Stainless steel and preparation method thereof

By adding magnesium and boron to duplex stainless steel to form fine crystal strengthening, the problem of limited performance improvement after niobium is solved, the mechanical and corrosion resistance of steel is improved, and the use of precious alloys is reduced, and the process is optimized. The process improves the stability and safety of the product.

CN116426820BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310283346.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-12-03
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

After the existing duplex stainless steel is added to the steel, its performance improvement is limited. When the niobium increases, the number of NbMo phases increases, the size increases, and the shape becomes sharp edges and angles, resulting in a decrease in mechanical properties and corrosion resistance, and the use of precious alloys increases. , high cost.

Method used

By increasing the content of magnesium and boron in steel, a fine crystal strengthening effect is formed, mechanical properties and corrosion resistance are improved, and the addition of precious alloys such as nickel and molybdenum are reduced. The arc furnace, AOD furnace and LF refining technology are used for smelting and continuous refining. Casting, hot rolling and heat treatment form fine and diffuse MgO particles and magnesium oxide, optimizing the chemical composition and process of steel.

Benefits of technology

The composition uniformity, cost reduction, process simplicity and performance improvement of steel are achieved, tensile strength, yield strength and corrosion resistance are improved, production costs are reduced, and product safety and reliability are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004138802980000071
    Figure BDA0004138802980000071
  • Figure BDA0004138802980000081
    Figure BDA0004138802980000081
  • Figure BDA0004138802980000091
    Figure BDA0004138802980000091
Patent Text Reader

Abstract

The invention relates to a stainless steel and a preparation method thereof. The chemical composition of the stainless steel is C: 0.010%-0.025%, Si: 0.20%-0.60%, Mn: 1.0%-1.5%, P≤0.03%, S≤0.0006%, Cr: 21%-23%, Ni: 3.5%-4.4%, Mo: 1.5%-2.4%, B: 0.0010%-0.0026%, Mg: 0.0015%-0.0030%, TO: 0.0010%-0.0030%, N: 0.13%-0.20%, and the rest is iron and impurities. By increasing the content of magnesium and boron in the steel, the effect of fine grain strengthening is achieved, the mechanical properties, corrosion resistance and welding properties of the steel are improved, and the addition amount of precious alloys such as nickel and molybdenum is reduced, resources are saved, and production costs are reduced; the production process of the stainless steel is simple, the product performance is stable, and the use is safe and reliable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel production, in particular to stainless steel and a preparation method thereof. Background Art

[0002] Duplex stainless steel is composed of two phases, austenite and ferrite, and the volume percentage of one phase is greater than 30%. Under the premise of reasonable control of chemical composition and heat treatment process, duplex stainless steel can combine the advantages of austenitic stainless steel and ferritic stainless steel, that is, it has the excellent toughness and weldability of austenitic stainless steel, and the high strength and good chloride corrosion resistance of ferritic stainless steel. Therefore, it is widely used in industrial fields such as petroleum, chemical industry, and energy.

[0003] The Chinese patent application with application number 202111009802.5 discloses a "stainless steel smelting method, modification method and stainless steel". During the smelting process, the oxygen content in the atmosphere is controlled between 10ppm-100ppm, the nitrogen content is not higher than 400ppm, and the Ti content in the stainless steel is controlled to be greater than 0 but not more than 0.05wt%. Through precise smelting process control, dispersed tiny Ti203 particles can be generated in situ in the stainless steel. The stability of the Ti203 particles is significantly higher than that of TiN and carbides, which can optimize the stainless steel structure and enhance the performance. At the same time, it can also be inherited to effectively inhibit the growth of the welding heat affected zone during the welding process, thereby optimizing the welding performance of the stainless steel. However, Ti203 is easy to aggregate and grow in molten steel, float to the surface of the molten steel and enter the steel slag, resulting in a reduction in Ti203 particles in the steel. At the same time, because Ti203 is easy to aggregate and grow, it is unevenly distributed in the steel, resulting in uneven organization and performance of the steel.

[0004] The Chinese patent application with application number 201911407032.2 discloses "a duplex stainless steel strengthened by microalloying element Nb and its preparation method". The composition and mass percentage of the duplex stainless steel are: C: ≤0.03%, Si≤1.0%, Mn≤2.0%, S≤0.02%, P≤0.03%, Cr: 21-23%, Ni: 4.5-6.5%, Mo: 2.5-3.5%, Nb: 0.03-0.05%, N: 0.08-0.20%, and the rest is Fe and unavoidable impurities. The duplex stainless steel is a duplex stainless steel in which a trace amount of Nb is added to 2205 duplex stainless steel to make 2205 duplex stainless steel have better mechanical properties without reducing its corrosion resistance, which can effectively reduce the cost of duplex stainless steel and expand its application range. The preparation method is simple, and it has important engineering application value and significant economic benefits. However, after adding niobium to the steel, the improvement in performance is very limited. At the same time, when the amount of niobium added is slightly higher, the number and size of the NbMo phase in the stainless steel increase, and the shape changes from the granular state at the initial precipitation to a spindle-like shape with sharp edges. This is very unfavorable to the mechanical properties and corrosion resistance of duplex stainless steel, resulting in reduced mechanical properties and corrosion resistance.

[0005] Therefore, there is an urgent need to develop a stainless steel and a preparation method thereof with uniform composition, low cost, simple process, safe and reliable performance, and improved product quality. Summary of the invention

[0006] The present invention provides a stainless steel and a preparation method thereof. The effects of fine grain strengthening are achieved by increasing the contents of magnesium and boron in the steel, thereby improving the mechanical properties, corrosion resistance and welding properties of the steel, and reducing the amount of precious alloys such as nickel and molybdenum added, thereby saving resources and reducing production costs. The stainless steel has a simple production process, stable product performance, and is safe and reliable to use.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A stainless steel, the chemical composition of which is calculated by weight percentage as follows: C: 0.010%-0.025%, Si: 0.20%-0.60%, Mn: 1.0%-1.5%, P≤0.03%, S≤0.0006%, Cr: 21%-23%, Ni: 3.5%-4.4%, Mo: 1.5%-2.4%, B: 0.0010%-0.0026%, Mg: 0.0015%-0.0030%, TO: 0.0010%-0.0030%, N: 0.13%-0.20%, and the rest is iron and unavoidable impurities.

[0009] Furthermore, the steel has fine dispersed MgO particles, and the mass percentage of the MgO particles in the steel is 0.0025% to 0.0050%.

[0010] Furthermore, the tensile strength of the finished steel plate is 800-980MPa, the yield strength is 560-670MPa, and the elongation is 45%-60%. When the corrosion resistance is tested using a simulated oil field as the corrosion solution, the corrosion current density is 2.1-2.5μA / cm 2 .

[0011] A method for preparing stainless steel includes smelting, continuous casting, hot rolling and heat treatment processes; the specific control process is as follows:

[0012] 1) Smelting;

[0013] Electric arc furnace primary smelting: scrap steel, ferrochrome, electrolytic nickel and ferromolybdenum alloy are put into the electric arc furnace for smelting. After heating and melting, the temperature of the molten steel is controlled at 1650-1680℃ and then added to the AOD furnace for smelting;

[0014] AOD smelting: The molten steel is heated in the AOD furnace, and a mixed gas of oxygen and argon is blown into the molten steel for decarburization; ferrosilicon alloy is added to reduce the slag in the later stage of smelting, and the smelting temperature is controlled at 1705-1758℃ to recover the chromium element in the slag, and the steel is tapped after more than 92% of the slag is removed;

[0015] LF refining: During LF refining, lime, fluorite and aluminum segments are added, CaO and CaF2 are added for slag making, the binary basicity of the refined slag is controlled at 2.0-2.2, and the active oxygen in the molten steel is controlled at 10×10 -6 ~20×10 -6 At this time, magnesium-containing raw materials are added for magnesium treatment, so that the active oxygen in the molten steel reacts with magnesium to generate fine and dispersed magnesium oxide. At the same time, magnesium reacts with sulfur in the molten steel and floats into the slag, so that the sulfur content in the molten steel is less than 0.0006%;

[0016] 2) Continuous casting;

[0017] Cast the molten steel after LF refining treatment, and protect it during the casting process to control the superheat at 20-30℃;

[0018] 3) hot rolling;

[0019] The ingot is heated to 1150-1250°C, kept at this temperature for 2.0-3.0 hours, and then rolled, with the final rolling temperature being greater than 950°C;

[0020] 4) Heat treatment;

[0021] The rolled steel plate is heated to 1000-1050°C, kept at this temperature for 1.0-2.0h, and then subjected to water cooling and solution treatment to obtain a finished steel plate.

[0022] Furthermore, in the LF refining process in step 1), the magnesium-containing raw material block adopts a block-shaped nickel-magnesium alloy with a particle size of 30 to 80 mm, and the mass percentage of magnesium in the nickel-magnesium alloy is 10% to 14%; the nickel-magnesium alloy is directly added to the LF furnace when the active oxygen content of the molten steel reaches the set requirement, and the added amount is 0.025% to 0.040% of the mass of the molten steel.

[0023] Furthermore, in the LF refining process in step 1), the magnesium-containing raw material block uses magnesium iron wire; magnesium iron wire is purified magnesium powder The magnesium iron wire is coated with iron sheet, the thickness of the iron sheet is 0.1-0.4 mm; the magnesium iron wire is fed into the molten steel at a speed of 3.0-5.0 m / s, and the added amount is 0.010%-0.020% of the mass of the molten steel.

[0024] Furthermore, the thickness of the finished steel plate is 5 to 40 mm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1) Form fine and dispersed MgO particles with a mass percentage of 0.0025% to 0.0050% in the steel to achieve the effect of fine grain strengthening and improve the mechanical properties of the steel; the fine grain effect can reduce the segregation degree of the grain boundary and improve the corrosion resistance of the steel; at the same time, the fine and dispersed MgO particles in the steel can inhibit the microstructure growth of the welding heat affected zone during welding, thereby optimizing the welding performance of stainless steel;

[0027] 2) Magnesium plays a role in further deoxidation and desulfurization in the nickel-magnesium alloy added during LF refining; after magnesium treatment, the active oxygen in the molten steel reacts with magnesium to form fine and dispersed magnesium oxide, and at the same time, magnesium reacts with sulfur in the molten steel and floats to the slag, achieving an ultra-low sulfur level of less than 0.0006%;

[0028] 3) By increasing the content of magnesium and boron in steel, the effect of fine grain strengthening is achieved, the mechanical properties, corrosion resistance and welding performance of the steel are improved, and the amount of precious alloys such as nickel and molybdenum added is reduced, resources are saved, and production costs are reduced;

[0029] 4) The stainless steel of the present invention has a simple production process, stable product performance, and is safe and reliable to use. DETAILED DESCRIPTION

[0030] The stainless steel disclosed by the present invention has the following chemical components by weight: C: 0.010%-0.025%, Si: 0.20%-0.60%, Mn: 1.0%-1.5%, P≤0.03%, S≤0.0006%, Cr: 21%-23%, Ni: 3.5%-4.4%, Mo: 1.5%-2.4%, B: 0.0010%-0.0026%, Mg: 0.0015%-0.0030%, TO: 0.0010%-0.0030%, N: 0.13%-0.20%, and the rest is iron and unavoidable impurities.

[0031] Furthermore, the steel has fine dispersed MgO particles, and the mass percentage of the MgO particles in the steel is 0.0025% to 0.0050%.

[0032] Furthermore, the tensile strength of the finished steel plate is 800-980MPa, the yield strength is 560-670MPa, and the elongation is 45%-60%. When the corrosion resistance is tested using a simulated oil field as the corrosion solution, the corrosion current density is 2.1-2.5μA / cm 2 .

[0033] The method for preparing stainless steel of the present invention comprises smelting, continuous casting, hot rolling and heat treatment processes; the specific control process is as follows:

[0034] 1) Smelting;

[0035] Electric arc furnace primary smelting: scrap steel, ferrochrome, electrolytic nickel and ferromolybdenum alloy are put into the electric arc furnace for smelting. After heating and melting, the temperature of the molten steel is controlled at 1650-1680℃ and then added to the AOD furnace for smelting;

[0036] AOD smelting: The molten steel is heated in the AOD furnace, and a mixed gas of oxygen and argon is blown into the molten steel for decarburization; ferrosilicon alloy is added to reduce the slag in the later stage of smelting, and the smelting temperature is controlled at 1705-1758℃ to recover the chromium element in the slag, and the steel is tapped after more than 92% of the slag is removed;

[0037] LF refining: During LF refining, lime, fluorite and aluminum segments are added, CaO and CaF2 are added for slag making, the binary basicity of the refined slag is controlled at 2.0-2.2, and the active oxygen in the molten steel is controlled at 10×10 -6 ~20×10 -6 At this time, magnesium-containing raw materials are added for magnesium treatment, so that the active oxygen in the molten steel reacts with magnesium to generate fine and dispersed magnesium oxide. At the same time, magnesium reacts with sulfur in the molten steel and floats into the slag, so that the sulfur content in the molten steel is less than 0.0006%;

[0038] 5) Continuous casting;

[0039] Cast the molten steel after LF refining treatment, and protect it during the casting process to control the superheat at 20-30℃;

[0040] 6) hot rolling;

[0041] The ingot is heated to 1150-1250°C, kept at this temperature for 2.0-3.0 hours, and then rolled, with the final rolling temperature being greater than 950°C;

[0042] 7) Heat treatment;

[0043] The rolled steel plate is heated to 1000-1050°C, kept at this temperature for 1.0-2.0h, and then subjected to water cooling and solution treatment to obtain a finished steel plate.

[0044] Furthermore, in the LF refining process in step 1), the magnesium-containing raw material block adopts a block-shaped nickel-magnesium alloy with a particle size of 30 to 80 mm, and the mass percentage of magnesium in the nickel-magnesium alloy is 10% to 14%; the nickel-magnesium alloy is directly added to the LF furnace when the active oxygen content of the molten steel reaches the set requirement, and the added amount is 0.025% to 0.040% of the mass of the molten steel.

[0045] Furthermore, in the LF refining process in step 1), the magnesium-containing raw material block uses magnesium iron wire; magnesium iron wire is purified magnesium powder The magnesium iron wire is coated with iron sheet, the thickness of the iron sheet is 0.1-0.4 mm; the magnesium iron wire is fed into the molten steel at a speed of 3.0-5.0 m / s, and the added amount is 0.010%-0.020% of the mass of the molten steel.

[0046] Furthermore, the thickness of the finished steel plate is 5 to 40 mm.

[0047] The chemical composition of the stainless steel described in the present invention is set for the following reasons:

[0048] Carbon: Carbon can promote the formation of austenite and stabilize the austenite structure; but when the carbon content is too high, chromium-rich carbides are easily formed, leading to intergranular corrosion; therefore, the present invention controls the carbon content to 0.010% to 0.025%.

[0049] Silicon: Silicon is a ferrite forming and stabilizing element, and is used for deoxidation during the smelting process to improve the cleanliness of molten steel. Too high a silicon content will accelerate the precipitation of intermetallic phases. Therefore, the present invention controls the silicon content to 0.20% to 0.60%.

[0050] Manganese: Manganese is an austenite-forming and stabilizing element. Manganese can replace nickel to a certain extent to obtain austenite structure and improve the stability of austenite. At the same time, adding manganese can also significantly increase the solubility of nitrogen; but excessive manganese will reduce the corrosion resistance of steel; therefore, the present invention controls the manganese content to 1.0% to 1.5%.

[0051] Sulfur and phosphorus: Sulfur and phosphorus are harmful elements in steel. Sulfur can easily cause hot brittleness of steel, deteriorate the hot workability of stainless steel, and reduce the corrosion resistance of stainless steel due to the formation of manganese sulfide. Therefore, the sulfur content should be strictly controlled. The present invention controls the sulfur content to below 0.0006%. Phosphorus can easily cause cold brittleness of steel. Phosphorus segregation in grain boundaries or phase boundaries will lead to a decrease in the corrosion resistance and toughness of duplex stainless steel. Therefore, the present invention controls the phosphorus content to below 0.030%.

[0052] Chromium: Adding a certain amount of chromium to steel can improve the heat resistance and corrosion resistance of the steel. To ensure good corrosion resistance, a higher amount of chromium needs to be added. However, chromium is the main ferrite-forming element. Excessive chromium will lead to an excessively high chromium equivalent in the steel and an imbalance in the nickel-chromium equivalent ratio. Therefore, the present invention controls the chromium content to 21% to 23%.

[0053] Nickel: Nickel can improve the toughness of steel. Nickel is an element that strongly forms austenite and expands the austenite zone, and plays a major role in ensuring the austenite phase of duplex stainless steel. In order to save costs, it is necessary to reduce the content of expensive nickel and replace nickel with other austenite phase forming elements (such as manganese and nitrogen). However, excessive reduction of the nickel content requires excessive increase of the manganese and nitrogen contents, which will reduce the corrosion resistance and hot workability of the duplex stainless steel. Therefore, the present invention controls the nickel content to 3.5% to 4.4%.

[0054] Molybdenum: Molybdenum is an element that strongly forms the ferrite phase and reduces the austenite zone. Molybdenum can significantly improve the pitting corrosion resistance of duplex stainless steel. The corrosion resistance of molybdenum can only be displayed when there is enough chromium in the steel, and the effective effect of molybdenum increases with the increase of chromium content. However, in order to save costs, it is necessary to reduce the content of expensive molybdenum. Therefore, the molybdenum content is controlled within 1.5% to 2.4% in the present invention.

[0055] Boron: Boron can strengthen the grain boundaries of steel, enhance the bonding force of grain boundaries during hot rolling, improve the hot working properties of steel, and improve the intergranular corrosion resistance of stainless steel. However, too high a boron content will reduce the plasticity and toughness of the material, so the present invention controls the boron content to 0.0010% to 0.0026%.

[0056] Magnesium: When the oxygen content in molten steel is low, magnesium can play a role in desulfurization, forming magnesium sulfide that enters the slag and combines with oxygen to form fine-sized magnesium oxide, which plays a nucleation role in the steel and refines the grains of the steel, thereby improving the strength and plasticity of the product and improving the corrosion resistance; however, excessive magnesium oxide has an adverse effect on the performance of the steel, so the present invention controls the magnesium content to 0.0015% to 0.0030%.

[0057] Oxygen: Oxygen in steel exists in the form of dispersed oxides, which is equivalent to a nucleating agent distributed in the steel, which can improve the nucleation efficiency during the solidification of molten steel and refine the grains; but too much oxide will deteriorate the performance of the steel, so the present invention controls the total oxygen content to 0.0010% to 0.0030%.

[0058] Nitrogen: Nitrogen is a strong austenite-forming element, which can replace nickel to a certain extent to promote austenite formation and stabilize the austenite structure; but when the nitrogen content is too high, pores are easily formed in the ingot, resulting in material scrapping. Therefore, the present invention controls the nitrogen content to 0.13% to 0.20%.

[0059] The method for preparing stainless steel described in the present invention includes smelting (arc furnace primary smelting + AOD smelting + LF refining), continuous casting, hot rolling and heat treatment processes. The details are as follows:

[0060] (1) Primary smelting in electric arc furnace: Scrap steel, ferrochrome, electrolytic nickel and ferromolybdenum alloy are added to the electric arc furnace for smelting. After heating and melting, the temperature of the molten steel is controlled at 1650-1680℃ and then added to the AOD furnace for smelting.

[0061] (2) AOD smelting: The molten steel is heated in an AOD furnace and a mixed gas of oxygen and argon is blown into the molten steel for decarburization. Ferrosilicon alloy is added to reduce the slag in the later stage of smelting. The smelting temperature is controlled at 1705-1758°C to recover the chromium element in the slag. The steel is tapped after more than 92% of the slag is removed.

[0062] (3) LF refining: During LF refining, lime, fluorite and aluminum wire segments are added, and CaO and CaF2 are added for slag formation, and the binary basicity of the refined slag is controlled at 2.0-2.2; the amount of aluminum wire segments added is adjusted to control the active oxygen in the molten steel at (10-20)×10 -6 , at this time, add the magnesium-containing raw material.

[0063] There are two ways to add magnesium-containing raw materials:

[0064] The first is the block alloy addition method; nickel-magnesium alloy is used, the particle size of the nickel-magnesium alloy is 30-80mm, the magnesium content in the nickel-magnesium alloy is 10%-14%, and the nickel-magnesium alloy is directly added to the LF furnace when the active oxygen content of the molten steel meets the requirements, and the added amount accounts for 0.025%-0.040% of the mass of the molten steel; the magnesium in the nickel-magnesium alloy plays a role in further deoxidation and desulfurization. After magnesium treatment, the active oxygen in the molten steel and magnesium generate fine and dispersed magnesium oxide. At the same time, magnesium reacts with the sulfur in the molten steel and floats to the slag, which can achieve an ultra-low sulfur level of less than 0.0006% sulfur content.

[0065] The second method is to feed the wire; that is, to feed the magnesium iron wire, which is made of purified magnesium powder. The iron sheet is coated with iron sheet with a thickness of 0.1-0.4mm. The magnesium iron wire is fed into the molten steel at a speed of 3.0-5.0m / s, and the amount added is 0.010%-0.020% of the mass of the molten steel. The magnesium in the magnesium iron wire plays a role in further deoxidation and desulfurization. After magnesium treatment, the active oxygen in the molten steel reacts with magnesium to generate fine and dispersed magnesium oxide. At the same time, magnesium reacts with sulfur in the molten steel and floats to the steel slag, which can achieve an ultra-low sulfur level of less than 0.0006%.

[0066] (4) Continuous casting: The molten steel after LF refining is transported to the continuous casting platform for casting. During the casting process, protection should be done to prevent the inhalation of air, which will cause the molten steel to increase in oxygen and nitrogen. The casting temperature of the molten steel is controlled to be higher than the liquidus temperature, that is, the superheat is controlled at 20-30°C.

[0067] (5) Hot rolling: The ingot is heated to 1150-1250℃ in a heating furnace for 2.0-3.0h, and then rolled out of the furnace. The final rolling temperature is greater than 950℃, and the thickness of the steel plate after rolling is 5-40mm.

[0068] (6) Heat treatment: The steel plate is heated to 1000-1050°C for 1.0-2.0 h, and then subjected to water-cooling solution treatment to obtain a finished steel plate.

[0069] The mechanical properties of the stainless steel plate were tested, and the tensile strength of the steel plate was 800-980MPa, the yield strength was 560-670MPa, and the elongation was 45%-60%. The corrosion resistance was tested using a simulated oil field as the corrosion solution, and the corrosion current density was 2.1-2.5μA / cm 2 .

[0070] To further describe the present invention, the present invention is described in more detail below in conjunction with embodiments:

[0071] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0072] [Example]

[0073] The chemical composition of the stainless steel in each embodiment and comparative example is shown in Table 1. The chemical composition of the stainless steel in each embodiment is in accordance with the composition ratio of the stainless steel described in the present invention, namely, C: 0.010% to 0.025%, Si: 0.20% to 0.60%, Mn: 1.0% to 1.5%, P≤0.03%, S≤0.006%, Cr: 21% to 23%, Ni: 3.5% to 4.4%, Mo: 1.5% to 2.4%, B: 0.0010% to 0.0026%, Mg: 0.0015% to 0.0030%, TO: 0.0010% to 0.0030%, N: 0.13% to 0.20%, and the rest is iron and unavoidable impurities.

[0074] Table 1 Chemical composition of steel in various embodiments and comparative examples (wt%)

[0075]

[0076]

[0077] The smelting process of stainless steel in each embodiment is as follows:

[0078] Primary smelting in electric arc furnace: Scrap steel, ferrochrome, electrolytic nickel and ferromolybdenum alloy are smelted in an electric arc furnace. After heating and melting, the temperature of the molten steel is controlled at 1650-1680℃ and added to the AOD furnace for smelting. The molten steel is heated in the AOD furnace, and a mixed gas of oxygen and argon is blown into the molten steel for decarburization. In the later stage of smelting, ferrosilicon alloy is added to reduce the slag. The smelting temperature is controlled at 1705-1758℃, and the chromium element in the slag is recovered. After removing more than 92% of the slag, the steel is tapped. During LF refining, lime, fluorite and aluminum wire segments are added, and CaO and CaF2 are added for slag making. The binary basicity of the refined slag is controlled at 2.0-2.2, and the amount of aluminum wire segments added is adjusted to control the active oxygen in the molten steel at (10-20)×10 -6 The smelting process parameters of stainless steel in each embodiment and comparative example are shown in Table 2.

[0079] Table 2 Stainless steel smelting process parameters of each embodiment and comparative example

[0080] Example Electric arc furnace molten steel temperature, ℃ AOD melting temperature, °C Slag removal rate % Refining slag basicity <![CDATA[Activity oxygen of molten steel, 10 -6 > Embodiment 1, 6 1650 1710 92 2.0 20 Embodiment 2, 7 1680 1758 93 2.2 10 Embodiment 3, 8 1676 1705 94 2.1 18 Embodiment 4, 9 1664 1749 92 2.2 15 Embodiment 5, 10 1658 1724 93 2.0 13 Comparative Example 1 1660 1730 93 2.1 3 Comparative Example 2 1671 1734 94 2.2 2

[0081] When the active oxygen in the molten steel is controlled within the set range during LF refining, magnesium-containing raw materials are added. There are two ways to add magnesium-containing raw materials:

[0082] One is the block alloy addition method, using nickel-magnesium alloy, the particle size of the nickel-magnesium alloy is 30-80mm, the magnesium content in the alloy is 10%-14%, and it is directly added to the LF furnace when the active oxygen content of the molten steel reaches the requirement, and the addition amount accounts for 0.025%-0.040% of the mass of the molten steel. The magnesium in the nickel-magnesium alloy plays a role in further deoxidation and desulfurization. After magnesium treatment, the active oxygen in the molten steel and magnesium generate fine and dispersed magnesium oxide, which reduces the active oxygen in the steel to below 0.0003%. At the same time, magnesium reacts with sulfur in the molten steel and floats to the slag, which can achieve an ultra-low sulfur level of less than 0.0006%. Examples 1-5 use the block alloy addition method, and their process parameters are shown in Table 3.

[0083] Table 3 Nickel-magnesium alloy and its addition amount in Examples 1-5

[0084] Example Particle size, mm Magnesium content, % Addition amount accounts for the ratio of molten steel % Example 1 30 10 0.040 Example 2 80 14 0.025 Example 3 50 13 0.028 Example 4 40 12 0.030 Example 5 65 11 0.035

[0085] The second is the wire feeding method, that is, feeding magnesium iron wire, which is used to purify magnesium powder. The iron sheet is coated with iron sheet, the thickness of the iron sheet is 0.1-0.4mm, the magnesium iron wire is fed into the molten steel at a speed of 3-5m / s, and the addition amount accounts for 0.01-0.02% of the mass of the molten steel. The magnesium in the magnesium iron wire plays a role in further deoxidation and desulfurization. After magnesium treatment, the active oxygen in the molten steel and magnesium generate fine and dispersed magnesium oxide, which reduces the active oxygen in the steel to below 0.0003%. At the same time, magnesium reacts with sulfur in the molten steel and floats to the steel slag, which can achieve an ultra-low sulfur level of less than 0.0006%. Examples 6-7 adopt the wire feeding method.

[0086] The method adopted in Comparative Examples 1 and 2 is to use metallic aluminum for complete deoxidation during the LF refining process, and then feed the calcium silicon wire into the molten steel.

[0087] The parameters and addition amounts of the magnesium iron wire in Examples 6 to 7 and the silicon calcium wire in Comparative Examples 1 and 2 are shown in Table 4.

[0088] Table 4 Parameters and addition amount of magnesium iron wire in Examples 6-10 and calcium silicon wire in each comparative example

[0089]

[0090] The molten steel after LF refining treatment is transported to the continuous casting platform for casting. During the casting process, protection is carried out to prevent the inhalation of air, which causes the molten steel to increase oxygen and nitrogen. The casting temperature of the molten steel is controlled to be higher than the liquidus temperature, that is, the superheat degree is 20 to 30°C. The ingot is heated to 1150 to 1250°C in a heating furnace for 2.0 to 3.0 hours, and then rolled out of the furnace. The final rolling temperature is greater than 950°C, and the thickness of the rolled steel plate is 5 to 40mm. The rolled steel plate is heated to 1000 to 1050°C for 1 to 2 hours, and then water-cooled solution treatment is performed to obtain a finished steel plate. The process parameters of continuous casting, hot rolling and heat treatment of each embodiment and comparative example are shown in Table 5.

[0091] Table 5 Process parameters of continuous casting, hot rolling and heat treatment in various embodiments and comparative examples

[0092]

[0093] The mechanical properties of the finished steel plates were tested, and the corrosion resistance of the steel plates was tested under the same corrosion conditions, and a comparative test was performed. The properties of the stainless steel plates in the embodiments and comparative examples are shown in Table 6.

[0094] Table 6 Properties of stainless steel plates in various embodiments and comparative examples

[0095]

[0096] As can be seen from Table 6, the results of mechanical property testing of finished steel plates in Examples 1-10 show that the tensile strength of the steel plates is 800-980 MPa, the yield strength is 560-670 MPa, and the elongation is 45-60%. The corrosion resistance test using the simulated oil field as the corrosion solution shows that the corrosion current density is 2.1-2.5 μA / cm 2 All performances are better than those of Comparative Examples 1 and 2.

[0097] Conclusion: The present invention utilizes magnesium for deoxidation in the later stage of refining to generate fine dispersed magnesium oxide inclusions, thereby achieving the fine grain strengthening effect of steel and improving the mechanical properties of steel. Due to the reduction of grain size, the segregation of grain boundaries and the effect of boron, the corrosion resistance of stainless steel is improved.

[0098] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing stainless steel, characterized in that: The chemical composition of the stainless steel is C: 0.014%-0.025%, Si: 0.50%-0.60%, Mn: 1.0%-1.5%, P≤0.03%, S≤0.0006%, Cr: 22.04%-23%, Ni: 4.2%-4.4%, Mo: 1.5%-2.4%, B: 0.0018%-0.0026%, Mg: 0.0015%-0.0018%, TO: 0.0010%-0.0030%, N: 0.16%-0.20%, and the rest is iron and unavoidable impurities; The preparation method of the stainless steel includes smelting, continuous casting, hot rolling and heat treatment processes; the specific control process is as follows: 1) Smelting; Electric arc furnace primary smelting: scrap steel, ferrochrome, electrolytic nickel and ferromolybdenum alloy are put into the electric arc furnace for smelting. After heating and melting, the temperature of the molten steel is controlled at 1650-1680℃ and then added to the AOD furnace for smelting; AOD smelting: The molten steel is heated in the AOD furnace, and a mixed gas of oxygen and argon is blown into the molten steel for decarburization; ferrosilicon alloy is added to reduce the slag in the later stage of smelting, and the smelting temperature is controlled at 1705-1758℃ to recover the chromium element in the slag. The steel is tapped after more than 92% of the slag is removed; LF refining: During LF refining, lime, fluorite and aluminum segments are added, CaO and CaF2 are added for slag making, the binary basicity of the refined slag is controlled at 2.0-2.2, and the active oxygen in the molten steel is controlled at 10×10 -6 ~20×10 -6 At this time, magnesium-containing raw materials are added for magnesium treatment, so that the active oxygen in the molten steel reacts with magnesium to generate fine and dispersed magnesium oxide. At the same time, magnesium reacts with sulfur in the molten steel and floats into the slag, so that the sulfur content in the molten steel is less than 0.0006%; 2) Continuous casting; The molten steel after LF refining is cast, and the whole casting process is protected to control the superheat at 20-28℃; 3) Hot rolling; The ingot is heated to 1150-1180°C, kept at this temperature for 2.0-3.0 hours, and then rolled, with the final rolling temperature being greater than 950°C; 4) Heat treatment; The rolled steel plate is heated to 1000-1050°C, kept warm for 1.0-2.0h, and then subjected to water-cooling solid solution treatment to obtain a finished steel plate, in which fine dispersed MgO particles are present, and the mass percentage of MgO particles in the steel is 0.0025%-0.0050%; the finished steel plate has a tensile strength of 800-980MPa, a yield strength of 560-670MPa, and an elongation of 45%-60%; when the corrosion resistance is tested using a simulated oil field as a corrosion solution, the corrosion current density is 2.1-2.5µA / cm 2 .

2. A method for preparing stainless steel as claimed in claim 1, characterized in that: In the LF refining process in step 1), the magnesium-containing raw material is a blocky nickel-magnesium alloy with a particle size of 30 to 80 mm, and the mass percentage of magnesium in the nickel-magnesium alloy is 10% to 14%; the nickel-magnesium alloy is directly added to the LF furnace when the active oxygen content of the molten steel reaches the set requirement, and the added amount is 0.025% to 0.040% of the mass of the molten steel.

3. A method for preparing stainless steel as claimed in claim 1, characterized in that: In the LF refining process in step 1), the magnesium-containing raw material is magnesium iron wire; The magnesium iron wire is made of purified magnesium powder coated with iron sheet of ø10-ø15 mm, and the thickness of the iron sheet is 0.1-0.4 mm; the magnesium iron wire is fed into the molten steel at a speed of 3.0-5.0 m / s, and the added amount is 0.010%-0.020% of the mass of the molten steel.

4. A method for preparing stainless steel as claimed in claim 1, characterized in that: The thickness of the finished steel plate is 5 to 40 mm.