.15%; Si: 0.4%; Mn: 0.6%; Cr: 19.7%; Ni: 2%; Mo: 1.1%; B: 0.7%; Nb: 0.53%; Ti: 1.0%; N: 0.45, and the balance is iron.

[0071] Five different areas of the metal coating were tested for Rockwell hardness (HRC), which were 52.4, 50.9, 53.5, 52.8 and 51.7 respectively, with an average of 52.3.

[0072] The corrosion rate of the metal coating was measured by the sulfuric acid-ferric sulfate method according to GB / T 4334.2-2020 (C method), and the corrosion rate (mm / a) was 0.81.

[0073] Example 6

[0074] The metal flux core is prepared according to the following formula, calculated by mass fraction: C: 0.55; Si: 1.3%; Mn: 1.50%; Cr: 25%; Ni: 5.00%; Mo: 5.0%; Nb: 2.25%; B: 3.0%; Ti: 1.3%; N: 1.25%; the remainder is Fe, and the sum of the mass percentages of the above components is 100%. The prepared metal flux core is placed in a 410 stainless steel strip for wrapping, and the filling rate of the powder is controlled at 30wt.%, and the flux-cored welding wire is prepared by drawing.

[0075] The flux-cored welding wire is used for laser cladding, and the obtained laser cladding metal coating is: C: 0.153%; Si: 0.32%; Mn: 0.34%; Cr: 19.1%; Ni: 1.50%; Mo: 1.60%; B: 0.20%; Nb: 0.6%; Ti: 0.87%; N: 0.38, and the balance is iron.

[0076] Five different areas of the metal coating were tested for Rockwell hardness (HRC), which were 48.2, 49.7, 50, 49.3 and 49.2 respectively, with an average of 49.3.

[0077] The corrosion rate of the metal coating was measured by the sulfuric acid-ferric sulfate method according to GB / T 4334.2-2020 (C method), and the corrosion rate (mm / a) was 0.98.

[0078] The present invention further proposes a method for preparing the metal flux-cored welding wire for laser cladding, which is a method for drawing a 430 stainless steel strip or a 410 stainless steel strip wrapped with powder, and can prepare a stainless steel wire material with a diameter of φ1.0mm-φ1.2mm for laser cladding treatment of the surface of the hydraulic support cylinder. The invention optimizes the formula ratio so that the stainless steel wire material has excellent corrosion resistance and high hardness.

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A boron-nitrogen-reinforced metal coating resistant to intergranular corrosion, characterized in that: In terms of mass fraction, it includes C: 0.15-0.18%, Si: 0.20-0.40%, Mn: 0.3-0.6%, Cr: 18.50-19.7%, Ni: 1.50-2.0%, Mo: 1.1-1.60%, Ti: 0.50-1.00%, Nb: 0.50-0.75%, N: 0.30-0.45% and B: 0.20-0.70%, and the balance is Fe; The surface hardness of the metal coating is 47-52HRC; The boron-nitrogen strengthened metal coating contains boride, nitride, niobium carbide and titanium carbide.

2. The boron-nitrogen-reinforced metal coating for resisting intergranular corrosion according to claim 1, characterized in that: The corrosion rate of the metal coating measured by the sulfuric acid-ferric sulfate method is ≤1.0 mm / a.

3. The boron-nitrogen strengthened metal coating according to claim 1 or 2, characterized in that: The metal coating is obtained by laser cladding of a metal flux-cored welding wire, wherein the metal flux-cored welding wire is composed of a welding skin and a metal flux-cored powder, wherein the metal flux-cored powder is wrapped by the welding skin; and the metal flux-cored powder is arranged along the length direction of the welding skin.

4. The boron-nitrogen strengthened metal coating according to claim 3, characterized in that: When the weld skin is 430 stainless steel strip, the composition of the metal core powder is: C: 0.50-0.60wt.%, Si: 1.00-1.50wt.%, Mn: 1.50-2.00wt.%, Cr: 24.00-26.00wt.%, Ni: 5.00-6.00wt.%, Mo: 4.00-5.00wt.%, Nb: 2.00-2.50wt.%, Ti: 1.50-2.00wt.%, N: 1.00-1.50wt.%, B: 3.0-4.0wt.%, and the balance is Fe.

5. The boron-nitrogen reinforced metal coating for resisting intergranular corrosion according to claim 3, characterized in that: When the weld skin is 410 stainless steel strip, the composition of the metal core powder is: C: 0.50-0.60wt.%, Si: 0.90-1.40wt.%, Mn: 1.50-2.00wt.%, Cr: 34.50-38.00wt.%, Ni: 5.30-6.30wt.%, Mo: 4.00-5.00wt.%, Nb: 2.00-2.50wt.%, Ti: 1.50-2.00wt.%, N: 1.00-1.50wt.%, B: 3.0-4.0wt.%, and the balance is Fe.

6. The boron-nitrogen reinforced metal coating for resisting intergranular corrosion according to claim 3, characterized in that: The filling rate of the metal cored welding wire is 30wt.%-33wt.%.

7. The boron-nitrogen reinforced metal coating for resisting intergranular corrosion according to claim 3, characterized in that: The diameter of the metal flux-cored welding wire is 1.0-1.2 mm.

8. A method for preparing the boron-nitrogen reinforced metal coating resistant to intergranular corrosion according to claim 1, characterized in that: The boron nitrogen strengthened metal coating is prepared on the bracket by laser cladding of a metal flux-cored welding wire, wherein the metal flux-cored welding wire is composed of welding skin and metal flux-cored powder, and the metal flux-cored powder is wrapped by the welding skin.

9. The method for preparing a boron-nitrogen reinforced metal coating resistant to intergranular corrosion according to claim 8, characterized in that: The preparation process of the metal flux-cored welding wire is as follows: a target metal flux-cored powder is weighed, and the metal flux-cored powder is wrapped with a welding skin to obtain the metal flux-cored welding wire.

10. The method for preparing a boron-nitrogen reinforced metal coating resistant to intergranular corrosion according to claim 8, characterized in that: The metal flux-cored welding wire is made by drawing.