A kind of erbium-containing yttrium hydride material and preparation method thereof

By preparing erbium-containing yttrium hydride materials, combined with their high temperature stability and hydrogen storage capabilities, the problems of neutron slowing and reactivity control in traditional nuclear reactors are solved, and the dual effects of fuel life extension and material stability are achieved.

CN116002620BActive Publication Date: 2024-11-29NUCLEAR POWER INSTITUTE OF CHINA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310060840.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-11-29
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

In traditional nuclear reactors, it is difficult to achieve neutron slowing and reactivity control at the same time, and the material stability in high temperature environments is poor, which affects the fuel life.

Method used

Using erbium-containing yttrium hydride material, erbium-containing yttrium hydride powder is mixed, and hydrogen permeates in a vacuum environment after sintering, to prepare erbium-containing yttrium hydride core pellets, combining high temperature stability and hydrogen storage capacity to achieve neutron slowing and reaction The dual role of sexual control.

Benefits of technology

It provides a high-temperature solid slowing material, which consumes slower than traditional combustible poisons, extends fuel life, and is simple in preparation, replacing the problem of erbium-doped fuel pellets, achieving the dual effects of neutron slowing and reactivity control. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application belongs to the field of material design technology, and specifically relates to an erbium-containing yttrium hydride material and a preparation method thereof; the erbium-containing yttrium hydride material comprises erbium with a mass content of 0.1%-10%, and a hydrogen-yttrium atomic ratio of 1.56-2.11. The erbium-containing yttrium hydride material solves the problems of high-temperature neutron moderation and reactivity control, and can be applied to nuclear reactor reactivity control and neutron moderation, and can also be applied to the field of high-temperature hydrogen storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of material design, and specifically relates to an erbium-containing yttrium hydride material and a preparation method thereof. Background Art

[0002] In thermal neutron nuclear reactors, it is usually necessary to moderate the neutrons produced in nuclear fission to improve the economy of neutrons; on the other hand, it is necessary to add burnable poisons to control the reactivity of the fuel in the reactor and extend the fuel life. In traditional nuclear reactors, water is used as a moderator and gadolinium oxide is combined with nuclear fuel to achieve neutron moderation and reactivity control. Summary of the invention

[0003] The purpose of this application is to provide an erbium-containing yttrium hydride material and a preparation method thereof to solve the problems of high-temperature neutron moderation and reactivity control. The erbium-containing yttrium hydride material can be used for nuclear reactor reactivity control and neutron moderation, and can also be used in the field of high-temperature hydrogen storage.

[0004] Technical solution to achieve the purpose of this application:

[0005] A first aspect of an embodiment of the present application provides an erbium-containing yttrium hydride material, comprising erbium with a mass content of 0.1%-10%, and a hydrogen-yttrium atomic ratio of 1.56-2.11.

[0006] A second aspect of an embodiment of the present application provides a method for preparing an erbium-containing yttrium hydride material, characterized in that it is used to prepare the erbium-containing yttrium hydride material according to claim 1; the method comprises:

[0007] Mixing yttrium hydride and erbium hydride powders according to the weight ratio of yttrium and erbium metals to obtain a green body of a mixture of yttrium and erbium hydride;

[0008] The green body is sintered to obtain an erbium-containing yttrium hydride core block;

[0009] The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace for hydrogenation to obtain the erbium-containing yttrium hydride material.

[0010] Optionally, the sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace for hydrogenation to obtain the erbium-containing yttrium hydride material, which specifically includes:

[0011] The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace and vacuumed to a temperature not less than 4×10 -4 Pa, heated to 400°C at a heating rate of 10°C / min, slowly introduced hydrogen with a purity of 7N until the hydrogen absorption was saturated, and then cooled to room temperature with the furnace. After the hydrogen absorption was balanced, the erbium-containing yttrium hydride material was obtained.

[0012] Optionally, the green body is sintered to obtain the erbium-containing yttrium hydride core block, specifically comprising:

[0013] The green body is in a vacuum of not less than 4×10 -4 After being kept at 1000°C for 2 hours in a vacuum environment of 1.5 Pa, the furnace was cooled to room temperature to obtain erbium-containing yttrium hydride core blocks.

[0014] Optionally, the sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace for hydrogenation, and then further comprises:

[0015] The sintered material is polished with sandpaper of 800 mesh or above to obtain erbium-containing yttrium hydride material.

[0016] Optionally, the powders of yttrium hydride and erbium hydride are obtained according to the following steps:

[0017] Using metallic erbium and metallic yttrium as raw materials, placing them in a sample chamber of a hydrogenation furnace, and performing hydrogenation treatment in the sample chamber to obtain yttrium hydride blocks and erbium hydride blocks;

[0018] The yttrium hydride block and the erbium hydride block are crushed into powder by a hammer mill in a dry inert gas protection environment.

[0019] Optionally, the powders of yttrium hydride and erbium hydride are obtained according to the following steps:

[0020] Using metallic erbium and metallic yttrium as raw materials, smelting in an electric arc furnace according to the weight ratio of yttrium to erbium metal to obtain a yttrium-erbium alloy;

[0021] The yttrium-erbium alloy is placed in a sample chamber of a hydrogenation furnace, and hydrogenation treatment is performed in the sample chamber to obtain yttrium hydride bulk and erbium hydride bulk;

[0022] The yttrium hydride block and the erbium hydride block are crushed into powder by a hammer mill in a dry inert gas protection environment.

[0023] Optionally, the hydrogenation treatment is performed in the sample chamber to obtain the yttrium hydride bulk and the erbium hydride bulk, specifically comprising:

[0024] At room temperature, evacuate the sample chamber to a vacuum of no less than 4 × 10 -4 Pa, heated to 700°C ~ 800°C at a heating rate of 20°C / min, introduced hydrogen with a purity of 7N until saturated, kept the hydrogen partial pressure and temperature unchanged for 1 hour, cooled to 200°C ~ 300°C at a cooling rate of about 40°C / min, after saturated with hydrogen absorption at a constant temperature, cooled to room temperature with the furnace, and after the hydrogen absorption equilibrium was reached, yttrium hydride block and erbium hydride block were obtained.

[0025] Optionally, the method of crushing the yttrium hydride block and the erbium hydride block into powder using a hammer mill in a dry inert gas protection environment specifically includes:

[0026] The yttrium hydride and erbium hydride blocks were crushed into 400 mesh powders by a hammer mill in a dry argon protection environment.

[0027] Optionally, the smelting in an electric arc furnace to obtain the yttrium-erbium alloy specifically includes:

[0028] Before melting, the vacuum was pumped to 4 × 10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

[0029] A third aspect of an embodiment of the present application provides a method for preparing an erbium-containing yttrium hydride material, characterized in that it is used to prepare the erbium-containing yttrium hydride material according to claim 1; the method comprises:

[0030] Using metallic erbium and metallic yttrium as raw materials, smelting in an electric arc furnace according to the weight ratio of yttrium to erbium metal to obtain a yttrium-erbium alloy;

[0031] The yttrium-erbium alloy is subjected to hydrogenation treatment to obtain erbium-containing yttrium hydride material.

[0032] Optionally, the smelting in an electric arc furnace to obtain the yttrium-erbium alloy specifically includes:

[0033] Before melting, the vacuum was pumped to 4 × 10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

[0034] Optionally, the step of subjecting the yttrium-erbium alloy to hydrogenation treatment to obtain the erbium-containing yttrium hydride material specifically includes:

[0035] At a vacuum degree higher than 4×10 -4 After annealing at 850°C and 7N hydrogen for 12 hours, slowly introduce 7N hydrogen within 50 hours until it reaches 100 kPa; keep the pressure stable and cool to 700°C at a rate of -40°C / h; after maintaining stability at 700°C and 100 kPa hydrogen partial pressure, turn off the hydrogen and stop heating, and cool to room temperature with the furnace.

[0036] Optionally, the step of subjecting the yttrium-erbium alloy to hydrogenation treatment further comprises:

[0037] When lathe processing is performed on the samples obtained after hydrogenation, an inert environment is required for dry processing, while non-aqueous coolants are used for cooling during wet processing; finally, sandpaper with a mesh size of 800 or above is used for mechanical polishing.

[0038] The beneficial technical effects of this application are:

[0039] An erbium-containing yttrium hydride material and a preparation method thereof are provided in an embodiment of the present application. The yttrium hydride has good high-temperature stability and strong hydrogen storage capacity, and is a high-temperature solid moderator material. Compared with the traditional Gd, the burnable poison Er is consumed slowly and is suitable for long-life fuel design. At the same time, Er is also one of the traditional hydrogen storage materials. The burnable poison Er is mixed with yttrium hydride in the form of a hydride to form an erbium-containing yttrium hydride material, which can achieve the dual effects of neutron moderation and reactor reactivity control, thereby extending the fuel life. In terms of the preparation of burnable poisons, the preparation method of erbium-containing yttrium hydride pellets is simple, and replaces the solution of erbium-doped fuel pellets, avoiding the difficulty of preparing erbium-doped fuel pellets. DETAILED DESCRIPTION

[0040] In order to make those skilled in the art better understand the present application, the technical scheme in the embodiment of the present application will be clearly and completely described in conjunction with the embodiment of the present application below. Obviously, the embodiment described below is only a part of the embodiment of the present application, not all. Based on the embodiment recorded in the present application, all other embodiments obtained by those skilled in the art without paying creative work are within the scope of protection of the present application.

[0041] The inventors of this application found in their research that in power reactors, the initial residual reactivity of new reactors is relatively large. In addition to using control rods, burnable poisons are usually used to compensate for this residual reactivity. Erbium (Er) is one of the burnable poison materials for light water reactors. Natural erbium contains six isotopes: 163 Er(0.14%), 164 Er (1.61%), 166 Er (33.6%), 167 Er(22.95%), 168 Er (26.8%) and 170 Er(14.9%), the main absorber is 167 Er, its thermal neutron absorption cross section is 740 target, and 166 After absorbing a neutron, Er transforms into 167 Er. Compared with the commonly used burnable poison gadolinium, erbium is consumed more slowly and is more suitable for long-life refueling design. Erbium-doped fuel pellets, which are mixed with nuclear fuel uranium dioxide in the form of erbium oxide, can reduce the core power density, improve the reliability of fuel assemblies, increase burnup, and reduce the volume of spent fuel. Irradiation tests have been carried out in Russian graphite reactors, and it is planned to replace the traditional burnable poison gadolinium in light water reactors in 2020. Therefore, the method of erbium doping to achieve core reactivity control is feasible.

[0042] On the other hand, metal hydrides have the same or even higher hydrogen atom concentration than pure water and liquid hydrogen, and their moderation performance is equivalent to or even better than that of traditional cooling water. Among them, ZrHx and YHx have the advantages of low introduction activity, low neutron absorption cross section, low hydrogen decomposition pressure, high hydrogen density, phase stability and low cost, and are widely considered to be moderated materials and neutron reflective materials for nuclear reactors. Zirconium hydride has been used as a moderator material for pulse reactors and small thermal reactors in the aviation field. In an atmosphere with a hydrogen partial pressure of 1atm, zirconium hydride begins to decompose rapidly at around 800℃, while yttrium hydride can remain stable at around 1000℃. Therefore, yttrium hydride is more suitable for high-temperature application environments. According to the different hydrogen content, yttrium hydride is divided into solid solution α phase (αY), hydride δ phase YH2 and ε phase YH3, and the crystal structures are HCP, FCC and FCT structures respectively. In addition, erbium is also a commonly used hydrogen storage material, and its hydride has α, β and γ phases. The γ phase is a metastable state, usually in the form of ErH3, with an HCP crystal structure; the β phase is a thermodynamically stable state, close to the form of ErH2, with an FCC crystal structure, and the α phase is hydrogen solid dissolved in metallic erbium, with the same crystal structure as metallic erbium, generally with an HCP structure. ErH2 can remain stable above 800°C at a hydrogen partial pressure of 500Pa. From the crystal structure, high temperature stability and mutual solubility of the metallic state, it can be seen that yttrium hydride doped with erbium (in the form of erbium hydride) is technically and theoretically feasible.

[0043] If the combustible poison is combined with a solid moderator material and an appropriate structural design is performed, the design requirements of the reactivity coefficient and the longevity can be met at the same time. Erbium and yttrium are compatible, and a mutually soluble erbium-yttrium binary alloy can be obtained through vacuum melting. Erbium can be used as both a combustible poison and a moderator material for hydrogen storage. It is highly feasible in theory and technology to combine it with yttrium hydride, which has better high-temperature stability, to form a moderator material containing a combustible poison. Therefore, in the embodiment of the present application, the combustible poison erbium is doped into yttrium hydride in the form of erbium hydride to realize an erbium-containing yttrium hydride moderator material to achieve the purpose of high-temperature moderation of neutrons and reactivity control.

[0044] Based on the above content, in order to clearly and in detail illustrate the above advantages of the present application, the specific implementation methods of the present application will be described below.

[0045] An erbium-containing yttrium hydride material provided in an embodiment of the present application includes erbium with a mass content of 0.1%-10%, and a hydrogen-yttrium atomic ratio of 1.56-2.11.

[0046] The embodiment of the present application also provides a method for preparing an erbium-containing yttrium hydride material, which is used to prepare an erbium-containing yttrium hydride material provided in the above embodiment. The method can be divided into two schemes: mixing yttrium hydride powder and erbium hydride powder and directly hydrogenating a yttrium erbium alloy and then crushing it into powder to prepare yttrium erbium hydride mixed powder, which are explained one by one below.

[0047] First: Mix yttrium hydride powder and erbium hydride powder.

[0048] The present application provides a method for preparing an erbium-containing yttrium hydride material, comprising:

[0049] Mixing yttrium hydride and erbium hydride powders according to the weight ratio of yttrium and erbium metals to obtain a green body of a mixture of yttrium and erbium hydride;

[0050] The green body is sintered to obtain an erbium-containing yttrium hydride core block;

[0051] The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace for hydrogenation to obtain the erbium-containing yttrium hydride material.

[0052] In the embodiments of the present application, the powders of yttrium hydride and erbium hydride can be obtained according to the following two methods, which are described below with examples one by one.

[0053] In one example, powders of yttrium hydride and erbium hydride can be directly obtained according to the following steps:

[0054] Using metallic erbium and metallic yttrium as raw materials, placing them in a sample chamber of a hydrogenation furnace, and performing hydrogenation treatment in the sample chamber to obtain yttrium hydride blocks and erbium hydride blocks;

[0055] The yttrium hydride block and the erbium hydride block are crushed into powder by a hammer mill in a dry inert gas protection environment.

[0056] In another example, powders of yttrium hydride and erbium hydride are obtained according to the following steps:

[0057] Using metallic erbium and metallic yttrium as raw materials, smelting in an electric arc furnace according to the weight ratio of yttrium to erbium metal to obtain a yttrium-erbium alloy;

[0058] The yttrium-erbium alloy is placed in a sample chamber of a hydrogenation furnace, and hydrogenation treatment is performed in the sample chamber to obtain yttrium hydride bulk and erbium hydride bulk;

[0059] The yttrium hydride block and the erbium hydride block are crushed into powder by a hammer mill in a dry inert gas protection environment.

[0060] The following is a detailed description with reference to specific embodiments:

[0061] Embodiment 1:

[0062] Step 1: Use metallic erbium and metallic yttrium as raw materials with a purity of not less than 99.95% in the form of rods or blocks; use sandpaper or a file to grind the metal to remove the surface oxide layer; then wash it with analytical pure acetone and let it air dry naturally; cut the cleaned metal into metal sheets and place them into the sample chamber of the hydrogenation furnace according to the weight ratio of yttrium to erbium metal.

[0063] Step 2: At room temperature, evacuate the sample chamber to a vacuum of no less than 4 × 10 -4 Pa, heat to 700℃~800℃ at a heating rate of 20℃ / min, introduce hydrogen with a purity of 7N until saturation, and keep the hydrogen partial pressure and temperature unchanged; about 1 hour, reduce the temperature to 200℃~300℃ at a cooling rate of about 40℃ / min, after saturation of hydrogen absorption at constant temperature, cool to room temperature with the furnace, open the sample chamber after hydrogen absorption equilibrium, release the remaining hydrogen, and take out the sample.

[0064] Step 3: Use a hammer mill to crush the yttrium hydride and erbium hydride blocks into 400 mesh powder in a dry argon protection environment.

[0065] Step 4: Pour the yttrium hydride and erbium hydride powders into a double cone mixer and mix for about 30 minutes; pour into a graphite mold and use a hydraulic press to maintain a pressure of 40 MPa for 10 minutes to obtain a green body of the yttrium and erbium hydride mixture.

[0066] Step 5: Sintering of green body in vacuum environment with vacuum degree not less than 4×10 -4 After being kept at 1000°C for 2 hours, the furnace is cooled to room temperature to obtain erbium-containing yttrium hydride core blocks;

[0067] Step 6: Place the sintered erbium-containing yttrium hydride core in a hydrogenation furnace and evacuate the sample chamber to 8×10 -5 Pa~4×10 -4 Pa, heated to 400℃ at a heating rate of 10℃ / min, slowly introduced hydrogen with a purity of 7N until the hydrogen absorption was saturated, cooled to room temperature with the furnace, and after the hydrogen absorption was balanced, opened the sample chamber, released the remaining hydrogen, and took out the sample.

[0068] Step 7: The sintered sample is polished with sandpaper of 800 mesh or above to obtain erbium-containing yttrium hydride material.

[0069] Embodiment 2:

[0070] Step 1: Use metallic erbium and metallic yttrium as raw materials, with a purity of not less than 99.95%, in the form of rods or blocks; use sandpaper or a file to grind the metal to remove the surface oxide layer; then wash it with analytical pure acetone and let it air dry naturally; cut the cleaned metal into metal sheets.

[0071] Step 2: Use an electric arc furnace to melt the yttrium-erbium alloy. Put the two metals, yttrium and erbium, into the furnace according to the weight ratio of the metals. Before melting, draw the vacuum to 4×10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

[0072] Step 3: At room temperature, evacuate the sample chamber to a vacuum of no less than 4 × 10 -4 Pa, heat to 700℃~800℃ at a heating rate of 20℃ / min, introduce hydrogen with a purity of 7N until saturation, and keep the hydrogen partial pressure and temperature unchanged; about 1 hour, reduce the temperature to 200℃~300℃ at a cooling rate of about 40℃ / min, after saturation of hydrogen absorption at constant temperature, cool to room temperature with the furnace, open the sample chamber after hydrogen absorption equilibrium, release the remaining hydrogen, and take out the sample.

[0073] Step 4: Use a hammer mill to crush the yttrium hydride and erbium hydride blocks into 400 mesh powder in a dry argon protection environment.

[0074] Step 5: Pour the yttrium hydride and erbium hydride powders into a double cone mixer and mix for about 30 minutes; pour into a graphite mold and use a hydraulic press to maintain a pressure of 40 MPa for 10 minutes to obtain a green body of the yttrium and erbium hydride mixture.

[0075] Step 6: Sintering of green body in vacuum environment 2, vacuum degree not less than 4×10 -4 P, after being kept at 1000°C for 2 hours, the furnace is cooled to room temperature to obtain an erbium-containing yttrium hydride core block;

[0076] Step 7: Place the sintered erbium-containing yttrium hydride core block in a hydrogenation furnace and evacuate the sample chamber to a vacuum of not less than 4×10 -4 Pa, heated to 400℃ at a heating rate of 10℃ / min, slowly introduced hydrogen with a purity of 7N until the hydrogen absorption was saturated, cooled to room temperature with the furnace, and after the hydrogen absorption was balanced, opened the sample chamber, released the remaining hydrogen, and took out the sample.

[0077] Step 8: The sintered sample is polished with sandpaper of 800 mesh or above to obtain erbium-containing yttrium hydride material.

[0078] Embodiment 3

[0079] This embodiment is a method for preparing a cylindrical yttrium hydride (Φ10mm×10mm) containing 10% Er, wherein the atomic ratio of hydrogen to yttrium is about 1.56. The specific steps are:

[0080] (1) Preparation of metal samples: Use metal erbium and metal yttrium rods with a purity of not less than 99.95%; use 3000-grit sandpaper to polish the metal to remove the surface oxide layer; then clean it with analytical pure acetone and let it air dry naturally; cut the cleaned metal into metal sheets and place them in the sample chamber of the hydrogenation furnace at a weight ratio of erbium to yttrium of 1:9.

[0081] (2) Hydrogen permeation: At room temperature, the sample chamber was evacuated to 4×10 -4 Pa, heat to 800℃ at a heating rate of 20℃ / min, introduce hydrogen with a purity of 7N until saturation; after maintaining constant temperature and pressure for 1h, maintain the hydrogen partial pressure and reduce it to 300℃ at a cooling rate of about 40℃ / min; after maintaining constant temperature and pressure for 1h, cool to room temperature with the furnace, open the sample chamber after hydrogen absorption equilibrium, release the remaining hydrogen and take out the sample.

[0082] (3) Crushing: Using a hammer mill, crush the yttrium hydride and erbium hydride blocks into 400 mesh powder in a dry argon protection environment.

[0083] (4) Billet making: Pour the yttrium hydride and erbium hydride powders into a double cone mixer and mix for about 30 minutes; pour into a Φ10 mm graphite mold, and after compaction, the height is about 20 mm. Use an oil press to maintain a pressure of 40 MPa for 10 minutes to obtain a green billet of the yttrium and erbium hydride mixture.

[0084] (5) Sintering: at a vacuum degree of 4×10 -4 After being kept at 1000°C for 2 hours in a vacuum environment of 500 Pa, the furnace was cooled to room temperature and the erbium-containing yttrium hydride core block was removed.

[0085] (6) Secondary hydrogenation: The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace. The sample chamber is evacuated to 4×10 -4 Pa, heated to 400℃ at a heating rate of 10℃ / min, slowly introduced hydrogen with a purity of 7N until the hydrogen absorption was saturated, cooled to room temperature with the furnace, and after the hydrogen absorption was balanced, opened the sample chamber, released the remaining hydrogen, and took out the sample.

[0086] (7) Finishing: The sintered samples were polished with sandpaper of 800 mesh or above.

[0087] Second: Use yttrium erbium alloy to directly hydrogenate and then crush and powder.

[0088] The embodiment of the present application also provides a method for preparing an erbium-containing yttrium hydride material, which is used to prepare an erbium-containing yttrium hydride material provided in the above embodiment.

[0089] The present application provides a method for preparing an erbium-containing yttrium hydride material, comprising:

[0090] Using metallic erbium and metallic yttrium as raw materials, smelting in an electric arc furnace according to the weight ratio of yttrium to erbium metal to obtain a yttrium-erbium alloy;

[0091] The yttrium-erbium alloy is subjected to hydrogenation treatment to obtain erbium-containing yttrium hydride material.

[0092] The following is a detailed description with a specific example:

[0093] Embodiment 4:

[0094] A method for preparing 0.1% Er yttrium hydride cylinder (Φ10mm×10mm) by direct hydrogenation, wherein the atomic ratio of hydrogen to yttrium is about 1.98, and the specific steps are:

[0095] Step 1: Use metallic erbium and metallic yttrium as raw materials, with a purity of not less than 99.95%, in the form of rods or blocks; use sandpaper or a file to grind the metal to remove the surface oxide layer; then wash it with analytical pure acetone and let it air dry naturally; cut the cleaned metal into metal sheets.

[0096] Step 2: Use an electric arc furnace to melt the yttrium-erbium alloy. Put the two metals of erbium and yttrium into the furnace at a metal weight ratio of 1:99; before melting, draw the vacuum to 4×10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

[0097] Step 3: Remove the burrs of the yttrium erbium alloy and cut it into a designed shape, such as a cylinder or a polygonal block, and mechanically polish the surface. For example, cut the alloy ingot into a Φ10mm×10mm rod and use 3000-grit sandpaper to mechanically polish the surface.

[0098] Step 4: When the vacuum degree is higher than 4×10 -4 After annealing at 850°C and 7N hydrogen for 12 hours, slowly introduce 7N hydrogen to 100 kPa for a long time (about 50 hours); keep the pressure stable and cool to 700°C at a rate of -40°C / h; after maintaining stability at 700°C and 100 kPa hydrogen partial pressure, turn off the hydrogen and stop heating, and cool to room temperature with the furnace.

[0099] Step 5: When lathing the sample obtained after hydrogenation, an inert environment is required for dry machining, and non-aqueous coolants are used for cooling during wet machining. Finally, mechanical polishing is performed using sandpaper with a mesh size of 800 or above.

[0100] Embodiment five:

[0101] This embodiment is a method for preparing 0.1% Er yttrium hydride cylinder (Φ10mm×10mm) by powder sintering method, wherein the atomic ratio of hydrogen to yttrium is about 2.11. The specific steps are:

[0102] Step 1: Use metallic erbium and metallic yttrium as raw materials, with a purity of not less than 99.95%, in the form of rods or blocks; use sandpaper or a file to grind the metal to remove the surface oxide layer; then wash it with analytical pure acetone and let it air dry naturally; cut the cleaned metal into metal sheets.

[0103] Step 2: Use an electric arc furnace to melt the yttrium-erbium alloy. Put the two metals of erbium and yttrium into the furnace at a metal weight ratio of 1:99; before melting, draw the vacuum to 4×10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

[0104] Step 3: Use a hammer mill to crush the yttrium hydride and erbium hydride blocks into 400 mesh powder in a dry argon protection environment.

[0105] Step 4: Pour the yttrium hydride and erbium hydride powders into a double cone mixer and mix for about 30 minutes; pour into a Φ10 mm graphite mold, and after compaction, the height is about 20 mm. Use a hydraulic press to maintain a pressure of 40 MPa for 10 minutes to obtain a green body of the yttrium and erbium hydride mixture.

[0106] Step 5: Vacuum 4×10 -4 After being kept at 1000°C for 2 hours in a vacuum environment of 500 Pa, the furnace was cooled to room temperature and the erbium-containing yttrium hydride core block was removed.

[0107] Step 6: Place the sintered erbium-containing yttrium hydride core in a hydrogenation furnace and evacuate the sample chamber to 4×10 -4 Pa, heated to 400℃ at a heating rate of 10℃ / min, slowly introduced hydrogen with a purity of 7N until the hydrogen absorption was saturated, cooled to room temperature with the furnace, and after the hydrogen absorption was balanced, opened the sample chamber, released the remaining hydrogen, and took out the sample.

[0108] Step 7: The sintered sample is polished with sandpaper of 800 grit or above.

[0109] Comparative Example 1

[0110] The preparation was carried out according to the implementation process of Example 3 (wherein the atomic ratio of hydrogen to yttrium was about 1.86) except that: in step (2), 7N hydrogen was introduced after heating to 700°C, and the temperature was lowered to 200°C to absorb hydrogen saturation, and then cooled to room temperature in the furnace.

[0111] The pellets obtained in the above embodiments and comparative examples were measured for hydrogen content at different temperatures using an ICP-MS to obtain the H / Y atomic ratio, and the measurement results are shown in Table 1. The erbium content in Example 3 is relatively high. Since the high-temperature stability of erbium hydride is worse than that of yttrium, the hydrogen content of Example 1 is lower than that of other embodiments, but the hydrogen content of all hydrides at 800°C is basically the same. The Vickers hardness of all embodiments and comparative examples at room temperature measured using a Vickers hardness tester is shown in Table 2, and it can be seen that the hardness of the pellet is closely related to the hydrogen content.

[0112] Table 1 shows the variation of hydrogen content of Examples 3 to 5 and Comparative Example 1 with temperature.

[0113] Room temperature 200℃ 400℃ 800℃ Example 3 1.568 1.515 1.482 1.327 Example 4 1.989 1.602 1.518 1.445 Example 5 2.112 1.711 1.556 1.451 Comparative Example 1 1.86 1.613 1.539 1.447

[0114] Table 2 Vickers hardness of Examples 3 to 5 and Comparative Example 1 at room temperature

[0115] Example 1 Example 2 Example 3 Comparison 1 Room temperature hardness (GPa) 2.8 3.6 3.8 3.3

[0116] The present application is described in detail above in conjunction with the embodiments, but the present application is not limited to the above embodiments, and various changes can be made within the knowledge of ordinary technicians in the field without departing from the purpose of the present application. Any content not described in detail in the present application can adopt the existing technology.

Claims

1. An application of erbium-containing yttrium hydride material in nuclear reactor reactivity control and neutron moderation, characterized in that: In the erbium-containing yttrium hydride material, the combustible poison erbium is doped into yttrium hydride in the form of erbium hydride, including erbium with a mass content of 0.1%-10%, and a hydrogen-yttrium atomic ratio of 1.56-2.

11.

2. A method for preparing erbium-containing yttrium hydride material, characterized in that: The method comprises: Mixing yttrium hydride and erbium hydride powders according to the weight ratio of yttrium and erbium metals to obtain a green body of a mixture of yttrium and erbium hydride; The green body is sintered to obtain an erbium-containing yttrium hydride core block; The sintered erbium-containing yttrium hydride core block is placed in a hydriding furnace for hydrogenation to obtain the erbium-containing yttrium hydride material used in nuclear reactor reactivity control and neutron moderation; Among them, the combustible poison erbium in the erbium-containing yttrium hydride material is doped with yttrium hydride in the form of erbium hydride, including an erbium content of 0.1%-10% by mass, and a hydrogen-yttrium atomic ratio of 1.56-2.

11.

3. The method for preparing erbium-containing yttrium hydride material according to claim 2, characterized in that: The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace for hydrogenation to obtain the erbium-containing yttrium hydride material, which specifically includes: The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace and vacuumed to a temperature not less than 4×10 -4 Pa, heated to 400°C at a heating rate of 10°C / min, slowly introduced hydrogen with a purity of 7N until the hydrogen absorption was saturated, and then cooled to room temperature with the furnace. After the hydrogen absorption was balanced, the erbium-containing yttrium hydride material was obtained.

4. The method for preparing erbium-containing yttrium hydride material according to claim 2, characterized in that: The green body is sintered to obtain the erbium-containing yttrium hydride core block, which specifically includes: The green body is in a vacuum of not less than 4×10 -4 After being kept at 1000°C for 2 hours in a vacuum environment of 1.5 Pa, the furnace was cooled to room temperature to obtain erbium-containing yttrium hydride core blocks.

5. The method for preparing erbium-containing yttrium hydride material according to claim 2, characterized in that: The sintered erbium-containing yttrium hydride core block is placed in a hydrogenation furnace for hydrogenation, and then the method further comprises: The sintered material is polished with sandpaper of 800 mesh or above to obtain erbium-containing yttrium hydride material.

6. The method for preparing erbium-containing yttrium hydride material according to claim 2, characterized in that: The powders of yttrium hydride and erbium hydride are obtained according to the following steps: Using metallic erbium and metallic yttrium as raw materials, placing them in a sample chamber of a hydrogenation furnace, and performing hydrogenation treatment in the sample chamber to obtain yttrium hydride blocks and erbium hydride blocks; The yttrium hydride block and the erbium hydride block are crushed into powder by a hammer mill in a dry inert gas protection environment.

7. The method for preparing erbium-containing yttrium hydride material according to claim 2, characterized in that: The powders of yttrium hydride and erbium hydride are obtained according to the following steps: Using metallic erbium and metallic yttrium as raw materials, smelting in an electric arc furnace according to the weight ratio of yttrium to erbium metal to obtain a yttrium-erbium alloy; The yttrium-erbium alloy is placed in a sample chamber of a hydrogenation furnace, and hydrogenation treatment is performed in the sample chamber to obtain yttrium hydride bulk and erbium hydride bulk; The yttrium hydride block and the erbium hydride block are crushed into powder by a hammer mill in a dry inert gas protection environment.

8. The method for preparing erbium-containing yttrium hydride material according to claim 6 or 7, characterized in that: Performing hydrogenation treatment in the sample chamber to obtain yttrium hydride bulk and erbium hydride bulk specifically includes: At room temperature, evacuate the sample chamber to a vacuum of no less than 4 × 10 -4 Pa, heated to 700°C ~ 800°C at a heating rate of 20°C / min, introduced hydrogen with a purity of 7N until saturated, kept the hydrogen partial pressure and temperature unchanged for 1 hour, cooled to 200°C ~ 300°C at a cooling rate of about 40°C / min, after saturated with hydrogen absorption at a constant temperature, cooled to room temperature with the furnace, and after the hydrogen absorption equilibrium was reached, yttrium hydride block and erbium hydride block were obtained.

9. The method for preparing erbium-containing yttrium hydride material according to claim 6 or 7, characterized in that: The method of using a hammer mill to crush the yttrium hydride block and the erbium hydride block into powder in a dry inert gas protection environment specifically includes: The yttrium hydride and erbium hydride blocks were crushed into 400 mesh powders by a hammer mill in a dry argon protection environment.

10. The method for preparing erbium-containing yttrium hydride material according to claim 7, characterized in that: The smelting in an electric arc furnace to obtain a yttrium-erbium alloy specifically comprises: Before melting, the vacuum was pumped to 4 × 10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

11. A method for preparing erbium-containing yttrium hydride material, characterized in that: The method comprises: Using metallic erbium and metallic yttrium as raw materials, smelting in an electric arc furnace according to the weight ratio of yttrium to erbium metal to obtain a yttrium-erbium alloy; The yttrium-erbium alloy is subjected to hydrogenation treatment to obtain erbium-containing yttrium hydride material used in nuclear reactor reactivity control and neutron moderation; Among them, the combustible poison erbium in the erbium-containing yttrium hydride material is doped with yttrium hydride in the form of erbium hydride, including an erbium content of 0.1%-10% by mass, and a hydrogen-yttrium atomic ratio of 1.56-2.

11.

12. The method for preparing erbium-containing yttrium hydride material according to claim 11, characterized in that: The smelting in an electric arc furnace to obtain a yttrium-erbium alloy specifically comprises: Before melting, the vacuum was pumped to 4 × 10 -4 Pa, and then high-purity argon is filled to 40kPa, the temperature is increased for melting, and then cooled in a water-cooled crucible; the alloy is taken out and cut into small pieces for mixing, and then melted again, and this is repeated 3 times to obtain a uniformly mixed yttrium and erbium alloy.

13. The method for preparing erbium-containing yttrium hydride material according to claim 11, characterized in that: The method of subjecting the yttrium-erbium alloy to hydrogenation treatment to obtain the erbium-containing yttrium hydride material specifically comprises: At a vacuum degree higher than 4×10 -4 After annealing at 850°C and 7N hydrogen for 12 hours, slowly introduce 7N hydrogen within 50 hours until it reaches 100 kPa; keep the pressure stable and cool to 700°C at a rate of -40°C / h; after maintaining stability at 700°C and 100 kPa hydrogen partial pressure, turn off the hydrogen and stop heating, and cool to room temperature with the furnace.

14. The method for preparing erbium-containing yttrium hydride material according to claim 11, characterized in that: The method of subjecting the yttrium-erbium alloy to hydrogenation treatment further comprises: When lathe processing is performed on the samples obtained after hydrogenation, an inert environment is required for dry processing, while non-aqueous coolants are used for cooling during wet processing; finally, sandpaper with a mesh size of 800 or above is used for mechanical polishing.

Citation Information

Patent Citations

  • Rare earth hydrogen storage alloy and preparation method and application thereof