Catalyst and preparation method thereof, and method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol
By introducing specific proportions of Group IIA, Group IB and Group IIB oxides into the catalyst, the problem of long initiation time and easy structure degradation of the catalyst is solved, and the generation selectivity and catalytic performance of 4-methyl-1-pentene are improved. , a more efficient methyl isobutylmethanol dehydration reaction is achieved.
Patent Information
- Application Number
- CN202111262302.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-12-13
- Estimated Expiration
- 2041-10-28
AI Technical Summary
The catalyst for preparing 4-methyl-1-pentene in the prior art has problems such as long initiation time, easy structure degradation, strong reductionism, and easy reaction with the support, which limits its promotion in industrial applications.
A catalyst is provided that comprises 80-99.85 wt% of the main active component, 0.04-9 wt% of the Group IIA oxide, 0.06-8 wt% of the Group IB oxide and 0.05-7.5 wt% of the Group IIB oxide, by specific The proportion of components and preparation method of the catalyst can improve the control of acidity and medium-strong acidic centers, inhibit carbon deposits, and enhance catalytic performance and selectivity.
The high selectivity and stable catalytic performance of the catalyst are achieved, the occurrence of side reactions is reduced, the reaction rate is extended, the channel blockage is slowed, and the generation selectivity of 4-methyl-1-pentene is improved.
Smart Images

Figure BDA0003326221450000161 
Figure BDA0003326221450000172 
Figure BDA0003326221450000181
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alcohol dehydration, and in particular to a method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol. Background Art
[0002] 4-Methyl-1-pentene (abbreviated as 4MP1) is an important branched α-olefin. As an important organic chemical raw material, it has great application prospects. On the one hand, it can be copolymerized with ethylene to prepare high-quality linear low-density polyethylene (LLDPE) comonomers, which are superior to LLDPE prepared with 1-butene or 1-hexene as comonomers in terms of impact resistance, tear resistance, optical properties, etc. On the other hand, it can also be used as a monomer for manufacturing poly-4-methyl-1-pentene (TPX). TPX can be used in the artificial leather industry to make high-performance leather release paper; in addition, it can also be copolymerized with certain high-grade α-olefins to form impact-resistant polymers; in addition, it can also be used to produce chemical products such as methyl isobutyl ketone, 2-isobutyl-6-methylheptene-1, and isoprene. At present, the main methods for preparing 4-methyl-1-pentene (4MP1) are propylene dimerization and methyl isobutyl methanol dehydration, among which propylene dimerization has been applied to actual industrial production.
[0003] PCT / IB2019 / 055898 discloses a catalyst and preparation method for propylene dimerization. The catalyst in the present invention is a mixed metal oxide loaded with an alkali metal or an alkali metal complex, and the mixed metal oxide carrier includes at least one of the first column metal and the third column metal, the fourth column metal or the lanthanide element. The alkali metal is sodium (Na), potassium (K), cesium (Cs) or a complex or mixture thereof. The catalyst may have less than 50wt% of a metal carbonate, and the method uses sodium zirconate loaded with potassium metal or NaK alloy as a catalyst, and the selectivity of the branched aliphatic olefin after 6 hours is 60%; using potassium zirconate loaded with NaK alloy as a catalyst, the ratio of 4-methyl-1-pentene to methylpentene is 93%. However, metallic potassium has strong reducibility and can react with a variety of carriers, thus limiting its further application.
[0004] CN111574317A discloses a synthesis process of 4-methyl-1-pentene, which includes using an alkaline salt loaded with an alkali metal as a catalyst, wherein the alkali metal includes Na, K, and NaK alloy; dimerization of propylene occurs on the basis of dehydration and deoxygenation, and then separation of the mixture is performed using a separation tower. The purity of the 4-methyl-1-pentene obtained by the separation process can reach 99.5%, and the yield can reach 85%. At the same time, α-olefins such as 1-hexene are produced as byproducts, which meets the industrial requirements for the polymerization reaction of 4-methyl-1-pentene. However, the alkali metal catalyst on the carbonate has a relatively long initiation time and will degenerate structurally during use.
[0005] So far, the production chain of 4-methyl-1-pentene is still some distance away from achieving industrialization, so it is urgent to explore new methods and key technologies for producing 4-methyl-1-pentene. Summary of the invention
[0006] The purpose of the present invention is to overcome the problems of long initiation time, easy structural degradation, strong reducibility, easy reaction with a carrier, etc. of the catalyst for preparing 4-methyl-1-pentene in the prior art, and to provide a catalyst and a preparation method thereof and a method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol.
[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a catalyst, which comprises, based on the total amount of the catalyst, 80-99.85wt% of a main active component, 0.04-9wt% of a Group IIA oxide, 0.06-8wt% of a Group IIB oxide and 0.05-7.5wt% of a Group IIB oxide; the main active component is selected from at least one of a Group IVB oxide, a Group IIIA oxide and a Group IVA oxide.
[0008] The second aspect of the present invention provides a method for preparing a catalyst, wherein the method comprises: mixing a main active component source, a group IIA source, a group IB source and a group IIB source in a solvent at a weight ratio of 1:0.0001-0.2:0.0001-0.2:0.0005-0.2 to obtain a mixed solution; then contacting the mixed solution with a precipitant to perform a co-precipitation reaction, and then aging the obtained reaction product; then calcining the product obtained by aging; wherein the main active component source is selected from at least one of a group IVB source, a group IIIA source and a group IVA source.
[0009] The third aspect of the present invention provides a catalyst prepared according to the method described in the second aspect.
[0010] The fourth aspect of the present invention provides a method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol, the method comprising: in the presence or absence of a carrier gas, contacting methyl isobutyl carbinol with the catalyst described in the first aspect or the third aspect in a reactor to carry out a dehydration reaction.
[0011] Through the above technical scheme, the catalyst provided by the present invention has high catalytic activity when used for the dehydration reaction of methyl isobutyl carbinol, and has higher selectivity for generating 4-methyl-1-pentene (α-olefin); after long-term life assessment, the catalyst of the present invention has stable catalytic performance, accelerates the reaction rate, reduces carbon deposition, and alleviates pore blockage. DETAILED DESCRIPTION
[0012] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0013] As mentioned above, the first aspect of the present invention provides a catalyst, which, based on the total amount of the catalyst, comprises: 80-99.85wt% of a main active component, 0.04-9wt% of a Group IIA oxide, 0.06-8wt% of a Group IIB oxide and 0.05-7.5wt% of a Group IIB oxide; the main active component is selected from at least one of a Group IVB oxide, a Group IIIA oxide and a Group IVA oxide.
[0014] The inventors of the present invention have found that by introducing a specific amount of secondary active components (IIA group oxides, IIB group oxides and IIB group oxides) into the main component, the acidity and the amount of medium-strong acid centers of the catalyst can be controlled within a certain range, and the carbon deposition phenomenon of the catalyst in the dehydration reaction of methyl isobutyl carbinol can be suppressed, the catalytic performance of the catalyst can be improved, the selectivity of 4-methyl-1-pentene can be increased, and the occurrence of side reactions (cyclization, dehydrogenation or hydrogenation) can be suppressed, thereby promoting the efficient dehydration reaction of methyl isobutyl carbinol.
[0015] According to the present invention, under preferred conditions, based on the total amount of the catalyst, the catalyst comprises: 90-99.65wt% of the main active component, 0.08-4.5wt% of the Group IIA oxide, 0.15-3wt% of the Group IIB oxide and 0.12-2.8wt% of the Group IIB oxide; under the above preferred conditions, the content of the acidic and medium-strong acidic centers in the catalyst can be further optimized, thereby improving the selectivity of the catalyst for the product 4-methyl-1-pentene (α-olefin).
[0016] According to the present invention, in order to further improve the selectivity of 4-methyl-1-pentene, under preferred conditions, the weight ratio of the main active component to the secondary active component is 10-100:1, preferably 15-75:1; further preferably, in the secondary active component, the weight ratio of the Group IIA oxide, the Group IB oxide and the Group IIB oxide is 0.1-20:0.1-25:1, preferably 0.25-18:0.3-8:1, and more preferably 0.5-9:0.8-4:1.
[0017] In some preferred embodiments of the present invention, based on the total weight of the catalyst, the content of the main active component relative to every 100 parts by weight of the catalyst is more than 80 parts by weight, preferably 90-99.65 parts by weight, for example, it can be 90 parts by weight, 90.5 parts by weight, 91 parts by weight, 91.5 parts by weight, 92 parts by weight, 92.5 parts by weight, 93 parts by weight, 93.5 parts by weight, 94 parts by weight, 94.5 parts by weight, 95 parts by weight, 95.5 parts by weight, 96 parts by weight, 96.5 parts by weight, 97 parts by weight, 97.5 parts by weight, 98 parts by weight, 98.5 parts by weight, 99 parts by weight, 99.65 parts by weight, or any value in the range composed of any two of the above numerical values.
[0018] In some preferred embodiments of the present invention, based on the total weight of the catalyst, the content of the Group IIA oxide is 0.04-9 parts by weight, preferably 0.08-4.5 parts by weight, per 100 parts by weight of the catalyst. For example, it can be 0.08 parts by weight, 0.1 parts by weight, 0.5 parts by weight, 1 parts by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, or any value in the range consisting of any two of the above values.
[0019] In some preferred embodiments of the present invention, based on the total amount of the catalyst, the content of the Group IB oxide can be 0.06-8 parts by weight, preferably 0.15-3 parts by weight, for example, 0.12 parts by weight, 0.2 parts by weight, 0.5 parts by weight, 0.75 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 2.8 parts by weight, 3 parts by weight, or any value in the range consisting of any two of the above values, relative to every 100 parts by weight of the catalyst.
[0020] In some preferred embodiments of the present invention, based on the total amount of the catalyst, the content of the Group IIB oxide can be 0.05-7.5 parts by weight, preferably 0.12-2.8 parts by weight, for example, 0.12 parts by weight, 0.2 parts by weight, 0.5 parts by weight, 0.75 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 2.8 parts by weight, or any value in the range consisting of any two of the above values.
[0021] In the present invention, under preferred conditions, the main active component is selected from at least one of zirconium dioxide, aluminum oxide, titanium dioxide and silicon dioxide; more preferably zirconium dioxide.
[0022] In the present invention, the introduction of secondary active components can improve the pore diffusivity and pore structure stability of the catalyst, reduce unwanted side reactions, and better exert the performance of the catalyst; under preferred conditions, the IIA group oxide is selected from at least one of magnesium oxide, calcium oxide, strontium oxide and barium oxide; more preferably calcium oxide and / or magnesium oxide.
[0023] In the present invention, preferably, the Group IB oxide is selected from copper oxide and / or silver oxide; more preferably copper oxide or silver oxide.
[0024] In the present invention, under preferred conditions, the Group IIB oxide is selected from zinc oxide or chromium oxide, and zinc oxide is most preferred.
[0025] In the present invention, in order to improve the selectivity of the catalyst for α-olefins, the catalyst should also have a specific surface area and pore volume. Under preferred conditions, the specific surface area of the catalyst is 75-165m 2 ·g -1 ; Further preferably, the pore volume of the catalyst is 0.05-0.6 mL·g -1 ; More preferably, the total pore volume of the catalyst has a pore volume content of 70-90% with a pore diameter in the range of 1.7-2.6 nm, for example, 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90% or any value in the range consisting of any two of the above values.
[0026] In the present invention, the specific surface area, pore volume and the proportion of pores with different pore radii of the catalyst are measured by a nitrogen adsorption-desorption method, for details, refer to GB / T6609.35-2009.
[0027] According to the present invention, under preferred conditions, the ammonia adsorption capacity of the catalyst is 0.18-0.38 mmol·g -1 , preferably 0.18-0.21 mmol g -1 Further preferably, the content of the medium-strong acid center is less than 45% based on the total amount of the medium-strong acid center and the weak acid center of the catalyst; the amount of the medium-strong acid center of the catalyst refers to the NH3-TPD test method of the catalyst at 250-450°C. Desorption amount .
[0028] The present invention has no particular limitation on the composite mode of the main component and the IIA group oxide, IB group oxide and IIB group oxide. The IIA group oxide, IB group oxide and IIB group oxide can be supported on the main component or dispersed in the main component; in the present invention, they are preferably dispersed in the main component. In the present invention, the dispersion or support of the IIA group oxide, IB group oxide and IIB group oxide has little effect on the microstructure of the catalyst, so the obtained catalyst has a pore structure similar to that of the main component.
[0029] In the present invention, the catalyst can be prepared by an existing method.
[0030] In a preferred embodiment of the present invention, the second aspect of the present invention provides a method for preparing a catalyst, wherein the method comprises: mixing a main active component source, a group IIA source, a group IB source and a group IIB source in a solvent at a weight ratio of 1: 0.0001-0.2: 0.0001-0.2: 0.0005-0.2 to obtain a mixed solution; then contacting the mixed solution with a precipitant for a co-precipitation reaction, and aging the obtained reaction product; then calcining the aging product; wherein the main active component source is selected from at least one of a group IVB source, a group IIIA source and a group IVA source.
[0031] In the above catalyst preparation method, those skilled in the art can understand that: if the main active component source already contains the required amount of Group IIA source, Group IB source and Group IIB source, then only this raw material (main active component source) needs to be used for molding; if the raw material providing the main active component source does not contain Group IIA source, Group IB source and Group IIB source or the content of the elements is low (insufficient), then the required elements can be additionally introduced.
[0032] In the present invention, since the Group IIA source, Group IB source and Group IIB source are introduced during the preparation process of the main active component, the Group IIA oxide, Group IB oxide and Group IIB oxide are mainly present in the bulk phase of the main active component, that is, dispersed in the main active component.
[0033] According to the present invention, under preferred conditions, the IVB group source is a compound containing an IVB group element, preferably selected from a zirconium source and / or a titanium source; preferably, the zirconium source is selected from at least one of zirconium oxychloride, zirconium nitrate, zirconium oxynitrate and zirconium oxy sulfate, more preferably zirconium oxychloride; the titanium source is preferably selected from titanium dioxide; preferably, the IVA group source is a compound containing an IVA group element, preferably selected from a silicon source; preferably, the silicon source is selected from an aqueous sodium silicate solution; the IIIA group source is a compound containing a IIIA group element, preferably selected from an aluminum source; preferably, the aluminum source is selected from pseudo-boehmite.
[0034] According to the present invention, under preferred conditions, the precipitant is selected from at least one of ammonia water, urea, sodium hydroxide and sodium carbonate, preferably ammonia water.
[0035] In the present invention, the Group IIA source exists in the form of a solution of a Group IIA salt (referred to as solution A), and the Group IIA salt is selected from at least one of Group IIA nitrates, Group IIA formates, Group IIA oxalates and Group IIA lactates; preferably, Group IIA nitrates; further preferably, the Group IIA nitrates are selected from at least one of magnesium nitrate, calcium nitrate, strontium nitrate and barium nitrate; the solvent in the solution is selected from water and / or ethanol, preferably water.
[0036] In the present invention, the Group IB source exists in the form of a solution of a Group IB salt (referred to as solution B), and the Group IB salt is selected from at least one of Group IB nitrates, Group IB formates, Group IB oxalates and Group IB lactates; preferably, Group IB nitrates; further preferably, the Group IB nitrates are selected from copper nitrate and / or silver nitrate; the solvent in the solution is selected from water and / or ethanol, preferably water.
[0037] In the present invention, the Group IIB source is present in the form of a Group IIB salt solution (referred to as Solution C), preferably an aqueous solution of a zinc salt; the zinc salt is selected from at least one of zinc nitrate, zinc formate, zinc oxalate and zinc lactate; preferably zinc nitrate; the solvent in the solution is selected from water and / or ethanol, preferably water.
[0038] In the present invention, solution A, solution B and solution C can be mixed and then added to the system containing the main active component source, or they can be added separately to the system containing the main active component source; when they are added separately to the system containing the main active component source, there is no special limitation on the order of adding the solution A, the solution B and the solution C.
[0039] According to the present invention, under preferred conditions, the aging conditions include: a temperature of 65-95°C, for example, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, or any value in the range formed by any two of the above values; preferably, the aging time is 0.5-9h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, or any value in the range formed by any two of the above values.
[0040] According to the present invention, under preferred conditions, the method further comprises: centrifuging, washing and drying the product obtained by aging; wherein the drying time can be reasonably selected according to the drying temperature, the amount of material and the type of drying equipment, so that the moisture content of the dried material does not affect the subsequent roasting. Under preferred conditions, the drying temperature is 70-140°C, for example, it can be 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C or any value in the range of any two of the above values; the drying time is 4-19h; for example, it can be 4h, 4.5h, 5h , 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, 12.5h, 13h, 14h, 14.5h, 15h, 15.5h, 16h, 16.5h, 17h, 17.5h, 18h, 18.5h, 19h or any value in the range of any two of the above values.
[0041] According to the present invention, roasting can remove the crystal water in the salt and decompose the salt to generate oxides. Under preferred conditions, the roasting conditions include: a temperature of 500-1000°C and a time of 2-18h; illustratively, the roasting temperature can be 500°C, 525°C, 550°C, 600°C, 625°C, 650°C, 675°C, 700°C, 725°C, 750°C, 800°C, 825°C, 850°C, 900°C, 925°C, 950°C, 1000°C or a range consisting of any two of the above values. the calcination time can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, 12.5h, 13h, 13.5h, 14h, 14.5h, 15h, 15.5h, 16h, 16.5h, 17h, 17.5h, 18h or any value in the range of any two of the above values.
[0042] The third aspect of the present invention provides a catalyst prepared according to the method described in the second aspect.
[0043] Under preferred conditions, the catalyst comprises, based on the total amount of the catalyst, 80-99.85wt% of a main active component, 0.04-9wt% of a Group IIA oxide, 0.06-8wt% of a Group IIB oxide and 0.05-7.5wt% of a Group IIB oxide; preferably, the weight ratio of the Group IIA oxide, the Group IB oxide and the Group IIB oxide is 0.1-20:0.1-25:1; the main active component is selected from at least one of a Group IVB oxide, a Group IIIA oxide and a Group IVA oxide;
[0044] Preferably, the specific surface area of the catalyst is 75-165m 2 ·g -1 The pore volume of the catalyst is 0.05-0.60 mL·g -1 Further preferably, based on the total pore volume of the catalyst, the content of pore volume with pore diameter in the range of 1.7-2.6 nm is 70-90%.
[0045] Preferably, the ammonia adsorption capacity of the catalyst is 0.18-0.38 mmol·g -1 ; Based on the total amount of the medium-strong acid centers and weak acid centers of the catalyst, the content of the medium-strong acid centers is less than 45%; in the present invention, the total amount of the medium-strong acid centers and weak acid centers of the catalyst is the ammonia adsorption amount of the catalyst.
[0046] The fourth aspect of the present invention provides a method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol, wherein the method comprises: contacting methyl isobutyl carbinol with the catalyst described in the first aspect or the third aspect in a reactor in the presence or absence of a carrier gas to carry out a dehydration reaction;
[0047] Preferably, the conditions of the dehydration reaction include: temperature of 240-360°C, preferably 260-340°C; pressure of 0.08-0.24 MPa; liquid phase volume space velocity of 0.15-0.75 h -1 , preferably 0.2-0.5h -1 ;
[0048] Preferably, when a carrier gas is present, the flow rate of the carrier gas is 15-45 mL min -1 , preferably 15-40 mL min -1 .
[0049] In the present invention, the type of the reactor can be selected according to actual needs, for example, it can be a fixed bed reactor, a high-pressure stirred tank reactor or a tubular reactor; preferably a fixed bed reactor.
[0050] In the following examples, the elemental composition of the catalyst was analyzed by ICP-MS; testing instrument: VISTA Pro CCD spectrometer (Varian);
[0051] The specific surface area, pore volume and the proportion of pore volume with different pore diameters of the catalyst were measured by nitrogen adsorption-desorption method (BET). For the specific method, please refer to GB / T6609.35-2009; Instrument name: Automatic Micropore & Chemisorption Analyzer; Instrument model: ASAP2420, MICROMERITICS (Micro Instruments, Inc., USA);
[0052] The ammonia adsorption of the catalyst was tested by NH3-TPD, the desorption temperature was 120-600℃, and the test conditions were: accurately weigh about 0.1g of sample into the sample tube, and then purged with He gas at 10℃min -1 Raise to 600℃, stay for 1h, then lower to 120℃, change the gas to 10% NH3-He mixed gas, adsorb for 60min, then change to He gas purge for 1h, start counting after the baseline is stable, at 10℃min -1 Raise to 600℃, maintain for 30min, stop recording, and the experiment is completed. Integrate the peak area to calculate the NH3 desorption amount (the basic position of the catalyst); Test instrument: Automated Catalyst Characterization System; Instrument model: Autochem 2920, a product of MICROMERITICS, USA;
[0053] The amount of medium-strong acidic centers of the catalyst is tested in the same way as the amount of ammonia adsorption of the catalyst, except that the desorption temperature is 250-450°C;
[0054] The carbon deposit of the catalyst was tested by O2-TPO. The test conditions were as follows: accurately weigh 0.2g of sample, use argon with a flow rate of 40mL / min as carrier gas, pretreat the sample at 150℃ for 60min, cool to 100℃, and use a mixed gas of oxygen and argon with a flow rate of 40mL / min (oxygen volume fraction is 20%) as analytical gas. The temperature was programmed to 900℃ at a rate of 10℃ / min for programmed temperature oxidation, and the signals of gases such as CO2 and CO were detected during the programmed temperature process. Test instrument: fully automatic programmed temperature chemical adsorption instrument; instrument model: AutoChem Ⅱ 2920, a product of Micromeritics, USA.
[0055] Example 1
[0056] Dissolve 369 g zirconium oxynitrate, 9.13 g calcium nitrate tetrahydrate, 1.97 g copper nitrate trihydrate, and 4.32 g zinc nitrate hexahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.53 mol L -1 , Ca 2+ The concentration is 0.013 mol L -1 , Cu 2+ The concentration is 0.003 mol L -1 、Zn 2+ The concentration is 0.005 mol L -1 A mixed solution of: in a water bath at 85°C with vigorous stirring, adding an aqueous ammonia solution (25 wt%) dropwise to adjust the pH to 9.9 to obtain a precipitate system; the precipitate system is allowed to stand in a beaker for 2.5 h; then centrifuged, and the obtained precipitate is washed with deionized water to a pH of 6.5, followed by drying at 70°C for 2 h and then at 130°C for 2 h; finally, the dried product is calcined in a muffle furnace at 500°C for 2 h to obtain a sample ZrO2 / CaO / CuO / ZnO, recorded as catalyst A-1, and the test results are shown in Tables 1 and 2.
[0057] Example 2
[0058] 220.74g of pseudo-boehmite, 27.48g of calcium nitrate tetrahydrate, 3.71g of silver nitrate and 1.19g of zinc nitrate hexahydrate were dissolved in 3L of deionized water; in a 65°C water bath with vigorous stirring, an aqueous ammonia solution (25wt%) was added dropwise to adjust the pH to 10 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.4h; then centrifuged and the obtained precipitate was washed with deionized water to pH=6.5, then dried at 80°C for 2h and then dried at 120°C for 2h; finally, the dried product was calcined in a muffle furnace at 900°C for 2h to obtain a sample Al2O3 / CaO / Ag2O / ZnO, denoted as catalyst A-2, and the test results are shown in Tables 1 and 2.
[0059] Example 3
[0060] 127.79g titanium dioxide, 0.54g calcium nitrate tetrahydrate, 4.50g silver nitrate and 6.54g zinc nitrate hexahydrate were dissolved in 3L deionized water; in a 95°C water bath with vigorous stirring, an aqueous ammonia solution (25wt%) was added dropwise to adjust the pH to 9.9 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.4h; then centrifuged and the obtained precipitate was washed with deionized water to pH=6.5, then dried at 750°C for 2h and then dried at 135°C for 2h; finally, the dried product was calcined in a muffle furnace at 900°C for 2h to obtain a sample TiO2 / CaO / Ag2O / ZnO, denoted as catalyst A-3, and the test results are shown in Tables 1 and 2.
[0061] Example 4
[0062] 195.2g sodium silicate, 9.37g calcium nitrate tetrahydrate, 1.45g copper nitrate trihydrate and 0.93g zinc nitrate hexahydrate were dissolved in 3L deionized water; in a 70°C water bath with vigorous stirring, an aqueous ammonia solution (25wt%) was added dropwise to adjust the pH to 10 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.5h; then centrifuged and the obtained precipitate was washed with deionized water to pH=6.5, then dried at 85°C for 2h and then dried at 140°C for 2h; finally, the dried product was calcined in a muffle furnace at 550°C for 2h to obtain a sample SiO2 / CaO / CuO / ZnO, denoted as catalyst A-4, and the test results are shown in Tables 1 and 2.
[0063] Example 5
[0064] Dissolve 369 g zirconium oxynitrate, 0.66 g calcium nitrate tetrahydrate, 8.67 g silver nitrate, and 2.38 g zinc nitrate hexahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.53 mol L -1 , Ca 2+ The concentration is 0.001 mol L -1 、Ag + The concentration is 0.017 mol L -1 、Zn 2+ The concentration is 0.003 mol L -1A mixed solution of: in a 65°C water bath with vigorous stirring, adding an aqueous ammonia solution (25wt%) dropwise to adjust the pH to 10.1 to obtain a precipitate system; the precipitate system is allowed to stand in a beaker for 2.5h; then centrifuged, and the obtained precipitate is washed with deionized water to a pH of 6.5, followed by drying at 85°C for 2h and then at 135°C for 2h; finally, the dried product is calcined in a muffle furnace at 700°C for 2h to obtain a sample ZrO2 / CaO / Ag2O / ZnO, recorded as catalyst A-5, and the test results are shown in Tables 1 and 2.
[0065] Example 6
[0066] Dissolve 369 g zirconium oxynitrate, 37.4 g calcium nitrate tetrahydrate, 0.43 g silver nitrate, and 6.05 g cadmium nitrate tetrahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.54 mol L -1 , Ca 2+ The concentration is 0.053 mol L -1 、Ag + The concentration is 0.00088 mol L -1 、Cd 2+ The concentration is 0.006 mol L -1 A mixed solution of: in a 60°C water bath with vigorous stirring, adding an aqueous ammonia solution (25wt%) dropwise to adjust the pH to 9.8 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.4h; then centrifuged, and the obtained precipitate was washed with deionized water to pH=6.5, followed by drying at 90°C for 2h and then at 125°C for 2h; finally, the dried product was calcined in a muffle furnace at 650°C for 2h to obtain a sample ZrO2 / CaO / Ag2O / CdO, recorded as catalyst A-6, and the test results are shown in Tables 1 and 2.
[0067] Example 7
[0068] Dissolve 369 g zirconium oxynitrate, 18.81 g magnesium nitrate hexahydrate, 12.46 g copper nitrate trihydrate, and 0.86 g zinc nitrate hexahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.54 mol L -1 Mg 2+ The concentration is 0.024 mol L -1 , Cu 2+ The concentration is 0.022 mol L -1 、Zn 2+ The concentration is 0.001 mol L -1A mixed solution of: in a 75°C water bath with vigorous stirring, adding an aqueous ammonia solution (25 wt%) dropwise to adjust the pH to 10.1 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.7 h; then centrifuged, and the obtained precipitate was washed with deionized water to a pH of 6.5, followed by drying at 70°C for 2 h and then at 135°C for 2 h; finally, the dried product was calcined in a muffle furnace at 800°C for 2 h to obtain a sample ZrO2 / MgO / CuO / ZnO, recorded as catalyst A-7, and the test results are shown in Tables 1 and 2.
[0069] Example 8
[0070] Dissolve 369 g zirconium oxynitrate, 0.13 g barium nitrate, 51.82 g copper nitrate trihydrate, and 0.36 g zinc nitrate hexahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.54 mol L -1 , Ba 2+ The concentration is 0.00017 mol L -1 , Cu 2+ The concentration is 0.066 mol L -1 、Zn 2+ The concentration is 0.0004 mol L -1 A mixed solution of: in a water bath at 85°C with vigorous stirring, adding an aqueous ammonia solution (25 wt%) dropwise to adjust the pH to 10 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.8 h; then centrifuged, and the obtained precipitate was washed with deionized water to a pH of 6.5, followed by drying at 85°C for 2 h and then at 125°C for 2 h; finally, the dried product was calcined in a muffle furnace at 850°C for 2 h to obtain a sample ZrO2 / BaO / CuO / ZnO, recorded as catalyst A-8, and the test results are shown in Tables 1 and 2.
[0071] Example 9
[0072] Dissolve 369 g zirconium oxynitrate, 36.24 g strontium nitrate, 0.17 g silver nitrate, and 54.05 g zinc nitrate hexahydrate in 3 L deionized water to prepare a zirconium concentration of 0.54 mol L -1 , Sr 2+ The concentration is 0.057 mol L -1 、Ag + The concentration is 0.00034 mol L -1 、Zn 2+ The concentration is 0.0606 mol L -1A mixed solution of: in a 90°C water bath with vigorous stirring, adding an aqueous ammonia solution (25wt%) dropwise to adjust the pH to 10.1 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.3h; then centrifuged, and the obtained precipitate was washed with deionized water to pH=6.5, followed by drying at 90°C for 2h and then at 130°C for 2h; finally, the dried product was calcined in a muffle furnace at 650°C for 2h to obtain a sample ZrO2 / SrO / Ag2O / ZnO, recorded as catalyst A-9, and the test results are shown in Tables 1 and 2.
[0073] Comparative Example 1
[0074] The catalyst was prepared according to the method of Example 1, except that zirconium oxide powder was used as the main active component source and the calcination temperature was 500°C during the preparation of the catalyst. Sample ZrO2 (powder) / CaO / CuO / ZnO was obtained, which was recorded as catalyst D-1. The test results are shown in Tables 1 and 2.
[0075] Comparative Example 2
[0076] The catalyst was prepared according to the method of Example 1, except that zirconium oxide powder was used as the main active component source, and the calcination temperature during the preparation of the catalyst was 1200°C. After cooling, a sample ZrO2 (powder) / CaO / CuO / ZnO was obtained, which was recorded as catalyst D-2. The test results are shown in Tables 1 and 2.
[0077] Comparative Example 3
[0078] Dissolve 369 g zirconium oxynitrate, 9.13 g calcium nitrate tetrahydrate, and 1.97 g copper nitrate trihydrate in 3 L of deionized water to prepare a zirconium concentration of 0.53 mol L -1 , Ca 2+ The concentration is 0.013 mol L -1 , Cu 2+ The concentration is 0.003 mol L -1 A mixed solution of: in a water bath at 85°C with vigorous stirring, adding an aqueous ammonia solution (25wt%) dropwise to adjust the pH to 9.9 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.5h; then centrifuged, and the obtained precipitate was washed with deionized water to a pH of 6.5, followed by drying at 70°C for 2h and then at 130°C for 2h; finally, the dried product was calcined in a muffle furnace at 500°C for 2h to obtain a sample ZrO2 / CaO / CuO, recorded as catalyst D-3, and the test results are shown in Tables 1 and 2.
[0079] Comparative Example 4
[0080] The catalyst was prepared according to the method of Example 1, except that 72 g of zinc nitrate hexahydrate was weighed and dissolved in 3 L of deionized water to obtain a sample ZrO2 / CaO / CuO / ZnO, recorded as catalyst D-4. The test results are shown in Tables 1 and 2.
[0081] Comparative Example 5
[0082] Dissolve 369 g zirconium oxynitrate, 9.13 g calcium nitrate tetrahydrate, and 4.32 g zinc nitrate hexahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.53 mol L -1 , Ca 2+ The concentration is 0.013 mol L -1 、Zn 2+ The concentration is 0.005 mol L -1 a mixed solution; in a water bath at 85°C with vigorous stirring, adding an aqueous ammonia solution (25wt%) dropwise to adjust the pH to 9.9 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.5h; then centrifuged, and the obtained precipitate was washed with deionized water to pH=6.5, followed by drying at 70°C for 2h and then at 130°C for 2h; finally, the dried product was calcined in a muffle furnace at 500°C for 2h to obtain a sample ZrO2 / CaO / ZnO, recorded as catalyst D-5, and the test results are shown in Tables 1 and 2.
[0083] Comparative Example 6
[0084] The catalyst was prepared according to the method of Example 1, except that 72 g of copper nitrate trihydrate was weighed and dissolved in 3 L of deionized water to obtain a sample ZrO2 / CaO / CuO / ZnO, recorded as catalyst D-6. The test results are shown in Tables 1 and 2.
[0085] Comparative Example 7
[0086] Dissolve 369 g zirconium oxynitrate, 1.97 g copper nitrate trihydrate, and 4.32 g zinc nitrate hexahydrate in 3 L of deionized water to prepare a zirconium concentration of 0.53 mol L -1 , Cu 2+ The concentration is 0.003 mol L -1 、Zn 2+ The concentration is 0.005 mol L -1a mixed solution; in a water bath at 85°C with vigorous stirring, adding an aqueous ammonia solution (25 wt%) dropwise to adjust the pH to 9.9 to obtain a precipitate system; the precipitate system was allowed to stand in a beaker for 2.5 h; then centrifuged, and the obtained precipitate was washed with deionized water to a pH of 6.5, followed by drying at 70°C for 2 h and then at 130°C for 2 h; finally, the dried product was calcined in a muffle furnace at 500°C for 2 h to obtain a sample ZrO2 / CuO / ZnO, recorded as catalyst D-7, and the test results are shown in Tables 1 and 2.
[0087] Comparative Example 8
[0088] The catalyst was prepared according to the method of Example 1, except that 124 g of calcium nitrate tetrahydrate was weighed and dissolved in 3 L of deionized water to obtain a sample of ZrO2 / CaO / CuO / ZnO, recorded as catalyst D-8. The test results are shown in Tables 1 and 2.
[0089] Comparative Example 9
[0090] The catalyst was prepared according to the method of Example 1, except that the calcination temperature during the preparation of the catalyst was 250°C. The sample ZrO2 / CaO / CuO / ZnO (250°C) was obtained, which was recorded as catalyst D-9. The test results are shown in Tables 1 and 2.
[0091] Comparative Example 10
[0092] The catalyst was prepared according to the method of Example 1, except that the calcination temperature was 1000°C during the preparation of the catalyst. Sample ZrO2 / CaO / CuO / ZnO (1000°C) was obtained, which was recorded as catalyst D-10. The test results are shown in Tables 1 and 2.
[0093] Table 1
[0094]
[0095]
[0096] Note: * The content refers to the weight of Group IIA oxide relative to 100 g of catalyst;
[0097] ** Content refers to the weight of Group IB oxide relative to 100g of catalyst;
[0098] *** The content refers to the weight of the Group IIB oxide relative to 100 g of the catalyst.
[0099] Table 2
[0100]
[0101] Note: * Medium-strong acid refers to the percentage of the medium-strong acid center of the catalyst based on the total amount of the weak acid center and the medium-strong acid center of the catalyst;
[0102] * 1.7-2.6 nm refers to the percentage of pore volume with pore diameters in the range of 1.7-2.6 nm to the total pore volume of the catalyst.
[0103] Test Example 1
[0104] This test example is used to illustrate the method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol (MIBC).
[0105] Weigh 50 mL of catalyst into a fixed bed reactor, preheat with nitrogen at 300 °C for 1 h, and use a metering pump to deliver methyl isobutyl carbinol into the reaction system. The liquid phase volume space velocity of methyl isobutyl carbinol is 0.3 h -1 The dehydration reaction was carried out in the reactor at a temperature of 310°C and a pressure of 0.1 MPa. After the reaction stabilized (i.e., after 500 hours of reaction), the reaction liquid was sampled and analyzed. The analysis results are listed in Table 2.
[0106] The sampling and analysis method is gas chromatography, which is calibrated by preparing correction factors of standard samples;
[0107] The conversion rate and selectivity were calculated based on the molar content of each component in the reaction solution (methyl isobutyl carbinol is abbreviated as MIBC, 4-methyl-1-pentene is 4MP1, 4-methyl-2-pentene is 4MP2, and methyl isobutyl ketone is MIBK).
[0108] MIBC conversion rate = 100% - n1 / [(n1+n2+n3+n4)+2×n5]×100%
[0109] 4MP1 selectivity = n2 / [(n2+n3+n4)+2×n5]×100%
[0110] 4MP2 selectivity = n3 / [(n2+n3+n4)+2×n5]×100%
[0111] Wherein, n1 is the molar content of MIBC in the reaction solution; n2 is the molar content of 4MP1 in the reaction solution; n3 is the molar content of 4MP2 in the reaction solution; n4 is the molar content of MIBK in the reaction solution; and n5 is the molar content of oligomers in the reaction solution.
[0112] 4MP1 ratio = 4MP1 / (4MP2+4MP1)×100%
[0113] The 4MP1 proportion is the ratio of 4MP1 selectivity to the sum of 4MP1 and 4MP2 selectivities, that is, the ratio of α-olefin to the sum of α-olefin and β-olefin, indicating that the product generated by the reaction has more α-olefin, that is, the selectivity of α-olefin is high.
[0114] Table 3
[0115]
[0116]
[0117] As can be seen from Table 3, after 1800h of catalytic reaction, the conversion rate and selectivity of composite catalysts A-1 to A-9 did not change significantly compared with 500h, the conversion rate of MIBC decreased by no more than 1.5%, and the proportion of 4MP1 decreased by no more than 1%, while the conversion rate and selectivity of comparative catalysts D-1 to D-10 decreased significantly after 1800h of catalytic reaction compared with 500h, the conversion rate decreased by 20-40%, and the proportion of 4MP1 decreased by 22%-44%. In addition, after 1800h of catalytic reaction, the carbon deposits of the catalysts prepared in the embodiments of the present invention were all less than 2wt%; the carbon deposits of the catalysts prepared in the comparative examples reached 3.5-7.6wt%, which shows that the catalysts prepared in the embodiments of the present invention have a longer service life.
[0118] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing 4-methyl-1-pentene by dehydrating methyl isobutyl carbinol, characterized in that: The method comprises: contacting methyl isobutyl carbinol with a catalyst in a reactor to carry out a dehydration reaction in the presence or absence of a carrier gas; Based on the total amount of the catalyst, the catalyst comprises: 80-99.85 wt% of a main active component, 0.04-9 wt% of a Group IIA oxide, 0.06-8 wt% of a Group IIB oxide, and 0.05-7.5 wt% of a Group IIB oxide; The main active component is selected from at least one of Group IVB oxides, Group IIIA oxides, and Group IVA oxides.
2. The method according to claim 1, wherein: Based on the total amount of the catalyst, the catalyst comprises: 90-99.65 wt% of a main active component, 0.08-4.5 wt% of a Group IIA oxide, 0.15-3 wt% of a Group IIB oxide and 0.12-2.8 wt% of a Group IIB oxide.
3. The method according to claim 1 or 2, wherein: The weight ratio of the Group IIA oxide, the Group IB oxide and the Group IIB oxide is 0.1-20:0.1-25:
1.
4. The method according to claim 1 or 2, wherein: The weight ratio of the Group IIA oxide, the Group IB oxide and the Group IIB oxide is 0.5-9:0.8-4:
1.
5. The method according to claim 1 or 2, wherein: The main active component is selected from at least one of zirconium dioxide, aluminum oxide, titanium dioxide and silicon dioxide; and / or, the Group IIA oxide is at least one selected from magnesium oxide, calcium oxide, strontium oxide and barium oxide; and / or, the Group IB oxide is selected from copper oxide and / or silver oxide; And / or, the Group IIB oxide is selected from zinc oxide.
6. The method according to claim 1 or 2, wherein: The specific surface area of the catalyst is 75-165m 2 ·g -1 ; And / or, the pore volume of the catalyst is 0.05-0.6 mL·g -1 ; And / or, based on the total pore volume of the catalyst, the content of pore volume with pore diameters in the range of 1.7-2.6 nm is 70-90%.
7. The method according to claim 1 or 2, wherein: The ammonia adsorption capacity of the catalyst is 0.18-0.38 mmol·g -1 ; And / or, based on the total amount of the medium-strong acid centers and the weak acid centers of the catalyst, the content of the medium-strong acid centers is less than 45%.
8. The method according to claim 1 or 2, wherein: The preparation method of the catalyst comprises: mixing a main active component source, a group IIA source, a group IB source and a group IIB source in a solvent at a weight ratio of 1:0.0001-0.2:0.0001-0.2:0.0005-0.2 to obtain a mixed solution; then contacting the mixed solution with a precipitant to perform a coprecipitation reaction, and then aging the obtained reaction product; and then roasting the aged product; Wherein, the main active component source is selected from at least one of a group IVB source, a group IIIA source and a group IVA source.
9. The method according to claim 8, wherein: The IVB group source is a compound containing an IVB group element; and / or, the Group IVA source is a compound containing Group IVA elements; and / or, the Group IIIA source is a compound containing Group IIIA elements; And / or, the precipitant is selected from at least one of ammonia water, urea, sodium hydroxide and sodium carbonate.
10. The method according to claim 9, wherein: The Group IVB source is selected from a zirconium source and / or a titanium source; and / or, the Group IVA source is a compound containing Group IVA elements selected from a silicon source; And / or, the Group IIIA source is a compound containing Group IIIA elements selected from aluminum sources.
11. The method according to claim 10, wherein: The zirconium source is selected from at least one of zirconium oxychloride, zirconium nitrate, zirconyl nitrate and zirconyl sulfate; And / or, the titanium source is selected from titanium dioxide; And / or, the aluminum source is selected from pseudo-boehmite; And / or, the silicon source is selected from a sodium silicate aqueous solution; And / or, the precipitant is selected from aqueous ammonia.
12. The method according to claim 8, wherein: The aging conditions include: temperature of 65-95°C and time of 0.5-9h; And / or, the calcination conditions include: temperature of 500-1000° C. and time of 2-18 h.
13. The method according to claim 1, wherein: The conditions of the dehydration reaction include: temperature of 240-360°C; pressure of 0.08-0.24 MPa; liquid phase volume space velocity of 0.15-0.75 h -1 .
14. The method according to claim 1, wherein: The conditions of the dehydration reaction include: temperature of 260-340°C; pressure of 0.08-0.24 MPa; liquid phase volume space velocity of 0.2-0.5 h -1 .
15. The method according to claim 1, wherein: When carrier gas is present, the flow rate of the carrier gas is 15-45 mL‧min -1 .
16. The method according to claim 15, wherein: The flow rate of the carrier gas is 15-40 mL‧min -1 .
17. The method according to claim 1, wherein: The reactor is selected from a fixed bed reactor, a high pressure stirred tank reactor or a tubular reactor.
18. The method according to claim 17, wherein: The reactor is a fixed bed reactor.
Citation Information
Patent Citations
Synthesis process of 4-methyl-1-pentene
CN111574317A
Copper-zirconium based catalyst for removing trace amounts of carbon monoxide, as well as preparation method and use thereof
CN101462057A
Method for preparing copper-zinc-zirconium composite oxide catalyst
CN102078814A