A method for preparing lithium iron phosphate positive electrode material using industrial waste iron mud

By purifying industrial scrap iron sludge into iron red and reacting with other chemical sources, lithium iron phosphate positive electrode material is prepared, which solves the problem of supply and demand imbalance of anhydrous iron phosphate and soaring prices, and realizes cheap and efficient preparation of lithium iron phosphate positive electrode material .

CN116216680BActive Publication Date: 2024-11-29HUBEI LIBAO NEW MATERIAL TECH DEV CO LTD

Patent Information

Application Number
CN202211690936.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-11-29
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

In the existing lithium iron phosphate positive electrode material preparation process, due to the supply and demand imbalance of anhydrous iron phosphate and the soaring price, the development of enterprises is restricted.

Method used

Industrial scrap iron sludge is used as the iron source, iron red is produced through purification and chemical reaction processes, and reacted with phosphorus, lithium source and carbon source to prepare lithium iron phosphate positive electrode material. The process includes oxidation and calcination, acid-soluble filtration, pH adjustment and precipitation of iron, filtration and water washing, drying and crushing, and preparation of lithium iron phosphate.

Benefits of technology

Effective utilization of cheap industrial scrap iron sludge has improved the iron source supply of lithium iron phosphate positive electrode material, simplified the process flow, reduced costs, and solved the problems of impurity removal and iron loss in traditional impurity removal processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116216680B_ABST
    Figure CN116216680B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing lithium iron phosphate positive electrode material using industrial waste iron mud, the method comprising: using industrial waste iron mud as an iron source for purification and chemical reaction to obtain iron red, and then reacting the iron red with a phosphorus source, a lithium source and a carbon source to obtain lithium iron phosphate; specifically comprising the following steps: S1 oxidation roasting step, S2 acid dissolution and filtration step, S3 pH adjustment and iron precipitation step, S4 filtration and water washing step, S5 drying and crushing step, S6 lithium iron phosphate preparation step. The method of the present invention solves the problem of iron mud treatment, greatly improves the utilization value of iron mud, and enriches the iron source of the lithium iron phosphate preparation process; the method of the present invention solves the problem that it is difficult to remove some impurity elements in the existing impurity removal process, and also solves the problem of large-scale iron loss in the impurity removal process; compared with the current mainstream process of preparing lithium iron phosphate using anhydrous iron phosphate, the method of the present invention omits the process of preparing anhydrous iron phosphate, and the process is simpler and the cost is lower.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode material preparation, and more specifically, to a method for preparing lithium iron phosphate positive electrode material by utilizing industrial waste iron mud. Background Art

[0002] Lithium iron phosphate cathode material is a commonly used battery cathode material. The current mainstream process is to use anhydrous iron phosphate as the iron and phosphorus source, lithium carbonate as the lithium source, add carbon source, and prepare lithium iron phosphate cathode material through mixing, sand milling, spray drying, roller furnace sintering, air flow crushing and other processes. However, due to the explosive growth of the lithium iron phosphate market in the past two years, anhydrous iron phosphate is in short supply and the price continues to soar, which seriously restricts the rapid development of lithium iron phosphate companies.

[0003] Therefore, it is very necessary to develop a new process that can directly use cheap raw materials to produce lithium iron phosphate. Summary of the invention

[0004] In view of the fact that the existing technology is limited by the production capacity of anhydrous ferric phosphate, and in order to effectively utilize the by-product iron sludge of nitro reduction (iron sludge: in the process of preparing amines by reducing nitro groups with iron powder, the black mud obtained after separating the products, the main component of which is ferroferric oxide, and also mixed with some organic matter.), the present invention provides a method for preparing lithium iron phosphate positive electrode material using cheap industrial waste iron sludge as an iron source.

[0005] The present invention provides a method for preparing lithium iron phosphate positive electrode material by using industrial waste iron mud. The method comprises: using industrial waste iron mud as an iron source for purification and chemical reaction to obtain iron red, and then reacting the iron red with a phosphorus source, a lithium source and a carbon source to obtain lithium iron phosphate; the method comprises the following steps: S1 oxidation roasting step, S2 acid dissolution and filtration step, S3 pH adjustment and iron precipitation step, S4 filtration and water washing step, S5 drying step, and S6 lithium iron phosphate preparation step.

[0006] The beneficial effects of the present invention are:

[0007] (1) The iron mud, a byproduct of the nitro reduction process, is used as an iron source to prepare lithium iron phosphate positive electrode materials, which solves the problem of iron mud treatment, greatly improves the utilization value of iron mud, and enriches the iron source of lithium iron phosphate preparation process;

[0008] (2) In solving the problem of excessive impurities in the acid-soluble filtrate, the method is different from the traditional method of adding impurity removal reagents to remove impurities. Instead, the method adopts reverse thinking and reasonably controls the pH to reduce the required Fe 3+ Precipitation, while impurity ions do not precipitate, but remain in the solution, and then filtered and washed to obtain a pure iron source, which solves the problem that it is difficult to remove some impurity elements in the existing impurity removal process, and also solves the problem of large iron loss in the impurity removal process;

[0009] (3) Directly using iron oxide red as the iron source to prepare lithium iron phosphate, compared with the current mainstream process of using anhydrous iron phosphate to prepare lithium iron phosphate, the process of preparing anhydrous iron phosphate is omitted, the process is simpler and the cost is lower. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 It is the overall process flow chart of the present invention;

[0011] Figure 2 This is the charge and discharge curve of the battery made of the lithium iron phosphate positive electrode material prepared in Example 1. DETAILED DESCRIPTION

[0012] The present invention provides a method for preparing lithium iron phosphate positive electrode material by using industrial waste iron mud. The method comprises: using industrial waste iron mud as an iron source for purification and chemical reaction to obtain iron red, and then reacting the iron red with a phosphorus source, a lithium source and a carbon source to obtain lithium iron phosphate; the method comprises the following steps: S1 oxidation roasting step, S2 acid dissolution and filtration step, S3 pH adjustment and iron precipitation step, S4 filtration and water washing step, S5 drying step, and S6 lithium iron phosphate preparation step.

[0013] The main impurity elements of iron sludge are shown in Table 1:

[0014] Table 1

[0015]

[0016] Specifically, the overall process is as follows:

[0017] S1. Oxidation roasting process

[0018] The iron mud is roasted in air at a temperature of 300-500°C for 1-3 hours to obtain an oxidized roasted material.

[0019] S2, acid dissolution and filtration process

[0020] Add sulfuric acid to the above-mentioned oxidizing roasting material, heat to 80-100°C, stir and react for 1-5 hours, then filter to obtain an acid-soluble filtrate; wherein the concentration of sulfuric acid is 30-50%, and the ratio of the amount of sulfuric acid to the amount of iron in the oxidizing roasting material is (3-3.5):2.

[0021] S3, pH adjustment iron precipitation process

[0022] A pH regulator is added to the acid-soluble filtrate to adjust the pH to 2.3-3.0, and the reaction is fully stirred to obtain an iron precipitation slurry, wherein the pH regulator is one of ammonia water, sodium hydroxide, and potassium hydroxide.

[0023] S4, Filtration and Washing Process

[0024] The iron precipitate slurry is filtered and the filter cake is washed with pure water. The washing end point is that the conductivity of the rinsing water is ≤300 μs / cm.

[0025] S5, drying and crushing process

[0026] The filter cake is dried and crushed to obtain iron red powder, wherein the drying temperature is 100-200° C. and the particle size D50 after crushing is controlled to be 1-3 μm.

[0027] S6. Process for preparing lithium iron phosphate

[0028] The red iron powder is mixed with a phosphorus source, a lithium source and a carbon source, and the mixture is ground, dried, sintered and crushed to prepare a lithium iron phosphate positive electrode material.

[0029] Specifically, step S6 includes the following steps:

[0030] a. Mix the iron red powder obtained in step S5 with a phosphorus source, a lithium source and a carbon source, and add pure water and stir evenly to obtain a premixed slurry, wherein the phosphorus source is one of LiH2PO4, Li3PO4, H3PO4, NH4H2PO4, (NH4)2HPO4, the lithium source is one of LiH2PO4, Li3PO4, Li2CO3, LiOH, and the carbon source is one of glucose and sucrose. The amount of the iron red powder, the phosphorus source and the lithium source added is determined according to the molar ratio of iron phosphorus to lithium (0.97-1):1:(1-1.03), the amount of the carbon source added is determined according to the carbon content in the lithium iron phosphate of 1.4-2.0%, and the amount of pure water added is determined according to the solid content of the premixed slurry of 30-45%;

[0031] b. Grinding the premixed slurry to a D50 of ≤320 nm, and then spray drying to obtain a lithium iron phosphate precursor;

[0032] c. Sinter the lithium iron phosphate precursor in a nitrogen atmosphere for 10-15 hours at a sintering temperature of 680-800°C, and then crush it with air flow to control the particle size D50 to 0.8-1.5 μm. Remove iron by screening to obtain a lithium iron phosphate positive electrode material.

[0033] Combine the following Figure 1 , the present invention will be described in more detail by way of examples.

[0034] Embodiment 1:

[0035] The iron mud used in this embodiment comes from a domestic m-phenylenediamine production enterprise, and the iron content and impurity element analysis thereof are shown in Table 2 below:

[0036] Table 2

[0037]

[0038] It can be seen from Table 2 that the main impurity elements in the iron mud are Na: 3171.34 ppm, Mn: 1057.12 ppm, Ca: 1073.19 ppm, and Al: 931.58 ppm.

[0039] S1. Oxidation roasting process

[0040] The iron mud is roasted in air at a temperature of 400°C for 2 hours to obtain an oxidized roasted material.

[0041] S2, acid dissolution and filtration process

[0042] Add sulfuric acid solution to the above-mentioned oxidized roasting material, heat to 90°C, stir and react for 4 hours, then filter to obtain an acid-soluble filtrate; wherein the concentration of the sulfuric acid solution is 30%, and the ratio of the amount of sulfuric acid to the amount of iron in the oxidized roasting material is 3.3:2.

[0043] The iron content and impurity element analysis in the acid filtrate are shown in Table 3 below:

[0044] Table 3

[0045] Fe Na K Mg Mn Ca Al Co Ni Cr Cu Ti V Pb Cd % ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm 7.83 375.55 45.63 28.13 121.39 6.42 109.20 7.44 14.52 31.34 6.72 9.59 9.99 0.15 1.36

[0046] From the comparison between Table 3 and Table 2, it can be seen that after the S1 oxidation roasting process and the S2 acid dissolution filtration process, the iron content in the acid-soluble filtrate is 7.83%, the content of the main impurities Na is reduced to 375.55ppm, the content of Mn is reduced to 121.39ppm, and the content of Al is reduced to 109.20ppm. - Calcium sulfate precipitate is formed, so the Ca content is very low, only 6.42ppm.

[0047] S3, pH adjustment iron precipitation process

[0048] Ammonia water as a pH adjuster was added to the acid-soluble filtrate to adjust the pH to 2.6, and the mixture was stirred and reacted to obtain an iron precipitation slurry.

[0049] S4, Filtration and Washing Process

[0050] The above iron precipitate slurry was filtered and the filter cake was washed with pure water. The washing end point was that the conductivity of the rinsing water was ≤300 μs / cm (the actual measurement was 285 μs / cm).

[0051] S5, drying and crushing process

[0052] The filter cake was dried and crushed to obtain iron red powder, wherein the drying temperature was 160° C. and the particle size D50 after crushing was controlled to be 2 μm. The analysis of each impurity element in the iron red is shown in Table 4 below.

[0053] Table 4

[0054] Na K Mg Mn Ca Al Co Ni Cr Cu Ti V Pb Cd ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm ppm 33.71 4.10 2.53 16.35 0.58 49.01 0.67 1.30 5.06 1.09 85.19 1.08 0.02 0.15

[0055] From the comparison between Table 4 and Table 3, it can be seen that after the processes S3-S5, the contents of various impurities in the obtained iron red powder are greatly reduced. Specifically, the content of the main impurity Na is reduced to 33.71ppm, the content of Mn is reduced to 16.35ppm, the content of Al is reduced to 49.01ppm, and the content of Ca is only 0.58ppm.

[0056] S6, a lithium iron phosphate synthesis process, comprising the following steps:

[0057] a. Mix the iron red powder obtained in step S5 with a phosphorus source (NH4H2PO4), a lithium source (Li2CO3) and a carbon source (glucose), and add pure water and stir evenly to obtain a premixed slurry. The amount of the iron red powder, the phosphorus source and the lithium source added is determined according to the molar ratio of iron phosphorus to lithium of 0.98:1:1.01, the amount of the carbon source added is determined according to the carbon content in the lithium iron phosphate of 1.5%, and the amount of pure water added is determined according to the solid content of the premixed slurry of 37%;

[0058] b. Grinding the premixed slurry to a D50 of 320 nm, and then spray drying to obtain a lithium iron phosphate precursor;

[0059] c. The lithium iron phosphate precursor was sintered in a nitrogen atmosphere for 15 h at a sintering temperature of 750° C., and then pulverized by air flow to control the particle size D50 at 1.2 μm. The iron was removed by screening to obtain a lithium iron phosphate positive electrode material.

[0060] Example 2-3

[0061] These embodiments are used to illustrate the method for preparing battery-grade iron phosphate using iron mud provided by the present invention.

[0062] Except that the specific data conditions of each step in the embodiment are shown in Table 5 below, the lithium iron phosphate positive electrode material is prepared by the same method as in Example 1.

[0063] Table 5

[0064]

[0065] Comparative Example

[0066] In this comparative example, anhydrous iron phosphate is used to replace the phosphorus source (NH4H2PO4) in step a of step S6 and the iron red powder prepared in steps S1 to S5 in Example 1, wherein the added amounts of anhydrous iron phosphate and the lithium source (Li2CO3) are determined according to a ratio of the amounts of the two substances of 1:0.505. In addition, the same method as steps ac in step S6 in Example 1 is used to prepare lithium iron phosphate positive electrode material.

[0067] The prepared lithium iron phosphate positive electrode material is tested below.

[0068] The lithium iron phosphate positive electrode materials prepared in Examples 1-3 and the comparative example were tested respectively, and the test results are shown in Table 6. Among them, D50 was tested using a Malvern 3000 laser particle size analyzer, and the compaction density was measured using a powder compaction density meter.

[0069] In order to further study the electrochemical properties of the lithium iron phosphate positive electrode materials obtained in Examples 1 to 3 of the present invention and the comparative example, they were mixed with SP and PVDF in a mass ratio of 8:1:1 in N-methylpyrrolidone (NMP) to form a slurry, which was coated on a carbon-coated aluminum foil, and then dried, rolled, and punched to obtain a positive electrode sheet. Then, a button cell was assembled with metallic lithium as the negative electrode, a polypropylene film as the diaphragm, and lithium hexafluorophosphate as the electrolyte, and a charge and discharge test was performed. The voltage range was between 2.5V and 3.65V. The electrical performance test results are shown in Table 6. The charge and discharge curves of the battery made of the lithium iron phosphate positive electrode material obtained in Example 1 are shown in Table 6. Figure 2 .

[0070] Table 6

[0071]

[0072] From the results in Table 6, it can be seen that the content of each impurity is close to that of each impurity in the lithium iron phosphate positive electrode material prepared by using anhydrous iron phosphate as the phosphorus source and iron source, and the discharge specific capacity is above 155 mAh / g, the first charge and discharge efficiency is greater than 97%, and the electrical performance is equivalent to that of the comparative example. The method provided by the present invention uses iron mud as the iron source, and through purification and chemical reaction processes, iron red with extremely low impurity content is first prepared, and then the iron red can be used to prepare a lithium iron phosphate positive electrode material with good performance.

Claims

1. A method for preparing lithium iron phosphate positive electrode material using industrial waste iron mud, characterized in that: The method comprises: using industrial waste iron mud as an iron source for purification and chemical reaction to obtain iron red, and then reacting the iron red with a phosphorus source, a lithium source and a carbon source to obtain lithium iron phosphate; specifically comprising the following steps: S1 oxidation roasting step, S2 acid dissolution and filtration step, S3 pH adjustment and iron precipitation step, S4 filtration and water washing step, S5 drying and crushing step, S6 lithium iron phosphate preparation step; S2 acid dissolution and filtration step comprises: adding sulfuric acid solution to the oxidation roasting material, heating to 80-100°C, stirring for reaction for 1-5h and then filtering to obtain an acid-soluble filtrate; The concentration of the sulfuric acid solution is 30-50%; S3 pH adjustment iron precipitation process includes: adding a pH regulator to the acid-soluble filtrate, adjusting the pH to 2.3-3.0, stirring fully to react, and obtaining an iron precipitation slurry; S4 filtering and washing process includes: filtering the iron precipitation slurry and washing the filter cake with pure water, and the washing end point is that the conductivity of the rinsing water is ≤300μS / cm; S5 drying and crushing process includes: drying and crushing the filter cake to obtain iron red powder; step S6 includes the following steps: a, mixing the iron red powder obtained in step S5 with a phosphorus source, The lithium source and the carbon source are mixed, and pure water is added and stirred evenly to obtain a premixed slurry, wherein the phosphorus source is one of LiH2PO4, Li3PO4, H3PO4, NH4H2PO4, (NH4)2HPO4, the lithium source is one of LiH2PO4, Li3PO4, Li2CO3, LiOH, and the carbon source is one of glucose and sucrose. The amount of iron red powder added to the phosphorus source and the lithium source is determined according to the molar ratio of iron, phosphorus and lithium of (0.97-1):1:(1-1.03), and the amount of carbon source added is (0.97-1):1:(1-1.03). The amount of pure water added is determined according to the carbon content of lithium iron phosphate being 1.4-2.0%, and the amount of pure water added is determined according to the solid content of the premixed slurry being 30-45%; b. grinding the above premixed slurry to D50≤320nm, and then spray drying to obtain a lithium iron phosphate precursor; c. sintering the above lithium iron phosphate precursor in a nitrogen atmosphere for 10-15h, wherein the sintering temperature is 680-800℃, and then pulverizing with air flow to control the particle size D50 to 0.8-1.5μm, and removing iron by screening to obtain a lithium iron phosphate positive electrode material.

2. The method according to claim 1, characterized in that S1 oxidation roasting process includes: roasting iron mud in air at a temperature of 300-500°C for 1-3 hours to obtain oxidation roasting material.

3. The method according to claim 1, characterized in that The ratio of the amount of sulfuric acid to the amount of iron in the oxidative roasting material is (3-3.5):

2.

4. The method according to claim 1, characterized in that: In step S3, the pH regulator is one of ammonia water, sodium hydroxide, and potassium hydroxide.

5. The method according to claim 1, characterized in that In step S5, the drying temperature is 100-200° C., and the particle size D50 after crushing is controlled to be 1-3 μm.

Citation Information

Patent Citations

  • Method for preparing spherical iron phosphate for lithium iron phosphate cell material

    CN102205953A

  • Preparation method and application of lithium iron phosphate positive electrode material

    CN112897491A

Cited By

  • Water saving method in preparation process of iron oxide red